BAW resonator and electronic apparatus

The BAW resonator design addresses high resistance issues in high frequency applications by using an intermediate insulator layer and a low acoustic impedance electrode, achieving efficient energy confinement and improved filter characteristics in 5G applications.

WO2024203457A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010236
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

BAW resonators with heavy metal electrodes for high acoustic impedance suffer from high resistance issues, particularly in high frequency applications like 5G, leading to deteriorated filter characteristics due to thin electrode thickness and increased wiring resistance.

Method used

A BAW resonator design featuring a supporting base material, an acoustic mirror layer with alternating high and low acoustic impedance layers, an intermediate insulator layer with higher impedance than the low acoustic impedance layer, and a first electrode with lower acoustic impedance than the high impedance layer, configured to enhance energy confinement while reducing wiring resistance.

Benefits of technology

The design effectively reduces wiring resistance and improves energy confinement, enabling stable operation in high frequency applications like 5G filters with enhanced piezoelectric properties and reduced noise generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010236_03102024_PF_FP_ABST
    Figure JP2024010236_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a bulk acoustic wave (BAW) resonator capable of reducing wiring resistance and exhibiting an energy confinement effect. A BAW resonator (1) according to the present invention includes, in the following order: a support base material (10); an acoustic mirror layer (20) in which one or more pairs of high acoustic impedance layers (21) and low acoustic impedance layers (22) are alternately stacked; a first electrode (40); a piezoelectric layer (50) having a wurtzite crystal structure; and a second electrode (60). An intermediate layer (30) comprising an insulator is provided between the acoustic mirror layer (20) and the first electrode (40). The intermediate layer (30) has an acoustic impedance higher than that of the low acoustic impedance layer (22), and the first electrode (40) has an acoustic impedance lower than that of the high acoustic impedance layer (21).
Need to check novelty before this filing date? Find Prior Art

Description

BAW resonator and electronic device

[0001] The present invention relates to a BAW resonator and an electronic device.

[0002] A bulk acoustic wave (BAW) resonator has a piezoelectric layer made of a piezoelectric material between two electrode layers. BAW resonators are used in electronic devices as electronic components such as BAW filters, utilizing the piezoelectric effect of the piezoelectric layer.

[0003] As a BAW resonator, for example, a BAW resonator has been disclosed in which an acoustic stack is arranged on a reflective element of a substrate, the acoustic stack including a first electrode, a first diffusion barrier layer, a piezoelectric layer, a second diffusion barrier layer, and a second electrode (see, for example, Patent Document 1).

[0004] In the BAW resonator of Patent Document 1, in order to confine energy from a reflective element provided in the substrate, the first electrode disposed on the substrate of the BAW resonator is formed using a heavy metal with high acoustic impedance, such as Mo.

[0005] U.S. Patent No. 1,101,8651

[0006] However, if the first electrode is formed using a heavy metal with high acoustic impedance, such as Mo, the resistance of the first electrode will be high, which is disadvantageous when using the first electrode as a transmission line. Also, the thickness of the electrode needs to be thinner as the resonant frequency increases, and when the first electrode is used in a high-frequency range such as for 5G applications, the first electrode will be very thin, which will result in resistance loss and may cause degradation of the filter characteristics of the BAW resonator.

[0007] An object of one embodiment of the present invention is to provide a BAW resonator that can reduce wiring resistance and exhibit an energy trapping effect.

[0008] One aspect of the BAW resonator according to the present invention comprises a support substrate, an acoustic mirror layer formed by alternately stacking one or more pairs of high acoustic impedance layers and low acoustic impedance layers, a first electrode, a piezoelectric layer having a wurtzite crystal structure, and a second electrode, stacked in this order; an intermediate layer is provided between the surface of the acoustic mirror layer facing the first electrode and the first electrode, the intermediate layer being made of an insulator and having a higher acoustic impedance than the low acoustic impedance layer; and the first electrode has a lower acoustic impedance than the high acoustic impedance layer.

[0009] One aspect of the BAW resonator according to the present invention can reduce wiring resistance and exert an energy trapping effect.

[0010] 1 is a schematic cross-sectional view showing the configuration of a BAW resonator according to an embodiment of the present invention.

[0011] Hereinafter, embodiments of the present invention will be described in detail. To facilitate understanding of the description, the same components in each drawing are denoted by the same reference numerals, and duplicate descriptions will be omitted. The scale of each component in the drawings may differ from the actual scale. In this specification, unless otherwise specified, the symbol "to" indicating a range of values ​​means that the values ​​before and after it are included as the lower and upper limits.

[0012] <Piezoelectric element> Fig. 1 is a schematic cross-sectional view showing the configuration of a piezoelectric element according to this embodiment. As shown in Fig. 1, the BAW resonator 1 includes a support substrate 10, an acoustic mirror layer 20, an intermediate layer 30, a first electrode 40, a piezoelectric layer 50, and a second electrode 60, which are laminated in this order from the support substrate 10 side. The BAW resonator 1 may be formed in any shape, such as a sheet (film).

[0013] In this specification, a three-dimensional Cartesian coordinate system with three axes (X-axis, Y-axis, and Z-axis) is used, with the width direction of the BAW resonator 1 defined as the X-axis, the length direction defined as the Y-axis, and the height (thickness) direction (vertical direction) defined as the Z-axis. The second electrode 60 side in the Z-axis direction is defined as the +Z-axis, and the supporting substrate 10 side is defined as the -Z-axis. In the following description, for convenience of explanation, the +Z-axis direction will be referred to as up or upward, and the -Z-axis direction will be referred to as down or downward, but this does not represent a universal up-down relationship.

[0014] The BAW resonator 1 has an intermediate layer 30 between the acoustic mirror layer 20 and the first electrode 40, the intermediate layer 30 having a higher acoustic impedance than the low acoustic impedance layer 22 of the acoustic mirror layer 20, and the acoustic impedance of the first electrode 40 is made lower than the high acoustic impedance layer 21 of the acoustic mirror layer 20. This allows the BAW resonator 1 to create a difference in acoustic impedance between the acoustic mirror layer 20, the intermediate layer 30, and the first electrode 40. Furthermore, the first electrode 40 can be formed from a material with low acoustic impedance, thereby reducing its resistivity. Therefore, the BAW resonator 1 can achieve the effect of trapping vibration energy transmitted from the acoustic mirror layer 20 while reducing the wiring resistance of the first electrode 40.

[0015] [Supporting Base] As shown in FIG. 1, the supporting base 10 is a substrate on which a laminate of an acoustic mirror layer 20, an intermediate layer 30, a first electrode 40, a piezoelectric layer 50, and a second electrode 60 is placed, and may be flexible so as to impart flexibility to the BAW resonator 1.

