Silicon nitride powder and resin composition using same
The development of silicon nitride powder with controlled oxygen localization and surface characteristics addresses the water resistance issue in resin compositions, enhancing the water resistance and preventing dielectric breakdown in electronic components.
Patent Information
- Application Number
- PCT/JP2024/006300
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-02-21
- Publication Date
- 2024-10-03
AI Technical Summary
Existing resin compositions using silicon nitride powder lack water resistance due to the reactivity of silicon nitride with moisture, leading to potential dielectric breakdown, as the water resistance of silicon nitride powder is not adequately considered in previous technologies.
A silicon nitride powder with specific surface characteristics, including controlled oxygen localization on the particle surface, is developed to enhance water resistance, characterized by a narrow oxygen localization index, high surface oxygen rate, and optimized specific surface area, which is then used as a filler in resin compositions.
The silicon nitride powder exhibits improved water resistance, effectively preventing dielectric breakdown when used in resin compositions, ensuring reliable heat dissipation in electronic components.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Silicon nitride powder and resin composition using same
[0001] The present disclosure relates to a silicon nitride powder and a resin composition using the same.
[0002] Heat generated by passing current through an electronic component is dissipated via a heat sink. To improve heat dissipation efficiency, a technique for filling the space between the electronic component and the heat sink with a heat dissipation material is known. One heat dissipation material is a resin composition containing a resin and inorganic particles, and it is known that silicon nitride powder can be used as the inorganic particles (see, for example, Patent Document 1).
[0003] Furthermore, Patent Document 2 discloses silicon nitride powder for use in another application, which has an internal oxygen content of 0.6 mass % or less, as a silicon nitride powder from which a silicon nitride sintered body having high thermal conductivity can be obtained.
[0004] JP 2022-522814 A International Publication No. 2020 / 203695
[0005] When a resin composition comes into contact with moisture, ammonia may be generated by hydrolysis of the silicon nitride powder in the resin composition. Because ammonia may cause dielectric breakdown in the resin composition, silicon nitride powder used as a filler in the resin composition is required to have low reactivity with water (i.e., water resistance). However, Patent Documents 1 and 2 do not consider the water resistance of silicon nitride powder at all.
[0006] In view of these circumstances, one embodiment of the present invention aims to provide a silicon nitride powder for use as a filler for resin compositions, which silicon nitride powder is water-resistant. Furthermore, another embodiment of the present invention aims to provide a resin composition using the silicon nitride powder according to one embodiment.
[0007] A first aspect of the present invention is a silicon nitride powder containing a plurality of silicon nitride particles, which satisfies the following formula (1): 0%≦|X−Y| / Y×100<240.0% (1), where X (nm) is the SiO converted from the total oxygen content TO (mass%) of the silicon nitride powder. 2 Y (nm) is the thickness of the coating, and Y (nm) is the SiO2 calculated from the surface oxygen ratio SO (atom%) of the silicon nitride particles. 2 The thickness of the coating.
[0008] A second aspect of the present invention is the silicon nitride powder according to the first aspect, which satisfies the following formula (2): 0<X (nm)<50.0 (2)
[0009] A third aspect of the present invention is the silicon nitride powder according to the first or second aspect, which satisfies the following formula (3): SO (atom %) / SA (m 2 / g)>10.1 (atom% / (m 2 / g)) (3) where SA(m 2 / g) is the specific surface area of the silicon nitride powder.
[0010] A fourth aspect of the present invention is the silicon nitride powder according to any one of the first to third aspects, wherein the total oxygen content TO (mass%) of the silicon nitride powder satisfies the following formula (4): TO (mass%)<1.21 (4)
[0011] A fifth aspect of the present invention is the silicon nitride powder according to any one of the first to fourth aspects, wherein the surface oxygen ratio SO (atom %) of the silicon nitride particles satisfies the following formula (5): SO (atom %)>10.0 (5)
[0012] In the sixth aspect of the present invention, the specific surface area is 2.66 m 2 6. The silicon nitride powder according to any one of Aspects 1 to 5, wherein the silicon nitride powder has a surface roughness of less than 1 / g.
[0013] A seventh aspect of the present invention is the silicon nitride powder according to any one of the first to sixth aspects, wherein the silicon nitride powder has a surface roughness Ra of less than 0.97 nm.
[0014] Aspect 8 of the present invention is the silicon nitride powder according to any one of Aspects 1 to 7, wherein the β-phase ratio is 65% or more.
[0015] A ninth aspect of the present invention is the silicon nitride powder according to any one of aspects 1 to 8, wherein the ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge is 1% or less, and the maximum particle size of the silicon nitride particles is 6.8 μm or more.
[0016] A tenth aspect of the present invention is a resin composition comprising a resin and the silicon nitride powder according to any one of the first to ninth aspects.
[0017] The silicon nitride powder according to one embodiment of the present invention can exhibit sufficient water resistance by controlling the ratio of the amount of oxygen present on the particle surface to the amount of oxygen present in the entire powder. Also, a resin composition according to another embodiment of the present invention can exhibit high water resistance because it uses the silicon nitride powder according to one embodiment.
[0018] [Silicon nitride powder] The present inventors conducted extensive research to obtain a silicon nitride powder that can achieve excellent water resistance. They discovered that silicon nitride powder with excellent water resistance can be obtained by significantly localizing oxygen on the surface of the silicon nitride particles that make up the silicon nitride powder. To indirectly determine the water resistance of silicon nitride powder, the present inventors introduced a new index that indicates the degree of surface oxygen localization, and based on this index, they were able to obtain silicon nitride powder with high water resistance.
