Steel sheet, member, and production methods for these
The development of a steel plate with specific microstructural composition and surface characteristics addresses the challenge of high-strength steel plates' poor energy absorption, enabling stable collision performance and weight reduction for improved fuel efficiency and environmental impact.
Patent Information
- Application Number
- PCT/JP2024/006907
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-02-27
- Publication Date
- 2024-10-03
AI Technical Summary
High-strength steel plates with tensile strength of 780 MPa or more struggle to demonstrate stable energy absorption characteristics when used in energy-absorbing components, leading to potential breakage during collisions, while materials with lower tensile strength lack the necessary weight reduction for improved fuel efficiency and environmental impact.
A steel plate composition with a ferrite area ratio of 20-70%, bainitic ferrite and tempered martensite area ratio of 20-70%, and retained austenite area ratio of 3-20%, along with a surface soft layer, is developed, featuring a tensile strength of 780-1180 MPa, high yield stress, excellent total and local elongation, and enhanced bendability and energy absorption properties.
The steel plate achieves stable energy absorption and improved bendability, making it suitable for energy-absorbing applications in the automotive industry while reducing weight and maintaining safety, thus contributing to environmental protection and fuel efficiency.
Smart Images

Figure JPOXMLDOC01-APPB-M000001 
Figure JPOXMLDOC01-APPB-M000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Steel plates, components, and their manufacturing methods
[0001] The present invention relates to a high-strength steel sheet and a member having excellent crashworthiness, and a method for producing the same. The steel sheet of the present invention can be suitably used mainly as a steel sheet for automobiles.
[0002] From the perspective of global environmental conservation, CO 2 In order to reduce emissions, reducing the weight of automobile bodies while maintaining their strength and improving automobile fuel efficiency have always been important challenges in the automotive industry. To achieve weight reduction while maintaining the strength of automobile bodies, it is effective to increase the strength of steel sheets used as raw materials for automobile parts and thereby reduce their thickness. On the other hand, the premise of automobile parts made from steel sheets is to ensure the safety of people inside the vehicle in the event of a collision. Therefore, high-strength steel sheets used as raw materials for automobile parts are required to have not only the desired strength but also excellent crashworthiness.
[0003] In recent years, the use of high-strength steel sheets with a tensile strength (TS) of 780 MPa or more in automobile bodies has been expanding. From the perspective of crashworthiness, automotive components are broadly divided into non-deformable components such as pillars and bumpers and energy-absorbing components such as side members. Each component is required to have the necessary crashworthiness to ensure the safety of occupants in the event of a collision while the vehicle is in motion. Progress has been made in increasing the strength of non-deformable components, and high-strength steel sheets with a tensile strength (TS) of 780 MPa or more have already been put into practical use. However, when applied to energy-absorbing components, high-strength steel sheets with a tensile strength of 780 MPa or more are prone to fracture during a collision originating from areas subjected to primary processing such as forming, resulting in an inability to stably absorb collision energy. Therefore, materials with a tensile strength of 590 MPa or less are primarily used. Therefore, there is room for reducing component fracture during a collision and stably absorbing high energy, thereby ensuring safety during a collision, while contributing to environmental conservation through weight reduction. For these reasons, it is required to use high-strength steel plates with a TS of 780 MPa or more, which have excellent crashworthiness, for energy absorbing members.
[0004] As an example of a steel sheet that can be used as a material for such automobile parts, Patent Document 1 discloses a high-strength hot-dip galvanized steel sheet having a component composition containing, by mass%, 0.05 to 0.3% C, 0.01 to 2.5% Si, 0.5 to 3.5% Mn, 0.003 to 0.100% P, 0.02% or less S, 0.010 to 1.5% Al, 0.007% or less N, with the balance being Fe and unavoidable impurities, and having a microstructure containing, by area ratio, 20 to 87% ferrite, 3 to 10% martensite and retained austenite in total, and 10 to 60% tempered martensite, with a high TS-El balance, excellent stretch flangeability, and low YR and excellent workability.
[0005] Patent Document 2 also describes a high-strength hot-dip galvanized steel sheet having a thickness of 0.6 to 5.0 mm and a plating layer on the surface of the steel sheet, the steel sheet structure containing 40 to 90% by volume of a ferrite phase and 3 to 25% by volume of a retained austenite phase, the retained austenite phase having a solute carbon content of 0.70 to 1.00%, an average particle size of 2.0 μm or less, an average distance between particles of 0.1 to 5.0 μm, a thickness of a decarburized layer in the surface layer of the steel sheet of 0.01 to 10.0 μm, an average particle size of oxides contained in the surface layer of the steel sheet of 30 to 120 nm, and an average density of 1.0 × 10 12 pieces / m 2 The above also discloses a high-strength hot-dip galvanized steel sheet that has excellent mechanical cutting properties, while ensuring high strength of a maximum tensile strength of 900 MPa or more, and is characterized by having an average work-hardening coefficient (n value) of 0.080 or more at the time of plastic deformation of 3 to 7%.
[0006] Furthermore, Patent Document 3 discloses a high-strength hot-dip galvanized steel sheet excellent in delayed fracture resistance, characterized in that the steel sheet has, by volume fraction, 40 to 90% of a ferrite phase and 5% or less of a retained austenite phase, the proportion of unrecrystallized ferrite in the entire ferrite phase being 50% or less, the grain size ratio, which is the value obtained by dividing the average grain size of crystal grains of the ferrite phase in the rolling direction by the average grain size in the sheet width direction, is 0.75 to 1.33, the length ratio, which is the value obtained by dividing the average length of hard structures dispersed in an island shape in the rolling direction by the average length in the sheet width direction, is 0.75 to 1.33, and the average aspect ratio of inclusions is 5.0 or less.
[0007] Patent No. 5256689 Patent No. 5354135 Patent No. 5352793
[0008] However, Patent Document 1 discloses a high-strength hot-dip galvanized steel sheet in which both ductility, which is the press formability inside the steel sheet, and stretch flangeability, which is the press formability at the end of the steel sheet, are improved, but it cannot be said that the bendability and energy absorption characteristics are sufficient.
[0009] Patent Document 2 discloses a high-strength hot-dip galvanized steel sheet in which ductility is improved by generating retained austenite inside the steel sheet and mechanical cutting properties are improved by forming a decarburized layer on the surface layer of the steel sheet. However, it cannot be said that the bendability and energy absorption properties are sufficient.
[0010] Patent Document 3 discloses a high-strength hot-dip galvanized steel sheet in which the main structure inside the steel sheet is soft ferrite and the amount of unrecrystallized ferrite is limited to a small amount, thereby improving ductility, and the delayed fracture resistance and anisotropy thereof are improved by forming a decarburized layer in the surface layer of the steel sheet. However, it cannot be said that the bendability and energy absorption characteristics are sufficient.
[0011] From the above, it cannot be said that the steel sheets disclosed in Patent Documents 1 to 3 have a TS of 780 MPa or more and less than 1180 MPa, a high YS, excellent total elongation and local elongation, excellent bendability, and excellent energy absorption properties.
[0012] The present invention has been made in view of the above circumstances, and aims to provide a steel plate, a member, and a method for manufacturing the same, which have a tensile strength TS of 780 MPa or more and less than 1180 MPa, a high yield stress YS, excellent total elongation and local elongation, excellent bendability, and excellent energy absorption characteristics.
[0013] The steel sheet referred to here also includes a galvanized steel sheet, and the galvanized steel sheet is a hot-dip galvanized steel sheet (hereinafter also referred to as GI), a galvannealed hot-dip galvanized steel sheet (hereinafter also referred to as GA), or an electro-galvanized steel sheet (hereinafter also referred to as EG).
[0014] Here, the tensile strength TS is measured by a tensile test in accordance with JIS Z 2241 (2011).
[0015] Furthermore, having a high yield stress YS, excellent total elongation (T-El) and local elongation (L-El), excellent bendability, and excellent energy absorption properties means that the following is satisfied.
[0016] A high yield stress YS means that the YS measured in a tensile test in accordance with JIS Z 2241 (2011) satisfies the following formula (A) or (B) depending on the TS measured in the tensile test: (A) 400 MPa ≦ YS ≦ 650 MPa when 780 MPa ≦ TS < 980 MPa; (B) 600 MPa ≦ YS ≦ 980 MPa when 980 MPa ≦ TS.
[0017] Total elongation correlates with stretch formability, and excellent total elongation means that the total elongation (T-El) measured in a tensile test conforming to JIS Z 2241 (2011) satisfies the following formula (A) or (B) depending on the TS measured in the tensile test: (A) 17.0% ≦ T-El when 780 MPa ≦ TS < 980 MPa; (B) 11.0% ≦ T-El when 980 MPa ≦ TS.
[0018] Local elongation correlates with stretch flangeability, and excellent local elongation means that the local elongation (L-El) measured in a tensile test in accordance with JIS Z 2241 (2011) satisfies the following formula (A) or (B) depending on the TS measured in the tensile test: (A) 7.0%≦L-El when 780 MPa≦TS<980 MPa; (B) 5.0%≦L-El when 980 MPa≦TS.
[0019] "Having excellent bendability" means that the outer bend angle (limit bend angle (α)) of the central part of the plate-shaped test piece when the load F from the push-bending jig is maximum in a bending test conforming to the VDA standard (VDA238-100) specified by the German Association of the Automotive Industry is 80° or more.
[0020] The term "excellent energy absorption properties" means that the load F (N) - stroke X (mm) curve obtained by performing a bending test on a steel plate in accordance with the VDA standard (VDA238-100) specified by the German Association of the Automotive Industry is such that the stroke X (mm) at which the load reaches its maximum value after deformation begins is the maximum value. max This means that the integral value AE (N·mm) of the load F (N) up to the load point satisfies the following formula (1), and preferably satisfies the following formula (2).
[0021]
[0022]
[0023] In the above formulas (1) and (2), F: load (N) X: stroke (mm) X max : Stroke (mm) at which the load reaches its maximum value AE: Stroke X at which the load reaches its maximum value after deformation begins max Integral value of load F up to (N mm)
[0024] The present inventors have conducted extensive research to solve the above problems and have found the following: By appropriately adjusting the chemical composition of a base steel sheet, a steel structure is obtained in which, in area ratios, ferrite is 20.0% to 70.0%, the total of tempered martensite and bainitic ferrite is 20.0% to 70.0%, retained austenite is 3.0% to 20.0%, and fresh martensite is 20.0% or less (including 0.0%), the area ratio of bainitic ferrite among the total area ratio of bainitic ferrite and tempered martensite is 40% or more, and the average grain size of a hard second phase including retained austenite and fresh martensite present in the bainitic ferrite is 3.0 μm or less, and in the base steel sheet, the total area ratio of structures other than ferrite is S A / 2 or less (S A When the soft surface layer is a region where the area is 0.01 mm or more from the surface of the base steel sheet in the thickness direction, the soft surface layer has a thickness of 20 μm or more and a tensile strength of 780 MPa or more but less than 1180 MPa. It has been found that this makes it possible to obtain a steel sheet with a high YS, excellent press formability (bendability and ductility of the steel sheet), and excellent energy absorption properties during bending deformation.
