Polyester film

A polyester film with a furandicarboxylic acid and ethylene glycol composition, optimized for low cyclic dimer content and haze, addresses the issue of whitening during heat treatment, ensuring transparency and mechanical strength for industrial and packaging uses.

WO2024202870A1PCT designated stage expired Publication Date: 2024-10-03TOYOBO CO LTD

Patent Information

Application Number
PCT/JP2024/007310
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-02-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Polyester films containing furandicarboxylic acid units from biomass face challenges with high cyclic dimer content, leading to whitening and reduced transparency when heat-treated, making them unsuitable for applications requiring high transparency such as food packaging and optical uses.

Method used

A polyester film with a dicarboxylic acid component mainly composed of furandicarboxylic acid and a glycol component mainly composed of ethylene glycol, with a planar orientation coefficient within a specific range, low haze, and cyclic dimer content of 1.0% by mass or less, and a laminated structure to maintain transparency even after heating.

Benefits of technology

The film maintains excellent transparency and mechanical properties, suitable for industrial and packaging applications, with a cyclic dimer content reduced to prevent whitening during heat treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is a polyester film in which a furan dicarboxylic acid derived from biomass is used and the contained amount of cyclic dimers is less, and in which the transparency hardly decreases even when being heated. This polyester film comprises dicarboxylic acid components in which a furan dicarboxylic acid is the main component, and glycol components in which ethylene glycol is the main component, and satisfies the following requirements (1)-(3). (1) The plane orientation coefficient ΔP is 0.100-0.170. (2) The haze of the polyester film is 15% or less. (3) When Hz0 (%) represents the haze of the polyester film and Hz30(%) represents the haze of the polyester film after being heated for 30 minutes at 150°C, Hz30-Hz0≤15 is satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

Polyester film

[0001] The present invention relates to a polyester film having furandicarboxylic acid units.

[0002] Polyester resins such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), which are thermoplastic resins with excellent heat resistance and mechanical properties, are used in a wide variety of fields, including plastic films, electronics, energy, packaging materials, automobiles, etc. Among plastic films, biaxially oriented PET film is widely used in industrial and packaging fields because it offers an excellent balance between mechanical properties, heat resistance, dimensional stability, chemical resistance, optical properties, and cost.

[0003] In recent years, environmentally sustainable resins made from biomass-derived raw materials have been attracting attention as a means of moving away from petroleum. Polyethylene furanoate (PEF) contains biomass-derived furandicarboxylic acid (FDCA) and has a planar structure, making it a renewable resin that is expected to have heat resistance equivalent to or even superior to conventional petroleum-derived resins, such as polyethylene terephthalate (PET). Furthermore, both the carboxylic acid component and the diol component of PEF can easily be derived from biomass-derived raw materials.

[0004] Patent Document 1 proposes a polyester film having a specific range of planar orientation coefficient and dimensional stability suitable for industrial and packaging applications, which is produced by biaxially stretching a resin composed of a dicarboxylic acid component primarily composed of furandicarboxylic acid and a glycol component primarily composed of ethylene glycol (Patent Document 1).

[0005] Japanese Patent No. 6440336 Japanese Patent Application Laid-Open No. 2022-155579

[0006] Although Patent Document 1 discloses a polyester film having excellent mechanical strength, it has been found that the polyester film has a problem of whitening when heated, making it difficult to use in applications requiring high transparency, such as food packaging films and optical applications.

[0007] The present inventors speculate that low-molecular-weight components contained in the polyester film lead to the whitening of the film. For example, Patent Document 2 discloses a polyester resin having a 2,5-furandicarboxylic acid unit and an ethylene glycol unit as a polyester resin with reduced cyclic dimers, which are low-molecular-weight components. It is conceivable to produce a polyester film using the polyester resin disclosed in Patent Document 2.

[0008] However, the polyester resin described in Patent Document 2 did not have a sufficient reduction in cyclic dimers. Furthermore, when producing a film, the polyester resin is remelted in a melt extrusion process, but there was a problem in that a large amount of cyclic dimers was produced during the remelting. Films produced from the polyester resin described in Patent Document 2 exhibited severe whitening due to the precipitation of the cyclic dimers contained in the polyester resin on the film surface upon heating, making them difficult to use as industrial or packaging films.

[0009] The present invention aims to provide a polyester film using biomass-derived furandicarboxylic acid, which has a low content of cyclic dimers and is resistant to deterioration in transparency even when heated.

[0010] That is, the present invention includes the following inventions: [1] A polyester film comprising a dicarboxylic acid component mainly composed of furandicarboxylic acid and a glycol component mainly composed of ethylene glycol, which satisfies the following requirements (1) to (3): (1) a planar orientation coefficient ΔP of 0.100 or more and 0.170 or less, (2) a haze of the polyester film of 15% or less, and (3) a haze of the polyester film of 15% or less in Hz. 0 (%), and the haze after heating the polyester film at 150°C for 30 minutes was measured in Hz. 30 (%), Hz 30 -Hz 0[2] The polyester film according to the above item [1], further satisfying the following requirement (4): (4) The content of cyclic dimer is 1.0 mass% or less [3] The polyester film according to the above item [1], further satisfying the following requirements (5) and (6): (5) The polyester film has a laminate structure of three or more layers; and (6) The content of cyclic dimer is 1.0 mass% or less on at least one surface.

[0011] The polyester film of the present invention is a polyester film having a furandicarboxylic acid unit derived from biomass, but has a low content of cyclic dimers and is a polyester film that is resistant to loss of transparency even when heated, making it suitable for use as an industrial or packaging film.

[0012] The polyester film of the present invention comprises a dicarboxylic acid component primarily composed of furandicarboxylic acid and a glycol component primarily composed of ethylene glycol. That is, the polyester film of the present invention is produced using a polyethylene furandicarboxylate resin containing furandicarboxylic acid as the dicarboxylic acid component and ethylene glycol as the glycol component. Here, "primarily" and "mainly" mean that furandicarboxylic acid accounts for 80 mol% or more of 100 mol% of all dicarboxylic acid components, and ethylene glycol accounts for 80 mol% or more of 100 mol% of all glycol components. Of the 100 mol% of all dicarboxylic acid components, furandicarboxylic acid accounts for preferably 90 mol% or more, more preferably 95 mol% or more. Of the 100 mol% of all glycol components, ethylene glycol accounts for preferably 90 mol% or more, more preferably 95 mol% or more.

