Support plate and method for manufacturing support plate
The support plate with a regionally varying coating layer of metal carbides and metalloid carbides addresses the issue of side reactions and durability in cermet cutting tool manufacturing, ensuring high-quality and stable cutting tools by reducing adhesion and peeling, and enhancing thermal resistance.
Patent Information
- Application Number
- PCT/JP2024/009448
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-11
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional support plates used in the firing process for cermet cutting tool manufacturing often cause side reactions with the molded bodies, leading to quality deterioration and reduced durability due to the susceptibility of titanium carbide to impact and temperature changes.
A support plate with a coating layer comprising metal carbides and metalloid carbides, where the content ratio of these materials varies by region to enhance durability and reduce adhesion, featuring a higher content ratio in the outer surface region for improved resistance to impact and temperature changes, and a higher content ratio in the inner surface region to minimize thermal expansion differences.
The solution effectively reduces side reactions, maintains the quality of the cutting tool, and enhances the durability of the coating layer, preventing peeling and adhesion issues, thereby ensuring stable and high-quality cutting tool manufacturing.
Smart Images

Figure JP2024009448_03102024_PF_FP_ABST
Abstract
Description
Support plate and method for manufacturing the same
[0001] SUMMARY OF THE INVENTION The disclosed embodiments relate to a support plate and a method for manufacturing the support plate.
[0002] A conventional technique for manufacturing a cermet cutting tool is known (see, for example, Patent Document 1), in which a metal carbide powder, a cobalt powder, and a nickel powder are crushed, mixed, and molded, and the molded body is fired. A support plate called a setter is used during firing of the molded body (see, for example, Patent Document 2).
[0003] JP 2016-052696 A JP 2005-219943 A
[0004] A support plate according to one aspect of the embodiment includes a base and a coating layer. The base has a first surface and a second surface opposite to the first surface. The coating layer is located on at least one of the first surface and the second surface of the base. The coating layer includes at least one of a metal carbide and a metalloid carbide. The coating layer has a central region and an outer surface region. The central region includes the center of the coating layer in the thickness direction. The outer surface region includes an end portion of the coating layer on the surface side. The mass % content of the metal carbide and the metalloid carbide in the outer surface region is greater than the mass % content of the metal carbide and the metalloid carbide in the central region.
[0005] FIG. 1 is a perspective view showing an example of the configuration of a support plate according to an embodiment. FIG. 2 is a cross-sectional view showing an example of the configuration of a support plate according to an embodiment. FIG. 3 is an enlarged view of the vicinity of the coating layer in the support plate shown in FIG. 2. FIG. 4 is a cross-sectional view showing an example of the configuration of a support plate according to another embodiment. FIG. 5 is a graph showing the change in the size of the inscribed circle in a cutting tool fired with the support plate of the example. FIG. 6 is a graph showing the change in the size of the inscribed circle in a cutting tool fired with the support plate of Reference Example 3. FIG. 7 is a graph showing the results of XPS analysis of the coating layer surface in the support plates of the example, Reference Example 1, and Reference Example 2. FIG. 8 is a SEM image showing an example of the crystalline structure of the upper surface of a fired body fired with the support plate of the example. FIG. 9 is a SEM image showing an example of the crystalline structure of the lower surface of a fired body fired with the support plate of the example. FIG. 10 is a SEM image showing an example of the crystalline structure of the upper surface of a fired body fired with the support plate of Reference Example 3. FIG. 11 is a view showing an SEM image showing an example of the crystal structure on the lower surface side of the sintered body sintered using the support plate of Reference Example 3.
[0006] Hereinafter, embodiments of the support plate and the method for manufacturing the support plate disclosed in the present application will be described. Note that the present disclosure is not limited to the embodiments described below.
[0007] In the prior art described in Patent Document 1, a side reaction may occur between the compact and the support plate on which the compact is placed during the firing process in a high-temperature environment. This may result in a deterioration in the quality of the cutting tool. In addition, in the prior art described in Patent Document 2, a coating layer is formed by thermally spraying a powdered material containing titanium carbide as the main component.
[0008] In order to reduce side reactions between the compact and the support plate on which it is placed, it is necessary to increase the titanium carbide content in the coating layer. However, it has been found that simply increasing the titanium carbide content in the coating layer reduces the durability of the coating layer. This is thought to be because titanium carbide is vulnerable to impacts and sudden temperature changes, and repeated use in firing processes under high-temperature environments rapidly deteriorates the coating layer.
[0009] Therefore, there is a need for a technology that can solve the above problems, provide a support plate with good durability, and maintain the quality of the supported object.
[0010] 1 is a perspective view showing an example of the configuration of a support plate 1 according to an embodiment. As shown in FIG. 1, the support plate 1 is, for example, in the form of a flat plate. A plurality of molded bodies M to be molded into a predetermined shape in a cutting tool manufacturing process are supported on a main surface of the support plate 1.
