Tantalum carbide coating material and compound semiconductor growth device

The tantalum carbide coating material, characterized by reduced crack intersections and enhanced adhesion, addresses the peeling issue in high-temperature environments, improving the durability and cost-effectiveness of compound semiconductor manufacturing by preventing peeling and maintaining coating integrity.

WO2024203038A1PCT designated stage expired Publication Date: 2024-10-03SHIN ETSU CHEMICAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008317
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-05
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Compound semiconductors, such as SiC, face high manufacturing costs due to the need for highly heat-resistant components that withstand harsh environments exceeding 2000°C, where existing tantalum carbide coatings are prone to peeling in high-temperature corrosive conditions.

Method used

A tantalum carbide coating material with a reduced number of crack intersections per unit area (≤25 pieces/cm²), a surface roughness curve element length of 10 μm or less, and an adhesion strength of 5 MPa or more, applied using a CVD method to a carbon base material with a controlled linear thermal expansion coefficient, enhancing durability and preventing peeling.

Benefits of technology

The solution significantly reduces the likelihood of tantalum carbide coating film peeling in high-temperature corrosive environments, ensuring the coating's integrity and extending its usage in SiC single crystal production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008317_03102024_PF_FP_ABST
    Figure JP2024008317_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention is a tantalum carbide coating material 1 including a base material 12 and a tantalum carbide coating film 11 that coats at least a part of the base material 12, wherein the number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area is 25 / cm2 or less. A compound semiconductor growth device according to the present invention uses the tantalum carbide coating material according to the present invention. With the present invention, it is possible to provide a tantalum carbide coating material capable of suppressing peeling of a tantalum carbide coating film in a high-temperature, corrosive environment, and provide a compound semiconductor growth device using the tantalum carbide coating material.
Need to check novelty before this filing date? Find Prior Art

Description

Tantalum carbide coating material and compound semiconductor growth equipment

[0001] The present invention relates to a tantalum carbide coated material in which a tantalum carbide coating film is coated on the surface of a substrate, and a compound semiconductor growth apparatus using the tantalum carbide coated material.

[0002] Carbides such as tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, and tungsten carbide have high melting points and excellent chemical stability, strength, toughness, and corrosion resistance. Therefore, coating a carbon substrate with a carbide can improve the heat resistance, chemical stability, strength, toughness, corrosion resistance, and other properties of the carbon substrate. Carbide-coated carbon materials, particularly tantalum carbide-coated carbon materials, in which a carbide film is coated on the surface of a carbon substrate, are used as components of compound semiconductor growth devices for compound semiconductors such as SiC (silicon carbide), GaN (gallium nitride), and AlN (aluminum nitride). For example, Patent Document 1 discloses the use of a crucible whose inner surface is coated with tantalum carbide on a graphite substrate in order to obtain higher quality crystals in a SiC single crystal manufacturing device. Patent Document 2 also discloses the use of a guide member whose inner wall is coated with tantalum carbide in a SiC single crystal manufacturing device.

[0003] JP 2019-99453 A JP 2019-108611 A

[0004] However, compound semiconductors have the problem of higher manufacturing costs compared to conventional Si semiconductors. To further reduce this manufacturing cost, highly heat-resistant components with improved corrosion resistance are required. For example, the manufacturing environment for SiC single crystals is a harsh environment with temperatures exceeding 2000°C. Tantalum carbide coated materials are required to have high durability and not suffer from peeling of the tantalum carbide coating film even in such a high-temperature, corrosive environment.

[0005] Therefore, an object of the present invention is to suppress peeling of a tantalum carbide coating film in a high-temperature corrosive environment.