[0016] As the material for forming the support substrate 10, any material can be used, regardless of type, as long as it can stably support the laminate. For example, a plastic substrate, a metal foil, a metal plate, a silicon (Si) substrate, an inorganic dielectric substrate, a glass substrate, etc. may be used.

[0017] When a plastic substrate is used, it is preferable to use a flexible material that can impart flexibility to the BAW resonator 1 including the piezoelectric layer 50 .

[0018] Examples of materials that can be used to form the plastic substrate include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate (PC), acrylic resins, cycloolefin polymers, polyamide (PA) resins, polyimide (PI) resins, polyphenylene sulfide (PPS), polytetrafluoroethylene (PTFE), and diallyl phthalate resin (PDAP).

[0019] The metal foil may be made of a metal such as Au, Pt, Ag, Ti, Al, Mo, Ru, or Cu.

[0020] The metal plate may be made of a material such as aluminum, copper, stainless steel, or tantalum.

[0021] Examples of materials that may be used to form the inorganic dielectric substrate include MgO and sapphire.

[0022] The thickness of the support substrate 10 is not particularly limited and may be appropriately determined depending on the application of the BAW resonator 1, the material of the support substrate 10, etc., and may be, for example, 20 μm to 725 μm. If the thickness of the support substrate 10 is 20 μm to 725 μm, it can stably support the laminate including the laminate of the acoustic mirror layer 20, the intermediate layer 30, the first electrode 40, the piezoelectric layer 50, and the second electrode 60. Furthermore, warping of the support substrate 10 is suppressed, and the influence of warping of the support substrate 10 on the piezoelectric characteristics can be reduced, allowing the BAW resonator 1 to have the desired flexibility.

[0023] In this specification, the thickness of the support substrate 10 refers to the length in the direction perpendicular to the main surface of the support substrate 10. The method for measuring the thickness of the support substrate 10 is not particularly limited, and any measurement method can be used. The thickness of the support substrate 10 may be, for example, the thickness measured at an arbitrary location on the cross section of the support substrate 10, or may be the average value of the measured values ​​measured at several arbitrary locations. Hereinafter, the definition of thickness is similarly defined for other members.

[0024] [Acoustic Mirror Layer] As shown in Fig. 1 , the acoustic mirror layer 20 is provided on the upper principal surface (top surface) 101 of the support substrate 10. The acoustic mirror layer 20 may be composed of acoustic multilayer films with different specific acoustic impedances. The acoustic mirror layer 20 is a multilayer film in which two or more pairs of high acoustic impedance layers 21 having a predetermined specific acoustic impedance and low acoustic impedance layers 22 having a lower specific acoustic impedance than the high acoustic impedance layers 21 are alternately stacked.

[0025] When resonant vibrations are transmitted to the acoustic mirror layer 20, the vibration energy of the resonance is reflected by the acoustic mirror layer 20. The speed at which vibration waves (elastic waves) propagate through the high acoustic impedance layer 21 is different from the speed at which they propagate through the low acoustic impedance layer 22. By designing the thickness so that the reflected waves reinforce each other due to interference at the interfaces of the layers that make up the acoustic mirror layer 20, the vibration energy of the resonance is returned in the direction of incidence of the elastic waves without being affected by the support substrate 10, while the thermal energy is released in the direction of the support substrate 10.

[0026] The high acoustic impedance layer 21 is made of W, Mo, Ta, 2 O 5 The low acoustic impedance layer 22 is made of a material having a higher density or bulk modulus than the high acoustic impedance layer 21, such as ZnO.

[0027] The low acoustic impedance layer 22 is made of SiO 2 The low acoustic impedance layer 22 may be formed of a material having a low density or a low deposition modulus of elasticity, such as a material having a low density or a low deposition modulus of elasticity. The low acoustic impedance layer 22 may be an amorphous layer or a layer in which the amorphous phase is predominant. By forming the low acoustic impedance layer 22 as a layer in which the amorphous phase is predominant, stress in the high acoustic impedance layer 21 can be alleviated.

[0028] The high acoustic impedance layer 21 and the low acoustic impedance layer 22 are formed on the support substrate 10 by sputtering or the like.

[0029] [Intermediate Layer] As shown in FIG. 1 , the intermediate layer 30 is provided on the upper surface 201 of the acoustic mirror layer 20 on the first electrode 40 side, and is provided between the acoustic mirror layer 20 and the first electrode 40 .

[0030] The intermediate layer 30 is an insulating layer that reflects vibration energy excited by a piezoelectric resonator composed of the first electrode 40, the piezoelectric layer 50, and the second electrode 60. If the intermediate layer 30 is a conductive layer such as a conductor, the intermediate layer 30 is regarded as an electrode, and the thickness of the electrode is the sum of the thickness of the intermediate layer 30 and the thickness of the first electrode 40. Therefore, the intermediate layer 30 is regarded as having a larger mass than the actual mass of the first electrode 40. As a result, vibration is difficult to excite, resulting in a shift to a lower frequency. Note that the intermediate layer 30 may be a layer containing other components, such as a metal, in addition to an insulator, as long as it has insulating properties.

[0031] The intermediate layer 30 preferably has an acoustic impedance higher than that of the low acoustic impedance layer 22 of the acoustic mirror layer 20, and has an acoustic impedance between that of the high acoustic impedance layer 21 and the first electrode 40. By having an acoustic impedance intermediate between that of the high acoustic impedance layer 21 and the first electrode 40, the intermediate layer 30 can have a difference in acoustic impedance between the acoustic mirror layer 20, the intermediate layer 30, and the first electrode 40 in the order of low, high, and low, thereby efficiently reflecting vibration energy and further demonstrating the trapping effect between the electrodes.

[0032] The acoustic impedance of the intermediate layer 30 is 3.0×10 7 kg / (m 2 s) ~ 6.0 × 10 7 kg / (m 2 s), preferably 3.3 × 10 7 kg / (m 2 s) ~ 5.5 x 10 7 kg / (m 2 s), more preferably 3.5 × 10 7 kg / (m 2 s) ~ 5.0 × 10 7 kg / (m 2 It is more preferable that the acoustic impedance of the metals generally used for the electrodes, piezoelectric layers, etc. that constitute the BAW resonators is shown in Table 1.

[0033]

[0034] As can be seen from Table 1, if the acoustic impedance of the intermediate layer 30 is within the above-mentioned preferred range, the intermediate layer 30 can be formed using ZnO or AlN, and therefore the intermediate layer 30 can be easily formed.

