Electromagnetic wave absorbing member

The electromagnetic wave absorbing member with a resistive layer having regions of varying conductor patterns ensures stable performance across thickness variations, addressing the instability issue in existing technologies by optimizing electromagnetic wave absorption across a broader frequency range.

WO2024202255A1PCT designated stage expired Publication Date: 2024-10-03LINTEC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/043461
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2023-12-05
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing electromagnetic wave absorbing members with varying spacer layer thicknesses do not maintain stable performance.

Method used

An electromagnetic wave absorbing member comprising a resistive layer, a spacer layer, and a reflective layer, where the resistive layer has regions with different electromagnetic wave absorption characteristics due to varying conductor pattern shapes, sizes, and arrangement intervals, ensuring stable performance across thickness variations.

Benefits of technology

The solution provides a stable electromagnetic wave absorbing member that maintains consistent performance even with large variations in spacer layer thickness, enhancing the absorption characteristics across a broader frequency range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023043461_03102024_PF_FP_ABST
    Figure JP2023043461_03102024_PF_FP_ABST
Patent Text Reader

Abstract

An electromagnetic wave absorbing member (10) comprises a resistive layer (20), a spacer layer (30), and a reflective layer (40). The resistive layer (20), the spacer layer (30), and the reflective layer (40) are laminated in this order. The resistive layer (20) has a plurality of regions which are equal in area in plan view to the electromagnetic wave absorption member (10) and which are different from one another in electromagnetic wave absorption characteristics. Each region includes two or more types of conductor pattern (22) formed in parallel to one another on the spacer layer (30). Each of the two or more types of conductor pattern (22) is formed of a plurality of units arranged in one direction with a certain interval therebetween. The region is different in at least one of the shape of the unit forming the conductor pattern (22), the size of the unit, and the arrangement interval of the unit from another adjacent region.
Need to check novelty before this filing date? Find Prior Art

Description

Electromagnetic wave absorbing materials

[0001] The present invention relates to an electromagnetic wave absorbing member. This application claims priority to Japanese Patent Application No. 2023-053539, filed on March 29, 2023, the contents of which are incorporated herein by reference.

[0002] A sheet-like electromagnetic wave absorbing member that selectively absorbs electromagnetic waves of a predetermined frequency is known. The electromagnetic wave absorbing member, for example, includes a first frequency selective shielding layer and a second frequency selective shielding layer. In such an electromagnetic wave absorbing member, each layer absorbs electromagnetic waves of a predetermined frequency by means of fine line patterns of FSS (Frequency Selective Surface) elements formed in the first frequency selective shielding layer and the second frequency selective shielding layer, and as a whole, the electromagnetic wave absorbing member selectively blocks electromagnetic waves of two different frequencies.

[0003] Patent Document 1 describes a frequency selective surface on which circuit elements can be arranged in a number less than the number of conductors. Patent Document 2 describes a radio wave absorber having a structure in which a full-surface conductor layer made of a conductor, a first dielectric layer, a high-resistance conductor layer having a surface resistivity within a predetermined range, a second dielectric layer, and a pattern layer having a plurality of patterns made of a conductor are sequentially laminated, and each pattern in the pattern layer is different in at least one of size and shape from other adjacent patterns.

[0004] Patent No. 6861907 Patent No. 4461974

[0005] However, in the inventions described in Patent Documents 1 and 2, when the thickness of the spacer layer varies greatly, an electromagnetic wave absorbing member having stable performance cannot be obtained.

[0006] The present invention has been made in view of the above circumstances, and has an object to provide an electromagnetic wave absorbing member that exhibits stable performance even when the thickness of the spacer layer varies greatly.

[0007] The present invention provides the following electromagnetic wave absorbing member: [1] An electromagnetic wave absorbing member having a resistive layer, a spacer layer, and a reflective layer, wherein the resistive layer, the spacer layer, and the reflective layer are laminated in this order, the resistive layer has a plurality of regions that are equal in area in a plan view of the electromagnetic wave absorbing member and have different electromagnetic wave absorption properties from one another, each of the regions having two or more types of conductor patterns formed parallel to one another on the spacer layer, each of the two or more types of conductor patterns consisting of a plurality of units arranged in one direction at regular intervals, and the region differs from adjacent regions in at least one of the shape of the units that make up the conductor pattern, the size of the units, and the arrangement interval of the units. [2] The electromagnetic wave absorbing member according to [1], wherein the regions are provided repeatedly at regular intervals.

[0008] According to the present invention, it is possible to provide an electromagnetic wave absorbing member that can provide stable performance even when the thickness of the spacer layer varies greatly.

[0009] Fig. 1 is a cross-sectional view of a plane along the thickness, which schematically shows an electromagnetic wave absorbing member according to an embodiment of the present invention; Fig. 2 is a plan view schematically showing one region of a resistance layer of the electromagnetic wave absorbing member according to an embodiment of the present invention; Fig. 3 is a top view showing an example of a resistance layer constituting the electromagnetic wave absorbing member according to an embodiment of the present invention; Fig. 4 is a top view showing an example of a resistance layer constituting the electromagnetic wave absorbing member according to an embodiment of the present invention; Fig. 5 is a top view showing an example of a resistance layer constituting the electromagnetic wave absorbing member according to an embodiment of the present invention;

[0010] An embodiment of the electromagnetic wave absorbing member of the present invention will be described. Note that this embodiment is specifically described to provide a better understanding of the gist of the invention, and does not limit the present invention unless otherwise specified.

[0011] In this specification, the term "conductor pattern" refers to an aggregate of geometrically shaped units, and refers to an object that selectively absorbs electromagnetic waves of a certain frequency. A "conductor pattern" can also be said to have the same function as an antenna. In this specification, "electromagnetic waves in the millimeter wave region" refers to electromagnetic waves with a wavelength of 1 mm to 10 mm. "Electromagnetic waves in the millimeter wave region" can also be said to be electromagnetic waves with a frequency of 30 GHz to 300 GHz. In this specification, the symbol "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower and upper limits.

