Polyester fiber and tricot nitted fabric

The use of an eccentric core-sheath cross-section polyester fiber with specific structural parameters addresses the crimp alignment and unevenness issues in tricot knitted fabrics, achieving superior abrasion resistance and stretchability.

WO2024203518A1PCT designated stage expired Publication Date: 2024-10-03TORAY INDUSTRIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010476
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing tricot knitted fabrics face issues with crimp alignment and unevenness due to the round cross-section of typical eccentric core-sheath composite fibers, leading to poor stretchability and abrasion resistance, while side-by-side type modified cross-sections lack balance between crimp and abrasion resistance.

Method used

A polyester fiber with an eccentric core-sheath cross-section having a degree of irregularity (Y/X) between 1.1 and 3.0, a core-to-sheath ratio (L/X) of 2.6 to 5.0, and an interface unevenness of 15% or less, utilizing polytrimethylene terephthalate or polybutylene terephthalate as the high shrinkage core and ethylene terephthalate as the low shrinkage sheath, which disperses stress and maintains crimpability.

Benefits of technology

The solution provides high-quality tricot knitted fabrics with excellent abrasion resistance and stretchability, preventing crimp coil alignment and maintaining fabric quality under friction or impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010476_03102024_PF_FP_ABST
    Figure JP2024010476_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a polyester fiber capable of realizing a tricot knitted fabric that prevents the occurrence of vertical streaks when knitted into a tricot fabric by dispersing the crimp of individual yarns without having to align the crimp phases, and that has excellent abrasion resistance and stretchability. The present invention is a polyester fiber having an eccentric core-sheath cross-section in the fiber cross-section, wherein a degree of deformation (Y / X) calculated by a major diameter Y and a minor diameter X which is orthogonal to Y and which passes through the centroid of the fiber is 1.2 to 3.0 in a deformation cross-section, the ratio L / X of the minor diameter X and the circumference L of the core section is 2.6 to 5.0, and the degree of irregularity at the interface of the core section is 15% or less. Interface irregularity: a value indicated by the following equation, where W is a straight line passing through the most convex point of the core contour on the side where the thickness of the sheath is the greatest and parallel to the minor diameter X, and Z is the distance between line X and line W. Degree of irregularity = Z / X × 100
Need to check novelty before this filing date? Find Prior Art

Description

Polyester and tricot knit fabrics

[0001] The present invention relates to a polyester fiber and a tricot knit fabric. More specifically, the present invention relates to a composite cross-section fiber made of two types of polyester polymers, and to a tricot knit fabric that has excellent abrasion resistance, high quality, and excellent stretchability.

[0002] In recent years, among woven and knitted fabrics, there has been a strong demand for stretch woven and knitted fabrics that offer a comfortable wearing experience. To satisfy this demand, many woven and knitted fabrics have been used that have been given stretchability by blending polyurethane-based fibers with polyester-based fibers, for example. However, polyurethane-based fibers have problems such as being difficult to dye with disperse dyes used for polyester-based fibers, making the dyeing process complicated, and becoming embrittled over long-term use, resulting in a decrease in stretchability. To avoid these drawbacks, crimped polyester-based fiber yarns have been used instead of polyurethane-based fibers.

[0003] Polyester fibers containing polytrimethylene terephthalate (hereinafter referred to as PTT) as the main component have high elongation recovery and low Young's modulus, resulting in excellent soft stretchability. By using this PTT in side-by-side or eccentric core-sheath type composite fibers, soft stretchable fabrics can be produced, and PTT-based composite fibers are being actively researched and developed for a wide range of applications, from clothing to non-clothing.

[0004] For example, the invention described in Patent Document 1 proposes an aromatic polyester conjugate fiber that disperses stress acting on the yarn by increasing the interfacial perimeter of the sea-island component, and has excellent abrasion resistance and interfacial peeling resistance, as well as latent crimping ability suitable for stretch fabrics.

[0005] Furthermore, the invention described in Patent Document 2 proposes a bulky polyester composite yarn that is a raw yarn with a side-by-side or eccentric core-sheath cross section, has excellent crimp development ability like a false-twisted yarn, and has soft stretchability when made into a fabric.