[0013] Dicarboxylic acid components other than furandicarboxylic acid and glycol components other than ethylene glycol may be copolymerized within a range that does not impair the object of the present invention. The copolymerization amount of dicarboxylic acid components other than furandicarboxylic acid is less than 20 mol%, preferably less than 10 mol%, and particularly preferably less than 5 mol%, based on the total dicarboxylic acid components. The copolymerization amount of glycol components other than ethylene glycol is less than 20 mol%, preferably less than 10 mol%, and particularly preferably less than 5 mol%, based on the total glycol components.

[0014] Examples of dicarboxylic acid components other than furandicarboxylic acid include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, 4,4'-dicarboxybiphenyl, and 5-sodium sulfoisophthalic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 2,5-norbornenedicarboxylic acid, and tetrahydrophthalic acid; and aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, adipic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, octadecanedioic acid, fumaric acid, maleic acid, itaconic acid, mesaconic acid, citraconic acid, and dimer acid.

[0015] Examples of glycol components other than ethylene glycol include aliphatic glycols such as 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2-methyl-1,3-propanediol, 2-amino-2-ethyl-1,3-propanediol, 2-amino-2-methyl-1,3-propanediol, 1,10-decanediol, dimethyloltricyclodecane, diethylene glycol, and triethylene glycol; ethylene oxide adducts or propylene oxide adducts of bisphenol A, bisphenol S, bisphenol C, bisphenol Z, bisphenol AP, and 4,4'-biphenol; and alicyclic glycols such as 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, and 1,4-cyclohexanedimethanol.

[0016] <Polyethylene furandicarboxylate Resin> As a polymerization method for the polyethylene furandicarboxylate resin, any production method can be used, such as a direct polymerization method in which furandicarboxylic acid is directly reacted with ethylene glycol, and, as necessary, with other dicarboxylic acid components and glycol components, or a transesterification method in which a dimethyl ester of furandicarboxylic acid (containing, as necessary, a dimethyl ester of other dicarboxylic acid) is subjected to a transesterification reaction with ethylene glycol (containing, as necessary, another glycol component).

[0017] The intrinsic viscosity of the polyethylene furan dicarboxylate resin is preferably 0.30 dL / g or more and 1.20 dL / g or less, more preferably 0.55 dL / g or more and 1.00 dL / g or less, and even more preferably 0.70 dL / g or more and 0.95 dL / g or less. If the intrinsic viscosity is lower than 0.30 dL / g, the polyester film may tear. On the other hand, if the intrinsic viscosity is higher than 1.20 dL / g, the increase in filtration pressure becomes too large, making high-precision filtration difficult, making it difficult to extrude the resin through the filter, or the effect of improving mechanical properties may become saturated.

[0018] The content of cyclic dimers contained in the polyethylene furan dicarboxylate resin is preferably 1.0% by mass or less, more preferably 0.7% by mass or less, and even more preferably 0.5% by mass or less. During the extrusion process in film production, the polyethylene furan dicarboxylate resin is melted, and since the cyclic dimers are regenerated during melting, the content of cyclic dimers contained in the polyethylene furan dicarboxylate resin is preferably 1.0% by mass or less. The lower the content of cyclic dimers contained in the polyethylene furan dicarboxylate resin, the better, but due to technical difficulties, the practical lower limit is 0.1% by mass.

[0019] <Additives> The polyester film of the present invention may contain additives to the extent that the purpose of the present invention is not impaired. The additives used in the present invention include inert particles such as inorganic particles, organic particles, heat-resistant polymer particles, and crosslinked polymer particles, fluorescent brighteners, ultraviolet inhibitors, infrared absorbing dyes, surfactants, antioxidants, and heat stabilizers, selected according to the purpose of use. Only one type of additive may be contained, or two or more types may be contained. Furthermore, the timing of adding the additives is not particularly limited as long as the additives do not impair the physical properties of the resulting polyester film.

[0020] The inert particles are preferably at least one selected from the group consisting of inorganic particles and organic particles. Any inorganic particles can be selected, including, for example, silica, calcium carbonate, barium sulfate, calcium sulfate, alumina, kaolinite, and talc. From the viewpoint of transparency, silica particles, especially amorphous silica particles, are preferred, as their refractive index is relatively close to that of the resin component.

[0021] The inorganic particles preferably have an average particle size of 1 to 10 μm, more preferably 1.5 to 7 μm, and even more preferably 2 to 5 μm. When the inorganic particles have an average particle size of 1 μm or more, a roughened structure suitable for imparting lubricity to the surface can be imparted. On the other hand, when the inorganic particles have an average particle size of 10 μm or less, high transparency can be maintained. Furthermore, the content of inactive particles in the polyester is preferably 0.005 to 1.0 mass%, more preferably 0.008 to 0.5 mass%. When the content of fine particles is 0.005 mass% or more, a roughened structure suitable for imparting lubricity to the surface of the surface layer can be imparted. On the other hand, when the content of fine particles is 1.0 mass% or less, high transparency can be maintained.

[0022] Any ultraviolet absorber can be selected as the ultraviolet absorber, and can be selected from known ones depending on the purpose of use. Examples of the ultraviolet absorber include organic ultraviolet absorbers such as benzotriazole compounds and benzophenone compounds, and inorganic ultraviolet absorbers such as zinc oxide, titanium oxide, and cerium oxide in the form of fine particles with a particle size of 0.2 μm or less. Any antioxidant can be selected, and examples include aromatic amines and phenols. Examples of the heat stabilizer include phosphorus-based ones such as phosphoric acid and phosphate esters, sulfur-based ones, and amine-based ones.

[0023] <Physical Properties of Polyester Film> The intrinsic viscosity of the polyester film of the present invention is preferably 0.30 dl / g or more and 1.20 dl / g or less, more preferably 0.40 dl / g or more and 1.00 dl / g or less, and even more preferably 0.50 dl / g or more and 0.80 dl / g or less. If the intrinsic viscosity is lower than 0.30 dl / g, the polyester film may tear. On the other hand, if the intrinsic viscosity is higher than 1.20 dl / g, the effect of improving the mechanical properties may become saturated.

[0024] The planar orientation coefficient ΔP of the polyester film of the present invention is 0.100 or more and 0.170 or less, preferably 0.110 or more and 0.160 or less, and more preferably 0.120 or more and 0.160 or less. The planar orientation coefficient can be calculated according to JIS K 7142-1996 5.1 (Method A) by measuring the refractive index nx in the machine direction (MD) of the film, the refractive index ny in the perpendicular direction (TD) thereto, and the refractive index nz in the thickness direction using an Abbe refractometer with sodium D line as a light source, and then calculating the planar orientation coefficient ΔP according to the following formula: ΔP={(nx+ny)-2nz} / 2

[0025] Both nx and ny are preferably 1.570 or more, more preferably 1.580 or more, even more preferably 1.590 or more, even more preferably 1.600 or more, particularly preferably 1.610 or more, and most preferably 1.620 or more. By setting nx and ny to 1.570 or more, sufficient film breaking strength and breaking elongation can be obtained, resulting in sufficient mechanical properties of the film, facilitating post-processing such as printing and bag making on the film, and preventing the film from breaking on a printer or coater during subsequent printing or coating, which is preferable. From the standpoint of production and thermal shrinkage, nx and ny are preferably less than 1.700.

