Curable resin composition, coating material, and article

The curable resin composition, featuring a specific polyester polyol and acrylic polyol blend, addresses the limitations of conventional acrylic resin compositions by enhancing chemical resistance and adhesion, resulting in a cured film with superior appearance and durability for various industrial applications.

WO2024203370A1PCT designated stage expired Publication Date: 2024-10-03DIC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009909
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-14
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional acrylic resin compositions used in paints and coatings face challenges with poor chemical resistance, particularly sunscreen resistance, while also lacking in appearance and adhesion on plastic substrates.

Method used

A curable resin composition is developed containing specific polyester polyols and acrylic polyols, where the polyester polyol is a reaction product of polyhydric carboxylic acid and polyhydric alcohol, with a high concentration of aliphatic dicarboxylic acid and trifunctional alcohol, enhancing the ester group concentration and molecular weight to improve chemical resistance and adhesion.

Benefits of technology

The composition provides a cured coating film with excellent appearance, adhesion, water resistance, and chemical resistance, suitable for applications in automotive, industrial, and plastic surfaces, outperforming comparative examples in terms of texture and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is a curable resin composition comprising a polyester polyol (A) that is a reaction product of a polycarboxylic acid (a1) and a polyhydric alcohol (a2) and an acrylic polyol (B), the curable resin composition being characterized in that the polycarboxylic acid (a1) comprises an aliphatic dicarboxylic acid (a1-1) having a linear C4-10 alkyl group, the polyhydric alcohol (a2) comprises at least one diol (a2-1) selected from the group consisting of ethylene glycol, diethylene glycol, 1,2-propanediol and 1,3-propanediol and also comprises a trifunctiolal or higher alcohol (a2-2), and the ester group concentration in the polyester polyol (A) is 6 to 11 mmol / g. The curable resin composition can be formed into a cured coating film having excellent appearance (high build), adhesiveness, water resistance and chemical resistance. Therefore, the curable resin composition is suitable for use in various coating materials.
Need to check novelty before this filing date? Find Prior Art

Description

Curable resin composition, coating material and article

[0001] The present invention relates to a curable resin composition, a coating material, and an article.

[0002] Acrylic resin compositions have traditionally been used in applications such as paints, inks, adhesives, and synthetic leather due to their excellent chemical resistance, weather resistance, flexibility, and adhesion. In particular, their paint applications are used in fields such as automobiles, home appliances, and building materials. In these fields, coating films that have excellent adhesion to plastic substrates, chemical resistance (sunscreen resistance, alcohol resistance) that anticipate actual use situations, and excellent appearance (thickness) are required.

[0003] As a coating composition that provides a coating film with a good thickness, a two-component coating composition has been proposed that contains, as a main component, at least one of an oxidatively polymerizable unsaturated fatty acid and an alkyd resin having an oxidatively polymerizable group, and a copolymer of an acrylic copolymer and a silicone having at least one of a hydroxyl group and an alkoxysilyl group (see, for example, Patent Document 1). However, systems that use these unsaturated fatty acids and alkyd resins have the problem of poor chemical resistance, such as sunscreen resistance.

[0004] Patent No. 5688523 specification

[0005] The problem to be solved by the present invention is to provide a curable resin composition that can give a cured coating film that is excellent in appearance (thickness), adhesion, water resistance, and chemical resistance; a coating material; and an article having a cured coating film of the coating material.

[0006] As a result of extensive research aimed at solving the above problems, the present inventors have found that a curable resin composition containing a specific polyester polyol and an acrylic polyol can provide a cured coating film that is excellent in appearance (thickness), adhesion, water resistance, and chemical resistance, and have completed the present invention.

[0007] That is, the present invention relates to a curable resin composition containing a polyester polyol (A) which is a reaction product of a polycarboxylic acid (a1) and a polyhydric alcohol (a2), and an acrylic polyol (B), wherein the polycarboxylic acid (a1) contains 20 mol% or more of an aliphatic dicarboxylic acid (a1-1) having a linear alkyl group having 4 to 10 carbon atoms, the polyhydric alcohol (a2) contains 20 mol% or more of one or more diols (a2-1) selected from the group consisting of ethylene glycol, diethylene glycol, 1,2-propanediol, and 1,3-propanediol, and contains 5 to 20 mol% of a trifunctional or higher functional alcohol (a2-2), and the ester group concentration of the polyester polyol (A) is 6 to 11 mmol / g.

