Silicon nitride powder and resin composition using same

The silicon nitride powder with specific characteristics addresses the limitations in thermal diffusivity of current resin compositions by enhancing the contact area and number of thermal diffusion paths, leading to improved heat dissipation in electronic components.

WO2024202733A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO CHEM CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006293
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current resin compositions used for heat dissipation in electronic components have limitations in thermal diffusivity, particularly due to the shape and properties of silicon nitride particles, which hinder effective heat dissipation as electronic devices generate increasing amounts of heat.

Method used

A silicon nitride powder with specific characteristics, including silicon nitride particles having two parallel sides, an appropriate area ratio, high apparent density, low surface roughness, and a high β conversion rate, is used as a filler in a resin composition to enhance thermal diffusivity by increasing the contact area and number of thermal diffusion paths.

Benefits of technology

The use of the specified silicon nitride powder as a filler in the resin composition significantly improves thermal diffusivity, allowing for more effective heat dissipation in electronic components, even at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-M000001
    Figure JPOXMLDOC01-APPB-M000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is a silicon nitride powder that contains silicon nitride particles containing first silicon nitride particles having an outer shape with two parallel sides in plan view. When the total area of all the silicon nitride particles in said plan view is 100%, the ratio of the area occupied by the first silicon nitride particles is more than 1.2% and less than 100%.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon nitride powder and resin composition using same

[0001] The present disclosure relates to a silicon nitride powder and a resin composition using the same.

[0002] Heat generated by passing current through an electronic component is dissipated via a heat sink. To improve heat dissipation efficiency, a technique for filling the space between the electronic component and the heat sink with a heat dissipation material is known. One heat dissipation material is a resin composition containing a resin and inorganic particles, and it is known that silicon nitride powder can be used as the inorganic particles (see, for example, Patent Document 1).

[0003] Patent Document 1 discloses a low-aluminum spherical β-silicon nitride powder for use as a filler in electronic packaging materials. The silicon nitride powder is characterized by a sphericity of 0.5 to 0.99, an Al impurity content of less than 500 ppm, and a particle size range of 0.5 μm to 50 μm.

[0004] Patent Document 2 discloses a method for producing silicon nitride powder suitable for producing silicon nitride sintered bodies, and silicon nitride powder obtained by said method. The silicon nitride powder has an average particle size of 1 to 50 μm, a metal oxide content of 0 to 10 wt %, and an impurity content of less than 1 wt %, preferably the metal oxide content in the silicon nitride powder is less than 1 wt %, and the sintered body has a thermal conductivity of 90 W / mK or more and a bending strength of 700 MPa or more, and preferably the sintering conditions for the sintered body are as follows: the silicon nitride powder is mixed with MgO, Y 2 O 3 The powder is mixed with the above powder, polished, and the powder is dry-press molded, and the powder is gas-pressure sintered at 1900°C and a nitrogen gas pressure of 1 MPa for 8 hours.

[0005] Patent Document 3 discloses a silicon nitride powder suitable for producing a highly thermally conductive silicon nitride sintered body. The silicon nitride powder is characterized by having a β fraction of 30 to 100%, an oxygen content of less than 0.5 wt%, an average particle size of 0.2 to 10 μm, an aspect ratio of 10 or less, and containing columnar particles with grooves formed in the long axis direction of the particle.

[0006] JP 2022-522814 A JP 2022-541208 A JP 2004-262756 A

[0007] In recent years, the increase in heat generation in ICs due to the high integration of ICs in electronic devices and the increase in heat generation in electronic components due to the use of high-current-driven electronic components due to the electrification of electric vehicles, aircraft, etc. have become problems. In order to achieve more effective heat dissipation, there is a demand for further improvement in the thermal diffusivity of resin compositions.

[0008] In Patent Document 1, increasing the sphericity of silicon nitride powder (i.e., making it spherical particles) enables high loading into a resin composition, thereby improving the thermal diffusivity of the resin composition. However, there is still room for further investigation into the shape of silicon nitride particles in order to further improve the thermal diffusivity.

[0009] The silicon nitride powders in Patent Documents 2 and 3 disclose silicon nitride powders for use in silicon nitride sintered bodies, and therefore do not discuss mixing them with resins to form resin compositions, nor do they discuss silicon nitride powders suitable as fillers for resin compositions.

[0010] In view of these circumstances, one embodiment of the present invention aims to provide a silicon nitride powder for use as a filler for a resin composition, which is capable of improving the thermal diffusivity of the resin composition. Furthermore, another embodiment of the present invention aims to provide a resin composition using the silicon nitride powder.

[0011] A first aspect of the present invention is a silicon nitride powder comprising silicon nitride particles, the silicon nitride particles including first silicon nitride particles having an outer shape including two parallel sides in a planar view, wherein, when the total area of ​​all the silicon nitride particles in the planar view is taken as 100%, the proportion of the area occupied by the first silicon nitride particles is more than 1.2% but less than 100%.

[0012] In aspect 2 of the present invention, the apparent density is 3.17 g / cm 3 2. The silicon nitride powder according to claim 1, wherein the silicon nitride powder has a molecular weight of 1.0 or more.

[0013] A third aspect of the present invention is the silicon nitride powder according to the first or second aspect, wherein the silicon nitride powder has a surface roughness Ra of less than 0.97 nm.

[0014] A fourth aspect of the present invention is the silicon nitride powder according to any one of the first to third aspects, wherein the silicon nitride particles have an average aspect ratio of their minor axis to their major axis of greater than 0.50.

