Powder for thermal spraying material
The thermal spray material powder with specific fluidity and alumina content characteristics addresses the issue of film thickness variability and reproducibility, enhancing the consistency and efficiency of thermal spraying by minimizing agglomeration and ensuring stable film formation across different lots.
Patent Information
- Application Number
- PCT/JP2024/008660
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-03
AI Technical Summary
Thermal spray materials face challenges with variations in film thickness and reproducibility due to the cohesive properties of aluminum powder, which affect the fluidity and agglomeration of powders, leading to clogged transport paths and inefficient film formation.
A thermal spray material powder with an angle of repose of 35° or less and a water concentration of 100 mg/kg or less, combined with a preferred alumina content of 20% to 60% by weight, is used to improve fluidity and reduce agglomeration, ensuring consistent film thickness and reproducibility across different lots.
The solution reduces variations in film thickness and improves reproducibility by enhancing the fluidity and cohesiveness of the powder, resulting in more stable and efficient thermal spraying processes.
Smart Images

Figure JP2024008660_03102024_PF_FP_ABST
Abstract
Description
Thermal spray powder
[0001] The present invention relates to a powder for a thermal spray material.
[0002] For example, International Publication No. 2015 / 079906 (Patent Document 1) proposes a thermal spray material that can efficiently form a thermal spray coating made of ceramics having a dense and fine structure.
[0003] International Publication No. 2015 / 079906
[0004] When thermally spraying aluminum powder, the powder is pneumatically transported from a powder supply device to the spray nozzle of a coating device. However, aluminum powder has a high tendency to agglomerate if its particle size is approximately 10 μm or less. Therefore, continuous transport becomes difficult due to the influence of agglomerated powder. As a result, problems such as powder clogging in the transport path and large variations in the thickness of the formed film occur.
[0005] The cohesion of the powder is improved by improving the flowability of the powder. To improve the flowability of the powder, alumina powder has conventionally been mixed with aluminum powder for thermal spraying. The ratio of alumina powder to the total mixed powder is, for example, about 50% by weight or less. However, if the ratio of alumina powder mixed is low, a small amount of agglomerated powder may remain. This may result in problems such as uneven film thickness during film formation. However, if the alumina powder content is increased to exceed 50% by weight, the film formation efficiency decreases accordingly.
[0006] Furthermore, the cohesion of aluminum powder varies between different lots. In other words, the optimal ratio of alumina powder to be mixed varies for each aluminum powder lot. Therefore, even if alumina powder is mixed at the same ratio, the state of the aluminum powder will change for each lot. As a result, there is an issue of being unable to achieve reproducibility in the film formation.
[0007] The above-mentioned International Publication No. 2015 / 079906 discloses a thermal spray material in which the purity of ceramic particles is much higher than 50% by weight, but does not consider the above-mentioned viewpoint.
[0008] The present invention has been made in view of the above-mentioned problems, and has as its object to provide a powder for a thermal spray material that reduces the variation in film thickness after formation and that can achieve reproducible reduction in film thickness variation even between different lots.
[0009] The thermal spray powder according to the present disclosure has an angle of repose of 35° or less and a moisture concentration of 100 mg / kg or less.
[0010] According to the above, it is possible to provide a powder for a thermal spray material that reduces the variation in film thickness after formation and that can achieve reproducible reduction in film thickness variation even between different lots.
[0011] 1. A schematic diagram showing the configuration of a film forming apparatus according to the present embodiment. 2. A schematic diagram showing the configuration of equipment used to measure the angle of repose of powder. 3. A schematic diagram showing a mechanism for measuring powder deposited on a pedestal. 4. A schematic diagram of a model in which an angle of repose is formed by an angle measurement method. 5. A schematic diagram showing a state in which a large amount of moisture adheres to the periphery of aluminum powder. 6. A schematic diagram showing the state in which the aluminum powder of FIG. 5 is aggregated. 7. A schematic diagram showing an ideal state of aluminum powder. 8. A photograph showing the appearance of aluminum powder from different lots. 9. A photograph showing the appearance of aluminum powder and a mixed powder of aluminum powder and alumina powder. 10. A graph showing the thickness of a film formed by thermal spraying for each lot of powder in which aluminum powder and alumina powder are mixed, with and without heat treatment. 11. A graph showing the change in the amount of moisture contained in the powder and the angle of repose of the powder, with respect to the heating time of the powder. 12. A photograph showing the appearance of the mixed powder from which the data of FIG. 11 was obtained, before and after heating. 13. A schematic diagram showing a plan view of a film formed on a substrate. 14. A hatched color map showing the planar shape of a thin film formed by thermal spraying using powder without heat treatment. 17 is a hatched color map showing the planar shape of a thin film formed by thermal spraying using a heat-treated powder. FIG. 18 is a graph showing the relationship between the heating time of a powder and the variation in film thickness of a film formed by thermal spraying of the powder. FIG. 19 is a hatched color map of a film formed by thermal spraying of each sample shown in FIG. 16. FIG. 19 is a graph showing the relationship between the heating time of a powder and the moisture content and angle of repose. FIG. 19 is a graph showing the relationship between the weight percentage of alumina powder in a powder and the angle of repose and deposition efficiency of the powder. FIG. 19 is a graph showing the difference in angle of repose between heated and unheated mixed powders of aluminum and alumina. FIG. 19 is a graph showing the difference in deposition efficiency between heated and unheated mixed powders of aluminum and alumina.
