Silicon nitride powder and resin composition using same

The use of silicon nitride powder with specific characteristics as a filler in resin compositions addresses the issue of high dielectric loss in existing materials, achieving efficient heat dissipation and improved electronic component performance.

WO2024202729A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO CHEM CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006272
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing silicon nitride powders used in resin compositions for heat dissipation do not effectively minimize dielectric loss, which is crucial for electronic components due to their proximity to electronic components.

Method used

A silicon nitride powder with specific characteristics, including a crystallite diameter of more than 70.2 nm, an apparent density of 3.17 g/cm³, a specific surface area of 3.50 m²/g or less, a β conversion rate of 65% or more, and a maximum particle diameter with a low aspect ratio, is used as a filler in a resin composition to reduce dielectric loss.

Benefits of technology

The specified silicon nitride powder effectively forms a resin composition with low dielectric loss, enhancing heat dissipation efficiency while maintaining ease of dispersion and filling rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This silicon nitride powder contains a plurality of silicon nitride particles, and has a crystallite diameter of more than 70.2 nm as measured by the Scherrer method.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon nitride powder and resin composition using same

[0001] The present disclosure relates to a silicon nitride powder and a resin composition using the same.

[0002] Heat generated by passing current through an electronic component is dissipated via a heat sink. To improve heat dissipation efficiency, a technique for filling the space between the electronic component and the heat sink with a heat dissipation material is known. One heat dissipation material is a resin composition containing a resin and inorganic particles, and it is known that silicon nitride powder can be used as the inorganic particles (see, for example, Patent Document 1).

[0003] Patent Document 1 discloses a low-aluminum spherical β-silicon nitride powder for use as a filler in electronic packaging materials. The silicon nitride powder is characterized by a sphericity of 0.5 to 0.99, an Al impurity content of less than 500 ppm, and a particle size range of 0.5 μm to 50 μm.

[0004] Patent Document 2 discloses a method for producing silicon nitride powder suitable for producing silicon nitride sintered bodies, and silicon nitride powder obtained by said method. The silicon nitride powder has an average particle size of 1 to 50 μm, a metal oxide content of 0 to 10 wt %, and an impurity content of less than 1 wt %, preferably the metal oxide content in the silicon nitride powder is less than 1 wt %, and the sintered body has a thermal conductivity of 90 W / mK or more and a bending strength of 700 MPa or more, and preferably the sintering conditions for the sintered body are as follows: the silicon nitride powder is mixed with MgO, Y 2 O 3 The powder is mixed with the above powder, polished, and the powder is dry-press molded, and the powder is gas-pressure sintered at 1900°C and a nitrogen gas pressure of 1 MPa for 8 hours.

[0005] Patent Document 3 discloses a silicon nitride powder suitable for producing a highly thermally conductive silicon nitride sintered body. The silicon nitride powder is characterized by having a β fraction of 30 to 100%, an oxygen content of less than 0.5 wt%, an average particle size of 0.2 to 10 μm, an aspect ratio of 10 or less, and containing columnar particles with grooves formed in the long axis direction of the particle.

[0006] JP 2022-522814 A JP 2022-541208 A JP 2004-262756 A

[0007] Resin compositions used as heat dissipation materials are desirably placed near electronic components, and therefore must have low dielectric loss. Therefore, there is a demand for silicon nitride powders that can form resin compositions with low dielectric loss. However, the silicon nitride powders described in Patent Documents 1 to 3 have not been considered for forming resin compositions with low dielectric loss.

[0008] In view of these circumstances, one embodiment of the present invention aims to provide a silicon nitride powder for use as a filler for resin compositions, which is capable of forming a resin composition with low dielectric loss. Furthermore, another embodiment of the present invention aims to provide a resin composition using the silicon nitride powder.

[0009] A first aspect of the present invention is a silicon nitride powder comprising a plurality of silicon nitride particles, the crystallite size being greater than 70.2 nm as measured by the Scherrer method.

[0010] In aspect 2 of the present invention, the apparent density is 3.17 g / cm 3 2. The silicon nitride powder according to claim 1, wherein the silicon nitride powder has a molecular weight of 1.0 or more.

[0011] In the third aspect of the present invention, the specific surface area is 3.50 m 2 / g or less.