[0015] A fifth aspect of the present invention is the silicon nitride powder according to any one of the first to fourth aspects, wherein the β-phase ratio is 65% or more.

[0016] A sixth aspect of the present invention is the silicon nitride powder according to any one of the first to fifth aspects, wherein the ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge is 1% or less, and the maximum particle size of the silicon nitride particles is 6.8 μm or more.

[0017] A seventh aspect of the present invention is a resin composition comprising a resin and the silicon nitride powder according to any one of the first to sixth aspects.

[0018] By using the silicon nitride powder according to one embodiment of the present invention as a filler, a resin composition having a high thermal diffusivity can be obtained.

[0019] FIG. 2 is a schematic diagram for explaining a method for identifying the sides of silicon nitride particles contained in silicon nitride powder.

[0020] [Silicon nitride powder] The present inventors have investigated silicon nitride powder used as a filler in resin compositions from various perspectives in order to achieve more effective heat dissipation. As a result, they have discovered for the first time that in order to sufficiently form heat conduction paths between silicon nitride particles contained in the silicon nitride powder in a resin composition, it is important to control the shape of the silicon nitride particles, and in particular, that it is important that the silicon nitride powder contains a certain amount or more of silicon nitride particles having two parallel sides in a planar view, which led to the completion of the present invention.

[0021] A silicon nitride powder according to an embodiment of the present invention is intended to be mixed with a resin as a filler for a resin composition. The silicon nitride powder comprises silicon nitride particles, including first silicon nitride particles having an outer shape including two parallel sides in a planar view, and the ratio of the area occupied by the first silicon nitride particles (hereinafter also referred to as "area ratio") to the total area of ​​all silicon nitride particles in the planar view is taken as 100%. These characteristics enable the thermal diffusivity of the resin composition to be improved. Each characteristic is described below.

[0022] (Area ratio of first silicon nitride particles) The silicon nitride powder of this embodiment contains silicon nitride particles. In particular, silicon nitride particles having an outer shape including two parallel sides in a planar view are referred to as "first silicon nitride particles." In the silicon nitride powder of this embodiment, when the total area of ​​all silicon nitride particles is taken as 100% in a planar view, the area ratio occupied by the first silicon nitride particles is more than 1.2% but less than 100%. The planar view refers to a shape that appears in a two-dimensional image that can be obtained, for example, by a scanning electron microscope image (SEM image).

[0023] The "outer shape including two parallel sides" of the first silicon nitride particle will be described in detail below. First, the sides that are the "two parallel sides" are determined as follows.

[0024] Hereinafter, a method for determining a side will be described with reference to Fig. 1. In Fig. 1, three points p are intentionally drawn in a range of the contour line 10L of the silicon nitride particle 10 that is unlikely to be recognized as a "side." 1 ~p 3 Please note that the following is set.

[0025] A planar image of a silicon nitride particle (for example, an SEM image) is acquired, and three arbitrary points p are drawn on the contour line 10L of one silicon nitride particle 10. 1 ~p 3 (See Figure 1.) When all of the following conditions (i) to (iii) are satisfied, the line segment p 1 p 3 is identified as one of the “sides” of the silicon nitride particle 10. (i) Three points p1 ~p 3 (ii) Three points p 1 ~p 3 A line connecting any two points (point p 1 and point p 2 A line connecting point p 1 and point p 3 The line connecting the points p 2 and point p 3 The longest line segment defined by the two points (in Figure 1, point p 1 and point p 3 Line segment p 1 p 3 (iii) The length a of the longest line segment is 2 μm or more. 1 and point p 3 ) the length of the contour line 10L between the two points is b, 1 p 3 The relationship between the length a and the length b satisfies the following formula (1): 1≦b / a<1.01 (1)

[0026] The "coefficient of determination R2" is calculated by the following formula (2), and is calculated by squaring the correlation coefficient.

[0027] Here, x is the average value of xi (i=1-n), and y is the average value of yi (i=1-n).

[0028] Three arbitrary points are selected multiple times on the contour line 10L of the silicon nitride particle 10, and it is verified whether the three points satisfy all of the above conditions (i) to (iii), thereby identifying multiple "sides." Note that if none of the above conditions (i) to (iii) are satisfied no matter how the three points are selected, the silicon nitride particle 10 is determined to have no "sides."

[0029] Two sides are selected from a plurality of sides, and if the angle between the two sides is less than 2°, the two sides are deemed to be parallel. However, the two sides are selected so that the silicon nitride particle 10 is sandwiched between the two sides. In other words, when the two sides are selected, the two sides are selected on the premise that the set range of three points set to define one side does not overlap with the set range of three points set to define the other side. When drawing the sides, it is desirable to perform the operation to draw the sides around the position on the contour line 10L of the silicon nitride particle 10 where two parallel sides are expected to be drawn.

[0030] A silicon nitride particle 10 having an outline (outline 10L) including two parallel sides is referred to as a "first silicon nitride particle."