[0012] Hereinafter, embodiments of the present disclosure will be described. Note that the same reference numerals are used to designate the same components, and the description thereof will not be repeated.
[0013] 1 is a schematic diagram showing the configuration of a film formation apparatus according to the present embodiment. Referring to FIG. 1, the film formation apparatus 100 mainly includes a spray gun 2 including a nozzle 2 b, a powder supply unit 3, a gas supply unit 4, and a mask jig 1.
[0014] The spray gun 2 mainly includes a spray gun main body 2a, a nozzle 2b, a heater 2c, and a temperature sensor 9. The nozzle 2b is connected to a first end, which is the front end of the spray gun main body 2a. A pipe 6 is connected to a second end, which is the rear end of the spray gun main body 2a. The pipe 6 is connected to a gas supply unit 4 via a valve 7. The gas supply unit 4 supplies operating gas to the spray gun 2 via the pipe 6. The supply state of operating gas from the gas supply unit 4 to the spray gun 2 can be controlled by opening and closing the valve 7. A pressure sensor 8 is installed in the pipe 6. The pressure sensor 8 measures the pressure of the operating gas supplied to the pipe 6 from the gas supply unit 4.
[0015] The working gas supplied from the second end of the spray gun body 2a to the interior of the spray gun body 2a is heated by a heater 2c. The heater 2c is located on the second end side of the spray gun body 2a. The working gas flows inside the spray gun body 2a along the arrow 31. A temperature sensor 9 is connected to the connection between the nozzle 2b and the spray gun body 2a. The temperature sensor 9 measures the temperature of the working gas flowing inside the spray gun body 2a.
[0016] A pipe 5 is connected to the nozzle 2b. The pipe 5 is connected to the powder supply unit 3. The powder supply unit 3 supplies powder, which is a film-forming raw material, to the nozzle 2b of the spray gun 2 via the pipe 5.
[0017] The mask jig 1 is placed between the substrate 20 and the spray gun 2. A through hole 1a is formed in the mask jig 1. The through hole 1a defines a film formation area on the surface of the substrate 20. However, the film formation apparatus 100 does not necessarily have to be provided with the mask jig 1. The mask jig 1 does not necessarily have to be used in the film formation process using the film formation apparatus 100.
[0018] <Operation of the Film Forming Apparatus> In the film forming apparatus 100 shown in FIG. 1 , an operating gas is supplied from the gas supply unit 4 to the spray gun 2 via a pipe 6, as indicated by an arrow 30. Examples of the operating gas that can be used include nitrogen, helium, dry air, and mixtures thereof. The operating gas has a pressure of, for example, approximately 1 MPa. The flow rate of the operating gas is, for example, 300 L / min or more and 500 L / min or less. The operating gas supplied to the second end of the spray gun main body 2a is heated by a heater 2c. The heating temperature of the operating gas is set appropriately depending on the composition of the film forming raw material, but can be, for example, 100°C or more and 500°C or less. The operating gas flows from the spray gun main body 2a to the nozzle 2b. Powder 10, which serves as a film forming raw material, is supplied to the nozzle 2b from the powder supply unit 3 via a pipe 5, as indicated by an arrow 32. For example, aluminum powder is used as the powder 10.
[0019] The powder 10 supplied to the nozzle 2b is sprayed together with the operating gas from the tip of the nozzle 2b toward the substrate 20. A mask jig 1 is placed on the surface of the substrate 20. The sprayed powder 10 reaches the surface of the substrate 20 through the through holes 1a of the mask jig 1. A film made of the sprayed powder 10 as a raw material is formed on the surface of the substrate 20.
[0020] <Regarding Powder 10> In this embodiment, the powder 10 (thermal spray powder) used has an angle of repose of 35° or less. Here, the angle of repose is a well-known index that indicates the fluidity of a powder. The angle of repose is the angle of the slope of a powder mound formed when the powder is dropped onto a horizontal plane from a height of, for example, 160 mm, relative to the horizontal plane.