[0012] A fourth aspect of the present invention is the silicon nitride powder according to any one of the first to third aspects, wherein the β-phase ratio is 65% or more.

[0013] A fifth aspect of the present invention is the silicon nitride powder according to any one of the first to fourth aspects, wherein the ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge is 1% or less, and the maximum particle size of the silicon nitride particles is 6.8 μm or more.

[0014] A sixth aspect of the present invention is a resin composition comprising a resin and the silicon nitride powder according to any one of the first to fifth aspects.

[0015] By using the silicon nitride powder according to one embodiment of the present invention as a filler, a resin composition with low dielectric loss can be obtained.

[0016] [Silicon nitride powder] The present inventors have investigated silicon nitride powders used as fillers in resin compositions from various perspectives in order to realize resin compositions with low dielectric loss. As a result, they have discovered for the first time that it is important to control the crystallite size of the silicon nitride powder, as measured by the Scherrer method, to a predetermined value or more, and have completed the present invention. Below, details of each requirement specified in the embodiments of the present invention are shown.

[0017] (Crystallite diameter) The silicon nitride powder according to the embodiment of the present invention comprises a plurality of silicon nitride particles and has a crystallite diameter of more than 70.2 nm as measured by the Scherrer method. Since there are no defects within the crystallites of silicon nitride powder, the larger the crystallite diameter, the lower the dielectric loss. Therefore, by using a silicon nitride powder with a large crystallite diameter, a resin composition with low dielectric loss can be obtained. Preferably, the crystallite diameter is 70.5 nm or more, more preferably 72.0 nm or more, even more preferably 76.0 nm or more, even more preferably 80.0 nm or more, and particularly preferably 85.0 nm or more. The upper limit is not particularly limited, but may be less than 300 nm, 200 nm or less, or 150 nm or less. In this specification, "crystallite" refers to the smallest unit of crystal that contributes to X-ray diffraction. On the other hand, in this specification, the term "single crystal particle" as described below refers to a relatively large crystal in which, when a boundary with a crystal misorientation (oblique angle) exceeding 15° (also called a high-angle grain boundary) is defined as a crystal grain boundary as a result of EBSD analysis, the crystal grain boundary does not exist (i.e., a boundary with a crystal misorientation of 15° or less may exist). In this specification, the term "single crystal particle" may include, for example, multiple "crystallites."

[0018] As described above, the crystallite size of the silicon nitride powder according to the embodiment of the present invention is measured by the Scherrer method. Specifically, a diffraction pattern of the silicon nitride powder is obtained by powder X-ray diffraction (X-ray source: CuKα radiation). From the diffraction pattern, the diffraction angle θ and half-width β of the peak for each plane of the (110), (200), (101), and (210) (or (120)) planes of β-type silicon nitride are determined, and these are substituted into the following Scherrer equation (1) to determine the crystallite size D. The average value of the crystallite size values ​​calculated for each plane is taken as the crystallite size of the silicon nitride powder. D = Kλ / β cos θ (1) In the above equation (1), K is the Scherrer constant (= 0.94), β is the half-width of the peak (rad.), θ is the diffraction angle (rad.), and λ is 0.15418 nm.

[0019] (Apparent Density) The apparent density of the silicon nitride powder according to the embodiment of the present invention is 3.17 g / cm 3 It is preferable that the density is greater than 3.18 g / cm 3 This makes it possible to obtain a silicon nitride powder containing many silicon nitride particles with a small amount of internal voids, making it easier to obtain a resin composition with lower dielectric loss. The upper limit of the apparent density is, for example, 3.44 g / cm 3 In addition, if the apparent density is not too high, it is expected that the powder will be less likely to settle when mixed with a resin and will be easier to disperse. In order to achieve such an effect, the apparent density of the silicon nitride powder should be 3.30 g / cm 3 It is preferable that the density is 3.25 g / cm or less, and more preferably 3.25 g / cm 3 The following is the result.

[0020] The apparent density of the silicon nitride powder is measured by the pycnometer method in accordance with JIS R 1620:1995. The measurement is carried out five or more times, and the average value is taken as the apparent density of the silicon nitride powder. For the measurement, for example, an Accupyc 1330 (Micromeritics) can be used.