[0026] The polyester film of the present invention has a haze of 15% or less. When the haze is 15% or less, the film is less cloudy, making it easier to inspect the contents for defects in food packaging applications. The haze is preferably 10% or less, more preferably 8% or less, even more preferably 5% or less, and particularly preferably 3% or less. A lower haze is preferable, but the lower limit is, for example, 0.1% due to the inherent refractive index of the polyester film.

[0027] The haze of the polyester film of the present invention is expressed as Hz 0 (%), and the haze after heating the polyester film at 150°C for 30 minutes was measured in Hz. 30 (%), HZ 30 From HZ 0The value ΔHz obtained by subtracting the value ΔHz from the haze is 15% or less, preferably 13% or less, and more preferably 10% or less. The polyester film of the present invention has a haze of 15% or less and a ΔHz of 15% or less, and therefore has excellent transparency and suppresses whitening of the film when heated. If the ΔHz exceeds 15%, when the film is subjected to heat treatment in post-processing, cyclic dimers precipitate and contaminate the process, making it difficult to use as a packaging or industrial film. Conversely, if the ΔHz is 15% or less, the film is less likely to contaminate the process even when subjected to heat treatment in post-processing, and whitening of the film is suppressed, making it usable as a packaging or industrial film. The lower limit of ΔHz is not particularly limited, but due to technical difficulties, it is, for example, 0% or more, preferably 2% or more.

[0028] HZ 30 The haze value (haze after heating the polyester film at 150°C for 30 minutes) is preferably 18% or less, more preferably 15% or less, and even more preferably 12% or less. 30 When the HZ is 18% or less, the film is less likely to contaminate the process even when heat treatment is performed in post-processing, and whitening of the film is suppressed, making it easy to use as a packaging or industrial film. 30 The lower limit of is not particularly limited, but is, for example, 1% or more due to technical difficulties.

[0029] The polyester film of the present invention preferably has a heat shrinkage rate (hereinafter simply referred to as heat shrinkage rate) of 10% or less in both the MD and TD directions when heated at 150°C for 30 minutes, more preferably 8% or less, and even more preferably 5% or less. A high heat shrinkage rate can cause the film to shrink on a printer or coater, making printing or coating difficult, or can cause poor appearance due to film deformation during high-temperature processing. In particular, during processing using a printer or coater, the film is prone to shrinkage in the width direction (TD) and poor appearance due to the lack of constraint between the rolls transporting the film. A low heat shrinkage rate is preferred, but due to technical difficulties, the lower limit is, for example, 0.01%.

[0030] In the present invention, the oxygen permeability of the polyester film at a temperature of 23° C. and a humidity of 65% is not particularly limited, but is preferably 0.1 mL / m 2 / day / MPa or more, 1000mL / m 2 / day / MPa or less, more preferably 0.1 mL / m 2 / day / MPa or more, 200mL / m 2 / day / MPa or less, and more preferably 0.1 mL / m 2 / day / MPa or more, 120mL / m 2 / day / MPa or less, and even more preferably 0.1 mL / m 2 / day / MPa or more, 100mL / m 2 / day / MPa or less. 2 If the pressure exceeds 0.1 mL / m / day / MPa, when the film is used as a packaging film, the oxygen that permeates the film may deteriorate the substance or the shelf life of the food may be poor. 2 The lower limit is considered to be / day / MPa. It is possible to further improve the oxygen permeability by applying methods such as printing or coating to the film, or methods such as co-extrusion.

[0031] The polyester film of the present invention has high oxygen barrier properties (low oxygen permeability) due to the polyester having a furandicarboxylic acid unit itself, but the oxygen barrier properties can be further improved by forming the polyester film into one that satisfies the stretching process described below or by providing a thin film layer whose main component is an inorganic compound.

[0032] In the present invention, the water vapor permeability of the polyester film at a temperature of 37.8°C and a humidity of 90% is not particularly limited, but is preferably 0.1 g / m 2 / day or more, 40g / m 2 / day or less, more preferably 30 g / m 2 / day or less, and more preferably 20 g / m 2 / day or less. 2If the film thickness exceeds 0.1 g / m² / day, the substance may be deteriorated by the water vapor that has passed through the film, and the preservation quality of the food may be deteriorated. 2 The water vapor permeability can be further improved by applying methods such as printing and coating to the film, and methods such as co-extrusion.

[0033] The polyester film of the present invention has high water vapor barrier properties (low water vapor permeability) due to the polyester having a furandicarboxylic acid unit itself, but the water vapor barrier properties can be further improved by forming the polyester film into one that satisfies the stretching process described below or by providing the film with a thin film layer containing an inorganic compound as a main component.

[0034] The polyester film of the present invention preferably has a breaking strength of 75 MPa or more in both the MD and TD directions. The breaking strength is more preferably 100 MPa or more, even more preferably 150 MPa or more, particularly preferably 200 MPa or more, and most preferably 220 MPa or more in both the MD and TD directions. If the breaking strength is less than 75 MPa, the mechanical strength of the film will be insufficient, and problems such as elongation and slippage may occur during the film processing process. In consideration of manufacturing, the upper limit of the breaking strength is 1000 MPa or less.

[0035] The polyester film of the present invention preferably has a breaking elongation of 10 to 300% in both the MD and TD directions. If the breaking elongation is less than 10%, the mechanical elongation of the film will be insufficient, and problems such as cracking and tearing may occur during the film processing process. In addition, taking manufacturing into consideration, the upper limit of the breaking elongation is preferably 300% or less. The breaking elongation is more preferably 15 to 150%, even more preferably 20 to 100%, and particularly preferably 30 to 80%, in both the MD and TD directions.

[0036] The coefficient of friction of the polyester film of the present invention is not particularly limited, but it is preferable that the static friction coefficient (μs) is 1.0 or less and the dynamic friction coefficient (μd) is 1.0 or less. The static friction coefficient (μs) is more preferably 0.8 or less, and even more preferably 0.6 or less. The dynamic friction coefficient (μd) is more preferably 0.8 or less, and even more preferably 0.6 or less. If the static friction coefficient (μs) or the dynamic friction coefficient (μd) exceeds 1.0, the slipperiness will be poor, and scratches and wrinkles may occur due to rubbing during film running. The static friction coefficient (μs) is the static friction coefficient between one side and the other side of the laminated polyester film of the present invention, and the dynamic friction coefficient (μd) is the dynamic friction coefficient between one side and the other side of the polyester film of the present invention.