[0019] The characteristics of the silicon nitride powder according to the embodiment of the present invention will be described below.
[0020] The silicon nitride powder according to the embodiment contains a plurality of silicon nitride particles and further satisfies the following formula (1): 0%≦|X−Y| / Y×100<240.0% (1), where X (nm) is the SiO converted from the total oxygen content TO (mass%) of the silicon nitride powder. 2 Y (nm) is the thickness of the coating, and Y (nm) is the SiO2 calculated from the surface oxygen ratio SO (atom%) of the silicon nitride particles. 2 The method for calculating the thicknesses X and Y will be described in detail later.
[0021] The "|X-Y| / Y x 100" (%) in the middle of formula (1) is a new index that indicates the degree to which oxygen is localized on the surface of silicon nitride particles. This is called the "oxygen localization index." The thickness X is calculated from the total oxygen content TO (mass%) of the silicon nitride powder. 2 The thickness of the coating is the thickness of the silicon nitride particle. When a large amount of oxygen is contained inside the silicon nitride particle, the thickness X becomes large. The thickness Y is calculated from the content of oxygen (surface oxidation rate SO) contained in the surface of the silicon nitride particle (up to a depth of about 10 nm). 2 Even if a large amount of oxygen is contained inside the silicon nitride particles (excluding the surface), the effect on the thickness Y is small.
[0022] The closer the values of X and Y are (i.e., the less oxygen is contained inside the silicon nitride particles), the closer the oxygen localization index is to 0%. In other words, when most of the total oxygen amount TO (mass%) contained in the silicon nitride powder is localized on the surface of the silicon nitride particles, the index approaches 0%. On the other hand, the more the values of X and Y differ (i.e., the more oxygen is contained inside the silicon nitride particles), the larger the oxygen localization index becomes. In other words, when the degree of oxygen localization on the surface is low, the oxygen localization index becomes a value farther from 0%.
[0023] The inventors have found that when the oxygen localization index is 0% or more and less than 240.0%, the effect of oxygen localizing on the surface is exerted, and the water resistance of the silicon nitride powder can be improved. The oxygen localization index is preferably 0% or more and 230.0% or less, more preferably 0.01% or more and 220.0% or less, even more preferably 0.1% or more and 200.0% or less, still more preferably 0.5% or more and 180.0% or less, and particularly preferably 1.0% or more and 170.0% or less.
[0024] (Regarding Total Oxygen Content TO (% by mass) and Thickness X) The total oxygen content TO (% by mass) of the silicon nitride powder refers to the total amount of oxygen in the silicon nitride powder, and is measured by an inert gas fusion-infrared absorption method in accordance with JIS G 1239:2014.
[0025] The total oxygen content TO (mass%) of the silicon nitride powder can be set to, for example, less than 1.21 mass% (i.e., satisfying the following formula (4)). TO (mass%) < 1.21 (4) The total oxygen content TO (mass%) of the silicon nitride powder may be 1.00 mass% or less, 0.70 mass% or less, 0.60 mass% or less, or even 0.50 mass% or less. There is no particular restriction on the lower limit of the total oxygen content TO, but in order to better exhibit the water resistance effect, it is preferably 0.05 mass% or more, more preferably 0.10 mass% or more, even more preferably 0.20 mass% or more, and particularly preferably 0.25 mass% or more.
[0026] From the total oxygen content TO (mass%) of the silicon nitride powder, SiO 2 The method for converting the thickness of the coating to X (nm) is as follows: First, the silicon nitride particles constituting the silicon nitride powder are Si 3 N 4 and SiO 2 It is composed of Si 3 N 4 and SiO 2 The volume density of each silicon nitride particle is assumed to be the same. The particle size D50 of the silicon nitride particle at 50% cumulative size from the fine particle side of the cumulative particle size distribution on a volume basis is used as the silicon nitride particle size. The method for measuring D50 will be described later.
[0027] The silicon content l (mol %), oxygen content m (mol %), and nitrogen content n (mol %) relative to the total oxygen content TO (mass %) in silicon nitride can be calculated as follows.