[0031] One hundred silicon nitride particles present in a planar image (e.g., an SEM image) are selected, and the area of ​​each of these 100 silicon nitride particles (the area of ​​the region surrounded by the outline 10L in FIG. 1 ) is determined, and each silicon nitride particle is analyzed to determine whether it is a "first silicon nitride particle." The total area of ​​the 100 silicon nitride particles (total area St of silicon nitride particles) and the total area of ​​those silicon nitride particles that correspond to "first silicon nitride particles" (total area S1 of first silicon nitride particles) are then determined. The proportion of the area occupied by the first silicon nitride particles (area ratio) is calculated from these total areas St and S1 and the following formula (3): Area ratio (%) of first silicon nitride particles = S1 / St × 100 (3)

[0032] In the silicon nitride powder according to this embodiment, the area ratio of the first silicon nitride particles is more than 1.2% and less than 100%. When the area ratio of the first silicon nitride particles is within this range, it is presumed that when used as a filler for a resin composition, a resin composition with high thermal diffusivity can be obtained for the following reasons.

[0033] It can be assumed that first silicon nitride particles having an outer shape including two parallel sides in a planar view (two-dimensional) also have a flat surface in a three-dimensional shape (three-dimensional). Therefore, when silicon nitride powder is used as a filler for a resin composition, first silicon nitride particles having an outer shape including two parallel sides can contact adjacent silicon nitride particles at a flat surface corresponding to one of the two sides. When adjacent silicon nitride particles also have sides in a planar view (i.e., have a flat surface in a three-dimensional shape), the contact area between particles can be increased. In particular, when the area ratio of the first silicon nitride particles is high (i.e., when the proportion of first silicon nitride particles in the silicon nitride powder increases), the probability that two adjacent silicon nitride particles are both first silicon nitride particles increases. When two adjacent silicon nitride particles are both first silicon nitride particles, the sides (three-dimensional flat surfaces) of each particle in a planar view can come into contact with each other, further increasing the contact area. As a result, the number of thermal diffusion paths in the resin composition increases, and a resin composition with high thermal diffusivity can be obtained.

[0034] Furthermore, adjacent silicon nitride particles are more likely to move along the sides of the first silicon nitride particles, which can improve the filling rate of the silicon nitride powder in the resin composition. However, if adjacent silicon nitride particles are all first silicon nitride particles, the sides of each particle may adhere to each other, which may actually hinder their movement. As a result, the filling rate of the silicon nitride powder in the resin composition may decrease.

[0035] In order to increase the thermal diffusion paths in the resin composition while improving the filling rate of the silicon nitride powder in the resin composition, in the silicon nitride powder of this embodiment, the area ratio of the first silicon nitride particles is specified to be more than 1.2% and less than 100%, preferably 2.0% or more and 80.0% or less, more preferably 3.0% or more and 50.0% or less, even more preferably 5.0% or more and 30.0% or less, still more preferably 10.0% or more and 29.0% or less, and particularly preferably 14.0% or more and 25.0% or less.

[0036] (Apparent density) The apparent density of silicon nitride powder is 3.17 g / cm 3 More preferably, it is greater than 3.18 g / cm3 More preferably, it is 3.19 g / cm 3 This results in a silicon nitride powder containing many silicon nitride particles with a small amount of internal voids, that is, a silicon nitride powder with high thermal diffusivity and thermal conductivity. The upper limit of the apparent density is, for example, 3.44 g / cm 3 In addition, if the apparent density is not too high, it is expected that the powder will be less likely to settle when mixed with a resin and will be easier to disperse. In order to achieve such an effect, the apparent density of the silicon nitride powder should be 3.30 g / cm 3 It is preferable that the density is 3.25 g / cm or less, and more preferably 3.25 g / cm 3 The following is the result.

[0037] The apparent density of silicon nitride particles is measured by the pycnometer method in accordance with JIS R 1620:1995. The measurement is carried out five or more times, and the average value is taken as the apparent density of the silicon nitride powder. For the measurement, for example, an Accupyc 1330 (Micromeritics) can be used.

[0038] (Surface roughness Ra) The surface roughness Ra (arithmetic mean roughness) of the silicon nitride powder is preferably less than 0.97 nm. If the surface roughness Ra is less than 0.97 nm, aggregation of silicon nitride particles is suppressed when the silicon nitride is mixed with a resin, allowing the silicon nitride to be dispersed in the resin and highly packed. The surface roughness Ra is preferably less than 0.97 nm, more preferably 0.95 nm or less, even more preferably less than 0.93 nm, still more preferably 0.90 nm or less, even more preferably 0.80 nm or less, and particularly preferably 0.75 nm or less.

[0039] To measure the surface roughness Ra, a 100 nm x 100 nm measurement area on the surface of any silicon nitride particle is observed using a scanning probe microscope (SPM). The surface roughness Ra is calculated from the obtained shape image. The surface roughness Ra is measured for four silicon nitride particles, and the average value is taken as the surface roughness Ra of the silicon nitride powder.

[0040] (Average aspect ratio of silicon nitride particles) The average aspect ratio of the minor axis to the major axis of the silicon nitride particles contained in the silicon nitride powder is preferably greater than 0.50, more preferably 0.55 or more, even more preferably greater than 0.60, and even more preferably 0.65. On the other hand, the average aspect ratio of the silicon nitride particles is preferably less than 0.87, more preferably 0.86 or less, and even more preferably 0.85 or less. When the average aspect ratio of the silicon nitride particles is within an appropriate range, the filling rate of the silicon nitride powder in the resin composition can be further improved, and the number of thermal diffusion paths in the resin composition can be further increased, resulting in a resin composition with a higher thermal diffusivity.

