Method for repairing light-emitting device, and light-emitting device

The method addresses the challenge of repairing μLEDs in light emitting devices by using a repair conductive film with larger or harder conductive particles for stable bonding, ensuring reliable lighting and minimizing re-repairs in light emitting devices.

WO2024203690A1PCT designated stage expired Publication Date: 2024-10-03DEXERIALS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010942
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

In light emitting devices with μLEDs mounted on a transparent substrate via a conductive film, the repair of defective μLEDs is challenging due to the hardening of the insulating resin layer, leading to increased conduction resistance and potential failure of the repair μLED to light up, necessitating additional repairs.

Method used

A method involving the use of a repair conductive film with conductive particles of larger size or higher compressive elastic modulus than the original conductive film particles, facilitating stable thermocompression bonding and ensuring effective electrical conduction between electrodes.

Benefits of technology

The method allows for successful repair of defective μLEDs, ensuring they light up reliably and reducing the need for further repairs by maintaining stable conduction and crushability of conductive particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010942_03102024_PF_FP_ABST
    Figure JP2024010942_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a method for repairing a light-emitting device in which a plurality of µLEDs are mounted through a first electroconductive film in which first electroconductive particles are held by a first insulating resin layer, wherein the µLED to be repaired is identified from among the mounted µLEDs, the identified µLED is removed from a translucent substrate by a laser lift-off method, an electroconductive film for repair in which second electroconductive particles are held by a second insulating resin layer is installed in the shape of an individual piece on the portion of the translucent substrate from which the µLED was removed, and next a µLED for repair is installed, after which the µLED for repair is mounted to the translucent substrate by thermocompression bonding, and finally the operation of the light-emitting device is confirmed. In particular, as the second electroconductive particles of the second electroconductive film for repair, particles having a particle diameter larger than that of the first electroconductive particles of the first electroconductive film are used, or particles that are less likely to collapse than the first electroconductive particles of the first electroconductive film are used.
Need to check novelty before this filing date? Find Prior Art

Description

Light-emitting device repair method and light-emitting device

[0001] The present invention relates to a method for repairing a light-emitting device that includes μLEDs (Light Emitting Diodes) as light-emitting elements, and the light-emitting device. Specifically, the present invention relates to a method for repairing a μLED that is defective among a plurality of mounted μLEDs to a good μLED, and a light-emitting device that includes the repaired μLED.

[0002] In recent years, light-emitting devices such as full-color displays that mount a large number of μLEDs on a panel substrate have been attracting attention (see FIG. 7 ). Such light-emitting devices 10 have a structure in which a large number of μLEDs 100 are mounted by thermocompression on a light-transmitting substrate 104 via an (anisotropic) conductive film 103 in which conductive particles 102 are held in a thermosetting insulating resin layer 101. In this structure, to ensure electrical continuity between the μLEDs 100 and the light-transmitting substrate 104, the conductive particles 102 are mounted by thermocompression between an electrode 100 a of the μLED 100 and an electrode (not shown) of the light-transmitting substrate 104, thereby crushing the conductive particles 102.

[0003] In such a light-emitting device 10, when some μLEDs become unlit, the unlit μLEDs are repaired (see, for example, Patent Documents 1 and 2). Specifically, as shown in Fig. 8 , first, the unlit μLEDs 100 are selectively removed from the translucent substrate 104 together with the conductive film 103 by irradiating them with a laser L from the translucent substrate 104 side using a laser lift-off method. Next, as shown in Fig. 9 , a repair conductive film 103a having the same configuration as the conductive film 103 except for being separated into individual pieces and a repair μLED 100R having the same configuration as the μLED 100 are installed on the portion of the translucent substrate 104 from which the unlit μLEDs were removed using a stamping method, a laser lift-off method, or the like. Then, as shown in Fig. 10 , the repair μLED 100R is pressed into the translucent substrate 104 using a heat tool 105 having a surface area much larger than that of the repair μLED 100R.