[0028] (i) Regarding the silicon content l (mol%), all N in n (mol%) is Si 3 N 4 Origin, m (mol%) O is all SiO 2 From this, the silicon content l (mol%) can be calculated using the formula (6): l = 3 / 4 × n + 1 / 2 × m (6)
[0029] (ii) Silicon content (mass%) The silicon content (mass%) can be calculated using formula (7) from the atomic weight of silicon = 28 and the silicon content l (mol%). Furthermore, by substituting formula (6) into formula (7), formula (8) is obtained. Silicon content (mass%) = 28 x l (7) Silicon content (mass%) = 28 x 3 / 4 x n + 28 x 1 / 2 x m = 21 x n + 14 x m (8)
[0030] (iii) Since the atomic weight of nitrogen is 14 and the atomic weight of oxygen is 16, the nitrogen content (mass%) and oxygen content (mass%) can be calculated from equations (9) and (10), respectively. Nitrogen content (mass%) = 14 × n (9) Oxygen content (mass%) = 16 × m (10)
[0031] (iv) Assuming that silicon nitride is composed only of silicon, nitrogen, and oxygen, the total mass of silicon nitride can be expressed from equations (8) to (10) as equation (11): (21 x n + 14 x m) + 14 x n + 16 x m (11)
[0032] (v) Total Oxygen Content TO (mass %) Assuming that silicon nitride is composed only of silicon, nitrogen, and oxygen, the total oxygen content TO (mass %) can be calculated by dividing the right side of equation (10) by the left side of equation (11). In other words, the following equation (12) holds true for the total oxygen content TO (mass %): TO (mass %) = 16 × m × 100 / {(21 × n + 14 × m) + 14 × n + 16 × m} (12)
[0033] (vi) Next, assuming that silicon nitride is composed only of silicon, nitrogen, and oxygen, the amount of substance for the entire silicon nitride is given by equation (13): (3 / 4 x n + 1 / 2 x m) + n + m = 100 (13) From equations (12) and (13), the oxygen content m (mol %) and nitrogen content n (mol %) can be calculated using the following equations (14) and (15), respectively: m = 5 / 4 x TO (14) n = (800 - 15 x TO) / 14 (15)
[0034] Next, among the Si in silicon nitride, Si 3 N 4 and SiO2 The proportion (mol%) of each of the substances can be calculated from the following formulas (16) and (17). 3 N 4 Ratio of the amount of Si substance derived from the silicon dioxide (mol%) / 3 = 3n / 4 = (2400 - 45 x TO) / 56 (16) (SiO 2 The proportion of the amount of Si (mol%) derived from the carbon dioxide (CO₂) = m / 2 = 5 / 8 × TO (17)
[0035] Si 3 N 4 and SiO 2 The volume density of Si is equal to that of Si. 3 N 4 The entire surface of the particle is covered with SiO 2 Assuming that the coating is formed with a uniform thickness, the Si 3 N 4 Regarding the ratio k of the film thickness of the film, the following equation (18) holds: 3 = (3 / 4 × n) / (3 / 4 × n + 1 / 2 × m) = 3 × n / (3 × n + 2 × m) (18)
[0036] In addition, SiO 2 The film thickness (thickness X) of the coating is expressed by the following formula (19) using the particle diameter D50 (nm): SiO 2 Film thickness (thickness X) (nm) = D50 × (1 - k) / 2 (19) By substituting equations (14) and (15) into equation (18) to find k, and substituting the value of k and the value of D50 into equation (19), SiO 2 The thickness of the coating can be calculated.
[0037] SiO converted from the total oxygen content TO (mass%) of the silicon nitride powder 2The thickness X (nm) of the coating is preferably greater than 0 nm and less than 50 nm. In other words, it is preferable to satisfy the following formula (2). Such a silicon nitride powder can have improved water resistance: 0 < X (nm) < 50 (2) The thickness X is more preferably greater than 0 nm and not greater than 30 nm, even more preferably 0.5 nm or greater and not greater than 15.0 nm, still more preferably 1.0 nm or greater and not greater than 11.0 nm, even more preferably 3.0 nm or greater and not greater than 10.0 nm, still more preferably 6.1 nm or greater and not greater than 10.0 nm, and particularly preferably 7.1 nm or greater and not greater than 10.0 nm.
[0038] (Regarding the surface oxygen ratio SO (atom %) and thickness Y) The surface oxygen ratio SO (atom %) of silicon nitride particles refers to the amount of oxygen localized on the surface of the silicon nitride particles contained in the silicon nitride powder. XPS measurement of the silicon nitride powder (more precisely, the silicon nitride particles) is performed to measure the content of each of the elements Si, N, C, and O present on the surface of the silicon nitride particles. The content (atom %) of the O element when the total content of these four elements is 100 atom % is the surface oxygen ratio SO (atom %). In other words, SO can be calculated using the following formula (20): SO = [O] / ([Si] + [N] + [C] + [O]) × 100 (20) Here, [Si], [N], [C], and [O] are the contents (atom %) of Si, N, C, and O present on the surface of the silicon nitride particles.
[0039] The measurement target (XPS measurement portion) of the XPS measurement is the portion from the surface of the silicon nitride particle to a depth of 10 nm, and it is considered that the elements contained in the XPS measurement portion are all detected with equal intensity regardless of the depth from the surface. XPS measurement of the silicon nitride particle surface is performed, for example, using a JFS-9010 model manufactured by JEOL Ltd., with excitation X-rays: AlKα, an X-ray output of 110 W, a photoelectron escape angle of 45 degrees, and a pass energy of 50 EV, to measure the contents of the elements Si, N, C, and O on the silicon nitride particle surface.
[0040] The surface oxygen fraction SO (atom %) of the silicon nitride particles is preferably, for example, greater than 10.0 atom % (i.e., satisfying the following formula (5)). This increases the amount of localized oxygen present on the surface of the silicon nitride particles, thereby improving the water resistance of the silicon nitride powder. SO (atom %) > 10.0 (5) The surface oxygen fraction SO (atom %) of the silicon nitride particles may be 11.0 atom % or more, 13.0 atom % or more, or even 15.0 atom % or more, or even 20.0 atom % or more. The upper limit of the surface oxygen fraction SO of the silicon nitride particles is not particularly limited, but is, for example, 60.0 atom % or less.
[0041] From the surface oxygen ratio SO (atom%) of silicon nitride particles, SiO 2 The method for converting to the thickness Y (nm) of the coating is as follows: First, among the elements measured by XPS, all N elements were Si 3 N 4 All O elements are derived from SiO 2 It is assumed that the origin is Si 3 N 4 and SiO 2 It is composed of Si 3 N 4 and SiO 2 The volume density of SiO is assumed to be the same. 2 Membrane, Si 3 N 4 It is assumed that the thickness of each film is proportional to the Si content of each film. Based on these assumptions, Equation (21) is obtained.