[0006] As a result of extensive research, the present inventors discovered that the fewer the number of crack intersections present on the surface of a tantalum carbide coating film, the less likely the tantalum carbide coating film will peel off after use in producing SiC single crystals, and completed the present invention. The gist of the present invention is as follows: [1] A tantalum carbide coating material comprising a substrate and a tantalum carbide coating film covering at least a portion of the substrate, wherein the number of crack intersections present on the surface of the tantalum carbide coating film per unit area is 25 / cm 2 [2] The tantalum carbide coating material according to [1] or [2] above, wherein the average length Rsm of the roughness curve elements on the surface of the tantalum carbide coating film is 10 μm or less. [3] The tantalum carbide coating material according to [1] or [2] above, wherein the average length Rsm of the roughness curve elements at the interface between the substrate and the tantalum carbide coating film is 0.1 mm or more and 5.0 mm or less. [4] The tantalum carbide coating material according to any one of [1] to [3] above, wherein the substrate is a carbon substrate containing carbon as a main component. [5] The tantalum carbide coating material according to any one of [1] to [4] above, wherein the adhesive strength between the tantalum carbide coating film and the substrate is 5 MPa or more. [6] The linear thermal expansion coefficient of the substrate is 3.5×10 -6 / ℃ or more 7.5 x 10 -6 / °C or less. [7] A compound semiconductor growth apparatus using the tantalum carbide coating material according to any one of [1] to [6] above.

[0007] According to the present invention, it is possible to provide a tantalum carbide coating material that can suppress peeling of the tantalum carbide coating film in a high-temperature corrosive environment, and a compound semiconductor growth apparatus that uses the tantalum carbide coating material.

[0008] FIG. 1 is a schematic cross-sectional view illustrating a tantalum carbide-coated material according to this embodiment. FIG. 2 is a schematic diagram of an external thermal low-pressure CVD apparatus. FIG. 3(a) is an image of a film surface having two cracks per unit area, with the cracks intersecting, and FIG. 3(b) is an image of the a-a' cross section of FIG. 3(a). FIG. 4(a) is an image of a film surface having two cracks per unit area, with the cracks not intersecting, and FIG. 4(b) is an image of the b-b' cross section of FIG. 4(a). FIG. 5 is a scanning electron microscope (SEM) photograph of the surface of a tantalum carbide-coated carbon material after use in the production of SiC single crystals. FIG. 6 is a diagram for explaining a method for measuring the adhesion strength between a tantalum carbide coating film and a substrate.

[0009] Referring to FIG. 1, a tantalum carbide coating material according to one embodiment of the present invention will be described.

[0010] [Tantalum carbide coated material] A tantalum carbide coated material 1 according to one embodiment of the present invention includes a substrate 12 and a tantalum carbide coating film 11 that coats at least a portion of the substrate 12. The number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area is 25 / cm. 2 The following is the result.

[0011] (Substrate) The substrate 12 in the tantalum carbide coated material 1 according to one embodiment of the present invention is not limited to a specific type as long as it is suitable for the intended use. Examples of the substrate 12 include carbon substrates primarily composed of carbon, such as isotropic graphite, extruded graphite, pyrolytic graphite, and carbon fiber-reinforced carbon composites (C / C composites), and high-melting-point metal substrates primarily composed of tantalum or other high-melting-point metal materials. Among these, the substrate 12 in the tantalum carbide coated material 1 according to one embodiment of the present invention is preferably a carbon substrate primarily composed of carbon. The shape and properties of the substrate are not particularly limited, and a substrate processed into any shape depending on the intended use can be used.

[0012] <Coefficient of Linear Thermal Expansion> The coefficient of linear thermal expansion of the substrate 12 is preferably 3.5×10 -6 / ℃ or more 7.5 x 10 -6 / °C or less. The linear thermal expansion coefficient of the carbon substrate 12 is 3.5 × 10 -6 / ℃ or more 7.5 x 10 -6 / °C or less, the occurrence of cracks on the surface of the tantalum carbide coating material 1 can be further suppressed. From this viewpoint, the linear thermal expansion coefficient of the carbon substrate 12 is more preferably 3.5 × 10 -6 / ℃ or more 7.5 x 10 -6 / °C or less, and more preferably 5.6 × 10 -6 / ℃ or more 7.5 x 10 -6 / °C or less. The linear thermal expansion coefficient of the tantalum carbide coating film 11 is approximately 6.3 × 10 -6 / °C. The linear thermal expansion coefficient of the substrate can be measured in accordance with JIS R 1618.

[0013] (Tantalum carbide coating film) The tantalum carbide coating film 11 contains tantalum carbide as a main component and coats the substrate 12. The tantalum carbide coating film 11 may coat a portion of the substrate 12 or the entire substrate 12.