[0012] [Electromagnetic wave absorbing member] Fig. 1 is a cross-sectional view of a surface along the thickness direction, which schematically shows an electromagnetic wave absorbing member according to one embodiment of the present invention. Fig. 2 is a plan view schematically showing one region of an electromagnetic wave absorbing member according to one embodiment of the present invention. As shown in Fig. 1, an electromagnetic wave absorbing member 10 of this embodiment has a resistance layer 20, a spacer layer 30, and a reflective layer 40. The resistance layer 20, the spacer layer 30, and the reflective layer 40 are laminated in this order.

[0013] The reflective layer 40 is disposed on the other surface (back surface) 20b of the resistive layer 20. The spacer layer 30 is disposed between the resistive layer 20 and the reflective layer 40. That is, the resistive layer 20 and the reflective layer 40 are stacked with the spacer layer 30 interposed therebetween.

[0014] The resistive layer 20 may be a single layer, or may include a substrate 21 and a conductive pattern 22 formed on the substrate 21, as shown in Fig. 1. When the resistive layer 20 is a single layer, the resistive layer 20 is made of the same material as the conductive pattern 22 described below.

[0015] "Resistive Layer" The resistive layer 20 is made of a frequency selective surface (FSS). A frequency selective surface is a surface that can block or transmit only electromagnetic waves of a specific frequency by forming a continuous structure with a shape smaller than the wavelength using a conductive material or the like.

[0016] 2 is a top view showing, as an example, one region of the resistive layer in this embodiment. As shown in Fig. 2, the resistive layer 20 has a flat substrate 21 and a conductor pattern 22 formed on one surface 21a of the substrate 21. The conductor pattern 22 is made up of a first conductor pattern 51, a second conductor pattern 52, and a third conductor pattern 53.

[0017] (First Conductive Pattern) As shown in FIG. 2, the first conductive pattern 51 is composed of a plurality of first units u1. Each of the first units u1 is a geometric figure. In other words, the first conductive pattern 51 can be said to be a collection of first units u1, which are geometric figures. Each of the first units u1 functions as an antenna. The first conductive pattern 51 may be, for example, a thin line pattern of an FSS element.

[0018] In the first conductor pattern 51, a plurality of first arrays R1 are formed, each of which has a plurality of first units u1 arranged along the direction indicated by the double-headed arrow P in FIG. 2 . It can also be said that the first conductor pattern 51 has a plurality of first arrays R1. The first conductor pattern 51 can be configured by forming a plurality of first arrays R1 on the substrate 21 at predetermined intervals along the direction indicated by the double-headed arrow P. The intervals between the plurality of first arrays R1 are not particularly limited. The intervals between the first arrays R1 may be regular or irregular.

[0019] As shown in Figure 2, the first unit u1 has a cross shape that is symmetrical in both the vertical and horizontal directions. Specifically, the first unit u1 has one cross portion S1 and four end portions T1. The cross portion S1 is composed of a straight line portion parallel to the x-axis direction and a straight line portion parallel to the y-axis direction in Figure 2. Linear end portions T1 contact both ends of the straight line portion parallel to the x-axis direction and both ends of the straight line portion parallel to the y-axis direction, respectively, so as to be perpendicular to each straight line portion.

[0020] By adjusting the length of the first unit u1 in the x-axis direction and the length of each of the four ends T1 in the x-axis direction, the electromagnetic wave transmission characteristics of the first unit u1 functioning as a single antenna can be adjusted. Similarly, the electromagnetic wave transmission characteristics can be adjusted in the y-axis direction.

[0021] However, the shape of the first unit u1 is not limited to a cross shape. The shape of the first unit u1 is not particularly limited as long as the frequency value at which the amount of electromagnetic wave transmitted through the first conductor pattern 51 reaches a maximum value is A [GHz]. For example, the shape of the figure that is the first unit u1 may be a circle, an annular shape, a linear shape, a square shape, a polygonal shape, an H-shape, a Y-shape, a V-shape, etc.

[0022] In the resistive layer 20, the shapes of the multiple first units u1 are the same. However, the shapes of the multiple first units u1 do not have to be the same figures. In another example of the present invention, the shapes of the multiple first units u1 may be the same or different as long as the transmission characteristics can be adjusted to the target frequency.

[0023] The first conductor pattern 51 selectively transmits electromagnetic waves having a frequency of A [GHz]. The frequency value A [GHz] is the frequency value at which the amount of electromagnetic waves transmitted by the first conductor pattern 51 reaches a maximum value in the range of 20 GHz to 110 GHz.

[0024] The first conductor pattern 51 transmits electromagnetic waves having a frequency A [GHz] determined by the above-described method X. In the resistive layer 20 of this embodiment, the frequency value A is preferably 20 GHz to 110 GHz, more preferably 60 GHz to 100 GHz, even more preferably 65 GHz to 95 GHz, and particularly preferably 70 GHz to 90 GHz. When the frequency value A is within the above numerical range, the resistive layer 20 can transmit electromagnetic waves in the millimeter wave region, making it easier to apply to automobile parts, road-related components, building exterior wall-related materials, windows, communication equipment, radio telescopes, and the like.

[0025] The material of the first unit u1 is not particularly limited as long as the transmission characteristics can be adjusted to the desired frequency. Examples of materials for the first unit u1 include thin metal wires, conductive thin films, and conductive paste fixations. Examples of metal materials include copper, aluminum, tungsten, iron, molybdenum, nickel, titanium, silver, gold, and alloys containing two or more of these metals (e.g., steels such as stainless steel and carbon steel, brass, phosphor bronze, zirconium-copper alloys, beryllium copper, iron-nickel, nichrome, nickel-titanium, Kanthal, Hastelloy, and rhenium-tungsten). Examples of materials for the conductive thin film include metal particles, carbon nanoparticles, and carbon fibers.