[0011] Furthermore, the plurality of compacts M are placed in a firing furnace together with the support plate 1, and are fired. As a result, a fired body (i.e., a cutting tool) is formed from the compacts M.
[0012] Although Figure 1 shows an example in which the support plate 1 is configured in a flat plate shape, the present disclosure is not limited to such an example, and any shape is acceptable as long as a mounting surface is formed on which the molded body M can be placed.
[0013] Furthermore, although Figure 1 shows an example in which a chip-shaped molded body M is placed on the support plate 1, the present disclosure is not limited to such an example, and molded bodies of various shapes, such as drill-shaped or tap-shaped, may be placed on the support plate 1.
[0014] Fig. 2 is a cross-sectional view showing an example of the configuration of the support plate 1 according to the embodiment. As shown in Fig. 2, the support plate 1 according to the embodiment has a base 2 and a coating layer 3. The base 2 has substantially the same shape as the support plate 1, for example, a flat plate shape.
[0015] The base 2 has a first surface 2 a and a second surface 2 b. The second surface 2 b is located on the opposite side of the first surface 2 a. For example, the first surface 2 a is one of the main surfaces of the base 2, and the second surface 2 b is the other main surface of the base 2.
[0016] The coating layer 3 is located on at least one of the first surface 2a and the second surface 2b of the base 2. In the example of Fig. 2, the coating layer 3 is located on both the first surface 2a and the second surface 2b of the base 2. In the present disclosure, the coating layer 3 may cover the entire first surface 2a or the second surface 2b, or the coating layer 3 may cover only a part of the first surface 2a or the second surface 2b.
[0017] In the embodiment, the coating layer 3 may contain at least one of a metal carbide and a metalloid carbide. This reduces the amount of foreign matter adhering to the sintered body (i.e., the cutting tool) after sintering, compared to a case in which a metal carbide powder is spread on the main surface of the base 2, and then the molded body M (see FIG. 1 ) is placed on the support plate 1 and sintered.
[0018] The metal component constituting the metal carbide is not limited to a specific element. Examples of the metal component include titanium, nickel, cobalt, tungsten, and niobium. In particular, when the coating layer 3 contains a carbide of one of these metal components commonly used as a material for cermets, side reactions such as diffusion of the metal component from the compact to the support plate 1 are likely to be reduced, and deterioration of the coating layer 3 is less likely to progress.
[0019] The metalloid component constituting the metalloid carbide is not limited to a specific element. For example, the metalloid component may be boron, silicon, arsenic, tellurium, germanium, or antimony. Of these materials, silicon is relatively inexpensive. Therefore, when silicon is used as the metalloid component, the support plate 1 can be produced at low cost.
[0020] As shown in Figure 3, the coating layer 3 is divided into three regions along the thickness direction. First, the middle region including the center of the coating layer 3 in the thickness direction is referred to as the central region 3a. Next, the region located closer to the substrate 2 than the central region 3a is referred to as the inner surface region 3c. Finally, the region located farther from the substrate 2 than the central region 3a is referred to as the outer surface region 3b. The inner surface region 3c includes the end of the coating layer 3 that comes into contact with the substrate 2. In other words, the inner surface region 3c includes the inner surface of the coating layer 3. The outer surface region 3b includes the end of the coating layer 3 that is on the outer surface side. In other words, the outer surface region 3b includes the outer surface of the coating layer 3.
[0021] The thicknesses of the central region 3 a, the inner surface region 3 c, and the outer surface region 3 b are not limited to any particular value. In this embodiment, the thicknesses of the central region 3 a, the inner surface region 3 c, and the outer surface region 3 b are set to the same value. That is, the coating layer 3 is divided into three regions of the same thickness, and these regions are the central region 3 a, the inner surface region 3 c, and the outer surface region 3 b.
[0022] Here, the mass % content ratio of the metal carbide and metalloid carbide contained in the coating layer 3 is designated MA, the mass % content ratio of the metal carbide and metalloid carbide in the central region 3 a is designated M1, the mass % content ratio of the metal carbide and metalloid carbide in the outer surface region 3 b is designated M2, and the mass % content ratio of the metal carbide and metalloid carbide in the outer surface region 3 b is designated M3. Note that when the coating layer 3 contains a metal carbide and a metalloid carbide, the mass % content ratio of the metal carbide and the metalloid carbide is the sum of the mass % content ratio of the metal carbide and the mass % content ratio of the metal carbide.
[0023] In the coating layer 3 according to the embodiment, the content ratio M2 in the outer surface region 3b may be greater than the content ratio M1 in the central region 3a. That is, the content ratio MA in the coating layer 3 is not simply a large value. When the content ratio M1 in the central region 3a is a relatively small value, the resistance of the coating layer 3 to impacts and temperature changes is improved, and the durability of the coating layer 3 can be improved. Furthermore, when the content ratio M2 in the outer surface region 3b is a relatively large value, the adhesion of foreign matter to the baked cutting tool can be reduced.
[0024] Therefore, according to the embodiment, the quality of the sintered body is well maintained, and a high-quality cutting tool can be manufactured.
