Plated steel sheet, member, and production methods for same
The described steel composition and manufacturing process for automotive sheets achieve high tensile strength and delayed fracture resistance while maintaining excellent plating properties, addressing the limitations of existing technologies.
Patent Information
- Application Number
- PCT/JP2024/010398
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-03
AI Technical Summary
Automotive steel sheets require high tensile strength and excellent delayed fracture resistance, but existing technologies fail to achieve tensile strength of 1180 MPa or more with adequate delayed fracture resistance and maintain good plating properties.
A steel composition with specific elements like C, Si, Mn, B, and Nb, combined with a manufacturing process involving hot rolling, pickling, cold rolling, multiple annealing steps, and sub-zero treatment to achieve a microstructure with high martensite and bainite area ratios, non-uniform B segregation, and a plating layer on the steel sheet.
The solution achieves a tensile strength of 1180 MPa or more, excellent delayed fracture resistance, and maintains good plating properties, ensuring no unplated areas on the steel sheets.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Plated steel sheets, components, and their manufacturing methods
[0001] The present invention relates to a plated steel sheet, a member, and a method for manufacturing the same.
[0002] In addition to strength, automotive steel sheets require excellent delayed fracture resistance. Patent Document 1 discloses a high-strength steel sheet with excellent workability and a manufacturing method thereof. Patent Document 2 discloses a high-strength cold-rolled steel sheet and a manufacturing method thereof.
[0003] JP 2013-147736 A JP 2008-106351 A
[0004] However, the steel plates described in Patent Documents 1 and 2 both have a tensile strength TS of less than 1180 MPa, and delayed fracture resistance is not taken into consideration.
[0005] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a plated steel sheet, a member, and a method for manufacturing the same, which have a high strength with a tensile strength TS of 1180 MPa or more and excellent delayed fracture resistance and plateability.
[0006] In the present invention, high strength means that the tensile strength TS measured in accordance with JIS Z2241 (2011) is 1180 MPa or more.
[0007] Furthermore, "excellent resistance to delayed fracture" means that no cracks occur after 100 hours of immersion in a hydrochloric acid solution of pH 3 after a test piece is subjected to a constant load test with a tensile stress of 1800 MPa on the surface layer.
[0008] Furthermore, "excellent plating ability" means that there are no unplated areas when visually inspected for the presence or absence of unplated areas.
[0009] The present inventors have conducted extensive research to achieve the above-mentioned object, and as a result have obtained the following findings.
[0010] To obtain a tensile strength TS of 1180 MPa or more, it is recommended that martensite or bainite be the main phase. In addition, it is effective to add 0.0015 mass % or more of B to improve delayed fracture resistance.
[0011] It is believed that B has the effect of strengthening the grain boundaries, which serve as fracture paths, by segregating at prior austenite grain boundaries. On the other hand, when B is added, oxides of Si and Mn containing B are concentrated on the surface during annealing, resulting in reduced platability. It was found that the effect on platability is small if the B content is less than 0.0015 mass%. Therefore, a method of improving delayed fracture resistance by setting the B content to less than 0.0015% was investigated. It was then conceived that uneven segregation of B at prior austenite grain boundaries creates grain boundaries with high and low B concentrations, and that a sufficient amount of B segregating at some grain boundaries improves delayed fracture resistance even with a B content of less than 0.0015%.
[0012] Therefore, we investigated a means for non-uniformly segregating B on prior austenite grain boundaries and increasing the B concentration at some grain boundaries. We found that non-uniform B segregation can be achieved by performing the process of B segregation on grain boundaries twice and nucleating new austenite grains the second time. When cold-rolled steel is annealed in the austenite region, B segregates at the austenite grain boundaries. However, at this point, diffusion of B is insufficient and solute B is present, so the segregated B is non-uniform but insufficiently concentrated. If this steel is cooled once to form a martensite and bainite structure and then annealed a second time, an austenite reverse transformation structure is formed. In this regard, if retained austenite is present after the first annealing and cooling, it serves as a nucleus to form an austenite structure with the same crystal orientation as in the first annealing. Furthermore, martensite and bainite contain a large number of dislocations, and the B dissolved in them rapidly diffuses to the austenite grain boundaries through the dislocations during the second annealing, resulting in uniform segregation of B. However, uniform segregation results in a low B concentration at the grain boundaries, so it is necessary to segregate B thickly only at some grain boundaries and thinly at others. Therefore, we focused on the fact that if subzero treatment is performed after the first annealing to remove some of the retained austenite, martensite with a high C concentration is formed, and during the second annealing, new austenite with a different crystal orientation from the austenite formed in the first annealing is nucleated from that martensite. The newly formed austenite grain boundaries are positioned differently from the austenite grain boundaries formed in the first annealing, so the boron concentration is thin and non-uniform. The retained austenite transformed into martensitic structure during subzero treatment is mainly blocky, while film-like retained austenite remains even after subzero treatment. From these thin film-like retained austenite, austenite with the same crystal orientation as during the first annealing is generated. When this structure is cooled, ferrite is generated from the grain boundaries where the B concentration is low and non-uniform. If the area fraction of ferrite is 3.0% or less, a high strength of 1180 MPa or more can be ensured. In the structure thus formed, even if the B content is less than 0.0015%, B is concentrated at the prior austenite grain boundaries sandwiched on both sides by martensite, making it possible to improve delayed fracture resistance.
[0013] The present invention has been made based on the above findings. That is, the gist and configuration of the present invention are as follows. [1] A steel sheet comprising, in mass%, C: 0.10% or more and 0.30% or less, Si: more than 1.20% and 2.00% or less, Mn: 2.5% or more and 4.0% or less, P: 0.050% or less, S: 0.020% or less, Al: 0.10% or less, N: 0.01% or less, Ti: 0.100% or less, Nb: 0.002% or more and 0.050% or less, and B: 0.0008% or more and less than 0.0015%, and satisfying the following formula (1) with the balance consisting of Fe and unavoidable impurities, wherein the total area fraction of martensite and bainite is 95.0% or more, the area fraction of retained austenite is 4.8% or less, the area fraction of ferrite is 0.2% or more and 3.0% or less, and the prior austenite grain size is 10 μm or less, A plated steel sheet comprising: a steel sheet in which the B concentration at prior austenite grain boundaries between adjacent martensite grains is 0.05% or more by mass, the variation in the B concentration at prior austenite grain boundaries between adjacent martensite grains is less than 0.010% by mass within the same grain boundary, and the variation in the B concentration at prior austenite grain boundaries between martensite and ferrite is 0.010% or more by mass, and a plating layer formed on at least one surface of the steel sheet. ([%N] / 14) / ([%Ti] / 47.9)<1.0...Equation (1) In Equation (1), [%N] and [%Ti] represent the N and Ti contents (mass%) in the steel, respectively. [2] The plated steel sheet according to [1] above, wherein the chemical composition further contains, by mass%, at least one selected from V: 0.100% or less, Mo: 0.500% or less, Cr: 1.00% or less, Cu: 1.00% or less, Ni: 0.50% or less, Sb: 0.200% or less, Sn: 0.200% or less, Ta: 0.200% or less, W: 0.400% or less, Zr: 0.0200% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, Co: 0.020% or less, REM: 0.0200% or less, Te: 0.020% or less, Hf: 0.10% or less, and Bi: 0.200% or less. [3] A member made using the plated steel sheet according to [1] or [2] above.[4] A hot rolling process in which a steel slab having the chemical composition according to [1] or [2] is hot rolled to obtain a hot rolled sheet; a pickling process in which the hot rolled sheet is pickled; a cold rolling process in which the hot rolled sheet after the pickling process is cold rolled to obtain a cold rolled sheet; a first annealing process in which the cold rolled sheet is heated to a first heating temperature of Ac3 point or higher; a cooling process in which cooling of the cold rolled sheet after the first annealing process is started from the first heating temperature and cooled to a cooling stop temperature of 100°C or higher but lower than Ms point at an average cooling rate of 50°C / s or higher; a reheating process in which, after the cooling process, the cold rolled sheet is heated to a reheating temperature of 300°C or higher and 400°C or lower, and held at the reheating temperature for 60 seconds or longer to cool to room temperature; a subzero treatment process in which, after the reheating process, a subzero treatment is performed; and a second annealing process in which, after the subzero treatment process, the cold rolled sheet is heated to a second heating temperature of Ac3 point or higher to obtain a steel sheet. [5] A method for producing a plated steel sheet according to [4] above, comprising a plating step of plating the steel sheet to obtain a plated steel sheet. [6] A method for producing a member, comprising a step of forming or joining the plated steel sheet according to [1] or [2] above to produce a member.