[0037] The polyester film of the present invention preferably has a total light transmittance of 75% or more. A total light transmittance of 75% or more can improve the accuracy of detecting internal foreign matter that could be a defect in the film. The total light transmittance is more preferably 80% or more, even more preferably 85% or more, particularly preferably 88% or more, and most preferably 88.5% or more. In order to improve the accuracy of detecting internal foreign matter that could be a defect in the film, the higher the total light transmittance, the better. However, it is technically difficult to achieve a total light transmittance of 100%, and the upper limit is, for example, 98%.

[0038] The lower limit of the impact strength of the polyester film of the present invention, calculated as 15 μm, is not particularly limited, but is preferably 0.4 J / 15 μm, more preferably 0.6 J / 15 μm, and even more preferably 0.8 J / 15 μm. If it is less than 0.4 J / 15 μm, the strength may be insufficient when used as a bag. The upper limit of the impact strength (impact resistance) is preferably 3.0 J / 15 μm, and if it exceeds 3.0 J / 15 μm, the improvement effect will saturate.

[0039] The thickness of the polyester film of the present invention is 1 to 300 μm, preferably 5 to 200 μm, more preferably 10 to 100 μm, and even more preferably 10 to 40 μm. A thickness of more than 300 μm is problematic in terms of cost and tends to reduce visibility when used as a packaging material. On the other hand, a thickness of less than 1 μm may reduce mechanical properties and may not function as a film.

[0040] The content of the cyclic dimer contained in the polyester film of the present invention (the content of the cyclic dimer relative to the total polyester film of the present invention) is preferably 1.05% by mass or less. It is more preferably 1.0% by mass or less, even more preferably 0.9% by mass or less, and particularly preferably 0.8% by mass or less. The inventors have found that the cyclic dimer precipitated on the film surface becomes a nucleus of foreign matter, causing whitening of the film. When the cyclic dimer content is 1.05% by mass or less, the cyclic dimer is less likely to precipitate during post-processing steps of the film and contaminate the process, making it less likely to cause defects, such as during printing or lamination. Furthermore, it has been found that the film is less likely to whiten because only a small amount of cyclic dimer precipitates on the film even when heated. Details of the method for measuring the cyclic dimer content are described below. Measurement was performed using HPLC analysis, but similar values ​​were obtained using NMR.

[0041] The polyester film of the present invention may have a single layer or a multi-layer laminate structure, but preferably has a laminate structure of three or more layers. For example, if the outermost layers are Layer B and Layer D, and the layers other than the outermost layer are Layer A and Layer C, the layer structure in the film thickness direction may be Layer B / Layer A / Layer B, Layer B / Layer A / Layer D, Layer B / Layer A / Layer C / Layer B, Layer B / Layer A / Layer C / Layer D, or Layer B / Layer A / Layer C / Layer A / Layer B. The resin compositions of the layers A to D may be the same or different, but it is preferable that the resin compositions of each layer be the same or that the layer be a Layer B / Layer A / Layer B structure (a two-type, three-layer structure). The method for producing a laminated polyester film is not particularly limited, but it can be produced, for example, by coextrusion.

[0042] While the polyester with reduced cyclic dimer content as described above can be used for each layer of the film, it is preferable to use a polyester with reduced cyclic dimer content on at least one surface, and more preferably on both surfaces. The cyclic dimer content on at least one surface (preferably both surfaces) is preferably 1.0% by mass or less, more preferably 0.9% by mass or less, and even more preferably 0.8% by mass or less. In another preferred embodiment, even if the cyclic dimer content throughout the film is greater than 0.9% by mass (preferably greater than 0.9% by mass and 1.5% by mass or less), precipitation of the cyclic dimer on the film surface can be suppressed by keeping the cyclic dimer content on the surface 0.9% by mass or less (preferably 0.8% by mass or less). While the lower the cyclic dimer content, the better due to technical difficulties. For example, the cyclic dimer content on at least one surface (preferably both surfaces) is 0.2% by mass or more. The "cyclic dimer content on the surface" refers to the cyclic dimer content within a thickness of 1 μm from the surface.

[0043] As described above, the polyester film of the present invention may contain additives, and when it has a multi-layer structure, a polyethylene furan dicarboxylate resin layer containing additives may be used only in the surface layer. Such a film may have, for example, a three-layer structure (b / a / b) in which a central layer (a) and a surface layer (b layer) containing additives are laminated on both sides of the central layer (a layer) by a coextrusion method, or a three-layer structure (b / c / b) in which both the central layer (c layer) and the surface layer contain additives and the additives in each layer have different concentrations.

[0044] <Method for Producing Polyester Resin> Hereinafter, a method for producing the polyester resin used in producing the polyester film of the present invention will be described, but the method is not limited to the following method.

[0045] The method for producing the polyester resin used in the present invention involves melt polymerization, followed by preliminary crystallization treatment, and then solid-phase polymerization, thereby reducing the amount of cyclic dimers in the polyester resin.

[0046] <Melt Polymerization of Polyester Resin> The conditions for the esterification reaction between a dicarboxylic acid and a diol and the transesterification reaction between a dicarboxylic acid ester and a diol, such as temperature, time, and pressure, can be within the range of conventional polyester production methods. The production method described in WO 2021 / 172215 is particularly preferred, but is not limited to the production method described therein. In WO 2021 / 172215, a starting mixture containing 2,5-furandicarboxylic acid or its diester and ethylene glycol is subjected to an esterification reaction to obtain a hydroxyethyl ester composition, and the hydroxyethyl ester composition is then subjected to a polycondensation reaction under reduced pressure in the presence of a polycondensation catalyst to obtain a polycondensate. The polycondensation catalyst contains an aluminum compound and a phosphorus compound, and the phosphorus compound contains one or more compounds selected from the group consisting of phosphoric acid compounds containing an aromatic group and phosphinic acid compounds containing an aromatic group.

[0047] <Pre-crystallization of polyester resin> If the temperature is rapidly raised to the reaction temperature for solid-phase polymerization after melt polymerization, the surface of the polyester resin will partially melt, causing the resin to adhere to itself and form clumps, which may make handling difficult and may hinder the progress of the solid-phase polymerization reaction. Therefore, it is preferable to pre-crystallize the surface of the polyester resin by starting heating from about 80 to 100°C and gradually increasing the temperature to about 150 to 180°C. However, pre-crystallization must be carried out in a short time because a long period of pre-crystallization will cause the resin to become discolored. In the explanation of pre-crystallization, "polyester resin" means the polyester resin immediately after melt polymerization.