[0014] <Number of Crack Intersections> The number of crack intersections present on the surface of the tantalum carbide coating film 11 per unit area is 25 / cm. 2 The number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area is 25 / cm 2 If the number is greater than 1, damage to the substrate 12 caused by cracks present on the surface of the tantalum carbide coating film 11 will become greater in a high-temperature corrosive environment, and the tantalum carbide coating film 11 may peel off. From this perspective, the number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area is preferably 24.9 / cm. 2 More preferably, 23 particles / cm or less. 2 More preferably, it is 21.3 particles / cm or less. 2 and even more preferably 13.4 cells / cm or less. 2 and particularly preferably 6.8 particles / cm 2 The lower limit of the range of the number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area is 0 / cm. 2The number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area can be adjusted by the average length Rsm of the roughness curve elements on the surface of the substrate 12 and the linear thermal expansion coefficient of the substrate 12.

[0015] The reason why a small number of crack intersections per unit area on the surface of the tantalum carbide coating film 11 can suppress peeling of the tantalum carbide coating film 11 is explained below. This explanation does not limit the tantalum carbide coating material of the present invention. It is known that when a tantalum carbide coating material 1 having cracks on the surface of the tantalum carbide coating film 11 is exposed to a high-temperature corrosive environment of 2000°C or higher, the substrate 12 is damaged around the cracks (see, for example, Japanese Patent Application Laid-Open No. 2022-87846). As the damaged portion of the substrate 12 becomes larger, the substrate 12 is no longer able to support the tantalum carbide coating film 11, resulting in peeling of the tantalum carbide coating film 11. Near the intersection of the cracks, two cracks cause greater damage to the substrate 12, so the damage to the substrate 12 rapidly increases. As a result, peeling of the tantalum carbide coating film 11 becomes even more likely to occur. Furthermore, when peeling of the tantalum carbide coating film 11 occurs, damage to the portion of the substrate 12 from which the tantalum carbide coating film 11 has peeled progresses. As a result, peeling of the tantalum carbide coating film 11 progresses further. The tantalum carbide coating material then falls into a vicious cycle of peeling of the tantalum carbide coating film 11 and damage to the substrate 12. Therefore, if the number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area is small, the progression of damage to the substrate caused by two cracks is suppressed, and peeling of the tantalum carbide coating film 11 is suppressed.

[0016] Here, when two cracks exist per unit area on the surface of the tantalum carbide coating film 11, we consider two cases: when the two cracks intersect (see FIG. 3 ) and when they do not intersect (see FIG. 4 ). When each tantalum carbide coating material 1 is exposed to a high-temperature corrosive environment, damage to the substrate 12 begins near the crack 31. However, when the cracks 31 have an intersection 30, the size of the damage 32 near the intersection 30 is expected to be larger than when the cracks 31 do not intersect (see FIGS. 3( b) and 4( b)). For this reason, peeling of the tantalum carbide coating film is more likely to occur near the crack intersection 30 than near a normal crack 31.

[0017] 5 is an image of the surface of the tantalum carbide-coated carbon material after use in a SiC single crystal growth environment, observed with a scanning electron microscope (SEM), and it can be seen that peeling of the tantalum carbide coating film has occurred at the intersections of the cracks. Therefore, if the number of intersections of the cracks present on the surface of the tantalum carbide coating film 11 per unit area is small, that is, if the number of intersections of the cracks present on the surface of the tantalum carbide coating film 11 per unit area is 25 / cm 2 If the thickness is less than this, peeling of the tantalum carbide coating film is less likely to occur when the tantalum carbide coated material is exposed to a high-temperature corrosive environment.

[0018] The number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area can be measured as follows: Because cracks occurring in the tantalum carbide coating material are not large enough to be seen with the naked eye, the number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area is measured by one or both of the following two methods.