[0014] According to the present invention, it is possible to provide a plated steel sheet, a member, and a method for manufacturing the same, which have a high strength with a tensile strength TS of 1180 MPa or more and excellent delayed fracture resistance and plateability.
[0015] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments.
[0016] The plated steel sheet according to this embodiment contains, in mass%, C: 0.10% or more and 0.30% or less, Si: more than 1.20% and 2.00% or less, Mn: 2.5% or more and 4.0% or less, P: 0.050% or less, S: 0.020% or less, Al: 0.10% or less, N: 0.01% or less, Ti: 0.100% or less, Nb: 0.002% or more and 0.050% or less, and B: 0.0008% or more and less than 0.0015%, and satisfies the following formula (1), with the balance being Fe and unavoidable impurities. The total area ratio of martensite and bainite is 95.0% or more, and the area ratio of retained austenite is 4.0% or more. The steel sheet has a B concentration of 0.05% or more by mass, a ferrite area ratio of 0.2% to 3.0%, a prior austenite grain size of 10 μm or less, a prior austenite grain boundary between adjacent martensite grains having a B concentration of 0.05% or more by mass, a variation in the B concentration of the prior austenite grain boundary between adjacent martensite grains within the same grain boundary of less than 0.010% by mass, and a coating layer formed on at least one surface of the steel sheet. ([%N] / 14) / ([%Ti] / 47.9)<1.0...Equation (1) In equation (1), [%N] and [%Ti] represent the N and Ti contents (mass%) in the steel, respectively.
[0017] [Component Composition] First, the appropriate range of the component composition of the steel sheet and the reasons for its limitation will be described. In the following description, "%" representing the content of component elements in the steel sheet means "% by mass" unless otherwise specified. "ppm" means "ppm by mass" unless otherwise specified. Furthermore, in this specification, a numerical range expressed using "to" means a range that includes the numerical values written before and after "to" as the lower and upper limits.
[0018] C: 0.10% or more and 0.30% or less C has the effect of strengthening the martensite-bainite structure. If the C content is less than 0.10%, the area ratio of martensite and bainite decreases, and a tensile strength TS (hereinafter sometimes simply referred to as TS) of 1180 MPa or more cannot be obtained. Therefore, the C content is set to 0.10% or more. The C content is preferably set to 0.11% or more. On the other hand, if the C content exceeds 0.30%, carboborides of B and iron are formed during annealing, making it impossible to segregate a sufficient amount of B on the grain boundaries. Therefore, the C content is set to 0.30% or less. The C content is preferably set to 0.28% or less.
[0019] Si: more than 1.20% and not more than 2.00% Si is an element effective for solid solution strengthening and also has the effect of suppressing carbide precipitation, which deteriorates delayed fracture resistance, so a content of more than 1.20% is required. If the content is 1.20% or less, carbide precipitation occurs, the B concentration at grain boundaries decreases, and delayed fracture resistance deteriorates. Therefore, the Si content is set to more than 1.20%. The Si content is preferably set to 1.30% or more. On the other hand, since Si is a ferrite stabilizing element and raises the transformation point, if the content exceeds 2.00%, the annealing temperature becomes too high and it becomes impossible to make the prior austenite grain size 10 μm or less. Therefore, the Si content is set to 2.00% or less. The Si content is preferably set to 1.80% or less.
[0020] Mn: 2.5% or more and 4.0% or less Mn is effective in improving hardenability. If the Mn content is less than 2.5%, the area ratio of martensite and bainite decreases, resulting in a decrease in strength. Therefore, the Mn content is set to 2.5% or more. The Mn content is preferably set to 2.8% or more. On the other hand, if the Mn content exceeds 4.0%, the segregated portions become excessively hardened, resulting in a decrease in delayed fracture resistance. Therefore, the Mn content is set to 4.0% or less. The Mn content is preferably set to 3.5% or less.
[0021] P: 0.050% or less P segregates at prior austenite grain boundaries and reduces delayed fracture resistance, so the P content is set to 0.050% or less. The P content is preferably set to 0.025% or less. There is no particular lower limit for the P content, and it may be 0%, but a P content of less than 0.001% increases production costs, so a P content of 0.001% or more is preferred.
[0022] S: 0.020% or less S segregates at prior austenite grain boundaries and reduces delayed fracture resistance, so the S content is set to 0.020% or less. The S content is preferably set to 0.018% or less. The S content is more preferably set to 0.0040% or less, and further preferably set to 0.0020% or less. There is no particular lower limit for the S content, but since a content of less than 0.0001% increases production costs, it is preferably set to 0.0001% or more.
[0023] Al: 0.10% or less Al is an element that acts as a deoxidizer, and to obtain this effect, the Al content is preferably 0.005% or more. On the other hand, if the Al content exceeds 0.10%, ferrite is more likely to be formed, resulting in a decrease in strength. Therefore, the Al content is set to 0.10% or less. The Al content is preferably set to 0.05% or less.
[0024] N: 0.01% or less N forms nitrides with Nb and B, reducing the effects of adding Nb and B. Therefore, the N content is set to 0.01% or less. The N content is preferably set to 0.006% or less. Although there is no particular lower limit, from the viewpoint of production costs, the N content is preferably set to 0.0001% or more.
[0025] Ti: 0.100% or less Ti fixes N in steel as TiN, suppresses the formation of BN and NbN, improves the effects of adding Nb and B, and has the effect of improving delayed fracture resistance. To obtain these effects, the Ti content is preferably 0.005% or more. On the other hand, if the Ti content exceeds 0.100%, coarse Ti carbides are formed on grain boundaries, which reduces delayed fracture resistance. Therefore, the Ti content is set to 0.100% or less. The Ti content is preferably set to 0.050% or less.
