Method for producing molten iron
By controlling the slag ratio and carbon content in the submerged arc furnace method for producing hot metal, the energy efficiency of the process is improved, enabling the efficient use of low-grade iron ore and reducing costs.
Patent Information
- Application Number
- PCT/JP2024/007240
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-02-28
- Publication Date
- 2024-10-03
AI Technical Summary
The direct reduction method for producing hot metal using submerged arc furnaces faces challenges in achieving high energy efficiency, particularly when processing low-grade iron ore, as existing methods do not effectively manage the slag ratio and energy consumption, leading to increased costs and inefficiencies.
The method involves melting reduced iron in a submerged arc furnace while maintaining a specific slag ratio (S/P) between 0.15 to 2.0, adjusting the basicity of the molten slag (CaO/SiO2) to 1.0 to 1.3, and adding carbon to achieve a C content of 2 to 5% in the hot metal, optimizing the energy efficiency by controlling the slag ratio and carbon content.
This approach significantly reduces power consumption and enhances power efficiency, allowing for the effective use of low-grade iron ore and improving the overall energy efficiency of the hot metal production process.
Smart Images

Figure JP2024007240_03102024_PF_FP_ABST
Abstract
Description
Molten iron manufacturing method
[0001] The present invention relates to a method for producing molten iron by melting an iron source material containing reduced iron in a submerged arc furnace. 3 In this specification, the term "x to y" representing a numerical range means x or more and y or less, including the boundary value. Furthermore, "t-p" is a unit representing the mass of molten iron.
[0002] In recent years, CO 2 In the steel industry, CO emissions are also being reduced. 2 As an alternative to the blast furnace process, which has a high carbon dioxide emissions, the direct reduction (DR) process for producing pig iron has been attracting attention. In the DR process, for example, iron-containing agglomerates are reduced in a shaft furnace to produce direct reduced iron (DRI). This reduced iron or iron source material, such as iron scrap, is charged into an electric arc furnace (EAF) or submerged arc furnace (SAF) and heated and melted, and the pig slag is separated to produce pig iron.
[0003] Pellets and lump ore are used as agglomerates for direct reduction. Pellets are made by mixing and granulating fine ore or dust with auxiliary materials and a binder, and then firing the mixture. Bentonite is often used as the binder.
[0004] Patent Document 1 proposes a raw material for reduction that suppresses hydrogen-based reduction of iron oxide in the temperature range of 550 to 600°C and promotes reduction of iron oxide at 700°C or higher, thereby suppressing reduction disintegration and ensuring the strength of the raw material for reduction. This raw material for reduction is a pellet with a two-layer structure having a porous body and a coating layer. The porous body portion is the Fe 2 O 3 The coating layer contains 0.1 parts by mass or more and 10.0 parts by mass or less of bentonite relative to the total content of the Ca compound and the Fe compound contained therein.
[0005] Patent Document 2 proposes the use of smectite clay pretreated with a dispersant to improve pellet strength. The smectite clay contains bentonite, and the amount of smectite clay blended is, for example, about 0.2 to about 1.0 kg, about 0.4 to about 0.8 kg, or about 0.4 to about 0.7 kg per 1 MT (megaton) of pellet-forming particles.
[0006] Japanese Patent Application Laid-Open No. 2017-119910 Special Publication No. 2021-507116
[0007] Conventionally, electric arc furnaces (EAFs) have been used primarily as equipment for melting reduced iron in the DR process. Due to equipment limitations, EAFs require the use of high-quality reduced iron with a low slag ratio (high Fe content). Consequently, high-grade iron ore has inevitably been used as the raw material for the reduced iron, i.e., the raw ore for iron ore pellets. Examples of high-grade iron ore include South American ore, concentrate ore whose grade has been improved by prior ore dressing treatment, and pellet feed ore.
[0008] However, there are challenges in utilizing South American ore, concentrate ore, and pellet feed ore in Japan. Due to Japan's geographical conditions, South American ore inevitably increases freight rates. Concentrate ore and pellet feed ore are also derived from high-grade iron ore, as beneficiation of high-grade iron ore is more efficient than beneficiation of low-grade iron ore, and for the same reason, freight rates increase. Therefore, the direct reduction process using high-grade iron ore poses a cost challenge.
[0009] Therefore, in Japan, studies are underway to apply the DR process to low-grade iron ore produced in Australia, India, etc. However, it is difficult to melt reduced iron produced from low-grade iron ore using the current EAF, so the use of a submerged arc furnace (SAF) is being considered.
[0010] Here, since the melting process using the SAF requires a very large amount of energy (electricity), it is desirable to improve energy efficiency even as much as possible. However, until now, no appropriate operational guidelines have been provided for achieving high energy efficiency in the series of molten iron production processes, which involve producing iron ore pellets from low-grade iron ore as a raw material, reducing the iron in a solid reduction furnace to produce reduced iron, and melting the reduced iron in an SAF furnace.