[0021] The moisture concentration of powder 10 is 100 mg / kg or less. Here, the moisture concentration is the amount of moisture expressed as a concentration. In other words, the moisture concentration indicates the ratio of the mass of water contained in powder 10 to the total mass of powder 10. In other words, the moisture concentration of powder 10 is the mass-based moisture content based on the Karl Fischer method. A moisture concentration of powder 10 of 100 mg / kg or less indicates that the amount of moisture contained in 1 kg of powder 10 is 100 mg or less. Furthermore, a moisture concentration of powder 10 of 100 mg / kg or less is equivalent to a moisture concentration of powder 10 of 100 ppm. The moisture in powder 10 is mainly present on the surface of powder 10.
[0022] The powder 10 preferably has a particle diameter of 10 μm or less. This means that the average particle diameter of the powder 10 is 10 μm or less. Even if the powder 10 contains multiple types of materials, as described below, the average diameter of all particles contained in the powder 10 is 10 μm or less, regardless of the type of material. The average particle diameter of the powder 10 is measured by a laser diffraction / scattering particle size distribution measurement method using an MT3300EXII manufactured by Microtrac.
[0023] In this embodiment, the powder 10 preferably comprises aluminum (Al) powder. However, the powder 10 of this embodiment is not limited to aluminum powder, and can be applied to powders of other materials that aggregate due to moisture. In addition, the powder 10 may be alumina (Al 2 O 3 In this case, the content of the alumina powder in the entire powder 10 is preferably 20% by weight or more and 60% by weight or less. In particular, the content of the alumina powder in the powder 10 is preferably 30% by weight or more and 50% by weight or less.
[0024] <Manufacturing Method> The powder 10 containing only aluminum powder is formed by preparing aluminum powder and heating it under vacuum, normal air, or an inert gas atmosphere, which removes at least a portion of the moisture contained in the powder.
[0025] The same applies to the powder 10 containing both aluminum powder and alumina powder: first, the aluminum powder and the alumina powder are mixed together, and then, in the same manner as in the case of only aluminum powder, the moisture is removed by heating.
[0026] The heating temperature in the above manufacturing method is preferably 150°C or higher and 200°C or lower. <Method of Measuring Parameters> The angle of repose of powder 10 is measured using a commonly known powder property measuring device. FIG. 2 is a schematic diagram showing the configuration of equipment used to measure the angle of repose of a powder. Referring to FIG. 2, the angle of repose of powder 10 can be measured using, for example, an apparatus called Powder Tester (registered trademark) PT-X. The above-mentioned angle of repose measuring device comprises a sieve 41, a funnel 42, and a base 43. In this measuring device, as shown in FIG. 2, the sieve 41 is placed on the funnel 42, and the funnel 42 is placed on the base 43 at a distance from each other. The sieve 41 used is a JIS-Z 8801 sieve for testing. The JIS-Z 8801 sieve 41 has a mesh size of 150 μm. The funnel 42 has a discharge outlet diameter of 5.0 mm. The portion of base 43 where the powder is placed (the portion indicated by the lead line in FIG. 2 ) is circular, and the diameter of the circle in plan view is 80 mm. The portion of base 43 where the powder is placed is located at a vertical distance of, for example, 160 mm from the outlet, which is the lowest part of funnel 42.
[0027] During measurement, powder 10 is first poured onto sieve 41. Then, sieve 41 is vibrated to sieve off the powder 10. The sieved off powder 10 passes through funnel 42. The powder 10 is piled up on base 43 in a mountain-like shape. The angle of repose θ1 shown in FIG. 2 is determined as follows.
[0028] FIG. 3 is a schematic diagram showing a mechanism for measuring powder deposited on a pedestal. Referring to FIG. 3, the angle of repose θ1 in FIG. 2 is measured by angle measurement using image processing. Specifically, as shown in the upper part of FIG. 3, a pedestal 43 is first installed between a camera 44 and an LED light source 45 so that they are spaced apart in the horizontal direction. As shown in the lower part of FIG. 3, light 46 emitted by the LED light source 45 and a shadow 47 are binarized. The shadow 47 is formed by the powder 10 blocking the light 46. The shadow 47 has a triangular shape in FIG. 3. The angle of the ridge of the shadow 47 relative to the horizontal direction is defined as the angle of repose θ1.