[0026] Nb: 0.002% or more and 0.050% or less Nb precipitates as a solid solution or as fine carbides, suppressing the growth of austenite grains during annealing. It also refines the grain size, complicating the fracture path and improving delayed fracture resistance. To achieve this effect, the Nb content is set to 0.002% or more. The Nb content is preferably set to 0.005% or more. On the other hand, if the Nb content exceeds 0.050%, not only does the effect saturate, but coarse Nb carbides precipitate, deteriorating delayed fracture resistance. Therefore, the Nb content is set to 0.050% or less. Furthermore, the Nb content is preferably set to 0.040% or less.
[0027] B: 0.0008% or more and less than 0.0015% B segregates at prior austenite grain boundaries, increasing grain boundary strength and improving delayed fracture resistance. To achieve this effect, the B content is set to 0.0008% or more. The B content is preferably set to 0.0009% or more. On the other hand, if the B content is 0.0015% or more, B concentrates on the steel sheet surface together with Si and Mn during annealing to form oxides, degrading the surface appearance and platability. In addition, carboborides are formed, degrading delayed fracture resistance. Therefore, the B content is set to less than 0.0015%. The B content is preferably set to 0.0014% or less.
[0028] ([%N] / 14) / ([%Ti] / 47.9)<1.0...Equation (1) In order to obtain the above-mentioned effects of adding B and Nb, N, which easily bonds with these elements, needs to be fixed by Ti. For this purpose, the molar fraction of N is made smaller than the molar fraction of Ti. In other words, the contents of N and Ti in the steel are adjusted so as to satisfy the above equation (1). ([%N] / 14) / ([%Ti] / 47.9) is preferably 0.6 or less. In addition, in equation (1), [%N] and [%Ti] represent the contents (mass%) of N and Ti in the steel, respectively.
[0029] The balance other than the above-mentioned components is Fe and inevitable impurities. Note that, for the optional components described below, if the content is less than the lower limit, the effect of the present invention is not impaired, so if these optional elements are contained in an amount less than the lower limit, they are treated as inevitable impurities.
[0030] [Optional Components] In addition to the above-described component composition, the plated steel sheet according to this embodiment may further contain, in mass %, at least one element selected from V: 0.100% or less, Mo: 0.500% or less, Cr: 1.00% or less, Cu: 1.00% or less, Ni: 0.50% or less, Sb: 0.200% or less, Sn: 0.200% or less, Ta: 0.200% or less, W: 0.400% or less, Zr: 0.0200% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, Co: 0.020% or less, REM: 0.0200% or less, Te: 0.020% or less, Hf: 0.10% or less, and Bi: 0.200% or less.
[0031] V: 0.100% or less V has the effect of forming fine carbides and increasing strength. If the V content exceeds 0.100%, coarse V carbides may precipitate, resulting in a decrease in delayed fracture resistance. Therefore, when V is contained, the V content is set to 0.100% or less. The V content is preferably 0.080% or less, and more preferably 0.060% or less. There is no particular restriction on the lower limit of the V content, and it may be 0.000%. However, since V has the effect of forming fine carbides and increasing strength, it is preferably set to 0.001% or more. The V content is more preferably 0.005% or more, and even more preferably 0.010% or more.
[0032] Mo: 0.500% or less Mo has the effect of improving hardenability and increasing the area fraction of bainite and martensite. If the Mo content exceeds 0.500%, the effect saturates. Therefore, when Mo is contained, the Mo content is set to 0.500% or less. The Mo content is preferably 0.200% or less, and more preferably 0.150% or less. There is no particular limitation on the lower limit of the Mo content, and it may be 0.000%, but since Mo has the effect of improving hardenability and increasing the area fraction of bainite and martensite, it is preferably 0.010% or more. The Mo content is more preferably 0.020% or more, and even more preferably 0.030% or more.
[0033] Cr: 1.00% or less Cr has the effect of improving hardenability and increasing the area ratio of bainite and martensite. If the Cr content exceeds 1.00%, the effect saturates. Therefore, when Cr is contained, the Cr content is set to 1.00% or less. The Cr content is preferably 0.300% or less, and more preferably 0.250% or less. There is no particular limitation on the lower limit of the Cr content, and it may be 0.000%, but since Cr has the effect of improving hardenability and increasing the area ratio of bainite and martensite, it is preferably 0.01% or more. The Cr content is more preferably 0.015% or more, and even more preferably 0.030% or more.
[0034] Cu: 1.00% or less Cu has the effect of increasing strength through solid solution. Cu also has the effect of improving delayed fracture resistance. If the Cu content exceeds 1.00%, grain boundary cracking is more likely to occur. Therefore, when Cu is contained, the Cu content is set to 1.00% or less. The Cu content is preferably 0.60% or less, and more preferably 0.30% or less. There is no particular limitation on the lower limit of the Cu content, and it may be 0.00%, but since Cu has the effect of increasing strength through solid solution, it is preferably 0.01% or more. The Cu content is more preferably 0.02% or more, and even more preferably 0.05% or more.
[0035] Ni: 0.50% or less Ni has the effect of improving hardenability, but if the Ni content exceeds 0.50%, the effect saturates. Therefore, when Ni is contained, the Ni content is set to 0.50% or less. The Ni content is preferably 0.20% or less, and more preferably 0.15% or less. The lower limit of the Ni content is not particularly limited and may be 0.00%, but since Ni has the effect of improving hardenability, it is preferably 0.01% or more. The Ni content is more preferably 0.02% or more, and even more preferably 0.03% or more.
[0036] Sb: 0.200% or less Sb has the effect of suppressing surface oxidation, nitriding, and decarburization of the steel sheet, but if the Sb content exceeds 0.200%, the effect saturates. Therefore, when Sb is contained, the Sb content is set to 0.200% or less. The Sb content is preferably 0.050% or less, and more preferably 0.020% or less. There is no particular restriction on the lower limit of the Sb content, and it may be 0.000%. However, since Sb has the effect of suppressing surface oxidation, nitriding, and decarburization of the steel sheet, it is preferably set to 0.001% or more. The Sb content is more preferably 0.002% or more, and even more preferably 0.005% or more.
[0037] Sn: 0.200% or less Like Sb, Sn has the effect of suppressing surface oxidation, nitriding, and decarburization of the steel sheet. If the Sn content exceeds 0.200%, the effect saturates. Therefore, when Sn is contained, the Sn content is set to 0.200% or less. The Sn content is preferably 0.050% or less, and more preferably 0.020% or less. There is no particular limitation on the lower limit of the Sn content, and it may be 0.000%, but since Sn has the effect of suppressing surface oxidation, nitriding, and decarburization of the steel sheet, it is preferably 0.001% or more. The Sn content is more preferably 0.002% or more, and even more preferably 0.005% or more.
[0038] Ta: 0.200% or less Ta has the effect of forming fine carbides and increasing strength. If the Ta content exceeds 0.200%, coarse Ta carbides may precipitate, resulting in a decrease in delayed fracture resistance. Therefore, when Ta is contained, the Ta content is set to 0.200% or less. The Ta content is preferably 0.100% or less, and more preferably 0.070% or less. The lower limit of the Ta content is not particularly limited and may be 0.000%, but since Ta has the effect of forming fine carbides and increasing strength, it is preferably set to 0.001% or more. The Ta content is more preferably 0.005% or more, and even more preferably 0.010% or more.