[0026] The spacing between the ends of the first unit u1 is not particularly limited as long as the transmission characteristics can be adjusted to the desired frequency. For example, the spacing between the ends of the first unit u1 may all be the same or may be different from each other. However, it is preferable that the spacing between the ends of the first unit u1 be the same, as this makes it easier to design a resistive layer that is less susceptible to the influence of the surrounding environment and improves the accuracy of the frequency band of the electromagnetic waves absorbed during manufacturing.

[0027] 2, the second conductor pattern 52 is composed of a plurality of second units u2. The second conductor pattern 52 is formed in the same manner as the first conductor pattern 51.

[0028] The second conductor pattern 52 selectively transmits electromagnetic waves having a frequency of B [GHz] that satisfies the following formula (2). The frequency value B [GHz] is the frequency value at which the amount of electromagnetic waves transmitted by the second conductor pattern 52 exhibits a maximum value. The frequency value B [GHz] satisfies the following formula (1): 1.037×A≦B≦1.30×A (1)

[0029] As shown in the above formula (2), the second conductor pattern 52 transmits electromagnetic waves with frequencies of 1.037×A [GHz] to 1.30×A [GHz]. The second conductor pattern 52 preferably transmits electromagnetic waves with frequencies of 1.17×A [GHz] to 1.30×A [GHz]. Because the second conductor pattern 52 transmits electromagnetic waves with frequencies of 1.037×A [GHz] or higher, the peak of the amount of electromagnetic wave transmitted by the second conductor pattern 52 and the peak of the amount of electromagnetic wave transmitted by the first conductor pattern 51 sufficiently overlap in the frequency band higher than A [GHz]. As a result, the frequency band of electromagnetic waves that can be transmitted by the entire electromagnetic wave-absorbing film is expanded to a frequency band higher than A [GHz], compared to a film having the first conductor pattern 51 alone. Since the second conductor pattern 52 transmits electromagnetic waves with frequencies of 1.30×A [GHz] or less, the frequency difference between the peak of the transmission amount of electromagnetic waves through the second conductor pattern 52 and the peak of the transmission amount of electromagnetic waves through the first conductor pattern 51 becomes small in the frequency band higher than A [GHz]. As a result, a single peak is formed at which the transmission amount of electromagnetic waves transmitted through the entire electromagnetic-wave-absorbing film reaches a local maximum value. As described above, since the second conductor pattern 52 transmits electromagnetic waves with frequencies of 1.037×A [GHz] to 1.30×A [GHz], the transmission amount of electromagnetic waves transmitted through the entire electromagnetic-wave-absorbing film is extended into the higher-frequency frequency band.

[0030] The material of the second units u2 constituting the second conductor pattern 52 is not particularly limited as long as it can absorb electromagnetic waves of B [GHz] and the absorption characteristics can be adjusted to the desired frequency. The material of the second units u2 is the same as that described for the material of the first units u1.

[0031] 2, the third conductor pattern 53 is composed of a plurality of third units u3. The third conductor pattern 53 is formed in the same manner as the first conductor pattern 51.

[0032] The third conductor pattern 53 selectively transmits electromagnetic waves having a frequency of C [GHz] that satisfies the following formula (3). The frequency value C [GHz] is the frequency value at which the amount of electromagnetic waves transmitted by the third conductor pattern 53 exhibits a maximum value. The frequency value C [GHz] satisfies the following formula (2): 0.60×A≦C≦0.963×A (2)

[0033] As shown in the above formula (3), the third conductor pattern 53 transmits electromagnetic waves with frequencies of 0.60×A [GHz] to 0.963×A [GHz]. The third conductor pattern 53 preferably transmits electromagnetic waves with frequencies of 0.60×A [GHz] to 0.83×A [GHz]. Because the third conductor pattern 53 transmits electromagnetic waves with frequencies of 0.60×A [GHz] or higher, the frequency difference between the peak amount of electromagnetic wave transmission by the third conductor pattern 53 and the peak amount of electromagnetic wave transmission by the first conductor pattern 51 is reduced in the frequency band lower than A [GHz]. As a result, a single peak is formed at which the amount of electromagnetic wave transmission through the entire resistive layer 20 is maximized. Because the third conductor pattern 53 transmits electromagnetic waves with frequencies of 0.963×A [GHz] or less, the peak of the amount of electromagnetic waves transmitted by the third conductor pattern 53 and the peak of the amount of electromagnetic waves transmitted by the first conductor pattern 51 fully overlap in the frequency band lower than A [GHz]. As a result, the frequency band of electromagnetic waves that can be transmitted through the entire electromagnetic-wave-absorbing film is expanded to a frequency band lower than A [GHz], compared to a film having only the first conductor pattern 51. As described above, because the third conductor pattern 53 transmits electromagnetic waves with frequencies of 0.60×A [GHz] to 0.963×A [GHz], the amount of electromagnetic waves transmitted through the entire resistive layer 20 is expanded to a frequency band on the lower frequency side.

[0034] The material of the third unit u3 constituting the third conductor pattern 53 is not particularly limited as long as it can transmit electromagnetic waves of C [GHz] and the transmission characteristics can be adjusted to the desired frequency. The material of the third unit u3 is the same as that described for the material of the first unit u1.

[0035] In the resistive layer 20 shown in FIG. 2 , the first array R1, the second array R2, and the third array R3 are arranged adjacent to one another along the direction indicated by the double-headed arrow P. Because the first array R1, the second array R2, and the third array R3 are arranged adjacent to one another on the substrate 21, the frequency band of the electromagnetic waves selectively transmitted by the second conductor pattern 52 and the frequency band of the electromagnetic waves selectively transmitted by the third conductor pattern 53 overlap, based on the frequency value A [GHz] of the peak position of the electromagnetic waves selectively transmitted by the first conductor pattern 51. As a result, the transmission range of the electromagnetic waves transmitted through the entire resistive layer 20 is easily expanded toward both the high-frequency side and the low-frequency side, based on the frequency value A [GHz] of the peak position.