[0006] Furthermore, the invention described in Patent Document 3 proposes a spunbond nonwoven fabric that is bulky and flexible by taking advantage of the high crimp properties of eccentric core-sheath composite fibers or bimetallic composite fibers, at least one of which is made of polybutylene terephthalate.

[0007] Japanese Patent Publication No. 2018-9261 Japanese Patent Publication No. 2002-61031 Japanese Patent Publication No. 2003-13354

[0008] However, the composite fiber described in Patent Document 1 is a typical eccentric sheath-core yarn with a round cross section, and although it exhibits high crimping performance specific to side-by-side or eccentric sheath-core composite fibers, when crimping occurs, the crimping torque causes the crimped coils of each single yarn to align in the same direction, resulting in the multifilament becoming one large spring coil.When made into a tricot knitted fabric, the coil protrudes between the loops of the surface fabric, resulting in a problem of deterioration in warp strength quality.

[0009] Furthermore, although the composite fiber described in Patent Document 2 proposes a side-by-side type modified cross section, it does not propose an eccentric core-sheath type modified cross section, and no proposal has been made for a cross section that achieves both abrasion resistance and warp strength quality of a tricot knitted fabric.

[0010] Furthermore, although the conjugate fiber described in Patent Document 3 exhibits high crimping properties in a spunbond nonwoven fabric made of an eccentric core-sheath type or bimetal type conjugate fiber, there is no description of the difference in viscosity between the two polyester polymers or the design of a discharge hole meter, and the unevenness at the polymer interface increases, so it is not possible to obtain the stretchability required for a tricot knitted fabric.

[0011] The present invention solves the above-mentioned problems and provides a polyester fiber that has an eccentric core-sheath modified cross section in which the crimp phases of the single yarns are not aligned after heat treatment and the crimps are spread out, making it possible to provide a tricot knitted fabric that is high quality, has excellent abrasion resistance and stretchability, and is less likely to develop warp streaks when made into a tricot knitted fabric.

[0012] The above problems are solved by the following means: (1) A polyester fiber having an eccentric sheath-core cross section, wherein the cross section of the polyester fiber has an irregular cross section with a degree of irregularity (Y / X) calculated from the major axis Y and the minor axis X, which is perpendicular to the major axis Y and passes through the center of gravity of the fiber, of 1.1 to 3.0, the ratio L / X of the minor axis X to the circumferential length L of the core being 2.6 to 5.0, and the irregularity at the interface of the core being 15% or less. Irregularity: A value expressed by the following formula, where W is a line parallel to the minor axis X and passing through the most convex point of the core outline on the side where the sheath thickness is greatest, and Z is the distance between line X and line W. Irregularity = Z / X × 100. (2) The polyester fiber according to (1) above, wherein the cross section of the fiber has a ratio S / X of the minimum thickness S of the sheath to the minor axis X being 0.01 to 0.1. (3) The polyester fiber according to (1) or (2), wherein the polyester component of the core has a main repeating structural unit of trimethylene terephthalate or butylene terephthalate, and the polyester component of the sheath has a main repeating structural unit of ethylene terephthalate. (4) A tricot knitted fabric made of the polyester fiber according to any one of (1) to (3).

[0013] The polyester fiber of the present invention can provide a tricot knitted fabric that is excellent in abrasion resistance, has no warp streaks, is high quality, and has excellent stretchability.

[0014] Fig. 1 is a schematic diagram illustrating the composite form of a fiber cross section. Fig. 2 is a front cross-sectional view of a main part constituting a composite spinneret, showing an example of the composite spinneret, illustrating the method for producing a polyester fiber of the present invention. Fig. 3 is an example of the shape of the discharge holes of the discharge plate of the composite spinneret, showing the method for producing a polyester fiber of the present invention. Fig. 4 is a schematic diagram illustrating an example of a spinning process (direct spinning and drawing method) preferably used in the present invention.

[0015] The polyester fiber of the present invention has an eccentric sheath-core cross section, and in its cross section, the non-circularity (Y / X) calculated from the major axis Y and the minor axis X perpendicular to the major axis Y and passing through the center of gravity of the fiber is 1.1 to 3.0, and the ratio L / X of the minor axis X to the circumferential length L of the core is 2.6 to 5.0, and the degree of irregularity at the interface of the core is 15% or less.