[0039] W: 0.400% or less W has the effect of forming fine carbides and increasing strength. If the W content exceeds 0.400%, coarse W carbides may precipitate, resulting in a decrease in delayed fracture resistance. Therefore, when W is contained, the W content is set to 0.400% or less. The W content is preferably 0.300% or less, and more preferably 0.250% or less. There is no particular restriction on the lower limit of the W content, and it may be 0.000%, but since W has the effect of forming fine carbides and increasing strength, it is preferably set to 0.001% or more. The W content is more preferably 0.005% or more, and even more preferably 0.010% or more.
[0040] Zr: 0.0200% or less Zr has the effect of spheroidizing the shape of inclusions and suppressing stress concentration, thereby improving toughness. If the Zr content exceeds 0.0200%, a large amount of inclusions may be formed, resulting in a decrease in toughness. Therefore, when Zr is contained, the Zr content is set to 0.0200% or less. The Zr content is preferably 0.0150% or less, and more preferably 0.0100% or less. The lower limit of the Zr content is not particularly limited and may be 0.0000%, but since Zr has the effect of spheroidizing the shape of inclusions, suppressing stress concentration, and improving toughness, it is preferably 0.0001% or more. The Zr content is more preferably 0.0010% or more, and even more preferably 0.0020% or more.
[0041] Ca: 0.0200% or less Ca can be used as a deoxidizer. If the Ca content exceeds 0.0200%, a large amount of Ca-based inclusions may be formed, which may result in a decrease in delayed fracture resistance. Therefore, when Ca is contained, the Ca content is set to 0.0200% or less. The Ca content is preferably 0.0100% or less, and more preferably 0.0080% or less. There is no particular restriction on the lower limit of the Ca content, and it may be 0.0000%, but since Ca can be used as a deoxidizer, it is preferably 0.0001% or more. The Ca content is more preferably 0.0005% or more, and even more preferably 0.0010% or more.
[0042] Mg: 0.0200% or less Mg can be used as a deoxidizer. If the Mg content exceeds 0.0200%, a large amount of Mg-based inclusions may be formed, which may reduce delayed fracture resistance. Therefore, when Mg is contained, the Mg content is set to 0.0200% or less. The Mg content is preferably 0.0100% or less, and more preferably 0.0080% or less. There is no particular restriction on the lower limit of the Mg content, and it may be 0.0000%, but since Mg can be used as a deoxidizer, it is preferably 0.0001% or more. The Mg content is more preferably 0.0005% or more, and even more preferably 0.0010% or more.
[0043] Co: 0.020% or less Co has the effect of increasing strength through solid solution strengthening. If the Co content exceeds 0.020%, the effect saturates. Therefore, when Co is contained, the Co content is set to 0.020% or less. The Co content is preferably 0.015% or less, and more preferably 0.010% or less. There is no particular limitation on the lower limit of the Co content, and it may be 0.000%, but since Co has the effect of increasing strength through solid solution strengthening, it is preferably 0.001% or more. The Co content is more preferably 0.002% or more, and even more preferably 0.005% or more.
[0044] REM: 0.0200% or less REM has the effect of spheroidizing the shape of inclusions and suppressing stress concentration, thereby improving toughness. If the REM content exceeds 0.0200%, a large amount of inclusions may be formed, resulting in a decrease in toughness. Therefore, when REM is contained, the REM content is set to 0.0200% or less. The REM content is preferably 0.0100% or less, and more preferably 0.0050% or less. There is no particular restriction on the lower limit of the REM content, and it may be 0.0000%, but since REM has the effect of spheroidizing the shape of inclusions and suppressing stress concentration, thereby improving toughness, it is preferably set to 0.0001% or more. The REM content is more preferably 0.0005% or more, and even more preferably 0.0010% or more. Here, REM refers to scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanoid elements ranging from lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. The REM concentration refers to the total content of one or more elements selected from the above-mentioned REM. The REM preferably contains La, Ce, and Nd.
[0045] Te: 0.020% or less Te has the effect of spheroidizing the shape of inclusions and suppressing stress concentration, thereby improving toughness. If the Te content exceeds 0.020%, a large amount of inclusions may be formed, resulting in a decrease in toughness. Therefore, when Te is contained, the Te content is set to 0.020% or less. The Te content is preferably 0.015% or less, and more preferably 0.010% or less. There is no particular lower limit for the Te content, and it may be 0.000%, but since Te has the effect of spheroidizing the shape of inclusions and suppressing stress concentration, thereby improving toughness, it is preferably set to 0.001% or more. The Te content is more preferably 0.002% or more, and even more preferably 0.004% or more.
[0046] Hf: 0.10% or less Hf has the effect of spheroidizing the shape of inclusions and suppressing stress concentration, thereby improving toughness. If the Hf content exceeds 0.10%, a large amount of inclusions is formed, resulting in a decrease in toughness. Therefore, when Hf is contained, the Hf content is set to 0.10% or less. The Hf content is preferably 0.08% or less, and more preferably 0.05% or less. There is no particular lower limit for the Hf content, and it may be 0.00%, but since Hf has the effect of spheroidizing the shape of inclusions, suppressing stress concentration, and improving toughness, it is preferably set to 0.01% or more.
[0047] Bi: 0.200% or less Bi has the effect of reducing segregation and improving bendability. If the Bi content exceeds 0.200%, a large amount of inclusions may form, resulting in reduced bendability. Therefore, when Bi is contained, the Bi content is set to 0.200% or less. The Bi content is preferably 0.100% or less, more preferably 0.050% or less. The Bi content is further preferably 0.010% or less, and even more preferably 0.005% or less. There is no particular lower limit for the Bi content, and it may be 0.000%, but because Bi has the effect of reducing segregation and improving bendability, it is preferably 0.001% or more. The Bi content is more preferably 0.002% or more, and even more preferably 0.003% or more.
[0048] [Steel Structure] Next, the steel structure of the steel plate will be described.
[0049] Sum of area fractions of martensite and bainite: 95.0% or more Both martensite and bainite are hard phases and are necessary to achieve a TS of 1180 MPa or more. Therefore, the sum of the area fractions of martensite and bainite is set to 95.0% or more. The sum of the area fractions of martensite and bainite is preferably 96.0% or more. Because ferrite forms from grain boundaries with non-uniform B concentration, the upper limit of the sum of the area fractions of martensite and bainite is 99.8%.
[0050] Area fraction of retained austenite: 4.8% or less Retained austenite may be contained as a residual structure other than martensite and bainite. Therefore, the area fraction of retained austenite is set to 4.8% or less. More preferably, it is 4.7% or less, and even more preferably, it is 4.5% or less. Furthermore, the area fraction of retained austenite is preferably 4% or less. More preferably, it is 3.8% or less, even more preferably, it is 3.7% or less, and even more preferably, it is 3.5% or less. The area fraction of retained austenite may be 0% or may exceed 0%.
