Steel plate
A steel plate with a tailored chemical composition and cementite density improves drawing workability and suppresses burr formation, addressing the challenges of existing steel plates in the can manufacturing process.
Patent Information
- Application Number
- PCT/JP2023/044529
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2023-12-12
- Publication Date
- 2024-10-03
AI Technical Summary
Steel plates used for drawing cans often suffer from poor drawing workability and burr formation during trimming, which can compromise the quality of battery cans.
A steel plate with a specific chemical composition (C: 0.010-0.100%, Si: 0.350% or less, Mn: 1.00% or less, P: 0.070% or less, S: 0.025% or less, sol. Al: 0.005-0.100%, N: 0.0060% or less, and B: 0.50 to 2.50 times the N content) and a controlled number density of cementite (1150 to 7000 pieces/mm²) is developed to enhance drawing workability and suppress burr formation.
The steel plate achieves excellent drawing workability and effectively reduces burr occurrence during trimming, maintaining the integrity of the can manufacturing process.
Smart Images

Figure JP2023044529_03102024_PF_FP_ABST
Abstract
Description
steel plate
[0001] The present disclosure relates to a steel sheet, and more particularly to a steel sheet suitable for use in drawn cans. In this specification, the term "drawn can" refers to a can formed by drawing and a can formed by drawing and ironing (DI) processing.
[0002] Battery cans, such as those for secondary batteries, are manufactured by drawing or DI processing steel sheets or plated steel sheets. Therefore, the steel sheets used as the raw materials for such drawn cans are required to have excellent drawing workability.
[0003] WO 2016 / 060248 (Patent Document 1) proposes a steel sheet with excellent drawability. The steel sheet for drawn cans disclosed in Patent Document 1 has a chemical composition, in mass%, of C: over 0.150 to 0.260%, sol. Al: 0.005 to 0.100%, B: 0.0005 to 0.02%, Si: 0.50% or less, Mn: 0.70% or less, P: 0.070% or less, S: 0.05% or less, N: 0.0080% or less, Nb: 0.003% or less, and Ti: 0.003% or less, with the balance being Fe and impurities. Furthermore, the boron content and nitrogen content in the chemical composition of this steel sheet satisfy, in mass%, 0.4≦B / N≦2.5. This steel sheet has a microstructure containing ferrite with an average grain size of 2.7 to 4.0 μm and granular cementite. A tensile test is conducted after aging the steel sheet at 100°C for 1 hour, with the tensile direction parallel to the rolling direction. The yield strength, measured in MPa, is YP, the total elongation is EL, the yield point elongation is YP-EL, and the yield ratio is YR. The steel sheet of Patent Document 1 has a higher C content than conventional steel sheets and also contains B. This results in excellent drawing formability.
[0004] International Publication No. 2016 / 060248
[0005] When a drawn can product is formed by drawing a steel sheet, a flange portion is formed on the drawn can after the drawing process. The flange portion is an unnecessary part of the drawn can product. Therefore, after the drawing process, the flange portion is removed by trimming. During this trimming process, burrs may occur on the cut edge of the drawn can after the flange portion is cut. When a battery is manufactured using a drawn can with such burrs, the burrs may penetrate into the drawn can. Such burrs degrade battery performance. Therefore, it is preferable to suppress the generation of burrs during trimming after drawing. Patent Document 1 does not consider means for suppressing the generation of burrs during trimming.
[0006] An object of the present disclosure is to provide a steel sheet that can obtain excellent drawing formability and can suppress the generation of burrs during trimming.
[0007] The steel sheet of the present disclosure contains, in mass%, C: 0.010 to 0.100%, Si: 0.350% or less, Mn: 1.00% or less, P: 0.070% or less, S: 0.025% or less, sol. Al: 0.005 to 0.100%, N: 0.0060% or less, and B: 0.50 to 2.50 times the N content, with the balance consisting of Fe and impurities, and has a surface roughness of 0.30 μm. 2 The number density ND of cementite having an area of 1150 pieces / mm 2 More than 7000 pieces / mm 2 is less than.
[0008] The steel sheet according to this embodiment has excellent drawing formability and can suppress the generation of burrs during trimming.
[0009] Fig. 1A is a perspective view of a cylindrical can obtained by cylindrical deep drawing in a drawing workability evaluation test in the Examples. Fig. 1B is a side view of the cylindrical can of Fig. 1A. Fig. 2 is a cross-sectional photograph of the end of the cut surface after trimming in a trimming workability evaluation test in the Examples. Fig. 3 is a cross-sectional photograph of the end of the cut surface after trimming in a trimming workability evaluation test in the Examples, which is different from Fig. 2.
[0010] The present inventors first studied the chemical composition of a steel sheet suitable for can drawing applications, and as a result, they concluded that a chemical composition containing, by mass%, C: 0.010 to 0.100%, Si: 0.350% or less, Mn: 1.00% or less, P: 0.070% or less, S: 0.025% or less, sol. Al: 0.005 to 0.100%, and N: 0.0060% or less, with the balance being Fe and impurities, would be appropriate.