[0048] Considering the influence on the subsequent solid-state polymerization process, the film-forming process, and the film quality, it is preferable to perform a heat treatment in the presence of a polyester resin and a supercritical inert gas as a pre-crystallization treatment, and then reduce the pressure from the pressure in the supercritical state to atmospheric pressure. In order to suppress the formation of cyclic dimers, it is particularly important to use a supercritical inert gas. In order to shorten the pre-crystallization time, known methods such as adding a crystal nucleating agent to the polyester resin or promoting crystallization using a solvent may be used as appropriate.

[0049] Because the inert gas dissolves in the polyester resin and plasticizes it, the crystallization behavior during treatment with the inert gas under high pressure differs from that under normal atmospheric pressure. Therefore, the heat treatment temperature is preferably from the crystallization temperature −70° C. to the crystallization temperature +10° C., more preferably from the crystallization temperature −60° C. to the crystallization temperature, even more preferably from the crystallization temperature −35° C. to the crystallization temperature −5° C., particularly preferably from the crystallization temperature −30° C. to the crystallization temperature −10° C., and most preferably from the crystallization temperature −25° C. to the crystallization temperature −15° C. The method for measuring the crystallization temperature will be described later.

[0050] The inert gas is not particularly limited as long as it does not activate the polyester resin, and examples thereof include oxygen, methane, propane, nitrogen dioxide, nitrogen, argon, helium, carbon dioxide, etc., and among these, it is preferable to use carbon dioxide. Note that carbon dioxide may react with some compounds and may not be usable as an inert gas, but in this specification, "inert gas" refers to a gas that does not activate the polyester resin.

[0051] If the pressure during heat treatment is high, the inert gas dissolves in the polyester resin and plasticizes it, resulting in crystallization in a short period of time. Therefore, the pressure during heat treatment is preferably 5 MPa or more, more preferably 8 MPa or more, even more preferably 10 MPa or more, particularly preferably 15 MPa or more, and most preferably 18 MPa or more. The upper limit of the pressure during heat treatment is not particularly limited, but is, for example, 50 MPa or less. A reaction vessel that can withstand pressures exceeding 50 MPa would need to be made of very thick metal, which is not practical.

[0052] To increase the pressure during heat treatment above atmospheric pressure, for example, a polyester resin is placed in a high-pressure reactor and connected to a gas cylinder, a pump, a pressure relief valve, a pressure gauge, a safety valve, etc. After the high-pressure reactor is heated to a predetermined temperature, an inert gas is pumped in through a pump and the pressure is adjusted to a predetermined level by the pressure relief valve.

[0053] The heat treatment time is preferably 10 minutes or more, more preferably 15 minutes or more, even more preferably 20 minutes or more, and particularly preferably 25 minutes or more. If the heat treatment time is 10 minutes or more, the inert gas can be sufficiently dissolved in the polyester resin. The upper limit of the heat treatment time is not particularly limited, but is, for example, 200 minutes or less, preferably 180 minutes or less, and more preferably 150 minutes or less. If it exceeds 200 minutes, the effect of increasing the crystallinity will saturate.

[0054] The time required to reduce the pressure from the pressure in the supercritical state to atmospheric pressure is preferably 0.5 to 20 minutes, more preferably 1.5 to 10 minutes, and even more preferably 3 to 5 minutes.

[0055] The pressure reduction rate from the pressure in the supercritical state to atmospheric pressure is preferably 1 to 30 MPa / min, more preferably 2 to 25 MPa / min, even more preferably 3 to 15 MPa / min, particularly preferably 4 to 10 MPa / min, and most preferably 5 to 7 MPa / min.

[0056] <Solid-state polymerization of polyester resin> The method of solid-state polymerization is not particularly limited, but examples include a method in which the polyester resin obtained in the above-mentioned polycondensation reaction step is heated under an inert gas atmosphere or under reduced pressure. As the inert gas, the gas used in the preliminary crystallization may be used appropriately, and it is preferable to use the same inert gas as in the preliminary crystallization. The solid-state polymerization may be carried out with the polyester resin pellets or powder left to stand or with stirring. When stirring, stirring may be carried out by installing a stirring blade in the reaction vessel or by moving the reaction vessel.

[0057] The reaction temperature of the solid-state polymerization is preferably high from the viewpoint of reducing the amount of cyclic dimer, and is preferably 180°C or higher, more preferably 190°C or higher. The upper limit of the reaction temperature is the melting point of the polyester resin. The reaction time of the solid-state polymerization is preferably 1 hour or longer, more preferably 3 hours or longer. On the other hand, since there is a risk of coloration, it is preferably 50 hours or shorter, more preferably 40 hours or shorter, and even more preferably 30 hours or shorter.

[0058] <Method for producing polyester film> The method for producing the polyester film of the present invention will be described. First, a polyester resin such as PEF pellets or PEF chips is dried or hot-air dried so that the moisture content is less than 200 ppm. Next, the raw materials are weighed, mixed, and fed to an extruder, where they are melt-extruded into a sheet. The molten sheet is then brought into close contact with a rotating metal roll (casting roll) using an electrostatic application method and cooled and solidified to obtain an unstretched film (unstretched sheet).

[0059] Furthermore, high-precision filtration can be performed to remove foreign matter contained in the molten resin at any location where the molten resin is maintained at a temperature between melting point +5°C and melting point +60°C. The filter material used for high-precision filtration of the molten resin is not particularly limited, but a filter material made of sintered stainless steel is suitable because it has excellent performance in removing aggregates and high-melting-point organic matter whose main components are Si, Ti, Sb, Ge, and Cu.

[0060] When a laminate structure of three or more layers is formed by coextrusion, the raw materials for each layer are extruded using two or more extruders, and the two layers are joined using a multilayer feed block (for example, a joining block having a rectangular joining portion), extruded into a sheet form through a slit die, and cooled and solidified on a casting roll to form an unstretched film. Alternatively, a multi-manifold die may be used instead of the multilayer feed block.

[0061] Even if the amount of cyclic dimer in a polyester resin is reduced by pre-crystallization and solid-state polymerization, the amount of cyclic dimer increases during the process of melting the polyester resin and melt-extruding it into a sheet. Therefore, it is also important to suppress the increase in the amount of cyclic dimer during the process of producing a film using the polyester resin. The meltline residence time is the time from when the resin contacts the screw of the extruder until the resin is melted and extruded into a sheet form from the die. By shortening the meltline residence time, thermal decomposition during melt extrusion can be suppressed, thereby suppressing the increase in cyclic dimer. The meltline residence time is preferably 10 minutes or less, more preferably 8 minutes or less, even more preferably 5 minutes or less, and particularly preferably 3 minutes or less. While the lower limit is not particularly limited, the resin must be melted and kneaded to a certain degree uniformly, so the practical lower limit is 1 minute or more.