[0021] (Specific Surface Area) The specific surface area of ​​the silicon nitride powder according to the embodiment of the present invention is a BET specific surface area measured by a krypton adsorption method based on JIS Z 8830:2013, and is 3.50 m 2 / g or less, and more preferably 2.66m 2 / g, more preferably less than 2.00 m 2 / g or less, more preferably 1.50m 2 / g or less, and particularly preferably 1.36m 2 This reduces the number of interfaces with the resin, and as a result, it is expected that the dielectric loss of the resin composition can be reduced. The lower limit of the specific surface area is not particularly limited, but is, for example, 0.01 m 2 / g or more, and 2 / g or more, and 2 / g or more, and 2 / g or more.

[0022] (β-Proportion) The β-proportion of the silicon nitride powder is preferably 65% ​​or more. A β-proportion of 65% or more makes it easier to obtain a resin composition with lower dielectric loss. The β-proportion is more preferably 70% or more, even more preferably 80% or more, still more preferably 85% or more, and particularly preferably 90% or more.

[0023] In this specification, the "β-phase ratio" refers to the content (volume %) of β-type silicon nitride relative to all silicon nitrides contained in the silicon nitride powder.

[0024] In calculating the β-phase ratio, a diffraction pattern of silicon nitride powder was obtained by powder X-ray diffraction (X-ray source: CuKα ray), and the diffraction pattern was analyzed by the Gazzara & Messier method (G.P. Gazzara and D.P. Messier, "Determination of Phase Content of Si 3 N 4 The β-phase ratio is calculated by analyzing the β-phase by X-ray Diffraction Analysis, Am. Ceram. Soc. Bull., 56[9]777-80 (1977)).

[0025] (The maximum particle size of silicon nitride particles having a ratio (L2 / L1) of the total length L2 of the internal boundaries to the outer edge length L1 of 1% or less is 6.8 μm or more.) The fewer grain boundaries and cavities there are inside a silicon nitride particle, the lower the dielectric loss of the silicon nitride particle. Therefore, the ratio (L2 / L1) of the total length L2 of the boundaries to the outer edge length L1 is introduced as an indicator of the content of grain boundaries inside a silicon nitride particle. L1 and L2 are determined by observing the cross section of a silicon nitride particle. Note that the terms "grain boundary" and "boundary line" used here refer to boundaries where the crystal orientation misorientation (oblique angle) exceeds 15° as a result of EBSD analysis (also called high-angle grain boundaries).

[0026] When the length of the outer edge of one silicon nitride particle is L1 and the total length of the boundary lines of that silicon nitride particle is L2, silicon nitride particles with a small value of L2 / L1 can be said to have a low content of boundary lines. In this embodiment, silicon nitride particles with an L2 / L1 ratio of 1% or less are considered to be silicon nitride particles made of a single crystal (referred to as "single crystal particles"). Single crystal particles can be said to be silicon nitride particles with low dielectric loss.

[0027] In this embodiment, the maximum particle size of the silicon nitride particles having an L2 / L1 ratio of 1% or less (i.e., single crystal) is preferably 6.8 μm or more, more preferably 10.0 μm or more, even more preferably 15.0 μm or more, and particularly preferably 20.0 μm or more, which makes it easier to obtain a resin composition with low dielectric loss.

[0028] (Average aspect ratio of silicon nitride particles) The average aspect ratio of the minor axis to the major axis of the silicon nitride particles contained in the silicon nitride powder is preferably more than 0.50, more preferably more than 0.60, even more preferably 0.70 or more, and even more preferably 0.72 or more. On the other hand, the average aspect ratio of the silicon nitride particles is preferably less than 0.87, more preferably 0.85 or less, and even more preferably 0.80 or less. When the average aspect ratio of the silicon nitride particles is within an appropriate range, the filling rate in the resin composition can be further improved.

[0029] The average aspect ratio of silicon nitride particles is measured as follows. SEM images of silicon nitride particles contained in silicon nitride powder are analyzed using image processing software (e.g., Image J (manufactured by the National Institute of Health)). The maximum particle size of the silicon nitride particles (referred to as the "major axis") is identified, and the particle size in the direction perpendicular to the major axis is referred to as the "minor axis". The major and minor axes are measured for 20 random silicon nitride particles, and the ratio of the minor axis to the major axis (minor axis / major axis) is determined for each particle. The arithmetic mean value of these ratios is taken as the average aspect ratio of the silicon nitride particles.