[0011] The present inventors further investigated means for obtaining excellent drawing formability and suppressing the generation of burrs during trimming. As proposed in Patent Document 1, boron (B) randomizes the texture of the steel sheet, bringing the r value (Lankford value), which is the plastic strain ratio, closer to 1. This improves the earring properties and improves the drawing formability. Furthermore, improved earring properties allow for uniform flange formation during drawing. Therefore, it is believed that burrs are less likely to occur during trimming.
[0012] Therefore, the inventors thought that burrs during trimming could be suppressed by further adding B to the above chemical composition, and by mass percent, containing C: 0.010 to 0.100%, Si: 0.350% or less, Mn: 1.00% or less, P: 0.070% or less, S: 0.025% or less, sol. Al: 0.005 to 0.100%, N: 0.0060% or less, and B: 0.50 to 2.50 times the N content, with the balance being Fe and impurities.
[0013] However, even with steel sheets having the above chemical composition, it was not possible to sufficiently suppress the generation of burrs during trimming. Therefore, the present inventors conducted further studies. As a result, it was found that if the number density of coarse cementite in a steel sheet is high, the generation of burrs during trimming is suppressed. Therefore, the present inventors conducted further studies on the relationship between the size and number density of cementite and the frequency of burr generation. As a result, in steel sheets having the above chemical composition, it was found that the generation of burrs during trimming is suppressed when the number density of coarse cementite is high. 2 The number density ND of cementite having an area of 1150 pieces / mm 2It has been found that if the above conditions are met, the generation of burrs can be sufficiently suppressed when trimming is performed.
[0014] On the other hand, 0.30 μm 2 It has been found that if the number density ND of cementite having an area of 0.30 μm or more is too high, the drawing workability is reduced. 2 The relationship between the number density ND of cementite having an area of 0.30 μm or more and drawing workability was further investigated. 2 The number density ND of cementite having an area of 7000 pieces / mm 2 It has been found that excellent drawing workability can be obtained if the thickness is less than 1000 MPa.
[0015] The gist of the steel sheet of this embodiment, which has been completed based on the above technical concept, is as follows.
[0016] The steel sheet of the first configuration contains, in mass%, C: 0.010 to 0.100%, Si: 0.350% or less, Mn: 1.00% or less, P: 0.070% or less, S: 0.025% or less, sol. Al: 0.005 to 0.100%, N: 0.0060% or less, and B: 0.50 to 2.50 times the N content, with the balance consisting of Fe and impurities, and has a thickness of 0.30 μm 2 The number density ND of cementite having an area of 1150 pieces / mm 2 More than 7000 pieces / mm 2 is less than.
[0017] The steel sheet of the second configuration is the steel sheet of the first configuration, further comprising one layer selected from the group consisting of a Ni plating layer, a Ni diffusion plating layer, a Ni alloy plating layer, and a Ni alloy diffusion plating layer formed on the surface of the steel sheet.
[0018] The steel sheet according to this embodiment will be described in detail below. Unless otherwise specified, "%" for elements means mass %.
[0019] [Features of Steel Sheet of This Embodiment] The steel sheet of this embodiment satisfies the following features 1 and 2. (Feature 1) The chemical composition contains, in mass%, C: 0.010 to 0.100%, Si: 0.350% or less, Mn: 1.00% or less, P: 0.070% or less, S: 0.025% or less, sol. Al: 0.005 to 0.100%, N: 0.0060% or less, and B: 0.50 to 2.50 times the N content, with the balance consisting of Fe and impurities. (Feature 2) 0.30 μm 2 The number density ND of cementite having an area of 1150 pieces / mm 2 More than 7000 pieces / mm 2 Below, feature 1 and feature 2 will be explained.
[0020] [(Feature 1) Chemical Composition] The chemical composition of the steel sheet according to this embodiment contains the following elements.
[0021] C: 0.010 to 0.100% Carbon (C) increases the strength of steel sheet. If the C content is less than 0.010%, the above effect cannot be fully achieved. On the other hand, if the C content exceeds 0.100%, excessive coarse carbides are formed. In this case, the machinability of the steel sheet decreases. Therefore, the C content is 0.010 to 0.100%. The preferred lower limit of the C content is 0.015%, more preferably 0.020%, and even more preferably 0.025%. The preferred upper limit of the C content is 0.090%, more preferably 0.080%, and even more preferably 0.070%. The preferred range of the C content is, for example, 0.015 to 0.090%, more preferably 0.020 to 0.080%, and even more preferably 0.025 to 0.070%.
[0022] Si: 0.350% or less Silicon (Si) is an unavoidable impurity. In other words, the Si content is greater than 0%. Si reduces the plating adhesion of steel sheets. Si also reduces the paint adhesion of steel sheets after can manufacturing. Therefore, the Si content is 0.350% or less. The lower the Si content, the more preferable it is. However, excessive reduction in the Si content increases manufacturing costs. Therefore, taking industrial productivity into consideration, the preferred lower limit of the Si content is 0.001%, more preferably 0.002%, and even more preferably 0.005%. The preferred upper limit of the Si content is 0.250%, more preferably 0.100%, even more preferably 0.050%, and even more preferably 0.030%. The Si content is preferably in the range of, for example, 0.001 to 0.250%, more preferably 0.002 to 0.100%, even more preferably 0.005 to 0.050%, and still more preferably 0.005 to 0.030%.