[0025] The present invention was made based on such findings, and its gist is as follows: [1] A steel plate having a base steel plate, the base steel plate containing, in mass %, C: 0.05 to 0.30%, Si: 0.10 to 2.00%, Mn: 1.00 to 3.50%, P: 0.001 to 0.100%, S: 0.0001 to 0.0200%, sol. and a steel structure in which, at a 1 / 4 position of the sheet thickness of the base steel sheet, the area ratios are: ferrite: 20.0% to 70.0%; a total of bainitic ferrite and tempered martensite: 20.0% to 70.0%; retained austenite: 3.0% to 20.0%; and fresh martensite: 20.0% or less (including 0.0%), the area ratio of bainitic ferrite being 40% or more of the total area ratio of the bainitic ferrite and tempered martensite, and the average grain size of a hard second phase which is present in the bainitic ferrite and includes the retained austenite and the fresh martensite is 3.0 μm or less. Furthermore, the steel sheet has a surface soft layer formed to a thickness of 20 μm or more from the surface of the base steel sheet in the sheet thickness direction, and the total area ratio of structures other than ferrite in the steel structure is ½ or less at the ¼ position in the sheet thickness, and has a tensile strength of 780 MPa or more and less than 1180 MPa.[2] The composition further includes, in mass%, Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Cu: 1.000% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less, Zn: 0.0200% or less, Co: 0.0200% or less, Zr: 0.1000% or less, Ca: 0.0200% or less, Se: 0.0200% or less, The steel sheet according to [1] above, containing at least one selected from Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM: 0.0200% or less. [3] The steel sheet according to [1] or [2] above, wherein one or both sides of the base steel sheet are provided with a zinc-plated layer. [4] A member made using the steel sheet according to any one of [1] to [3] above.[5] A hot rolling process in which a steel slab having the chemical composition according to [1] or [2] is hot rolled to obtain a hot rolled steel sheet; A pickling process in which the hot rolled steel sheet is pickled; An annealing process in which the steel sheet after the pickling process is heated and annealed under conditions of an annealing temperature of 720°C or more and 860°C or less, a holding time of 20 seconds or more, and an atmosphere with a dew point of -10°C or more; A rapid heating process in which the steel sheet is rapidly heated from the annealing temperature to a temperature of the annealing temperature + 10°C or more under conditions of a heating rate of 10°C / second or more; A first cooling process in which the steel sheet after the rapid heating process is cooled to a first cooling stop temperature of 400°C or more and 600°C or less; A holding process in which the steel sheet is held in a temperature range of 400°C or more and 600°C or less for a holding time of less than 300 seconds; A second cooling process in which the steel sheet after the holding process is cooled to a second cooling stop temperature of 100°C or more and 300°C or less. a reheating and holding step of heating the steel sheet after the second cooling step to a tempering temperature of 460°C or less and holding the steel sheet in the temperature range for a tempering time of 10 seconds or more and 2000 seconds or less, or further including a cold rolling step of cold rolling the steel sheet after the pickling step and before the annealing step at a rolling reduction of 20% or more and 80% or less to obtain a cold-rolled steel sheet. [6] The method for producing a steel sheet according to [5] above, wherein the threading speed LS (m / min) of the steel sheet in the annealing step satisfies the following formula (1): 3.0 / (t×W×4.716×10. ―4 )<LS<390.0 / (t×W×4.716×10 ―4 ) Formula (1) Wherein, t: sheet thickness (mm) after the pickling process and before the annealing process, W: sheet width (mm) after the pickling process and before the annealing process. [7] A method for producing a steel sheet according to [5] or [6] above, comprising, after the holding process and before the second cooling process, a hot-dip galvanizing process of applying a galvanizing treatment to a surface of the steel sheet to form a galvanized layer on the surface of the steel sheet, or further comprising an alloying treatment process of applying an alloying treatment to the steel sheet on which the galvanized layer has been formed. [8] A method for producing a steel sheet according to [5] or [6] above, comprising, after the reheating and holding process, an electrogalvanizing process of immersing the steel sheet in an electrogalvanizing bath to form a galvanized layer on the steel sheet. [9] A method for producing a member, comprising a step of subjecting the steel sheet according to any of [1] to [3] above to at least one of forming and joining to form a member.
[0026] According to the present invention, it is possible to obtain a steel sheet having a tensile strength TS of 780 MPa or more but less than 1180 MPa, a high yield stress YS, and excellent total elongation, local elongation, bendability, and energy absorption properties. A member obtained by subjecting the steel sheet of the present invention to forming processing, welding, or the like can be suitably used as an energy absorption member for use in the automotive field.
[0027] The present invention will be described in detail below.
[0028] [1. Steel Plate] The steel plate of the present invention is a steel plate having a base steel plate, and the base steel plate contains, in mass %, C: 0.05 to 0.30%, Si: 0.10 to 2.00%, Mn: 1.00 to 3.50%, P: 0.001 to 0.100%, S: 0.0001 to 0.0200%, sol. The steel sheet has a chemical composition containing Al: 0.005 to 2.000% and N: 0.010% or less, with the balance being Fe and unavoidable impurities, and at a 1 / 4 position in the sheet thickness of the base steel sheet, the area ratios of ferrite are 20.0% to 70.0%, the total of bainitic ferrite and tempered martensite are 20.0% to 70.0%, retained austenite is 3.0% to 20.0%, fresh martensite is 20.0% or less (including 0.0%), and the total of bainitic ferrite and tempered martensite is ... and a steel structure in which the area ratio of bainitic ferrite is 40% or more of the total area ratio of rutensite, and a hard second phase, including retained austenite and fresh martensite, is present in the bainitic ferrite and has an average grain size of 3.0 μm or less. The steel sheet further has a surface soft layer formed to a thickness of 20 μm or more from the surface of the base steel sheet in the thickness direction, where the total area ratio of phases other than ferrite in the steel structure is ½ or less at the ¼ position in the sheet thickness. The steel sheet has a tensile strength of 780 MPa or more and less than 1180 MPa. The steel sheet has a tensile strength TS (hereinafter, tensile strength TS may also be simply referred to as TS) of 780 MPa or more and a high yield stress YS (hereinafter, yield stress YS may also be simply referred to as YS), and is excellent in total elongation, local elongation, bendability, and energy absorption characteristics. The steel sheet may have a zinc-plated layer as the outermost layer on one or both sides of the steel sheet. A steel sheet having a zinc plating layer may be referred to as a zinc-plated steel sheet. More specifically, a steel sheet having a hot-dip galvanized layer among zinc plating layers may be referred to as a hot-dip galvanized steel sheet. A steel sheet having a galvannealed hot-dip galvanized layer among zinc plating layers may be referred to as a galvannealed hot-dip galvanized steel sheet. A steel sheet having an electrogalvanized layer among zinc plating layers may be referred to as an electrogalvanized steel sheet.
[0029] First, the chemical composition of the base steel sheet of the steel sheet according to one embodiment of the present invention will be described. Note that the units for the chemical compositions are all "mass %", but hereinafter, unless otherwise specified, they will be simply expressed as "%".
[0030] C: 0.05 to 0.30% C is an effective element for generating appropriate amounts of fresh martensite, tempered martensite, bainitic ferrite, and retained austenite to ensure a TS of 780 MPa or more but less than 1180 MPa and a high YS. Here, if the C content is less than 0.05%, the area fraction of ferrite increases, making it difficult to achieve a TS of 780 MPa or more. On the other hand, if the C content exceeds 0.30%, the area fraction of fresh martensite increases excessively, making it difficult to achieve a TS of less than 1180 MPa. Furthermore, fresh martensite can serve as a starting point for void formation during VDA bending tests, which may prevent the desired bendability of the steel sheet from being achieved. Therefore, the C content is set to 0.05% or more but less than 0.30%. The C content is preferably 0.07% or more, more preferably 0.09% or more. The C content is preferably 0.25% or less, more preferably 0.20% or less.
[0031] Si: 0.10 to 2.00% Si suppresses the formation of carbides during cooling after annealing and promotes the formation of retained austenite. That is, Si is an element that affects the volume fraction of retained austenite. Here, if the Si content is less than 0.10%, the volume fraction of retained austenite decreases, and ductility decreases. On the other hand, if the Si content exceeds 2.00%, the C concentration in austenite during annealing increases excessively with an increase in the area fraction of ferrite, making it impossible to achieve the desired local elongation. Therefore, the Si content is set to 0.10% or more and 2.00% or less. The Si content is preferably 1.50% or less. Furthermore, the Si content is preferably 0.50% or more.
[0032] Mn: 1.00 to 3.50% Mn is an element that adjusts the area ratio of ferrite, bainitic ferrite, tempered martensite, etc. Here, if the Mn content is less than 1.00%, the area ratio of ferrite increases excessively, making it difficult to achieve a TS of 780 MPa or more. On the other hand, if the Mn content exceeds 3.50%, the area ratio of ferrite decreases, making it difficult to obtain the desired total elongation. Therefore, the Mn content is set to 1.00% or more and 3.50% or less. The Mn content is preferably 2.00% or more. Furthermore, the Mn content is preferably 3.00% or less.
[0033] P: 0.001 to 0.100% P is an element that has the effect of solid solution strengthening and increases the TS and YS of steel sheets. To achieve this effect, the P content is set to 0.001% or more. On the other hand, if the P content exceeds 0.100%, P segregates at the prior austenite grain boundaries, embrittling the grain boundaries. As a result, the amount of voids generated during the VDA bending test increases, making it impossible to achieve the desired bendability. Therefore, the P content is set to 0.001% or more and 0.100% or less. The P content is preferably 0.030% or less.
[0034] S: 0.0001 to 0.0200% S exists as sulfides in steel. In particular, if the S content exceeds 0.0200%, the amount of voids generated increases after shearing the steel sheet, making it impossible to achieve the desired bendability of the sheared edge. Therefore, the S content is set to 0.0200% or less. The S content is preferably set to 0.0080% or less. Furthermore, due to constraints in production technology, the S content is set to 0.0001% or more.
[0035] Sol. Al: 0.005 to 2.000% Al suppresses carbide formation during cooling after annealing and promotes the formation of retained austenite. That is, Al is an element that affects the volume fraction of retained austenite. To achieve this effect, the sol. Al content is set to 0.005% or more. On the other hand, if the sol. Al content exceeds 2.000%, the ferrite area fraction increases excessively, making it difficult to achieve a TS of 780 MPa or more. This also results in a decrease in YS. In addition, the C concentration in austenite during annealing increases excessively, making it impossible to achieve the desired bendability. Therefore, the Al content is set to 0.005% or more and 2.000% or less. The Al content is preferably 0.010% or more. The Al content is more preferably 0.015% or more. The Al content is preferably 1.000% or less.
[0036] N: 0.010% or less N exists as nitrides in steel. In particular, if the N content exceeds 0.010%, the amount of voids generated increases after a VDA bending test is performed on the steel sheet, making it impossible to achieve the desired bendability. Therefore, the N content is set to 0.010% or less. The N content is preferably 0.0050% or less. Although there is no particular lower limit for the N content, due to constraints on production technology, the N content is preferably 0.0005% or more.
[0037] The basic chemical composition of the base steel sheet of the steel sheet according to one embodiment of the present invention has been described above, but the base steel sheet of the steel sheet according to one embodiment of the present invention has a chemical composition containing the basic chemical components with the balance other than the basic chemical components including Fe (iron) and unavoidable impurities. Here, it is preferable that the base steel sheet of the steel sheet according to one embodiment of the present invention has a chemical composition containing the basic chemical components with the balance consisting of Fe and unavoidable impurities.
[0038] In addition to the basic components, the base steel sheet of a steel sheet according to one embodiment of the present invention may contain at least one selected from the optional components shown below. Note that the effects of the present invention can be obtained so long as the optional components shown below are contained in amounts up to the upper limit amounts shown below, so no lower limit is particularly set. Note that when the optional elements listed below are contained in amounts less than the preferred lower limit values described below, the elements are considered to be included as inevitable impurities.
[0039] Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0. 200% or less, Sn: 0.200% or less, Cu: 1.000% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less, Zn: 0.0200% or less, Co: 0.0200 %, Zr: 0.1000% or less, Ca: 0.0200% or less, Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and at least one selected from REM: 0.0200% or less
[0040] Nb: 0.200% or less Nb forms fine carbides, nitrides, or carbonitrides during hot rolling or annealing, thereby increasing TS and YS. To achieve this effect, the Nb content is preferably 0.001% or more. The Nb content is more preferably 0.005% or more. On the other hand, if the Nb content exceeds 0.200%, large amounts of coarse precipitates and inclusions may be formed. In such cases, the coarse precipitates and inclusions may become the starting points for cracks during a VDA bending test, and the desired bendability of the steel sheet may not be achieved. Therefore, when Nb is contained, the Nb content is preferably 0.200% or less. The Nb content is more preferably 0.060% or less.