[0036] The distance d1 between the first unit u1 and the second unit u2, the distance d2 between the second unit u2 and the third unit u3, and the distance d3 between the third unit u3 and the first unit u1, shown in FIG. 2, may be the same as or different from one another. The distance d1 may be, for example, 0.2 mm to 4 mm, 0.3 mm to 2 mm, or 0.5 mm to 1 mm. The distance d2 may be, for example, 0.2 mm to 4 mm, 0.3 mm to 2 mm, or 0.5 mm to 1 mm. The distance d3 may be, for example, 0.2 mm to 4 mm, 0.3 mm to 2 mm, or 0.5 mm to 1 mm. When the distances d1, d2, and d3 are each within the above-described ranges, the transmission range of electromagnetic waves transmitted through the entire resistive layer 20 is likely to be further expanded relative to the frequency value A [GHz] at the peak position.

[0037] In the resistive layer 20, the first unit u1, the second unit u2, and the third unit u3 have the same shape. However, the shapes of the first unit u1, the second unit u2, and the third unit u3 do not have to be the same. That is, in another example of the present invention, the shapes of the first unit u1, the second unit u2, and the third unit u3 may be the same or different from each other.

[0038] 3 , in the electromagnetic wave absorbing member 10 of this embodiment, the resistance layer 20 has two regions 20A and 20B that have the same area but different electromagnetic wave absorption characteristics in a plan view of the electromagnetic wave absorbing member 10. The regions 20A and 20B have the same shape. In the electromagnetic wave absorbing member 10 of this embodiment, the two regions 20A and 20B have a similar shape (here, a square) to the electromagnetic wave absorbing member 10 in a plan view of the electromagnetic wave absorbing member 10. In the electromagnetic wave absorbing member 10 of this embodiment, the two regions 20A and the two regions 20B are arranged at diagonal corners of the resistance layer 20 in a plan view of the electromagnetic wave absorbing member 10, and the diagonal lines of the two regions 20A and the diagonal lines of the two regions 20B are perpendicular to each other. As a result, the regions 20A and the regions 20B are arranged adjacent to each other in a lattice pattern.

[0039] Region 20A and region 20B each have, for example, the first conductor pattern 51, second conductor pattern 52, and third conductor pattern 53 described above. Region 20A differs from adjacent region 20B in at least one of the shapes of the units (first unit u1, second unit u2, and third unit u3) constituting conductor pattern 22 (first conductor pattern 51, second conductor pattern 52, and third conductor pattern 53), the size of the units, and the arrangement intervals of the units. This results in different electromagnetic wave transmission characteristics between region 20A and region 20B. For example, if region 20A has multiple conductor pattern groups as described above, region 20B preferably has conductor pattern groups of the same type, and at least one of the surface area, thickness, and arrangement intervals of the conductor pattern groups are reduced by a predetermined amount. Specifically, the surface area or thickness of each of the conductor patterns in region 20B is preferably 99 to 60%, and more preferably 95 to 80%, of the conductor patterns in region 20A. The arrangement spacing of region 20B is preferably 99 to 60%, and more preferably 90 to 70%, of the conductor patterns in region 20A.

[0040] The substrate 21 is not particularly limited as long as it has a flat plate shape and is capable of forming the first conductor pattern 51, the second conductor pattern 52, and the third conductor pattern 53 on one surface 21 a. The substrate 21 may have a single-layer structure or a multi-layer structure.

[0041] The thickness of the substrate 21 may be, for example, 5 μm to 500 μm, 15 μm to 200 μm, or 25 μm to 100 μm. The thicknesses of the first conductor pattern 51, the second conductor pattern 52, and the third conductor pattern 53 are not particularly limited. These thicknesses can be changed as desired depending on the desired characteristics. Furthermore, these three thicknesses may be the same or different from one another, but are preferably the same in terms of productivity. From the viewpoint of achieving both electromagnetic wave transparency and curved surface conformability, the thicknesses of the first conductor pattern 51, the second conductor pattern 52, and the third conductor pattern 53 are preferably 10 nm to 300 μm, more preferably 40 nm to 100 μm, and particularly preferably 80 nm to 1 μm.

[0042] The material of the substrate 21 can be selected appropriately depending on the application of the electromagnetic wave absorbing member 10. For example, the substrate 21 may be made of a transparent material in order to provide transparency to the electromagnetic wave absorbing member 10. Alternatively, the substrate 21 may be made of a flexible material in order to provide conformability to the curved surface of the electromagnetic wave absorbing member 10. The surface of the substrate 21 may be smoothed in order to improve the transparency and three-dimensional formability of the electromagnetic wave absorbing member 10.

[0043] For example, the substrate 21 can be made of a resin. The resin may be a thermoplastic resin or a thermosetting resin. However, when the three-dimensional formability of the electromagnetic wave absorbing member 10 is taken into consideration, the substrate 21 preferably contains a thermoplastic resin. Examples of thermoplastic resins include polyolefin resins, polyester resins, polyester-polyether resins, polyacrylic resins, polystyrene resins, polyimide resins, polyimideamide resins, polyamide resins, polyurethane resins, polycarbonate resins, polyarylate resins, melamine resins, epoxy resins, urethane resins, silicone resins, and fluororesins. Specific examples of polyolefin resins include polypropylene and polyethylene. Specific examples of polyester resins include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate.

[0044] The substrate 21 may contain optional components within the scope of not impairing the effects of the present invention. Examples of the optional components include inorganic fillers, colorants, curing agents, antioxidants, light stabilizers, flame retardants, conductive agents, antistatic agents, and plasticizers.