[0041] The average aspect ratio of silicon nitride particles is measured as follows. SEM images of silicon nitride particles contained in silicon nitride powder are analyzed using image processing software (e.g., Image J (manufactured by the National Institute of Health)). The maximum particle size of the silicon nitride particles (referred to as the "major axis") is identified, and the particle size in the direction perpendicular to the major axis is referred to as the "minor axis". The major and minor axes are measured for 20 random silicon nitride particles, and the ratio of the minor axis to the major axis (minor axis / major axis) is determined for each particle. The arithmetic mean value of these ratios is taken as the average aspect ratio of the silicon nitride particles.

[0042] (β-phase ratio) The β-phase ratio of the silicon nitride powder is preferably 65% ​​or more. A β-phase ratio of 65% or more can improve the thermal diffusivity of the silicon nitride particles and the resin composition. The β-phase ratio is more preferably 70% or more, even more preferably 80% or more, even more preferably 85% or more, and particularly preferably 90% or more.

[0043] In this specification, the "β-phase ratio" refers to the content (volume %) of β-type silicon nitride relative to all silicon nitrides contained in the silicon nitride powder.

[0044] In calculating the β-phase ratio, the silicon nitride powder was measured by powder X-ray diffraction, and the diffraction pattern was analyzed by the Gazzara & Messier method (G.P. Gazzara and D.P. Messier, "Determination of Phase Content of Si 3 N 4 The β-phase ratio is calculated by analyzing the β-phase by X-ray Diffraction Analysis, Am. Ceram. Soc. Bull., 56[9]777-80 (1977)).

[0045] (The maximum particle size of silicon nitride particles having a ratio (L2 / L1) of the total length L2 of the internal boundaries to the outer edge length L1 of 1% or less is 6.8 μm or more.) The fewer grain boundaries and cavities there are inside the silicon nitride particles, the more this can contribute to improving the thermal diffusivity of the silicon nitride particles. Therefore, the ratio (L2 / L1) of the total length L2 of the boundaries to the outer edge length L1 is introduced as an indicator of the content of grain boundaries inside the silicon nitride particles. L1 and L2 are determined by observing the cross section of the silicon nitride particle. Note that here, "grain boundary" and "boundary line" refer to boundaries (also called high-angle grain boundaries) where, as a result of EBSD analysis, the crystal orientation misorientation (oblique angle) exceeds 15°.

[0046] When the length of the outer edge of one silicon nitride particle is L1 and the total length of the boundary lines of that silicon nitride particle is L2, silicon nitride particles with a small L2 / L1 value are said to have a low content of boundary lines. In this embodiment, silicon nitride particles with an L2 / L1 ratio of 1% or less are considered to be silicon nitride particles made of a single crystal (referred to as "single crystal particles"). Single crystal particles have a high thermal diffusivity, so they are likely to improve thermal diffusivity when used as a filler for resin compositions.

[0047] In this embodiment, the maximum particle size of silicon nitride particles having an L2 / L1 ratio of 1% or less (i.e., single crystal) is preferably 6.8 μm or more, more preferably 7.0 μm or more, even more preferably 10.0 μm or more, still more preferably 15.0 μm or more, even more preferably 40.0 μm or more, and particularly preferably 60.0 μm or more. Such silicon nitride particles form long heat conduction paths when filled into a resin, thereby improving the thermal diffusivity of the resin composition.

[0048] (Particle diameter D50 of the cumulative 50% from the fine particle side of the cumulative particle size distribution on a volume basis) The silicon nitride powder preferably has a particle diameter D50 of the cumulative 50% from the fine particle side of the cumulative particle size distribution on a volume basis (hereinafter simply referred to as "D50") of 1.5 μm or more, more preferably 2.0 μm or more, even more preferably 3.0 μm or more, still more preferably 10.0 μm or more, and particularly preferably 30 μm or more. The upper limit is not particularly limited, but is, for example, preferably 500.0 μm or less, more preferably 300.0 μm or less, and even more preferably 200.0 μm or less.

[0049] The D50 of silicon nitride powder is measured by laser diffraction. Specifically, the powder is dispersed in water and irradiated with a laser beam, and the diffraction is measured to determine the particle size. A measuring device such as the 1090L manufactured by CILAS can be used.

[0050] [Method for Producing Silicon Nitride Powder] A method for producing silicon nitride powder according to an embodiment of the present invention will be described. The method for producing silicon nitride powder includes the steps of: (1) synthesizing silicon nitride synthetic crystals by combustion synthesis in a nitrogen atmosphere using raw materials containing Si; (2) crushing the silicon nitride synthetic crystals to obtain coarsely pulverized silicon nitride powder; and (3) finely pulverizing the coarsely pulverized silicon nitride powder to obtain finely pulverized silicon nitride powder. Optionally, the method may further include the step of: (4) heat-treating the finely pulverized silicon nitride powder.

[0051] Step (1): Synthesizing silicon nitride composite crystals. For example, Si powder is used as the raw material containing Si. The average particle diameter D50 of the raw material is, for example, within the range of 2 to 10 μm. This allows the amount of oxygen impurities to be suppressed, and the combustion rate to be increased, allowing for a higher synthesis temperature, resulting in good crystal growth. As an example, the average particle diameter D50 of Si is 5 μm.

[0052] The diluent is used to adjust the amount of Si in the raw materials. A separately prepared silicon nitride powder is used as the diluent. The diluent may be either α-type silicon nitride powder or β-type silicon nitride powder, or a mixture of these. The average particle diameter D50 of the diluent is preferably in the range of 0.5 to 2.0 μm. As an example, the average particle diameter D50 of the diluent is 1.0 μm. The amount of diluent added is less than 10 mass% of the total raw materials (including the diluent). As an example, the diluent is added in an amount of 5 to 8 mass% of the total raw materials. By adding the amount of diluent within the above range, a predetermined amount of silicon nitride particles having an outer shape including two parallel sides in a planar view can be produced.