[0051] Ferrite area fraction: 0.2% or more and 3.0% or less Ferrite forms from austenite grain boundaries with non-uniform B concentration. If the ferrite area fraction is 0.2% or more, the B concentration at prior austenite grain boundaries where ferrite is not formed is sufficiently high, resulting in good delayed fracture resistance. Therefore, the ferrite area fraction is set to 0.2% or more. The ferrite area fraction is preferably set to 0.3% or more, and more preferably set to 0.5% or more. On the other hand, if the ferrite area fraction exceeds 3.0%, the strength decreases. Therefore, the ferrite area fraction is set to 3% or less. The ferrite area fraction is preferably set to 2.5% or less, and more preferably set to 2.0% or less.
[0052] Here, the area ratio of each structure is measured as follows. The area ratio of retained austenite is determined by chemically polishing the rolled surface of a test piece taken from each steel plate up to the t / 4 position in the plate thickness of the steel plate, measuring the X-ray diffraction intensity and diffraction peak position of the polished surface using an X-ray diffraction (XRD) device, calculating the volume ratio, and using this number as the area ratio of retained austenite. Next, a cross section of the plate thickness parallel to the rolling direction of each steel plate is polished and then corroded with 3 vol% nital, and the t / 4 position in the plate thickness is used as the observation surface. SEM images of the observation surface are taken at a magnification of 2000 times, with a field of view of 57.1 μm × 42.9 μm, and from three fields of view. The obtained SEM images are analyzed to determine the total area ratio of martensite, bainite, and retained austenite, as well as the area ratio of the structure other than martensite, bainite, and retained austenite (ferrite). The area fractions of martensite and bainite are calculated by subtracting the area fraction of retained austenite obtained by XRD from the area fractions of martensite, bainite, and retained austenite obtained by image analysis. The average value of the three fields of view is taken as the area fraction of the structure.
[0053] Prior austenite grain size: 10 μm or less Complicating the crack propagation path can improve delayed fracture resistance. To achieve this effect, the prior austenite grain size must be 10 μm or less. Therefore, the prior austenite grain size is 10 μm or less. The prior austenite grain size is preferably 9 μm or less. There is no particular lower limit for the grain size of the prior austenite grains, but from the viewpoint of production technology, the prior austenite grain size is preferably 1 μm or more. Furthermore, the prior austenite grain size is more preferably 2 μm or more, and even more preferably 3 μm or more.
[0054] Here, the grain size of the prior austenite grains is measured as follows. A cross section of each steel sheet parallel to the rolling direction is polished and then etched with picral to obtain an observation surface. On the observation surface, the microstructure at a position t / 4 of the sheet thickness is photographed with an SEM at a magnification of 2000 times, with a field of view of 57.1 μm × 42.9 μm, and three fields of view are obtained to obtain SEM images. The grain size of each prior austenite grain is determined from the obtained structural image by image analysis, and the average value of the three fields of view is taken as the grain size (average crystal grain size) of the prior austenite grains.
[0055] B concentration at prior austenite grain boundaries between adjacent martensite structures: 0.05% or more by mass. B segregates at prior austenite grain boundaries, strengthening the grain boundaries and improving delayed fracture resistance. The above-mentioned effects can be achieved when the B concentration at prior austenite grain boundaries is 0.05% or more by mass. Therefore, the B concentration at prior austenite grain boundaries between adjacent martensite structures (prior austenite grain boundaries sandwiched between martensite structures) is set to 0.05% or more by mass. The B concentration at prior austenite grain boundaries is preferably 0.07% or more by mass, and more preferably 0.10% or more by mass. While there is no upper limit to the B concentration at prior austenite grain boundaries, it is preferably less than 6% in order to effectively prevent the precipitation of hard carboborides on the grain boundaries and further improve delayed fracture resistance. More preferably, it is 2% or less by mass.
[0056] Variation in the B concentration within the same grain boundary at the prior austenite grain boundary between adjacent martensite: less than 0.010% by mass. To improve delayed fracture resistance, it is important that the B concentration on the grain boundary be uniform regardless of the grain boundary. Variations of 0.010% or more result in strength differences within the grain boundary, making cracks more likely to occur in areas with locally low B concentration, thereby reducing the delayed fracture resistance. Therefore, the variation in the B concentration within the same grain boundary at the prior austenite grain boundary between adjacent martensite (prior austenite grain boundary sandwiched between martensite structures) is set to less than 0.010% by mass. The variation is preferably 0.009% or less by mass, and more preferably 0.008% or less by mass. While smaller variations are preferable, a variation of 0.001% or more is sufficient from the viewpoint of production technology. Moreover, the grain boundary where B segregation contributes to improving delayed fracture resistance is a grain boundary where both sides are martensite.
[0057] Variation in B concentration within the same grain boundary at prior austenite grain boundaries between martensite and ferrite: 0.010% or more by mass By forming a grain boundary between martensite and ferrite, the B concentration at the prior austenite grain boundary sandwiched between martensite on both sides can be made 0.05% by mass or more. If the variation in B concentration within the same grain boundary at prior austenite grain boundaries between martensite and ferrite is less than 0.010%, ferrite will not form. Therefore, the variation in B concentration within the same grain boundary at prior austenite grain boundaries between martensite and ferrite (prior austenite grain boundaries sandwiched between martensite and ferrite) is set to 0.010% or more by mass. The variation is preferably 0.012% or more by mass, and more preferably 0.014% or more by mass. Although there is no particular upper limit, the variation is preferably 0.200% or less in mass %, and more preferably 0.100% or less in mass %.
[0058] Here, the B concentration and variation at the prior austenite grain boundary are measured as follows. A needle-shaped sample is prepared from a region including the prior austenite grain boundary using the SEM-FIB (Focused Ion Beam) method. 3DAP analysis is performed on the obtained needle-shaped sample using a 3DAP device (LEAP4000XSi, manufactured by AMETEK). Measurement is performed in laser mode. The sample temperature is 80 K or less. The B concentration at the prior austenite grain boundary is determined from the number of B ions and the number of other ions detected at the prior austenite grain boundary. The B concentration is taken as the average value of two samples. Five non-overlapping circular regions with a diameter of 5 nm to 10 nm are set on the surface of the measured prior austenite grain boundary, and a cylindrical volume extending in the normal direction to the grain boundary is set for each circle. The B concentration at the grain boundary is determined for each cylinder, and the standard deviation is taken as the variation in B concentration. In the above measurement, since the prior austenite grain size is very large compared to the area sampled by the SEM-FIB method, all grain boundaries targeted by a single sample are the same grain boundary. For example, while the prior austenite grain size is about 9 μm, the sample area is about 0.1 μm in diameter. Therefore, the variation in the obtained B concentration is a variation within the same grain boundary. Furthermore, whether or not a prior austenite grain boundary exists between martensite and ferrite can be confirmed by observing the SEM image using the above-mentioned method. Furthermore, whether or not a prior austenite grain boundary exists between adjacent martensite can also be confirmed by observing the SEM image using the above-mentioned method.
[0059] According to the present invention, it is possible to provide a plated steel sheet having a tensile strength of 1180 MPa or more. The tensile strength of the plated steel sheet is preferably 1250 MPa or more.
[0060] The above-mentioned plated steel sheet has a plating layer formed on at least one surface of the steel sheet. The plating layer is preferably any one of a hot-dip galvanized layer, a galvannealed hot-dip galvanized layer, and an electrogalvanized layer. The composition of the plating layer is not particularly limited and may be a known composition.