[0008] The curable resin composition of the present invention can give a cured coating film that is excellent in appearance (thickness), adhesion, water resistance, and chemical resistance, and can therefore be suitably used in various coatings for automobile exteriors, automobile repairs, plastics, industrial machinery, building materials, wooden floors, etc.

[0009] The curable resin composition of the present invention is a resin composition containing a polyester polyol (A) which is a reaction product of a polycarboxylic acid (a1) and a polyhydric alcohol (a2), and an acrylic polyol (B), in which the polycarboxylic acid (a1) contains 20 mol% or more of an aliphatic dicarboxylic acid (a1-1) having a linear alkyl group having 4 to 10 carbon atoms, the polyhydric alcohol (a2) contains 20 mol% or more of one or more diols (a2-1) selected from the group consisting of ethylene glycol, diethylene glycol, 1,2-propanediol, and 1,3-propanediol, and contains 5 to 20 mol% of a tri- or higher functional alcohol (a2-2), and the ester group concentration of the polyester polyol (A) is 6 to 11 mmol / g.

[0010] The polyester polyol (A) is a reaction product of a polycarboxylic acid (a1) and a polyhydric alcohol (a2), and can be obtained by a known condensation reaction.

[0011] It is important that the polycarboxylic acid (a1) contains 20 mol % or more of an aliphatic dicarboxylic acid (a1-1) having a linear alkyl group having 4 to 10 carbon atoms, since this allows a coating film with excellent thickness to be obtained.

[0012] Examples of the aliphatic dicarboxylic acid (a1-1) having a linear alkyl group having 4 to 10 carbon atoms include succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, maleic acid, fumaric acid, etc., as well as methyl esters and acid chlorides of these aliphatic dicarboxylic acids, with succinic acid and sebacic acid being more preferred. These aliphatic dicarboxylic acids (a1-1) can be used alone or in combination of two or more.

[0013] In the present invention, the dicarboxylic acid includes anhydrides of the dicarboxylic acid.

[0014] As the polycarboxylic acid (a1), a polycarboxylic acid (a1-2) other than the dicarboxylic acid (a1-1) can be used in combination.

[0015] Examples of the other polycarboxylic acids (a1-2) include aliphatic dicarboxylic acids other than the dicarboxylic acids (a1-1), alicyclic dicarboxylic acids, aromatic dicarboxylic acids, etc. These polycarboxylic acids (a1-2) can be used alone or in combination of two or more.

[0016] Examples of the aliphatic dicarboxylic acid other than the dicarboxylic acid (a1-1) include decanedicarboxylic acid and dimer acid.

[0017] Examples of the alicyclic dicarboxylic acid include 1,3-cyclopentanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid.

[0018] Examples of the aromatic dicarboxylic acid include terephthalic acid, isophthalic acid, orthophthalic acid, naphthalenedicarboxylic acid, biphenyldicarboxylic acid, 1,2-bis(phenoxy)ethane-p,p'-dicarboxylic acid, p-hydroxybenzoic acid, p-(2-hydroxyethoxy)benzoic acid, trimellitic acid, and pyromellitic acid.

[0019] The aliphatic dicarboxylic acid (a1-1) having a linear alkyl group having 4 to 10 carbon atoms in the polycarboxylic acid (a1) is preferably present in an amount of 30 to 90 mol % because this further improves the thickness of the resulting coating film.

[0020] It is important that the polyhydric alcohol (a2) contains 20 mol % or more of one or more diols (a2-1) selected from the group consisting of ethylene glycol, diethylene glycol, 1,2-propanediol, and 1,3-propanediol, in order to obtain a coating film with excellent thickness.

[0021] Furthermore, it is important that the polyhydric alcohol (a2) contains 5 to 20 mol % of a tri- or higher functional alcohol (a2-2), since this allows a coating film with excellent chemical resistance to be obtained.