[0023] Mn: 1.00% or less Manganese (Mn) is an unavoidable impurity. In other words, the Mn content is greater than 0%. Mn excessively increases the number density of coarse cementite. This hardens the steel sheet. As a result, the drawability of the steel sheet deteriorates. Therefore, the Mn content is 1.00% or less. The lower the Mn content, the more preferable it is. However, excessive reduction in the Mn content increases manufacturing costs. Therefore, considering industrial productivity, the preferred lower limit of the Mn content is 0.01%, more preferably 0.02%, and even more preferably 0.05%. The preferred upper limit of the Mn content is 0.90%, more preferably 0.80%, and even more preferably 0.70%. The preferred range of the Mn content is, for example, 0.01 to 0.90%, more preferably 0.02 to 0.80%, and even more preferably 0.05 to 0.70%.
[0024] P: 0.070% or less Phosphorus (P) is an unavoidable impurity. In other words, the P content is greater than 0%. P reduces the drawability of steel sheets. Therefore, the P content is 0.070% or less. The lower the P content, the better. However, excessive reduction in the P content increases manufacturing costs. Therefore, taking industrial productivity into consideration, the preferred lower limit of the P content is 0.001%, more preferably 0.002%, and even more preferably 0.005%. The preferred upper limit of the P content is 0.060%, more preferably 0.050%, and even more preferably 0.040%. The preferred range of the P content is, for example, 0.001 to 0.060%, more preferably 0.002 to 0.050%, and even more preferably 0.005 to 0.040%.
[0025] S: 0.025% or less Sulfur (S) is an unavoidable impurity. In other words, the S content is greater than 0%. S reduces the hot workability of steel sheets and causes cracks in the steel sheets during hot working. Therefore, the S content is 0.025% or less. The lower the S content, the better. However, excessive reduction in the S content increases manufacturing costs. Therefore, taking industrial productivity into consideration, the preferred lower limit of the S content is 0.001%, more preferably 0.002%, and even more preferably 0.005%. The preferred upper limit of the S content is 0.020%, more preferably 0.015%, and even more preferably 0.012%. The preferred range of the S content is, for example, 0.001 to 0.020%, more preferably 0.002 to 0.015%, and even more preferably 0.005 to 0.012%.
[0026] Sol. Al: 0.005 to 0.100% Aluminum (Al) deoxidizes steel. If the sol. Al content is less than 0.005%, the above effect cannot be sufficiently obtained. On the other hand, if the sol. Al content exceeds 0.100%, coarse nitrides and / or oxides are formed, reducing the drawability of the steel sheet. Therefore, the sol. Al content is 0.005 to 0.100%. The preferred lower limit of the sol. Al content is 0.010%, more preferably 0.015%, and even more preferably 0.020%. The preferred upper limit of the sol. Al content is 0.090%, more preferably 0.080%, and even more preferably 0.070%. The Al content is preferably in the range of 0.010 to 0.090%, more preferably 0.015 to 0.080%, and even more preferably 0.020 to 0.070%. Note that sol. Al means "acid-soluble Al".
[0027] N: 0.0060% or less Nitrogen (N) is an unavoidable impurity. In other words, the N content is greater than 0%. N age-hardens steel sheets and reduces draw formability. N also generates stretcher strain. Therefore, the N content is 0.0060% or less. The N content is preferably as low as possible. However, excessive reduction of the N content increases manufacturing costs. Therefore, considering industrial productivity, the preferred lower limit of the N content is 0.0001%, more preferably 0.0005%, and even more preferably 0.0010%. The preferred upper limit of the N content is 0.0055%, more preferably 0.0050%, and even more preferably 0.0045%. The preferred range of the N content is, for example, 0.0001 to 0.0055%, more preferably 0.0005 to 0.0050%, and even more preferably 0.0010 to 0.0045%.
[0028] B: 0.50 to 2.50 times the N content Boron (B) bonds with N to form BN, reducing the amount of solute N in the steel sheet. This suppresses age hardening due to solute N. B also randomizes the texture of the steel sheet, bringing the r-value (Lankford value), which is the compositional strain ratio, closer to 1 and improving earring properties. This improves drawability. Furthermore, it suppresses the generation of burrs during trimming. If the B content is less than 0.50 times the N content, the above effects cannot be fully achieved. On the other hand, if the B content exceeds 2.50 times the N content, the amount of solute B in the steel sheet becomes excessive. In this case, the steel sheet becomes hard and the earring properties deteriorate. B also suppresses the coarsening of cementite. Therefore, it is not possible to fully suppress the generation of burrs during trimming. Therefore, the B content is 0.50 to 2.50 times the N content. The preferred lower limit of the B content is 0.55 times the N content, more preferably 0.60 times the N content, and even more preferably 0.65 times the N content. The preferred upper limit of the B content is 2.45 times the N content, more preferably 2.40 times the N content, and even more preferably 2.35 times the N content. The preferred range of the B content is, for example, 0.55 to 2.45 times the N content, more preferably 0.60 to 2.40 times the N content, and even more preferably 0.65 to 2.35 times the N content.