[0011] In Patent Document 1, iron ore pellets after sintering are prone to pulverization in a solid reduction furnace, and the object is to suppress this reduction pulverization and ensure the strength of the sintered pellets. Patent Document 2 also aims to improve the strength of the pellets. Both of these methods only consider the properties of the pellets, and do not consider the realization of high energy efficiency in the series of molten iron production processes described above.
[0012] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing molten pig iron that can achieve high energy efficiency in the melting step when producing molten pig iron by melting reduced iron in a submerged arc furnace.
[0013] As a result of intensive research to solve the above-mentioned problems, the inventors have found that the energy efficiency of the melting process can be improved by keeping the ratio of the amount of slag accumulated in a submerged arc furnace to the amount of molten pig iron within a predetermined range. That is, the method for producing molten pig iron according to the present invention, which advantageously solves the above-mentioned problems, comprises melting an iron source material containing reduced iron in a submerged arc furnace to obtain molten pig iron, and adjusting the basicity (CaO / SiO 2 and adding a carbonaceous material to adjust the C content of the molten pig iron, and the operation is carried out so that the slag ratio S / P represented by the following formula (1) falls within the range of 0.15 to 2.0 t / t-p, wherein the basicity (CaO / SiO 2 ) is the SiO of CaO 2 S / P={S (DRI) +S(SCR) +S (FLUX)} / {P (DRI) +P (SCR)} (1) where S (DRI) : amount of slag derived from reduced iron in the submerged arc furnace (t), S (SCR) : Amount of slag derived from iron source materials other than reduced iron in the submerged arc furnace (t), S (FLUX) : Amount of slag derived from added slag formers and added carbonaceous materials in the submerged arc furnace (t), P (DRI) : amount of molten iron derived from reduced iron in the submerged arc furnace (t), P (SCR) : Amount (t) of molten iron derived from iron source materials other than reduced iron in a submerged arc furnace
[0014] The method for producing molten pig iron according to the present invention further comprises: (a) a step of preparing raw materials for direct reduction, which further comprises an optional step of preparing iron ore pellets produced from low-grade iron ore having a total Fe content of 63% by mass or less; and a step of producing reduced iron from the raw materials for direct reduction; (b) the raw materials for direct reduction used in the step of producing reduced iron include lump ore; (c) intentionally setting one or more factors selected from the timing and amount of addition of the reduced iron, iron source raw materials other than the reduced iron, and additive slag formers, and the timing and amount of discharge of the molten pig iron and slag from a submerged arc furnace, so that the slag ratio S / P is in the range of 0.15 to 2.0; (d) operating the furnace so that the slag ratio S / P is in the range of 0.25 to 0.9; (e) adjusting the basicity (CaO / SiO 2 (f) adding the carbon material so that the C content in the molten iron is in the range of 2 to 5 mass %, etc., can be more preferable solutions.
[0015] According to the method for producing molten pig iron of the present invention, high energy efficiency can be achieved when iron source materials containing reduced iron are melted in a submerged arc furnace to produce molten pig iron.
[0016] 1 is a schematic diagram illustrating a method for producing molten pig iron according to an embodiment of the present invention; 2 is a graph showing the relationship between the slag ratio S / P in a submerged arc furnace and the power consumption rate; 3 is a graph showing the relationship between the slag ratio S / P in a submerged arc furnace and the power efficiency;
[0017] The following is a detailed description of embodiments of the present invention. The following embodiments are intended to exemplify equipment and methods for embodying the technical concept of the present invention, and are not intended to limit the configuration to those described below. In other words, the technical concept of the present invention can be modified in various ways within the technical scope defined in the claims.
[0018] 1 is a schematic diagram illustrating the configuration of a submerged arc furnace suitable for use in a method for producing molten pig iron according to one embodiment of the present invention. The submerged arc furnace 1 holds molten pig iron P and molten slag S within a furnace wall 2. In the submerged arc furnace 1, electrodes 3 are inserted into the molten slag S, and an arc is generated between the multiple electrodes 3 or between the electrodes 3 and the molten pig iron P, heating and melting the raw materials by resistance heating.