[0053] In this embodiment, a diluent is mixed with the raw materials and then filled into an insulated heat-resistant container. This insulated heat-resistant container has a thermal conductivity of 1 W / mK or less, and although alumina or zirconia can be used as the material, carbon is preferred to prevent impurities from being mixed in. After the raw materials are filled, the container is covered with a lid made of the same material as the insulated heat-resistant container. Furthermore, to increase the temperature inside the composite during combustion, the thickness of the mixed raw materials is set to more than 100 mm, preferably more than 100 mm and 150 mm or less. Combustion synthesis is performed in a nitrogen atmosphere in the range of 0.5 to 1 MPa (e.g., 0.9 MPa). Adjusting the pressure range within this range enables efficient synthesis while suppressing increases in equipment costs.

[0054] When the mixed raw material is filled into the crucible, a layer of powder (silicon nitride) having a thickness of 1 mm to 80 mm is spread on the bottom and sides of the crucible, the mixed raw material is then filled, and the top surface is further covered with a layer of powder having a thickness of 1 mm to 80 mm. By covering the entire surface with the powder, the mixed raw material can be kept warm, and a predetermined amount of silicon nitride particles having an outer shape including two parallel sides in a plan view can be produced.

[0055] To promote crystal growth more effectively, a catalyst may be used, for example, Y 2 O 3 , Fe 2 O 3 , CaO, Ni, Co, C, etc. are added in an amount of about 0.01 to 0.1 mass %. In addition, external auxiliary heating is performed in the range of 500°C to 1700°C (for example, 1500°C), and the combustion temperature is also increased in the combustion synthesis method by self-ignition.

[0056] Step (2): Obtaining a coarsely pulverized silicon nitride powder. The silicon nitride composite crystal is in the form of an agglomeration of multiple silicon nitride particles. In step (2), the silicon nitride composite crystal is crushed to obtain a coarsely pulverized silicon nitride powder. For example, the composite is crushed using a common crushing device such as a hammer mill or a disk mill until it passes through a sieve with a specified mesh size (for example, a sieve with mesh sizes in the range of 400 μm to 500 μm).

[0057] Step (3): Step of Obtaining Finely Pulverized Silicon Nitride Powder The coarsely pulverized silicon nitride powder is further pulverized to obtain a finely pulverized silicon nitride powder. The pulverization is carried out using a pulverizing device such as a jet mill or a ball mill. If necessary, the resulting finely pulverized powder may be classified. Classification may be carried out by sieving, wet classification, or the like. The resulting finely pulverized powder may be used as is as the silicon nitride powder, or may be subjected to a heat treatment step (step (4) described below) before use as the silicon nitride powder.

[0058] Step (4): Heat-treating the finely pulverized silicon nitride powder. Optionally, the finely pulverized silicon nitride powder may be heat-treated. Heat treatment forms an oxide film on the surface of the silicon nitride particles, which has the effect of chemically stabilizing the silicon nitride particles. The heat treatment is carried out, for example, in air at a temperature of 500°C or higher and 1200°C or lower. The heat treatment time can be adjusted appropriately according to the heat treatment temperature. The heat treatment time is, for example, 5 hours.

[0059] In the method for producing silicon nitride powder, silicon nitride synthetic crystals are synthesized using the heat generated by combustion synthesis, and then the silicon nitride powder according to this embodiment can be produced by crushing, classifying, and pulverizing the synthesized crystals.

[0060] [Resin composition] By using the silicon nitride powder according to the embodiment of the present invention as a filler for a resin composition, a resin composition with high thermal diffusivity can be obtained. The resin composition contains a resin and the silicon nitride powder according to the embodiment of the present invention.

[0061] Resin compositions containing silicon nitride powder according to embodiments of the present invention have high thermal diffusivities, and the blending ratios can be appropriately determined depending on the purpose and application. For example, the resin composition (composite) may contain 5 to 75 volume % of resin and 95 to 25 volume % of silicon nitride powder. The filling rate of the silicon nitride powder in the resin composition refers to the content (volume %) of silicon nitride powder when the volume of the resin composition (including the silicon nitride powder) is taken as 100 volume %.

[0062] A method for producing a resin composition will be described. A resin composition can be obtained by mixing silicon nitride powder and a resin using a commonly used known method. For example, when the resin is liquid (e.g., liquid epoxy resin), the resin composition can be obtained by mixing the liquid resin, silicon nitride powder, and a curing agent, and then curing the mixture with heat or ultraviolet light. Known curing agents, mixing methods, and curing methods can be used. On the other hand, when the resin is solid, the desired resin composition can be obtained by mixing the silicon nitride powder and the resin, and then kneading the mixture using a known method such as melt kneading.

[0063] The resin used in the resin composition can be a known resin such as an epoxy resin. The type of resin can be selected from thermoplastic resins, thermoplastic elastomers, and thermosetting resins. The resins can be used alone or in combination of two or more.

[0064] Furthermore, these resin compositions may contain, as needed, known additives such as plasticizers, curing accelerators, coupling agents, fillers, pigments, flame retardants, antioxidants, surfactants, compatibilizers, weather resistance agents, antiblocking agents, antistatic agents, leveling agents, and release agents, either singly or in combination, within the scope of the invention.