[0016] The polyester fiber of the present invention is composed of two types of polyester polymers: a core and a sheath. Examples of the polyester polymer include polyethylene terephthalate (PET) or its copolymer, polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), and polylactic acid (PLA).

[0017] The coil-like crimping properties are achieved by combining two components with different thermal shrinkage rates as composite cross-section fibers. This ability is achieved by the stretching behavior of the high-shrinkage component, with the low-shrinkage component as the fulcrum. Therefore, the polyester polymer used for the high-shrinkage component must have high extensibility and recovery. The high-shrinkage component is preferably polytrimethylene terephthalate or polybutylene terephthalate in terms of its mechanical and chemical properties. More preferably, the high-shrinkage component is polytrimethylene terephthalate, which allows for a large difference in shrinkage rates, and the low-shrinkage component is preferably polyethylene terephthalate.

[0018] The polyester fiber of the present invention has a conjugated cross section formed by bonding two different polymers. Two polymers with different polymer properties are present in a bonded state without being substantially separated, and the fiber is an eccentric core-sheath type in which the component B completely covers the component A. Here, the term "eccentric" as used in the present invention refers to the fact that the center of gravity of the component A polymer in the core of the conjugated cross section is different from the center of gravity of the fiber with the conjugated cross section, and this will be explained using Figure 1.

[0019] In FIG. 1, the sheath is B, the core is A, the center of gravity of the core A in the composite cross section is a, and the center of gravity of the composite cross section fiber is C.

[0020] In the present invention, it is important that the centers of gravity a and C are far apart, so that the fiber will bend significantly toward the high-shrinkage component after heat treatment. As a result, the composite fiber continues to bend in the fiber axis direction, forming a three-dimensional spiral structure and exhibiting good crimp.

[0021] In the present invention, since component B completely covers component A, whitening or fluffing does not occur even when the fibers or fabric are subjected to friction or impact, and the quality of the fabric can be maintained.

[0022] The polyester fiber of the present invention is a long fiber, including textured yarn. The total fineness is 33 dtex to 167 dtex, and the number of filaments is 12 to 72. From the viewpoint of soft stretchability when woven into a fabric, the total fineness is preferably 56 dtex to 84 dtex, and the number of filaments is preferably 12 to 72. More preferably, the total fineness is 56 dtex, and the number of filaments is 24.

[0023] In the polyester fiber of the present application, the relationship between the minor axis X in the composite cross section and the circumferential length L of the core is L / X, which is 2.6 or more. L / X is a parameter that indicates the relationship between the minor axis X of the irregular eccentric sheath-core cross section and the contour length of the core. By setting L / X to 2.6 or more, stress applied per unit interface is dispersed, thereby improving abrasion resistance. Preferably, L / X is 3.0 or more.

[0024] The polyester fiber of the present invention has a non-circularity of 1.1 to 3.0. The non-circularity is the value obtained by dividing the major axis Y of the fiber cross section by the minor axis X passing through the center of gravity of the fiber. By setting the non-circularity Y / X to 3.0 or less, the crimped coil does not become too large and the physical power of the crimped coil is maintained, thereby achieving sufficient stretchability in the tricot knitted fabric. In addition, since it is possible to eliminate the movement of each single yarn in the same direction when crimp torque is generated, it is possible to reduce the likelihood of the crimped coil phases becoming aligned and prevent warp streaks. On the other hand, the lower the non-circularity Y / X, the better the stretchability of the tricot knitted fabric. However, a small L / X leads to reduced abrasion resistance and a tendency for the crimped coil phases to become aligned, which tends to deteriorate the quality of the warp streaks in the tricot knitted fabric. Therefore, the non-circularity Y / X is 1.1 or more. The non-circularity Y / X is preferably 1.2 to 2.9, more preferably 1.4 to 2.3.

[0025] The polyester fiber of the present invention has a core irregularity of 15% or less. The irregularity is calculated by drawing a line W parallel to the minor axis X passing through the most convex point of the core profile on the side where the sheath thickness is greatest at the interface of the eccentric core-sheath cross section, and passing through the center of gravity C of the fiber, and dividing Z by X, where Z is the distance between the two lines (X-W). By setting the irregularity to 15% or less, the distance between the centers of gravity of the two components increases, improving the crimpability of the polyester fiber and maintaining sufficient stretchability in a tricot knitted fabric. A preferable irregularity is 10% or less.