[0025] The carbon content ratio M3 in the inner surface region 3 c may be greater than the carbon content ratio M1 in the central region 3 a. By making the carbon content ratio M3 in the inner surface region 3 c greater than the carbon content ratio M1 in the central region 3 a, in other words, by keeping the carbon content ratio M1 in the central region 3 a small, the difference in thermal expansion coefficient with the base 2 can be kept small, making it less likely for peeling of the coating layer 3 to occur. Furthermore, by making the carbon content ratio M3 in the inner surface region 3 c a relatively large value, carbon diffusion from the base 2 is likely to be reduced.
[0026] In addition, when both the content ratio M2 in the outer surface region 3b and the content ratio M3 in the inner surface region 3c are greater than the content ratio M1 in the central region 3a, the difference in thermal expansion between the outer surface region 3b and the inner surface region 3c is easily suppressed. As a result, warping due to the difference in thermal expansion is less likely to occur in the coating layer 3, and the coating layer 3 is less likely to peel off. From this perspective, the ratio of the content ratio M2 to the content ratio M3, (content ratio M2) / (content ratio M3), is preferably about 0.8 to 1.2.
[0027] On the other hand, the content ratio M2 in the outer surface region 3 b may be greater than the content ratio M3 in the inner surface region 3 c, which can suppress coating peeling and reduce adhesion of foreign matter to the baked cutting tool.
[0028] The content ratio M1 in the central region 3a, the content ratio M2 in the outer surface region 3b, and the content ratio M3 in the inner surface region 3c are not limited to any particular value. For example, the content ratio M1 may be 60% to 97% by weight. The content ratios M2 and M3 may each be 85% to 100% by weight.
[0029] When the content ratio M2 is greater than the content ratio M1, the ratio (M1 / M2) may be 0.6 to 0.95. When the ratio M1 / M2 is 0.6 or greater, the difference in thermal expansion between the central region 3a and the outer surface region 3b is prevented from becoming excessively large. As a result, cracks are less likely to occur inside the coating layer 3. When the ratio M1 / M2 is 0.95 or less, the effect of improving the durability of the coating layer 3 by the central region 3a and the effect of reducing adhesion of foreign matter to the cutting tool by the outer surface region 3b can be satisfactorily achieved.
[0030] When the content ratio M3 is greater than the content ratio M1, the ratio (M1 / M3) may be 0.6 to 0.95. When the ratio M1 / M3 is 0.6 or greater, the difference in thermal expansion between the central region 3a and the inner surface region 3c can be prevented from becoming excessively large. As a result, cracks are less likely to occur inside the coating layer 3. Furthermore, when the ratio M1 / M3 is 0.95 or less, it is possible to satisfactorily achieve both the effect of improving the durability of the coating layer 3 by the central region 3a and the effect of reducing carbon diffusion from the substrate 2 by the inner surface region 3c.
[0031] In the embodiment, the coating layer 3 may contain at least one of titanium carbide (TiC) and silicon carbide (SiC), which can reduce adhesion of the sintered body after the sintering treatment to the support plate 1. Therefore, according to the embodiment, cutting tools can be stably manufactured.
[0032] In the present disclosure, coating layer 3 is not limited to containing at least one of titanium carbide and silicon carbide, and may contain, for example, tungsten carbide (WC) or niobium carbide (NbC).
[0033] In the embodiment, when the surface of the coating layer 3 (i.e., the surface of the outer surface region 3b) is analyzed by XPS (X-ray Photoelectron Spectroscopy), the TiC value and TiO value obtained from the observed peaks are 2 TiO calculated from the value 2 The ratio may be 0.2 or less.
[0034] Here, the TiC value is the value of TiP in the XPS spectrum of the surface of the coating layer 3. 3/2 is the maximum value of the emitted electron intensity per unit time at the peak in the range of 454 eV to 456 eV corresponding to
[0035] Also, TiO 2 The value is the value of Ti2P in the XPS spectrum of the surface of the coating layer 3. 3/2 is the maximum value of the emitted electron intensity per unit time at the peak in the range of 457 eV to 459 eV corresponding to
[0036] And TiO 2 The ratio is calculated from the following formula (1): TiO 2 Ratio=TiO 2 value / (TiO 2 value + TiC value) ... (1)
[0037] Thus, titanium oxide (TiO 2 By providing the coating layer 3 with a low content of titanium carbide and a high content of titanium carbide, it is possible to reduce adhesion of the sintered body to the support plate 1 after the sintering treatment. Therefore, according to the embodiment, cutting tools can be stably manufactured.
[0038] In this case, the TiC content in mass % in the outer surface region 3 b may be greater than the TiC content in mass % in the central region 3 a. A relatively large TiC content in mass % in the outer surface region 3 b can reduce adhesion of foreign matter to the baked cutting tool. Furthermore, a relatively small TiC content in mass % in the central region 3 a can improve the resistance of the coating layer 3 to impacts and temperature changes, thereby improving the durability of the coating layer 3.