[0019] (1) Measurement by scanning electron microscope (SEM) The sample is processed to a size that can be observed by SEM, and its surface is observed. In this case, the information obtained from one image is about 6 mm at most. 2 (= 2mm x 3mm), so 1cm 2To observe a range of 170 minutes, it is necessary to acquire approximately 17 images. Furthermore, to avoid bias due to local observation, it is necessary to acquire approximately 17 images at another location that is sufficiently distant. This operation is repeated 10 times to acquire a total of 170 or more images, and the number of crack intersections is counted from these 170 or more images. The value obtained by dividing the number of crack intersections by the area of ​​the portion observed using the acquired 170 or more images is the number of crack intersections per unit area (cracks / cm) present on the surface of the tantalum carbide coating film 11. 2 )

[0020] (2) Measurement using flaw detection agent Depending on the shape of the sample, processing may be necessary for SEM observation, and during this processing, cracks may appear on the surface of the tantalum carbide coating film. To eliminate this possibility, cracks are visualized using a flaw detection agent that can detect cracks on the order of μm, and the cracks are then measured by visual inspection or by using an optical microscope. 2 The number of crack intersections per hit may be measured.

[0021] <Average Length Rsm of Roughness Curve Elements> The average length Rsm of the roughness curve elements on the surface of the tantalum carbide coating film 11 is preferably 10 μm or less. If the average length Rsm of the roughness curve elements on the surface of the tantalum carbide coating film 11 is 10 μm or less, it is possible to prevent dust particles and the like from adhering to the surface of the tantalum carbide coating film 11 in the atmosphere. From this perspective, the average length Rsm of the roughness curve elements on the surface of the tantalum carbide coating film 11 is more preferably 9.8 μm or less, and even more preferably 6.5 μm or less. The lower limit of the range of the average length Rsm of the roughness curve elements on the surface of the tantalum carbide coating film 11 is not particularly limited, but is usually 1.1 μm.

[0022] The average length Rsm of the roughness curve elements at the interface between the substrate 12 and the tantalum carbide coating film 11 is preferably 0.1 mm or more and 5.0 mm or less. When the average length Rsm of the roughness curve elements at the interface between the substrate 12 and the tantalum carbide coating film 11 is 0.1 mm or more and 5.0 mm or less, the adhesion strength between the substrate 12 and the tantalum carbide coating film 11 can be further increased. Furthermore, when the average length Rsm of the roughness curve elements at the interface between the substrate 12 and the tantalum carbide coating film 11 is 0.1 mm or more and 5.0 mm or less, the number of intersections of cracks present per unit area on the surface of the tantalum carbide coating film 11 can be further reduced. From this perspective, the average length Rsm of the roughness curve elements at the interface between the substrate 12 and the tantalum carbide coating film 11 is more preferably 0.5 mm or more and 5.0 mm or less, even more preferably 1.0 mm or more and 5.0 mm or less, and even more preferably 2.0 mm or more and 5.0 mm or less. The average length Rsm of the roughness curve elements at the interface between the substrate 12 and the tantalum carbide coating film 11 is the same value as the average length Rsm of the roughness curve elements on the surface of the substrate 12. Therefore, by setting the average length Rsm of the roughness curve elements on the surface of the substrate 12 within the above range, the average length Rsm of the roughness curve elements at the interface between the substrate 12 and the tantalum carbide coating film 11 can be set within the above range. The average length Rsm of the roughness curve elements on the surface of the substrate 12 may be due to an intentionally created pattern or may be due to marks left by a cutting tool during machining.

[0023] The average length RSm of the roughness curve element can be measured using a commercially available surface roughness meter or a microscopic image of the fracture cross section, and is the average length of the roughness curve element specified in JIS B0601:2013 and ISO 4287:1997. The average length RSm of the roughness curve element is calculated by multiplying the distance x from the i-th peak to the (i+1)-th peak of the cross-sectional profile curve. i Using m, the number of intervals between peaks, it can be expressed by the following formula: Rsm = (1 / m) × Σx i(i = 1 to m) The minimum height to be judged as a mountain is 10% of the average height Rz of the cross-sectional profile. It can be said that the larger the value of the average length Rsm of the roughness curve element, the larger the periodic interval of the roughness formed, and the smaller the value of the average length Rsm of the roughness curve element, the smaller the periodic interval of the roughness formed.

[0024] The adhesion strength between the tantalum carbide coating film 11 and the substrate 12 is preferably 5 MPa or more. When the adhesion strength between the tantalum carbide coating film 11 and the substrate 12 is 5 MPa or more, peeling of the tantalum carbide coating film in a high-temperature corrosive environment can be further suppressed. From this perspective, the adhesion strength between the tantalum carbide coating film 11 and the substrate 12 is more preferably 5.1 MPa or more, and even more preferably 6.5 MPa or more. The upper limit of the range of the adhesion strength between the tantalum carbide coating film 11 and the substrate 12 is not particularly limited, but is usually 18.5 MPa.