[0004] JP 2022-140934 A JP 2021-144970 A

[0005] 10 , the insulating resin layer 101 constituting the conductive film 103 between the μLEDs 100 around the repair μLED 100R and the translucent substrate 104 has already hardened, making it difficult to deform when pressed with the heat tool 105. For this reason, when the repair μLED 100R can only be pressed to the same height as the surrounding μLEDs 100 and the heat tool 105 is pulled up, a springback phenomenon occurs as shown in FIG. 11 , and the conductive particles 102a between the electrode 100Ra of the repair μLED 100R and the electrode (not shown) of the translucent substrate 104 are not crushed, increasing the conduction resistance and possibly causing the repair μLED 100R to stop lighting, necessitating another repair.

[0006] The present invention seeks to solve the problems of the conventional art, and aims to repair a μLED that is not lighting properly in a light-emitting device in which multiple μLEDs are mounted by thermocompression on a translucent substrate via a conductive film in which conductive particles are held in an insulating resin layer, when repairing a μLED that is not lighting properly.

[0007] The inventors hypothesized that the above-described conventional problems were due to the use of the same repair conductive film as the initial conductive film used when initially installing the μLEDs on the translucent substrate as the repair conductive film used when installing the repair μLEDs on the translucent substrate. Based on this assumption, the inventors investigated the conductive particles constituting each of the initial conductive film and the repair conductive film. As a result, as described below, they found that the above-described problems of the present invention can be solved if the conductive particles of the repair conductive film have a larger particle size than the conductive particles of the initial conductive film, or if the conductive particles of the repair conductive film are more resistant to crushing than the conductive particles of the initial conductive film, which led to the completion of the present invention.

[0008] That is, the present invention provides a method for repairing a light-emitting device in which a plurality of μLEDs are mounted by thermocompression on a translucent substrate via a first conductive film in which first conductive particles are held in a first insulating resin layer, the method comprising the following steps (A) to (F): (Step A) a step of identifying a μLED to be repaired from the plurality of mounted μLEDs; (Step B) a step of removing the μLED to be repaired from the translucent substrate by a laser lift-off method; (Step C) a step of installing a repair conductive film in which second conductive particles are held in a second insulating resin layer in an individual piece on a part of the translucent substrate from which the μLED has been removed; (Step D) a step of installing the repair μLED on the repair conductive film installed on the translucent substrate; (Step E) a step of mounting the repair μLED on the translucent substrate by thermocompression; and (Step F) a step of checking the operation of the light-emitting device in which the repair μLED is mounted. This is a repair method in which the second conductive particles of the second repair conductive film have a larger particle size than the first conductive particles of the first conductive film, or the second conductive particles of the second repair conductive film are more difficult to crush than the first conductive particles of the first conductive film.

[0009] The present invention also provides a light-emitting device in which a plurality of μLEDs are mounted on a light-transmitting substrate, wherein a majority of the μLEDs are mounted to the light-transmitting substrate by compression bonding (e.g., thermocompression bonding) via a first conductive film in which first conductive particles are held by a first insulating resin layer, and a remaining small number of μLEDs are mounted to the light-transmitting substrate by compression bonding (e.g., thermocompression bonding) via a second repair conductive film in which second conductive particles are held by a second insulating resin layer, and wherein the second conductive particles of the second repair conductive film have a larger particle size than the first conductive particles of the first conductive film, or the second conductive particles of the second repair conductive film are not crushed more than the first conductive particles of the first conductive film.

[0010] The light-emitting device repair method of the present invention is characterized in that (a) the second conductive particles of the second repair conductive film have a larger particle size than the first conductive particles of the first conductive film, or (b) the second conductive particles of the second repair conductive film are more resistant to crushing than the first conductive particles of the first conductive film (i.e., have a 20% higher compressive modulus). This allows for stable conduction between the opposing electrodes to be connected. Therefore, according to the light-emitting device repair method of the present invention, in a light-emitting device in which multiple μLEDs are mounted by compression bonding (e.g., thermocompression bonding) to a translucent substrate via a conductive film in which the conductive particles are held in an insulating resin layer, repairing a μLED that is not lighting properly can restore the repaired μLED to lighting properly, eliminating the need for further repair.