[0045] The thickness, dielectric constant, electrical conductivity, and magnetic permeability of the substrate 21 can be set as appropriate to further improve the electromagnetic wave absorption performance of the electromagnetic wave absorbing member 10. When the electrical characteristics of the electromagnetic waves to be absorbed are taken into consideration, the substrate 21 may be a high dielectric constant layer. If the substrate 21 is a high dielectric constant layer, the thickness of the electromagnetic wave absorbing member 10 can be made relatively thin.

[0046] The resistance layer 20 can be fabricated, for example, by the following method. First, a substrate 21 is prepared. Next, a first conductor pattern 51, a second conductor pattern 52, and a third conductor pattern 53 are formed on one surface 21a of the substrate 21. When forming each conductor pattern, the conductor patterns are formed so that the frequency value at which the amount of electromagnetic wave transmitted by each conductor pattern shows a maximum value is a predetermined value [GHz]. The order in which each conductor pattern is formed is not particularly limited. Each conductor pattern may be formed in the same process, or may be formed in separate processes.

[0047] The method for forming each conductor pattern is not particularly limited as long as it can form a predetermined frequency. Examples of the method for forming each conductor pattern include the following: A printing method in which each conductor pattern is printed on one surface 21a of the substrate 21 using a conductive paste. A development method in which each conductor pattern is developed on one surface 21a of the substrate 21. A method in which a metal thin film is provided on one surface 21a of the substrate 21 by sputtering, vacuum deposition, or lamination of a metal foil, and a pattern of the metal thin film is formed on one surface 21a of the substrate 21 by photolithography. A method in which a metal wire is disposed on one surface 21a of the substrate 21.

[0048] "Spacer Layer" The spacer layer 30 is provided on the other surface 20b of the resistive layer 20. The spacer layer 30 has two surfaces 30a and 30b. One surface 30a of the spacer layer 30 faces the other surface 20b of the resistive layer 20. A reflective layer 40 is provided on the other surface 30b of the spacer layer 30. The spacer layer 30 may have a single-layer structure or a multi-layer structure.

[0049] The material of the spacer layer 30 can be appropriately selected depending on the application, and examples thereof include plastic film, paper, cloth, nonwoven fabric, rubber sheet, and foam sheet. Among these, a foam sheet is preferred from the viewpoint of easily increasing the thickness while reducing the weight. For example, a foam sheet formed by foaming the resin constituting the plastic film and forming it into a sheet can be used. Specific examples of foam sheets include polyethylene foam, polypropylene foam, and polyurethane foam.

[0050] When considering the wavelength shortening effect of the spacer layer 30, the thickness of the spacer layer 30 is appropriately changed depending on the wavelength of the electromagnetic wave to be absorbed and the relative dielectric constant of the spacer layer 30. When considering the wavelength shortening effect of the spacer layer 30, the thickness of the spacer layer 30 preferably satisfies the following formula (3): (Thickness of the spacer layer 30 in the z-axis direction) = (λ) × (¼) / (ε) ½ ... formula (3) In the above formula (3), λ is the wavelength of the incident electromagnetic wave, and ε is the relative dielectric constant of the spacer layer 30. The thickness of the spacer layer 30 may be appropriately adjusted to suit the absorption characteristics. For example, the thickness can be changed within a range of 0.1 to 3.0 times the thickness of the spacer layer 30 obtained by the above formula (3).

[0051] When the relationship between the thickness of the spacer layer 30 and the wavelength λ satisfies the above formula (3), the electromagnetic wave absorbing member 10 has a so-called λ / 4 structure. This further increases the maximum absorption of electromagnetic waves by the electromagnetic wave absorbing member 10. The thickness of the spacer layer 30 can be appropriately set depending on the wavelength λ of the electromagnetic waves to be absorbed. The thickness of the spacer layer 30 may be, for example, 25 μm to 5000 μm, 300 μm to 4000 μm, or 1000 μm to 3000 μm. The spacer layer 30 may be made of a material with a high dielectric constant. If the spacer layer 30 has a high dielectric constant, the thickness of the spacer layer 30 can be made relatively thin. When the dielectric constant of the spacer layer 30 is taken into consideration, the spacer layer 30 preferably contains at least one material selected from the group consisting of barium titanate, titanium oxide, and strontium titanate.

[0052] "Reflective Layer" The reflective layer 40 has two surfaces 40a and 40b. One surface 40a of the reflective layer 40 faces the other surface 30b of the spacer layer 30. The reflective layer 40 is not particularly limited as long as it can reflect electromagnetic waves that arrive at the surface of the electromagnetic wave absorbing member 10 and transmit through the electromagnetic wave absorbing member 10. A portion of the electromagnetic waves that arrive at the electromagnetic wave absorbing member 10 is reflected by or absorbed by the resistive layer 20. On the other hand, electromagnetic waves that are not reflected or absorbed by the resistive layer 20 transmit through the resistive layer 20. The electromagnetic waves that transmit through the resistive layer 20 are reflected by the reflective layer 40 toward the resistive layer 20. For example, if the reflective layer 40 has conductivity in the surface direction of either of the two surfaces 40a and 40b, it can reflect the electromagnetic waves that transmit through the resistive layer 20. Specifically, a metal foil such as aluminum foil or copper foil, or a metal plate such as a copper plate, laminated to a resin film such as polyethylene terephthalate may be used as the reflective layer 40. Instead of the metal foil or metal plate, a transparent conductive film such as ITO, or a mesh sheet formed of metal wires may be used. Among these, a metal plate is preferred in terms of high conductivity.

[0053] Considering the reflective properties of the reflective layer 40, a metal wire, a conductive thread, a twisted thread containing a metal wire and a conductive thread, or a conductive thin film may be provided on the other surface 40b of the reflective layer 40. The conductive thin film can be provided on the surface 40b by, for example, a printing method such as screen printing, gravure printing, or inkjet printing; a sputtering method or vacuum deposition; or photolithography.