[0041] Ti: 0.200% or less Like Nb, Ti forms fine carbides, nitrides, or carbonitrides during hot rolling or annealing, thereby increasing TS and YS. To achieve this effect, the Ti content is preferably 0.001% or more. The Ti content is more preferably 0.005% or more. On the other hand, if the Ti content exceeds 0.200%, large amounts of coarse precipitates and inclusions may be formed. In such cases, the coarse precipitates and inclusions may become the starting points for cracks during a VDA bending test, and the desired bendability of the steel sheet may not be achieved. Therefore, when Ti is contained, the Ti content is preferably 0.200% or less. The Ti content is more preferably 0.060% or less.
[0042] V: 0.200% or less Like Nb and Ti, V forms fine carbides, nitrides, or carbonitrides during hot rolling and annealing, thereby increasing TS and YS. To achieve this effect, the V content is preferably 0.001% or more. The V content is more preferably 0.005% or more. The V content is further preferably 0.010% or more, and even more preferably 0.030% or more. On the other hand, if the V content exceeds 0.200%, large amounts of coarse precipitates and inclusions may be formed. In such cases, the coarse precipitates and inclusions may become the starting points for cracks during a VDA bending test, and the desired bendability of the steel sheet may not be achieved. Therefore, when V is contained, the V content is preferably 0.200% or less. The V content is more preferably 0.060% or less.
[0043] B: 0.0100% or less B is an element that segregates at austenite grain boundaries to improve hardenability. Furthermore, B is an element that suppresses the formation and grain growth of ferrite during cooling after annealing. To achieve this effect, the B content is preferably 0.0001% or more. The B content is more preferably 0.0002% or more. The B content is further preferably 0.0005% or more, and even more preferably 0.0007% or more. On the other hand, if the B content exceeds 0.0100%, cracks may occur inside the steel sheet during hot rolling. Furthermore, when the steel sheet is subjected to a VDA bending test, the amount of voids generated may increase, making it difficult to achieve the desired bendability. Therefore, when B is contained, the B content is preferably 0.0100% or less. The B content is more preferably 0.0050% or less.
[0044] Cr: 1.000% or less. Cr is an element that improves hardenability, so the addition of Cr produces a large amount of tempered martensite, ensuring a TS of 780 MPa or more and a high YS. To achieve this effect, the Cr content is preferably 0.0005% or more. The Cr content is more preferably 0.010% or more. The Cr content is even more preferably 0.030% or more, and even more preferably 0.050% or more. On the other hand, if the Cr content exceeds 1.000%, the area fraction of hard fresh martensite increases excessively, and the fresh martensite may become the origin of void formation in a VDA bending test, potentially preventing the desired bendability of the steel sheet. Therefore, when Cr is contained, the Cr content is preferably 1.000% or less. The Cr content is more preferably 0.800% or less, and even more preferably 0.700% or less.
[0045] Ni: 1.000% or less Since Ni is an element that improves hardenability, the addition of Ni results in the formation of a large amount of tempered martensite, ensuring a TS of 780 MPa or more and a high YS. To achieve this effect, the Ni content is preferably 0.005% or more. The Ni content is more preferably 0.020% or more. The Ni content is further preferably 0.040% or more, and even more preferably 0.060% or more. On the other hand, if the Ni content exceeds 1.000%, the area fraction of fresh martensite increases excessively, and fresh martensite may become the origin of void formation in a VDA bending test, potentially preventing the desired bendability of the steel sheet. Therefore, when Ni is contained, the Ni content is preferably 1.000% or less. The Ni content is more preferably 0.800% or less. The Ni content is more preferably 0.600% or less, and even more preferably 0.400% or less.
[0046] Mo: 1.000% or less Mo is an element that improves hardenability, and the addition of Mo results in the formation of a large amount of tempered martensite, ensuring a TS of 780 MPa or more and a high YS. To achieve this effect, the Mo content is preferably 0.010% or more. The Mo content is more preferably 0.030% or more. On the other hand, if the Mo content exceeds 1.000%, the area fraction of fresh martensite increases excessively, and fresh martensite may become the origin of void formation in a VDA bending test, potentially preventing the desired bendability of the steel sheet. Therefore, when Mo is contained, the Mo content is preferably 1.000% or less. The Mo content is more preferably 0.500% or less, even more preferably 0.450% or less, and even more preferably 0.400% or less. The Mo content is more preferably 0.350% or less, and even more preferably 0.300% or less.
[0047] Sb: 0.200% or less Sb is an element that suppresses the diffusion of C near the steel sheet surface during annealing and is effective in controlling the formation of a soft layer near the steel sheet surface. If the soft layer increases excessively near the steel sheet surface, it becomes difficult to achieve a TS of 780 MPa or more. This also leads to a decrease in YS. Therefore, the Sb content is preferably 0.002% or more. The Sb content is more preferably 0.005% or more. On the other hand, if the Sb content exceeds 0.200%, a soft layer is not formed near the steel sheet surface, which may lead to a decrease in the bendability of the steel sheet. Therefore, when Sb is contained, the Sb content is preferably 0.200% or less. The Sb content is more preferably 0.020% or less.
[0048] Sn: 0.200% or less Like Sb, Sn is an element that suppresses the diffusion of C near the steel sheet surface during annealing and is effective in controlling the formation of a soft layer near the steel sheet surface. If the soft layer increases excessively near the steel sheet surface, it becomes difficult to achieve a TS of 780 MPa or more. This also leads to a decrease in YS. Therefore, the Sn content is preferably 0.002% or more. The Sn content is more preferably 0.005% or more. On the other hand, if the Sn content exceeds 0.200%, a soft layer is not formed near the steel sheet surface, which may lead to a decrease in the bendability of the steel sheet. Therefore, when Sn is contained, the Sn content is preferably 0.200% or less. The Sn content is more preferably 0.020% or less.
[0049] Cu: 1.000% or less Cu is an element that improves hardenability, so the addition of Cu produces a large amount of tempered martensite, ensuring a TS of 780 MPa or more and a high YS. To achieve this effect, the Cu content is preferably 0.005% or more. The Cu content is more preferably 0.008% or more, and even more preferably 0.010% or more. The Cu content is more preferably 0.020% or more. On the other hand, if the Cu content exceeds 1.000%, the area fraction of fresh martensite may increase excessively, resulting in the formation of large amounts of coarse precipitates and inclusions. In such cases, the fresh martensite and coarse precipitates and inclusions may become the starting points for void formation during a VDA bending test, potentially preventing the desired bendability of the steel sheet. Therefore, when Cu is added, the Cu content is preferably 1.000% or less. The Cu content is more preferably 0.200% or less.
[0050] Ta: 0.100% or less Like Ti, Nb, and V, Ta increases TS and YS by forming fine carbides, nitrides, or carbonitrides during hot rolling and annealing. Additionally, Ta partially dissolves in Nb carbides and Nb carbonitrides to form complex precipitates such as (Nb, Ta)(C, N). This suppresses coarsening of precipitates and stabilizes precipitation strengthening. This further improves TS and YS. To achieve this effect, the Ta content is preferably 0.001% or more. The Ta content is more preferably 0.002% or more, and even more preferably 0.004% or more. On the other hand, if the Ta content exceeds 0.100%, a large amount of coarse precipitates and inclusions may be formed. In such cases, the coarse precipitates and inclusions may become the starting points for void formation during the VDA bending test, and the desired bendability of the steel sheet may not be achieved. Therefore, when Ta is contained, the Ta content is preferably 0.100% or less. The Ta content is more preferably 0.090% or less, and even more preferably 0.080% or less.
[0051] W: 0.500% or less. W is an element that improves hardenability, so the addition of W produces a large amount of tempered martensite, ensuring a TS of 780 MPa or more and a high YS. To achieve this effect, the W content is preferably 0.001% or more. The W content is more preferably 0.030% or more. On the other hand, if the W content exceeds 0.500%, the area fraction of hard fresh martensite increases excessively, and fresh martensite may become the origin of void formation in a VDA bending test, potentially preventing the desired bendability of the steel sheet. Therefore, when W is contained, the W content is preferably 0.500% or less. The W content is more preferably 0.450% or less, and even more preferably 0.400% or less. The W content is even more preferably 0.300% or less.
[0052] Mg: 0.0200% or less. Mg is an element effective in spheroidizing inclusions such as sulfides and oxides and improving the bendability of the sheared edge. To achieve this effect, the Mg content is preferably 0.0001% or more. The Mg content is more preferably 0.0005% or more, and even more preferably 0.0010% or more. On the other hand, if the Mg content exceeds 0.0200%, large amounts of coarse precipitates and inclusions may be formed. In such cases, the coarse precipitates and inclusions may become the starting point for void formation during VDA bending tests, potentially preventing the desired bendability of the steel sheet. Therefore, when Mg is contained, the Mg content is preferably 0.0200% or less. The Mg content is more preferably 0.0180% or less, and even more preferably 0.0150% or less.
[0053] Zn: 0.0200% or less Zn is an element effective in spheroidizing the shape of inclusions and improving the bendability of the sheared edge. To achieve this effect, the Zn content is preferably 0.0010% or more. The Zn content is more preferably 0.0020% or more, and even more preferably 0.0030% or more. On the other hand, if the Zn content exceeds 0.0200%, a large amount of coarse precipitates and inclusions may be formed. In such cases, the coarse precipitates and inclusions may become the starting point for void formation during a VDA bending test, which may prevent the desired bendability of the steel sheet from being achieved. Therefore, when Zn is contained, the Zn content is preferably 0.0200% or less. The Zn content is more preferably 0.0180% or less, and even more preferably 0.0150% or less.
[0054] Co: 0.0200% or less Like Zn, Co is an effective element for spheroidizing inclusions and improving the bendability of the sheared edge. To achieve this effect, the Co content is preferably 0.0010% or more. The Co content is more preferably 0.0020% or more, and even more preferably 0.0030% or more. On the other hand, if the Co content exceeds 0.0200%, a large amount of coarse precipitates and inclusions may be formed. In such cases, the coarse precipitates and inclusions may become the starting point for void formation during a VDA bending test, which may prevent the desired bendability of the steel sheet from being achieved. Therefore, when Co is contained, the Co content is preferably 0.0200% or less. The Co content is more preferably 0.0180% or less, and even more preferably 0.0150% or less.
[0055] Zr: 0.1000% or less Like Zn and Co, Zr is an element that effectively spheroidizes the shape of inclusions and improves the bendability of the sheared edge. To achieve this effect, the Zr content is preferably 0.0010% or more. On the other hand, if the Zr content exceeds 0.1000%, a large amount of coarse precipitates and inclusions may be formed. In such cases, the coarse precipitates and inclusions may become the starting point for void formation during a VDA bending test, which may prevent the desired bendability of the steel sheet from being achieved. Therefore, when Zr is contained, the Zr content is preferably 0.1000% or less. The Zr content is more preferably 0.0300% or less, and even more preferably 0.0100% or less.
[0056] Ca: 0.0200% or less Ca exists as inclusions in steel. Here, if the Ca content exceeds 0.0200%, a large amount of coarse inclusions may be formed. In such cases, the coarse precipitates and inclusions may become the starting point for void formation during a VDA bending test, and the desired bendability of the steel sheet may not be achieved. Therefore, when Ca is contained, the Ca content is preferably 0.0200% or less. The Ca content is preferably 0.0020% or less. Note that the lower limit of the Ca content is not particularly limited, but the Ca content is preferably 0.0005% or more. Furthermore, due to constraints in production technology, the Ca content is more preferably 0.0010% or more.
[0057] Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, REM: 0.0200% or less. Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM are all effective elements for improving bendability during VDA testing. To achieve this effect, the contents of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM are preferably 0.0001% or more. On the other hand, if the contents of Se, Te, Ge, Sr, Cs, Hf, Pb, Bi, and REM exceed 0.0200% each, or if the content of As exceeds 0.0500%, large amounts of coarse precipitates and inclusions may be formed. In such cases, the coarse precipitates and inclusions may become the origin of void formation during VDA bending tests, potentially preventing the desired bendability of the steel sheet. Therefore, when at least one of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM is contained, it is preferable that the contents of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM are each 0.0200% or less, and the content of As is 0.0500% or less. The Se content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Se content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The Te content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Te content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The Ge content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Ge content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The As content is more preferably 0.0010% or more, and even more preferably 0.0015% or more.The As content is more preferably 0.0400% or less, and even more preferably 0.0300% or less. The Sr content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Sr content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The Cs content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Cs content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The Hf content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Hf content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The Pb content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Pb content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The Bi content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Bi content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The REM content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The REM content is more preferably 0.0180% or less, and even more preferably 0.0150% or less.