[0035] The material for forming the intermediate layer 30 may be an insulator having a higher acoustic impedance than the low acoustic impedance layer 22, and may be the same material as the piezoelectric layer 50. Examples of materials for forming the intermediate layer 30 include ZnO, AlN, and Al. 2 O 3 , SiON, SiOC, etc. can be used. These may be used alone or in combination of two or more. Among these, ZnO and AlN are preferred, and ZnO is more preferred. The intermediate layer 30 preferably contains ZnO as a main component, and may contain other components as secondary components in any appropriate amounts.

[0036] The intermediate layer 30 can be formed using sputtering, a chemical vapor deposition (CVD) method, a sol-gel method, or the like.

[0037] The thickness of the intermediate layer 30 is preferably 15 nm to 35 nm. The lower limit of the thickness of the intermediate layer 30 is more preferably 20 nm or more, and even more preferably 25 nm or more. If the thickness of the intermediate layer 30 is 15 nm to 35 nm, the intermediate layer 30 can function as an acoustic impedance layer with a higher impedance than the low acoustic impedance layer 22, and can increase the reflection efficiency of vibration energy.

[0038] 1 , the first electrode 40 is provided on the main surface (upper surface) 301 above the intermediate layer 30. The first electrode 40 may be formed as a thin film on a part of or the entire surface of the intermediate layer 30.

[0039] The first electrode 40 has an acoustic impedance lower than that of the high acoustic impedance layer 21 of the acoustic mirror layer 20 .

[0040] The first electrode 40 can be made of a conductive material that has a lower acoustic impedance than the high acoustic impedance layer 21. Examples of the material that can be used include metals such as Pt, Au, Ag, Cu, Mg, Al, Si, Ti, Cr, Fe, Ni, Zn, Y, Sc, Rb, Zr, Hf, Nb, Rh, Pd, Sn, and Ta.

[0041] The acoustic impedance of the first electrode 40 is set to be lower than that of the intermediate layer 30, and is therefore set to 3.0×10 7 kg / (m 2 s), preferably less than 2.5 × 10 7 kg / (m 2 s) or less, and more preferably 2.0 × 10 7 kg / (m 2 It is more preferable that the acoustic impedance of the first electrode 40 is 3.0×10 7 kg / (m 2 If the thickness is less than s, it becomes easier to select a material for forming the intermediate layer 30 having a higher acoustic impedance than the first electrode 40 .

[0042] The resistivity of the first electrode 40 is 3.0×10 -7 It is preferable that the resistance is Ωm or less, and 2.8×10 -7 More preferably, it is 2.5×10 Ωm or less. -7 It is more preferable that the resistivity is Ωm or less. Table 2 shows the resistivities of metals that are generally used for the electrodes that make up BAW resonators.

[0043]

[0044] From Table 2, the resistivity of the first electrode 40 is 3.0×10 -7 If the resistivity is Ωm or less, it becomes easier to select a material for forming the intermediate layer 30 having a higher resistivity than the first electrode 40 .

[0045] The ratio of the thickness of the first electrode 40 to the intermediate layer 30 (film thickness ratio) is preferably 3 to 11, more preferably 4 to 10, and even more preferably 5 to 9. When the film thickness ratio is within the above-mentioned preferred range, the intermediate layer 30 can fully exhibit its function, can fully reflect sound waves, and can suppress an increase in wiring resistance and suppress attenuation.

[0046] The surface resistivity of the first electrode 40 is preferably less than 0.24 Ω / sq, more preferably 0.22 Ω / sq or less, and even more preferably 0.20 Ω / sq or less. If the surface resistivity is less than 0.24 Ω / sq, an increase in the wiring resistance of the first electrode 40 can be suppressed, and attenuation can be suppressed. The lower limit of the surface resistivity of the first electrode 40 is not particularly limited and may be any appropriate value.

[0047] The surface resistivity can be calculated by dividing the resistivity of the first electrode 40 by the thickness according to the following formula (1): Surface resistivity = Resistivity of first electrode 40 / Thickness of first electrode 40 (1)

[0048] The first electrode 40 may be an amorphous film from the viewpoint of suppressing unevenness and grain boundaries at the interface between the first electrode 40 and the piezoelectric layer 50. By using an amorphous film, it is possible to suppress unevenness on the surface of the first electrode 40 and the generation of grain boundaries that cause leak paths.

[0049] The thickness of the first electrode 40 can be appropriately designed and may be, for example, 40 nm to 300 nm. If the thickness of the first electrode 40 is 40 nm to 300 nm, the function of the electrode can be exhibited and the BAW resonator 1 can be made thinner.

[0050] 1, the piezoelectric layer 50 is provided on the main surface (upper surface) 401 above the first electrode 40. The piezoelectric layer 50 preferably contains an inorganic material as a main component. The term "main component" means that the content of the inorganic material is 95 atm % or more, preferably 98 atm % or more, and more preferably 99 atm % or more.

[0051] As the inorganic material, a piezoelectric material having a perovskite crystal structure (perovskite crystal material), a piezoelectric material having a wurtzite crystal structure (wurtzite crystal material), or the like can be used.

[0052] The wurtzite crystal structure is represented by the general formula AB, where A is an electropositive element and B is an electronegative element. Wurtzite crystal materials have a hexagonal unit cell with a polarization vector parallel to the c-axis.

[0053] As the wurtzite crystal material, it is preferable to use a material that exhibits piezoelectric properties above a certain value and can be crystallized in a low-temperature process at 200°C or less. The wurtzite crystal material contains Zn, Al, Ga, Cd, Si, etc. as the electropositive element A represented by the general formula AB. Examples of wurtzite crystal materials that can be used include zinc oxide (ZnO), zinc sulfide (ZnS), zinc selenide (ZnSe), zinc telluride (ZnTe), aluminum nitride (AlN), gallium nitride (GaN), cadmium selenide (CdSe), cadmium telluride (CdTe), and silicon carbide (SiC). Among these, ZnO is preferred as the wurtzite crystal material because it is relatively easy to achieve good c-axis orientation even in a low-temperature process. These materials may be used alone or in combination of two or more. When two or more wurtzite crystal materials are used in combination, one or more of these may be contained as the main component and other components may be contained as optional components. In addition, each material may be laminated, or multiple targets may be used to form a single layer.

[0054] The wurtzite crystal material preferably contains ZnO, more preferably consists essentially of ZnO, and even more preferably consists only of ZnO. "Substantially" means that the wurtzite crystal material may contain, in addition to ZnO, inevitable impurities that may be inevitably contained during the manufacturing process.