[0054] When the spacer layer 30 is formed on a conductive material such as metal, the conductive material such as metal serves as the reflective layer 40, and therefore the reflective layer 40 can be omitted.

[0055] For the purpose of applying the electromagnetic wave absorbing member 10 to the surfaces of various articles, an adhesive layer may be provided on the other surface 40b of the reflective layer 40. When an adhesive layer is provided on the other surface 40b of the reflective layer 40, a release film may be provided on the surface of the adhesive layer opposite to the side that comes into contact with the other surface 40b. The release film is removed when the electromagnetic wave absorbing member 10 is used. Covering the adhesive surface with the release film improves handling during distribution.

[0056] Examples of adhesives constituting the adhesive layer include heat-sealing adhesives that bond by heat; adhesives that develop adhesiveness by wetting; and pressure-sensitive adhesives (adhesives) that bond by pressure. Among these, pressure-sensitive adhesives (pressure-sensitive adhesives) are preferred from the viewpoint of simplicity. Specific examples of adhesives include acrylic adhesives, urethane adhesives, rubber adhesives, polyester adhesives, silicone adhesives, polyvinyl ether adhesives, and the like. Among these, at least one selected from the group consisting of acrylic adhesives, urethane adhesives, and rubber adhesives is preferred, with acrylic adhesives being more preferred.

[0057] The electromagnetic wave absorbing member 10 of this embodiment may also include a protective layer formed on one surface (front surface) 20a of the resistance layer 20. The protective layer is not particularly limited as long as it can protect the resistance layer 20.

[0058] According to the electromagnetic wave absorbing member 10 of this embodiment, the resistive layer 20 has two regions 20A and 20B that are equal in area in a plan view of the electromagnetic wave absorbing member 10 but have different electromagnetic wave transmission characteristics. Region 20A is different from adjacent region 20B in at least one of the shape of the units constituting the conductor pattern 22, the size of the units, and the arrangement interval of the units. This results in different electromagnetic wave transmission characteristics between regions 20A and 20B. By configuring the resistive layer 20 with regions 20A and 20B that have different electromagnetic wave transmission characteristics, the electromagnetic wave transmission characteristics of the resistive layer 20 are an average of the electromagnetic wave transmission characteristics of region 20A and region 20B. As a result, even if the thickness of the spacer layer 30 varies significantly, the thickness variation can be offset to provide an electromagnetic wave absorbing member 10 with stable performance.

[0059] The electromagnetic wave absorption characteristic refers to the electromagnetic wave transmittance in the resistance layer 20 (regions 20A and 20B).

[0060] Other Embodiments The present invention is not limited to the above-described embodiments.

[0061] For example, the configurations of the electromagnetic wave absorbing members according to the first to sixth modified examples shown in FIGS. 4(a), 4(b), 5(a), 5(b), and 5(c) may be adopted.

[0062] As in the electromagnetic wave absorbing member 100 according to the first modified example shown in Fig. 4(a), the resistance layer 120 has two regions 120A and 120B that have the same area but different electromagnetic wave transmission characteristics in a plan view of the electromagnetic wave absorbing member 100. The regions 120A and 120B have the same shape. In the electromagnetic wave absorbing member 100 of this embodiment, the regions 120A and 120B have a similar shape (here, a square) to the electromagnetic wave absorbing member 100 in a plan view of the electromagnetic wave absorbing member 100. In the electromagnetic wave absorbing member 100 of this embodiment, the regions 120A and 120B are arranged alternately adjacent to each other in a plan view of the electromagnetic wave absorbing member 100, and eight regions 120A and eight regions 120B are arranged in a lattice pattern.

[0063] Region 120A and region 120B each have, for example, the first conductor pattern 51, the second conductor pattern 52, and the third conductor pattern 53 described above. Region 120A differs from adjacent region 120B in at least one of the shape, size, and arrangement interval of the units (first unit u1, second unit u2, and third unit u3) constituting conductor pattern 22 (first conductor pattern 51, second conductor pattern 52, and third conductor pattern 53). This results in regions 120A and 120B having different electromagnetic wave transmission characteristics. Furthermore, regions 120A and 120B preferably have the same surface area, thickness, and arrangement interval relationships of the conductor pattern groups as regions 20A and 20B in FIG. 3 described above.

[0064] As in the electromagnetic wave absorbing member 200 according to the second modified example shown in Fig. 4(b), the resistance layer 220 has two regions 220A and 220B that have the same area but different electromagnetic wave transmission characteristics in a plan view of the electromagnetic wave absorbing member 200. The regions 220A and 220B have the same shape. In the electromagnetic wave absorbing member 200 of this embodiment, the regions 220A and 220B have a similar shape (here, a square) to the electromagnetic wave absorbing member 200 in a plan view of the electromagnetic wave absorbing member 200. In the electromagnetic wave absorbing member 200 of this embodiment, the regions 220A and 220B are arranged alternately adjacent to each other in a plan view of the electromagnetic wave absorbing member 200, and 32 regions 220A and 32 regions 220B are arranged in a lattice pattern.

[0065] Region 220A and region 220B each have, for example, the first conductor pattern 51, second conductor pattern 52, and third conductor pattern 53 described above. Region 220A differs from adjacent region 220B in at least one of the shapes of the units (first unit u1, second unit u2, and third unit u3) constituting conductor pattern 22 (first conductor pattern 51, second conductor pattern 52, and third conductor pattern 53), the size of the units, and the arrangement spacing of the units. This results in regions 220A and 220B having different electromagnetic wave transmission characteristics. Furthermore, regions 220A and 220B preferably have the same surface area, thickness, and arrangement spacing relationships of the conductor pattern groups as regions 20A and 20B in FIG. 3 described above. Furthermore, the number of different regions is not limited to two, and may be three or more. For example, three different regions, region 220A, region 220B, and region 220C, may be repeated. In this case, with region 220B as the reference, it is preferable that region 220A has at least one of the surface area, thickness, and arrangement spacing of the conductor pattern group of 101 to 150%, and more preferably 105 to 130%. It is preferable that region 220C has at least one of the surface area, thickness, and arrangement spacing of the conductor pattern group of 99 to 60%, and more preferably 95 to 70%. In this case, it is preferable that region 220A, region 220B, and region 220C are arranged repeatedly in this order.