[0039] In addition, TiO in the outer surface region 3b 2 The content ratio in mass % of TiO in the central region 3a is 2 In this case, the content ratio of TiC in mass % in the outer surface region 3b is likely to be increased.
[0040] The TiC content in mass% in the inner surface region 3c may be greater than the TiC content in mass% in the central region 3a. By making the TiC content in mass% in the inner surface region 3c greater than the TiC content in mass% in the central region 3a, in other words, by keeping the TiC content in mass% in the central region 3a small, the difference in thermal expansion coefficient with the base 2 can be kept small, making peeling of the coating layer 3 less likely to occur. Furthermore, by making the TiC content in mass% in the inner surface region 3c a relatively large value, carbon diffusion from the base 2 is likely to be reduced.
[0041] In addition, when both the TiC content ratio in mass% in the outer surface region 3b and the TiC content ratio in mass% in the inner surface region 3c are greater than the TiC content ratio in mass% in the central region 3a, the difference in thermal expansion between the outer surface region 3b and the inner surface region 3c is easily suppressed. As a result, warping due to the difference in thermal expansion is less likely to occur in the coating layer 3, and the coating layer 3 is less likely to peel off. From this perspective, it is desirable that the ratio of (TiC content ratio in mass% in the outer surface region 3b) / (TiC content ratio in mass% in the inner surface region 3c) be approximately 0.8 to 1.2.
[0042] TiO in the inner surface region 3c 2 The content ratio in mass % of TiO in the central region 3a is 2 In this case, the content ratio of TiC in mass % in the inner surface region 3c can be easily increased.
[0043] The TiC content in mass % in the outer surface region 3 b may be greater than the TiC content in mass % in the inner surface region 3 c, which can reduce the adhesion of foreign matter to the baked cutting tool while suppressing coating peeling.
[0044] In the embodiment, the base 2 may be mainly composed of carbon. For example, the base 2 may be made of graphite. This can reduce deterioration of the base 2 during firing of the compact M in a high-temperature environment. Therefore, according to the embodiment, cutting tools can be stably manufactured.
[0045] In the present disclosure, the substrate 2 is not limited to being made of graphite. For example, the substrate 2 may be made of silicon nitride (Si 3 N 4 ), silicon carbide or aluminum oxide (Al 2 O 3 In the present disclosure, the substrate 2 may be formed by disposing W (tungsten), Mo (molybdenum), or the like on the surface of a plate material formed of graphite.
[0046] In the embodiment, the purity of the metal carbide and metalloid carbide in the coating layer 3 may be 95% or more, and preferably 99% or more. By providing the coating layer 3 with a high content of metal carbide and metalloid carbide in this way, it is possible to reduce adhesion of the fired body to the support plate 1 after firing treatment.
[0047] Therefore, according to the embodiment, cutting tools can be manufactured stably.
[0048] In the embodiment, the thickness of the coating layer 3 may be 20 μm to 200 μm, and preferably 50 μm to 200 μm, which further reduces adhesion of the fired body to the support plate 1 after firing treatment and enables the support plate 1 to be manufactured in a short time.
[0049] In the embodiment, the surface roughness Sa of the coating layer 3 may be 10 μm to 50 μm, and preferably 20 μm to 30 μm. This further reduces adhesion of the sintered body to the support plate 1 after the sintering treatment. Therefore, according to the embodiment, cutting tools can be manufactured more stably.
[0050] In addition, in this embodiment, by increasing the surface roughness Sa of the coating layer 3 to a range of 10 μm to 50 μm, it is possible to promote the reaction with the carbon-containing gas in the manufacturing process of the support plate 1 described later.
[0051] In the embodiment described so far, the support plate 1 is shown supporting a plurality of molded bodies M that will be sintered to become cutting tools, but the present disclosure is not limited to such an example. Fig. 4 is a cross-sectional view showing an example of the configuration of the support plate 1 according to another embodiment.
[0052] 4, in another embodiment, the support plate 1 may be used to support a sample S such as a semiconductor wafer inside a semiconductor manufacturing apparatus 10. The semiconductor manufacturing apparatus 10 may be, for example, an apparatus that epitaxially grows a semiconductor crystal on the sample S by using a gas phase reaction, or may be, for example, an apparatus that grows a semiconductor crystal by using a metal organic chemical vapor deposition (MOCVD) method.
[0053] 4, semiconductor manufacturing apparatus 10 includes support plate 1, chamber 11, gas supply path 12, gas exhaust path 13, support columns 14, and heater 15. Support plate 1 is, for example, disk-shaped. Chamber 11 houses support plate 1, support columns 14, and heater 15.
[0054] The gas supply line 12 is connected between a gas supply unit (not shown) and the chamber 11, and supplies gas supplied from the gas supply unit to the inside of the chamber 11. The gas supplied via the gas supply line 12 is a gas that will be a material for the semiconductor to be grown on the sample S.