[0030] (Surface roughness Ra) The surface roughness Ra (arithmetic mean roughness) of the silicon nitride powder is preferably less than 0.97 nm. If the surface roughness Ra is less than 0.97 nm, when used as a filler for a resin composition, the interface with the resin will be reduced, and as a result, it can be expected that the dielectric loss of the resin composition can be reduced. The surface roughness Ra is preferably less than 0.97 nm, more preferably 0.95 nm or less, even more preferably less than 0.93 nm, still more preferably 0.90 nm or less, and even more preferably 0.80 nm or less.

[0031] To measure the surface roughness Ra, a 100 nm x 100 nm measurement area on the surface of any silicon nitride particle is observed using a scanning probe microscope (SPM). The surface roughness Ra is calculated from the obtained shape image. The surface roughness Ra is measured for four silicon nitride particles, and the average value is taken as the surface roughness Ra of the silicon nitride powder.

[0032] [Method for Producing Silicon Nitride Particles] The silicon nitride powder according to an embodiment of the present invention can be produced by a production method including the following steps: (1) synthesizing silicon nitride synthetic crystals by combustion synthesis in a nitrogen atmosphere using raw materials containing Si, (2) crushing the silicon nitride synthetic crystals to obtain coarsely pulverized silicon nitride powder, (3) finely pulverizing the coarsely pulverized silicon nitride powder to obtain finely pulverized silicon nitride powder, and (4) heat-treating the finely pulverized silicon nitride powder to obtain silicon nitride powder. Each step is described in detail below.

[0033] Step (1): Synthesizing silicon nitride composite crystals. For example, Si powder is used as the raw material containing Si. The average particle diameter D50 of the raw material is, for example, within the range of 2 to 10 μm. This allows the amount of oxygen impurities to be suppressed, and the combustion rate to be increased, allowing for a higher synthesis temperature, resulting in good crystal growth. As an example, the average particle diameter D50 of Si is 5 μm.

[0034] The diluent is used to adjust the amount of Si in the raw materials. A separately prepared silicon nitride powder is used as the diluent. The diluent may be either α-type silicon nitride powder or β-type silicon nitride powder, or a mixture of these. The average particle diameter D50 of the diluent is preferably in the range of 0.5 to 2.0 μm. For example, the average particle diameter D50 of the diluent is 1.0 μm. The amount of diluent added is less than 10% by mass of the total raw materials (including the diluent). For example, the diluent is added in an amount of 5 to 8% by mass of the total raw materials. By keeping the amount of diluent added within the above range, it becomes easier to obtain silicon nitride powder with a predetermined crystallite size.

[0035] In this embodiment, a diluent is mixed with the raw materials and filled into an insulated heat-resistant container. This insulated heat-resistant container has a thermal conductivity of 1 W / mK or less, and although alumina or zirconia can be used as the material, carbon is preferred in consideration of the risk of impurities being mixed in. After the raw materials are filled, the container is covered with a lid made of the same material as the insulated heat-resistant container. Furthermore, to increase the temperature inside the composite during combustion, the thickness of the mixed raw materials is set to more than 100 mm, preferably more than 100 mm and no more than 150 mm. Combustion synthesis is performed under a nitrogen atmosphere in the range of 0.5 to 1 MPa (e.g., 0.9 MPa). Adjusting the pressure range within the above range enables efficient synthesis while suppressing increases in equipment costs.

[0036] When the mixed raw material is filled into the crucible, a layer of powder (silicon nitride) having a thickness of 1 mm to 80 mm is laid on the bottom and sides of the crucible, the mixed raw material is then filled, and the top surface is covered with a layer of powder having a thickness of 1 mm to 80 mm. The thickness of the powder is 100 mm or less, preferably 1 mm to 80 mm. Covering the powder allows the mixed raw material to be kept warm, making it easier to obtain silicon nitride powder with a predetermined crystallite size.