[0055] In addition to the above-mentioned ZnO, AlN, ZnS, ZnSe, and ZnTe, inorganic materials such as wurtzite crystal materials may contain alkaline earth metals such as Mg, Ca, and Sr, or metals such as V, Ti, Zr, Si, Sr, and Li, in a predetermined range of proportions. These components may be contained in the elemental state or in the oxide state. Among these, Mg-doped ZnO (MgZnO), in which ZnO is doped with Mg, is preferred as the inorganic material because it achieves both a K value, which is an index of the piezoelectric properties of the piezoelectric layer 50, and a Q value, which is an index of the steepness of the piezoelectric properties, and therefore exhibits excellent piezoelectric properties.

[0056] The K value is the value of the electromechanical coupling constant k. The square value (k 2 The k value) indicates the energy conversion efficiency of the electrical energy determined for the piezoelectric material. The higher the energy conversion efficiency of the electrical energy, the better the operating efficiency of the BAW resonator 1 including the piezoelectric layer 50, and the BAW resonator 1 has excellent piezoelectric characteristics. For the same material and composition, the smaller the disorder in the crystal orientation of the piezoelectric material contained in the piezoelectric layer 50, the higher the k value of the piezoelectric material. 2 The value increases and then gradually becomes constant. That is, as the disorder of the crystal orientation of the piezoelectric material decreases, the energy conversion efficiency of the piezoelectric material increases and then gradually becomes constant, and the piezoelectricity becomes constant. Therefore, the larger the electromechanical coupling constant k, the 2 The larger the value of k, the higher the energy conversion efficiency of the piezoelectric material, which means that the piezoelectric properties are improved. Also, the larger the electromechanical coupling constant k, the smaller the disturbance in the crystal orientation, which means that the crystal orientation is improved.

[0057] The Q value is a value that represents the sharpness (sharpness) of frequency characteristics. The larger the Q value, the sharper the frequency characteristics.

[0058] The content of the additive element in the piezoelectric layer 50 is not particularly limited as long as it is within a range that allows the piezoelectric layer 50 to have a wurtzite crystal structure. The method for measuring the content of the additive element contained in the piezoelectric layer 50 is not particularly limited as long as it is a measurable method. The content of the additive element contained in the piezoelectric layer 50 may be measured, for example, by Rutherford backscattering spectroscopy (RBS) using a Pelletron 3SDH (manufactured by NEC Corporation) as a measuring device, or may be measured by secondary ion mass spectrometry using dynamic SIMS (D-SIMS) or the like.

[0059] The thickness of the piezoelectric layer 50 is not particularly limited, and may be any thickness that provides sufficient piezoelectric properties, i.e., polarization properties proportional to pressure, and that can stably exhibit piezoelectric properties by reducing the occurrence of cracks or the like in the piezoelectric layer 50. The thickness of the piezoelectric layer 50 may be, for example, 50 nm to 5 μm. If the thickness of the piezoelectric layer 50 is 50 nm to 5 μm, the occurrence of cracks is suppressed and sufficient piezoelectric properties can be exhibited.

[0060] The crystal orientation of the piezoelectric layer 50 is preferably 5° or less. If the crystal orientation is 5° or less, the crystal orientation in the c-axis direction (c-axis orientation) of the piezoelectric material contained in the piezoelectric layer 50 is good, and the energy conversion efficiency is improved, thereby improving the piezoelectric characteristics in the thickness direction of the piezoelectric layer 50. If the piezoelectric layer 50 contains ZnO as the piezoelectric material, ZnO has a wurtzite crystal structure, and there is a higher correlation between the crystal orientation and the piezoelectric characteristics than with piezoelectric materials having other crystal structures. If the crystal orientation of ZnO is 5° or less, it is easier to increase the energy conversion efficiency, and therefore the piezoelectric characteristics of the BAW resonator 1 can be improved.

[0061] The crystalline orientation of the piezoelectric layer 50 can be evaluated by the full width at half maximum (FWHM) obtained when the surface of the piezoelectric layer 50 is measured by the X-ray rocking curve (XRC) method. That is, the crystalline orientation of the piezoelectric layer 50 is represented by the FWHM of the peak waveform of the rocking curve obtained when the diffraction from the (0002) plane of the crystal of the piezoelectric material contained as a main component in the piezoelectric layer 50 is measured by the XRC method. When the piezoelectric material contained in the piezoelectric layer 50 has a wurtzite crystal structure such as ZnO, the FWHM indicates the degree of parallelism of the crystals constituting the piezoelectric material in the c-axis direction. Therefore, the FWHM of the peak waveform of the rocking curve obtained by the XRC method can be used as an indicator of the c-axis orientation of the piezoelectric layer 50. Therefore, the smaller the FWHM of the rocking curve, the better the crystalline orientation of the piezoelectric layer 50 in the c-axis direction can be evaluated.

[0062] The crystal orientation of the piezoelectric layer 50 may be evaluated using the XRC method to measure diffraction from a specific crystal plane of the piezoelectric material (e.g., the (0002) plane of a ZnO crystal) in the piezoelectric layer 50, and may also be evaluated using the peak intensity as well as the FWHM of the rocking curve. That is, the crystal orientation of the piezoelectric layer 50 may be evaluated using the value obtained by dividing the integrated value of the peak intensity by the FWHM as an evaluation value. For example, the larger the evaluation value obtained by dividing the integrated value of the peak intensity by the FWHM, the better the crystal orientation of the piezoelectric layer 50 can be evaluated to be.

[0063] When two or more inorganic materials are used in combination, the piezoelectric layer 50 may be formed by laminating piezoelectric layers made of the respective inorganic materials.

[0064] 1 , the second electrode 60 is provided on the upper principal surface (top surface) 501 of the piezoelectric layer 50, and is disposed so as to face the first electrode 40. The second electrode 60 can be formed of any conductive material, and the same material as the first electrode 40 can be used.

[0065] Similar to the first electrode 40, the second electrode 60 may be formed as a thin film on a part of or the entire surface of the piezoelectric layer 50, or may be formed in any appropriate shape.

[0066] The thickness of the second electrode 60 can be designed as appropriate, and is preferably, for example, 40 nm to 300 nm. If the thickness of the second electrode 60 is within the above-mentioned preferred range, the function as an electrode can be exhibited and the BAW resonator 1 can be made thin.

[0067] There are no particular limitations on the method for manufacturing the BAW resonator 1, and any appropriate manufacturing method can be used. An example of the method for manufacturing the BAW resonator 1 will be described below.

[0068] First, the high acoustic impedance layer 21 and the low acoustic impedance layer 22 are stacked alternately as a pair on the upper surface of the support substrate 10 formed to a predetermined size, to form the acoustic mirror layer 20.

[0069] There are no particular limitations on the method for forming the high acoustic impedance layer 21 and the low acoustic impedance layer 22, and either a dry process or a wet process may be used. If a dry process is used as the method for forming the high acoustic impedance layer 21 and the low acoustic impedance layer 22, thin high acoustic impedance layer 21 and low acoustic impedance layer 22 can be easily formed.