[0055] The gas exhaust path 13 is connected between a gas exhaust unit (not shown) and the chamber 11, and exhausts the atmosphere inside the chamber 11. The support pillars 14 are positioned to extend vertically and support the support plate 1 and the heater 15. The support plate 1 is supported, for example, at the upper end of the support pillars 14, and the heater 15 is supported, for example, by the support pillars 14 below the support plate 1.
[0056] The heater 15 heats the support plate 1 , thereby heating the sample S supported by the support plate 1 .
[0057] In another embodiment, a support plate 1 that supports a sample S in a semiconductor manufacturing apparatus 10 has a base 2 (see FIG. 2) and a coating layer 3 (see FIG. 2). The coating layer 3 is located on at least one of a first surface 2a (see FIG. 2) and a second surface 2b (see FIG. 2) of the base 2.
[0058] In another embodiment, the coating layer 3 may contain at least one of a metal carbide and a metalloid carbide. For example, in another embodiment, the coating layer 3 may contain silicon carbide.
[0059] This makes it possible to reduce adhesion of foreign matter to the sample S during the semiconductor manufacturing process in the semiconductor manufacturing apparatus 10. Therefore, according to another embodiment, the quality of the sample S is well maintained, and high-quality semiconductor devices can be manufactured.
[0060] In another embodiment of the coating layer 3, the content ratio M2 in the outer surface region 3 b may be greater than the content ratio M1 in the central region 3 a. This improves the resistance of the coating layer 3 to impacts and temperature changes, thereby improving the durability of the coating layer 3. Furthermore, the relatively large content ratio M2 in the outer surface region 3 b can reduce adhesion of foreign matter to the baked cutting tool.
[0061] Examples of the present disclosure will be specifically described below. Note that in the examples described below, a support plate using graphite as a substrate and having a coating layer containing titanium carbide as a metal carbide or semi-metal carbide is shown, but the present disclosure is not limited to the following examples.
[0062] Example: First, a flat substrate made of graphite was prepared. Next, titanium (Ti) was sprayed onto the surface of this substrate to form a sprayed layer containing titanium as the main component. The thickness of this sprayed layer was 50 μm. The spraying process was performed by atmospheric plasma spraying.
[0063] Next, the substrate on which the titanium-based thermal sprayed layer was formed was carried into a heating furnace, and the furnace was evacuated and heated to a temperature of 1400°C or higher while a carbon-containing gas was supplied into the furnace. In the examples, argon (Ar) and methane (CH 4 ) mixed gas was used.
[0064] As a result, carbon components originating from the carbon-containing gas were added to the surface side of the sprayed layer, and the sprayed layer was transformed into a coating layer containing titanium carbide. Note that, in this high-temperature heat treatment, carbon components originating from the graphite of the substrate were also added to the back side of the sprayed layer, so that the back side of the sprayed layer was also carbonized. In this way, the support plate of the example was obtained.
[0065] Reference Example 1 First, a flat substrate made of graphite was prepared. Next, titanium (Ti) was sprayed onto the surface of this substrate to form a sprayed layer containing titanium as the main component. The treatment conditions for this spraying treatment were the same as those in the above examples. In this way, a support plate of Reference Example 1 was obtained.
[0066] Reference Example 2 First, a flat substrate made of graphite was prepared. Next, titanium (Ti) was sprayed onto the surface of this substrate to form a sprayed layer mainly composed of titanium. The treatment conditions for this spraying treatment were the same as those in the above examples.
[0067] Next, the substrate on which the metal sprayed layer was formed was carried into a heating furnace, and the substrate was heated to a temperature of 1400° C. or higher while the inside of the heating furnace was evacuated to a vacuum.
[0068] As a result, oxygen atoms that had been mixed into the sprayed layer during the thermal spraying process were expelled, and carbon components originating from the graphite of the substrate were added from the back side of the sprayed layer, carbonizing a portion of the sprayed layer. In this way, a support plate of Reference Example 2 was obtained.
[0069] Reference Example 3 First, a flat substrate made of graphite was prepared. Next, titanium carbide powder was spread over the surface of this substrate. In this way, a support plate of Reference Example 3 was obtained.
[0070] <Various Evaluations> Next, using the support plates of the Examples and Reference Examples 1 to 3 obtained above, a sintering treatment was carried out on a molded body, which is carried out in the manufacturing process of a cermet cutting tool. Various properties of the sintered body were then evaluated to determine whether the sintering treatment was performed well depending on the support plate. A summary of the evaluation results is shown in Table 1.
[0071]
[0072] As shown in Table 1, after the firing treatment, no adhesion of the fired body was observed to the support plates of the Example and Reference Example 3, whereas adhesion of the fired body was observed to the support plates of Reference Examples 1 and 2.
[0073] Furthermore, as shown in Table 1, after the firing treatment, no reaction with the support plate was observed in the fired bodies in the Examples, whereas reactions with the support plate were observed in the fired bodies in Reference Examples 1 to 3. Specifically, foreign matter was attached to the fired bodies fired with the support plates of Reference Examples 1 and 3, and many pinholes were generated on the surface of the fired body fired with the support plate of Reference Example 2.