[0058] In the present invention, REM refers to scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanoids ranging from lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. The REM content in the present invention refers to the total content of one or more elements selected from the above-mentioned REM. The REM is not particularly limited, but is preferably La and / or Ce.
[0059] That is, the base steel sheet of the steel sheet of the present invention contains, in mass %, C: 0.05 to 0.30%, Si: 0.10 to 2.00%, Mn: 1.00 to 3.50%, P: 0.001 to 0.100%, S: 0.0001 to 0.0200%, sol. Al: 0.005 to 2.000% and N: 0.010% or less, and optionally Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Cu: 1.000% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less, Zn: 0.0200% or less, Co: 0.020 and at least one selected from the group consisting of Cr: 0.0500% or less, Zr: 0.1000% or less, Ca: 0.0200% or less, Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM: 0.0200% or less, with the balance being Fe and unavoidable impurities.
[0060] Next, the steel structure of a steel sheet (base steel sheet) according to one embodiment of the present invention will be described. The steel sheet of the present invention has a steel structure in which, at a 1 / 4 position in the sheet thickness of the base steel sheet, the area ratios are ferrite: 20.0% to 70.0%, the total of bainitic ferrite and tempered martensite: 20.0% to 70.0%, retained austenite: 3.0% to 20.0%, and fresh martensite: 20.0% or less (including 0.0%), the area ratio of bainitic ferrite out of the total area ratio of bainitic ferrite and tempered martensite is 40% or more, and the average grain size of a hard second phase that is present in the bainitic ferrite and includes retained austenite and fresh martensite is 3.0 μm or less.
[0061] Ferrite area ratio: 20.0% or more and 70.0% or less Soft ferrite is a phase that improves ductility. From the viewpoint of ensuring high ductility, the ferrite area ratio is set to 20.0% or more. The ferrite area ratio is preferably 30.0% or more, more preferably 40.0% or more. On the other hand, if the ferrite area ratio increases excessively, it becomes difficult to achieve a TS of 780 MPa or more. Therefore, the ferrite area ratio is set to 70.0% or less. The ferrite area ratio is preferably 60.0% or less, more preferably 50.0% or less.
[0062] Total area ratio of bainitic ferrite and tempered martensite (excluding retained austenite): 20.0% or more and 70.0% or less. Bainitic ferrite and tempered martensite have intermediate hardness between soft ferrite and hard fresh martensite, and are important phases for ensuring good yield stress (YS) of steel sheets. They are also important for ensuring TS. Therefore, the total area ratio of bainitic ferrite and tempered martensite is set to 20.0% or more, preferably 30.0% or more, and more preferably 40% or more. On the other hand, if the total area ratio of bainitic ferrite and tempered martensite increases excessively, total elongation and / or local elongation decrease. Therefore, the total area ratio of bainitic ferrite and tempered martensite is set to 70.0% or less. The total area ratio of bainitic ferrite and tempered martensite is preferably 60.0% or less, and more preferably 50.0% or less. Bainitic ferrite refers to upper bainitic ferrite that is produced in a relatively high temperature range and contains few carbides.
[0063] Area fraction of retained austenite: 3.0% or more and 20.0% or less From the viewpoint of obtaining good ductility, the area fraction of retained austenite is set to 3.0% or more. The area fraction of retained austenite is preferably 5.0% or more, and more preferably 7.0% or more. On the other hand, if the area fraction of retained austenite increases excessively, fresh martensite formed by stress-induced transformation during shear processing becomes the starting point for void generation, and the desired local elongation (L-El) cannot be obtained. Therefore, the area fraction of retained austenite is set to 20.0% or less. The area fraction of retained austenite is preferably 15.0% or less, and more preferably 10.0% or less.
[0064] Area fraction of fresh martensite: 20.0% or less (including 0.0%) If the area fraction of fresh martensite is excessively increased, in a bending test conforming to the VDA standard (VDA238-100) specified by the German Association of the Automotive Industry, the fresh martensite becomes the origin of void generation, and the desired bendability of the steel sheet (limit bending angle (α) in the VDA bending test) cannot be achieved. From the viewpoint of ensuring good bendability of the steel sheet, the area fraction of fresh martensite is 15.0% or less, preferably 10.0% or less. The lower limit of the area fraction of fresh martensite is not particularly limited and may be 0.0%. Note that fresh martensite is as-quenched (untempered) martensite.
[0065] The proportion of the area fraction of bainitic ferrite to the total area fraction of bainitic ferrite and tempered martensite is 40% or more. Bainitic ferrite contributes to improving ductility. If the area fraction of bainitic ferrite is less than 40% of the total area fraction of bainitic ferrite and tempered martensite, the effect of improving ductility cannot be sufficiently obtained. Therefore, the area fraction of bainitic ferrite is 40% or more of the total area fraction of bainitic ferrite and tempered martensite, preferably 50% or more, and more preferably 60% or more. There is no particular upper limit for the proportion of the area fraction of bainitic ferrite to the total area fraction of bainitic ferrite and tempered martensite, but an excessive increase may result in a decrease in tensile strength (TS). Therefore, the upper limit is preferably 90% or less, more preferably 80% or less.
[0066] Average grain size of the hard second phase, including retained austenite and fresh martensite, present in bainitic ferrite: 3.0 μm or less. Among the hard second phases including retained austenite and fresh martensite, the hard second phase present in bainitic ferrite has a high solute C concentration. Therefore, the retained austenite is highly stable and improves total elongation through stress-induced transformation, while the fresh martensite, although hard, contacts with the intermediate-hardness phase bainitic ferrite, thereby ensuring local elongation and improving tensile strength. Thus, the hard second phase plays an extremely important role in ensuring total elongation and tensile strength. However, if the average grain size of the retained austenite and fresh martensite present in the bainitic ferrite exceeds 3.0 μm, voids will form at the interface between the bainitic ferrite and the hard fresh martensite formed by stress-induced transformation of the hard fresh martensite and / or retained austenite during tensile testing, reducing local elongation. Therefore, the average grain size of the hard second phase including retained austenite and fresh martensite present in the bainitic ferrite is 3.0 μm or less, preferably 2.0 μm or less, and more preferably 1.0 μm or less. Although there is no particular lower limit, the average grain size of the hard second phase present in the bainitic ferrite may be 0.1 μm or more, or may be 0.3 μm or more. In the present invention, the hard second phase includes retained austenite and fresh martensite, or may be composed of retained austenite and fresh martensite.
[0067] The area ratio of the remaining structure other than the above is preferably 20.0% or less. The area ratio of the remaining structure is more preferably 10.0% or less. The area ratio of the remaining structure may also be 0.0%. The remaining structure is not particularly limited, and examples thereof include carbides such as pearlite and cementite. The type of the remaining structure can be confirmed, for example, by observation using a SEM (Scanning Electron Microscope).
[0068] Soft surface layer: The total area ratio of structures other than ferrite is 1 / 2 or less at the 1 / 4 position of the plate thickness. The soft surface layer contributes to suppressing the progression of bending cracks during press forming and vehicle collisions, improving the energy absorption characteristics during bending deformation. The soft surface layer means a decarburized layer, and the total area ratio of structures other than ferrite in the cross section at the 1 / 4 position of the plate thickness is S A When the total area ratio of the structure other than ferrite is S A / 2 or less. In order to obtain excellent energy absorption characteristics during bending deformation of the steel sheet, the soft surface layer is formed in a region of 20 μm or more from the surface of the base steel sheet in the sheet thickness direction. The thickness of the soft surface layer is preferably 25 μm or more, and more preferably 30 μm or more. There is no particular upper limit on the thickness of the soft surface layer, but since an excessively formed soft surface layer causes a decrease in TS, it is preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 120 μm or less. In addition, the total area ratio S of the structure other than ferrite as described above is A The position at 1 / 4 of the plate thickness of the steel plate where the measurement is performed is a non-surface soft layer (a layer in which the structure has not changed due to decarburization and which does not satisfy the conditions of the surface soft layer defined in the present invention).
[0069] Here, the area ratios of ferrite, bainitic ferrite, tempered martensite, and hard phase (hard second phase (retained austenite + fresh martensite)) at a quarter-thickness position of the base steel sheet are measured as follows. That is, a sample is cut out from the base steel sheet so that the thickness cross section parallel to the rolling direction of the base steel sheet serves as the observation surface. Next, the observation surface of the sample is mirror-polished using diamond paste. Next, the observation surface of the sample is finish-polished using colloidal silica, and then etched with 3 vol. % nital to reveal the structure. Then, using a SEM (Scanning Electron Microscope), three fields of view of 25.6 μm × 17.6 μm are photographed at the outermost layer position and the quarter-thickness position of the observation surface of the sample under conditions of an acceleration voltage of 15 kV and a magnification of 5000x. From the obtained structural image, ferrite, bainitic ferrite, tempered martensite, and hard phase (hard second phase (retained austenite + fresh martensite)) are identified as follows.
[0070] Ferrite: A region that is black and has a blocky shape. It contains almost no iron-based carbides. However, if iron-based carbides are contained, the area of the ferrite includes the area of the iron-based carbides. The same applies to bainitic ferrite and tempered martensite, which will be described later. Bainitic ferrite: A region that is black to dark gray and has a blocky or amorphous shape. It contains no iron-based carbides or a relatively small number of iron-based carbides. Tempered martensite: A region that is gray and has an amorphous shape. It contains a relatively large number of iron-based carbides. Hard phase (hard second phase (retained austenite + fresh martensite)): A region that is white to light gray and has an amorphous shape. It does not contain iron-based carbides. When the size is relatively large, the color gradually darkens as it moves away from the interface with other structures, and the interior may be dark gray. Carbides: White regions with a dotted or linear shape. They are contained in tempered martensite, bainitic ferrite, and ferrite. Remaining structure: Pearlite and internal oxides, etc., and their forms are well known.
[0071] Next, the area of each phase identified in the structural image was calculated using the following method. An equally spaced 20 × 20 grid was placed in an area of 25.6 μm × 19.2 μm in actual length on the SEM image at 5000x magnification, and the area ratios of ferrite, bainitic ferrite, tempered martensite, and hard phase (hard second phase) were investigated using a point counting method, in which the number of points on each phase was counted. The area ratio was calculated as the average of three area ratios determined on separate SEM images at 5000x magnification.
[0072] The average grain size of the hard second phase in the bainitic ferrite is measured as follows. Bainitic ferrite is identified in the structural image as described above, and the hard second phase contained in the bainitic ferrite region is identified. The major and minor axes of the hard second phase contained in the bainitic ferrite region are measured, and the sum of the major and minor axes is divided by 2 to determine the grain size. In an SEM image at 5000x magnification, 10 hard second phases with the largest grain sizes are selected from the hard second phases contained in the bainitic ferrite region with the largest continuous area, and their average grain sizes are measured. If 10 hard second phases are not contained in the bainitic ferrite region, the average grain sizes of all the hard second phases are measured. The three average grain sizes obtained using the same procedure for three separate SEM images are then averaged to determine the average grain size of the hard second phase in the bainitic ferrite.
[0073] The area fraction of retained austenite is measured as follows. The base steel sheet is mechanically ground in the thickness direction (depth direction) to a position one-quarter of the sheet thickness, and then chemically polished with oxalic acid to obtain an observation surface. The observation surface is then observed by X-ray diffraction. MoKα rays are used as the incident X-rays, and the ratios of the diffraction intensities of the (200), (220), and (311) planes of fcc iron (austenite) to the diffraction intensities of the (200), (211), and (220) planes of bcc iron are calculated, and the volume fraction of retained austenite is calculated from the ratio of the diffraction intensities of each plane. The retained austenite is then considered to be three-dimensionally homogeneous, and the volume fraction of retained austenite is taken as the area fraction of retained austenite.