[0025] The adhesion strength between the tantalum carbide coating film 11 and the substrate 12 was measured, for example, using a thin film adhesion strength measuring device (manufactured by Quad Group, product name "Romulus"), by adhering the tantalum carbide coating film 11 and a pin 46 with adhesive 45, pressing down with a pressing jig 44, and pulling the pin 46, as shown in Fig. 6, to measure the stress when the tantalum carbide coating film 41 peeled off. Five measurements were made, and the calculated average of the five measurements was taken as the adhesion strength.

[0026] <Method for producing tantalum carbide coated material> The tantalum carbide coated material of one embodiment of the present invention can be produced by forming a tantalum carbide coating film on the surface of a substrate. The tantalum carbide coating film can be formed on the surface of the substrate by methods such as chemical vapor deposition (CVD), sintering, and carbonization. Among these, the CVD method is preferred as a method for forming a tantalum carbide layer because it can form a uniform and dense film.

[0027] Furthermore, CVD methods include thermal CVD, photo-CVD, and plasma CVD, and for example, thermal CVD can be used to form a tantalum carbide coating film. Thermal CVD has advantages such as a relatively simple apparatus configuration and no damage caused by plasma. Formation of a tantalum carbide coating film by thermal CVD can be performed, for example, using an externally heated low-pressure CVD apparatus 20 as shown in Figure 2. In the externally heated low-pressure CVD apparatus 20, the substrate 12 is supported by a support means 25 in a reaction chamber 24 equipped with a heater 21, a raw material supply unit 22, an exhaust unit 23, etc.

[0028] A method for producing a tantalum carbide coated material according to one embodiment of the present invention will be described with reference to FIGS. 1 and 2. First, the substrate 12 is placed in the reaction chamber 24 of the externally heated reduced pressure CVD apparatus 20. The substrate 12 is supported by a support means 25 having a support portion with a pointed tip. Next, the heater 21 is heated. For example, the heater 21 is heated under reduced pressure at a temperature of 1000 to 2500°C. Next, a tantalum carbide coating film is formed on the surface of the substrate 12. Methane (CH 4 ) and tantalum pentachloride (TaCl 5 ) is supplied to the reaction chamber 24. Subsequently, the source gas supplied from the source supply unit 22 is subjected to a thermal CVD reaction at a high temperature of 1000 to 2500°C under reduced pressure, thereby forming a tantalum carbide coating film on the surface of the substrate 12.

[0029] The tantalum carbide coating material of one embodiment of the present invention is merely one example of the tantalum carbide coating material of the present invention, and therefore does not limit the tantalum carbide coating material of the present invention.

[0030] [Compound Semiconductor Growth Apparatus] The compound semiconductor growth apparatus of the present invention uses the tantalum carbide coating material of the present invention. The tantalum carbide coating material of the present invention is used as a component of a compound semiconductor growth apparatus for growing compound semiconductors such as SiC (silicon carbide), GaN (gallium nitride), and AlN (aluminum nitride).

[0031] The present invention will be explained in more detail below by showing examples, but the present invention is not limited to these examples.

[0032] Tantalum carbide-coated carbon materials of Examples 1 to 17 and Comparative Examples 1 to 6 were prepared as follows.

[0033] (Example 1) The substrate 12 is a glass substrate having a linear thermal expansion coefficient of 3.5×10 -6 Two isotropic carbon materials were prepared, each having a coefficient of thermal expansion of 1 / °C and a mean length Rsm of the surface roughness curve element of 4.3 mm. The linear thermal expansion coefficient of the same carbon material sample was measured using a thermomechanical analyzer (manufactured by Hitachi High-Tech Science Corporation, product name "TMA7300"). The mean length Rsm of the surface roughness curve element of the substrate 12 was measured using a surface roughness meter (manufactured by Mitutoyo Corporation, product name "SJ201"). Next, the substrate 12 was placed in the reaction chamber of the externally heated reduced pressure CVD apparatus 20 shown in Figure 2. The substrate 12 was supported by a support means 25 having three support portions with pointed tips. Next, the reaction chamber 24 was heated to a temperature of 1500°C, and then TaCl 5 Gas, CH 4 The gas and Ar gas were mixed, and the resulting mixed gas was supplied to the reaction chamber 24, where a tantalum carbide coating film was formed on the surface of the carbon substrate 12, thereby producing the tantalum carbide-coated carbon material of Example 1. 4 The flow rates of the gas and carrier gas (Ar) were controlled to be 1.0 SLM and 1.0 SLM, respectively.