[0061] The composition of the hot-dip galvanized layer is not particularly limited, and may be any common composition. In one example, the coating layer contains 20 mass% or less of Fe, 0.001 mass% to 1.0 mass% of Al, and further contains 0 mass% to 3.5 mass% in total of one or more elements selected from the group consisting of Pb, Sb, Si, Sn, Mg, Mn, Ni, Cr, Co, Ca, Cu, Li, Ti, Be, Bi, and REM, with the balance being Zn and unavoidable impurities. When the coating layer is a hot-dip galvanized layer, the Fe content in the coating layer is, in one example, less than 7 mass%, and when the coating layer is an alloyed hot-dip galvanized layer, the Fe content in the coating layer is, in one example, 7 mass% to 15 mass%, more preferably 8 mass% to 13 mass%.
[0062] The coating weight is not particularly limited, but the coating weight per one side of the plated steel sheet is 20 to 80 g / m 2 In one example, the plating layer is formed on both the front and back surfaces of a steel sheet (high-strength cold-rolled steel sheet).
[0063] Next, a method for producing a plated steel sheet will be described. a cold rolling process in which the hot-rolled sheet after the pickling process is cold-rolled to form a cold-rolled sheet; a first annealing process in which the cold-rolled sheet is heated to a first heating temperature of Ac3 point or higher; a cooling process in which cooling of the cold-rolled sheet after the first annealing process is started from the first heating temperature and cooled to a cooling stop temperature of 100°C or higher and lower than the Ms point at an average cooling rate of 50°C / s or higher; a reheating process in which, after the cooling process, the cold-rolled sheet is heated to a reheating temperature of 300°C or higher and 400°C or lower and held at the reheating temperature for 60 seconds or longer to cool to room temperature; a subzero treatment process in which, after the reheating process, a subzero treatment is performed; a second annealing process in which, after the subzero treatment process, the steel sheet is heated to a second heating temperature of Ac3 point or higher to obtain a steel sheet; and a plating process in which the steel sheet is plated to form a plated steel sheet.
[0064] First, a steel slab having the above-described chemical composition is manufactured. Here, an example of the manufacturing conditions for the steel slab before the hot rolling process is described. First, a steel material is melted to produce molten steel having the above-described chemical composition. The melting method is not particularly limited, and any known melting method, such as converter melting or electric furnace melting, is suitable. The resulting molten steel is solidified to produce a steel slab. The method for producing a steel slab from molten steel is not particularly limited, and a continuous casting method, an ingot casting method, a thin slab casting method, or the like can be used. The steel slab may be cooled and then reheated before hot rolling, or the cast steel slab may be continuously hot rolled without being cooled to room temperature. The slab heating temperature is preferably 1100°C or higher and 1300°C or lower, taking into account the rolling load and scale generation. The slab heating method is not particularly limited, and for example, it can be heated in a heating furnace according to a conventional method.
[0065] [Hot Rolling Process] The above-described steel slab is hot rolled to obtain a hot-rolled sheet. There are no particular limitations on the hot rolling, and it may be carried out according to a conventional method. There are also no particular limitations on the cooling after hot rolling, and it is cooled to the coiling temperature. Next, the hot-rolled sheet is wound into a coil. The coiling temperature is preferably 400°C or higher. This is because a coiling temperature of 400°C or higher facilitates coiling without increasing the strength of the hot-rolled sheet. The coiling temperature is more preferably 550°C or higher. Furthermore, in order to suitably prevent the formation of thick scale and further improve yield, the coiling temperature is preferably 750°C or lower. Note that the hot-rolled sheet may be heat-treated for the purpose of softening before pickling.
[0066] [Pickling Process] After the hot rolling process, the hot-rolled sheet is pickled in the pickling process. In the pickling process, scale can be removed from the hot-rolled sheet wound around a coil. There are no particular restrictions on the method for removing the scale, but in order to completely remove the scale, it is preferable to perform pickling while uncoiling the hot-rolled coil. There are no particular restrictions on the pickling method, and a conventional method may be used.
[0067] [Cold Rolling Step] After the pickling step, the hot rolled sheet is cold rolled in the cold rolling step to obtain a cold rolled sheet. For example, the hot rolled sheet from which the scale has been removed is appropriately cleaned and then cold rolled to obtain a cold rolled sheet. The cold rolling method is not particularly limited and may be a conventional method.
[0068] [First Annealing Step: Heating to a First Heating Temperature of Ac3 Point or Higher] Next, in the first annealing step, the cold-rolled sheet is heated to a first heating temperature of Ac3 point or higher and annealed in the austenite single-phase region. If the first heating temperature is lower than Ac3 point, ferrite is generated. This ferrite has fewer dislocations during annealing, and there are no dislocations that serve as diffusion paths for B (boron) during the second annealing, making it difficult to uniformly segregate boron. Furthermore, excessive heating increases the austenite grain size to more than 10 μm. Therefore, the first heating temperature is set to Ac3 point or higher. The first heating temperature is preferably Ac3 point + 10°C or higher, more preferably Ac3 point + 15°C or higher. Since the austenite structure generated in the second annealing has the same crystalline structure as the austenite structure generated in the first annealing, the first heating temperature is preferably set to 980°C or lower so that the austenite grain size is 10 μm or lower even during the first annealing. The first heating temperature is more preferably 950°C or lower. The Ac3 point is calculated using the following formula: Ac3 (°C) = 881 - 206 x [%C] + 53 x [%Si] - 15 x [%Mn] - 27 x [%Cu] - 20 x [%Ni] - 1 x [%Cr] + 41 x [%Mo] (In the above formula, [%M] is the content (mass%) of element M in the steel sheet, and the value of an element that is not contained is 0 (zero).)
[0069] [Cooling process: Cooling is initiated from the first heating temperature and cooled at an average cooling rate of 50°C / s or more to a cooling stop temperature of 100°C or higher but lower than the Ms point.] [Reheating process: Heat to a reheating temperature of 300°C or higher but lower than 400°C, hold at the reheating temperature for 60 seconds or longer, and then cool to room temperature.] After the first annealing process, the cold-rolled sheet is subjected to partial quenching and partitioning in the cooling process to create a structure in which retained austenite exists at the prior austenite grain boundaries. If the cooling stop temperature for partial quenching is lower than 100°C, martensitic transformation occurs before C partitioning occurs, making it impossible to obtain a sufficient amount of retained austenite before the second annealing. If the amount of retained austenite is insufficient, austenite with a different orientation from that in the first annealing is generated, making it difficult to uniformly segregate B (boron) at the grain boundaries of such austenite. Therefore, the cooling stop temperature in the cooling process is set to 100°C or higher. The cooling stop temperature is preferably 120°C or higher, and more preferably 150°C or higher. On the other hand, if the cooling stop temperature is above the Ms point, martensitic transformation does not occur, carbon distribution does not occur during subsequent reheating, and retained austenite is not formed before the second annealing. If the amount of retained austenite is insufficient, austenite with a different orientation than that formed during the first annealing will be formed, making it difficult to uniformly segregate B (boron) at the grain boundaries of such austenite. Therefore, the cooling stop temperature in the cooling process is set to below the Ms point. The cooling stop temperature is preferably the Ms point minus 10°C or lower, and more preferably the Ms point minus 20°C or lower. The Ms point is calculated using the following formula: Ms (°C) = 499 - 308 x [C] - 10.8 x [Si] - 32.4 x [Mn] - 16.2 x [Ni] - 27 x [Cr] - 10.8 x [Mo] (In the above formula, [M] is the content (mass%) of element M in the steel sheet, and the value of an element that is not contained is 0 (zero).)