[0074] The area fraction of fresh martensite is determined by subtracting the area fraction of retained austenite from the area fraction of the hard phase (hard second phase) determined as described above: [Area fraction of fresh martensite (%)] = [Area fraction of hard second phase (%)] - [Area fraction of retained austenite (%)]
[0075] The area ratio of the remaining structure is calculated by subtracting the area ratio of ferrite, the area ratio of bainitic ferrite, the area ratio of tempered martensite, and the area ratio of the hard phase (hard second phase) calculated as described above from 100.0%: [Area ratio of remaining structure (%)] = 100.0 - [Area ratio of ferrite (%)] - [Area ratio of bainitic ferrite (%)] - [Area ratio of tempered martensite (%)] - [Area ratio of hard second phase (%)]
[0076] For measuring the structure of the soft surface layer, if a zinc-plated layer is formed on the steel sheet, first peel off the zinc-plated layer, and measure the structure in the same manner as at the 1 / 4 position in the sheet thickness direction at 1 μm intervals from a position 1 μm from the surface of the base steel sheet in the sheet thickness direction to a position 100 μm in the sheet thickness direction, and then measure at 20 μm intervals to the center of the sheet thickness.
[0077] Next, the mechanical properties of the steel plate according to one embodiment of the present invention will be described.
[0078] Tensile strength (TS): 780 MPa or more and less than 1180 MPa The tensile strength TS of the steel plate according to one embodiment of the present invention is 780 MPa or more and less than 1180 MPa. The yield stress (YS), total elongation (T-El), local elongation (L-El), bendability of the steel plate, and energy absorption characteristics during bending deformation of the steel plate according to one embodiment of the present invention are as described above.
[0079] The tensile strength (TS), yield stress (YS), total elongation (T-El), and local elongation (L-El) are measured by a tensile test in accordance with JIS Z 2241 (2011) described later in the examples. The bendability of the steel sheet and the energy absorption characteristics during bending deformation are measured by a VDA bending test described later in the examples.
[0080] Galvanized Layer A steel sheet according to one embodiment of the present invention may have a galvanized layer formed on the base steel sheet, and this galvanized layer may be provided on only one surface of the base steel sheet, or on both surfaces.
[0081] The galvanized layer referred to here refers to a plated layer containing Zn as a main component (Zn content: 50.0 mass % or more), and examples thereof include a hot-dip galvanized layer, a galvannealed hot-dip galvanized layer, and an electrogalvanized layer.
[0082] Here, the hot-dip galvanized layer is preferably composed of, for example, Zn, 20.0 mass% or less Fe, and 0.001 mass% to 1.0 mass% Al. The hot-dip galvanized layer may optionally contain one or more elements selected from the group consisting of Pb, Sb, Si, Sn, Mg, Mn, Ni, Cr, Co, Ca, Cu, Li, Ti, Be, Bi, and REM in a total amount of 0.0 mass% to 3.5 mass%. The Fe content of the hot-dip galvanized layer is more preferably less than 7.0 mass%. The remainder other than the above elements is unavoidable impurities.
[0083] The galvannealed layer is preferably composed of, for example, Zn, 20% by mass or less of Fe, and 0.001% by mass to 1.0% by mass or less of Al. The galvannealed layer may optionally contain one or more elements selected from the group consisting of Pb, Sb, Si, Sn, Mg, Mn, Ni, Cr, Co, Ca, Cu, Li, Ti, Be, Bi, and REM in a total amount of 0.0% by mass to 3.5% by mass. The Fe content of the galvannealed layer is more preferably 7.0% by mass or more, and even more preferably 8.0% by mass or more. The Fe content of the galvannealed layer is more preferably 15.0% by mass or less, and even more preferably 12.0% by mass or less. The remainder other than the above elements is unavoidable impurities.
[0084] The electrogalvanized layer is preferably composed of, for example, Zn and 9.0 mass % to 25.0 mass % Ni, the remainder being unavoidable impurities.
[0085] In addition, the coating weight of the hot-dip galvanized layer and the galvannealed hot-dip galvanized layer per side is not particularly limited, but is preferably 20 g / m 2The coating weight of the hot-dip galvanized layer and the galvannealed hot-dip galvanized layer per side is preferably 80 g / m or more. 2 In addition, the plating weight of the electrogalvanized layer per side is not particularly limited, but is preferably 10 g / m or less. 2 The plating weight of the electrogalvanized layer on one side is preferably 70 g / m or more. 2 It is preferable to do the following:
[0086] The coating weight of a zinc-coated layer (hot-dip galvanized layer, galvannealed hot-dip galvanized layer, electrogalvanized layer) is measured as follows. That is, a treatment solution is prepared by adding 0.6 g of a corrosion inhibitor for Fe (Ivit 700BK (registered trademark) manufactured by Asahi Chemical Industry Co., Ltd.) to 1 L of a 10 mass % aqueous hydrochloric acid solution. Next, a steel sheet to be used as a test material is immersed in the treatment solution to dissolve the zinc-coated layer. The mass loss of the test material before and after dissolution is measured, and this value is divided by the surface area of the base steel sheet (the surface area of the part that was covered with the coating) to determine the coating weight (g / m 2 ) is calculated.
[0087] The thickness of the steel plate according to one embodiment of the present invention is not particularly limited, but is preferably 0.6 mm or more, more preferably 0.8 mm or more. The thickness is even more preferably 1.0 mm or more, and most preferably 1.2 mm or more. The thickness of the steel plate is preferably 3.5 mm or less. The thickness is more preferably 2.3 mm or less. The width of the steel plate according to the present invention is not particularly limited, but is preferably 500 mm or more, and more preferably 750 mm or more. The width of the steel plate is preferably 1600 mm or less, and more preferably 1450 mm or less. [2. Method for Manufacturing Steel Plate] Next, a method for manufacturing a steel plate according to one embodiment of the present invention will be described.
[0088] A method for producing a steel sheet according to one embodiment of the present invention includes a hot rolling step of hot rolling a steel slab having the above-described chemical composition to obtain a hot-rolled steel sheet; a pickling step of pickling the hot-rolled steel sheet; an annealing step of annealing the steel sheet after the pickling step under conditions of an annealing temperature of 720°C to 860°C, a holding time of 20 seconds or more, and an atmosphere with a dew point of -10°C or higher; a rapid heating step of rapidly heating the steel sheet from the annealing temperature to annealing temperature +10°C or higher at a heating rate of 10°C / second or higher; and a first cooling step of cooling the steel sheet after the rapid heating step to a first cooling stop temperature of 400°C to 600°C. The method includes a cooling step, a holding step in which the steel sheet is held in a temperature range of 400°C or higher and 600°C or lower for a holding time of less than 300 seconds, a second cooling step in which the steel sheet after the holding step is cooled to a second cooling stop temperature of 100°C or higher and 300°C or lower, and a reheating and holding step in which the steel sheet after the second cooling step is heated to a tempering temperature range of 460°C or lower and held in the above temperature range for a tempering time of 10 seconds or higher and 2000 seconds or lower, or may further include a cold rolling step in which the steel sheet after the pickling step and before the annealing step is cold rolled at a reduction ratio of 20% or higher and 80% or lower to obtain a cold-rolled steel sheet. The passing speed LS (m / min) of the steel sheet in the annealing step preferably satisfies the following formula (1): 3.0 / (t×W×4.716×10 ―4 )<LS<390.0 / (t×W×4.716×10 ―4 ) Equation (1) In equation (1), t is the plate thickness (mm) after the pickling process and before the annealing process, and W is the plate thickness (mm) after the pickling process and before the annealing process. Note that, unless otherwise specified, the above temperatures refer to the surface temperatures of the steel slab and the steel plate.
[0089] First, a steel slab having the above-described composition is prepared. For example, a steel material is melted to obtain molten steel having the above-described composition. The melting method is not particularly limited, and known melting methods such as converter melting and electric furnace melting can be used. Next, the obtained molten steel is solidified to obtain a steel slab. The method for obtaining a steel slab from molten steel is not particularly limited, and for example, a continuous casting method, an ingot casting method, or a thin slab casting method can be used. From the viewpoint of preventing macrosegregation, it is preferable to adopt a continuous casting method as a method for obtaining a steel slab from molten steel.
[0090] (Hot Rolling Process) Next, in the hot rolling process, the steel slab is hot rolled to produce a hot-rolled steel sheet. Hot rolling may be performed using an energy-saving process. Examples of the energy-saving process include direct rolling (a method in which the steel slab is not cooled to room temperature, but is charged into a heating furnace as a hot slab and hot-rolled) and direct rolling (a method in which the steel slab is briefly kept at a constant temperature and then immediately rolled).
[0091] The hot rolling conditions are not particularly limited, and can be, for example, the following conditions. That is, the steel slab is once cooled to room temperature, and then reheated and rolled. The slab heating temperature (reheating temperature) is preferably 1100°C or higher from the viewpoint of dissolving carbides and reducing the rolling load. Furthermore, in order to prevent an increase in scale loss, the slab heating temperature is preferably 1300°C or lower. The slab heating temperature is based on the temperature of the steel slab surface.
[0092] Next, the steel slab is subjected to rough rolling according to a conventional method to obtain a rough-rolled plate (hereinafter also referred to as a sheet bar). The sheet bar is then subjected to finish rolling to obtain a hot-rolled steel plate. When the slab heating temperature is low, it is preferable to heat the sheet bar using a bar heater or the like before finish rolling in order to prevent problems during finish rolling. The finish rolling temperature is preferably 800°C or higher to reduce the rolling load. Furthermore, if the reduction rate in the unrecrystallized austenite state becomes high, an abnormal structure elongated in the rolling direction may develop, which may reduce the workability of the annealed sheet. Furthermore, by setting the finish rolling temperature to 800°C or higher, the steel structure at the hot-rolled steel plate stage, and ultimately the steel structure of the final product, tends to become uniform. A non-uniform steel structure tends to reduce bendability. On the other hand, if the finish rolling temperature exceeds 950°C, the amount of oxide (scale) generated increases. As a result, the interface between the base steel and the oxide may become rough, which may deteriorate the surface quality of the steel sheet after pickling and cold rolling. Furthermore, the crystal grains may become coarse, which may cause a decrease in the strength and bendability of the steel sheet. Therefore, the finish rolling temperature is preferably set in the range of 950°C or less. For these reasons, the finish rolling temperature is preferably set in the range of 800°C or more and 950°C or less.
[0093] After finish rolling, the hot-rolled steel sheet is coiled. The coiling temperature is preferably 450°C or higher, and 750°C or lower.
[0094] Note that the sheet bars may be joined together during hot rolling and continuous finish rolling may be performed. The sheet bars may also be wound up before finish rolling. Furthermore, in order to reduce the rolling load during hot rolling, some or all of the finish rolling may be performed as lubricated rolling. Performing lubricated rolling is also effective from the viewpoint of uniforming the shape and material properties of the steel sheet. Note that the friction coefficient during lubricated rolling is preferably in the range of 0.10 to 0.25. In a hot rolling process (hot rolling process) including rough rolling and finish rolling, a steel slab is generally made into a sheet bar by rough rolling and then made into a hot-rolled steel sheet by finish rolling. However, depending on the mill capacity, etc., such classification is not essential as long as the desired size is achieved.
[0095] (Pickling process) The hot-rolled steel sheet after the hot rolling process is pickled. Pickling can remove oxides from the steel sheet surface, ensuring good chemical conversion treatability and plating quality. Pickling may be carried out once or multiple times. The pickling conditions are not particularly limited, and may be carried out in accordance with conventional methods.
[0096] (Cold Rolling Process) Next, if necessary, the hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. Cold rolling is performed, for example, by multi-pass rolling requiring two or more passes, such as tandem multi-stand rolling or reverse rolling. The cold-rolling reduction (cumulative reduction) is 20% or more and 80% or less. If the cold-rolling reduction is less than 20%, the steel structure is likely to become coarse and non-uniform in the annealing process, which may result in a decrease in TS and bendability in the final product. On the other hand, if the cold-rolling reduction exceeds 80%, the steel sheet is likely to have a defective shape and the amount of zinc coating may become non-uniform. Optionally, the cold-rolled steel sheet obtained after cold rolling may be pickled.