[0037] To promote crystal growth more effectively, a catalyst may be used, for example, Y 2 O 3 , Fe 2 O 3 , CaO, Ni, Co, C, etc. are added in an amount of about 0.01 to 0.1 mass %. In addition, external auxiliary heating is performed in the range of 500°C to 1700°C (for example, 1500°C), and the combustion temperature is also increased in the combustion synthesis method by self-ignition.

[0038] Step (2): Obtaining a coarsely pulverized silicon nitride powder. The silicon nitride composite crystal is in the form of an agglomeration of multiple silicon nitride particles. In step (2), the silicon nitride composite crystal is crushed to obtain a coarsely pulverized silicon nitride powder. For example, the composite is crushed using a common crushing device such as a hammer mill or a disk mill until it passes through a sieve with a specified mesh size (for example, a sieve with mesh sizes in the range of 400 μm to 500 μm).

[0039] Step (3): Obtaining a finely pulverized silicon nitride powder The coarsely pulverized silicon nitride powder is further pulverized to obtain a finely pulverized silicon nitride powder. The pulverization is carried out using a pulverizing device such as a jet mill or a ball mill. If necessary, the obtained finely pulverized powder may be classified. Classification can be carried out by sieving, wet classification, or the like.

[0040] Step (4): Step of Obtaining Silicon Nitride Powder The finely pulverized silicon nitride powder is heat-treated to obtain silicon nitride powder. The heat treatment forms an oxide film on the surface of the silicon nitride particles, chemically stabilizing the silicon nitride particles. The heat treatment is carried out in air at a temperature of 500°C or higher and 1200°C or lower, preferably higher than 800°C and lower than 1100°C. The heat treatment time can be adjusted appropriately depending on the heat treatment temperature. The heat treatment time is, for example, 5 hours.

[0041] In the method for producing silicon nitride powder, silicon nitride synthetic crystals are synthesized using the heat generated by combustion synthesis, and then the silicon nitride powder according to this embodiment can be produced by crushing, classifying, and pulverizing the synthesized crystals.

[0042] [Resin composition] By using the silicon nitride powder according to the embodiment of the present invention as a filler for a resin composition, a resin composition with low dielectric loss can be obtained. The resin composition contains a resin and the silicon nitride powder according to the embodiment of the present invention.

[0043] The resin / silicon nitride powder blending ratio of the resin composition according to the embodiment of the present invention can be appropriately determined depending on the purpose and / or application. As an example, the resin composition (composite) may contain 5 to 75 volume % of resin and 95 to 25 volume % of silicon nitride powder. The filling rate of the silicon nitride powder in the resin composition refers to the content (vol %) of silicon nitride powder when the volume of the resin composition (including the silicon nitride powder) is taken as 100 volume %.

[0044] A method for producing a resin composition will be described. A resin composition can be obtained by mixing silicon nitride powder and a resin using a commonly used known method. For example, when the resin is liquid (e.g., liquid epoxy resin), the resin composition can be obtained by mixing the liquid resin, silicon nitride powder, and a curing agent, and then curing the mixture with heat or ultraviolet light. Known curing agents, mixing methods, and curing methods can be used. On the other hand, when the resin is solid, the desired resin composition can be obtained by mixing the silicon nitride powder and the resin, and then kneading the mixture using a known method such as melt kneading.

[0045] The resin used in the resin composition can be a known resin such as an epoxy resin. The type of resin can be selected from thermoplastic resins, thermoplastic elastomers, and thermosetting resins. The resins can be used alone or in combination of two or more.

[0046] Furthermore, these resin compositions may contain, as needed, known additives such as plasticizers, curing accelerators, coupling agents, fillers, pigments, flame retardants, antioxidants, surfactants, compatibilizers, weather resistance agents, antiblocking agents, antistatic agents, leveling agents, and release agents, either singly or in combination, within the scope of the invention.

[0047] The silicon nitride powder according to the embodiment and the resin composition containing the silicon nitride powder are particularly suitable for use as a heat-dissipating material with low dielectric loss. Thus, one aspect of the present disclosure can provide a heat-dissipating silicon nitride powder with low dielectric loss and a heat-dissipating resin composition with low dielectric loss.

[0048] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples carried out to clarify the effects of the embodiments of the present invention. However, the embodiments of the present invention are not limited to the following examples.