[0029] The balance of the chemical composition of the steel sheet of this embodiment is composed of Fe and impurities. Here, the impurities refer to substances that are mixed in from raw materials such as ore and scrap, or the manufacturing environment, during industrial production of the steel sheet, and are acceptable within a range that does not adversely affect the steel sheet of this embodiment.
[0030] [Impurities] The chemical composition of the steel sheet of this embodiment may further contain, in place of a portion of Fe, one or more elements selected from the group consisting of Nb: 0-0.003%, Ti: 0-0.003%, Cu: 0-0.50%, Ni: 0-0.50%, Cr: 0-0.30%, and Sn: 0-0.05%. Any of these elements may be 0%. All of these elements are so-called tramp elements that may be contained in scrap, which is the raw material, and are all impurities.
[0031] [Method for Measuring Chemical Composition of Steel Sheet] The chemical composition of the steel sheet of this embodiment can be measured by a known elemental analysis method in accordance with JIS G0321:2017. Specifically, chips are collected from the steel sheet using a cutting tool such as a drill. The collected chips are dissolved in acid to obtain a solution. ICP-MS (Inductively Coupled Plasma Mass Spectrometry) is performed on the solution to perform elemental analysis of the chemical composition. The C content and S content are determined by a known high-frequency combustion method (combustion-infrared absorption method). The N content is determined using a known inert gas fusion-thermal conductivity method.
[0032] The content of each element is determined by rounding off the measured value to the nearest significant digit based on the significant digits specified in this embodiment, to obtain the value to the least significant digit of the content of each element specified in this embodiment. For example, the C content of the steel material in this embodiment is specified as a value to three decimal places. Therefore, the C content is determined as a value to three decimal places obtained by rounding off the fourth decimal place of the measured value. Similarly, the content of other elements other than the C content of the steel plate in this embodiment is determined as the value obtained by rounding off the measured value to the least significant digit specified in this embodiment. Note that rounding means rounding down if the fraction is less than 5, and rounding up if the fraction is 5 or more.
[0033] [Number density ND of coarse cementite] In the steel sheet of this embodiment, the number density ND of coarse cementite is further set to 0.30 μm. 2 The number density ND of cementite having an area of 1150 pieces / mm 2 More than 7000 pieces / mm 2 In the following description, the thickness is less than 0.30 μm. 2 Cementite having an area of 4.00 μm or more is also called "coarse cementite." Note that there is no particular upper limit on the area of the coarse cementite. From the viewpoint of crystal growth, the area of the coarse cementite is, for example, 4.00 μm 2 The following may also be used.
[0034] Coarse cementite improves the detachability of chips during trimming. Therefore, it suppresses the generation of burrs during trimming. In order to sufficiently suppress the generation of burrs, it is effective to increase the number density of coarse cementite. In a steel plate that satisfies Feature 1, the number density ND of coarse cementite is 1150 pieces / mm 2 If this is the case, the generation of burrs during trimming can be sufficiently suppressed.
[0035] On the other hand, if the number density ND of the coarse cementite is too high, the drawing workability will decrease. 2 More than 7000 pieces / mm 2 is less than.
[0036] The preferred lower limit of the number density ND of coarse cementite is 1400 pieces / mm 2 and more preferably 1500 pieces / mm 2 and more preferably 1600 pieces / mm 2 The preferred upper limit of the number density ND of the coarse cementite is 6100 pieces / mm 2 and more preferably 5500 pieces / mm 2 The preferred range of the number density ND of the coarse cementite is, for example, 1400 to 6100 pieces / mm 2 and more preferably 1500 to 5500 pieces / mm 2 and more preferably 1600 to 5500 pieces / mm 2 is.
[0037] [Method for Measuring Number Density ND of Coarse Cementite] The number density ND of coarse cementite can be determined by the following method. A sample is collected from an arbitrary location on a steel sheet. A cross section of the sample surface perpendicular to the rolling direction of the steel sheet is defined as the observation surface. The observation surface of the sample is polished, and then etched for 20 seconds using a 6% picral etchant (a etchant containing 6 g of picric acid and 94 mL of ethanol). Using a scanning electron microscope (SEM), five arbitrary observation regions (61 μm × 43 μm) on the etched observation surface are observed at a magnification of 2000 times, and particles (precipitates and inclusions) in the observation regions are photographed to generate photographic images that are secondary electron images.
[0038] Based on the contrast of the photographic image, cementite in the five observation regions is identified. The area of each identified cementite is calculated. The identification of cementite based on contrast and the area of each cementite can be calculated by well-known image processing. An example of image processing software is LUZEX AP MQ3104.0, a product name of Nireco Corporation.
[0039] 0.30 μm identified in five observation fields 2 Based on the total number of coarse cementite particles having an area of at least 100 mm and the total area of the five observation fields, the number density ND (pieces / mm 2 ) is required.