[0011] FIG. 1 is an explanatory diagram showing a state in which some μLEDs of a light-emitting device are not lit before the repair method of the present invention is applied. FIG. 2 is an explanatory diagram of the steps of the repair method of the present invention. FIG. 3 is an explanatory diagram of the steps of the repair method of the present invention. FIG. 4 is an explanatory diagram of the steps of the repair method of the present invention. FIG. 5 is an explanatory diagram of the steps of the repair method of the present invention. FIG. 6 is a schematic cross-sectional view of a light-emitting device after the repair method of the present invention has been applied. FIG. 7 is an explanatory diagram showing a state in which some μLEDs of a conventional light-emitting device are not lit. FIG. 8 is an explanatory diagram of the steps of a conventional light-emitting device repair method. FIG. 9 is an explanatory diagram of the steps of a conventional light-emitting device repair method. FIG. 10 is an explanatory diagram of the steps of a conventional light-emitting device repair method. FIG. 11 is an explanatory diagram showing a state in which some μLEDs of a light-emitting device are not lit after the conventional light-emitting device repair method has been applied.

[0012] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.

[0013] <Method for Repairing a Light-Emitting Device> The present invention relates to a method for repairing a light-emitting device, and a light-emitting device to which the repair method is applied typically has the structure shown in Fig. 1. That is, the method for repairing a light-emitting device 10 includes a plurality of μLEDs 1 mounted by thermocompression on a light-transmitting substrate 5 via a first conductive film 4 having first conductive particles 3 held in a first insulating resin layer 2, and includes the following steps (A) to (F). Below, each step will be described, followed by a description of the characteristics of the conductive particles that characterize the present invention, and then a description of each component applicable to the repair method.

[0014] (Process A) Process A is a process for identifying a μLED to be repaired from among the multiple mounted μLEDs. Indicators for identifying a μLED to be repaired include whether it is lit, whether the amount of light emitted is insufficient, whether there are any external abnormalities in color, shape, or size, and whether there are any alignment errors. Typically, an unlit μLED is the one to be repaired. In the case of FIG. 1 , the unlit μLED in the center is identified as the one to be repaired. Note that, as shown in FIG. 1 , the light-emitting device 10 before repair has a structure in which multiple μLEDs 1 are mounted by thermocompression on a translucent substrate 5 via a first conductive film 4 in which first conductive particles 3 are held by a thermoset first insulating resin layer 2. In such a light-emitting device 10, crushed first conductive particles 3 are disposed between the electrode 1 a of the μLED 1 and the electrode (not shown) of the translucent substrate 5.

[0015] (Step B) Step B is a step of removing a μLED to be repaired (e.g., an unlit μLED) from the translucent substrate by laser lift-off. Specifically, as shown in FIG. 2 , a laser L is irradiated onto the unlit μLED 1x to be removed from the translucent substrate 5 side of the light-emitting device 10, and the unlit μLED 1x, along with the first conductive film 4 directly below it (in other words, the first conductive film 4 located between the unlit μLED 1x and the translucent substrate 5), are selectively transferred to a separately prepared adhesive film and removed. A commercially available laser lift-off device (e.g., product name "Invisi LUM-XTR" manufactured by Shin-Etsu Engineering Co., Ltd.) can be used as a laser lift-off device for performing the laser lift-off method. The laser lift-off conditions can also be appropriately selected taking into account the shape, constituent materials, and structure of the μLED or light-emitting device to be repaired, the recommended conditions for the laser lift-off device to be used, and the like. The first conductive film 4 may be anisotropically conductive.