[0029] Fig. 4 is a schematic diagram of a model in which an angle of repose is formed by the angle measurement method. Referring to Fig. 4, the apex of the powder 10 deposited in the mountain shape (triangular shape) shown in Figs. 2 and 3 is detected. Then, the angle of repose θ1 is calculated from the positions of the apex and base of the triangular powder 10. The ridgeline average mode is used to calculate the angle of repose θ1. The angle of repose θ1 is given by
[0030]
[0031] The unit of θ1 is degrees. Note that Atan in formula (1) indicates the inverse function of tangent (tan). More specifically, the angles θ2 and θ3 of the slope of the powder 10 relative to the horizontal direction in FIG. 4 are calculated using
[0032]
[0033]
[0034] From equation (1), the angle of repose θ1 can be calculated as the average value of angles θ2 and θ3 in FIG. 4. X1 and X2 are the horizontal distances between vertices 49A and 49B, which intersect with base 48 of triangular powder 10 shown in FIG. 4, and vertex 49C at the top. The same calculation is performed multiple times (for example, three times), and the average of the obtained measurements is taken as the angle of repose θ1. Note that if the inclination angle of the peaks of powder 10 varies depending on the location (for example, if the ridgeline of the peaks is curved rather than straight), the angle of repose is taken as the angle of repose at the lowest point in the height direction.
[0035] The moisture concentration of powder 10 is measured as follows. The moisture concentration of powder 10 can be measured by coulometric titration using, for example, a moisture measuring device CA-310. Specifically, the moisture concentration of powder 10 is determined by measuring the amount of vaporized gas generated by heating at 150°C based on the Karl Fischer method (JIS K-0068 moisture vaporization method).
[0036] The mixing ratio of the alumina powder 10D to the entire powder 10 is measured as follows. The mixing ratio of the alumina powder 10D is measured, for example, using a multi-type inductively coupled plasma optical emission spectrometry (ICP-OES). Specifically, the mixing ratio of the alumina powder 10D is calculated by inductively coupled plasma optical emission spectrometry. That is, approximately 0.1 g of the powder 10 containing the aluminum powder 10A and the alumina powder 10D is added to 20 mL of liquid hydrochloric acid. The aluminum powder 10A is dissolved in the hydrochloric acid by heating. At this time, the alumina powder 10D does not dissolve in the hydrochloric acid. The alumina powder 10D is separated from the hydrochloric acid solution by filtration. The filtered solution is adjusted to a constant volume of 100 mL. The filtered solution is diluted 50 times. Next, the quantitative value X (mg / L) of the aluminum powder 10A dissolved in the filtered solution is measured by ICP optical emission spectrometry. From the measured quantitative value X, the ratio of aluminum powder 10A in powder 10 is calculated as follows:
[0037]
[0038] The unit of the numerical value R1 obtained by the formula (4) is %. The content ratio of the alumina powder 10D in the powder 10 is calculated by subtracting the content ratio of the aluminum powder 10A obtained by the formula (4) from 100%.
[0039] <Operations and Effects> Here, the problems to be solved will be explained again with reference to the drawings, and the operations and effects of this embodiment will be explained.
[0040] Fig. 5 is a schematic diagram showing a state in which a large amount of moisture adheres to the periphery of aluminum powder particles. Referring to Fig. 5, consider a case in which powder 10 includes aluminum powder particles 10A. Note that an oxide film 10B may already be formed on the surface of each aluminum powder particle 10A during production. When oxide film 10B is formed, water molecules 10C, which represent moisture contained in powder 10, adhere to oxide film 10B.
[0041] The oxide film 10B is aluminum oxide (Al) that is naturally formed on the surface of the aluminum powder 10A when the aluminum powder 10A combines with oxygen in the atmosphere. 2 O 3 ) film. In other words, the oxide film 10B is made of the same material as alumina. The oxide film 10B is very thin. The oxide film 10B is separate from the alumina powder that may be contained in the powder 10. Therefore, the content of the alumina powder contained in the powder 10 does not include the oxide film 10B. However, the oxide film 10B is included in the total mass of the powder 10.
[0042] FIG. 6 is a schematic diagram showing the agglomerated state of the aluminum powder of FIG. 5 . When a large number of water molecules 10C adhere to one aluminum powder 10A (or to its oxide film 10B on its surface), the water molecules 10C adhere to the adjacent aluminum powder 10A (or to its oxide film 10B on its surface), resulting in the state shown in FIG. 6 . Referring to FIG. 6 , the water molecules 10C adhering to the aluminum powders 10A (or to their oxide films 10B on their surfaces) adhere to each other, causing the aluminum powders to gather together and agglomerate. This results in a powder size that is substantially larger than when the aluminum powders 10A are not agglomerated. This is because the aluminum powders 10A are clumped together. This can cause the agglomerated aluminum powder 10A to stagnate in the piping and result in variations in the thickness of the deposited film. Furthermore, variations in the thickness of the deposited film can occur between multiple lots of powder 10 with different moisture concentrations and different degrees of agglomeration.