[0040] [Effects of the Steel Sheet of the Present Embodiment] The steel sheet of the present embodiment satisfies Features 1 and 2. Therefore, the steel sheet of the present embodiment has excellent drawing formability and can sufficiently suppress the generation of burrs during trimming.
[0041] [Preferable thickness of the cold-rolled steel sheet of this embodiment] The thickness of the cold-rolled steel sheet of this embodiment is not particularly limited. The thickness of the cold-rolled steel sheet of this embodiment is, for example, 0.15 to 1.00 mm.
[0042] [Microstructure of Steel Sheet of the Present Embodiment] The microstructure of the steel sheet of the present embodiment is mainly composed of ferrite and cementite. Specifically, in the microstructure of the steel sheet of the present embodiment, the total area ratio of ferrite and cementite is 95.0% or more. In the microstructure, structures other than ferrite and cementite are composed of one or more selected from the group consisting of pearlite, hard structures (martensite and bainite), retained austenite, precipitates other than cementite, and inclusions. In the microstructure, the total area ratio of structures other than ferrite and cementite is 5.0% or less.
[0043] [Method for Observing the Microstructure of Steel Sheet] The total area ratio of ferrite and cementite in the steel sheet of this embodiment is determined by the following method. A sample is taken from the center position of the steel sheet width. A cross section of the sample surface perpendicular to the rolling direction of the steel sheet is defined as the observation surface. The observation surface of the sample is mirror-polished. The mirror-polished observation surface is etched using 3% nitric acid alcohol (nital etchant). Five random observation fields (61 μm × 43 μm) of the etched observation surface are observed using a SEM at 2000x magnification.
[0044] In the observation field, ferrite and cementite can be easily distinguished from other structures due to their contrast. Ferrite is observed as a white area. Cementite is observed as grains that are less bright than ferrite. The area ratios (%) of ferrite and cementite are calculated based on the total area of ferrite and cementite in the five observation fields and the total area of the five observation fields.
[0045] [Regarding the Ni-Based Plating Layer] The steel sheet of this embodiment may have a Ni-based plating layer formed on its surface. The Ni-based plating layer may be, for example, one selected from the group consisting of a Ni plating layer, a Ni diffusion plating layer, a Ni alloy plating layer, and a Ni alloy diffusion plating layer. The Ni plating layer is a plating layer made of Ni. In the Ni diffusion plating layer, Fe migrated from the steel sheet into the plating layer is diffused into part or all of the Ni plating layer. That is, the Ni diffusion plating layer is a plating layer containing Ni and Fe. In the Ni alloy plating layer, part or all of the Ni plating layer is replaced with an alloy layer of Ni and a well-known metal element other than Fe. The Ni alloy diffusion plating layer is either a Ni alloy plating layer or a layer in which part of the Ni plating layer is replaced with a layer made of a well-known metal element other than Fe, and Fe is diffused into part or all of the Ni plating layer. Note that the steel sheet of this embodiment does not necessarily have a Ni-based plating layer formed on its surface.
[0046] [Method for manufacturing steel sheet according to this embodiment] An example of a method for manufacturing a steel sheet according to this embodiment will be described. A steel sheet satisfying Features 1 and 2 may be manufactured by a manufacturing method other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of the method for manufacturing a steel sheet according to this embodiment.
[0047] An example of the method for manufacturing a steel sheet according to the present embodiment includes the following steps: (Step 1) Material preparation step (Step 2) Hot rolling step (Step 3) Cold rolling step (Step 4) Continuous annealing step (Step 5) BAF annealing step Steps 1 to 5 will be described below.
[0048] [(Step 1) Material Preparation Step] In the material preparation step, molten steel satisfying Feature 1 is produced. The produced molten steel is used to produce a material (slab) by a casting method. For example, the molten steel is used to produce a slab by a well-known continuous casting method. The molten steel may also be used to produce an ingot by an ingot casting method. Through the above production steps, a slab or an ingot, which is the material for the steel plate, is prepared.
[0049] [(Step 2) Hot Rolling Step] In the hot rolling step, a slab or an ingot is hot rolled to produce a hot-rolled steel sheet. The hot rolling step includes a rough rolling step in which the slab or the ingot is rough rolled to produce a rough bar (intermediate steel sheet), and a finish rolling step in which the rough bar is finish rolled to produce a steel sheet.
[0050] In the rough rolling process, a material (slab or ingot) is heated. The heated material is rolled using a rough rolling mill to produce a rough bar. The heating temperature of the material in the rough rolling process is, for example, 1000 to 1300°C.
[0051] In the finish rolling process, the rough bar produced in the rough rolling process is further rolled (finish rolling) using a finish rolling mill to produce a hot-rolled steel sheet. In the finish rolling process, the finish rolling temperature is, for example, 800 to 1000°C, and the coiling temperature is, for example, 500 to 720°C.
[0052] [(Step 3) Cold Rolling Step] In the cold rolling step, the hot-rolled steel sheet is cold-rolled to produce a cold-rolled steel sheet. In the cold rolling step, for example, the cumulative reduction is set to 80% or more. The upper limit of the cumulative reduction is not particularly limited. However, in consideration of industrial productivity, the preferable upper limit of the cumulative reduction is 90%.