[0062] The lower the resin temperature during retention in the melt line, the more effectively the regeneration of cyclic dimers during melt extrusion can be suppressed. The resin temperature is preferably the melting point of the polyester resin + 60°C or less, and more preferably the melting point + 55°C or less. Although there are no particular restrictions on the lower limit, since the resin must be melted, the substantial lower limit is the melting point + 5°C or more.

[0063] Next, the unstretched film obtained by the above method is biaxially stretched and then heat-treated. For example, when an unstretched film having a furandicarboxylic acid unit is biaxially stretched to produce a biaxially oriented polyester film, a sequential biaxial stretching method in which uniaxial stretching is performed in the MD or TD direction and then stretched in the orthogonal direction, a simultaneous biaxial stretching method in which stretching is performed simultaneously in the MD and TD directions, or a method using a linear motor as a driving method for simultaneous biaxial stretching can be employed. In the sequential biaxial stretching method, MD stretching can be achieved by stretching in the MD direction using a heated roll to create a speed difference. An infrared heater or the like can also be used for heating. Subsequent TD stretching can be achieved by introducing the MD-stretched sheet into a tenter, holding both ends with clips, and stretching in the TD direction while heating. The film after TD stretching is subsequently heat-treated in the tenter. Heat treatment can be performed while the sheet is stretched in the TD, or while the sheet is relaxed in the TD. After heat treatment, the film can be wound up on a winder after cutting off both ends.

[0064] (i) Control of the MD stretch ratio of the film To obtain the polyester film of the present invention, stretching in the MD direction is preferably performed at a ratio of 2.5 to 10.0. The MD stretch ratio is more preferably 3.5 or more, even more preferably 3.8 or more, particularly preferably 4.0 or more, and most preferably 4.5 or more. By setting the MD stretch ratio to 2.5 or more, it is possible to obtain a film with excellent mechanical properties, such as a ΔP of 0.100 or more, a film breaking strength of 100 MPa or more, and a film breaking elongation of 15% or more. A MD stretch ratio of 10.0 or less is preferable because it reduces the frequency of breakage. The higher the MD stretch ratio, the higher the temperature in the heat setting step can be, and the lower the heat shrinkage rate can be.

[0065] (ii) Control of MD stretching temperature of film In order to obtain the polyester film of the present invention, it is preferable to perform stretching in the MD direction at 90°C or higher and 150°C or lower. More preferably, it is 100°C or higher and 125°C or lower. A stretching temperature in the MD direction of 90°C or higher is preferred because it reduces the frequency of breakage. A temperature of 150°C or lower is preferred because it allows uniform stretching.

[0066] (iii) Control of the Stretching Ratio in the TD Direction of the Film To obtain the polyester film of the present invention, stretching in the TD direction is preferably performed at a ratio of 2.5 to 10.0. The stretching ratio in the TD direction is more preferably 3.0 or more, even more preferably 3.5 or more, particularly preferably 4.0 or more, and most preferably 4.5 or more. By setting the stretching ratio in the TD direction to 2.5 or more, a film with excellent mechanical properties, such as a ΔP of 0.100 or more, a film breaking strength of 100 MPa or more, and a film breaking elongation of 15% or more, can be obtained. A stretching ratio in the TD direction of 10.0 or less is preferred because it reduces the frequency of breakage.

[0067] (iv) Control of TD Stretching Temperature In order to obtain the polyester film of the present invention, it is preferable to perform stretching in the TD direction at 80°C or higher and 200°C or lower. More preferably, it is 95°C or higher and 135°C or lower. A TD stretching temperature of 80°C or higher is preferable because the frequency of breakage decreases. A TD stretching temperature of 200°C or lower is preferable because uniform stretching can be achieved.

[0068] (v) Control of film heat setting temperature In order to obtain the polyester film of the present invention, it is preferable to perform heat setting treatment at 110°C or higher and 220°C or lower. If the heat setting temperature is 220°C or lower, the film is less likely to become opaque and the frequency of melt breakage is reduced, which is preferable. Increasing the heat setting temperature is preferable because it reduces the heat shrinkage rate, and 120°C or higher is more preferable, 140°C or higher is even more preferable, 160°C or higher is even more preferable, 175°C or higher is particularly preferable, and 185°C or higher is most preferable. Heat setting treatment tends to increase the planar orientation coefficient ΔP. In addition, the heat setting temperature is more preferably 210°C or lower.

[0069] (vi) Control of Heat-Setting Time of Film To obtain the polyester film of the present invention, the heat-setting treatment is preferably carried out for 5 to 20 seconds, more preferably 7 to 15 seconds, and even more preferably 8 to 12 seconds. The length of the heat-setting time affects the planar orientation coefficient ΔP.

[0070] (vii) Control of Relaxation Temperature in TD Direction In order to obtain the polyester film of the present invention, it is preferable to perform relaxation treatment in the TD direction at 100° C. or higher and 200° C. or lower. The relaxation temperature in the TD direction is more preferably 165° C. or higher and 195° C. or lower, and even more preferably 175° C. or higher and 195° C. or lower. By relaxing at the above relaxation temperature, the thermal shrinkage rate can be reduced.

[0071] (viii) Control of Relaxation Rate in TD To obtain the polyester film of the present invention, the relaxation rate in TD is preferably 0.5% or more and 10.0% or less, more preferably 2% or more and 6% or less. By relaxing at the above relaxation temperature, the thermal shrinkage rate can be reduced.

[0072] The film can be subjected to corona treatment or plasma treatment during or after the stretching process. Furthermore, by coating the film with a solution or dispersion of a suitable mixture of resins, crosslinking agents, particles, etc., dissolved in a solvent, it is possible to impart properties such as slipperiness, antiblocking, antistatic properties, and easy adhesion.

[0073] Furthermore, the functionality of the film can be improved by surface treatment after stretching and heat treatment, such as printing or coating.

[0074] Furthermore, by laminating a film that has been stretched and heat-treated or a surface-treated film with paper, it can be used for packaging, labels, decorative sheets, etc.

[0075] This application claims the benefit of priority based on Japanese Patent Application No. 2023-048171, filed on March 24, 2023. The entire contents of the specification of Japanese Patent Application No. 2023-048171, filed on March 24, 2023, are incorporated herein by reference.

[0076] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. The evaluation methods used in each example and comparative example are as follows.