[0042] The measurement results of the N content [N] (atom %) and the O content [O] (atom %) on the surface of the silicon nitride particles were substituted into the following formula (21) to obtain SiO 2 The thickness Y (nm) of the coating is calculated as follows: Y (nm) = 10 × ([O] / 2) / (3[N] / 4 + [O] / 2) (21) On the right side of the formula (21), "10" is the thickness of the XPS measurement part (= 10 nm), and "[O] / 2" is the thickness of SiO 2 The silicon content (atom%) derived from the silicon dioxide is 3[N] / 4.3 N 4 "([O] / 2) / (3[N] / 4+[O] / 2)" is the content (atom %) of silicon derived from SiO relative to the total silicon content. 2 The ratio of the silicon content derived from
[0043] The thickness Y is preferably 1.0 nm or more, more preferably 1.5 nm or more, even more preferably 2.0 nm or more, even more preferably 2.6 nm or more, and particularly preferably 3.6 nm or more.
[0044] (SO / SA value) The surface oxygen ratio SO (atom %) of silicon nitride particles is calculated by multiplying the specific surface area SA (m 2 / g), the value (SO / SA) is 10.1 (atom% / (m 2 / g) (i.e., satisfying the following formula (3)). When the value of SO / SA is large, that is, when the amount of surface oxygen per unit specific surface area is large, the oxide film becomes thicker, and it is expected that the water resistance will improve. SO (atom %) / SA (m 2 / g)>10.1 (atom% / (m 2 / g)) (3)
[0045] The SO / SA is more preferably 11.0 (atom% / (m 2 / g)) or more, more preferably 15.0 (atom% / (m 2 / g)) or more, and even more preferably 20.0 (atom% / (m 2 / g)) or more, and particularly preferably 22.0 (atom% / (m 2 / g) or more. The specific surface area SA (m 2 The method for measuring the molecular weight (mg / g) will be described later.
[0046] (Specific Surface Area) The specific surface area SA of the silicon nitride powder according to the embodiment is a BET specific surface area measured by a krypton adsorption method based on JIS Z 8830:2013. The specific surface area SA of the silicon nitride powder is 2.66 m 2 / g, and low SiO 2In this amount, the surface of the silicon nitride particles constituting the silicon nitride powder can be covered. 2 The smaller the specific surface area of silicon nitride particles containing silicon dioxide, the less SiO2 is formed on the surface. 2 The thickness of the film can be increased. Therefore, it is expected that the water resistance of the silicon nitride powder will be improved. The specific surface area of the silicon nitride powder is more preferably 2.00 m 2 / g or less, and more preferably 1.50m 2 / g or less, more preferably 1.36 m 2 The lower limit of the specific surface area is not particularly limited, but for example, it is 0.01 m 2 / g or more, and 2 / g or more, and 2 / g or more.
[0047] (Surface roughness Ra) The surface roughness Ra (arithmetic mean roughness) of the silicon nitride powder is preferably less than 0.97 nm. If the surface roughness Ra is less than 0.97 nm, the surface area becomes small, so that SiO 2 The film becomes thicker, which can improve water resistance. Furthermore, the small surface area reduces the contact area with water, which can improve water resistance. The surface roughness Ra is preferably less than 0.97 nm, more preferably 0.95 nm or less, even more preferably less than 0.93 nm, even more preferably 0.90 nm or less, even more preferably 0.80 nm or less, and particularly preferably 0.50 nm or less.
[0048] To measure the surface roughness Ra, a 100 nm x 100 nm measurement area on the surface of any silicon nitride particle is observed using a scanning probe microscope (SPM). The surface roughness Ra is calculated from the obtained shape image. The surface roughness Ra is measured for four silicon nitride particles, and the average value is taken as the surface roughness Ra of the silicon nitride powder.
[0049] (β-phase ratio) The β-phase ratio of the silicon nitride powder is preferably 65% or more. A β-phase ratio of 65% or more can improve the water resistance of the silicon nitride powder. The β-phase ratio is more preferably 70% or more, even more preferably 80% or more, even more preferably 85% or more, and particularly preferably 90% or more.
[0050] In this specification, the "β-phase ratio" refers to the content (volume %) of β-type silicon nitride relative to all silicon nitrides contained in the silicon nitride powder.
[0051] In calculating the β-phase ratio, the silicon nitride powder was measured by powder X-ray diffraction, and the diffraction pattern was analyzed by the Gazzara & Messier method (G.P. Gazzara and D.P. Messier, "Determination of Phase Content of Si 3 N 4 The β-phase ratio is calculated by analyzing the β-phase by X-ray Diffraction Analysis, Am. Ceram. Soc. Bull., 56[9]777-80 (1977)).
[0052] (The maximum particle size of silicon nitride particles having a ratio (L2 / L1) of the total length L2 of the internal boundaries to the outer edge length L1 of 1% or less is 6.8 μm or more.) The fewer grain boundaries and cavities there are inside a silicon nitride particle, the less moisture penetrates inside, and water resistance can be improved. Therefore, the ratio (L2 / L1) of the total length L2 of the boundaries to the outer edge length L1 is introduced as an indicator of the content of grain boundaries inside a silicon nitride particle. L1 and L2 are determined by observing the cross section of a silicon nitride particle. Note that here, "grain boundary" and "boundary line" refer to boundaries (also called high-angle grain boundaries) where, as a result of EBSD analysis, the crystal orientation difference (oblique angle) exceeds 15°.
[0053] When the length of the outer edge of one silicon nitride particle is L1 and the total length of the boundary lines of that silicon nitride particle is L2, silicon nitride particles with a small value of L2 / L1 can be said to have a low content of boundary lines. In this embodiment, silicon nitride particles with an L2 / L1 ratio of 1% or less are considered to be silicon nitride particles consisting of a single crystal (these are referred to as "single crystal particles").