[0065] The silicon nitride powder according to the embodiment and the resin composition containing the silicon nitride powder are particularly suitable for use as heat-dissipating materials. Thus, one aspect of the present disclosure can provide a heat-dissipating silicon nitride powder and a heat-dissipating resin composition.

[0066] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples carried out to clarify the effects of the embodiments of the present invention. However, the embodiments of the present invention are not limited to the following examples.

[0067] <Preparation of Silicon Nitride Powder> (Samples No. 1-3) Si powder (particle diameter = 5 μm) and silicon nitride powder (particle diameter = 1 μm) prepared separately as a diluent were mixed in a tumbling ball mill. The amount of diluent added was 5-8 mass% of the total raw material (including diluent). The mixed powder was packed into a carbonaceous, heat-resistant container with a layer of powder 1 mm to 80 mm thick on the bottom and sides, so that the raw material layer was thicker than 100 mm and not more than 150 mm. The raw material layer was then covered with a layer of powder 1 mm to 80 mm thick. A lid made of a carbonaceous, heat-resistant material was then placed in the container, and synthesis was carried out under a nitrogen atmosphere at 0.9 MPa. After synthesis, the mixture was coarsely crushed (disintegrated) in a mortar until it passed through a sieve with the specified mesh size. The mesh size of the sieve for each sample is shown in Table 1.

[0068] The obtained coarsely pulverized powder was further finely pulverized using a nanojetmizer (manufactured by Aisin Nano Technologies Co., Ltd.). A nanojetmizer with the model number listed in Table 1 was used for the fine pulverization. The obtained finely pulverized powder was classified using the method listed in Table 1. Note that classification was not performed for Sample No. 2. The obtained classified powders (Samples No. 1 and No. 3) and finely pulverized powder (Sample No. 2) were then placed in an alumina crucible and heat-treated in an air atmosphere using a small powder programmable electric furnace (MMF series, manufactured by AS ONE) under the conditions (heat treatment temperature, heat treatment time) listed in Table 1 to obtain silicon nitride powders (Samples Nos. 1 to 3).

[0069] (Samples Nos. 5 to 10) Coarsely pulverized powders were prepared in the same manner as in "Samples Nos. 1 to 3" above. The sieve used during coarse pulverization (disintegration) had a mesh size of 500 μm. The obtained coarsely pulverized powders were then finely pulverized in a ball mill. The obtained finely pulverized powders were sieved using a vibrating sieve according to the following procedure, and then further wet-classified to obtain silicon nitride powders (Samples Nos. 5 to 10) having the desired D50. - Sample No. 5: Silicon nitride particles remaining on a sieve with a mesh size of 150 μm (D50: 192.0 μm) - Sample No. Sample No. 6: When sieving using a 150 μm sieve, the powder remaining below the sieve was further sieved using a 106 μm sieve, and the silicon nitride particles remaining on the sieve (D50 was 118.0 μm). Sample No. 7: When sieving using a 106 μm sieve, the powder remaining below the sieve was further sieved using a 75 μm sieve, and the silicon nitride particles remaining on the sieve (D50 was 83.0 μm). Sample No. 8: When sieving using a 75 μm sieve, the powder remaining below the sieve was further sieved using a 63 μm sieve, and the silicon nitride particles remaining on the sieve (D50 was 58.0 μm). Sample No. Sample No. 9: Silicon nitride particles remaining under the sieve when sieved using a 63 μm sieve (D50 is 22.0 μm). Sample No. 10: Silicon nitride particles remaining under the sieve when sieved using a 63 μm sieve and then sieved using a 10 μm sieve (D50 is 3.5 μm).

[0070]

[0071] Various measurements were performed on the obtained Samples Nos. 1 to 3 and 5 to 10 (Examples) and, as a comparative example, a commercially available silicon nitride powder (manufactured by Aldrich, silicon nitride (predominantly β-phase, ≦10 micron primary particle size, product code 248622); hereinafter referred to as "Sample No. 4").

[0072] (1) Measurement of the β-phase ratio of silicon nitride powder A diffraction pattern of the sample (silicon nitride powder) was obtained using a powder X-ray diffractometer (manufactured by Rigaku Denki). The measurement conditions were as follows: X-ray source: CuKα radiation X-ray output: 45 kV, 200 mA Graphite monochromator Diffraction angle (2θ): Step scan in 0.02° increments over the range of 2 to 90° Scanning speed: 21.7 deg / min

[0073] When a sample contained components other than silicon nitride, the peaks of those components were compared with the corresponding peaks of standard samples of those components to determine the proportions of those components. For Samples No. 1 to 10, the powder X-ray diffraction patterns obtained confirmed that the samples were composed solely of α-type silicon nitride and β-type silicon nitride. The proportion of β-type silicon nitride in the sample (β-conversion ratio) was then calculated using the Gazzara & Messier method.

[0074] (2) Maximum particle size of silicon nitride particles with an L2 / L1 ratio of 1% or less (maximum particle size of single-crystal particles) A ​​sample for cross-sectional observation was prepared using the sample (silicon nitride particles). To prepare the sample for cross-sectional observation, the silicon nitride particles were embedded in resin, and then the resin and silicon nitride particles were cut using a diamond cutter. Subsequently, a protective film of platinum was vapor-deposited on the cross-section, and the cross-section was prepared by Ar ion milling. The sample was then fixed to the SEM sample stage with Cu double-sided tape, and SEM-EBSD measurement was performed without vapor deposition. The observation position was determined so that two or more silicon nitride particles were completely contained within the observation region (i.e., two or more silicon nitride particles did not come into contact with the frame of the observation region). Measurements were performed using β-type silicon nitride particles.