[0034] Of the two tantalum carbide-coated carbon materials thus produced, one was used for various measurements described below, and the other was used to produce SiC single crystals, and the number of uses was counted until peeling of the tantalum carbide coating film became visible to the naked eye.

[0035] For one of the prepared tantalum carbide-coated carbon materials, the number of crack intersections per unit area present on the surface of the tantalum carbide coating film, the average length Rsm of the roughness curve element of the surface of the tantalum carbide coating film, and the adhesion strength between the tantalum carbide coating film and the substrate were measured. The method for measuring the number of crack intersections per unit area present on the surface of the tantalum carbide coating film was as described above, using an SEM (manufactured by Keyence Corporation, product name "VE8800") and flaw detectors (Microcheck cleaning solution, Microcheck penetrant solution, and Microcheck developer, both manufactured by Ichinen Chemicals Corporation). The surface roughness of the tantalum carbide coating film was measured with a surface roughness meter (manufactured by Mitutoyo Corporation, product name "SJ201"). The adhesion strength between the substrate 12 and the tantalum carbide coating film 11 was measured with a thin film adhesion strength tester (manufactured by Quad Group, product name "Romulus").

[0036] (Example 2) The substrate 12 has a thermal expansion coefficient of 4.2 × 10 -6 Two isotropic carbon materials having a surface roughness of 4.2 mm, a viscosity of 1000 ppm / ° C., and an average length Rsm of the surface roughness curve element of 4.2 mm were prepared.

[0037] (Example 3) The substrate 12 has a thermal expansion coefficient of 4.5×10 -6 Two isotropic carbon materials having a surface roughness of 4.6 mm, a viscosity of 1000 ppm / ° C., and an average length Rsm of the surface roughness curve element of 4.6 mm were prepared.

[0038] (Example 4) The substrate 12 has a thermal expansion coefficient of 5.1 × 10 -6 Two isotropic carbon materials having a surface roughness of 4.1 mm, a viscosity of 1000 ppm / ° C., and an average length Rsm of the surface roughness curve element of 4.1 mm were prepared.

[0039] (Example 5) The substrate 12 has a thermal expansion coefficient of 5.6 × 10 -6 Two isotropic carbon materials having a surface roughness of 4.5 mm, a surface roughness of 4.5 mm, and an average length Rsm of the surface roughness curve element were prepared.

[0040] (Example 6) The substrate 12 has a thermal expansion coefficient of 6.0 × 10 -6Two isotropic carbon materials having a surface roughness of 4.4 mm, a viscosity of 1000 ppm / ° C., and an average length Rsm of the surface roughness curve element of 4.4 mm were prepared.

[0041] (Example 7) The substrate 12 has a thermal expansion coefficient of 6.4 × 10 -6 Two isotropic carbon materials having a surface roughness of 4.4 mm, a viscosity of 1000 ppm / ° C., and an average length Rsm of the surface roughness curve element of 4.4 mm were prepared.

[0042] (Example 8) The substrate 12 has a thermal expansion coefficient of 6.9 × 10 -6 Two isotropic carbon materials having a surface roughness of 4.3 mm, a viscosity of 1000 ppm / ° C., and an average length Rsm of the surface roughness curve element of 4.3 mm were prepared.

[0043] (Example 9) The substrate 12 has a thermal expansion coefficient of 7.5×10 -6 Two isotropic carbon materials having a surface roughness of 4.2 mm, a surface roughness curve element average length Rsm of 4.2 mm, and a surface roughness of 4.2 mm were prepared.

[0044] (Example 10) As the substrate 12, a material having a linear thermal expansion coefficient of 4.2 × 10 -6 Two isotropic carbon materials having a surface roughness of 0.1 mm and a mean length Rsm of the surface roughness curve element were prepared.