[0043] FIG. 7 is a schematic diagram showing an ideal state of aluminum powder. Referring to FIG. 7, in the ideal state, the amount of water molecules 10C on the aluminum powder particles 10A (or on the oxide film 10B on the surface thereof) is smaller than in FIGS. 5 and 6 . This state can be achieved by removing as many water molecules 10C as possible, for example, by evaporation due to heating. Removing as many water molecules 10C as possible on the aluminum powder particles 10A (or on the oxide film 10B on the surface thereof) minimizes the amount of moisture on the surface of each aluminum powder particle 10A. This makes the aluminum powder particles 10A less likely to aggregate. This reduces the variation in the effective size of each aluminum powder particle 10A. As a result, the thickness of the film formed by the powder 10 is stable. To achieve the ideal state shown in FIG. 7, the powder 10 for the thermal spray material of this embodiment has a moisture concentration of 100 mg / kg or less and an angle of repose of 35° or less.
[0044] Furthermore, the powder 10 is brought into the ideal state shown in FIG. 7 (water content concentration of 100 mg / kg or less, angle of repose of 35° or less). This improves the fluidity of the powder 10. As a result, the variation in water content concentration and cohesion between multiple different lots of powder 10 can be reduced. In other words, multiple different lots of powder 10 all have similarly low surface water content concentrations and little cohesion. This reduces the variation in the effective size of multiple different lots of powder 10. As a result, the variation in the thickness of deposited film and the like between multiple different lots of powder 10 is reduced, improving the reproducibility of the thickness of deposited film and the like between different lots.
[0045] The powder 10 of this embodiment may have a particle diameter of 10 μm or less. By making the particle diameter finer in this way, the powder 10 can be made denser, thereby improving the quality of the film formed by thermal spraying. However, if the particle diameter of the powder 10 is large (10 μm or more), the powder 10 is less likely to agglomerate.
[0046] The powder 10 of this embodiment preferably includes aluminum powder 10A. This increases the electrical conductivity of the film formed by thermal spraying. Thermal spraying is characterized by its ability to form thick films. Aluminum is soft, making it easy to apply films. Aluminum is a material suitable for forming films by thermal spraying.
[0047] However, similarly to the above, this embodiment can be applied to materials other than aluminum, for which the variation in film formation during thermal spraying can be improved by removing as many water molecules 10C (see FIGS. 5 to 7) as possible.
[0048] Referring again to FIG. 6 , the powder 10 of this embodiment may further include an alumina powder. In this case, alumina powder 10D is included in the powder 10 in addition to aluminum powder 10A. The inclusion of alumina powder 10D improves the fluidity and cohesiveness of the powder 10. In other words, the alumina powder 10D makes the powder 10 less susceptible to cohesion due to the adhesion of water molecules 10C. This is because the alumina powder 10D mixed with the powder 10 makes it easier for the alumina powder 10D to separate water molecules adhering to the surface of the aluminum powder 10A. Furthermore, the inclusion of alumina powder 10D in the powder 10 improves the quality of the film formed by thermal spraying.
[0049] The particle size (average particle size) of the alumina powder 10D contained in the powder 10 is preferably about twice the particle size (average particle size) of the aluminum powder 10A contained in the powder 10. More specifically, the particle size (average particle size) of the alumina powder 10D contained in the powder 10 is preferably 1.7 to 2.3 times the particle size (average particle size) of the aluminum powder 10A contained in the powder 10. In particular, the particle size of the alumina powder 10D is more preferably 1.8 to 2.2 times the particle size of the aluminum powder 10A.
[0050] In the powder 10 of the present embodiment, the alumina powder content is preferably 20% by weight or more and 60% by weight or less, which provides both the effect of maintaining high coating efficiency by thermal spraying and the effect of improving cohesion.
[0051] The basis for the above-mentioned effects will be described in detail in the following examples. <Reference Photographs> Figure 8 is a photograph showing the appearance of aluminum powders from different lots. Referring to Figure 8, although A5080 and A5081 are both aluminum powders, the different lot numbers result in different cohesion and different appearances.
[0052] 9 is a photograph showing the appearance of aluminum powder and a mixed powder of aluminum powder and alumina powder. Referring to FIG. 9, the photograph on the left consists of only aluminum powder, while the photograph on the right contains 70% by weight of aluminum powder and 30% by weight of alumina powder. By including alumina powder in the aluminum powder, the appearance differs from that of a powder that does not contain alumina powder. By including alumina powder, there is less powder aggregation compared to aluminum powder that does not contain alumina powder.