[0070] Examples of dry processes include sputtering and vapor deposition, and examples of wet processes include plating.

[0071] As the sputtering, for example, DC (direct current) or RF (radio frequency) magnetron sputtering or the like can be used.

[0072] By using sputtering as a method for forming the high acoustic impedance layer 21 and the low acoustic impedance layer 22, it is possible to easily form high-density, thin high acoustic impedance layer 21 and low acoustic impedance layer 22. For this reason, sputtering is preferred as a method for forming the high acoustic impedance layer 21 and the low acoustic impedance layer 22.

[0073] The high acoustic impedance layer 21 is formed, for example, by DC or RF magnetron sputtering. 2 O5 A thin film formed of a material with a high density or bulk modulus, such as ZnO, can be used.

[0074] The low acoustic impedance layer 22 is, for example, a SiO 2 film formed by DC or RF magnetron sputtering. 2 An oxide such as a film can be used.

[0075] When using DC or RF magnetron sputtering, the high acoustic impedance layer 21 or the low acoustic impedance layer 22 is Ta. 2 O 5 , ZnO, SiO 2 For example, when the high acoustic impedance layer 21 is a ZnO film formed by DC or RF magnetron sputtering, either a Zn sputtering target or a ZnO sputtering target may be used for sputtering, depending on the gas atmosphere.

[0076] Next, the intermediate layer 30 is formed on the upper surface 201 of the acoustic mirror layer 20. The method for forming the intermediate layer 30 is not particularly limited, and either a dry process or a wet process may be used, similar to the methods for forming the high acoustic impedance layer 21 and the low acoustic impedance layer 22. Details of the dry process and the wet process are similar to the methods for forming the high acoustic impedance layer 21 and the low acoustic impedance layer 22, and therefore will not be repeated here.

[0077] When the intermediate layer 30 is a metal oxide layer such as ZnO formed by DC or RF magnetron sputtering, the sputtering may be a metal sputtering or a metal oxide sputtering. For example, when the intermediate layer 30 is a ZnO film formed by DC or RF magnetron sputtering, the sputtering may be performed using a Zn sputtering target or a ZnO sputtering target depending on the gas atmosphere.

[0078] Next, the first electrode 40 is deposited (formed) on the upper surface 301 of the intermediate layer 30. The method for forming the first electrode 40 is not particularly limited, and either a dry process or a wet process may be used, similar to the method for forming the high acoustic impedance layer 21 and the low acoustic impedance layer 22. Details of the dry process and the wet process are similar to the method for forming the high acoustic impedance layer 21 and the low acoustic impedance layer 22, and therefore will not be described in detail.

[0079] The first electrode 40 may be formed on the entire upper surface 201 of the acoustic mirror layer 20. Alternatively, the first electrode 40 may be formed into any appropriate shape by processing it into a pattern having a predetermined shape by etching or the like.

[0080] Next, the piezoelectric layer 50 is formed on the upper surface of the first electrode 40. For example, the piezoelectric layer 50 may be formed by DC or RF magnetron sputtering in a mixed gas atmosphere containing an inert gas such as Ar and a trace amount of oxygen, using a target containing elements constituting the piezoelectric material. The piezoelectric layer 50 is formed by sputtering the piezoelectric material onto the first electrode 40.

[0081] The laminate including the support substrate 10, the acoustic mirror layer 20, the intermediate layer 30, and the first electrode 40 may be placed on a deposition plate, which serves as an anode, in a deposition chamber of a sputtering apparatus. The deposition plate may be rotatable, for example. By placing the laminate including the support substrate 10, the acoustic mirror layer 20, the intermediate layer 30, and the first electrode 40 on the deposition plate, the piezoelectric layer 50 can be deposited on the first electrode 40 in a batchwise manner.

[0082] Furthermore, the laminate including the support substrate 10, the acoustic mirror layer 20, the intermediate layer 30, and the first electrode 40 may be wound around a drum roll, which is a film-forming roll, instead of a film-forming plate, as an anode. By placing the drum roll in a film-forming chamber, the piezoelectric layer 50 can be continuously formed on the first electrode 40 while the laminate including the support substrate 10, the acoustic mirror layer 20, the intermediate layer 30, and the first electrode 40 is transported by a roll-to-roll method.

[0083] A target containing elements that constitute the piezoelectric material is used as a cathode.

[0084] When the piezoelectric material includes, for example, a wurtzite crystalline material, a target containing the wurtzite crystalline material may be used. The target containing the wurtzite crystalline material may be a single or multiple targets containing the wurtzite crystalline material contained as a main component in the piezoelectric layer 50. The single or multiple targets may be arranged to face the deposition plate at an interval. The piezoelectric layer 50 containing the wurtzite crystalline material can be formed by using a multi-target sputtering method when multiple targets are used as cathodes, or by using a one-dimensional sputtering method when a single target is used as the cathode.

[0085] When multiple targets are used as cathodes, each target contains a different type of material that constitutes the wurtzite crystal material contained as a main component in the piezoelectric layer 50. When multiple targets are used, for example, a target containing Zn, a target containing Si or Sn, and a target containing Al or Mg may be used. Note that each target may be a metal oxide target containing oxygen. The multiple targets may be arranged in the film formation chamber at intervals. During sputtering, the power applied to each target is adjusted depending on the type of wurtzite crystal material contained in the piezoelectric layer 50, thereby adjusting the atomic ratio between the materials that constitute the piezoelectric layer 50.

[0086] When a single target is used as the cathode, the single target contains the wurtzite crystalline material contained in the piezoelectric layer 50. When a single target is used, an alloy target in which the atomic ratio of the wurtzite crystalline material contained in the piezoelectric layer 50 is adjusted may be used. For example, an alloy target containing Zn, Si or Sn, and Al or Mg may be used. The alloy target may be a metal oxide target containing a wurtzite crystalline material and oxygen.

[0087] For example, when the piezoelectric material is a wurtzite crystal material made of ZnO, a ZnO sintered compact target may be used. The ZnO sintered compact target is placed in a sputtering apparatus, and a mixed gas containing an inert gas such as Ar and oxygen is supplied into the sputtering apparatus. By sputtering using the ZnO sintered compact target in an atmosphere of the mixed gas containing the inert gas and oxygen, the piezoelectric layer 50 can be obtained on the first electrode 40 while suppressing the amount of inert gas that enters during ZnO film formation.

[0088] For example, when the piezoelectric material is a wurtzite crystal material made of MgZnO containing ZnO and MgO in a predetermined mass ratio, a multi-sputtering method using a target made of ZnO sintered body and a target made of MgO sintered body may be used. Alternatively, a one-dimensional sputtering method using an alloy target containing ZnO and MgO, such as a ZnO sintered body target to which MgO has been added in advance at a predetermined ratio, may be used.