[0053] [(Step 4) Continuous Annealing Step] In the continuous annealing step, continuous annealing is performed using a continuous annealing line on the cold-rolled steel sheet after the cold rolling step or the cold-rolled steel sheet on which a Ni-based plating layer has been formed after the plating step described below. Continuous annealing is performed under the following conditions: (Condition 1) Annealing temperature T0: 710 to 830°C (Condition 2) Holding time t0 at annealing temperature T0: 6.5 to 32.0 seconds
[0054] When the annealing temperature T0 is 710 to 830°C and the holding time t0 is 6.5 to 32.0 seconds, recrystallization is promoted in the cold-rolled steel sheet, and cementite is generated. As a result, the total area ratio of ferrite and cementite in the microstructure of the produced steel sheet is 95.0% or more. Furthermore, by generating a certain amount of cementite in the continuous annealing process, the subsequent BAF annealing process is carried out, and the produced steel sheet has a 0.30 μm 2 The number density ND of cementite having an area of 1150 pieces / mm 2 More than 7000 pieces / mm 2 It will be less than.
[0055] If the BAF annealing step described below is performed without performing the continuous annealing step, the amount of cementite generated in the cold-rolled steel sheet before the BAF annealing step is insufficient. Therefore, even if the BAF annealing step is performed, the number density ND of coarse cementite is insufficient. Therefore, in the manufacturing method of this embodiment, the continuous annealing step is performed before performing the BAF annealing step. In the continuous annealing step, the cold-rolled steel sheet after continuous annealing is coiled and cooled to 100°C or less.
[0056] [(Step 5) BAF Annealing Step] The cold-rolled steel sheet after the continuous annealing step is subjected to BAF (Box Annealing Furnace) annealing at 100°C or less. BAF annealing is also called box annealing (or batch annealing). BAF annealing is performed under the following conditions: (Condition 3) Heating rate HR1: 0.90 to 4.80°C / min (Condition 4) Annealing temperature T1: 440 to 460°C (Condition 5) Holding time t1: 460 to 490 minutes (Condition 6) Cooling rate CR1: 0.30°C / min or less Conditions 3 to 6 will be explained below.
[0057] [Condition 3: Heating Rate HR1] In the heating process in the BAF annealing step, cementite formation sites are secured. If the heating rate HR1 is too fast, the ferrite structure in the steel sheet becomes coarse and the number of cementite formation sites decreases. If the heating rate HR is 4.80°C / min or less, recrystallization progresses in the heating process, and a sufficient number of cementite formation sites can be secured. Therefore, in the manufactured steel sheet,2 The number density ND of cementite having an area of 1150 pieces / mm 2 More than 7000 pieces / mm 2 The lower limit of the heating rate HR1 is not particularly limited. However, if the heating rate HR1 is too slow, productivity decreases. Therefore, the preferred lower limit of the heating rate HR1 is 0.90°C / min.
[0058] [(Conditions 4 and 5) Annealing Temperature T1 and Holding Time t1] By setting the annealing temperature T1 to 440 to 460°C and the holding time t1 to 460 to 490 minutes, cementite with a sufficient number density is generated. If the annealing temperature T1 is less than 440°C or the holding time t1 is less than 460 minutes, solute C remains in the steel sheet. In this case, the number density ND of coarse cementite is not sufficiently obtained in the manufactured steel sheet. On the other hand, if the annealing temperature T1 exceeds 460°C or the holding time t1 exceeds 490 minutes, the ferrite structure becomes coarse. In this case, the number of cementite formation sites decreases. As a result, the number density ND of coarse cementite is not sufficiently obtained.
[0059] [(Condition 6) Cooling rate CR1] During the cooling process in the BAF annealing step, the produced cementite grows coarsely. If the cooling rate CR1 exceeds 0.30°C / min, the cooling rate is too fast. In this case, cementite does not grow sufficiently. Therefore, the number density ND of coarse cementite is not sufficiently obtained in the manufactured steel sheet. Therefore, the cooling rate CR1 is set to 0.30°C / min or less. There is no particular restriction on the lower limit of the cooling rate CR1. However, if the cooling rate CR1 is too slow, productivity decreases. Therefore, the preferable lower limit of the cooling rate CR1 is 0.10°C / min.
[0060] The cold-rolled steel sheet after BAF annealing is cooled to 100° C. or less. Through the above manufacturing process, the steel sheet of this embodiment that satisfies Features 1 and 2 is manufactured.
[0061] [Optional Manufacturing Steps] The method for manufacturing a steel sheet according to this embodiment may further include a temper rolling step and / or a galvanizing step. The temper rolling step and the galvanizing step will be described below.
[0062] [Temper Rolling Process] The temper rolling process is an optional process and does not necessarily have to be performed. If performed, in the temper rolling process, the annealed steel sheet after the BAF annealing process is subjected to temper rolling (skin pass rolling) to produce a steel sheet. The cumulative reduction rate in temper rolling is, for example, 0.5 to 5.0%. In the temper rolling process, the surface roughness of the steel sheet and the hardness of the steel sheet are adjusted.