[0075] The following equipment was used for sample pretreatment and EBSD measurement: Equipment used Ion milling equipment: E-3500 (manufactured by Hitachi High-Tech Corporation) Ion sputtering equipment: E-1030 (manufactured by Hitachi, Ltd.) Schottky scanning electron microscope: SU5000 (manufactured by Hitachi High-Tech Corporation) Backscattered electron diffraction equipment: Velocity (manufactured by METEK Corporation)

[0076] The conditions for the EBSD measurement were as follows: Measurement area: 500.0 μm×400.0 μm Acceleration voltage: 15.0 kV Magnification: ×500 Vacuum degree: 30 Pa

[0077] In the obtained EBSD image, two or more silicon nitride particles that were not in contact with the frame of the observation area were selected, and the average of the outer edge length L1 of each silicon nitride particle was calculated using image processing software Image J (manufactured by the National Institute of Health). The total length L2 of the boundary lines was also calculated. The "total length L2 of the boundary lines" is the sum of the boundary lines contained within the silicon nitride particle and does not include the outer edge of the silicon nitride particle. The total length L2 of the boundary lines was calculated by adding the total length of the grain boundaries within the silicon nitride particle and the total length of the inner walls of the cavities (if any) within the silicon nitride particle.

[0078] This measurement was carried out once for 20 random silicon nitride particles, and silicon nitride particles with an L2 / L1 ratio of 1% or less were considered to be single crystal particles, and the length of their major axis was measured and recorded as the "maximum particle size of the single crystal particles." If the 20 silicon nitride particles measured contained multiple single crystal particles, the arithmetic average of their maximum particle sizes was calculated.

[0079] (3) Apparent Density of Silicon Nitride Powder The apparent density of the sample (silicon nitride powder) was measured in accordance with JIS R 1620:1995. The measurement method and conditions were as follows: Measurement method: Gas substitution method Sample drying: 200°C, 8 hours or more Apparatus used: Accupyc 1330 (Micromeritics) Measurement conditions Number of purges: 10 Purge filling pressure: 15.0 psig Number of measurements: 5 Measurement filling pressure: 15.0 psig Equilibrium pressure: 0.005 psig / min Measurement with set precision: Yes Allowable error of variation: 0.05% Sample cell size: 10 cm 3

[0080] (4) Average aspect ratio of silicon nitride particles SEM images of the sample (silicon nitride powder) were taken. The following equipment was used for taking the images. Equipment used: Scanning electron microscope: JSM-IT200 (manufactured by JEOL Ltd.) The imaging conditions were as follows: Acceleration voltage: 5.0 kV Signal: SED Probe current: Std. -PC55 Magnification: 1000x

[0081] The SEM images were processed using image processing software Image J (manufactured by the National Institute of Health), and the aspect ratios of 20 randomly selected silicon nitride particles in the SEM images were determined. The maximum diameter of the silicon nitride particles was taken as the major axis, and the particle size in the direction perpendicular to the major axis was taken as the minor axis. The major and minor axes of 20 randomly selected silicon nitride particles were measured, and the ratio of the minor axis to the major axis (minor axis / major axis) was determined for each particle. The arithmetic mean value of these ratios was taken as the average aspect ratio of the silicon nitride particles (referred to as "aspect ratio" in the table).

[0082] (5) Area Ratio of First Silicon Nitride Particles The SEM images obtained in "(4) Average Aspect Ratio of Silicon Nitride Particles" were analyzed to confirm whether 100 random silicon nitride particles were silicon nitride particles (first silicon nitride particles) with an outer shape including two parallel sides. Whether or not the particles had an "outer shape including two parallel sides" was determined using FIG. 1 and the method described above. The area of ​​each of the 100 silicon nitride particles was measured. The total area St of the 100 silicon nitride particles and the total area S1 of the first silicon nitride particles were calculated, and the proportion of the area occupied by the first silicon nitride particles (area ratio) was calculated using the following formula (3). Area ratio of first silicon nitride particles (%) = S1 / St × 100 (3)

[0083] (6) Measurement of surface roughness Ra A scanning probe microscope SPA300HV manufactured by Seiko Instruments Inc. was used to measure the surface roughness Ra. The measurement conditions were as follows: Probe station / unit SPI4000 / SPA300HV Cantilever: SI-DF20 Scanner: 20 μm Data type: Topographic image Observation mode: DFM (Dynamic Force Mode Microscope) Scanning area: 100 nm x 100 nm Scanning frequency: 0.25 Hz Analysis software: (attached to the measuring device)

[0084] Five silicon nitride particles were randomly selected from the image, and a measurement area of ​​100 nm × 100 nm on the surface of each particle was observed using a scanning probe microscope (SPM). The surface roughness Ra of each particle was calculated from the obtained shape image, and the average value was taken as the surface roughness Ra of the silicon nitride powder.

[0085] (7) Measurement of D50 of silicon nitride powder The particle size distribution of the sample (silicon nitride powder) was measured, and the cumulative 50% particle size D50 was determined. The particle size distribution of the silicon nitride powder was measured by laser diffraction. A sample dispersed in water was irradiated with a laser beam, and the diffraction was measured to determine the particle size. The measuring device used was a CILAS 1090L model. The particle size was taken as the circle-equivalent particle size. The circle-equivalent particle size is the particle size of a perfect circle that has the same area as a projected particle image. The particle size was measured by volume.