[0054] In this embodiment, the maximum particle size of silicon nitride particles having an L2 / L1 ratio of 1% or less (i.e., single crystal) is preferably 6.8 μm or more, more preferably 10.0 μm or more, and even more preferably 15.0 μm or more. There is no particular upper limit, but it may be, for example, 200.0 μm or less, 100.0 μm or less, or 80.0 μm or less.
[0055] (Average aspect ratio of silicon nitride particles) The average aspect ratio of the minor axis to the major axis of the silicon nitride particles contained in the silicon nitride powder is preferably more than 0.50, more preferably more than 0.60, even more preferably 0.70 or more, and even more preferably 0.72 or more. On the other hand, the average aspect ratio of the silicon nitride particles is preferably less than 0.87, more preferably 0.85 or less, and even more preferably 0.80 or less.
[0056] The average aspect ratio of silicon nitride particles is measured as follows. SEM images of silicon nitride particles contained in silicon nitride powder are analyzed using image processing software (e.g., Image J (manufactured by the National Institute of Health)). The maximum particle size of the silicon nitride particles (referred to as the "major axis") is identified, and the particle size in the direction perpendicular to the major axis is referred to as the "minor axis". The major and minor axes are measured for 20 random silicon nitride particles, and the ratio of the minor axis to the major axis (minor axis / major axis) is determined for each particle. The arithmetic mean value of these ratios is taken as the average aspect ratio of the silicon nitride particles.
[0057] (Particle diameter D50 at 50% cumulative size from the fine particle side of the cumulative particle size distribution on a volume basis) The silicon nitride powder preferably has a particle diameter D50 (hereinafter sometimes simply referred to as "D50") at 50% cumulative size from the fine particle side of the cumulative particle size distribution on a volume basis of 1.5 μm or more, more preferably 2.0 μm or more. The upper limit is not particularly limited, but is, for example, preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 200 μm or less.
[0058] The D50 of silicon nitride powder is measured by laser diffraction. Specifically, the powder is dispersed in water and irradiated with a laser beam, and the diffraction is measured to determine the particle size. A measuring device such as the 1090L manufactured by CILAS can be used.
[0059] [Method for Producing Silicon Nitride Powder] A method for producing silicon nitride powder according to an embodiment of the present invention will be described. The method for producing silicon nitride powder includes the steps of: (1) synthesizing silicon nitride synthetic crystals by combustion synthesis in a nitrogen atmosphere using raw materials containing Si; (2) crushing the silicon nitride synthetic crystals to obtain coarsely pulverized silicon nitride powder; and (3) finely pulverizing the coarsely pulverized silicon nitride powder to obtain finely pulverized silicon nitride powder. Optionally, the method may further include the step of: (4) heat-treating the finely pulverized silicon nitride powder.
[0060] Step (1): Synthesizing silicon nitride composite crystals. For example, Si powder is used as the raw material containing Si. The average particle diameter D50 of the raw material is, for example, within the range of 2 to 10 μm. This allows the amount of oxygen impurities to be suppressed, and the combustion rate to be increased, allowing for a higher synthesis temperature, resulting in good crystal growth. As an example, the average particle diameter D50 of Si is 5 μm.
[0061] The diluent is used to adjust the amount of Si in the raw materials. A separately prepared silicon nitride powder is used as the diluent. The diluent may be either α-type silicon nitride powder or β-type silicon nitride powder, or a mixture of these. The average particle diameter D50 of the diluent is preferably in the range of 0.5 to 2.0 μm. For example, the average particle diameter D50 of the diluent is 1.0 μm. The amount of diluent added is less than 10 mass% of the total raw materials (including the diluent). For example, the diluent is added in an amount of 5 to 8 mass% of the total raw materials. By adding the amount of diluent within the above range, a predetermined amount of silicon nitride particles with oxygen localized on the surfaces of the silicon nitride particles can be produced.
[0062] In this embodiment, a diluent is mixed with the raw materials and then filled into an insulated heat-resistant container. This insulated heat-resistant container has a thermal conductivity of 1 W / mK or less, and although alumina or zirconia can be used as the material, carbon is preferred to prevent impurities from being mixed in. After the raw materials are filled, the container is covered with a lid made of the same material as the insulated heat-resistant container. Furthermore, to increase the temperature inside the composite during combustion, the thickness of the mixed raw materials is set to more than 100 mm, preferably more than 100 mm and 150 mm or less. Combustion synthesis is performed in a nitrogen atmosphere in the range of 0.5 to 1 MPa (e.g., 0.9 MPa). Adjusting the pressure range within this range enables efficient synthesis while suppressing increases in equipment costs.
[0063] When the mixed raw material is charged into the crucible, a layer of powder (silicon nitride) having a thickness of 1 mm to 80 mm is laid on the bottom and sides of the crucible, the mixed raw material is then charged, and the top surface is further covered with a layer of powder having a thickness of 1 mm to 80 mm. Covering the entire surface with powder allows the mixed raw material to be kept warm, and a predetermined amount of silicon nitride particles having oxygen localized on the surfaces of the silicon nitride particles can be produced.
[0064] To promote crystal growth more effectively, a catalyst may be used, for example, Y 2 O 3 , Fe 2 O 3 , CaO, Ni, Co, C, etc. are added in an amount of about 0.01 to 0.1 mass %. In addition, external auxiliary heating is performed in the range of 500°C to 1700°C (for example, 1500°C), and the combustion temperature is also increased in the combustion synthesis method by self-ignition.