[0074] As shown in Table 1, the static properties of the sintered bodies were good (Rating A) in both the Example and Reference Example 3. On the other hand, the dimensional variation of the sintered bodies was good (Rating A) in the Example as shown in Fig. 5, whereas slight variation was observed in Reference Example 3 as shown in Fig. 6 (Rating B).
[0075] Furthermore, as shown in Table 1, the cutting performance of the sintered body (i.e., cutting tool) was good in both the working example and reference example 3 (rating A).
[0076] Next, for the support plates of the obtained Example, Reference Example 1, and Reference Example 2, the surfaces of the coating layers were subjected to XPS analysis using an X-ray photoelectron spectrometer PHI Quantera II manufactured by ULVAC-PHI, Inc. under the following measurement conditions.
[0077] The X-rays used were AlKα rays monochromated by a monochromator. The X-ray output was 25 W, the acceleration voltage was 15 kV, the measurement area was approximately 100 μm in diameter, the measurement interval for bond energy was 0.100 eV, and the measurement range for bond energy was 450 to 470 eV. The results of this XPS analysis are shown in Figure 7.
[0078] 7 is a graph showing the results of XPS analysis of the coating layer surfaces of the support plates of the Example, Reference Example 1, and Reference Example 2. As shown in FIG. 7, the coating layer of the support plate of Reference Example 1 is TiO 2 The majority of the peaks are due to TiO 2 It can be seen that the peak due to TiC decreases and the peak due to TiC increases.
[0079] Furthermore, the coating layer on the support plate of the example is TiO 2 It can be seen that almost no peaks due to TiC are observed, and the majority of the peaks are due to TiC.
[0080] In this manner, in the embodiment, by carbonizing the thermal sprayed layer from the surface side of the coating layer using a carbon-containing gas, it is possible to form a coating layer with a higher titanium carbide content.
[0081] The carbon-containing gas according to the embodiment is not limited to the case containing methane, but may also contain acetylene (C 2 H 2 On the other hand, by using methane, which is easy to handle, as the carbon-containing gas, the carbonization treatment of the thermal sprayed layer can be carried out more easily.
[0082] In addition, the background was removed from each of the XPS spectra of the Example, Reference Example 1, and Reference Example 2 shown in Figure 7. Then, in each of the XPS spectra from which the background was removed, Ti2P 3/2 The maximum value of the emitted electron intensity per unit time in the peak in the range of 454 eV to 456 eV corresponding to the TiC value was calculated as the TiC value.
[0083] Similarly, in each of the XPS spectra from which the background was removed, Ti2P 3/2 The maximum emitted electron intensity per unit time at the peak in the range of 457 eV to 459 eV corresponding to TiO 2 The values were calculated.
[0084] Then, the calculated TiC value and TiO 2 From the value, TiO is calculated based on the above formula (1). 2 The ratio was calculated, and the calculation results are shown in Table 1 above.
[0085] As shown in Table 1, in the embodiment, this TiO 2 By setting the ratio to 0.2 or less, it is possible to reduce adhesion of the sintered body to the support plate after the sintering treatment. Therefore, according to the embodiment, cutting tools can be stably manufactured.
[0086] Furthermore, as shown in Table 1, in the embodiment, this TiO 2 By setting the ratio to 0.2 or less, it is possible to reduce the reaction of the sintered body with the support plate after the sintering treatment. Therefore, according to the embodiment, the quality of the sintered body is well maintained, and a high-quality cutting tool can be manufactured.
[0087] Next, the upper surface (i.e., the side not facing the support plate) and the lower surface (i.e., the side facing the support plate) of the fired bodies fired with the support plate of Example and Reference Example 3 were observed with a SEM (Scanning Electron Microscope). The observation results are shown in Figures 8 to 11.
[0088] 8 and 9 are SEM images showing an example of the crystalline structure of the upper and lower surfaces of the sintered body sintered with the support plate of Example 1. Figures 10 and 11 are SEM images showing an example of the crystalline structure of the upper and lower surfaces of the sintered body sintered with the support plate of Reference Example 3.
[0089] As shown in Figures 8 and 9, the crystalline structure of the sintered body sintered using the support plate of Example 1 is almost uniform between the upper and lower surfaces. On the other hand, as shown in Figures 10 and 11, the crystalline structure of the sintered body sintered using the support plate of Reference Example 3 is somewhat uneven between the upper and lower surfaces.
[0090] In this manner, in the embodiment, by firing the compact using a support plate on which a coating layer containing metal carbide is formed, the crystalline structure of the fired body can be made more uniform.
[0091] Next, the surface roughness Sa of the coating layer of the obtained support plate of the example was measured using a one-shot 3D shape measuring instrument VR-3000 manufactured by Keyence Corp. As a result, the surface roughness Sa of the coating layer of the support plate of the example was 24 μm.