[0063] [Plating Step] The plating step is an optional step and may not be performed. If performed, the plating step may be performed after the BAF annealing step or after the temper rolling step. The plating step may be performed after the cold rolling step and before the continuous annealing step.
[0064] In the plating step, a Ni-based plating layer is formed on the surface of the steel sheet. A well-known method is used to form the plating layer. For example, the cold-rolled steel sheet is immersed in a plating bath for forming the Ni-based plating layer, and electrolytic plating or electroless plating is performed. Through the above steps, a Ni-based plating layer, i.e., a Ni plating layer or a Ni alloy plating layer, is formed on the cold-rolled steel sheet.
[0065] When the plating step is carried out after the BAF annealing step or the temper rolling step, the produced steel sheet has a Ni plating layer or a Ni alloy plating layer.
[0066] On the other hand, when the plating step is performed after the cold rolling step and before the continuous annealing step, Fe of the steel sheet diffuses into the Ni-plated layer or Ni alloy-plated layer formed on the cold-rolled steel sheet during the continuous annealing step, and therefore, in this case, the produced steel sheet has a Ni diffusion-plated layer or Ni alloy diffusion-plated layer.
[0067] The effects of one aspect of the steel sheet of this embodiment will be described more specifically below with reference to an example.
[0068] Cold-rolled steel sheets having the chemical compositions shown in Table 1 were produced.
[0069]
[0070] Specifically, molten steel was continuously cast to produce a slab. The slab was subjected to a hot rolling process (rough rolling process and finish rolling process). The slab was heated at 1100 to 1250°C. The heated slab was rolled in a rough rolling mill to produce a rough bar. The rough bar was further rolled using a finish rolling mill to produce a hot-rolled steel sheet. The finish rolling temperature was 850 to 940°C, and the coiling temperature was 500 to 720°C.
[0071] The hot-rolled steel sheet was subjected to a cold rolling process to produce a cold-rolled steel sheet. The cumulative rolling reduction was 80 to 90%. The cold-rolled steel sheet was subjected to a continuous annealing process. The annealing temperature T0 (°C) and holding time t0 (seconds) in the continuous annealing process were as shown in Table 2. The cold-rolled steel sheet after continuous annealing was coiled and cooled to room temperature (25°C).
[0072]
[0073] The cooled steel sheets were subjected to a BAF annealing step. The heating rate HR1 (°C / min), annealing temperature T1 (°C), holding time t1 (min) at annealing temperature T1, and cooling rate CR1 (°C / min) in the BAF annealing were as shown in Table 2. The BAF annealed steel sheets were cooled to room temperature.
[0074] The cooled steel plates were subjected to a temper rolling process. The cumulative reduction in temper rolling was set to 0.5 to 5.0%. Steel plates with each test number were manufactured by the above manufacturing process. The steel plates had a thickness of 0.30 mm.
[0075] [Evaluation Tests] The following evaluation tests were carried out on the steel sheets with each test number: (Test 1) Coarse cementite number density ND measurement test (Test 2) Microstructure observation test (Test 3) Drawing workability evaluation test (Test 4) Trimming work test Tests 1 to 4 will be described below.
[0076] [(Test 1) Measurement Test of Number Density ND of Coarse Cementite] In accordance with the method described in the above [Method for Measuring Number Density ND of Coarse Cementite], the number density ND (number / mm 2 The number density ND (pieces / mm 2 ) are shown in Table 3.
[0077]
[0078] [(Test 2) Microstructure Observation Test] The total area ratio (%) of ferrite and cementite in the steel plate of each test number was determined according to the method described in the above-mentioned [Method for Observing the Microstructure of Steel Plate]. The obtained total area ratios (%) are shown in Table 3. In all test numbers, the total area ratio of ferrite and cementite was 95.0% or more.
[0079] [(Test 3) Drawing Workability Evaluation Test] Disc-shaped test specimens were collected from the steel plates of each test number. The disc-shaped test specimens had a thickness of 0.30 mm and a diameter of 36.00 mm. Using a punch with a diameter of 21.55 mm, cylindrical deep drawing was performed on the disc-shaped test specimens to produce the cylindrical can 1 shown in FIG. 1A . FIG. 1B is a side view of the cylindrical can 1 shown in FIG. 1A . Referring to FIG. 1B , the maximum value Hmax of the crest height (earring crest height) of the can side wall of the cylindrical can 1 and the minimum value Hmin of the can side wall (valley height) of the cylindrical can 1 were determined for the obtained cylindrical can 1. Furthermore, the can side wall height of the cylindrical can 1 was measured over 360° at 0.8° intervals, and the average value Have was calculated. The obtained Hmax, Hmin, and Have were used to calculate the earring ratio according to the following formula: Earring rate = (Hmax - Hmin) / Have
[0080] When the earring ratio obtained was 3.0% or less, it was determined that excellent drawing workability was obtained (shown as "EX (Excellent)" in the "Drawing workability" column in Table 3). On the other hand, when the earring ratio obtained was more than 3.0%, it was determined that sufficient drawing workability was not obtained (shown as "B (Bad)" in the "Drawing workability" column in Table 3).