[0019] In this embodiment, iron source material 4 containing reduced iron is charged into a submerged arc furnace. At the same time, the basicity (CaO / SiO 2 The basicity of the molten slag (CaO / SiO 2 ) is the SiO of CaO in the molten slag 2 This refers to the mass fraction of
[0020] The ratio of the mass of slag S to the unit mass of molten iron P is defined as the slag ratio S / P (t / t-p), which is expressed by the following formula (1): S / P={S (DRI) +S (SCR) +S (FLUX)} / {P (DRI) +P (SCR)} (1) where S (DRI) : amount of slag derived from reduced iron in the submerged arc furnace (t), S (SCR): Amount of slag derived from iron source materials other than reduced iron in the submerged arc furnace (t), S (FLUX) : Amount of slag derived from added slag formers and added carbonaceous materials in the submerged arc furnace (t), P (DRI) : amount of molten iron derived from reduced iron in the submerged arc furnace (t), P (SCR) : Amount (t) of molten iron derived from iron source materials other than reduced iron in a submerged arc furnace
[0021] A slag ratio S / P in the range of 0.15 to 2.0 t / t-p can reduce the power consumption rate and improve power efficiency. Here, the power consumption rate refers to the power required to produce a unit mass of molten pig iron, and the power efficiency refers to the percentage ratio of the energy used to produce molten pig iron, i.e., melting and heating the iron source materials and slag, and reducing iron oxide, to the input power. A slag ratio S / P in the range of 0.25 to 0.9 t / t-p is preferred. If the slag ratio S / P is below the lower limit, the slag thickness is too thin, causing the heat from the arc to dissipate outside the furnace by radiation, increasing the power consumption rate and reducing power efficiency. If the slag ratio S / P exceeds the upper limit, power is consumed for the sensible heat of heating the slag and the heat of melting, increasing the power consumption rate for molten pig iron production and reducing power efficiency. One of the objectives of the present invention is to increase the use of low-grade iron ore. Therefore, if only low-grade iron ore is used and the components are not diluted with concentrate ore or pellet feed ore, the slag ratio S / P may exceed 0.6 t / t-p.
[0022] In this embodiment, the iron source raw material to be melted in the submerged arc furnace includes reduced iron. The reduced iron may be produced in advance by a direct reduction method, or commercially available reduced iron may be purchased and used. Iron scrap or scale may also be used as the iron source raw material. The mass ratio of the reduced iron to the iron source raw material is preferably 50 to 100%.
[0023] The slag-forming material is limestone (CaCO 3 ), quicklime (CaO), and SiO 2 The source is silica (SiO 2 It is preferable to add the basicity (CaO / SiO 2It is preferable that the basicity of the molten slag is in the range of 1.0 to 1.3. If the basicity of the molten slag is in this range, it is suitable for reuse as a roadbed material such as cement.
[0024] Coke or coal can be used as the carbonaceous material. In addition to charging in lumps, powdered material can also be sprayed by gas transportation. The ash content of the carbonaceous material other than carbon is added to the molten slag S. (FLUX) The C content in the molten pig iron P is preferably adjusted to the range of 2 to 5 mass %. If it is in this range, it is suitable for use as pig iron as it is or as a raw material for steelmaking in the next process.
[0025] (Step of Preparing Raw Materials for Direct Reduction) In this embodiment, it is preferable to have a step of preparing raw materials for direct reduction, which includes an optional step of preparing iron ore pellets produced from low-grade iron ore having a total Fe content (hereinafter referred to as T.Fe) of 63% by mass or less. The raw materials for iron ore pellets generally consist of iron ore, a binder, and auxiliary materials. In this embodiment, low-grade iron ore refers to iron ore having a T.Fe content of 63% by mass or less. It is also preferable that the low-grade iron ore has a crystal water content of 4% by mass or more.
[0026] Bentonite is preferred as a binder for iron ore pellets. Any known or arbitrary binder, such as an organic or inorganic binder, that provides a similar effect may also be used. Quicklime, limestone, dolomite, or the like may also be mixed as an auxiliary material for the iron ore pellets. Furthermore, lump ore may also be prepared as a raw material for direct reduction in addition to the iron ore pellets. Lump ore is generally iron ore with a size of approximately 10 to 35 mm, and is used in the reduced iron production process without being crushed.
[0027] Iron ore pellets may be prepared by being manufactured through a general crushing, mixing, granulation, and firing process, or pre-manufactured iron ore pellets may be prepared. When manufacturing iron ore pellets, each process can be carried out using conventionally known equipment and conditions as described below. The crushing process can be carried out using a crusher such as a general ball mill. The mixing process can be carried out using a general high-speed stirring mixer or concrete mixer. The granulation process can be carried out using a general pelletizer or drum mixer. The firing process can be carried out using a general rotary kiln or electric furnace.
[0028] (Reduced iron production process) In this embodiment, it is preferable to have a reduced iron production process consisting of any process of producing the reduced iron from raw materials for direct reduction. In the reduced iron production process, reduced iron is produced from iron ore pellets or lump ore as essential raw materials. A solid reduction furnace such as a general shaft furnace may be used to produce reduced iron. There are no particular restrictions on the reducing gas, but it is preferable to use, for example, hydrogen gas produced using renewable energy. For example, H 2 O 3 (vol %) may be used depending on the production method to be used. 2 : 55%, CO: 35%, balance CO 2 , CH 4 a mixed gas consisting of H 2 : 75%, CO: 20%, balance CO 2 , N 2 A mixed gas consisting of the following can be suitably used.