[0070] If the average cooling rate is less than 50°C / s, ferrite transformation occurs. Because this ferrite contains almost no dislocations, this ferrite transformation slows down the diffusion of boron during the second annealing, resulting in insufficient boron concentration at grain boundaries in the final structure. Therefore, the average cooling rate is set to 50°C / s or more. The average cooling rate is preferably 60°C / s or more, more preferably 70°C / s or more. There is no particular limit to the upper limit of the average cooling rate, but if the cooling rate is too high, it becomes difficult to control the first cooling stop temperature. Therefore, the average cooling rate is preferably 1000°C / s or less, more preferably 200°C / s or less. The average cooling rate (°C / s) in the cooling step is "(first heating temperature (°C)) - (cooling stop temperature (°C)) / (cooling time (seconds) from the first heating temperature (°C) to the cooling stop temperature (°C))".
[0071] If the reheating temperature is less than 300°C, carbon distribution will be insufficient, and retained austenite will not be formed before the second annealing. If the amount of retained austenite is insufficient, austenite with a different orientation from that in the first annealing will be formed, and it will be difficult to uniformly segregate B (boron) at the grain boundaries of such austenite. Therefore, the reheating temperature is set to 300°C or higher. The reheating temperature is preferably 310°C or higher, and more preferably 320°C or higher. On the other hand, if the reheating temperature exceeds 400°C, untransformed austenite will decompose into cementite, and retained austenite will not be formed before the second annealing. If the amount of retained austenite is insufficient, austenite with a different orientation from that in the first annealing will be formed, and it will be difficult to uniformly segregate B (boron) at the grain boundaries of such austenite. Therefore, the reheating temperature is set to 400°C or lower. The reheating temperature is preferably 390°C or lower, and more preferably 380°C or lower.
[0072] Furthermore, if the holding time at the reheating temperature (reheating holding time) is less than 60 seconds, carbon distribution is insufficient and retained austenite is not formed before the second annealing. If the amount of retained austenite is insufficient, austenite with a different orientation from that in the first annealing is formed, and it is difficult to uniformly segregate B (boron) at the grain boundaries of such austenite. Therefore, the holding time at the reheating temperature is set to 60 seconds or more. The holding time is preferably 80 seconds or more, more preferably 100 seconds or more. Furthermore, the holding time at the reheating temperature is preferably 900 seconds or less, more preferably 600 seconds or less. After holding at the reheating temperature, the steel is cooled to room temperature. Here, the room temperature, which is the cooling stop temperature in the reheating step, is not particularly limited, but can be set to 5 to 50°C.
[0073] [Subzero Treatment Step] Subzero treatment transforms massive retained austenite to obtain martensite with enriched carbon. From this obtained martensite, new austenite with a different orientation from the first treatment is nucleated, resulting in grain boundaries with non-uniform boron concentrations. Film-like retained austenite remains even after this treatment, and subsequent annealing forms an austenite structure with the same crystal orientation as the first austenite, with boron enriched and uniform at the grain boundaries. While the specific conditions for the subzero treatment are not particularly limited, it is preferable to immerse the cold-rolled sheet after the reheating step in liquid nitrogen (−196°C) for 30 minutes or more. It is also preferable to immerse the cold-rolled sheet in liquid nitrogen for 3 hours or less.
[0074] [Second Annealing Step: Heating to a Second Heating Temperature of Ac3 Point or Higher] In the second annealing step, the steel sheet (cold-rolled sheet) obtained as described above is again heated to a second heating temperature of Ac3 point or higher and annealed. During this process, austenite having the same orientation as the austenite formed in the first annealing is formed using film-like retained austenite as nuclei. During this formation process, B (boron) dissolved through dislocations in martensite before austenite transformation rapidly diffuses to the austenite grain boundaries, resulting in uniform boron segregation. If the second heating temperature is lower than the Ac3 point, ferrite is formed and strength is reduced. Therefore, the second heating temperature is set to the Ac3 point or higher. The second heating temperature is preferably the Ac3 point + 10°C or higher, more preferably the Ac3 point + 15°C or higher. On the other hand, excessive heating increases the austenite grain size to more than 10 μm, resulting in reduced delayed fracture properties. Therefore, the second heating temperature is preferably 980°C or lower. The second heating temperature is more preferably 950°C or lower.
[0075] [Plating step, alloying step] After the second annealing step described above, a plating step is performed in which at least one surface of the steel sheet is plated to obtain a plated steel sheet. After the plating step, in an alloying step, the plated steel sheet (high-strength plated steel sheet) may be heat-treated to alloy the plating layer of the plated steel sheet to obtain an alloyed plated steel sheet. Note that production conditions other than those described above can be performed according to conventional methods.
[0076] The plated steel sheet according to this embodiment obtained as described above preferably has a thickness of 0.5 mm or more, and more preferably 2.0 mm or less.
[0077] [Component] In this embodiment, a component can be provided that is at least partially made from the above-described plated steel sheet. In one example, the above-described plated steel sheet can be formed into a desired shape by press working to produce an automotive component. Note that the automotive component may contain, as a raw material, a steel sheet other than the plated steel sheet according to this embodiment. According to this embodiment, a plated steel sheet having a TS of 1180 MPa or more and excellent delayed fracture resistance and platability can be provided. Therefore, a component having a TS of 1180 MPa or more and excellent delayed fracture resistance and platability can be provided. The steel sheet according to this embodiment can be suitably used as an automotive component that contributes to weight reduction of the vehicle body. The plated steel sheet according to this embodiment can be suitably used in general automotive components, particularly components used as frame structural components or reinforcing components.
[0078] The method for manufacturing the above-mentioned member includes a step of subjecting the above-mentioned plated steel sheet to at least one of forming and joining to form the member. The forming can be performed by any common processing method, such as press working, without any restrictions. The joining can be performed by any common welding method, such as spot welding or arc welding, or by riveting or caulking, without any restrictions.
[0079] A steel having the chemical composition shown in Table 1, with the balance being Fe and unavoidable impurities, was melted in a converter to form a steel slab. The resulting slab was reheated, hot-rolled, and coiled to obtain a hot-rolled coil (hot-rolled sheet). The hot-rolled coil was then pickled while uncoiling, and cold-rolled to obtain a cold-rolled sheet. The thickness of the hot-rolled sheet was 3.0 mm, and the thickness of the cold-rolled sheet was 1.2 mm. Annealing (first annealing step, cooling step, reheating step, subzero treatment step, second annealing step) was performed in a continuous hot-dip galvanizing line under the conditions shown in Table 2 to obtain plated steel sheets (hot-dip galvanized steel sheet (GI), galvannealed steel sheet (GA)). The hot-dip galvanized steel sheet was immersed in a galvanizing bath at 460°C, and a galvannealing rate of 35 g / m per side was applied. 2 The coating weight of the galvannealed steel sheet was 45 g / m per side. 2After adjusting the coating weight to 1000 ppm, the steel sheets were subjected to alloying treatment by holding at 520°C for 40 seconds. Note that sub-zero treatment was performed on all steel sheets except for Steel Sheet No. 6, which was immersed in liquid nitrogen (-196°C) for 60 minutes.