[0016] (Step C) Step C is a step of disposing a repair conductive film, in which second conductive particles are held in a second insulating resin layer, in a piece on the portion of the translucent substrate from which the μLEDs have been removed. Specifically, as shown in FIG. 3 , a repair second conductive film 40, in which second conductive particles 30 are held in a second insulating resin layer 20, is disposed in a piece on the exposed surface of the translucent substrate 5 of the light-emitting device 10 from which the μLEDs have been removed. Although known methods such as stamping, screen printing, and inkjet printing can be used to dispose the repair second conductive film 40 in a piece, it is preferable to dispose it by laser lift-off. For example, a second repair conductive film 40 having second conductive particles 30 held in a second insulating resin layer 20 is formed on the entire surface of an adhesive layer of a transparent substrate (transparent substrate / adhesive layer / second repair conductive film), and a laser is irradiated from the transparent substrate side using a laser lift-off method to remove unnecessary second repair conductive film 40 so that the second repair conductive film 40 remains in the form of individual pieces, thereby obtaining a conductive film transfer sheet having a large number of individual pieces of second repair conductive film 40, and the second repair conductive film 40 of the conductive film transfer sheet is aligned with the exposed surface of the translucent substrate 5, and a laser is irradiated from the transparent substrate side of the conductive film transfer sheet to transfer the second repair conductive film 40 to the exposed surface of the translucent substrate 5. The second repair conductive film 40 may be anisotropically conductive.

[0017] (Process D) Process D is a process of installing a repair μLED on a repair conductive film installed on a light-transmitting substrate. Specifically, as shown in FIG. 4 , the repair μLED 1y is installed on the exposed second repair conductive film 40 of the light-emitting device 10 from which the μLED has been removed, with its electrode 1ya side facing the film. A known method can be used to install the repair μLED 1y on the second repair conductive film 40. For example, a laser lift-off method can be used to irradiate the repair μLED 1y with a laser from the backside of the μLED wafer substrate and transfer it directly to the second repair conductive film 40. Alternatively, the repair μLED may be transferred to an adhesive transfer sheet in advance and then transferred from the transfer sheet to the second repair conductive film 40.

[0018] (Step E) Step E is a step of thermocompression bonding the repair μLED to the light-transmitting substrate. Specifically, as shown in Fig. 5 , the repair μLED 1y is pressed into the light-transmitting substrate 5 while being heated with a heat tool H, and the second conductive particles 30 of the second repair conductive film 40 are crushed while the thermosetting second insulating resin layer 20 is thermally cured. This allows the light-emitting device 10 having the structure shown in Fig. 6 to be obtained.

[0019] (Step F) Step F is a step of checking the operation of the light-emitting device in which the repair μLED is mounted. Specifically, the light-emitting device is operated and it is checked that the repair μLED 1y lights up. This completes the repair of the light-emitting device.

[0020] <Characteristics of Conductive Particles Characterizing the Method for Repairing a Light-Emitting Device of the Present Invention> The method for repairing a light-emitting device of the present invention is characterized in that (a) the second conductive particles of the second repair conductive film have a larger particle size than the first conductive particles of the first conductive film, or (b) the second conductive particles of the second repair conductive film are more difficult to crush than the first conductive particles of the first conductive film (in other words, have a 20% higher compressive elastic modulus). Of course, both (a) and (b) may be satisfied simultaneously.

[0021] In the former case (a), when the repair conductive film and the repair μLED are placed on the translucent substrate in order to mount the repair μLED, the height of the repair μLED from the surface of the translucent substrate becomes greater than the height of the surrounding mounted μLEDs. As a result, when the repair μLED is mounted by thermocompression bonding using a heat tool, pressure can be sufficiently concentrated on the second conductive particles, and stable conduction can be achieved between the opposing electrodes to be connected.