[0026] The polyester fiber of the present invention preferably has a ratio S / X of the minimum thickness S of the sheath portion to the minor diameter X in the fiber cross section of 0.01 to 0.1. By setting S / X to 0.1 or less, it becomes possible to reduce the inhibition of the sheath portion from developing yarn crimp. Furthermore, by setting S / X to 0.01 or more, it becomes possible to suppress deterioration in the quality of the tricot knitted fabric due to abrasion. A preferred S / X is 0.02 to 0.08.

[0027] The cross-sectional shape of the polyester fiber of the present invention is not particularly limited as long as it is a flat shape with an irregularity degree of 1.1 to 3.0, but a pot-shaped cross section or a mushroom shape with a constriction occurring near the center is preferred from the viewpoint of preventing the crimp phase from being aligned.

[0028] The conjugation ratio of the polyester fiber of the present invention is preferably 70:30 to 30:70, more preferably 60:40 to 40:60, from the viewpoints of spinnability, expression of crimp performance, and dimensional uniformity of the coil pitch in the fiber length direction. The conjugation ratio is the area ratio of two types of polyester polymer components in a photograph of the fiber cross section.

[0029] Next, a preferred method for producing the polyester fiber of the present invention will be described. Examples of the method for producing the polyester fiber of the present invention include a method in which a fiber thread discharged from a spinneret is temporarily wound on a drum and then drawn, and a method in which a fiber thread is continuously drawn at the spinning stage. These production methods will be specifically described.

[0030] The polyester fiber of the present invention can be produced by a two-step method in which two different polyester polymers are melted and sent to a predetermined conjugate pack using a conjugate spinning machine, and the two polymers are filtered in the pack, and then conjugate-spun into an eccentric core-sheath type using a conjugate spinneret. The undrawn yarn is then taken up and drawn to a predetermined breaking elongation using a conventional drawing machine. Alternatively, the polyester fiber can be produced by a one-step method in which the fibers are extruded from a spinneret and conjugate-spun, and the fiber yarn is subsequently drawn without being taken up. In consideration of the ease of tension control during fiber structure formation, i.e., from spinning to winding, a one-step direct spinning and drawing method (hereinafter referred to as the DSD method) as shown in Figure 4 is preferred.

[0031] As a method for forming an eccentric core-sheath cross section, a distributor plate type die as exemplified in Japanese Patent Application Laid-Open No. 2011-174215, Japanese Patent Application Laid-Open No. 2011-208313, and Japanese Patent Application Laid-Open No. 2012-136804 can be suitably used to form a desired cross-sectional shape.

[0032] The composite spinneret shown in FIG. 2 is assembled into a spinning pack in a state where three main types of members, namely, a metering plate 1, a distribution plate 2 and a discharge plate 3, are stacked from the top, and is used for spinning.

[0033] In the spinneret member exemplified in FIG. 2, the metering plate 1 measures the amount of polymer per discharge hole 6 and allows it to flow in, the distributor plate 2 controls the composite cross section and cross-sectional shape of the single fiber, and the discharge plate 3 compresses the composite polymer flow formed by the distributor plate 2 and discharges it.

[0034] Although not shown in the drawings to avoid complicating the explanation of the composite spinneret, the components stacked above the metering plate 1 may be components with flow paths formed to match the spinning machine and spin pack. By designing the metering plate 1 to match existing flow path components, the existing spin pack and its components can be used as they are. Therefore, there is no need to dedicate a spinning machine specifically to this spinneret.

[0035] Furthermore, the nozzle hole shape of the nozzle plate 3 is preferably an asymmetric slit shape as shown in Figure 3(a). In a cross section where two components with different thermal shrinkage, i.e., different polymer viscosities, are joined, a flow velocity gradient occurs inside the nozzle. When this flow velocity gradient is relaxed immediately after discharging, the polymer immediately after discharging becomes twisted, resulting in poor discharge stability. In addition, the desired cross section cannot be obtained. By setting the nozzle hole diameter within an appropriate range depending on the viscosity of each component, it is possible to reduce the flow velocity difference between the two components, thereby ensuring stable discharge of the polymer immediately after discharging. This also dramatically improves the stability of cross section formation in a distributor plate type spinneret, making it possible to obtain an accurate eccentric core-sheath cross section.