[0045] (Example 11) As the substrate 12, a material having a linear thermal expansion coefficient of 4.2 × 10 -6 Two isotropic carbon materials having a surface roughness of 0.9 mm and a mean length Rsm of the surface roughness curve element were prepared.

[0046] (Example 12) As the substrate 12, a material having a linear thermal expansion coefficient of 4.2 × 10 -6 Two isotropic carbon materials having a surface roughness of 2.1 mm, a viscosity of 1000 ppm / ° C., and an average length Rsm of the surface roughness curve element of 2.1 mm were prepared.

[0047] (Example 13) As the substrate 12, a material having a linear thermal expansion coefficient of 4.2 × 10 -6Two isotropic carbon materials having a surface roughness of 3.5 mm, a surface roughness curve element average length Rsm of 3.5 mm, and a surface roughness of 3.5 mm were prepared.

[0048] (Example 14) As the substrate 12, a material having a linear thermal expansion coefficient of 4.2 × 10 -6 Two isotropic carbon materials having a surface roughness of 5.0 mm, a surface roughness of 5.0 mm, and an average length Rsm of the surface roughness curve element were prepared.

[0049] (Example 15) As the substrate 12, a material having a linear thermal expansion coefficient of 6.4 × 10 -6 Two isotropic carbon materials having a surface roughness of 0.04 mm, a surface roughness curve element average length Rsm of 0.04 mm, and a surface roughness of 0.04 mm were prepared.

[0050] (Example 16) As the substrate 12, a material having a linear thermal expansion coefficient of 6.9 × 10 -6 Two isotropic carbon materials having a surface roughness of 0.02 mm, a surface roughness curve element average length Rsm of 0.02 mm, and a surface roughness of 0.02 mm were prepared.

[0051] (Example 17) As the substrate 12, a material having a linear thermal expansion coefficient of 7.5 × 10 -6 Two isotropic carbon materials having a surface roughness of 0.06 mm Rsm were prepared.

[0052] (Comparative Example 1) The substrate 12 has a linear thermal expansion coefficient of 3.5 × 10 -6 Two isotropic carbon materials having a surface roughness of 0.04 mm, a surface roughness curve element average length Rsm of 0.04 mm, and a surface roughness of 0.04 mm were prepared.

[0053] (Comparative Example 2) The substrate 12 has a linear thermal expansion coefficient of 4.2 × 10 -6 Two isotropic carbon materials having a surface roughness of 0.06 mm Rsm were prepared.

[0054] (Comparative Example 3) The substrate 12 has a linear thermal expansion coefficient of 4.5 × 10 -6Two isotropic carbon materials having a surface roughness of 0.03 mm and a mean length Rsm of the surface roughness curve element were prepared.

[0055] Comparative Example 4: The substrate 12 has a linear thermal expansion coefficient of 5.1 × 10 -6 Two isotropic carbon materials having a surface roughness of 0.03 mm and a mean length Rsm of the surface roughness curve element were prepared.

[0056] Comparative Example 5: The substrate 12 has a linear thermal expansion coefficient of 5.6×10 -6 Two isotropic carbon materials having a surface roughness of 0.06 mm Rsm were prepared.

[0057] (Comparative Example 6) The substrate 12 has a linear thermal expansion coefficient of 6.0 × 10 -6 Two isotropic carbon materials having a surface roughness of 0.07 mm and a mean length Rsm of the surface roughness curve element were prepared.

[0058] The evaluation results of Examples 1 to 17 and Comparative Examples 1 to 6 are shown in Table 1.

[0059] <Evaluation Result 1> Examples 1 to 17 and Comparative Examples 1 to 6 are compared. The number of intersections of cracks present on the surface of the tantalum carbide coating film per unit area was 25 / cm. 2 If the crack density is less than 25 / cm, the number of intersections of cracks on the surface of the tantalum carbide coating film per unit area is 25 / cm. 2 In a SiC single crystal growth environment, the tantalum carbide coating material can be used for a longer period of time before the tantalum carbide coating film peels off, compared to when the number of crack intersections per unit area is 25 / cm. 2 It can be seen that if the temperature is below this, peeling of the tantalum carbide coating film is less likely to occur.