[0097] (Annealing step) Next, in one embodiment of the present invention, after the pickling step (or after the cold rolling step in the case of cold rolling), the steel sheet obtained as described above is heated and annealed (held) at an annealing temperature of 720°C or higher and 860°C or lower for a holding time (annealing time) of 20 seconds or longer. Note that the number of annealing steps may be two or more, but one time is preferred from the viewpoint of energy efficiency. The annealing step is a step including this temperature raising treatment and soaking treatment.
[0098] Annealing temperature: 720°C or higher and 860°C or lower. If the annealing temperature is lower than 720°C, the rate of carbon oxidation in the surface layer of the steel sheet decreases, making it impossible to achieve the desired soft surface layer thickness. Furthermore, the proportion of austenite generated during heating in the two-phase region of ferrite and austenite may be insufficient. As a result, the area fraction of ferrite may increase excessively after heat treatment, resulting in a decrease in TS. On the other hand, if the annealing temperature exceeds 860°C, the proportion of austenite, which has a slow carbon diffusion rate, increases, reducing the carbon diffusion rate to the surface layer where the decarburization reaction progresses, resulting in diffusion-limited behavior, making it impossible to achieve the desired soft surface layer thickness. Furthermore, the proportion of austenite generated during annealing may be excessive, resulting in the ferrite area fraction being less than 20.0% after heat treatment. Therefore, the annealing temperature is set to 720°C or higher and 860°C or lower. The annealing temperature is preferably 850°C or lower. The annealing temperature is the maximum temperature reached in the annealing process.
[0099] Holding time (annealing time): 20 seconds or more If the holding time is less than 20 seconds, the time for the decarburization reaction to occur in the surface layer is insufficient, and the desired soft surface layer thickness cannot be obtained. Therefore, the holding time (annealing time) is set to 20 seconds or more. The holding time is preferably 30 seconds or more, and more preferably 50 seconds or more. Although the upper limit of the holding time is not particularly limited, the holding time is preferably 900 seconds or less, and more preferably 800 seconds or less. The holding time is the holding time in a temperature range of (annealing temperature - 40°C) or more and the annealing temperature or less. In other words, the holding time (annealing time) includes not only the holding time at the annealing temperature but also the residence time in a temperature range of (annealing temperature - 40°C) or more and the annealing temperature or less during heating before reaching the annealing temperature.
[0100] Dew point of atmosphere in annealing step (annealing atmosphere): -10°C or higher In one embodiment of the present invention, the dew point of the atmosphere in the annealing step (annealing atmosphere) is -10°C or higher. By performing annealing in the annealing step with a dew point of the annealing atmosphere of -10°C or higher, the decarburization reaction is promoted and a soft surface layer having a desired thickness can be formed. The dew point of the annealing atmosphere in the annealing step is more preferably 0°C or higher, even more preferably 5°C or higher, and even more preferably 10°C or higher. There is no particular upper limit for the dew point of the annealing atmosphere in the annealing step, but in order to improve plating adhesion when a zinc-plated layer is formed, the dew point of the annealing atmosphere in the annealing step is preferably 30°C or lower.
[0101] 3.0 / (t×W×4.716×10 ―4 )<LS<390.0 / (t×W×4.716×10 ―4 ) Equation (1) In the present invention, from the viewpoint of production efficiency, it is preferable that the steel sheet threading speed LS (m / min) in the annealing process satisfies equation (1). In equation (1), t: sheet thickness (mm), W: sheet width (mm). The sheet thickness t is the sheet thickness after the pickling process and before the annealing process, and the sheet width W is the sheet width after the pickling process and before the annealing process. The production efficiency can be E, which is expressed by the following equation (2): E (ton / h) = LS x t x W x ρ x 60 x 10 ―6 ...Equation (2) In equation (2), t: plate thickness (mm), W: plate width (mm), ρ: specific gravity of iron (ton / m 3 ), and ρ=7.86 (ton / m 3), where E is preferably greater than 3.0 and less than 390.0. Based on this formula (2), the above formula (1) can be derived. If E is 3.0 ton / h or less, the soft surface layer may be excessively formed, resulting in insufficient TS. On the other hand, if E is 390.0 ton / h or more, the soft surface layer may not be sufficiently formed, resulting in insufficient energy absorption characteristics during bending deformation. Therefore, E is preferably greater than 3.0 and less than 390.0. Furthermore, E is more preferably 16.0 ton / h or more. Furthermore, E is more preferably 190.0 ton / h or less. From the above, LS (m / min) can be calculated by the following formula: 3.0 / (t×W×4.716×10 ―4 LS (m / min) is preferably 16.0 / (t×W×4.716×10 ―4 ) or more. LS (m / min) is 390.0 / (t×W×4.716×10 ―4 LS (m / min) is preferably less than 190.0 / (t×W×4.716×10 ―4 ) or less is more preferable.
[0102] The sheet passing speed LS (m / min) is calculated by dividing the distance (m) traveled by the steel sheet in the annealing process by the time (min) required for the steel sheet to be transported in the annealing process.
[0103] A radiant tube furnace is generally used as the heat treatment furnace for the annealing process. The annealing temperature is obtained using a thermometer that measures the surface temperature of the steel sheet. The temperature measurement method is not particularly limited, but for example, a radiation thermometer that measures the temperature by sensing infrared rays emitted by the steel sheet is suitable. In the case of a radiation thermometer, since it may be affected by reflected light of infrared rays emitted by the surrounding furnace body, a cover may be provided between the measurement part of the radiation thermometer and the detection part of the steel sheet. Furthermore, since it may be affected by the emissivity of the steel sheet surface, a multi-reflection measurement method that utilizes the wedge-shaped space between the transport roll in the furnace and the steel sheet may be adopted.
[0104] (Rapid Heating Step) In one embodiment of the present invention, after the annealing step, the steel sheet obtained as described above is heated (rapidly heated) from the annealing temperature to a temperature 10°C higher than the annealing temperature at a heating rate of 10°C / sec or more. When annealing is performed two or more times in the annealing step described above, the treatment in the rapid heating step performed after annealing may also be performed two or more times, but the treatment in the rapid heating step may be performed only once.
[0105] Heating rate from the annealing temperature: 10°C / sec or more. If the heating rate from the annealing temperature in the rapid heating step is less than 10°C / sec, Mn diffuses from ferrite to the austenite formed in the rapid heating step, reducing the amount of bainitic ferrite formed in the subsequent cooling and holding steps. As a result, a structure in which the area ratio of bainitic ferrite is 40% or more of the total area ratio of bainitic ferrite and tempered martensite cannot be obtained. Therefore, the heating rate from the annealing temperature in the rapid heating step is set to 10°C / sec or more. Furthermore, the heating rate in the rapid heating step is preferably 30°C / sec or more. By setting the heating rate to 30°C / sec or more, the diffusion of Mn from ferrite to austenite is suppressed, austenite can be generated only by the diffusion of C, and the line length can be further shortened. On the other hand, if the heating rate exceeds 300°C / sec, there is a risk of buckling deformation of the steel sheet due to thermal stress, and local high-temperature areas may occur in the sheet width direction, resulting in a loss of uniformity. Therefore, the temperature rise rate is preferably 300° C. / sec or less, and more preferably 150° C. / sec or less.
[0106] In the rapid heating step, the steel is rapidly heated to a temperature (rapid heating step temperature) that is 10°C or higher than the annealing temperature. If the temperature (rapid heating step temperature) in the rapid heating step is less than 10°C higher than the annealing temperature, austenite cannot be sufficiently formed by rapid heating, and a structure with the desired total area ratio of bainitic ferrite and tempered martensite, or a structure in which the area ratio of bainitic ferrite in the total area ratio of bainitic ferrite and tempered martensite is 40% or higher, cannot be formed. Therefore, the rapid heating does not improve at least one of YS, TS, ductility, and bendability, and the desired mechanical properties may not be ensured. The temperature (rapid heating step temperature) in the rapid heating step is preferably 30°C or higher than the annealing temperature, and more preferably 50°C or higher than the annealing temperature. The upper limit of the temperature reached in the rapid heating step is not particularly determined, but from the viewpoint of production efficiency, it is preferably the annealing temperature + 210°C or less, more preferably the annealing temperature + 150°C or less, and even more preferably the annealing temperature + 120°C or less.
[0107] The induction heating (IH) device in the rapid heating step rapidly heats the steel sheet by adjusting its output so that the temperature of the steel sheet is within the annealing temperature +10°C or more (preferably, 740°C or more and 940°C or less). Furthermore, when heating within this temperature range, the induction heating (IH) device is preferably a transverse type. The appropriate rapid heating temperature varies depending on the chemical composition of the steel sheet. Therefore, it is preferable to predict a suitable temperature range in advance by measurement, calculation, or simulation and set it taking into account the temperature of the steel sheet in the annealing step. The temperature reached in the rapid heating step can be measured using a thermometer that measures the surface temperature of the steel sheet. The temperature measurement method is not particularly limited, but a radiation thermometer that measures the temperature by sensing infrared rays emitted by the steel sheet is suitable. In the case of a radiation thermometer, since it may be affected by reflected light of infrared rays emitted by the surrounding furnace body, a cover may be provided between the measurement unit of the radiation thermometer and the detection unit of the steel sheet. Furthermore, since it may be affected by the emissivity of the steel sheet surface, a multi-reflection measurement method utilizing a wedge-shaped space between the transport roll in the furnace and the steel sheet may be adopted. It is also desirable to use a scanning radiation thermometer to measure the temperature at each position in the width direction of the steel plate.
[0108] (First Cooling Step) Next, the steel sheet after annealing as described above (after the rapid heating step) is cooled to a temperature of 400°C or higher and 600°C or lower (first cooling stop temperature) in the first cooling step.
[0109] First cooling stop temperature: 400°C or higher and 600°C or lower If the first cooling stop temperature is lower than 400°C, the formation of bainitic ferrite is promoted, and the area fraction of the retained austenite formed together with the bainitic ferrite exceeds a predetermined amount, making it impossible to achieve the desired local elongation. On the other hand, if the first cooling stop temperature exceeds 600°C, the area fraction of ferrite and pearlite increases excessively, causing the total area fraction of bainitic ferrite and tempered martensite to be less than 20.0%, resulting in a decrease in TS. Therefore, the first cooling stop temperature in the first cooling step is set to 400°C or higher and 600°C or lower. The first cooling stop temperature is preferably 460°C or higher. Furthermore, the first cooling stop temperature is preferably 550°C or lower.
[0110] (Holding Step) After the first cooling step, in the holding step, the steel sheet is held in a temperature range of 400° C. or higher and 600° C. or lower (hereinafter also referred to as a holding temperature range) for less than 300 seconds.
[0111] Holding time in the holding temperature range: less than 300 seconds. During the holding process, bainitic ferrite is generated, and C diffuses from the generated bainitic ferrite to the untransformed austenite adjacent to the bainitic ferrite. As a result, a predetermined area fraction of retained austenite is secured. Here, if the holding time in the holding temperature range is 300 seconds or longer, excessive diffusion of C and Mn from the bainitic ferrite to the untransformed austenite occurs, resulting in the formation of a coarse, hard second phase (retained austenite and fresh martensite) in the bainitic ferrite, which may prevent the desired bendability or local elongation from being achieved. Furthermore, excessive formation of bainitic ferrite may result in an excessive total area fraction of bainitic ferrite and tempered martensite, resulting in reduced local elongation. Therefore, the holding time in the holding temperature range is preferably less than 300 seconds. The holding time in the holding temperature range is more preferably less than 80 seconds, and even more preferably less than 60 seconds. The holding time in the holding temperature range does not include the residence time in the temperature range after the galvanizing treatment in the hot dip galvanizing step.