[0022] Examples of the tri- or higher functional alcohol (a2-2) include aliphatic polyol compounds such as trimethylolethane, trimethylolpropane, glycerin, hexanetriol, and pentaerythritol; aromatic polyol compounds such as trihydroxybenzene; and polyether-modified polyol compounds obtained by ring-opening polymerization of the aliphatic polyol compounds or aromatic polyol compounds with cyclic ether compounds such as ethylene oxide, propylene oxide, tetrahydrofuran, ethyl glycidyl ether, propyl glycidyl ether, butyl glycidyl ether, phenyl glycidyl ether, and allyl glycidyl ether. These tri- or higher functional alcohols (a2-2) can be used alone or in combination of two or more.

[0023] As the polyhydric alcohol (a2), other polyhydric alcohols (a2-3) other than the diols (a2-1) and the tri- or higher functional alcohols (a2-2) can be used in combination.

[0024] Examples of the other polyhydric alcohols (a2-3) include 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 2-ethyl-1,3-propanediol, 2-methyl-1,4-butanediol, 2-ethyl-2-methyl-1,3-propanediol, 2-ethylbutane-1,4-butanediol, 2,3-dimethyl-1,4-butanediol, 3-methyl-1,5-pentanediol, 2,4- Examples of the polyhydric alcohol (a2-3) include aliphatic diols such as dimethyl-1,5-pentanediol, 3,3-dimethylpentane-1,5-diol, 2,2-diethyl-1,3-propanediol, 3-propylpentane-1,5-diol, 2,2-diethyl-1,4-butanediol, 2,4-diethyl-1,5-pentanediol, 2,2-dipropyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, and 2,5-diethyl-1,6-hexanediol; alicyclic structure-containing diol compounds such as cyclohexanediol and cyclohexanedialcohol; aromatic ring-containing diol compounds such as biphenol and bisphenol; polyether diols; and polycarbonate diols. These other polyhydric alcohols (a2-3) can be used alone or in combination of two or more.

[0025] It is important that the ester group concentration of the polyester polyol (A) is 6 to 11 mmol / g in order to balance the chemical resistance of the resulting coating film and the compatibility with the acrylic polyol (B).

[0026] The ester group concentration (mmol / g) refers to the number of millimoles of ester groups in 1 g of polyester polyol (A), and can be determined, for example, by calculation from the amount of the polyester polyol (A) charged.

[0027] The hydroxyl value of the polyester polyol (A) is preferably 50 to 250 mgKOH / g, as this further improves the balance between the chemical resistance of the resulting coating film and the compatibility with the acrylic polyol (B).

[0028] The number average molecular weight of the polyester polyol (A) is preferably 800 to 5,000, as this further improves the balance between the chemical resistance of the resulting coating film and the compatibility with the acrylic polyol (B).

[0029] The hydroxyl value and acid value in the present invention are measured in accordance with JIS test method K 0070-1992, and the average molecular weight is a value converted into polystyrene based on measurement by gel permeation chromatography (hereinafter abbreviated as "GPC").

[0030] The acrylic polyol (B) can be obtained, for example, by copolymerizing an unsaturated monomer (b1) having a hydroxyl group and another unsaturated monomer (b2).

[0031] Examples of the unsaturated monomer (b1) having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxy-n-butyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-n-butyl (meth)acrylate, 3-hydroxy-n-butyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, glycerin mono(meth)acrylate, polyoxyethylene mono(meth)acrylate, polyoxypropylene mono(meth)acrylate, polyoxybutylene mono(meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, polycaprolactone-modified hydroxyethyl mono(meth)acrylate, etc. These unsaturated monomers (b1) having a hydroxyl group can be used alone or in combination of two or more.