[0081] [(Test 4) Trimming Test] A trimming test was performed on the steel plates of each test number using the following method, and the presence or absence of burrs after trimming was evaluated. Specifically, a disc-shaped test specimen was taken from each steel plate of each test number. The disc-shaped test specimen had a diameter of 36.00 mm and a plate thickness of 0.30 mm. The disc-shaped test specimen was subjected to flanged cylindrical drawing to produce a flanged cylinder with a flange width of 5.00 mm. The drawing ratio was 2.0. The obtained flanged cylinder was subjected to trimming to trim the entire flange portion. A tool blade was used for trimming. The trimming allowance was 5.00 mm. During trimming, a plate holding force of 5% of the maximum shear load was applied.
[0082] The cylinder with the trimmed flange was cut parallel to the axial direction. The edge of the cut surface formed by the trimming process in the cross section was observed with a scanning electron microscope (SEM) at 200x magnification to check for the presence or absence of burrs at the edge. As shown in Figure 2, if burrs 10 were observed on the edge cross section, it was determined that burrs were not sufficiently suppressed during the trimming process (indicated as "Present" in the "Presence or Absence of Burrs" column in Table 3). On the other hand, if burrs were not observed on the edge cross section, as shown in Figure 3, it was determined that burrs were sufficiently suppressed during the trimming process (indicated as "Absence or Absence of Burrs" column in Table 3).
[0083] [Evaluation Results] Referring to Tables 1 to 3, the steel sheets of test numbers 1 to 15 satisfied characteristics 1 and 2. Therefore, no burrs were observed in the trimming test, and the generation of burrs during trimming was sufficiently suppressed.
[0084] On the other hand, in test number 16, the B content was too low, so sufficient drawing workability was not obtained, and burrs were observed in the trimming test.
[0085] In test number 17, the B content was too high, and as a result, burrs were observed in the trimming test.
[0086] In test number 18, the annealing temperature T0 in the continuous annealing step was too low. Therefore, the number density ND of the coarse cementite was too low. As a result, burrs were observed in the trimming test.
[0087] In test number 19, the annealing temperature T0 in the continuous annealing step was too high. Therefore, the number density ND of the coarse cementite was too low. As a result, burrs were observed in the trimming test.
[0088] In test number 20, the holding time t0 in the continuous annealing step was too short. Therefore, the number density ND of the coarse cementite was too small. As a result, burrs were observed in the trimming test.
[0089] In test number 21, the holding time t0 in the continuous annealing step was too long. Therefore, the number density ND of the coarse cementite was too small. As a result, burrs were observed in the trimming test.
[0090] In the test No. 22, the heating rate HR1 in the BAF annealing step was too fast. Therefore, the number density ND of the coarse cementite was too small. As a result, burrs were observed in the trimming test.
[0091] In test number 23, the annealing temperature T1 in the BAF annealing step was too low. Therefore, the number density ND of the coarse cementite was too low. As a result, burrs were observed in the trimming test.
[0092] In test number 24, the annealing temperature T1 in the BAF annealing step was too high. Therefore, the number density ND of the coarse cementite was too low. As a result, burrs were observed in the trimming test.
[0093] In the test No. 25, the holding time t1 in the BAF annealing step was too short. Therefore, the number density ND of the coarse cementite was too small. As a result, burrs were observed in the trimming test.
[0094] In the test No. 26, the holding time t1 in the BAF annealing step was too long. Therefore, the number density ND of the coarse cementite was too small. As a result, burrs were observed in the trimming test.
[0095] In test number 27, the cooling rate CR1 in the BAF annealing step was too fast. Therefore, the number density ND of the coarse cementite was too low. As a result, burrs were observed in the trimming test.
[0096] In test number 28, the Mn content was too high. Therefore, the number density ND of coarse cementite was too high. As a result, the earring ratio in the drawing workability evaluation test was too high, and sufficient drawing workability was not obtained.
[0097] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments within the scope of the present disclosure.
Claims
1. The alloy contains, by mass, C: 0.010-0.100%, Si: 0.350% or less, Mn: 1.00% or less, P: 0.070% or less, S: 0.025% or less, sol. Al: 0.005-0.100%, N: 0.0060% or less, and B: 0.50-2.50 times the N content, with the remainder being Fe and impurities. 0.30 μm 2 The number density ND of cementite having an area of 1150 pieces / mm 2 More than 7000 pieces / mm 2 Less than steel plate.
2. The steel sheet according to claim 1, further comprising one layer selected from the group consisting of a Ni plating layer, a Ni diffusion plating layer, a Ni alloy plating layer, and a Ni alloy diffusion plating layer formed on the surface of the steel sheet.
Citation Information
Patent Citations
Steel sheet for drawn can, and method for manufacturing same
WO2016060248A1
Steel plate for drawn can having extremely low earing characteristics and manufacturing method therefor
JP2002060900A
Steel sheet for forming outer cylinder of battery having excellent anisotropy and its production method
JP2002088446A
Steel sheet for two-piece can and production method therefor
WO2018180404A1
Cold rolled steel sheet for drawn can and method for manufacturing same
WO2018194135A1