[0053] As a means of removing water molecules 10C (FIGS. 5 to 7), the powder was heated to evaporate the water. The thickness of the film formed by thermal spraying was compared between heated and unheated powders. FIG. 10 is a graph showing the thickness of the film formed by thermal spraying for each lot of powder containing a mixture of aluminum powder and alumina powder, with and without heat treatment. Referring to FIG. 10, five lots of mixed powder of aluminum powder and alumina powder were prepared. For each lot, the thickness of the film formed after thermal spraying was compared between those that were heat treated (where the water was reduced by evaporation) and those that were not heat treated.
[0054] The horizontal axis of the graph in FIG. 10 indicates the powder lot (lot number is written in the graph). The respective lot numbers are A3080, 15066, AZ036, AZ037, and 16003. The vertical axis of the graph in FIG. 10 indicates the average thickness of the film obtained by thermal spraying each lot of powder. In FIG. 10, film thickness data for 1,600 samples was obtained for each condition (each lot), and the average value is shown. As shown in FIG. 10, the film sprayed using powder without heat treatment has a large variation in thickness. In contrast, the film sprayed using heat-treated powder has a smaller variation in thickness than the film formed using unheated powder. Table 1 below is provided for a more detailed discussion of the results in FIG. 10.
[0055]
[0056] As shown in Table 1, when five types of powder lots without heat treatment were used, the film thickness variation was 17.0%. In contrast, when five types of powder lots with heat treatment were used, the film thickness variation was reduced to 5.3%. This shows that heat treatment of the powder can suppress the variation in film formation. This is thought to be because water molecules adhering to the surface of the aluminum powder are more easily removed from heat-treated powder than from powder without heat treatment. The removal of water molecules from heat-treated powder improves film formation efficiency compared to powder without heat treatment, and therefore the average film thickness of heat-treated powder is thought to be thicker than the average film thickness of powder without heat treatment.
[0057] The film thickness variation here is the value obtained by dividing the standard deviation of the average film thickness (shown in FIG. 10 ) of each lot under each heat treatment condition by the average film thickness (shown in Table 1 ) under each heat treatment condition, and multiplying the result by 100.
[0058] As described above, by reducing the moisture concentration through heating, the aggregation of the powder is reduced, and as a result, the thickness of the film formed by the powder is stabilized.
[0059] The change in the fluidity of powder 10 was investigated by adjusting the amount of moisture on the surface of aluminum powder 10A (see Figures 5 to 7) that constitutes powder 10. Figure 11 is a graph showing the change in the amount of moisture contained in the powder and the angle of repose of the powder depending on the heating time of the powder. Referring to Figure 11, the data is for a powder in which 70% by weight of aluminum powder is mixed with 30% by weight of alumina powder. The horizontal axis of the graph in Figure 11 represents the heating time of the mixed powder. Heating time 2 is longer than heating time 1, and heating time 3 is longer than heating time 2. The vertical axis of the graph in Figure 11 represents the amount of moisture indicated by the bar graph and the angle of repose indicated by the plotted data. The heating temperature of the powder at this time was 190°C.
[0060] The moisture content (moisture concentration) of the unheated mixed powder was 320 ppm (320 mg / kg). In contrast, the moisture contents of the powders heated for heating times 1, 2, and 3 were 81 ppm, 53 ppm, and 33 ppm, respectively. This indicates that the moisture content of the powder decreased as the heating time increased.
[0061] The angle of repose of the unheated mixed powder was approximately 48°. In contrast, the angles of repose of the powders heated for heating times 1, 2, and 3 were approximately 40°, 35°, and 35°, respectively. This shows that the angle of repose of the powder decreased as the heating time increased. In other words, the flowability of the powder improved as the heating time increased.
[0062] FIG. 12 is a photograph showing the appearance of the mixed powder from which the data in FIG. 11 was obtained, both before and after heating. That is, FIG. 12 shows a powder in which 70% by weight of aluminum powder is mixed with 30% by weight of alumina powder. Referring to FIG. 12, "before heating" corresponds to the "unheated" point in FIG. 11, and "after heating" corresponds to the "heating time 3" point in FIG. 11. It can be visually confirmed from FIG. 12 that the amount of agglomerated powder is reduced when the angle of repose of the powder is reduced to 35° or less by heating. This improves the flowability of powder 10.
[0063] The relationship between the improvement in the fluidity of the powder 10 in Example 2 and the change in the variation in film thickness (coating reproducibility) during thermal spraying using the powder 10 was investigated. FIG. 13 is a schematic diagram showing a plan view of a coating formed on a substrate. Note that a plan view means a view from directly above. Referring to FIG. 13, during thermal spraying using the coating deposition apparatus 100, the powder 10 adheres to the surface of the substrate 20 to form a coating. Here, the through holes 1a have a linear planar shape (a shape elongated in the left-right direction in the figure) in a plan view.