[0089] When the multi-target sputtering method is used, a multi-target sputtering apparatus is used as the sputtering apparatus, and a mixed gas containing an inert gas such as Ar and oxygen is supplied into the multi-target sputtering apparatus. In an atmosphere of the mixed gas containing the inert gas and oxygen, a ZnO sintered compact target and an MgO sintered compact target are simultaneously and independently sputtered onto the first electrode 40, thereby forming the piezoelectric layer 50 composed of an MgZnO thin film on the first electrode 40.

[0090] When the one-dimensional sputtering method is used, a sputtering apparatus is used to perform sputtering in a mixed gas atmosphere containing an inert gas such as Ar and oxygen, using, for example, a target of ZnO sintered body to which MgO has been added in advance at a predetermined ratio, thereby forming the piezoelectric layer 50 composed of an MgZnO thin film on the first electrode 40.

[0091] The gas atmosphere during sputtering may be an inert gas atmosphere or a mixed gas atmosphere containing an inert gas and oxygen.

[0092] The pressure in the gas atmosphere during sputtering may be appropriately determined depending on the type of piezoelectric material, the sputtering method, etc., and may be set to, for example, 0.1 Pa to 2.0 Pa.

[0093] The deposition temperature of the piezoelectric layer 50 is not particularly limited and may be appropriately selected depending on the layer structure of the BAW resonator 1, for example, the piezoelectric layer 50 may be deposited at 150° C. or lower.

[0094] By using a sputtering method to form the first electrode 40 and the piezoelectric layer 50, it is possible to form a uniform film with strong adhesion while maintaining the composition ratio of the compound target. Furthermore, by simply controlling the time, it is possible to form the first electrode 40 and the piezoelectric layer 50 with a desired thickness with high precision.

[0095] The piezoelectric layer 50 may be configured by laminating a plurality of layers.

[0096] Next, a second electrode 60 having a predetermined shape is formed on the upper surface 501 of the piezoelectric layer 50. The second electrode 60 can be formed using the same method as that used for forming the first electrode 40.

[0097] The thickness of the second electrode 60 can be designed appropriately and may be, for example, 40 nm to 300 nm.

[0098] The second electrode 60 may be formed on the entire top surface of the piezoelectric layer 50, or may be formed in any suitable shape.

[0099] The BAW resonator 1 is formed by forming a second electrode 60 on the upper surface of the piezoelectric layer 50 .

[0100] After the second electrode 60 is formed, the entire BAW resonator 1 may be heat-treated. This heat treatment can crystallize the first electrode 40 and the second electrode 60, thereby reducing their resistance. The heat treatment is not essential, and may not be performed after the BAW resonator 1 is formed, for example, when the support substrate 10 is made of a material that is not heat-resistant.

[0101] As described above, the BAW resonator 1 according to this embodiment includes the support substrate 10, the acoustic mirror layer 20, the intermediate layer 30, the first electrode 40, the piezoelectric layer 50, and the second electrode 60. The intermediate layer 30 is a layer made of an insulator and has a higher acoustic impedance than the low acoustic impedance layer 22 of the acoustic mirror layer 20. The first electrode 40 provided on the upper surface 301 of the intermediate layer 30 has a lower acoustic impedance than the high acoustic impedance layer 21 of the acoustic mirror layer 20.

[0102] The layer located at the top of the acoustic mirror layer 20 and in contact with the intermediate layer 30 is the low acoustic impedance layer 22. By providing the intermediate layer 30, which has a higher acoustic impedance than the low acoustic impedance layer 22, between the low acoustic impedance layer 22 and the first electrode 40, which has a lower acoustic impedance than the high acoustic impedance layer 21, a difference in acoustic impedance is generated between the low acoustic impedance layer 22, the intermediate layer 30, and the first electrode 40. Because the BAW resonator 1 can generate an impedance difference between the low acoustic impedance layer 22, the intermediate layer 30, and the first electrode 40, it can exert an effect of trapping vibration energy generated in the acoustic mirror layer 20.

[0103] The first electrode 40 is formed using a material with a lower acoustic impedance than the high acoustic impedance layer 21. Materials with a low acoustic impedance generally have low resistivity and high conductivity. Therefore, the first electrode 40 can be formed using a material with a low resistivity.

[0104] Therefore, the BAW resonator 1 has an intermediate layer 30 made of an insulator disposed between the acoustic mirror layer 20 and the first electrode 40, and by generating an impedance difference between the low acoustic impedance layer 22, the intermediate layer 30, and the first electrode 40, it is possible to reduce wiring resistance while achieving an energy trapping effect.

[0105] Furthermore, in the BAW resonator 1, the first electrode 40 can be formed using a material with low resistivity, and therefore the first electrode 40 can be used as a transmission line.

[0106] In the BAW resonator 1, the intermediate layer 30 can have an acoustic impedance between the high acoustic impedance layer 21 and the first electrode 40. This allows the acoustic impedances of the low acoustic impedance layer 22, the intermediate layer 30, and the first electrode 40 to be arranged in this order from low to high, and thus ensures the generation of an impedance difference. This allows the BAW resonator 1 to improve the energy trapping effect.

[0107] The BAW resonator 1 has an acoustic impedance of the intermediate layer 30 of 3.0×10 7 kg / (m 2 s) ~ 6.0 × 10 7 kg / (m 2 s). As a result, the intermediate layer 30 of the BAW resonator 1 can be formed using ZnO, AlN, or the like, and can have a lower acoustic impedance than the commonly used high acoustic impedance layer 21. Therefore, the BAW resonator 1 can easily be configured so that the acoustic impedance levels of the low acoustic impedance layer 22, the intermediate layer 30, and the first electrode 40 are in the order of low, high, and low, making it easy to create an impedance difference. Therefore, the BAW resonator 1 can easily improve the energy trapping effect.

[0108] The BAW resonator 1 has an acoustic impedance of the first electrode 40 of 3.0×10 7 kg / (m 2 s), and the resistivity of the first electrode 40 is 3.0×10 -7 As a result, the intermediate layer 30 can have an acoustic impedance of 3.0×10 7 kg / (m 2 The BAW resonator 1 can be formed using the above-mentioned common metals. Therefore, the BAW resonator 1 can be easily configured so that the acoustic impedance difference is generated in the order of low, high, and low in the low acoustic impedance layer 22, the intermediate layer 30, and the first electrode 40. Therefore, the BAW resonator 1 can easily improve the energy trapping effect.