[0036] Furthermore, from the viewpoint of improving discharge stability and cross-section formability, the difference in melt viscosity between the polymers used in the fiber of the present invention is also important. When two types of molten polymers forming a composite flow are contracted, the cross-sectional area is changed in the cross section perpendicular to the polymer flow direction in order to match the pressure losses of the two types of polymers. As a result, a difference in flow velocity occurs, and the center of gravity of each component is discharged with a bias, resulting in twisting of the discharged polymer flow. That is, a polymer with a high melt viscosity has a large cross-sectional area and therefore a slow flow velocity, while a polymer with a low melt viscosity has a small cross-sectional area and therefore a fast flow velocity. Therefore, by reducing the difference in melt viscosity between the polymers used, the difference in flow velocity between the polymers can be alleviated, and bending of the discharged polymer flow can be suppressed. From this viewpoint, it is preferable that the difference in melt viscosity between the combined polymers is small. However, in the polyester fiber of the present invention, considering factors such as crimp development, it is preferable that the difference in melt viscosity between the combined polymers is large. In view of the above, the difference in melt viscosity between the polymers to be combined is particularly preferably in the range of 100 Pa·s to 300 Pa·s.

[0037] By adopting such production conditions, it is possible to obtain polyester fibers having a non-circularity Y / X in the fiber cross section of 1.1 to 3.0, a ratio L / X of the minor diameter X to the circumferential length L of the core of 2.6 to 5.0, and an interface irregularity of the core of 15% or less, and further, a ratio S / X of the minimum thickness S of the sheath to the minor diameter X of 0.01 to 0.1.

[0038] The polyester fiber of the present invention is warped as raw silk and knitted on a tricot knitting machine. Further, the scouring and dyeing after knitting, as well as the subsequent presetting and final setting conditions, may be carried out according to known methods.

[0039] The examples and comparative examples were evaluated as follows.

[0040] (1) Melt Viscosity of Polymer Chip-shaped polymer was dried to a moisture content of 200 ppm or less using a vacuum dryer, and the melt viscosity was measured by changing the strain rate stepwise using a Capillograph 1B manufactured by Toyo Seiki Seisakusho Co., Ltd. The measurement temperature was the same as the spinning temperature. -1 The melt viscosity is shown in Table 1. Incidentally, the time from when the sample was placed in the heating furnace to when the measurement started was 5 minutes, and the measurement was carried out in a nitrogen atmosphere.

[0041] (2) Total Fineness A fiber sample was prepared into 100 skeins using a measuring machine with a frame circumference of 1.0 m, and the total fineness was calculated from the weight measured on a balance using the following formula: Total fineness (dtex) = Skein weight (g) × 100 (3) Minor diameter X, major diameter Y, core circumference L, distance between two straight lines Z, and sheath minimum thickness S in the fiber cross section Using a digital microscope (VHX-2000) manufactured by KEYENCE Corporation, the cross section of a polyester fiber was photographed at 100x to 500x magnification. The minor diameter X, major diameter Y, core circumference L, distance between two straight lines Z, and sheath minimum thickness S in the fiber cross section of one single yarn were measured. Five random single yarns were measured. The irregularities Y / X, L / X, and irregularity = Z / X × 100 and S / X were calculated from the average values ​​measured.

[0042] (4) Stretching Elongation Rate The stretching elongation rate was determined according to JIS L1013 (2010) Section 8.11, Method C (simplified method).

[0043] (5) Evaluation of tricot knit fabrics A 28G tricot half-structure knitted fabric was produced using polyester fibers obtained in each of the Examples and Comparative Examples for both the front and back yarns. The resulting fabric was scoured at 90°C for 1 minute and dyed at 130°C for 20 minutes. It was then pre-set at 130°C for 2 minutes and final set at 170°C for 1 minute to obtain a tricot knit fabric.

[0044] A. Stretchability (warp elongation rate) The warp elongation rate of the tricot knit fabric was determined according to JIS L1096 (2010) Section 8.16.1, Method A (constant speed elongation method). The elongation rate was evaluated using the following three levels, with S and A representing good stretchability. S: Warp elongation rate of 15% or more A: Warp elongation rate of 10% or more C: Warp elongation rate of less than 10%.