[0080]
[0081]
[0082] The steel sheets thus obtained were evaluated for the total area fraction of martensite and bainite, the area fraction of retained austenite, the area fraction of ferrite, the prior austenite grain size, the B concentration at the prior austenite grain boundaries between adjacent martensite grains, and the variation in the B concentration at the prior austenite grain boundaries within the same grain boundary (the variation in the B concentration at the prior austenite grain boundaries between adjacent martensite grains within the same grain boundary, and the variation in the B concentration at the prior austenite grain boundaries between martensite and ferrite within the same grain boundary) according to the methods described above. Furthermore, the tensile strength and delayed fracture resistance were evaluated according to the methods described below. The results are shown in Table 3.
[0083] [Tensile test] The obtained steel sheets were subjected to a tensile test in accordance with JIS Z 2241 (2011). JIS No. 5 tensile test pieces were taken with the longitudinal direction perpendicular to the rolling direction, and the tensile test was performed to measure the tensile strength (TS). A tensile strength TS of 1180 MPa or more was determined to be good.
[0084] [Delayed fracture test] The delayed fracture resistance of the steel sheets was evaluated as follows. A 30 mm × 110 mm test piece was taken from the obtained steel sheet, with the rolling direction as the longitudinal direction. A strain gauge was attached to this test piece, and it was bent at 90 degrees in a V-shape with a curvature radius of 7 mmR (R / t = 5.0). The opposing sheet surfaces were clamped together, and the tensile stress of the surface layer of the test piece was set to 1800 MPa to obtain a test piece for evaluating delayed fracture resistance. This test piece for evaluating delayed fracture resistance was immersed in a hydrochloric acid solution of pH 3, and the presence or absence of cracks after 100 hours was examined. Steel sheets that did not develop cracks after 100 hours were judged to have good delayed fracture resistance. In the table, steel sheets that did not develop cracks after 100 hours were rated as "excellent" in delayed fracture resistance, and other steel sheets were rated as "poor" in delayed fracture resistance.
[0085] [Evaluation of platability] For platability, each plated steel sheet was visually inspected for the presence or absence of unplated areas, and those without unplated areas were deemed to have good platability. In the table, steel sheets that were judged to have good platability were indicated as "excellent," and steel sheets that were judged to have poor platability were indicated as "poor."
[0086]
[0087] As can be seen from Table 3, the inventive examples have a tensile strength TS of 1180 MPa or more, and are excellent in delayed fracture resistance and platability. On the other hand, the comparative examples are inferior in at least one of tensile strength TS, delayed fracture resistance, and platability.
[0088] Furthermore, it was found that the steel sheets of the present invention were used to prepare members obtained by forming, joining, and further by forming and joining, and that they had high strength and excellent delayed fracture resistance and platability, similar to the steel sheets of the present invention, because the steel sheets of the present invention had high strength and excellent delayed fracture resistance and platability.
Claims
1. A steel sheet comprising, by mass%, C: 0.10% or more and 0.30% or less, Si: over 1.20% and 2.00% or less, Mn: 2.5% or more and 4.0% or less, P: 0.050% or less, S: 0.020% or less, Al: 0.10% or less, N: 0.01% or less, Ti: 0.100% or less, Nb: 0.002% or more and 0.050% or less, and B: 0.0008% or more and less than 0.0015%, and having a component composition which satisfies the following formula (1) with the balance consisting of Fe and unavoidable impurities, the sum of the area ratios of martensite and bainite being 95.0% or more, the area ratio of retained austenite being 4.8% or less, the area ratio of ferrite being 0.2% or more and 3.0% or less, and the prior austenite grain size being 10 μm or less, A plated steel sheet comprising: a steel sheet in which the B concentration of prior austenite grain boundaries between adjacent martensite is 0.05% or more by mass, the variation in the B concentration of prior austenite grain boundaries between adjacent martensite is less than 0.010% by mass, and the variation in the B concentration of prior austenite grain boundaries between martensite and ferrite is 0.010% or more by mass, and a plating layer formed on at least one surface of the steel sheet. ([%N] / 14) / ([%Ti] / 47.9)<1.0...Equation (1) In Equation (1), [%N] and [%Ti] respectively represent the N and Ti contents (mass%) in the steel.
2. The plated steel sheet according to claim 1, wherein the chemical composition further contains, by mass%, at least one selected from V: 0.100% or less, Mo: 0.500% or less, Cr: 1.00% or less, Cu: 1.00% or less, Ni: 0.50% or less, Sb: 0.200% or less, Sn: 0.200% or less, Ta: 0.200% or less, W: 0.400% or less, Zr: 0.0200% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, Co: 0.020% or less, REM: 0.0200% or less, Te: 0.020% or less, Hf: 0.10% or less, and Bi: 0.200% or less.
3. A member made using the plated steel sheet according to claim 1 or 2.
4. A hot rolling process in which a steel slab having the composition according to claim 1 or 2 is hot-rolled to obtain a hot-rolled sheet; a pickling process in which the hot-rolled sheet is pickled; a cold rolling process in which the hot-rolled sheet after the pickling process is cold-rolled to obtain a cold-rolled sheet; a first annealing process in which the cold-rolled sheet is heated to a first heating temperature of Ac3 point or higher; a cooling process in which cooling is started from the first heating temperature and cooled to a cooling stop temperature of 100°C or higher and lower than the Ms point at an average cooling rate of 50°C / s or higher for the cold-rolled sheet after the first annealing process; a reheating process in which, after the cooling process, the cold-rolled sheet is heated to a reheating temperature of 300°C or higher and 400°C or lower, and held at the reheating temperature for 60 seconds or more while being cooled to room temperature; a subzero treatment process in which, after the reheating process, a subzero treatment is performed; and a second annealing process in which, after the subzero treatment process, the sheet is heated to a second heating temperature of Ac3 point or higher to obtain a steel sheet. and a plating step of subjecting the steel sheet to a plating treatment to obtain a plated steel sheet.
5. The method for producing plated steel sheet according to claim 4, further comprising an alloying step of subjecting the plated steel sheet to an alloying treatment after the plating step.
6. A method for manufacturing a component, comprising the step of subjecting the plated steel sheet according to claim 1 or 2 to at least one of forming and joining to form the component.
Citation Information
Patent Citations
High formability super strength cold-roll steel sheet or steel strip, and manufacturing method therefor
US20170298466A1
Hot-dip zinc-coated steel sheet and method for manufacturing same
WO2020162561A1
Steel sheet, member, method for producing said steel sheet, and method for producing said member
WO2023008003A1
High strength steel sheet, high strength plated steel sheet, methods for producing these, and member
WO2023032423A1
High-strength steel plate, high-strength plated steel plate, method for producing same, and member
WO2023032424A1