[0022] The average particle diameter D1 of the first conductive particles in the first conductive film is preferably 1 μm or more, more preferably 1.5 μm or more, and preferably 5 μm or less, and more preferably 3 μm or less, from the viewpoints of particle capture efficiency and adaptability to the size of the μLED. Furthermore, the average particle diameter D2 of the second conductive particles in the second repair film is preferably 1.1 times or more, more preferably 1.3 times or more, and preferably 2 times or less, and more preferably 1.7 times or less, of the average particle diameter D1 of the first conductive particles, in order to adapt it to the size of the μLED and ensure repairability. The average particle diameter of the conductive particles can be measured by known methods, for example, using an imaging particle size analyzer (FPIA-3000, manufactured by Malvern Panalytical).

[0023] In the latter case (b), when the repair μLED is mounted by thermocompression bonding using a heat tool, the oxide film on the surface of the opposing electrode to be connected can be broken through with little pressure, thereby achieving stable conduction between the opposing electrodes to be connected.

[0024] The crushability of the conductive particles can be evaluated by their compressive modulus. This is because the higher the compressive modulus of the conductive particles, the more resistant they are to crushing. Furthermore, evaluation is performed at 20% compression (20% K value) because 20% compression stabilizes the conduction of the compressed conductive particles. The 20% compressive modulus E1 (20% K value) of the first conductive particles is preferably 2000 MPa or more, more preferably 3000 MPa or more, preferably 6000 MPa or less, and more preferably 5000 MPa or less in order to be applied to μLEDs. Furthermore, the 20% compressive modulus E2 (20% K value) of the second conductive particles is preferably 1.1 times or more, more preferably 1.3 times or more, preferably 2.5 times or less, more preferably 2 times or less, and preferably 4000 MPa or more and 10000 MPa or less, in order to adapt it to the size of the repair μLED and ensure repairability. The 20% compressive elastic modulus can be calculated by measuring the compressive deformation of the conductive particles when a compressive load is applied to the conductive particles using a microcompression tester (e.g., Fischerscope H-100, manufactured by Fischer Instruments), and using the following formula, where F is the load value (N) when the conductive particles are compressed and deformed by 20%, S is the compressive displacement (mm) when the conductive particles are compressed and deformed by 20%, and R is the average radius (mm) of the conductive particles.

[0025] 20% compression elastic modulus (20% K value) [N / mm 2 =MPa]=(3 / 2 1 / 2 )・F・S -3 / 2 ・R -1 / 2

[0026] As described above, according to the method for repairing a light-emitting device of the present invention, in a light-emitting device in which multiple μLEDs are mounted by thermocompression on a translucent substrate via a conductive film in which conductive particles are held in an insulating resin layer, by repairing a μLED that is not lighting up properly, the repaired μLED can be made to light up properly, making it unnecessary to repair it again.

[0027] <Explanation of an example of a component to which the repair method of the present invention is applied> (Light-emitting device 10) The light-emitting device 10 to which the repair method of the present invention is applied uses μLEDs as light-emitting elements, and examples thereof include image display devices such as full-color displays and lighting devices. Instead of μLEDs, the repair method can also be applied to other minute light-emitting elements such as mini-LEDs or minute components (electronic components). An example of the size is one with a maximum length of one side of 200 μm or less. It can also be as large as 10 to 30 μm square, making manual repair extremely difficult.

[0028] (μLED 1) μLED 1 can be a known type, preferably having a maximum length of 3 μm to 100 μm in plan view and a flip-chip type with an electrode on one side. The electrode can be any electrode used in known μLEDs, such as a transparent electrode made of indium ITO. The thickness of the electrode is preferably 0.1 μm or more, more preferably 1 μm or more, and preferably 5 μm or less, more preferably 3 μm or less.

[0029] (First Conductive Film 4) The first conductive film 4 has first conductive particles 3 held in the first insulating resin layer 2, and can be used as a conductive film or anisotropic conductive film. The first conductive film 4 may be applied in a solid state over the entire surface of the light-transmitting substrate 5, or may be applied in individual pieces by a stamping method, an inkjet method, a laser lift-off method, or the like.