[0065] Step (2): Obtaining a coarsely pulverized silicon nitride powder. The silicon nitride composite crystal is in the form of an agglomeration of multiple silicon nitride particles. In step (2), the silicon nitride composite crystal is crushed to obtain a coarsely pulverized silicon nitride powder. For example, the composite is crushed using a common crushing device such as a hammer mill or a disk mill until it passes through a sieve with a specified mesh size (for example, a sieve with mesh sizes in the range of 400 μm to 500 μm).
[0066] Step (3): Step of Obtaining Finely Pulverized Silicon Nitride Powder The coarsely pulverized silicon nitride powder is further pulverized to obtain a finely pulverized silicon nitride powder. The pulverization is carried out using a pulverizing device such as a jet mill or a ball mill. If necessary, the resulting finely pulverized powder may be classified. Classification may be carried out by sieving, wet classification, or the like. The resulting finely pulverized powder may be used as is as the silicon nitride powder, or may be subjected to a heat treatment step (step (4) described below) before use as the silicon nitride powder.
[0067] Step (4): Heat-treating the finely pulverized silicon nitride powder. Optionally, the finely pulverized silicon nitride powder may be heat-treated. By heat-treating, oxygen can be further localized on the surface, forming an oxide film on the surface of the silicon nitride particles. This has the effect of chemically stabilizing the silicon nitride particles, resulting in a silicon nitride powder with excellent water resistance. The heat treatment is carried out in air at a temperature of 500°C or higher and 1200°C or lower, preferably 550°C or higher and 1100°C or lower, and particularly preferably higher than 800°C and 1000°C or lower. The heat treatment time can be adjusted appropriately depending on the heat treatment temperature. The heat treatment time is, for example, 5 hours.
[0068] In the method for producing silicon nitride powder, silicon nitride synthetic crystals are synthesized using the heat generated by combustion synthesis, and then the silicon nitride powder according to this embodiment can be produced by crushing, classifying, and pulverizing the synthesized crystals.
[0069] [Resin Composition] The silicon nitride powder according to the embodiment of the present invention has excellent water resistance and is therefore suitable as a filler for a resin composition. The resin composition contains a resin and the silicon nitride powder according to the embodiment of the present invention.
[0070] The compounding ratio of the silicon nitride powder to the resin according to the embodiment of the present invention can be determined appropriately depending on the purpose and application. As an example, the resin may be 5 to 75 volume % and the silicon nitride powder may be 95 to 25 volume % relative to the resin composition (composite). The filling rate of the silicon nitride powder in the resin composition refers to the content (vol %) of the silicon nitride powder when the volume of the resin composition (including the silicon nitride powder) is taken as 100 volume %.
[0071] A method for producing a resin composition will be described. A resin composition can be obtained by mixing silicon nitride powder and a resin using a commonly used known method. For example, when the resin is liquid (e.g., liquid epoxy resin), the resin composition can be obtained by mixing the liquid resin, silicon nitride powder, and a curing agent, and then curing the mixture with heat or ultraviolet light. Known curing agents, mixing methods, and curing methods can be used. On the other hand, when the resin is solid, the desired resin composition can be obtained by mixing the silicon nitride powder and the resin, and then kneading the mixture using a known method such as melt kneading.
[0072] The resin used in the resin composition can be a known resin such as an epoxy resin. The type of resin can be selected from thermoplastic resins, thermoplastic elastomers, and thermosetting resins. The resins can be used alone or in combination of two or more.
[0073] Furthermore, these resin compositions may contain, as needed, known additives such as plasticizers, curing accelerators, coupling agents, fillers, pigments, flame retardants, antioxidants, surfactants, compatibilizers, weather resistance agents, antiblocking agents, antistatic agents, leveling agents, and release agents, either singly or in combination, within the scope of the invention.
[0074] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples carried out to clarify the effects of the embodiments of the present invention. However, the embodiments of the present invention are not limited to the following examples.
[0075] <Preparation of Silicon Nitride Powder> (Samples No. 1-3, 5, 6) Si powder (particle diameter = 5 μm) and silicon nitride powder (particle diameter = 1 μm) prepared separately as a diluent were mixed in a tumbling ball mill. The amount of diluent added was 5-8 mass% of the total raw material (including diluent). The mixed powder was packed into a carbonaceous, heat-resistant container with a layer of powder 1 mm to 80 mm thick on the bottom and sides, so that the raw material layer was thicker than 100 mm and not more than 150 mm. The raw material layer was then covered with a layer of powder 1 mm to 80 mm thick. A lid made of a carbonaceous, heat-resistant material was then placed, and synthesis was carried out under a nitrogen atmosphere at 0.9 MPa. After synthesis, the mixture was coarsely crushed (disintegrated) in a mortar until it passed through a sieve with the specified mesh size. The mesh size of the sieve for each sample is shown in Table 1.
[0076] The obtained coarsely pulverized powder was further pulverized using a nanojetmizer (manufactured by Aisin Nano Technologies Co., Ltd.). The nanojetmizer with the model number listed in Table 1 was used for pulverization. The obtained pulverized powder was classified using the method described in Table 1. Note that classification was not performed for Sample No. 2. The resulting classified powders (Samples No. 1, No. 3, and No. 6) and the finely pulverized powder (Sample No. 2) were then placed in an alumina crucible and heat-treated in an air atmosphere using a small-scale programmable electric furnace (MMF series, manufactured by AS ONE) under the conditions (heat treatment temperature, heat treatment time) listed in Table 1 to obtain silicon nitride powders (Samples Nos. 1 to 3 and 6). Note that the classified powder (Sample No. 5) was used as is as silicon nitride powder (Sample No. 5) without heat treatment.