[0064] Nozzle 2b (see Figure 1) with an opening diameter of 5 mm sprays powder 10 while moving from one end to the other along the extension direction of through-hole 1a, which has a linear shape in a plan view. This results in the formation of a thin film 21 having a linear shape as shown in Figure 13. The dimensions of thin film 21 were approximately 40 mm in the horizontal direction (length direction) and approximately 5 mm in the vertical direction (width direction).
[0065] Figure 14 is a hatched color map showing the planar shape of a thin film formed by thermal spraying using powder without heat treatment. Figure 15 is a hatched color map showing the planar shape of a thin film formed by thermal spraying using powder with heat treatment. The powder used in Figure 15 was heated for only "Heating Time 1" in Example 2. Referring to Figures 14 and 15, the planar shape of the thin film 21 in Figure 13 formed using powder 10 under different conditions indicates that the denser the hatching in the figure, the thicker the area. Both Figures 14 and 15 show thin films formed from a mixed powder containing 70 wt% aluminum powder and 30 wt% alumina powder. The moisture concentration of the powder in Figure 14 was approximately 300 ppm, and that of the powder in Figure 15 was approximately 80 ppm. Overall, each thin film is thicker in the center in the longitudinal direction (width direction) and thinner at both ends in the width direction.
[0066] In Figure 14, the thickness of the linear thin film varies in region A enclosed by an ellipse (the region enclosed by an ellipse on the left side of the figure). That is, part of the thickest region in the center is extremely thick, and the slightly thinner regions around it form chaotic waves in the left-right direction of the figure. That is, the thickness of the deposited film varies between regions. In contrast, in Figure 15, the thickness of the thickest region in the center is almost constant overall, and the slightly thinner regions around it extend in an almost linear fashion. That is, the thickness of the deposited film is stable between regions. It was observed that if the moisture contained in the powder is removed by, for example, 60% or more of the amount before heating, and the flowability of the powder is improved, the variation in the thickness of the deposited film tends to improve.
[0067] In relation to Example 1, the relationship between the heating time of the powder and the "film thickness variation" described in Example 1 was investigated in more detail. Figure 16 is a graph showing the relationship between the heating time of the powder and the film thickness variation of the film formed by thermal spraying of the powder. Referring to Figure 16, the horizontal axis of the graph shows powder samples 1 to 4. The vertical axis of the graph shows the film thickness variation of the film formed by thermal spraying of each sample.
[0068] As shown in Fig. 16, sample 1 was not heat treated. Samples 2 to 4 were heat treated at 190°C. The heating times for samples 2, 3, and 4 were 4.5 hours, 7.0 hours, and 9.5 hours, respectively.
[0069] To stabilize the film thickness, the goal is to keep film thickness variation to 10% or less. Samples 2 to 4 all meet this goal. Specifically, the film thickness variation was 12.5% for Sample 1, 7.8% for Sample 2, 6.2% for Sample 3, and 4.9% for Sample 4.
[0070] Figure 17 is a hatched color map of the coating formed by thermal spraying for each sample shown in Figure 16. Referring to Figure 17, Sample 1, which was not heat-treated, exhibits large variations in coating thickness. This can be seen from the hatched color map, which contains a random region A (circled on the left side of the figure) where the coating thickness is locally large. On the other hand, Samples 2 to 4 do not have such regions, and the overall coating thickness is approximately constant.
[0071] 16 and 17, it was found that heating at 190° C. for 4.5 hours or more reduced the moisture concentration of the powder and reduced the film thickness fluctuation during film formation.
[0072] In relation to Examples 2 and 4, the basis for the fact that the angle of repose is preferably 35° or less and the moisture concentration is preferably 100 mg / kg (100 ppm) or less in powder 10 of the present embodiment will be explained in this Example. FIG. 18 is a graph showing the relationship between the heating time of the powder and the moisture content and angle of repose. Referring to FIG. 18, Samples 1 to 4 on the horizontal axis are the same as Samples 1 to 4 in Example 4 (FIGS. 16 and 17). The vertical axis shows the moisture content and angle of repose, as in FIG. 11 of Example 2.
[0073] As shown in Figure 18, Samples 2 to 4, which reduce their moisture content upon heating and enable stable film formation, all have low angles of repose. The angles of repose for Samples 2 to 4 are 35° or less. Specifically, Sample 2 is 33.7°, Sample 3 is 33.5°, and Sample 4 is 34.4°. However, simply having an angle of repose of 35° or less leaves a significant amount of agglomerated powder remaining in the powder. On the other hand, if the angle of repose is 35° or less and the moisture content is 100 mg / kg (100 ppm) or less, agglomerated powder in the powder is almost completely eliminated. Specifically, Sample 2 is 100 ppm, Sample 3 is 90 ppm, and Sample 4 is 98 ppm. This leads to improved film thickness variation, as described in Example 4. Sample 1 has an angle of repose of 40.6° and a moisture content of 314 ppm.