[0049] <Preparation of Silicon Nitride Powder> Si powder (particle size = 5 μm) and silicon nitride powder (particle size = 1 μm) prepared separately as a diluent were mixed in a tumbling ball mill. The amount of diluent added was 5 to 8 mass% of the total raw materials (including diluent). The mixed powder was filled into a carbonaceous, heat-resistant container with a layer of powder 1 mm to 80 mm thick on the bottom and sides, so that the raw material layer was thicker than 100 mm and not more than 150 mm. The raw material layer was then covered with a layer of powder 1 mm to 80 mm thick. A lid made of a carbonaceous, heat-resistant material was then placed in the container, and synthesis was carried out under a nitrogen atmosphere at 0.9 MPa. After synthesis, the mixture was coarsely crushed (disintegrated) in a mortar until it passed through a sieve with the specified mesh size. The mesh size of the sieve used is shown in Table 1.

[0050] (Samples Nos. 1, 3, and 4) The obtained coarsely pulverized powder was further finely pulverized using a nanojetmizer (manufactured by Aisin Nano Technologies Co., Ltd.). A nanojetmizer with the model number listed in Table 1 was used for the fine pulverization. The obtained finely pulverized powder was classified using the method listed in Table 1. The D50 of the obtained classified powder of Sample No. 3 was 12.0 μm, and the D50 of the classified powder of Sample No. 4 was 14.0 μm. The obtained classified powder was then placed in an alumina crucible and heat-treated in an air atmosphere using a small powder programmable electric furnace (MMF series, manufactured by AS ONE) under the conditions (heat treatment temperature, heat treatment time) listed in Table 1 to obtain silicon nitride powders (Samples Nos. 1, 3, and 4).

[0051] (Sample No. 5) Coarsely pulverized powder was prepared in the same manner as in "Samples No. 1, 3, and 4" above. The sieve used during coarse pulverization (disintegration) had a mesh size of 500 μm. The obtained coarsely pulverized powder was then finely pulverized in a ball mill. The obtained finely pulverized powder was sieved using a vibrating sieve according to the following procedure, and then further wet-classified to obtain silicon nitride powder with the desired D50. The powder remaining below the sieve when sieving using a sieve with a mesh size of 63 μm was further sieved using a sieve with a mesh size of 10 μm. The obtained silicon nitride powder was then placed in an alumina crucible and heat-treated in an air atmosphere using a small powder programmable electric furnace (MMF series, manufactured by AS ONE) at a heat treatment temperature of 1100°C for 5 hours to obtain silicon nitride powder (Sample No. 5). The D50 of No. 5 was 3.5 μm.

[0052]

[0053] Various measurements were performed on the obtained Samples Nos. 1 and 3 to 5 (Examples) and, as a comparative example, a commercially available silicon nitride powder (manufactured by Aldrich, silicon nitride (predominantly β-phase, ≦10 micron primary particle size, product code 248622); hereinafter referred to as “Sample No. 2”).

[0054] (1) Crystallite Size The crystallite size of the sample (silicon nitride powder) was measured by the Scherrer method. Specifically, a diffraction pattern of the sample was obtained by powder X-ray diffraction (X-ray source: CuKα radiation). From the diffraction pattern, the diffraction angle θ and half-width β of the peak for each plane were determined for the (110), (200), (101), and (210) (or (120)) planes of β-type silicon nitride, and these were substituted into the following Scherrer formula (1) to determine the crystallite size D. The average value of the crystallite size values ​​calculated for each plane was taken as the crystallite size of the silicon nitride powder. D = Kλ / βcosθ (1) In the above formula (1), K is the Scherrer constant (= 0.94), β is the half-width of the peak (rad.), θ is the diffraction angle (rad.), and λ is 0.15418 nm.