[0032] Examples of the other unsaturated monomer (b2) include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, β-carboxyethyl (meth)acrylate, ω-carboxy-polycaprolactone mono(meth)acrylate, 2-(meth)acryloyloxyethyl succinate, and 2-(meth)acryloyloxyethylhexahydrophthalic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid, and half esters of these unsaturated dicarboxylic acids. unsaturated monomers having a carboxyl group, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylates having a hydrocarbon group such as butyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, behenyl (meth)acrylate, cyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and benzyl (meth)acrylate; acrylamide, N,N-dimethyl (meth)acrylamide, (meth)acrylonitrile, 3-(meth)acryloylpropyltrimethoxysilane, N,N-dimethylaminoethyl (meth)acrylate, glycidyl (meth)acrylate, 2-(meth)acryloyloxyethyl acid phosphate, styrene, α-methylstyrene, p-methylstyrene, and p-methoxystyrene. These other unsaturated monomers (b2) can be used alone or in combination of two or more.

[0033] The content of the unsaturated monomer (b1) having a hydroxyl group in the unsaturated monomer raw material of the acrylic polyol (B) is preferably 0.5 to 40 mass%, more preferably 1.5 to 35 mass%, because this further improves the balance between chemical resistance and adhesion.

[0034] The amount of the unsaturated monomer having a carboxyl group in the unsaturated monomer raw material of the acrylic polyol (B) is preferably 0.1 to 15% by mass, since this further improves the chemical resistance.

[0035] In the present invention, "(meth)acrylic acid" refers to either or both of methacrylic acid and acrylic acid, "(meth)acrylate" refers to either or both of methacrylate and acrylate, and "(meth)acryloyl" refers to either or both of methacryloyl and acryloyl.

[0036] The acrylic polyol (B) can be produced by a known polymerization method using the hydroxyl group-containing monomer (b1) and the other monomer (b2) as raw materials, but a solution radical polymerization method is preferred because it is simple.

[0037] Examples of the method for producing the acrylic polyol (B) by the solution radical polymerization method include a method in which each monomer as a raw material is dissolved in a solvent and / or the polyester polyol (A) and a polymerization reaction is carried out in the presence of a polymerization initiator. From the viewpoint of improving compatibility, it is preferable to carry out the polymerization reaction in the presence of the polyester polyol (A).

[0038] Examples of the solvent include hydrocarbon solvents such as toluene, xylene, cyclohexane, n-hexane, and octane; alcohol solvents such as methanol, ethanol, isopropanol, n-butanol, isobutanol, sec-butanol, and ethylene glycol monomethyl ether; ester solvents such as methyl acetate, ethyl acetate, n-butyl acetate, isobutyl acetate, and amyl acetate; and ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. These solvents can be used alone or in combination of two or more.

[0039] Examples of the polymerization initiator include azo compounds such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), and azobiscyanovaleric acid; organic peroxides such as tert-butyl peroxypivalate, tert-butyl peroxybenzoate, tert-butylperoxy-2-ethylhexanoate, di-tert-butyl peroxide, cumene hydroperoxide, benzoyl peroxide, and tert-butyl hydroperoxide; and inorganic peroxides such as hydrogen peroxide, ammonium persulfate, potassium persulfate, and sodium persulfate. These polymerization initiators can be used alone or in combination of two or more. The polymerization initiator is preferably used in an amount of 0.1 to 10% by mass relative to the total amount of the monomers that serve as raw materials for the acrylic polyol (A).

[0040] In addition to the polymerization initiator, a chain transfer agent such as lauryl mercaptan, octyl mercaptan, 2-mercaptoethanol, octyl thioglycolate, 3-mercaptopropionic acid, α-methylstyrene dimer, etc. may also be used, if necessary.

[0041] The weight average molecular weight (Mw) of the mixture of the polyester polyol (A) and the acrylic polyol (B) is preferably 8,000 to 150,000.

[0042] The curable resin composition of the present invention contains the polyester polyol (A) and the acrylic polyol (B). The mass ratio (A / B) of the polyester polyol (A) to the acrylic polyol (B) is preferably 10 / 90 to 70 / 30, more preferably 15 / 85 to 60 / 40, because this improves the balance between thickness and chemical resistance.

[0043] The hydroxyl value of the solid content of the curable resin composition of the present invention is preferably 30 to 150 mgKOH / g, as this further improves the balance between chemical resistance and adhesion.