[0112] (Galvanizing process (hot-dip galvanizing process, alloying process)) When a hot-dip galvanized steel sheet or a galvannealed hot-dip galvanized steel sheet is obtained, the steel sheet is subjected to a galvanizing process (hot-dip galvanizing process, or further to a galvannealed hot-dip galvanizing process) after the above-mentioned holding process and before the second cooling process. A galvanized steel sheet can be obtained by performing a galvanizing process. Examples of the galvanizing process here include a hot-dip galvanizing process and a galvannealed hot-dip galvanizing process (hot-dip galvanizing process and alloying process). A hot-dip galvanized steel sheet can be obtained by performing a hot-dip galvanizing process on a steel sheet, and a galvannealed hot-dip galvanized steel sheet can be obtained by further performing an alloying process. Hereinafter, the hot-dip galvanizing process and the alloying process will also be collectively referred to as a galvannealed hot-dip galvanizing process.
[0113] In the case of hot-dip galvanizing, it is preferable to immerse the steel sheet in a hot-dip galvanizing bath at 440°C or higher and 500°C or lower, and then adjust the coating weight by gas wiping or the like. The hot-dip galvanizing bath is not particularly limited as long as it provides the above-mentioned composition of the zinc coating layer, but it is preferable to use a plating bath with a composition containing 0.10 mass% or more of Al, with the balance consisting of Zn and unavoidable impurities. The Al content is preferably 0.23 mass% or lower.
[0114] Furthermore, in the case of alloying hot-dip galvanizing treatment, after performing the hot-dip galvanizing treatment as described above, it is preferable to perform alloying treatment by heating the galvanized steel sheet to an alloying temperature of 450°C or higher. The alloying temperature is preferably 600°C or lower. If the alloying temperature is lower than 450°C, the Zn-Fe alloying rate will be slow, and alloying may become difficult. On the other hand, if the alloying temperature exceeds 600°C, untransformed austenite will transform to pearlite, making it difficult to achieve a TS of 780 MPa or higher, and ductility will decrease. The alloying temperature is more preferably 470°C or higher. Furthermore, the alloying temperature is more preferably 570°C or lower.
[0115] The coating weight of both the hot-dip galvanized steel sheet (GI) and the galvannealed steel sheet (GA) was 20 g / m per side. 2 The coating weight of the zinc plating layer on one side is preferably 80 g / m or more. 2 It is preferable that the plating thickness is set to the following: The plating thickness can be adjusted by gas wiping or the like.
[0116] (Second Cooling Step) Next, the steel sheet after the galvanizing step in the case of obtaining a hot-dip galvanized steel sheet or a galvannealed hot-dip galvanized steel sheet, or after the holding step in the case of obtaining a steel sheet or an electrogalvanized steel sheet, is cooled to a second cooling stop temperature of 100°C or higher and 300°C or lower.
[0117] Second Cooling Stop Temperature: 100°C or More and 300°C or Less The second cooling step is necessary to control the area fraction of tempered martensite and the area fraction of retained austenite generated in the subsequent reheating and holding step within a predetermined range. Here, if the second cooling stop temperature is less than 100°C, the untransformed austenite present in the steel in the second cooling step is almost entirely transformed into martensite. Ultimately, the area fraction of tempered martensite increases excessively, making it impossible to achieve an area fraction of bainitic ferrite of 40% or more of the total area fraction of bainitic ferrite and tempered martensite, resulting in a decrease in El. On the other hand, if the second cooling stop temperature exceeds 300°C, the area fraction of tempered martensite decreases and the area fraction of fresh martensite increases. As a result, the desired bendability cannot be achieved. Therefore, the second cooling stop temperature is set to 100°C or more and 300°C or less. The second cooling stop temperature is preferably 120°C or more. The second cooling stop temperature is also preferably 280°C or less.
[0118] (Reheating and Holding Step) Next, the steel sheet is reheated to a tempering temperature of 460°C or lower (hereinafter also referred to as the reheating temperature range), and the steel sheet is held in the tempering temperature range of 460°C or lower for a tempering time of 10 seconds to 2000 seconds. This tempers the martensite present in the steel at the end of the second cooling step. In addition, the C supersaturated in the martensite is diffused into the untransformed austenite, thereby generating austenite that is stable at room temperature, i.e., retained austenite.
[0119] Tempering temperature (reheating temperature): 460°C or less. The lower limit of the tempering temperature (reheating temperature) is not particularly limited, but if the temperature is 300°C or less, the martensite present in the steel at the end of the second cooling step will not be sufficiently tempered, resulting in an excessive increase in fresh martensite. In addition, the coarsening of carbides in the tempered martensite will not proceed sufficiently, increasing the density of carbides in the tempered martensite. As a result, there is a risk of reduced bendability or local elongation. Therefore, the tempering temperature is preferably above 300°C. The tempering temperature is preferably 340°C or higher, and more preferably 360°C or higher. On the other hand, if the tempering temperature (reheating temperature) exceeds 460°C, the martensite present in the steel at the end of the second cooling step will be excessively tempered, making it difficult to achieve a TS of 780 MPa or higher. Furthermore, the untransformed austenite present in the steel at the end of the second cooling step will decompose into carbides (pearlite), resulting in reduced ductility. Therefore, the tempering temperature (reheating temperature) is set to 460° C. or lower. The tempering temperature is the maximum temperature reached in the reheating and holding step. The tempering temperature is preferably 440° C. or lower, and more preferably 420° C. or lower.
[0120] Tempering time (holding time) in the reheating temperature range: 10 seconds or more and 2000 seconds or less. If the tempering time (holding time) in the reheating temperature range is less than 10 seconds, the martensite present in the steel at the end of the second cooling step will not be sufficiently tempered, resulting in an excessive increase in fresh martensite. Furthermore, the carbides in the tempered martensite will not be sufficiently coarsened, resulting in an excessive density of the carbides in the tempered martensite. As a result, the desired bendability and local elongation cannot be achieved. On the other hand, if the tempering time (holding time) in the reheating temperature range exceeds 2000 seconds, the martensite present in the steel at the end of the second cooling step will be excessively tempered, making it difficult to achieve a TS of 780 MPa or more. Furthermore, the untransformed austenite present in the steel at the end of the second cooling step may decompose into carbides (pearlite), resulting in a decrease in ductility. Therefore, the tempering time (holding time) in the reheating temperature range is set to 10 seconds or more and 2000 seconds or less. The tempering time is preferably 20 seconds or more, more preferably 30 seconds or more. The tempering time is preferably 1000 seconds or less, more preferably 500 seconds or less, and even more preferably 100 seconds or less. The tempering time (holding time) in the reheating temperature range includes not only the holding time at the reheating temperature, but also the residence time in that temperature range during heating and cooling before and after reaching the reheating temperature.
[0121] The cooling conditions after holding in the reheating temperature range are not particularly limited and may be conventional. Examples of cooling methods that can be used include gas jet cooling, mist cooling, roll cooling, water cooling, and air cooling. From the viewpoint of preventing surface oxidation, the material is preferably cooled to 50°C or less after holding in the reheating temperature range, and more preferably cooled to room temperature. The average cooling rate after holding in the reheating temperature range is preferably, for example, 1°C / sec or more and 50°C / sec or less.
[0122] (Zinc plating step (electrogalvanizing step)) After cooling to room temperature, an electrogalvanizing treatment may be performed. By subjecting the steel sheet to electrogalvanizing treatment, an electrogalvanized steel sheet can be obtained. When electrogalvanizing the steel sheet surface, the treatment conditions for the electrogalvanizing treatment are not particularly limited, and may be performed in accordance with a conventional method.
[0123] The steel sheet obtained as described above may further be subjected to temper rolling. If the temper rolling reduction exceeds 2.00%, the yield stress increases, which may result in a decrease in dimensional accuracy when the steel sheet is formed into a component. Therefore, the temper rolling reduction is preferably 2.00% or less. The lower limit of the temper rolling reduction is not particularly limited, but is preferably 0.05% or more from the viewpoint of productivity. Furthermore, temper rolling may be performed on an apparatus continuous with the annealing apparatuses used for the above-mentioned processes (online), or may be performed on an apparatus discontinuous with the annealing apparatuses used for the above-mentioned processes (offline). Furthermore, the number of times of temper rolling may be one, two, or more. Furthermore, rolling using a leveler or the like may be performed as long as it can impart an elongation rate equivalent to that of temper rolling.
[0124] The conditions other than those mentioned above are not particularly limited, and may be those according to conventional methods.
[0125] [3. Member] Next, a member according to one embodiment of the present invention will be described. The member according to one embodiment of the present invention is a member made using (using as a raw material) the above-mentioned steel plate. For example, the raw material steel plate is subjected to at least one of forming and joining to form a member. Here, the above-mentioned steel plate has a TS of 780 MPa or more, a high YS, and excellent total elongation, local elongation, bendability, and energy absorption properties. Therefore, the member according to one embodiment of the present invention has high strength and excellent impact resistance properties. Therefore, the member according to one embodiment of the present invention is particularly suitable for application to impact energy absorbing members used in the automotive field.
[0126] [4. Manufacturing Method of Member] Next, a manufacturing method of a member according to one embodiment of the present invention will be described. The manufacturing method of a member according to one embodiment of the present invention includes a step of subjecting the above-mentioned steel plate (for example, a steel plate manufactured by the above-mentioned manufacturing method of steel plate) to at least one of forming and joining to form a member. Here, the forming method is not particularly limited, and for example, a general processing method such as press working can be used. Furthermore, the joining method is also not particularly limited, and for example, general welding such as spot welding, laser welding, and arc welding, rivet joining, caulking joining, etc. can be used. Note that the forming conditions and joining conditions are not particularly limited, and may be in accordance with conventional methods.
[0127] Steel materials having the chemical compositions shown in Table 1 (the balance being Fe and unavoidable impurities) were melted in a converter and then cast into steel slabs by continuous casting. In Table 1, "-" indicates the content of unavoidable impurities.
[0128] The obtained steel slabs were heated to 1200°C, and after heating, the steel slabs were subjected to hot rolling consisting of rough rolling and finish rolling at a finish rolling temperature of 900°C to obtain hot-rolled steel sheets. Next, of the obtained hot-rolled steel sheets, Nos. 1, 4 to 24, 27 to 49, 51 to 58, 61 to 75, 77 to 84, and 87 to 98 were subjected to pickling and cold rolling (reduction rate: 50%) to obtain cold-rolled steel sheets with the thicknesses shown in Table 2. In addition, of the obtained hot-rolled steel sheets, Nos. 2 to 3, 25 to 26, 50, 59 to 60, 76, and 85 to 86 were subjected to pickling to obtain hot-rolled steel sheets (white skin) with the thicknesses shown in Table 2. Next, the obtained cold-rolled steel sheet or hot-rolled steel sheet (white skin) was subjected to the annealing step, rapid heating step, first cooling step, holding step, galvanizing step, second cooling step, and reheating and holding step under the conditions shown in Table 2 to obtain a steel sheet. Also, the cold-rolled steel sheet was obtained by performing the treatments excluding the galvanizing step. The electrogalvanized steel sheet was obtained by performing the treatments excluding the holding step and galvanizing step, more specifically, the reheating and holding step followed by the electrogalvanizing step.
[0129] Here, the galvanizing process involves hot-dip galvanizing, galvannealing, or electrogalvanizing to obtain hot-dip galvanized steel sheets (hereinafter also referred to as GI), galvannealed hot-dip galvanized steel sheets (hereinafter also referred to as GA), or electrogalvanized steel sheets (hereinafter also referred to as EG). In Table 2, the types of plating processes are also indicated as "GI," "GA," and "EG." In Table 2, GI and EG steel sheets are not subjected to alloying treatment, and therefore the alloying temperature is indicated as "-." In Table 2, cold-rolled steel sheets obtained without undergoing galvanizing treatment in the galvanizing process are indicated as "CR."