[0030] (First Conductive Particles 3) The first conductive particles 3 constituting the first conductive film 4 can be appropriately selected from those used in known conductive films or anisotropic conductive films. Examples include metal particles such as nickel, copper, silver, gold, palladium, and solder, and metal-coated resin particles in which the surface of resin particles such as polyamide and polybenzoguanamine is coated with a metal such as nickel or gold. This allows conductivity even when the μLED does not have a connection site such as a solder bump.

[0031] Regarding the first conductive particles 3, the average particle diameter has already been described, but the lower limit of the particle surface density is preferably 500 particles / mm 2 The upper limit is preferably 200,000 pieces / mm 2 or less, more preferably 150,000 pieces / mm 2 Particularly preferably, 120,000 pieces / mm 2 It can be as follows:

[0032] The first conductive particles 3 may be arranged randomly in the field of view of the film surface, or preferably arranged independently. In this case, it is preferable that 95% or more of the conductive particles are independent by number. Furthermore, it is preferable that the conductive particles are not only arranged independently but also arranged regularly. In particular, an arrangement in which the particle arrangement in each of the mutually orthogonal directions in the field of view of the film surface is periodically repeated is preferable. Examples include lattice arrangements such as a hexagonal lattice, a rectangular lattice, an oblique lattice, a square lattice, and other rectangular lattices. Furthermore, an arrangement in which linear particle rows in which the conductive particles are arranged at a predetermined interval are parallel to each other at a predetermined interval may also be used. In this way, by regularly arranging the conductive particles in the field of view of the film surface, the conductive particle surface density can be made uniform, and the transfer rate of μLEDs by laser light irradiation can be further improved.

[0033] (First insulating resin layer 2) The first insulating resin layer 2 holds the first conductive particles 3, and is formed from a thermosetting resin composition that is thermally cured when thermocompressed with a heat tool H in order to securely hold the conductive particles. From the viewpoint of conductive particle capture, the layer thickness before thermocompression is preferably 3 μm or more, more preferably 4 μm or more, and preferably 10 μm or less, more preferably 7 μm or less.

[0034] The first insulating resin layer 2 preferably exhibits excellent cushioning properties (shock absorption properties) for stable attachment to the light-transmitting substrate 5. This can suppress defects such as displacement, deformation, breakage, and detachment of the μLEDs, and improve the transfer rate of the μLEDs by laser irradiation. Such cushioning properties can be evaluated by durometer A hardness and / or storage modulus, as described below.

[0035] The durometer A hardness of the first insulating resin layer 2 is preferably 20 or more and 40 or less, more preferably 20 or more and 35 or less, and particularly preferably 20 or more and 30 or less. If the durometer A hardness is too high, the first insulating resin layer 2 is too hard, and defects such as deformation and breakage of the μLEDs tend to occur easily. If the durometer A hardness is too low, the first insulating resin layer 2 is too soft, and defects such as displacement of the μLEDs tend to occur easily. The durometer A hardness of the first insulating resin layer 2 can be measured as rubber hardness (Japanese Industrial Standard JIS-A hardness) using a durometer A in accordance with JIS K6253.

[0036] The storage modulus of the first insulating resin layer 2 is preferably 60 MPa or less, more preferably 30 MPa or less, and particularly preferably 10 MPa or less. If the storage modulus is too high, the impact of the μLEDs ejected at high speed by laser irradiation cannot be absorbed, and the transfer rate of the μLEDs tends to decrease. The storage modulus can be determined by a dynamic viscoelasticity test using an indentation tester (temperature 30°C, frequency 200 Hz, using a flat punch with a diameter of 100 μm, target indentation depth 1 μm, and frequency sweeping in the range of 1 to 200 Hz).