[0109] In the BAW resonator 1, the ratio of the thickness of the first electrode 40 to the intermediate layer 30 can be set to 3 to 11. This allows the BAW resonator 1 to reduce the influence of the intermediate layer 30 and reflect vibration energy excited by the piezoelectric resonator made up of the first electrode 40, the piezoelectric layer 50, and the second electrode 60, while also suppressing an increase in the wiring resistance of the first electrode 40.

[0110] In the BAW resonator 1, the surface resistivity of the first electrode 40 can be set to less than 0.24 Ω / sq. This makes it possible to suppress an increase in the wiring resistance of the first electrode 40 and suppress attenuation in the BAW resonator 1.

[0111] In the BAW resonator 1, the intermediate layer 30 can be made of the same material as the piezoelectric layer 50.

[0112] The intermediate layer 30 of the BAW resonator 1 can contain ZnO as a main component. The intermediate layer 30 of the BAW resonator 1 can be composed of only ZnO or can contain MgZnO. When the first electrode 40 located above the intermediate layer 30 is made of, for example, Al, the first electrode 40 of the BAW resonator 1 can be formed to have a structure that is favorable for ZnO orientation.

[0113] The first electrode 40 of the BAW resonator 1 can be formed of aluminum. This allows the first electrode 40 of the BAW resonator 1 to be formed using a commonly used conductive material and also allows the first electrode 40 to be reliably formed of a material with low resistivity, so that the first electrode 40 can be used as a transmission line.

[0114] The BAW resonator 1 can include MgZnO as a piezoelectric material in the piezoelectric layer 50. Generally, there is a trade-off between the K value and Q value of a piezoelectric layer formed by doping a piezoelectric material with another element. For example, when a piezoelectric element is used in a high-frequency filter that extracts only signals in a high-frequency range, such as the 5 GHz band, and removes signals in other frequency bands, the Q value tends to decrease once the required K value is achieved in the high-frequency range. By including MgZnO as a piezoelectric material in the piezoelectric layer 50, there is no trade-off between the K value and Q value of MgZnO with respect to the Mg concentration, and both the K value and Q value can be achieved even in the high-frequency range. By including MgZnO as a piezoelectric material in the piezoelectric layer 50, the BAW resonator 1 can stably exhibit piezoelectric characteristics in the high-frequency range of a high-frequency filter, etc.

[0115] The BAW resonator 1A can reduce wiring resistance even in the high frequency band, while exerting an energy trapping effect to reduce noise generation and having excellent piezoelectric properties, and therefore can be effectively used as a high frequency filter such as a BAW filter.

[0116] Furthermore, since the BAW resonator 1A can reduce noise generation and have excellent piezoelectric characteristics, it can also be used in electronic devices for various purposes as an electronic component that utilizes the positive piezoelectric effect or the inverse piezoelectric effect in electronic devices, in addition to BAW filters.

[0117] Although the embodiments have been described above, they are presented as examples and the present invention is not limited to the above embodiments. The above embodiments can be implemented in various other forms, and various combinations, omissions, substitutions, modifications, etc. can be made without departing from the spirit of the invention. These embodiments and their modifications are included within the scope and spirit of the invention, and are also included in the inventions and their equivalents as set forth in the claims.

[0118] Hereinafter, the embodiment will be described in more detail with reference to examples and comparative examples, but the embodiment is not limited to these examples and comparative examples.

[0119] <Fabrication of BAW resonators and BAW filters> [Example 1] (Fabrication of acoustic mirror layer) An acoustic mirror layer consisting of a high acoustic impedance layer and a low acoustic impedance layer was formed. 1. Fabrication of high acoustic impedance layer A tungsten (W) film was formed as a high acoustic impedance layer on a Si substrate by DC magnetron sputtering in an Ar atmosphere using a tungsten sputtering target. The acoustic impedance of the high acoustic impedance layer was 1.0 × 10 8 kg / (m 2 s), and the thickness of the high acoustic impedance layer was 216 nm. 2. Fabrication of low acoustic impedance layer SiO was formed on the high acoustic impedance layer by RF magnetron sputtering in a mixed gas atmosphere of Ar and O2 using a silicon sputtering target. 2 The film was formed as a low acoustic impedance layer. The acoustic impedance of the low acoustic impedance layer was 1.3 × 10 7 kg / (m 2 ·s), and the thickness of the low acoustic impedance layer was set to 242 nm.

[0120] (Fabrication of Intermediate Layer) A ZnO film was formed as an intermediate layer on the low acoustic impedance layer by RF magnetron sputtering in an Ar gas atmosphere using a ZnO sputtering target. The acoustic impedance of the intermediate layer was 3.6×10 7 kg / (m 2 The thickness of the intermediate layer was 15 nm. (Fabrication of First Electrode) An Al film was formed as a first electrode on the intermediate layer by DC magnetron sputtering in an Ar atmosphere using an aluminum sputtering target. The acoustic impedance of the first electrode was 1.7×10 7 kg / (m 2The surface resistivity of the first electrode was calculated by dividing the resistivity of the first electrode by its thickness. (Fabrication of Piezoelectric Layer) On the first electrode, a piezoelectric layer was formed by RF sputtering in an Ar and O2 mixed gas atmosphere using a sputtering target in which the mass ratio of ZnO and MgO was adjusted to 88 wt%:12 wt%. The MgZnO thin film had a hexagonal wurtzite structure and the mass ratio of ZnO and MgO was adjusted to 88 wt%:12 wt%. The thickness of the MgZnO thin film was 290 nm. (Fabrication of Second Electrode) On the piezoelectric layer, a molybdenum film (Mo film) was formed as a second electrode by DC magnetron sputtering in an Ar gas atmosphere using a molybdenum sputtering target. The thickness of the Mo film was 89 nm.

[0121] In this way, a BAW resonator was fabricated, which included an acoustic mirror layer, an intermediate layer, a first electrode, a piezoelectric layer, and a second electrode laminated in this order on the substrate.

[0122] A plurality of the fabricated BAW resonators were connected to each other to fabricate a BAW filter.

[0123] [Examples 2 to 5, Comparative Examples 1 and 2] A BAW filter in which a plurality of BAW resonators were connected was fabricated in the same manner as in Example 1, except that the thicknesses of the intermediate layer and the first electrode in Example 1 were changed to the thicknesses shown in Table 3.

[0124] Comparative Example 3 A BAW filter having a plurality of connected BAW resonators was fabricated in the same manner as in Example 1, except that the intermediate layer was not provided and the thickness of the first electrode was changed to the thickness shown in Table 3.

[0125] Table 3 shows the type, acoustic impedance, and thickness of the high acoustic impedance layer, low acoustic impedance layer, intermediate layer, and first electrode that constitute the BAW resonators of each example and comparative example, as well as the ratio of the thickness of the first electrode to the thickness of the intermediate layer (film thickness ratio).