[0060] <Evaluation Result 2> Comparing Examples 1 to 14 with Examples 15 to 17 and Comparative Examples 1 to 6, it was found that when the average length Rsm of the roughness curve elements of the surface of the tantalum carbide coating film was 10 μm or less, the number of uses until the tantalum carbide coating film of the tantalum carbide coating material peeled off in a SiC single crystal growth environment was greater than when the average length Rsm of the roughness curve elements of the surface of the tantalum carbide coating film was greater than 10 μm. This shows that when the average length Rsm of the roughness curve elements of the surface of the tantalum carbide coating film is 10 μm or less, peeling of the tantalum carbide coating film becomes even less likely to occur.

[0061] <Evaluation Result 3> For Example 2, Examples 10 to 14, and Comparative Example 2, the linear thermal expansion coefficient was 4.2 × 10 -6 / °C carbon material was used as the substrate 12. When the average length Rsm of the roughness curve elements on the surface of the substrate was 0.1 mm or more and 5 mm or less (Example 2 and Examples 10 to 14), the number of intersections of cracks present on the surface of the tantalum carbide coating film per unit area was smaller and the number of uses until peeling of the tantalum carbide coating film occurred was greater than when the average length Rsm of the roughness curve elements on the surface of the substrate was 0.06 mm (Comparative Example 2). Therefore, it is clear that a case where the average length Rsm of the roughness curve elements on the surface of the substrate is 0.1 mm or more and 5 mm or less is preferable.

[0062] <Evaluation Result 4> Example 1 and Comparative Example 1, Example 2 and Comparative Example 2, Example 3 and Comparative Example 3, Example 4 and Comparative Example 4, Example 5 and Comparative Example 5, Example 6 and Comparative Example 6, Example 7 and Example 15, Example 8 and Example 16, and Example 9 and Example 17 are compared. When carbon materials with the same linear thermal expansion coefficient are used, when the average length Rsm of the roughness curve elements on the surface of the carbon material is 0.1 mm or more and 5 mm or less, the number of intersections of cracks present on the surface of the tantalum carbide coating film per unit area is smaller, the adhesion strength is greater (5 MPa or more), and the number of uses until peeling of the tantalum carbide coating film occurs is greater than when the average length Rsm of the roughness curve elements on the surface of the carbon material is less than 0.1 mm. Therefore, it can be seen that a case where the average length Rsm of the roughness curve elements on the surface of the substrate is 0.1 mm or more and 5 mm or less is preferable. Therefore, it can be seen that a case where the average length Rsm of the roughness curve elements at the interface between the substrate and the tantalum carbide coating film is 0.1 mm or more and 5.0 mm or less is preferable.

[0063] REFERENCE SIGNS LIST 1... Tantalum carbide coating material 11... Tantalum carbide coating film 12... Substrate 20... External heat type low pressure CVD apparatus 21... Heater 22... Raw material supply section 23... Exhaust section 24... Reaction chamber 25... Support means 30... Crack intersection 31... Crack 32... Damage 44... Holding jig 45... Adhesive 46... Pin

Claims

1. A tantalum carbide coating material comprising a substrate and a tantalum carbide coating film covering at least a portion of the substrate, wherein the number of intersections of cracks present on the surface of the tantalum carbide coating film per unit area is 25 / cm 2 Tantalum carbide coated material, which is:

2. The tantalum carbide coating material according to claim 1, wherein the average length Rsm of the roughness curve elements of the surface of said tantalum carbide coating film is 10 μm or less.

3. The tantalum carbide coating material according to claim 1, wherein the average length Rsm of the roughness profile elements at the interface between the substrate and the tantalum carbide coating film is 0.1 mm or more and 5.0 mm or less.

4. The tantalum carbide coating material according to claim 1, wherein the substrate is a carbon substrate containing carbon as a main component.

5. The tantalum carbide coated material according to claim 1, wherein the adhesive strength between said tantalum carbide coating film and said substrate is 5 MPa or more.

6. The linear thermal expansion coefficient of the substrate is 3.5 x 10 -6 / ℃ or more 7.5 x 10 -6 2. The tantalum carbide coating material according to claim 1, wherein the temperature is 0.15 to 1.5° C.

7. A compound semiconductor growth device using the tantalum carbide coating material according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Carbon composite material for reducing atmosphere furnace, and its production

    JP1998245285A

  • Carbon composite material

    JP2004084057A