[0055] (2) Apparent Density The apparent density of the sample (silicon nitride powder) was measured in accordance with JIS R 1620:1995. The measurement method and conditions were as follows: Measurement method: Gas substitution method Sample drying: 200°C, 8 hours or more Apparatus used: Accupyc 1330 (Micromeritics) Measurement conditions Number of purges: 10 Purge filling pressure: 15.0 psig Number of measurements: 5 Measurement filling pressure: 15.0 psig Equilibrium pressure: 0.005 psig / min Measurement with set precision: Yes Allowable error of variation: 0.05% Sample cell size: 10 cm 3

[0056] (3) Specific Surface Area The specific surface area of ​​the sample (silicon nitride powder) was measured. The specific surface area of ​​powder (solid) was measured by gas adsorption in accordance with JIS Z 8830:2013, using krypton as the adsorption gas. In the measurement, 1 g of silicon nitride powder was placed in a sample tube, and an adsorption / desorption isotherm was obtained. The specific surface area (m 2 / g) was calculated.

[0057] (4) β-Proportion The diffraction pattern of the sample (silicon nitride powder) was obtained using a powder X-ray diffractometer (manufactured by Rigaku Denki). The measurement conditions were as follows: X-ray source: CuKα radiation; X-ray output: 45 kV, 200 mA; Graphite monochromator; Diffraction angle (2θ): Step scan in the range of 2 to 90° in 0.02° increments; Scanning speed: 21.7 deg / min.

[0058] When a sample contained components other than silicon nitride, the peaks of those components were compared with the corresponding peaks of standard samples of those components to determine the proportions of those components. For Samples No. 1 and 2, the powder X-ray diffraction patterns obtained confirmed that the samples were composed solely of α-type silicon nitride and β-type silicon nitride. The proportion of β-type silicon nitride in the sample (β-conversion ratio) was then calculated using the Gazzara & Messier method.

[0059] (5) Maximum particle size of silicon nitride particles with an L2 / L1 ratio of 1% or less (maximum particle size of single-crystal particles) A ​​cross-sectional observation specimen was prepared using the sample (silicon nitride particles). To prepare the cross-sectional observation specimen, the silicon nitride particles were embedded in resin, and then the resin and silicon nitride particles were cut using a diamond cutter. Subsequently, a protective film of platinum was vapor-deposited on the cross-section, and the cross-section was prepared by Ar ion milling. The specimen was then fixed to the SEM sample stage with Cu double-sided tape, and SEM-EBSD measurement was performed without vapor deposition. The observation position was determined so that two or more silicon nitride particles were completely contained within the observation region (i.e., two or more silicon nitride particles did not come into contact with the frame of the observation region). Measurements were performed using β-type silicon nitride particles.

[0060] The following equipment was used for sample pretreatment and EBSD measurement: Equipment used Ion milling equipment: E-3500 (manufactured by Hitachi High-Tech Corporation) Ion sputtering equipment: E-1030 (manufactured by Hitachi, Ltd.) Schottky scanning electron microscope: SU5000 (manufactured by Hitachi High-Tech Corporation) Backscattered electron diffraction equipment: Velocity (manufactured by METEK Corporation)

[0061] The conditions for the EBSD measurement were as follows: Measurement area: 500.0 μm×400.0 μm Acceleration voltage: 15.0 kV Magnification: ×500 Vacuum degree: 30 Pa

[0062] In the obtained EBSD image, two or more silicon nitride particles that were not in contact with the frame of the observation area were selected, and the average of the outer edge length L1 of each silicon nitride particle was calculated using image processing software Image J (manufactured by the National Institute of Health). The total length L2 of the boundary lines was also calculated. The "total length L2 of the boundary lines" is the sum of the boundary lines contained within the silicon nitride particle and does not include the outer edge of the silicon nitride particle. The total length L2 of the boundary lines was calculated by adding the total length of the grain boundaries within the silicon nitride particle and the total length of the inner wall of the cavity (if there was a cavity within the silicon nitride particle). Note that here, "grain boundary" and "boundary line" refer to boundaries (also called high-angle grain boundaries) where the crystal orientation misorientation (oblique angle) exceeds 15° as a result of EBSD analysis.

[0063] This measurement was carried out once for 20 random silicon nitride particles, and silicon nitride particles with an L2 / L1 ratio of 1% or less were considered to be single crystal particles, and the length of their major axis was measured and recorded as the "maximum particle size of the single crystal particles." If the 20 silicon nitride particles measured contained multiple single crystal particles, the arithmetic average of their maximum particle sizes was calculated.