[0029] The power consumption rate and power efficiency per unit mass of molten iron were investigated using a 4- to 6-ton batch-type submerged arc furnace 1 as shown in Figure 1. Table 1 shows the composition of the reduced iron used in the investigation and the composition of blast furnace slag as an example.
[0030]
[0031] Reduced iron equivalent to 500 kg of molten pig iron and a predetermined amount of blast furnace slag were charged into the submerged arc furnace 1, and heating was initiated by applying current to the electrodes 3. After the start of current application, eight additional charges of 400 kg of reduced iron were added at 350 kWh power consumption each. The power consumption per unit mass of molten pig iron (kWh / t-p) was calculated from the power consumption when the molten pig iron temperature reached approximately 1600°C after all the charged reduced iron was melted. The power efficiency was calculated by dividing the theoretical sum of the heating energy of the molten pig iron, the heating energy of the slag, and the reduction energy of iron oxide by the power consumption. Table 2 shows the conditions and results for the additional charge. The slag basicity was 1.26, and the carbon content of the molten pig iron was adjusted to 2.5 to 4.5 mass%. The input power was constant at 2.7 MW.
[0032]
[0033] Figure 2 shows the relationship between the slag ratio S / P and the power consumption rate. Figure 3 shows the relationship between the slag ratio S / P and the power efficiency. These results show that the power consumption rate can be kept low and the power efficiency can be maintained at a high level when the slag ratio S / P is in the range of 0.15 to 2.0 t / t-p. Furthermore, when the slag ratio is in the range of 0.25 to 0.9 t / t-p, the power consumption rate can be further reduced and the power efficiency can be further increased.
[0034] 1 Submerged arc furnace (SAF) 2 Furnace wall 3 Electrode 4 (Charged) raw materials P Molten iron S Molten slag
Claims
1. An iron source material containing reduced iron is melted in a submerged arc furnace to obtain molten iron, and the basicity (CaO / SiO 2 and adding a carbonaceous material to adjust the C content of the molten pig iron, and the operation is carried out so that the slag ratio S / P represented by the following formula (1) falls within the range of 0.15 to 2.0 t / t-p. 2 ) is SiO of CaO 2 The mass fraction of molten iron is expressed as S / P={S (DRI) +S (SCR) +S (FLUX) } / {P (DRI) +P (SCR) } (1) where S (DRI) :Amount of slag derived from reduced iron in the submerged arc furnace (t), S (SCR) : Amount of slag derived from iron source materials other than reduced iron in the submerged arc furnace (t), S (FLUX) :Amount of slag derived from added slag former and added carbonaceous material in the submerged arc furnace (t), P (DRI) :Amount of molten iron derived from reduced iron in the submerged arc furnace (t), P (SCR) : Amount of molten iron (t) derived from iron source materials other than reduced iron in the submerged arc furnace 2. The method for producing molten iron according to claim 1, further comprising: a process for preparing raw materials for direct reduction, the process including an optional process for preparing iron ore pellets produced from low-grade iron ore having a total Fe content of 63 mass% or less; and a process for producing reduced iron, the process including an optional process for producing the reduced iron from the raw materials for direct reduction.
3. The method for producing molten iron according to claim 2, wherein the raw material for direct reduction used in the reduced iron production process includes lump ore.
4. A method for producing molten iron as claimed in any one of claims 1 to 3, wherein one or more of the timing and amounts of addition of the reduced iron, the iron source raw materials other than the reduced iron, and the additive slag former, and the timing and amounts of discharge of the molten iron and slag from a submerged arc furnace are intentionally set so that the slag ratio S / P is in the range of 0.15 to 2.
0.
5. A method for producing molten iron as claimed in claim 4, wherein the slag ratio S / P is in the range of 0.25 to 0.
9.
6. Basicity of the molten slag (CaO / SiO 2 6. The method for producing molten iron according to claim 1, wherein the slag former is added so that the ratio of slag yield to slag yield is in the range of 1.0 to 1.
3.
7. A method for producing molten iron according to any one of claims 1 to 6, wherein the carbon material is added so that the C content in the molten iron is in the range of 2 to 5 mass %.
Citation Information
Patent Citations
Reduction raw material, and method for producing reduction raw material
JP2017119910A
Mineral Processing
JP2021507116A
Method for producing molten iron
JP2004183070A
Method for producing molten iron
JP2017057431A
Integration of dr plant and electric DRI melting furnace for producing high performance iron
US20210301359A1