[0074] Figure 19 is a graph showing the relationship between the weight percent ratio of alumina powder in a powder and the angle of repose and deposition efficiency of the powder. Referring to Figure 19, the horizontal axis of the graph shows the mixing ratio of alumina powder in weight percent. The solid broken line of the graph shows the angle of repose, and the dotted broken line of the graph shows the deposition efficiency to the substrate, i.e., the coating efficiency, in units of %, when a coating is formed by thermal spraying the powder. Note that, as in the other examples, the powder used was a mixed powder containing aluminum powder in addition to alumina powder.
[0075] As shown in Figure 19, investigations were carried out on samples with alumina powder mixing ratios of 10 wt%, 30 wt%, 50 wt%, 70 wt%, and 90 wt%. Figure 19 shows that as the alumina powder mixing ratio increases, the angle of repose decreases, and the adhesion efficiency also decreases.
[0076] From the viewpoint of preventing a decrease in film formation efficiency, the adhesion efficiency is preferably 5.0% or more. Furthermore, from the viewpoint of ensuring fluidity, the angle of repose is preferably 41° or less. If the angle of repose exceeds 41°, the fluidity decreases, making the supply of the powder to the film formation target (substrate 20, etc.) unstable. From the above and the results of Figure 19, it is preferable that the mixing ratio of alumina powder be 20% by weight or more and 60% by weight or less.
[0077] Note that Figure 19 shows the test results for powder that was not heated. Figure 20 is a graph showing the difference in angle of repose between heated and unheated mixed powders of aluminum and alumina. Referring to Figure 20, the angle of repose of the unheated mixed powder of aluminum and alumina was 40.6°, while heating it for 7.0 hours increased the angle of repose to 33.3°. Although not shown, the moisture content of the unheated powder was 258.4 ppm, and the moisture content of the powder heated for 7.0 hours was 69.4 ppm. From this, it can be seen that if the powder used in the test shown in Figure 19 were heated, the angle of repose would be 35° or less.
[0078] FIG. 21 is a graph showing the difference in deposition efficiency between heated and unheated mixed powders of aluminum and alumina. The graph in FIG. 21 shows a case where the weight percent ratio of alumina powder was 30 wt %. Referring to FIG. 21, the deposition efficiency without heating was 6.1%, while the deposition efficiency after heating for 7.0 hours was 5.5%. In other words, there was almost no difference between the two, and both were above the desirable deposition efficiency standard value. Therefore, the deposition efficiency results were almost the same when the powder in FIG. 19 was heated. Therefore, even when heated mixed powder is used, it can be inferred that the deposition efficiency will be 5.0% or higher when the alumina powder mixing ratio is 20 wt % or more and 60 wt % or less, just like when the mixed powder is not heated as in FIG. 19.
[0079] 19, even when the angle of repose is 35° or less and the moisture concentration is 100 mg / kg or less, it is preferable that the mixing ratio of alumina powder is 20% by weight or more and 60% by weight or less. Among these, the mixing ratio of alumina powder is more preferably 30% by weight or more and 50% by weight or less.
[0080] The embodiments disclosed herein should be considered to be illustrative in all respects and not restrictive. Unless there is a contradiction, at least two of the features disclosed herein may be combined.
[0081] 1 Mask jig, 1a Through hole, 2 Spray gun, 2a Spray gun main body, 2b Nozzle, 2c Heater, 3 Powder supply unit, 4 Gas supply unit, 5, 6 Piping, 7 Valve, 8 Pressure sensor, 9 Temperature sensor, 10 Powder, 10A Aluminum powder, 10B Oxide film, 10C Water molecules, 10D Alumina powder, 20 Substrate, 21 Thin film, 30, 31, 32 Arrow, 41 Sieve, 42 Funnel, 43 Base, 44 Camera, 45 LED light source, 46 Light, 47 Shadow, 100 Film formation apparatus.
Claims
1. A powder for thermal spraying having an angle of repose of 35° or less and a moisture concentration of 100 mg / kg or less.
2. The thermal spray powder according to claim 1, having a particle size of 10 μm or less.
3. The thermal spray powder according to claim 1 or 2, comprising aluminum powder.
4. The thermal spray powder according to claim 3, further comprising an alumina powder.
5. The thermal spray powder according to claim 4, wherein the content of the alumina powder is 20% by weight or more and 60% by weight or less.
Citation Information
Patent Citations
Three-dimensional modeling apparatus
JP2018126974A
Additive manufacturing powder and additive manufacturing part made using same
US20210260650A1
Formation material and formation method which are used for forming structure
WO2015199244A1
Material for cold spraying
WO2020090528A1