[0037] Furthermore, the storage modulus (30°C) of the thermosetting resin layer formed by thermal curing of the first insulating resin layer 2, measured in a tensile mode in accordance with JIS K7244, is preferably 100 MPa or more, more preferably 2000 MPa or more. If the storage modulus at 30°C is too low, good conductivity cannot be obtained and connection reliability tends to decrease. The storage modulus at 30°C can be measured in a tensile mode using a viscoelasticity tester (Leovibron, manufactured by A&D Co., Ltd.) in accordance with JIS K7244 under measurement conditions of, for example, a frequency of 11 Hz and a temperature rise rate of 3°C / min.

[0038] The thermosetting resin composition for forming the first insulating resin layer 2 preferably contains a rubber component, a film-forming resin, a thermosetting resin, a thermosetting agent, and an inorganic filler. If necessary, other known additives may be added within a range that does not impair the effects of the invention.

[0039] *Rubber component The rubber component contained in the thermosetting resin composition is a component for imparting cushioning properties (shock absorption) to the first insulating resin layer, and is not particularly limited as long as it is an elastomer with good cushioning properties. Specific examples include acrylic rubber, silicone rubber, butadiene rubber, and polyurethane resin (polyurethane-based elastomer). Among these, one or more types selected from acrylic rubber and silicone rubber are preferred. The content of the rubber component is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler.

[0040] *Film-forming resin: From the viewpoint of film-forming properties, examples of the film-forming resin include various resins such as phenoxy resin, polyester resin, polyurethane resin, polyester urethane resin, acrylic resin, polyimide resin, and butyral resin, each having a weight-average molecular weight of preferably about 10,000 to 80,000. These may be used alone or in combination of two or more. Among these, phenoxy resin is preferred from the viewpoint of film formation state, connection reliability, and the like. The content of the film-forming resin is preferably 20 parts by mass or more, more preferably 25 parts by mass or more, particularly preferably 35 parts by mass or more, preferably 50 parts by mass or less, and more preferably 45 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler.

[0041] *Thermosetting resin Examples of thermosetting resins include epoxy compounds and (meth)acrylate compounds, with epoxy compounds being particularly preferred. These compounds may be monomers, oligomers, or polymers. The content of the thermosetting resin is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, particularly preferably 25 parts by mass or more, preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and particularly preferably 35 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler.

[0042] The epoxy compound that can be used as the thermosetting resin is not particularly limited as long as it is an epoxy compound having one or more epoxy groups in the molecule. For example, it may be a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, or a urethane-modified epoxy resin. Among these, high-purity bisphenol A type epoxy resin is preferably used. A specific example of a high-purity bisphenol A type epoxy resin is the product name "YL980" manufactured by Mitsubishi Chemical Corporation. When an epoxy compound is used as the thermosetting resin, the content of the epoxy compound is preferably 30 parts by mass or more, more preferably 35 parts by mass or more, preferably 60 parts by mass or less, more preferably 55 parts by mass or less, and even more preferably 45 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler.

[0043] *Thermosetting Agent The thermosetting agent is selected depending on the thermosetting resin. For example, when the thermosetting resin is an epoxy compound, a thermal anionic polymerization initiator or a thermal cationic polymerization initiator can be preferably selected, and a thermal cationic polymerization initiator that suppresses the curing reaction caused by laser light and enables rapid curing by heat can be more preferably selected. The content of the thermosetting agent can be determined depending on the type of thermosetting agent and the type of thermosetting resin. The content of the thermosetting agent is preferably 1 part by mass or more, more preferably 2 parts by mass or more, particularly preferably 3 parts by mass or more, preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and particularly preferably 6 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler.