[0077]
[0078] Various measurements were carried out on the obtained Samples Nos. 1 to 3 and 5 to 6 (Examples) and, as a comparative example, a commercially available silicon nitride powder (manufactured by Aldrich, silicon nitride (predominantly β-phase, ≦10 micron primary particle size, product code 248622); hereinafter referred to as "Sample No. 4").
[0079] (1) Measurement of the β-phase ratio of silicon nitride powder A diffraction pattern of the sample (silicon nitride powder) was obtained using a powder X-ray diffractometer (manufactured by Rigaku Denki). The measurement conditions were as follows: X-ray source: CuKα radiation X-ray output: 45 kV, 200 mA Graphite monochromator Diffraction angle (2θ): Step scan in 0.02° increments over the range of 2 to 90° Scanning speed: 21.7 deg / min
[0080] When a sample contained components other than silicon nitride, the peaks of those components were compared with the corresponding peaks of standard samples of those components to determine the proportions of those components. For Samples No. 1 to 6, the powder X-ray diffraction patterns obtained confirmed that the samples were composed solely of α-type silicon nitride and β-type silicon nitride. The proportion of β-type silicon nitride in the sample (β-conversion ratio) was then calculated using the Gazzara & Messier method.
[0081] (2) Maximum particle size of silicon nitride particles with an L2 / L1 ratio of 1% or less (maximum particle size of single-crystal particles) A sample for cross-sectional observation was prepared using the sample (silicon nitride particles). To prepare the sample for cross-sectional observation, the silicon nitride particles were embedded in resin, and then the resin and silicon nitride particles were cut using a diamond cutter. Subsequently, a protective film of platinum was vapor-deposited on the cross-section, and the cross-section was prepared by Ar ion milling. The sample was then fixed to the SEM sample stage with Cu double-sided tape, and SEM-EBSD measurement was performed without vapor deposition. The observation position was determined so that two or more silicon nitride particles were completely contained within the observation region (i.e., two or more silicon nitride particles did not come into contact with the frame of the observation region). Measurements were performed using β-type silicon nitride particles.
[0082] The following equipment was used for sample pretreatment and EBSD measurement: Equipment used Ion milling equipment: E-3500 (manufactured by Hitachi High-Tech Corporation) Ion sputtering equipment: E-1030 (manufactured by Hitachi, Ltd.) Schottky scanning electron microscope: SU5000 (manufactured by Hitachi High-Tech Corporation) Backscattered electron diffraction equipment: Velocity (manufactured by METEK Corporation)
[0083] The conditions for the EBSD measurement were as follows: Measurement area: 500.0 μm×400.0 μm Acceleration voltage: 15.0 kV Magnification: ×500 Vacuum degree: 30 Pa
[0084] In the obtained EBSD image, two or more silicon nitride particles that were not in contact with the frame of the observation area were selected, and the average of the outer edge length L1 of each silicon nitride particle was calculated using image processing software Image J (manufactured by the National Institute of Health). The total length L2 of the boundary lines was also calculated. The "total length L2 of the boundary lines" is the sum of the boundary lines contained within the silicon nitride particle and does not include the outer edge of the silicon nitride particle. The total length L2 of the boundary lines was calculated by adding the total length of the grain boundaries within the silicon nitride particle and the total length of the inner walls of the cavities (if any) within the silicon nitride particle.
[0085] This measurement was carried out once for 20 random silicon nitride particles, and silicon nitride particles with an L2 / L1 ratio of 1% or less were considered to be single crystal particles, and the length of their major axis was measured and recorded as the "maximum particle size of the single crystal particles." If the 20 silicon nitride particles measured contained multiple single crystal particles, the arithmetic average of their maximum particle sizes was calculated.
[0086] (3) Measurement of surface roughness Ra A scanning probe microscope SPA300HV manufactured by Seiko Instruments Inc. was used to measure the surface roughness Ra. The measurement conditions were as follows: Probe station / unit SPI4000 / SPA300HV Cantilever: SI-DF20 Scanner: 20 μm Data type: Topographic image Observation mode: DFM (Dynamic Force Mode Microscope) Scanning area: 100 nm x 100 nm Scanning frequency: 0.25 Hz Analysis software: (attached to the measuring device)
[0087] Five silicon nitride particles were randomly selected from the image, and a measurement area of 100 nm × 100 nm on the surface of each particle was observed using a scanning probe microscope (SPM). The surface roughness Ra of each particle was calculated from the obtained shape image, and the average value was taken as the surface roughness Ra of the silicon nitride powder.
[0088] (4) Measurement of total oxygen content TO of silicon nitride powder The total oxygen content TO (mass%) of the silicon nitride powder was measured by an inert gas fusion-infrared absorption method in accordance with JIS G 1239:2014.
[0089] (5) Measurement of Surface Oxygen Fraction SO of Silicon Nitride Particles Using a Thermo Fisher Scientific K-Alpha, the content (atom %) of each element Si, N, C, and O on the surface of the silicon nitride particles was measured using an excitation X-ray: AlKα, an X-ray output of 72 W, a photoelectron escape angle of 90 degrees, and a pass energy of 50 EV. The measurement results were substituted into the following equation (6) to determine the surface oxygen fraction SO (atom %) of the silicon nitride particles. SO (atom %) = [O] / ([Si] + [N] + [C] + [O]) × 100 (6) Here, [Si], [N], [C], and [O] are the contents (atom %) of Si, N, C, and O present on the surface of the silicon nitride particles.