[0045] B. Abrasion Resistance (Martindale (Times)) Evaluation was carried out using a tricot knitted fabric in accordance with JIS L1096 (2010) Section 8.19.5, Method E (Martindale Method). The test conditions were as follows: a standard abrasion cloth made of polyester was used as the friction element, and the number of abrasions was measured at a pressure load of 9 kPa until the discoloration of the abraded fabric reached Grade 3 on the discoloration gray scale, and the test was evaluated as follows. Pass levels were S and A. S: 5,000 times or more; A: 2,000 times or more but less than 5,000 times; C: Less than 2,000 times.

[0046] C. Quality The obtained tricot knit fabric was inspected by a skilled inspection technician and visually evaluated for the occurrence of warp streaks. Passing grades were S and A. S: No warp streaks, very good A: Some warp streaks present, but passable C: Many warp streaks present, failing grade.

[0047] Example 1: The core component was polytrimethylene terephthalate (PTT) with a melt viscosity of 100 Pa s, and the sheath component was polyethylene terephthalate (PET) with a melt viscosity of 30 Pa s. The PTT polymer and PET polymer were melted at 260°C and 280°C, respectively, using an extruder, and then metered with a pump to a spinning temperature of 275°C. The mixture was allowed to flow into a spinneret while maintaining the temperature. The PTT component and PET component were mixed in a 50 / 50 ratio, and the mixture was allowed to flow into a composite spinneret with an eccentric sheath-core cross section and 24 nozzle holes. The polymers merged inside the spinneret to form a composite cross section, and the desired eccentric sheath-core cross section, as shown in Figure 1(a), was extruded from the spinneret.

[0048] The spinneret used was a spinneret in which three types of members, namely, a metering plate 1, a distribution plate 2, and a discharge plate 3, were stacked from top to bottom, with the distribution plate being made up of multiple laminated plates to form fine flow channels, as shown in Fig. 2. The shape of the discharge holes in the discharge plate 3 was such that the diameter of the discharge holes on the side containing PTT as the main component was Φ0.25, and the diameter of the discharge holes on the PET side was Φ0.18, with a slit width of 0.13 mm and a slit length of 1.05 mm (Fig. 3(a)).

[0049] The yarn discharged from the spinneret was spun and drawn using the melt spinning equipment shown in Fig. 4. That is, the fiber yarn discharged from the composite spinneret i was cooled by a yarn cooling air blower ii, an oil was applied to the fiber by an oil application device iii in an amount of 0.8 wt % based on the fiber weight, pre-entangled by a pre-entanglement device iv at an air pressure of 0.03 MPa, and then taken up by a first hot roller (1 HR) v heated to a temperature of 60°C at a speed of 1,070 m / min. Without being taken up once, the yarn was drawn around a second hot roller (2 HR) vi heated to a temperature of 155°C at a speed of 3,780 m / min, drawn at a draw ratio of 3.5, and heat-set. Further, the yarn was subjected to main entanglement at an air pressure of 0.15 MPa using the main entanglement device vii, and then drawn around two godet rollers (third godet roller (3GR) viii and fourth godet roller (4GR) ix) at a speed of 3700 m / min, and then wound onto a package x at a package winding speed of 3670 m / min to obtain a polyester multifilament of 56 dtex-24 filaments. The properties of this polyester multifilament are shown in Table 1.

[0050] The resulting polyester multifilament was used as both the front yarn and the back yarn to produce a 28G tricot half-structure knitted fabric on a tricot knitting machine. The resulting fabric was then scoured at 90°C for 1 minute and dyed at 130°C for 20 minutes. It was then pre-set at 130°C for 2 minutes and final set at 170°C for 1 minute to obtain a tricot knitted fabric. The resulting tricot knitted fabric had excellent stretchability and abrasion resistance, and the knitted fabric had good quality with no warp streaks.

[0051] Examples 2 to 7 and Comparative Example 1 Polyester multifilaments were obtained in the same manner as in Example 1, except that the slit length of the discharge plate 3 was changed. The results are shown in Table 1.

[0052] Comparative Example 2 A polyester multifilament was obtained in the same manner as in Example 1, except that the discharge plate 3 was changed to a round shape as shown in Fig. 3(b) and the fiber was discharged from the spinneret with an eccentric core-sheath cross section as shown in Fig. 1(b). The results are shown in Table 1.