[0092] Next, the purity of titanium carbide in the coating layer of the obtained support plate of the example was measured by a known method and was found to be 95% or more.
[0093] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments, and various modifications are possible without departing from the spirit of the present disclosure.
[0094] For example, in the above embodiment, an example is shown in which the support plate of the present disclosure is applied to the manufacturing process of a cutting tool made of cermet, but the present disclosure is not limited to such an example, and the support plate of the present disclosure may also be applied to the manufacturing process of a cutting tool made of cemented carbide, for example.
[0095] Furthermore, in the above embodiment, an example has been shown in which a sprayed layer formed by a thermal spraying process of a metal element (for example, titanium) is carbonized to form a coating layer, but the present disclosure is not limited to such an example, and a metal layer or a semi-metal layer formed by various known thin film formation methods may also be carbonized to form a coating layer.
[0096] Furthermore, in the above embodiment, an example is shown in which the technology of the present disclosure is applied to a semiconductor manufacturing apparatus 10 that uses a gas-phase reaction to epitaxially grow semiconductor crystals on a sample S, but the support plate of the present disclosure may also be applied to apparatus used in various other semiconductor manufacturing processes.
[0097] Further advantages and other aspects may readily occur to those skilled in the art. Therefore, the disclosure in its broader aspects is not limited to the specific details and representative embodiments shown and described above. Accordingly, various modifications may be made without departing from the spirit or scope of the general inventive concept as defined by the appended claims and their equivalents.
[0098] The present technology can also be configured as follows: (1) A support plate comprising: a base having a first surface and a second surface located opposite to the first surface; and a coating layer located on at least one of the first surface and the second surface of the base, wherein the coating layer includes at least one of a metal carbide and a metalloid carbide, the coating layer having a central region including a center in a thickness direction and an outer surface region including an end portion on a surface side, and wherein a content ratio by mass % of the metal carbide and the metalloid carbide in the outer surface region is greater than a content ratio by mass % of the metal carbide and the metalloid carbide in the central region. (2) The support plate according to (1), wherein the coating layer includes at least one of titanium carbide and silicon carbide. (3) The support plate according to (1) or (2), wherein the coating layer further has an inner surface region including an end portion on the side in contact with the base, and wherein the content ratio of the metal carbide and the metalloid carbide in the inner surface region, in terms of mass%, is greater than the content ratio of the metal carbide and the metalloid carbide in the central region. (4) The support plate according to (3), wherein the content ratio of the metal carbide and the metalloid carbide in the outer surface region, in terms of mass%, is greater than the content ratio of the metal carbide and the metalloid carbide in the inner surface region. (5) A substrate having a first surface and a second surface located on the opposite side of the first surface, and a coating layer located on at least one of the first surface and the second surface of the substrate, wherein the coating layer has a central region including a center in a thickness direction and an outer surface region including an end portion on a surface side, the coating layer contains Ti element, and when the surface of the outer surface region is analyzed by XPS (X-ray photoelectron spectroscopy), TiP 3/2The maximum value of the emitted electron intensity per unit time at the peak in the range of 454 eV to 456 eV corresponding to TiC value is taken as the Ti2P 3/2 The maximum emitted electron intensity per unit time at the peak in the range of 457 eV to 459 eV corresponding to TiO 2 When the value is 2 value / (TiO 2 value + TiC value) to TiO 2 When expressed as a ratio, the TiO 2 The ratio of TiO in the outer surface region is 0.2 or less, and the content ratio of TiC in mass % in the outer surface region is greater than the content ratio of TiC in mass % in the central region. 2 The content ratio in mass % of TiO in the central region is 2 (7) The support plate according to (5) or (6), wherein the coating layer further has an inner surface region including an end portion on the side in contact with the base, and the content ratio of TiC in the inner surface region is greater than the content ratio of TiC in the central region. (8) The support plate according to (5) or (6), wherein the content ratio of TiO in the inner surface region is greater than the content ratio of TiC in the central region. 2 The content ratio in mass % of TiO in the central region is 2(9) The support plate according to (7) above, wherein the content ratio by mass of TiC in the outer surface region is smaller than the content ratio by mass of TiC in the inner surface region. (10) The support plate according to any one of (1) to (9) above, wherein the substrate is mainly composed of carbon. (11) A method for manufacturing a support plate, comprising: a step of spraying at least one of a metal and a metalloid onto a surface of a plate-shaped substrate mainly composed of carbon to form a sprayed layer; and a step of carbonizing the metal and the metalloid contained in the sprayed layer to form a coating layer containing at least one of a metal carbide and a metalloid carbide, wherein the coating layer forming step includes adding a carbon component to the sprayed layer from the surface side of the sprayed layer. (12) The method for manufacturing a support plate according to (11), wherein the step of forming the coating layer involves heating the substrate to 1400°C or higher in the presence of a carbon-containing gas to add a carbon component to the thermal spray layer. (13) The method for manufacturing a support plate according to (12), wherein the carbon-containing gas contains methane. (14) The method for manufacturing a support plate according to (12) or (13), wherein the step of forming the coating layer involves supplying the carbon-containing gas at a flow rate of 5 L / min or higher. (15) The method for manufacturing a support plate according to any one of (11) to (14), wherein the purity of the metal carbide and the metalloid carbide in the coating layer is 95% or higher. (16) The method for manufacturing a support plate according to any one of (11) to (15), wherein the thickness of the coating layer is 20 μm to 200 μm. (17) The method for manufacturing a support plate according to any one of (11) to (16), wherein the surface roughness Sa of the coating layer is 10 μm to 50 μm.