[0090] (6) SiO 2 The thickness X and Y of the coating and the oxygen localization index were calculated from the results of measuring the total oxygen content TO (mass%) of the silicon nitride powder using the method described in the embodiment. 2 The thickness X (nm) of the coating was determined, and the surface oxygen ratio SO (atom%) of the silicon nitride particles was measured to determine SiO 2 The thickness Y (nm) of the coating was determined. The D50 of the silicon nitride powder, which is necessary for determining the thickness, was measured as follows.
[0091] (Measurement of D50 of silicon nitride powder) The particle size distribution of the sample (silicon nitride powder) was measured, and the cumulative 50% particle size D50 was determined. The particle size distribution of the silicon nitride powder was measured by laser diffraction. A sample dispersed in water was irradiated with a laser beam, and the diffraction was measured to determine the particle size. The measuring device used was a CILAS 1090L model. The particle size was taken as the circle-equivalent particle size. The circle-equivalent particle size is the particle size of a perfect circle that has the same area as a projected particle image. The particle size was measured based on volume.
[0092] From the calculated thicknesses X and Y, the oxygen localization index (|X−Y| / Y×100(%)) was calculated.
[0093] (7) Ratio of the surface oxygen fraction SO of silicon nitride particles to the specific surface area SA of silicon nitride powder (SO / SA) The surface oxygen fraction SO (atom %) of silicon nitride particles is calculated by multiplying the specific surface area SA (m 2 / g) to determine the SO / SA.
[0094] (8) Ratio of the total oxygen content TO of the silicon nitride powder to the specific surface area SA of the silicon nitride powder (TO / SA) The total oxygen content TO (mass%) of the silicon nitride powder was calculated by multiplying the specific surface area SA (m 2 / g) to determine TO / SA.
[0095] (9) Specific Surface Area SA of Silicon Nitride Powder The specific surface area of the sample (silicon nitride powder) was measured. The specific surface area of powder (solid) was measured by gas adsorption in accordance with JIS Z 8830:2013, using krypton as the adsorption gas. In the measurement, 1 g of silicon nitride powder was placed in a sample tube, and an adsorption / desorption isotherm was obtained. The specific surface area (m 2 / g) was calculated.
[0096] (10) Water Resistance Test 2 g of silicon nitride was immersed in 18 g of pure water, heated to 80°C, and held for 72 hours. After that, ammonium ions (NH 4 + The NH 2 concentration was measured by ion chromatography in accordance with JIS K 0127:2013. 4 + If the concentration is 30 ppm or less, the water resistance of the silicon nitride is judged to be excellent (◎); if it is more than 30 ppm and less than 50 ppm, the water resistance is judged to be good (◯); and if it exceeds 50 ppm, the water resistance is judged to be poor (×).
[0097] The measurement results are summarized in Tables 2 and 3.
[0098]
[0099]
[0100] The measurement results are discussed below. The silicon nitride powders of Samples 1 to 3 and 5 to 6, which met the requirements of this embodiment, were evaluated as having good (◯) or excellent (◎) water resistance. On the other hand, the silicon nitride powder of Sample 4, which did not meet the requirements of this embodiment, was evaluated as having poor (×) water resistance.
[0101] This application claims priority from Japanese Patent Application No. 2023-058618, filed March 31, 2023. Japanese Patent Application No. 2023-058618 is incorporated herein by reference.
Claims
1. A silicon nitride powder containing a plurality of silicon nitride particles and satisfying the following formula (1): 0%≦|X-Y| / Y×100<240.0% (1) where X (nm) is the SiO 2 is the thickness of the coating, Y (nm) is the SiO 2 The thickness of the coating.
2. The silicon nitride powder according to claim 1, which satisfies the following formula (2): 0<X (nm)<50.0 (2) 3. The silicon nitride powder according to claim 1, which satisfies the following formula (3): SO (atom%) / SA (m 2 / g)>10.1 (atom% / (m 2 / g) (3) where SA(m 2 / g) is the specific surface area of the silicon nitride powder.
4. The silicon nitride powder according to claim 1, wherein the total oxygen content TO (mass%) of the silicon nitride powder satisfies the following formula (4): TO (mass%) < 1.21 (4) 5. The silicon nitride powder according to claim 1, wherein the surface oxygen ratio SO (atom%) of the silicon nitride particles satisfies the following formula (5): SO (atom%)>10.0 (5) 6. Specific surface area is 2.66 m 2 2. The silicon nitride powder of claim 1, wherein the silicon nitride powder has a molecular weight of less than 1.0 / g.
7. The silicon nitride powder according to claim 1, having a surface roughness Ra of less than 0.97 nm.
8. The silicon nitride powder according to claim 1, having a beta-conversion rate of 65% or more.
9. The silicon nitride powder according to claim 1, wherein the maximum particle size of silicon nitride particles having a ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge of 1% or less is 6.8 μm or more.
10. A resin composition comprising a resin and the silicon nitride powder according to any one of claims 1 to 9.
Citation Information
Patent Citations
Production of silicon nitride powder
JP1993221617A
Epoxy resin composition and semiconductor-sealed device
JP1993230181A
Production of silicon nitride powder, sintered compact of silicon nitride and its production
JP1995267614A
Epoxy resin composition for sealing semiconductor and semiconductor device
JP1999166074A
Silicon nitride-based filler and resin composition for sealing semiconductor
JP1999268903A