[0077] <Evaluation Method> (1) Intrinsic Viscosity (IV) A polyester resin or polyester film was pulverized and dried, and then dissolved in a mixed solvent of parachlorophenol / tetrachloroethane = 75 / 25 (mass ratio). Using an Ubbelohde viscometer, the flow time of a solution with a concentration of 0.4 g / dl at 30°C and the flow time of the solvent alone were measured, and the intrinsic viscosity of the polyester resin or polyester film was calculated from the ratio of these times using the Huggins equation and assuming that the Huggins constant was 0.38.

[0078] (2) Crystallization Temperature, Melting Point, and Glass Transition Temperature The crystallization temperature, melting point, and glass transition temperature of the polyester resin were measured using a differential scanning calorimeter (DSC214Polyma) manufactured by Netsch Japan.

[0079] (3) Film Thickness Using a Millitron, four 5 cm square samples were cut out from four arbitrary locations on the film to be measured, and measurements were taken at five locations on each sample (total of 20 locations), and the average value was taken as the film thickness.

[0080] (4) Breaking Strength and Breaking Elongation A sample was cut into a strip shape with a length of 140 mm and a width of 10 mm in the MD and TD directions of the film using a single-edged razor. The strip-shaped sample was then pulled using an Autograph AG-IS (manufactured by Shimadzu Corporation), and the breaking strength (MPa) and breaking elongation (%) in each direction were determined from the obtained load-strain curve. The measurements were performed in an atmosphere of 25°C, with a chuck distance of 40 mm, a crosshead speed of 100 mm / min, and a load cell of 1 kN. The breaking strength and breaking elongation were each measured five times, and the average values ​​were used as the breaking strength and breaking elongation of the film.

[0081] (5) Refractive index, plane orientation coefficient ΔP According to JIS K 7142-1996 5.1 (Method A), the refractive index nx in the MD direction in the film plane, the refractive index ny in the direction perpendicular to the MD direction, and the refractive index nz in the thickness direction were measured using an Abbe refractometer with sodium D line as a light source, and the plane orientation coefficient ΔP was calculated using the following formula. Three measurements were taken, and the average values ​​were used as the refractive index and plane orientation coefficient ΔP of the film. Methylene iodide was used as the mounting liquid. ΔP = {(nx + ny) - 2nz} / 2

[0082] (6) Total light transmittance and haze were measured in accordance with JIS K 7136. The measuring instrument used was a turbidity meter model NDH-5000 manufactured by Nippon Denshoku Industries Co., Ltd.

[0083] (7) Haze change ΔHz The film was cut into a 50 mm square, and the haze (Hz) before heating was measured in accordance with JIS K 7105 "Testing method for optical properties of plastics" haze (cloudiness). 0 The turbidity (%) was measured using a turbidimeter model NDH-300A manufactured by Nippon Denshoku Industries Co., Ltd. After the measurement, the film was placed in an oven heated to 150°C, and after 30 minutes, the film was taken out and the turbidity (%) was measured. 0 The haze was measured in the same manner as in Example 1, and the haze (Hz) after heating was 30 (%). Hz 30 from Hz 0 The value obtained by subtracting (Hz 30 -Hz 0 ) was defined as ΔHz (%).

[0084] (8) Heat Shrinkage in MD and TD A film was cut so that the measurement direction was 250 mm and the direction perpendicular to this was 10 mm, and marks were made at 150 mm intervals in the measurement direction. The spacing between the marks was measured under a constant tension of 5 gf, and this spacing was defined as A (mm). The cut film was then placed in an oven in an atmosphere of 150°C and heat-treated at 150±3°C for 30 minutes under no load, after which the spacing between the marks was measured under a constant tension of 5 gf, and this spacing was defined as B (mm). The heat shrinkage was calculated using the above values ​​of A and B according to the following formula: Heat shrinkage (%) = (A - B) / A × 100

[0085] (9) Amount of cyclic dimer contained in the entire film A polyester film was finely pulverized, and 50 mg of the pulverized polyester film was dissolved in 1.5 ml of a mixed solvent of hexafluoroisopropanol (HFIP) and chloroform (2 / 3 (volume ratio)). 10 ml of chloroform was added to the resulting solution and mixed uniformly. 5 ml of methanol was added to the resulting mixture to precipitate the polymer. Next, this mixture was filtered, and the resulting filtrate was concentrated to dryness using a rotary evaporator. 5 ml of dimethylformamide was added to the concentrated product, and the filtrate was subjected to HPLC analysis to quantify the amount of cyclic dimer. HPLC analysis conditions: Apparatus: Shimadzu UFLC Column: Imtakt Cadenza CD-C18 3 μm2 × 150 mm Mobile phase: A 0.1% formic acid, B acetonitrile 0 min (5% B) -18 (35) -45 (60) -50 (100) -55 (100) -55.01 (5) -60 (5) Flow rate: 0.4 mL / min Column temperature: 50 °C Injection volume: 5 μL Detection wavelength: 258 nm

[0086] (10) Amount of Cyclic Dimer on Film Surface A polyester film was scraped off from the surface to a thickness of 1 μm, and the amount of cyclic dimer on the film surface was determined using the same method as in (9) above.

[0087] (11) Color b * The color difference was evaluated using a ZE6000 colorimeter manufactured by Nippon Denshoku Industries Co., Ltd. Ten films were stacked and the reflection measurement was carried out using a white board. The value was rounded to the nearest tenth place and used as the color difference. * The value was set as

[0088] <Polyester Raw Materials> (1) Method for Producing PEF-A A starting mixture of 2,5-furandicarboxylic acid (FDCA) and ethylene glycol (EG) (the molar ratio of EG / FDCA is 1.5) was mixed with 149 ppm of tetraethylammonium hydroxide (N(Et) based on the molar amount of FDCA). 4A solution of basic aluminum acetate in ethylene glycol was used as the polycondensation catalyst, and a solution of 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid diethyl ester in ethylene glycol was used as the phosphorus compound. The amount of aluminum, based on the molar amount of FDCA in the starting mixture, was 202 ppm, and the amount of 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid diethyl ester was 435 ppm. The temperature was increased from 220°C to 270°C, and the pressure was reduced to 1 mmHg (approximately 133 Pa), and initial polycondensation was carried out for 60 minutes. Subsequently, a final polycondensation was carried out for 119 minutes at approximately 13 Pa and 270°C. At the end of the polycondensation, the pressure was returned to normal pressure, and the polycondensate was passed through a Hess-stranded water bath, cooled, and then cut into pellets. These pellets (raw material) were designated PEF-A. PEF-A had an intrinsic viscosity of 0.62 dL / g, a crystallization temperature of 170°C, a melting point of 215°C, a glass transition temperature of 86°C, and a cyclic dimer content of 1.1% by mass.