[0066] 5(a), the resistance layer 320 has two regions 320A and 320B that have the same area but different electromagnetic wave transmission characteristics in a plan view of the electromagnetic wave absorbing member 300. The regions 320A and 320B have the same shape. In the electromagnetic wave absorbing member 300 of this embodiment, the regions 320A and 320B are arranged along one direction of the electromagnetic wave absorbing member 300 in a plan view of the electromagnetic wave absorbing member 300. That is, the regions 320A and 320B are arranged in a strip shape along one direction of the electromagnetic wave absorbing member 300.

[0067] Region 320A and region 320B each have, for example, the first conductor pattern 51, the second conductor pattern 52, and the third conductor pattern 53 described above. Region 320A differs from adjacent region 320B in at least one of the shape, size, and arrangement interval of the units (first unit u1, second unit u2, and third unit u3) constituting conductor pattern 22 (first conductor pattern 51, second conductor pattern 52, and third conductor pattern 53). This results in regions 320A and 320B having different electromagnetic wave transmission characteristics. Furthermore, regions 320A and 320B preferably have the same surface area, thickness, and arrangement interval relationships of the conductor pattern groups as regions 20A and 20B in FIG. 3 .

[0068] As in the electromagnetic wave absorbing member 400 according to the fourth modified example shown in FIG. 5B , the resistance layer 420 has two regions 420A and 420B that have the same area but different electromagnetic wave transmission characteristics in a plan view of the electromagnetic wave absorbing member 400. The regions 420A and 420B have the same shape. In the electromagnetic wave absorbing member 400 of this embodiment, the regions 420A and 420B are arranged along one direction of the electromagnetic wave absorbing member 400 in a plan view of the electromagnetic wave absorbing member 400. That is, the regions 420A and 420B are arranged in a strip shape along one direction of the electromagnetic wave absorbing member 400. In the electromagnetic wave absorbing member 400 of this embodiment, the regions 420A and 420B are arranged alternately adjacent to each other in a plan view of the electromagnetic wave absorbing member 400, and the two regions 420A and the two regions 420B are arranged in a strip shape.

[0069] Region 420A and region 420B each have, for example, the first conductor pattern 51, the second conductor pattern 52, and the third conductor pattern 53 described above. Region 420A differs from adjacent region 420B in at least one of the shape, size, and arrangement interval of the units (first unit u1, second unit u2, and third unit u3) constituting conductor pattern 22 (first conductor pattern 51, second conductor pattern 52, and third conductor pattern 53). This results in regions 420A and 420B having different electromagnetic wave transmission characteristics. Furthermore, regions 420A and 420B preferably have the same surface area, thickness, and arrangement interval relationships of the conductor pattern groups as regions 20A and 20B in FIG. 3 .

[0070] As in the electromagnetic wave absorbing member 500 according to the fifth modified example shown in FIG. 5( c), the resistance layer 520 has two regions 520A and 520B that have the same area but different electromagnetic wave transmission characteristics in a plan view of the electromagnetic wave absorbing member 500. The regions 520A and 520B have the same shape. In the electromagnetic wave absorbing member 500 of this embodiment, the regions 520A and 520B are arranged along one direction of the electromagnetic wave absorbing member 500 in a plan view of the electromagnetic wave absorbing member 500. That is, the regions 520A and 520B are arranged in a strip shape along one direction of the electromagnetic wave absorbing member 500. In the electromagnetic wave absorbing member 500 of this embodiment, the regions 520A and 520B are arranged alternately adjacent to each other in a plan view of the electromagnetic wave absorbing member 500, and five regions 520A and five regions 520B are arranged in a strip shape.

[0071] Region 520A and region 520B each have, for example, the first conductor pattern 51, second conductor pattern 52, and third conductor pattern 53 described above. Region 520A differs from adjacent region 520B in at least one of the shape, size, and arrangement interval of the units (first unit u1, second unit u2, and third unit u3) constituting conductor pattern 22 (first conductor pattern 51, second conductor pattern 52, and third conductor pattern 53). This results in regions 520A and 520B having different electromagnetic wave transmission characteristics. Furthermore, regions 520A and 520B preferably have the same surface area, thickness, and arrangement interval relationships of the conductor pattern groups as regions 20A and 20B in FIG. 3 described above. Furthermore, the number of different regions is not limited to two, and may be three or more. For example, three different regions, region 520A, region 520B, and region 520C, may be repeated. In this case, with region 520B as the reference, region 520A preferably has at least one of the surface area, thickness, and arrangement spacing of the conductor pattern group of 101 to 150%, and more preferably 105 to 130%. Region 520C preferably has at least one of the surface area, thickness, and arrangement spacing of the conductor pattern group of 99 to 60%, and more preferably 95 to 70%. In this case, region 520A, region 520B, and region 520C are preferably arranged repeatedly in this order.

[0072] The present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0073] Comparative Example 1 "Preparation of Electromagnetic Wave Absorbing Member" A pattern of water-washable ink was printed on a substrate made of a 50 μm-thick PET film (product name: PET50A4160, manufactured by Toyobo Co., Ltd.), and a 100 nm-thick copper thin film was formed by vapor deposition. The ink was then washed away with water, and the copper thin film on the water-washable ink was removed, thereby patterning a conductor pattern to obtain a resistive layer. On the back surface of the obtained resistive layer, a 1.80 mm-thick urethane foam sheet (manufactured by Inoac Corporation) was attached as a spacer layer, and an aluminum-deposited PET film (flexural rigidity: 8.33 Pa mm) was attached as a reflective layer. 4 ) were laminated in this order to produce an electromagnetic wave absorbing member with absorption properties in the 76 to 81 GHz band. The resistive layer had the conductor pattern shown in Figure 2. Specifically, of the three patterns of large, medium, and small sizes, the medium size pattern was designed to have a size and shape that maximized transparency at 79 GHz, with the large pattern having a cross portion whose length was increased by 20%, and the small pattern having a cross portion whose length was reduced by 20%. The pattern widths were the same for the large, medium, and small patterns. As examples of different thicknesses on the spacer layer side, similar configurations were also produced for spacer layer thicknesses of 2.00 mm and 2.20 mm.