[0099] 1 Support plate 2 Base 2a First surface 2b Second surface 3 Covering layer 3a Central region 3b Outer surface region 3c Inner surface region M Molded object S Sample
Claims
1. A support plate comprising: a base having a first surface and a second surface opposite to the first surface; and a coating layer located on at least one of the first surface and the second surface of the base, wherein the coating layer includes at least one of a metal carbide and a metalloid carbide, the coating layer having a central region including a center in a thickness direction, and an outer surface region including an end portion on a surface side, wherein the content ratio by mass of the metal carbide and the metalloid carbide in the outer surface region is greater than the content ratio by mass of the metal carbide and the metalloid carbide in the central region.
2. The support plate according to claim 1, wherein the coating layer contains at least one of titanium carbide and silicon carbide.
3. A support plate as described in claim 1 or 2, wherein the coating layer further has an inner surface region including an end portion in contact with the base, and the content ratio by mass % of the metal carbide and the metalloid carbide in the inner surface region is greater than the content ratio by mass % of the metal carbide and the metalloid carbide in the central region.
4. The support plate according to claim 3, wherein the content ratio, by mass %, of the metal carbide and the metalloid carbide in the outer surface region is greater than the content ratio, by mass %, of the metal carbide and the metalloid carbide in the inner surface region.
5. A substrate having a first surface and a second surface located on the opposite side to the first surface, and a coating layer located on at least one of the first surface and the second surface of the substrate, the coating layer having a central region including a center in a thickness direction and an outer surface region including an end portion on a surface side, the coating layer containing Ti element, and when the surface of the outer surface region is analyzed by XPS (X-ray photoelectron spectroscopy), it is found that Ti2P 3/2 The maximum value of the emitted electron intensity per unit time at the peak in the range of 454 eV to 456 eV corresponding to TiC value, and Ti2P 3/2 The maximum emitted electron intensity per unit time at the peak in the range of 457 eV to 459 eV corresponding to TiO 2 When the value is set as TiO 2 value / (TiO 2 value + TiC value) is 2 When expressed as a ratio, the TiO 2 a ratio of 0.2 or less, and the TiC content by weight percent in the outer surface region is greater than the TiC content by weight percent in the central region.
6. TiO in the outer surface region 2 The content ratio in mass% of TiO in the central region is 2 The support plate according to claim 5 , wherein the content by mass % is less than 0.01% by mass.
7. A support plate as described in claim 5 or 6, wherein the coating layer further has an inner surface region including an end portion on the side in contact with the base, and the TiC content by mass % in the inner surface region is greater than the TiC content by mass % in the central region.
8. TiO in the inner surface region 2 The content ratio in mass% of TiO in the central region is 2 The support plate according to claim 7 , wherein the content by mass % is less than:
9. A support plate according to claim 7 or 8, wherein the TiC content by mass % in said outer surface region is greater than the TiC content by mass % in said inner surface region.
10. A support plate according to any one of claims 1 to 9, wherein the substrate is mainly composed of carbon.
11. A method for manufacturing a support plate, comprising: a step of spraying at least one of a metal and a metalloid onto the surface of a plate-shaped substrate mainly composed of carbon to form a sprayed layer; and a step of carbonizing the at least one of the metal and the metalloid contained in the sprayed layer to form a coating layer containing at least one of a metal carbide and a metalloid carbide, wherein the step of forming the coating layer comprises adding a carbon component to the sprayed layer from the surface side of the sprayed layer.
12. The method for manufacturing a support plate according to claim 11, wherein the step of forming the coating layer comprises heating the substrate to 1400°C or higher in the presence of a carbon-containing gas to add a carbon component to the thermal spray layer.
13. The method for manufacturing a support plate according to claim 12, wherein the carbon-containing gas contains methane.
14. The method for manufacturing a support plate according to claim 12 or 13, wherein the step of forming the coating layer comprises supplying the carbon-containing gas at a flow rate of 5 L / min or more.
15. A method for manufacturing a support plate according to any one of claims 11 to 14, wherein the purity of the metal carbide and the metalloid carbide in the coating layer is 95% or more.
16. A method for manufacturing a support plate according to any one of claims 11 to 15, wherein the coating layer has a thickness of 20 μm to 200 μm.
17. A method for manufacturing a support plate according to any one of claims 11 to 16, wherein the surface roughness Sa of the coating layer is 10 μm to 50 μm.
Citation Information
Patent Citations
Sagger