[0044] The acid value of the solid content of the curable resin composition of the present invention is preferably 0.5 to 20 mgKOH / g, as this further improves the balance between chemical resistance, adhesion and water resistance.

[0045] The method for mixing the polyester polyol (A) and the acrylic polyol (B) is not particularly limited, but from the viewpoint of improving compatibility, a method in which the acrylic polyol (B) is synthesized in the presence of the polyester polyol (A) is preferred.

[0046] The coating material of the present invention contains the curable resin composition of the present invention, and other ingredients may be used, such as inorganic pigments, organic pigments, extender pigments, coloring pigments, bright pigments, cellulose derivatives, waxes, surfactants, stabilizers, flow modifiers, dyes, leveling agents, rheology control agents, ultraviolet absorbers, antioxidants, plasticizers, antistatic agents, antifoaming agents, viscosity modifiers, light resistance stabilizers, weather resistance stabilizers, heat resistance stabilizers, pigment dispersants, and curing agents.

[0047] Use of a polyisocyanate compound (C) as the curing agent can further improve the physical properties of the coating film. Examples of the polyisocyanate compound (C) include aromatic diisocyanate compounds such as tolylene diisocyanate, diphenylmethane diisocyanate, m-xylylene diisocyanate, and m-phenylenebis(dimethylmethylene)diisocyanate; and aliphatic or alicyclic diisocyanate compounds such as pentamethylene diisocyanate, hexamethylene diisocyanate, lysine diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 2-methyl-1,3-diisocyanatocyclohexane, 2-methyl-1,5-diisocyanatocyclohexane, 4,4'-dicyclohexylmethane diisocyanate, and isophorone diisocyanate.

[0048] Examples of the polyisocyanate compound that can be used include prepolymers having an isocyanate group obtained by subjecting the above diisocyanate compounds to an addition reaction with a polyhydric alcohol; compounds having an isocyanurate ring obtained by cyclotrimerizing the above diisocyanate compounds; polyisocyanate compounds having a urea bond or a biuret bond obtained by reacting the above diisocyanate compounds with water; homopolymers of acrylic monomers having an isocyanate group, such as 2-isocyanatoethyl (meth)acrylate, 3-isopropenyl-α,α-dimethylbenzyl isocyanate, and (meth)acryloyl isocyanate; and copolymers having an isocyanate group obtained by copolymerizing the above acrylic monomers having an isocyanate group with monomers such as other acrylic monomers, vinyl ester compounds, vinyl ether compounds, aromatic vinyl monomers, and fluoroolefins.

[0049] The above polyisocyanate compounds (C) can be used alone or in combination of two or more kinds.

[0050] The amount of the polyisocyanate compound (C) used is such that the equivalent ratio (NCO / OH) of the isocyanate group (NCO) of the polyisocyanate compound (C) to the hydroxyl group (OH) of the curable resin composition is in the range of preferably 0.2 to 2, more preferably 0.5 to 1.5.

[0051] The above-mentioned raw materials used in the curable resin composition and coating material of the present invention may also be biomass raw materials.

[0052] The method for applying the coating material of the present invention varies depending on the article to be coated, but examples include methods using a gravure coater, roll coater, comma coater, knife coater, air knife coater, curtain coater, kiss coater, shower coater, wheeler coater, spin coater, dipping, screen printing, spraying, an applicator, a bar coater, a brush, and the like.

[0053] Furthermore, the coating material of the present invention can be diluted with an organic solvent to adjust the viscosity to a level suitable for the above-mentioned coating method. Examples of such organic solvents include aromatic hydrocarbon solvents such as toluene and xylene; alcohol solvents such as methanol, ethanol, isopropanol, t-butanol, propylene glycol monomethyl ether, propylene glycol normal propyl ether, ethylene glycol monobutyl ether, and diacetone alcohol; ester solvents such as ethyl acetate, butyl acetate, isobutyl acetate, normal propyl acetate, propylene glycol monomethyl ether acetate, and ethyl 3-ethoxypropionate; and ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, and cyclohexanone. These solvents can be used alone or in combination of two or more.