[0089] (2) Method for producing PEF-B PEF-A was dried under reduced pressure (1 Torr) at 80°C for 12 hours and then placed in a reaction vessel. Carbon dioxide was pumped from a pump connected to a carbon dioxide cylinder, and the pressure inside the reaction vessel was adjusted to 20 MPa using a pressure relief valve. A preliminary crystallization treatment was then carried out at 150°C for 30 minutes. After the preliminary crystallization treatment, the pressure was reduced to atmospheric pressure at 5 MPa / min, and solid-state polymerization was carried out at 190°C for 24 hours to obtain PEF-B. The intrinsic viscosity of PEF-B was 0.90 dL / g, and the amount of cyclic dimer was 0.43% by mass.

[0090] (3) Production method of PEF-C PEF-C was obtained by polymerization in the same manner as PEF-A, except that 0.05 mass% of silica particles (Sylysia 310 manufactured by Fuji Silysia Chemical Ltd., average particle size 2.7 μm) was added as an additive. The intrinsic viscosity of PEF-C was 0.62 dL / g, the crystallization temperature was 170°C, the melting point was 215°C, the glass transition temperature was 86°C, and the amount of cyclic dimer was 1.1 mass%.

[0091] (4) Method for Producing PEF-D PEF-C was dried under reduced pressure (1 Torr) at 80°C for 12 hours and then placed in a reaction vessel. Carbon dioxide was pumped from a pump connected to a carbon dioxide cylinder, and the pressure inside the reaction vessel was adjusted to 20 MPa using a pressure relief valve. A preliminary crystallization treatment was then carried out at 150°C for 30 minutes. After the preliminary crystallization treatment, the pressure was reduced to atmospheric pressure at 5 MPa / min, and solid-state polymerization was carried out at 190°C for 24 hours to obtain PEF-D. The intrinsic viscosity of PEF-D was 0.90 dL / g, and the amount of cyclic dimer was 0.43% by mass.

[0092] Example 1 PEF-D was used as the raw material. It was dried under reduced pressure (1 Torr) at 100°C for 24 hours to a moisture content of 80 ppm, and then fed to a twin-screw extruder (screw diameter 30 mm, L / D = 25). The raw material fed to the twin-screw extruder was melt-extruded into a sheet form from a T-die (die) at a resin temperature of 268°C in the extruder's melting section, kneading section, piping, and gear pump (resin temperature up to the gear pump) and 270°C in the piping after the gear pump. The time from when the resin contacted the extruder screw to when the sheet-shaped resin was extruded from the die (hereinafter referred to as melt line residence time) was 3 minutes.

[0093] The extruded resin was then cast onto a cooling drum having a surface temperature of 20° C., and adhered to the surface of the cooling drum using an electrostatic application method, followed by cooling and solidification to produce an unstretched film having a thickness of 300 μm.

[0094] The unstretched film was heated to 120°C using a group of rolls, and then stretched 5 times in the MD direction using a group of rolls with different peripheral speeds. The film was then introduced into a tenter, held with clips, and stretched in the TD direction at a stretching temperature of 105°C and a TD stretch ratio of 5 times. The film was then heat-treated at 200°C for 12 seconds, followed by a 5% relaxation treatment at 190°C to obtain a polyester film. The amount of cyclic dimer contained in the entire polyester film and the amount of cyclic dimer contained on the surface of the film were both 0.66% by mass (0.33 mol%). The physical properties of the resulting polyester film are shown in Table 2.

[0095] (Examples 2 to 5, Comparative Examples 1 to 3) Polyester films were obtained using the polyester raw materials shown in Table 1 in the same manner as in Example 1, except that the resin temperature up to the filter and the residence time in the melt line were changed to the conditions shown in Table 1. The physical properties of the obtained polyester films are shown in Table 2.

[0096] Example 6: As the raw material for the surface layer (B layer), PEF-B was dried under reduced pressure (1 Torr) at 100°C for 24 hours and then supplied to Extruder 1. As the raw material for the intermediate layer (A layer), PEF-A was dried under reduced pressure (1 Torr) at 100°C for 24 hours and then supplied to Extruder 2. The raw materials supplied to Extruder 1 and Extruder 2 were laminated in a B / A / B configuration using a three-layer confluence block, with the resin temperatures in the extruder's melting section, kneading section, polymer tube, gear pump, and filter (resin temperature up to the filter) set to 268°C and 270°C in the subsequent polymer tube. A sheet-like resin was then melt-extruded from the die. The thickness ratio of each layer was controlled using the gear pump for each layer to be B / A / B = 20 / 60 / 20. The melt line residence time was 3 minutes. After the sheet-like resin was melt-extruded, a polyester film was obtained using the same manufacturing method as in Example 1. The physical properties of the obtained polyester film are shown in Table 2.

[0097] (Examples 7 to 8, Comparative Example 4) Polyester films were obtained using the polyester raw materials shown in Table 1 in the same manner as in Example 6, except that the thickness ratio of each layer, the resin temperature up to the filter, and the residence time in the melt line were changed to the conditions shown in Table 1. The physical properties of the obtained polyester films are shown in Table 2.

[0098]

[0099]

[0100] Although the polyester film of the present invention uses biomass-derived furandicarboxylic acid, it has a low content of cyclic dimers and is less likely to lose transparency even when heated, making it suitable for use as an industrial or packaging film.

Claims

1. A polyester film consisting of a dicarboxylic acid component mainly composed of furandicarboxylic acid and a glycol component mainly composed of ethylene glycol, which satisfies the following requirements (1) to (3): (1) a plane orientation coefficient ΔP of 0.100 or more and 0.170 or less; (2) the haze of the polyester film is 15% or less; (3) the haze of the polyester film is Hz 0 (%), and the haze after heating the polyester film at 150° C. for 30 minutes was measured in Hz. 30 (%), Hz 30 -Hz 0 Meet ≦15 2. The polyester film according to claim 1, further satisfying the following requirement (4): (4) The content of cyclic dimer is 1.0% by mass or less.

3. The polyester film according to claim 1, which further satisfies the following requirements (5) and (6): (5) Having a laminated structure of three or more layers. (6) The content of cyclic dimers on at least one surface is 1.0% by mass or less.

Citation Information

Patent Citations

  • Polyester resin and molding comprising polyester resin

    JP2022155579A

  • Machine learning apparatus, machine learning method, and machine learning program

    JP2023048171A

  • Polyester film having a franjcarboxylic acid unit

    JP6440336B2

  • Method for producing polyester and polyester produced by said method

    WO2021172215A1

  • Laminated polyester film

    WO2017115736A1

Cited By

  • Polyester resin and production method therefor

    WO2026197164A1

  • Polyester film having furandicarboxylic acid unit and method for producing same

    WO2026211967A1