[0053]

[0054] In Comparative Example 1, the degree of deformation of the polyester fiber was large, and the crimped coil became large, so that the physical power of the coil could not be maintained. As a result, the warp elongation rate of the tricot knit fabric was low at 8%, and sufficient stretchability was not obtained.

[0055] In Comparative Example 2, the degree of deformation was small and L / X was small, resulting in low abrasion resistance of the tricot knit fabric with a Martindale of 1,500 times, and the deterioration of the warp quality was noticeable due to the aligned crimp phase.

[0056] Examples 8 to 11 and Comparative Example 3 Polyester fibers were obtained in the same manner as in Example 1, except that the distributor plate 2 and the degree of unevenness were changed. In Example 11, the fibers were extruded from the spinneret with an eccentric core-sheath composite cross section as shown in Figure 1(c). The results are shown in Table 2.

[0057] In Comparative Example 3, the unevenness was large and the distance between the centers of gravity of the polyester fibers was large, which reduced the crimping property, and the warp elongation rate of the tricot knit fabric was low at 6%, so sufficient stretchability was not obtained.

[0058]

[0059] Examples 12 to 14 and Comparative Examples 4 and 5 Polyester fibers were obtained in the same manner as in Example 1, except that the distributor plate 2 and the minimum thickness of the sheath portion were changed. The results are shown in Table 3.

[0060] In Comparative Example 4, the minimum thickness of the sheath was small, and the Martindale count of the tricot knit fabric was 1000 times, resulting in poor abrasion resistance.

[0061] In Comparative Example 5, the minimum thickness of the sheath was large, the crimping property of the polyester fiber was reduced, and the warp elongation rate of the tricot knit fabric was low at 8%, so sufficient stretchability was not obtained.

[0062] Example 15 A polyester fiber was obtained in the same manner as in Example 1, except that the core component was changed to polybutylene terephthalate (PBT) having a melt viscosity of 250 Pa s. The evaluation results of the obtained polyester multifilament are shown in Table 3.

[0063]

[0064] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-57259) filed on March 31, 2023, the contents of which are incorporated herein by reference.

[0065] The polyester fiber of the present invention can provide a high-quality tricot knit fabric that is excellent in abrasion resistance, free of warp streaks, and has excellent stretchability.

[0066] A: Core B: Sheath a: Center of gravity of core A in the composite cross section C: Center of gravity of the composite cross section fiber 1: Metering plate 2: Distribution plate 3: Discharge plate 4: Metering groove A 5: Metering groove B 6: Discharge hole i: Composite spinneret ii: Yarn cooling air blower iii: Oil application device iv: Pre-entangling device v: First hot roller vi: Second hot roller vii: Main entangling device viii: Third godet roller ix: Fourth godet roller x: Package xi: Contact roller

Claims

1. A polyester fiber having an eccentric core-sheath cross section, in which the cross section has an irregular cross section with an irregularity (Y / X) of 1.1 to 3.0 calculated from the major axis Y and the minor axis X perpendicular to the major axis Y and passing through the center of gravity of the fiber, the ratio L / X of the minor axis X to the circumference L of the core is 2.6 to 5.0, and the irregularity at the core interface is 15% or less. Irregularity: The value given by the following formula, where W is a straight line parallel to the minor axis X and passing through the most convex point of the core outline on the side where the sheath thickness is maximum, and Z is the distance between line X and line W. Irregularity = Z / X x 100 2. The polyester fiber according to claim 1, characterized in that in the cross section of the fiber, the ratio S / X of the minimum thickness S of the sheath portion to the minor diameter X is 0.01 to 0.

1.

3. A polyester fiber according to claim 1 or 2, wherein the polyester component of the core has a main repeating structural unit of trimethylene terephthalate or butylene terephthalate, and the polyester component of the sheath has a main repeating structural unit of ethylene terephthalate.

4. A tricot knit fabric made from the polyester fiber according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Conjugate fiber

    JP1982205520A

  • Bulky composite fiber

    JP1989092413A

  • Spontaneously crimpable conjugated fiber

    JP1997302529A

  • Eccentric core-sheath composite short-fiber

    JP2020158946A

  • Multi-layer woven knitted fabric

    WO2022176797A1