[0130] The galvanizing bath temperature was 470°C for both GI and GA production. The galvanizing coating weight was 10 to 70 g / m when producing EG. 2 When manufacturing GI, the weight is 45 to 72 g / m per side. 2 When manufacturing GA, the thickness is 45 g / m per side. 2 The zinc plating layers of the finally obtained zinc-plated steel sheets had the following compositions: GI: 0.1 to 1.0 mass% Fe, 0.2 to 0.33 mass% Al, and the balance being Zn and unavoidable impurities; GA: 8.0 to 12.0 mass% Fe, 0.1 to 0.23 mass% Al, and the balance being Zn and unavoidable impurities; EG: 9.0 to 25.0 mass% Ni, and the balance being Zn and unavoidable impurities. The zinc plating layers were formed on both sides of the base steel sheet in all cases.
[0131] Using the obtained steel sheet, the steel structure of the base steel sheet was identified in the manner described above. The measurement results are shown in Table 2. In Table 3, F is ferrite, BF is bainitic ferrite, TM is tempered martensite, RA is retained austenite, FM is fresh martensite, and P is pearlite. In addition, in the manner described above, the surface layer in which the total area ratio of structures other than ferrite was ½ or less at the ¼ position of the sheet thickness was determined to be the soft surface layer.
[0132] In addition, the tensile strength (TS), yield stress (YS), total elongation (T-El), local elongation (L-El), limit bending angle (α) in the VDA bending test, bending deformation absorbed energy amount, and production efficiency (E) were evaluated according to the following criteria.
[0133] ・TS ◯ (pass): 780 MPa or more and less than 1180 MPa × (fail): less than 780 MPa or 1180 MPa or more
[0134] ・YS 〇 (Pass): (A) If 780MPa≦TS<980MPa, then 400MPa≦YS≦650MPa (B) If 980MPa≦TS<1180MPa, then 600MPa≦YS≦900MPa × (Fail): (A) If 780MPa≦TS<980MPa, then 400MPa>YS or 650MPa<YS (B) If 980MPa≦TS<1180MPa, then 600MPa>YS or 900MPa<YS
[0135] ・T-El 〇 (Pass): (A) If 780MPa≦TS<980MPa, 17.0%≦T-El (B) If 980MPa≦TS<1180MPa, 11.0%≦T-El × (Fail): (A) If 780MPa≦TS<980MPa, 17.0%>T-El (B) If 980MPa≦TS<1180MPa, 11.0%>T-El ・L-El 〇 (Pass): (A) If 780MPa≦TS<980MPa, 7.0%≦L-El (B) If 980MPa≦TS<1180MPa, 5.0%≦L-El × (Fail): (A) If 780MPa≦TS<980MPa, 7.0%>L-El (B) When 980 MPa ≦ TS < 1180 MPa, 5.0% > L-Ll
[0136] ・VDA bending test limit bending angle (α) 〇 (pass): 80° or more × (fail): less than 80°
[0137] -Integrated value AE of load F from the start of deformation to the maximum load in the load-stroke curve in the VDA bending test 〇 (Pass): 55,000 N·mm or more × (Fail): Less than 55,000 N·mm
[0138] ・Production efficiency E (ton / h) = LS × t × W × ρ × 60 × 10―6 Pass (A): 16.0<E<190.0 Pass (B): 3.0<E≦16.0, or 190.0≦E<390.0 Pass (C): 3.0≧E or E≧390.0 Where, LS: sheet threading speed in annealing process (m / min) t: sheet thickness after pickling process and before annealing process (mm) W: sheet width after pickling process and before annealing process (mm) ρ: specific gravity of iron (ton / m 3 ) and ρ=7.86 (ton / m 3 )
[0139] (1) Tensile Test The tensile test was conducted in accordance with JIS Z 2241 (2011). That is, JIS No. 5 test specimens were taken from the obtained steel sheets so that the longitudinal direction was perpendicular to the rolling direction of the base steel sheet. Using the taken test specimens, a tensile test was conducted at a crosshead speed of 10 mm / min, and TS, YS, T-El, and L-El were measured. The results are shown in Table 3.
[0140] (2) VDA Bending Test The VDA bending test was conducted in accordance with the VDA standard (VDA238-100) specified by the German Association of the Automotive Industry. Specifically, 70 mm x 60 mm test pieces were taken from the obtained steel sheets by shearing. Here, the 60 mm side was parallel to the rolling (L) direction. One side of the test pieces was ground to a uniform thickness of 1.2 mm, with the inside of the bend being the ground surface. The VDA bending test was conducted on the test pieces under the following conditions. Steel sheets with a thickness of less than 1.2 mm were tested without grinding. Test method: Roll support, punch pushing; Roll diameter: φ30 mm; Punch tip R: 0.4 mm; Distance between rolls: (sheet thickness × 2) + 0.5 mm; Stroke speed: 20 mm / min; Bending direction: Orthogonal to rolling (C) direction. At this time, the angle of the outer bend at the center of the plate-shaped test piece when the load F from the pushing bending jig from above is maximum is measured as the bending angle (limit bending angle) (°). In addition, the obtained load-stroke curve is used to calculate the integral value (absorbed energy) of the load-stroke curve up to the maximum load. The above VDA bending test was performed three times, and the average values of the limit bending angle and the integral value (absorbed energy) of the load-stroke curve at the maximum load are designated α (°) and AE, respectively. The results are shown in Table 3.
[0141] In the VDA bending test of steel sheets with a thickness of more than 1.2 mm, the influence of the sheet thickness was taken into consideration, and all tests were performed on steel sheets with a thickness of 1.2 mm. Steel sheets with a thickness of more than 1.2 mm were ground on one side to make the sheet thickness 1.2 mm. Since the grinding process may affect the bendability of the steel sheet surface, the ground surface was set on the inside of the bend (the side that comes into contact with the punch) in the VDA bending test. On the other hand, in the VDA bending test of steel sheets with a thickness of less than 1.2 mm, the influence of the sheet thickness was small, so the test was performed without grinding.
[0142]
[0143]
[0144]
[0145]
[0146]
[0147] In Tables 1 to 3, underlined values indicate values outside the appropriate range of the present invention. As shown in Table 3, all of the inventive examples passed the test for tensile strength (TS), yield stress (YS), total elongation (T-El), local elongation (L-El), limiting bend angle (α) in the VDA bending test, and the integral value (absorbed energy) (AE) of the load-stroke curve in the VDA bending test. The production efficiency (E) was also good. On the other hand, the comparative examples were insufficient in at least one of tensile strength (TS), yield stress (YS), total elongation (T-El), local elongation (L-El), limiting bend angle (α) in the VDA bending test, and the integral value (absorbed energy) (AE) of the load-stroke curve in the VDA bending test.
[0148] Furthermore, it was found that the members obtained by forming or joining the steel sheets of the present invention had the excellent properties characteristic of the present invention in all of the tensile strength (TS), yield stress (YS), total elongation (T-El), local elongation (L-El), limiting bending angle (α) in the VDA bending test, and integral value (absorbed energy) (AE) of the load-stroke curve in the VDA bending test. It was also found that the production efficiency (E) was good.
[0149] According to the present invention, a steel sheet having a TS of 780 MPa or more and excellent energy absorption properties can be obtained. If a member obtained from the steel sheet of the present invention is used as an automobile part, it can contribute to reducing the weight of the automobile and greatly contribute to improving the performance of the automobile body.
Claims
1. A steel plate comprising a base steel plate, the base steel plate comprising, in mass %, C: 0.05 to 0.30%, Si: 0.10 to 2.00%, Mn: 1.00 to 3.50%, P: 0.001 to 0.100%, S: 0.0001 to 0.0200%, sol. a steel structure having a component composition containing Al: 0.005-2.000% and N: 0.010% or less, with the balance being Fe and unavoidable impurities, and at a 1 / 4 position of the sheet thickness of the base steel sheet, the steel structure has, in area ratios, ferrite: 20.0% or more and 70.0% or less, a total of bainitic ferrite and tempered martensite: 20.0% or more and 70.0% or less, retained austenite: 3.0% or more and 20.0% or less, and fresh martensite: 20.0% or less (including 0.0%), the proportion of the area ratio of bainitic ferrite in the total area ratio of the bainitic ferrite and tempered martensite is 40% or more, and a hard second phase which is present in the bainitic ferrite and contains the retained austenite and the fresh martensite has an average grain size of 3.0 μm or less, The steel sheet further has a surface soft layer formed to a thickness of 20 μm or more from the surface of the base steel sheet in the sheet thickness direction, the total area ratio of structures other than ferrite in the steel structure being ½ or less at the ¼ position in the sheet thickness, and the tensile strength being 780 MPa or more and less than 1180 MPa.
2. The composition further includes, in mass%, Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Cu: 1.000% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less, Zn: 0.0200% or less, Co: 0.0200% or less, Zr: 0.1000% or less, Ca: 0.0200% or less, Se: 0.0200% or less, The steel plate according to claim 1, containing at least one selected from Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM: 0.0200% or less.
3. The steel sheet according to claim 1 or 2, which has a zinc-plated layer on one or both sides of the base steel sheet.
4. A member made using the steel plate according to any one of claims 1 to 3.
5. A hot rolling process in which a steel slab having the chemical composition according to claim 1 or 2 is hot-rolled to obtain a hot-rolled steel sheet; a pickling process in which the hot-rolled steel sheet is pickled; an annealing process in which the steel sheet after the pickling process is heated and annealed under conditions of an annealing temperature of 720°C to 860°C, a holding time of 20 seconds or more, and an atmosphere with a dew point of -10°C or higher; a rapid heating process in which the steel sheet after the rapid heating process is rapidly heated from the annealing temperature to the annealing temperature + 10°C or higher under conditions of a heating rate of 10°C / sec or higher; a first cooling process in which the steel sheet after the rapid heating process is cooled to a first cooling stop temperature of 400°C to 600°C; a holding process in which the steel sheet is held in a temperature range of 400°C to 600°C for a holding time of less than 300 seconds; and a second cooling process in which the steel sheet after the holding process is cooled to a second cooling stop temperature of 100°C to 300°C. a reheating and holding step of heating the steel sheet after the second cooling step to a tempering temperature of 460°C or less and holding the steel sheet in the temperature range for a tempering time of 10 seconds or more and 2000 seconds or less, or further comprising a cold rolling step of cold rolling the steel sheet after the pickling step and before the annealing step at a rolling reduction of 20% or more and 80% or less to obtain a cold-rolled steel sheet.
6. The method for producing a steel sheet according to claim 5, wherein the steel sheet passing speed LS (m / min) in the annealing step satisfies the following formula (1): 3.0 / (t×W×4.716×10 ―4 )<LS<390.0 / (t×W×4.716×10 ―4 ) Formula (1) where, t: sheet thickness (mm) after the pickling process and before the annealing process, and W: sheet width (mm) after the pickling process and before the annealing process.
7. A method for producing a steel sheet according to claim 5 or 6, comprising, after the holding step and before the second cooling step, a hot-dip galvanizing step of applying a galvanizing treatment to a surface of the steel sheet to form a galvanized layer on the surface of the steel sheet, or further comprising an alloying treatment step of applying an alloying treatment to the steel sheet on which the galvanized layer has been formed.
8. The method for producing a steel sheet according to claim 5 or 6, further comprising, after the reheating and holding step, an electrogalvanizing step of immersing the steel sheet in an electrogalvanizing bath to form a zinc-plated layer on the steel sheet.
9. A method for manufacturing a component, comprising the step of subjecting the steel plate according to any one of claims 1 to 3 to at least one of forming and joining to form a component.
Citation Information
Patent Citations
High-strength hot-dip galvanized steel sheet with excellent workability and method for manufacturing the same
JP5256689B2
High-strength hot-dip galvanized steel sheet with excellent delayed fracture resistance and method for manufacturing the same
JP5352793B2
High-strength hot-dip galvanized steel sheet with excellent mechanical cutting properties, high-strength alloyed hot-dip galvanized steel sheet, and methods for manufacturing the same.
JP5354135B2
Cold-rolled steel sheet and manufacturing method for same
WO2013125400A1
High-strength cold-rolled thin steel sheet and method for producing high-strength cold-rolled thin steel sheet
WO2018088421A1
Cited By
Steel sheet and manufacturing method therefor