[0064] (6) Average aspect ratio of silicon nitride particles SEM images of the sample (silicon nitride powder) were taken. The following equipment was used for taking the images. Equipment used: Scanning electron microscope: JSM-IT200 (manufactured by JEOL Ltd.) The imaging conditions were as follows: Acceleration voltage: 5.0 kV Signal: SED Probe current: Std. -PC55 Magnification: 1000x

[0065] The SEM images were processed using image processing software Image J (manufactured by the National Institute of Health), and the aspect ratios of 20 randomly selected silicon nitride particles in the SEM images were determined. The maximum diameter of the silicon nitride particles was taken as the major axis, and the particle size in the direction perpendicular to the major axis was taken as the minor axis. The major and minor axes of 20 randomly selected silicon nitride particles were measured, and the ratio of the minor axis to the major axis (minor axis / major axis) was determined for each particle. The arithmetic mean value of these ratios was taken as the average aspect ratio of the silicon nitride particles (referred to as "aspect ratio" in Table 2).

[0066] (7) Surface Roughness Ra A scanning probe microscope SPA300HV manufactured by Seiko Instruments Inc. was used to measure the surface roughness Ra. The measurement conditions were as follows: Probe station / unit SPI4000 / SPA300HV Cantilever: SI-DF20 Scanner: 20 μm Data type: topographic image Observation mode: DFM (Dynamic Force Mode Microscope) Scanning area: 100 nm × 100 nm Scanning frequency: 0.25 Hz Analysis software: (attached to the measuring device)

[0067] Five silicon nitride particles were randomly selected from the image, and a measurement area of ​​100 nm × 100 nm on the surface of each particle was observed using a scanning probe microscope (SPM). The surface roughness Ra of each particle was calculated from the obtained shape image, and the average value was taken as the surface roughness Ra of the silicon nitride powder.

[0068] (8) Dielectric Loss of Resin Composition (Composite) Polypropylene resin (J105G manufactured by Prime Polymer Co., Ltd.) and a sample (silicon nitride powder) were mixed at a volume ratio of 60:40. Using a press molding machine, vacuum press molding was carried out under the following conditions to produce a silicon nitride powder-resin composite with a thickness of 600 μm.

[0069] The dielectric loss (tan δ) of the composite was measured under the following measurement conditions: Measurement device: Network analyzer 8720ES (manufactured by Agilent Technologies) Test piece dimensions: 50 mm x 50 mm Measurement frequency: 12 GHz Test environment: 22°C / 59% RH

[0070] The measurement results are summarized in Tables 2 and 3.

[0071]

[0072]

[0073] The measurement results are discussed below. The composites using silicon nitride powders of Samples 1 and 3 to 5, which met the requirements of this embodiment, exhibited low dielectric loss. On the other hand, the composite using silicon nitride powder of Sample 2, which did not meet the requirements of this embodiment, exhibited high dielectric loss.

[0074] This application claims priority from Japanese Patent Application No. 2023-058622, filed March 31, 2023. Japanese Patent Application No. 2023-058622 is incorporated herein by reference.

Claims

1. A silicon nitride powder comprising a plurality of silicon nitride particles, the crystallite size being greater than 70.2 nm as measured by the Scherrer method.

2. Apparent density is 3.17 g / cm 3 The silicon nitride powder of claim 1, wherein the silicon nitride powder has a molecular weight of 1.0 or more.

3. Specific surface area is 3.50 m 2 2. The silicon nitride powder according to claim 1, wherein the silicon nitride powder has a molecular weight of 1000 or less.

4. The silicon nitride powder according to claim 1, having a beta-conversion rate of 65% or more.

5. The silicon nitride powder according to claim 1, wherein the ratio (L2 / L1) of the total length L2 of the internal boundary line to the length L1 of the outer edge is 1% or less and the maximum particle size of the silicon nitride particles is 6.8 μm or more.

6. A resin composition comprising a resin and the silicon nitride powder according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Production of silicon nitride

    JP1997255310A

  • Manufacturing method of surface treatment powder for thermally-conductive grease and surface treatment powder for thermally-conductive grease

    JP2019172511A

  • Method of producing high purity silicon nitride powder

    JP2020023406A

  • High-purity, low-aluminum spherical β-silicon nitride powder, its manufacturing method and applications

    JP2022522814A

  • Method for producing high-purity silicon nitride powder

    WO2018110565A1