[0086] (8) Measurement of thermal diffusivity of resin composition (composite) Epoxy resin (main agent: room temperature curing potting resin 53 type (manufactured by Sankei Co., Ltd.) 010-8140, curing agent: room temperature curing potting resin 53 type (manufactured by Sankei Co., Ltd.) 010-8143) and a sample (silicon nitride powder) were mixed in a blending ratio (volume ratio) of 50:50, and the mixture was stirred and mixed using a Foam Mixer (manufactured by Thinky Corporation) to obtain an epoxy resin-filler (silicon nitride powder) composite. The filling rate of the silicon nitride powder in the resin composition was 50% by volume.

[0087] A 1 mm thick aluminum plate with a 1 cm x 10 cm rectangular hole was prepared as a mold frame. A PET film (back side film) coated with a release agent was attached to the back side of the mold frame so as to cover the rectangular hole, with the release agent-coated surface facing the mold frame. After the stirred composite was poured into the rectangular hole of the mold frame, a PET film (front side film) coated with a release agent was attached on top of it, with the release agent-coated surface facing the mold frame and resin composition. Furthermore, light pressure was applied from above with a metal roller to fit the composite into the rectangular hole of the mold frame. Another aluminum plate was placed on top of the front side film, and the composite was cured by heating at 100°C for 1 hour. After curing was complete, the aluminum plate was allowed to cool, and when the temperature of the aluminum plate had dropped to approximately room temperature, the aluminum plate was removed. The PET films on the front and back sides of the cured composite were then peeled off, respectively, to obtain a sheet-like sample for measuring thermal diffusivity.

[0088] The thermal diffusivity of the obtained sheet-like sample was measured. Measurement specimens measuring 10 mm in length, 10 mm in width, and 1 mm in thickness were prepared from the sheet-like sample of the resin composition described above, and the thermal diffusivity was measured at room temperature using temperature wave thermal analysis (TWA). The measurement device used was an iPhase Mobile manufactured by iPhase Corporation. The thermal diffusivity was measured at three random points on one measurement specimen, and the average value was calculated from the measurement results of the three points.

[0089] (9) Maximum Filling Rate Using the method described in "(8) Measurement of Thermal Diffusivity of Resin Composition (Composite)," resin compositions were prepared by varying the compounding ratio (volume ratio) of epoxy resin to sample from 50:50 to 30:70, and sheets were then produced. If the compounding ratio of the sample was excessively high, voids with a diameter of 1 mm or more would appear in the sheet, but the upper limit of the compounding ratio of the sample within the range where such voids were not visible by visual observation (i.e., the upper limit of the filling rate of silicon nitride powder in the resin composition) was defined as the maximum filling rate.

[0090] The measurement results are summarized in Tables 2 and 3.

[0091]

[0092]

[0093] The measurement results are discussed below. Composites using silicon nitride powders of Samples 1 to 3 and 5 to 10, which satisfied the requirements of this embodiment, exhibited excellent thermal diffusivity. On the other hand, composites using silicon nitride powder of Sample 4, which did not satisfy the requirements of this embodiment, exhibited poor thermal diffusivity. Furthermore, although the silicon nitride powders of Samples 1 to 3 and 5 to 10 had smaller aspect ratios and were expected to have lower maximum packing fractions than the silicon nitride powder of Sample 4, they exhibited the same maximum packing fraction as the comparative example. This is thought to be because the surface roughness of the silicon nitride powders of Samples 1 to 3 and 5 to 10 was smaller than that of the silicon nitride powder of Sample 4, and therefore, despite the smaller aspect ratios, they exhibited the same maximum packing fraction and were not inferior in packing properties.

[0094] This application claims priority from Japanese Patent Application No. 2023-058712, filed March 31, 2023. Japanese Patent Application No. 2023-058712 is incorporated herein by reference.

Claims

1. A silicon nitride powder comprising silicon nitride particles including first silicon nitride particles having an outer shape including two parallel sides in a planar view, wherein when the total area of ​​all of the silicon nitride particles in the planar view is taken as 100%, the proportion of the area occupied by the first silicon nitride particles is greater than 1.2% but less than 100%.

2. Apparent density is 3.17 g / cm 3 The silicon nitride powder of claim 1, wherein the silicon nitride powder has a molecular weight of 1.0 or more.

3. The silicon nitride powder according to claim 1, having a surface roughness Ra of less than 0.97 nm.

4. The silicon nitride powder according to claim 1, wherein the silicon nitride particles have an average aspect ratio of the minor axis to the major axis greater than 0.

50.

5. The silicon nitride powder according to claim 1, having a beta-conversion rate of 65% or more.

6. The silicon nitride powder according to claim 1, wherein the maximum particle size of silicon nitride particles having a ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge of the silicon nitride particles is 6.8 μm or more.

7. A resin composition comprising a resin and the silicon nitride powder according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Silicon nitride powder, silicon nitride sintered compact, and circuit board for electronic component using the sintered compact

    JP2004262756A

  • Manufacturing method of silicon nitride powder

    JP2017066017A

  • Production method of silicon nitride sintered body, silicon nitride sintered body, and heat radiation substrate using the same

    JP2019006673A

  • Method of producing high purity silicon nitride powder