[0054] The coating material of the present invention can provide a cured coating film that is excellent in appearance and various coating properties on the surface of various articles.

[0055] The coating composition of the present invention may be applied directly to the article to be coated, or a primer coating material suitable for the article to be coated may be applied first, and then the coating composition of the present invention may be applied.

[0056] Examples of materials for the article to be coated include various metals such as iron, copper, zinc, aluminum, magnesium, etc. and alloys of these; various plastics such as polycarbonate, acrylonitrile-butadiene-styrene copolymer, PC-ABS polymer alloy, polymethyl methacrylate, polyethylene terephthalate, polyamide, polypropylene, etc., and fiber-reinforced plastics in which fillers such as glass fibers are added to these plastics; and wood.

[0057] Examples of articles having a cured coating film formed using the coating material of the present invention include interior and exterior materials for various vehicles such as automobiles and railway cars; interior and exterior materials for buildings such as industrial machinery, exterior walls, roofs, glass, decorative panels, and wooden floors; civil engineering components such as soundproof walls and drainage ditches; housings for home appliances such as televisions, refrigerators, washing machines, and air conditioners; housings for electronic devices such as personal computers, smartphones, mobile phones, digital cameras, and game consoles; and housings for office automation equipment such as printers and facsimiles.

[0058] The present invention will be described in more detail below with reference to specific examples. The hydroxyl value and acid value were measured in accordance with JIS test method K 0070-1992. The average molecular weight (Mw) was measured under the following GPC measurement conditions.

[0059] [GPC Measurement Conditions] Measurement apparatus: High-speed GPC apparatus ("HLC-8220GPC" manufactured by Tosoh Corporation) Column: The following columns manufactured by Tosoh Corporation were used, connected in series: "TSKgel G5000" (7.8 mm I.D. x 30 cm) x 1 "TSKgel G4000" (7.8 mm I.D. x 30 cm) x 1 "TSKgel G3000" (7.8 mm I.D. x 30 cm) x 1 "TSKgel G2000" (7.8 mm I.D. x 30 cm) x 1 Detector: RI (differential refractometer) Column temperature: 40°C Eluent: tetrahydrofuran (THF) Flow rate: 1.0 mL / min Injection volume: 100 μL (tetrahydrofuran solution with a sample concentration of 4 mg / mL) Standard sample: A calibration curve was prepared using the following monodisperse polystyrene.

[0060] (Monodisperse polystyrene) "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation

[0061] Synthesis Example 1: Production of Polyester Polyol (A-1) 61 parts by mass of ethylene glycol, 314 parts by mass of diethylene glycol, 92 parts by mass of trimethylolpropane, 379 parts by mass of succinic acid, and 154 parts by mass of isophthalic acid were charged into a reaction vessel equipped with a stirrer, a condenser, and a thermometer. An esterification reaction was carried out for 12 hours at 200 to 250°C while stirring under a nitrogen stream, and 148.9 parts by mass of condensed water was removed to obtain polyester polyol (A-1). The number average molecular weight (Mn) of this polyester polyol (A-1) was 1,416, the hydroxyl value was 115 mgKOH / g, and the acid value was 7.1 mgKOH / g. Ester group concentration [mmol / g] = (number of moles of carboxyl groups [mol]) / (mass of polyester polyol [g]) × 1000 = 8.273 / 851.1 × 1000 [mmol / g] = 9.72 [mmol / g]

[0062] (Synthesis Examples 2 to 6: Production of Polyester Polyols (A-2) to (A-6)) Polyester polyols (A-2) to (A-6) were obtained in the same manner as in Synthesis Example 1, except that the raw materials used in Synthesis Example 1 were changed as shown in Table 1.

[0063] (Synthesis Examples 7 to 10: Production of Polyester Polyols (RA-1) to (RA-4)) Polyester polyols (RA-1) to (RA-4) were obtained in the same manner as in Synthesis Example 1, except that the raw materials used in Synthesis Example 1 were changed as shown in Table 2.

[0064] The resin compositions and properties of the polyester polyols (A-1) to (A-6) obtained above are shown in Tables 1 and 2.