[0074] [Comparative Example 2] "Preparation of Electromagnetic Wave Absorbing Member" For the resistive layer, the pattern widths of the large, medium, and small patterns of Comparative Example 1 were kept the same, but the lengths of the cross portions were each reduced to 90%. In addition, the distance between the patterns was reduced to 75% of that of Comparative Example 1. Otherwise, the electromagnetic wave absorbing member of Comparative Example 2 was prepared in the same manner as Comparative Example 1.

[0075] [Example 1] An electromagnetic wave absorbing member of Example 1 was produced in the same manner as in Comparative Example 1, except that the resistive layer shown in Fig. 3 was formed. The size of each unit was 32 mm x 32 mm, and 15 x 15 large, medium, and small patterns similar to those in Comparative Example 1 were arranged in one unit, and 20 x 20 large, medium, and small patterns similar to those in Comparative Example 2 were arranged in the other unit.

[0076] 4(a) was formed as the resistive layer, an electromagnetic wave absorbing member of Example 2 was produced in the same manner as in Comparative Example 1. The size of each unit was 12 mm x 12 mm, and in one unit, 7 x 7 large, medium, and small patterns similar to those in Comparative Example 1 were arranged, and in the other unit, 9 x 9 large, medium, and small patterns similar to those in Comparative Example 2 were arranged.

[0077] 4(b) was formed as the resistive layer, an electromagnetic wave absorbing member of Example 3 was produced in the same manner as Comparative Example 1. The size of each unit was 7 mm x 7 mm, and in one unit, 4 x 4 large, medium, and small patterns similar to those in Comparative Example 1 were arranged, and in the other unit, 5 x 5 large, medium, and small patterns similar to those in Comparative Example 2 were arranged.

[0078] 5(a) was formed as the resistive layer, an electromagnetic wave absorbing member of Example 4 was produced in the same manner as Comparative Example 1. Each unit was a strip with a width of 32 mm, and 15 rows of large, medium, and small patterns similar to those in Comparative Example 1 were arranged in one unit, and 20 rows of large, medium, and small patterns similar to those in Comparative Example 2 were arranged in the other unit.

[0079] 5(b) was formed as the resistive layer, an electromagnetic wave absorbing member of Example 5 was produced in the same manner as Comparative Example 1. Each unit was a strip with a width of 12 mm, and seven rows of large, medium, and small patterns similar to those in Comparative Example 1 were arranged in one unit, and seven rows of large, medium, and small patterns similar to those in Comparative Example 2 were arranged in the other unit.

[0080] 5(c) was formed as the resistive layer, an electromagnetic wave absorbing member of Example 6 was produced in the same manner as Comparative Example 1. Each unit was a strip with a width of 7 mm, and one unit had four rows of large, medium, and small patterns similar to Comparative Example 1 arranged therein, and the other unit had four rows of large, medium, and small patterns similar to Comparative Example 2 arranged therein.

[0081] [Evaluation] The electromagnetic wave absorbing members of Comparative Examples 1 and 2 and Examples 1 to 6 were evaluated as follows. The results are shown in Table 1.

[0082] [Electromagnetic Wave Absorption] The S11 values ​​(reflection coefficients) of the electromagnetic wave absorbing members of Comparative Examples 1 and 2 and Examples 1 to 6 at 76 to 81 GHz were obtained using a network analyzer by the free space method to evaluate the electromagnetic wave absorption properties of the electromagnetic wave absorbing members.

[0083]

[0084] The results shown in Table 1 show that the electromagnetic wave absorbing members of Examples 1 to 6 have excellent electromagnetic wave absorbing properties. On the other hand, the electromagnetic wave absorbing members of Comparative Examples 1 and 2 have poor electromagnetic wave absorbing properties.

[0085] The electromagnetic wave absorbing member of the present invention can be suitably used as an electromagnetic wave absorbing member for transportation equipment such as automobiles.

[0086] REFERENCE SIGNS LIST 10 Electromagnetic wave absorbing member 20 Resistive layer 20A, 20B Region 21 Base material 22 Conductive pattern 30 Spacer layer 40 Reflective layer 51 First conductive pattern 52 Second conductive pattern 53 Third conductive pattern

Claims

1. An electromagnetic wave absorbing material having a resistive layer, a spacer layer, and a reflective layer, wherein the resistive layer, the spacer layer, and the reflective layer are laminated in this order, the resistive layer has a plurality of regions which are equal in area when viewed in a plane of the electromagnetic wave absorbing material and have different electromagnetic wave absorption characteristics, each of the regions has two or more types of conductor patterns formed parallel to each other on the spacer layer, each of the two or more types of conductor patterns being composed of a plurality of units arranged in one direction at regular intervals, and the regions differ from adjacent regions in at least one of the shape of the units which make up the conductor pattern, the size of the units, and the arrangement interval of the units.

2. The electromagnetic wave absorbing member according to claim 1, wherein said regions are provided repeatedly at regular intervals.

Citation Information

Patent Citations

  • Fiber body manufacturing method

    JP2023053539A

  • Radio wave absorber

    JP4461974B2

  • Frequency Selective Surfaces and Wave Absorbers

    JP6861907B1

  • Electromagnetic wave absorber

    JP2005317945A

  • Electromagnetic wave absorber

    JP2020191398A