[0126] <Evaluation of BAW Resonators and BAW Filters> The attenuation and bandwidth of the BAW filters including the BAW resonators of each example and comparative example, and the wiring resistance of the BAW resonators were measured.

[0127] [Attenuation] The attenuation of a BAW filter in which a plurality of BAW resonators are connected was determined as the attenuation in the passband of a transmitted signal obtained by two-port measurement using a network analyzer. The measurement results are shown in Table 3.

[0128] The bandwidth of the BAW filter, which is made up of multiple connected BAW resonators, was determined as the width of the frequency band in which the attenuation was −3 dB or more in the pass band of the transmitted signal S21 obtained by two-port measurement using a network analyzer. The measurement results are shown in Table 3.

[0129] [Wiring Resistance] The wiring resistance of the BAW resonator was evaluated by the value of the real part of the impedance in the low frequency range of 1 GHz or less in the reflected signal S11 obtained by one-port measurement with a network analyzer. When the wiring resistance was 3 Ω or less, it was evaluated as "A", and when the wiring resistance was more than 3 Ω, it was evaluated as "B". The evaluation results are shown in Table 3.

[0130]

[0131] As can be seen from Table 3, in each example, the BAW filter had a small attenuation, a wide bandwidth, and a small wiring resistance of the BAW resonator. In Comparative Example 1, the BAW resonator had a large attenuation and a narrow bandwidth. In Comparative Example 2, the BAW resonator had a large wiring resistance. In Comparative Example 3, the BAW resonator had a large attenuation and almost no bandwidth.

[0132] Therefore, it was confirmed that the BAW resonators of each example have an intermediate layer made of an insulator between the acoustic mirror layer and the first electrode, the intermediate layer having a higher acoustic impedance than the low acoustic impedance layer, and the first electrode having a lower acoustic impedance than the high acoustic impedance layer, thereby reducing wiring resistance and exhibiting an energy trapping effect. Therefore, it can be said that the BAW resonators of each example can be effectively used as high frequency filters such as BAW filters.

[0133] Note that aspects of the present invention are as follows, for example. <1> A BAW resonator comprising: a support substrate; an acoustic mirror layer formed by alternately stacking one or more pairs of high acoustic impedance layers and low acoustic impedance layers; a first electrode; a piezoelectric layer having a wurtzite crystal structure; and a second electrode, stacked in this order; and an intermediate layer made of an insulator and provided between the acoustic mirror layer and the first electrode, the intermediate layer having a higher acoustic impedance than the low acoustic impedance layer, and the first electrode having a lower acoustic impedance than the high acoustic impedance layer. <2> The BAW resonator according to <1>, wherein the intermediate layer has an acoustic impedance between the high acoustic impedance layer and the first electrode. <3> The acoustic impedance of the intermediate layer is 3.0×10 7 kg / (m 2 s) ~ 6.0 × 10 7 kg / (m 2 <4> The BAW resonator according to <1> or <2>, wherein the acoustic impedance of the first electrode is between 3.0×10 7 kg / (m 2 s), and the resistivity of the first electrode is less than 3.0×10 -7 <5> The BAW resonator according to any one of <1> to <3>, wherein the ratio of the thickness of the first electrode to the intermediate layer is 3 to 11. <6> The BAW resonator according to any one of <1> to <5>, wherein the surface resistivity of the first electrode, calculated by dividing the resistivity by the thickness, is less than 0.24 Ω / sq. <7> The BAW resonator according to any one of <1> to <6>, wherein the intermediate layer is made of the same material as the piezoelectric layer. <8> The BAW resonator according to <7>, wherein the intermediate layer contains zinc oxide as a main component. <9> The BAW resonator according to any one of <1> to <8>, wherein the first electrode is made of aluminum. <10> An electronic device comprising the BAW resonator according to any one of <1> to <9>.

[0134] This application claims priority based on Japanese Patent Application No. 2023-55029, filed with the Japan Patent Office on March 30, 2023, and incorporates the entire contents of said application by reference.

[0135] REFERENCE SIGNS LIST 1 BAW resonator 10 Support substrate 20 Acoustic mirror layer 21 High acoustic impedance layer 22 Low acoustic impedance layer 30 Intermediate layer 40 First electrode 50 Piezoelectric layer 60 Second electrode 101, 201, 301, 401, 501 Main surface (upper surface) S Space

Claims

1. A BAW resonator comprising: a supporting substrate; an acoustic mirror layer having one or more pairs of alternating high acoustic impedance layers and low acoustic impedance layers; a first electrode; a piezoelectric layer having a wurtzite crystal structure; and a second electrode, laminated in this order; and an intermediate layer made of an insulator and provided between the acoustic mirror layer and the first electrode, wherein the intermediate layer has a higher acoustic impedance than the low acoustic impedance layer, and the first electrode has a lower acoustic impedance than the high acoustic impedance layer.

2. A BAW resonator as claimed in claim 1, wherein said intermediate layer has an acoustic impedance between said high acoustic impedance layer and said first electrode.

3. The acoustic impedance of the intermediate layer is 3.0×10 7 kg / (m 2 s) ~ 6.0 x 10 7 kg / (m 2 2. The BAW resonator of claim 1, wherein:

4. The acoustic impedance of the first electrode is 3.0×10 7 kg / (m 2 s), and the resistivity of the first electrode is less than 3.0×10 -7 2. The BAW resonator of claim 1, wherein the resistance is less than or equal to Ωm.

5. A BAW resonator as claimed in claim 1, wherein the ratio of the thickness of said first electrode to said intermediate layer is 3-11.

6. A BAW resonator according to claim 1, wherein the surface resistivity of said first electrode, calculated by dividing the resistivity by the thickness, is less than 0.24 Ω / sq.

7. A BAW resonator according to claim 1, wherein the intermediate layer is made of the same material as the piezoelectric layer.

8. The BAW resonator according to claim 7, wherein the intermediate layer contains zinc oxide as a main component.

9. The BAW resonator of claim 1, wherein said first electrode is aluminum.

10. An electronic device comprising the BAW resonator according to claim 1.

Citation Information

Patent Citations

  • Immersion diffraction element and method of manufacturing the same

    JP2023055029A

  • Bulk acoustic wave resonators having doped piezoelectric material and an adhesion and diffusion barrier layer

    US11018651B2

  • Bulk acoustic wave filter and method for eliminating unwanted side passbands

    JP2005260964A

  • Bulk acoustic wave filter having improved passband characteristics, combined laterally

    JP2018129839A

  • Laminate, piezoelectric device using same, production method for laminate, and production method for piezoelectric device

    WO2021193167A1