[0065]

[0066]

[0067] The resin compositions and property values ​​of the polyester polyols (RA-1) to (RA-4) obtained above are shown in Table 3.

[0068]

[0069] Example 1: Production of Curable Resin Composition (1) 200 parts by mass of polyester polyol (A-1) and 600 parts by mass of n-butyl acetate were added to a flask equipped with a cooling tube, thermometer, dropping funnel, and stirrer, and the internal temperature was raised to 100 ° C. Next, a mixture of 370.4 parts by mass of methyl methacrylate, 160.0 parts by mass of n-butyl methacrylate, 245.6 parts by mass of 2-hydroxyethyl methacrylate, 24.0 parts by mass of methacrylic acid, 160 parts by mass of n-butyl acetate, and 32 parts by mass of t-butylperoxy-2-ethylhexanoate was added dropwise over 3 hours. Thereafter, the polymerization reaction was carried out for 15 hours while maintaining the internal temperature at 100 ° C. Next, 250 parts by mass of n-butyl acetate was added, and the desired curable resin composition (1) was obtained. The weight average molecular weight (Mw) of the resulting resin was 25,540, the hydroxyl value of the solid content was 128 mgKOH / g, and the acid value of the solid content was 17.1 mgKOH / g.

[0070] (Examples 2 to 6: Production of curable resin compositions (2) to (6)) Curable resin compositions (2) to (6) were obtained in the same manner as in Example 1, except that the raw materials used in Example 1 were changed as shown in Table 4.

[0071] (Comparative Examples 1 to 4: Production of Curable Resin Compositions (R1) to (R4)) Curable resin compositions (R1) to (R4) were obtained in the same manner as in Example 1, except that the raw materials used in Example 1 were changed as shown in Table 5.

[0072] The resin compositions and property values ​​of the curable resin compositions (1) to (6) obtained above are shown in Table 4.

[0073]

[0074] The resin compositions and property values ​​of the curable resin compositions (R1) to (R4) obtained above are shown in Table 5.

[0075]

[0076] The abbreviations in the table are as follows: MMA: methyl methacrylate BMA: n-butyl methacrylate HEMA: 2-hydroxyethyl methyl methacrylate MAA: methacrylic acid

[0077] [Preparation of Paint] The curable resin composition obtained above and a curing agent (Sumidur N-3300, a polyisocyanate compound, manufactured by Sumika Covestro Urethane Co., Ltd.) were uniformly mixed. The blending ratio of the curable resin composition to the curing agent was such that the equivalent weight of hydroxyl groups in the curable resin composition and the equivalent weight of isocyanate groups in the curing agent were 1:1. Next, the paint was prepared by diluting the mixture with a mixed solvent (butyl acetate / diacetone alcohol / isobutyl acetate / ethyl acetate = 30 / 30 / 30 / 10 (mass ratio)) so that the viscosity was 9 to 10 seconds (23°C) measured using a Viscosity Cup NK-2 manufactured by Anest Iwata Corporation.

[0078] [Preparation of Cured Coating Film X for Evaluation] The coating material obtained above was spray-coated onto an ABS (acrylonitrile-butadiene-styrene copolymer) substrate (50 mm × 70 mm × 1 mm) so that the film thickness after drying would be 15 to 25 μm, and the coating was dried by heating in a dryer at 80° C. for 30 minutes, and then dried at 25° C. for 7 days to prepare Cured Coating Film X for evaluation.

[0079] [Preparation of Cured Coating Film Y for Evaluation] The coating material obtained above was spray-coated onto a PC (polycarbonate) substrate (50 mm × 70 mm × 1 mm) so that the film thickness after drying would be 20 to 30 μm, and the coating was dried by heating in a dryer at 80° C. for 30 minutes, and then dried at 25° C. for 7 days to prepare Cured Coating Film Y for evaluation.

[0080] [Evaluation of Adhesion] 1 mm wide cuts were made with a cutter on the cured coating film for evaluation obtained above, leaving 100 grids. Cellophane tape was then applied so as to cover all of the grids, and the tape was quickly peeled off four times. The adhesion was evaluated based on the number of grids remaining adhered, according to the following criteria: ○: 100 grids △: 70 to 99 grids ×: 69 grids or less

[0081] [Evaluation of Water-Resistant Adhesion] The cured coating film for evaluation obtained above was immersed in water at 40°C for 240 hours, and then the same procedure as in the adhesion evaluation above was carried out, and the water-resistant adhesion was evaluated according to the following criteria: ○: 100 pieces △: 70 to 99 pieces ×: 69 pieces or less

[0082] [Evaluation of Chemical Resistance] A chemical (Neutrogena Ultra Sheer Dry Touch Sunscreen, SPF 55) was applied to the cured coating film for evaluation obtained above at 20 mg / cm2, and then dried in a dryer at 55°C for 4 hours. The coating surface was then washed with a neutral detergent and left at room temperature for 24 hours, and the chemical resistance was evaluated according to the following criteria: ◎: No traces ○: Slight traces △: Traces ×: The base material of the substrate was exposed

[0083] [Evaluation of Appearance] The thickness of the cured coating film for evaluation obtained above was evaluated visually. ⊚: Very thick; ◯: Strong thick; Δ: Weak thick; ×: No thick.

[0084] The evaluation results of the paints (1) to (6) obtained above are shown in Table 6.

[0085]

[0086] The evaluation results of the paints (R1) to (R4) obtained above are shown in Table 7.

[0087]

[0088] It was confirmed that the cured coating films obtained from the curable resin compositions of the present invention in Examples 1 to 6 were excellent in appearance (thickness), adhesion, water resistance, and chemical resistance.

[0089] On the other hand, Comparative Example 1 is an example in which the amount of the tri- or higher functional alcohol (a2-2) in the polyhydric alcohol (a2) is less than the lower limit of the present invention, and it was confirmed that the chemical resistance of the cured coating film was insufficient.

[0090] Comparative Example 2 is an example in which the ester group concentration of the polyester polyol (A) is higher than the upper limit of the present invention, and it was confirmed that the compatibility with the acrylic polyol (B) was poor and the appearance of the cured coating film was insufficient.

[0091] Comparative Example 3 is an example in which the amount of diol (a2-1) in the polyhydric alcohol (a2) is less than the lower limit of the present invention, and it was confirmed that the appearance of the cured coating film was insufficient.

[0092] Comparative Example 4 is an example in which the amount of aliphatic dicarboxylic acid (a1-1) in the polycarboxylic acid (a1) is less than the lower limit of the present invention, and it was confirmed that the appearance of the cured coating film was insufficient.

Claims

1. A curable resin composition comprising a polyester polyol (A) which is a reaction product of a polyvalent carboxylic acid (a1) and a polyhydric alcohol (a2), and an acrylic polyol (B), wherein the polyvalent carboxylic acid (a1) contains 20 mol% or more of an aliphatic dicarboxylic acid (a1-1) having a linear alkyl group having 4 to 10 carbon atoms, the polyhydric alcohol (a2) contains 20 to 80 mol% of one or more diols (a2-1) selected from the group consisting of ethylene glycol, diethylene glycol, 1,2-propanediol, and 1,3-propanediol, and contains 5 to 20 mol% of a trifunctional or higher alcohol (a2-2), and the ester group concentration of the polyester polyol (A) is 6 to 11 mmol / g.

2. The curable resin composition according to claim 1, wherein the mass ratio (A / B) of the polyester polyol (A) to the acrylic polyol (B) is 10 / 90 to 70 / 30.

3. The curable resin composition according to claim 1, which has a hydroxyl value of the solid content of 30 to 150 mgKOH / g.

4. A coating material comprising the curable resin composition according to any one of claims 1 to 3 and a polyisocyanate compound (C).

5. An article having a cured coating film of the coating material according to claim 4.

Citation Information

Patent Citations

  • JP1974055788A

  • Film-forming hydrophilic resin and coating material composition

    JP1998338719A

  • Method for producing aqueous resin dispersion

    JP2004149593A

  • Adhesive layer and adhesive sheet

    JP2022079443A

  • Polyester polyol resin and coating

    WO2018084062A1