[0044] Incidentally, thermal cationic polymerization initiators that are preferably applicable to epoxy compounds are those that generate an acid capable of cationic polymerization of a cationic polymerizable compound by heat, and known iodonium salts, sulfonium salts, phosphonium salts, ferrocenes, etc. can be used. Among these, aromatic sulfonium salts that exhibit good temperature latency can be preferably used. A specific example of an aromatic sulfonium salt-based polymerization initiator is San-Aid SI-60L, a product of Sanshin Chemical Industry Co., Ltd. The content of such a thermal cationic polymerization initiator is preferably 1 part by mass or more, more preferably 2 parts by mass or more, particularly preferably 3 parts by mass or more, preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and particularly preferably 8 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler.

[0045] *Inorganic Filler The inorganic filler in the thermosetting resin composition is used for the purpose of adjusting the durometer A hardness, storage modulus at a frequency of 200 Hz, and storage modulus after curing of the first insulating resin layer 2, and can be silica filler, talc filler, titanium oxide filler, calcium carbonate filler, magnesium oxide filler, silane coupling agent filler, bulking agent filler, softener filler, colorant filler, flame retardant filler, thixotropic agent filler, etc. The inorganic filler may be used alone or in combination of two or more types.

[0046] The content of the inorganic filler is preferably 1 part by mass or more, more preferably 5 parts by mass or more, particularly preferably 8 parts by mass or more, and preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and particularly preferably 12 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler. In particular, when the content of the rubber component is 2 parts by mass or more and 10 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler, by setting the content of the inorganic filler to 8 parts by mass or more and 12 parts by mass or less, the desired durometer A hardness, storage modulus at a frequency of 200 Hz, and storage modulus after curing can be easily achieved.

[0047] (Individualized Second Conductive Film for Repair 40) The individualized second conductive film for repair 40 is a conductive film provided on an exposed portion of the light-transmitting substrate 5 from which the μLED to be repaired has been removed, and has second conductive particles 30 held in the second insulating resin layer 20. As a method for dividing the second conductive film for repair 40, a known method can be used, such as a screen printing method, an inkjet method, or a laser lift-off method, but the laser lift-off method can be preferably used.

[0048] The second insulating resin layer 20 and the second conductive particles 30 constituting the second repair conductive film 40 can have the same configuration as the first insulating resin layer 2 and the first conductive particles 3, except for the average particle size and crush resistance of the conductive particles described in paragraphs 0020 to 0026. They may have different configurations to be adjusted according to the purpose.

[0049] (Repair μLED 1y and its electrode 1ya) The repair μLED 1y and its electrode 1ya can have the same configuration as the μLED 1 and its electrode 1a already described.

[0050] (Light-Transmitting Substrate 5) As the light-transmitting substrate 5, a light-transmitting substrate of a known light-emitting device using μLEDs can be used, and for example, a glass substrate, a quartz substrate, a methacrylate substrate, a polycarbonate substrate, etc. The thickness and degree of light transmissivity of the light-transmitting substrate 5 may be any thickness and degree of light transmissivity that allow the laser lift-off method to be applied.

[0051] Light-Emitting Device The light-emitting device 10 itself, including repaired μLEDs obtained by carrying out the above-described light-emitting device repair method, is also part of the present invention. That is, as shown in Fig. 6 , a light-emitting device 10 having multiple μLEDs 1 mounted on a light-transmitting substrate 5 has a structure in which the majority of the μLEDs 1 are mounted to the light-transmitting substrate 5 by thermocompression bonding via a first conductive film 4 having first conductive particles 3 held in a first insulating resin layer 2, and the remaining few μLEDs 1y (repaired μLEDs) are mounted to the light-transmitting substrate 5 by thermocompression bonding via a repair second conductive film 40 having second conductive particles 30 held in a second insulating resin layer 20. In the embodiment shown in Fig. 6 , the first conductive film 4 and the repair second conductive film 40 are in a thermoset state.

[0052] In this light-emitting device 10, the second conductive particles 30 of the second repair conductive film 40 have a larger particle size than the first conductive particles 3 of the first conductive film 4, or the second conductive particles 30 of the second repair conductive film 40 are less crushed than the first conductive particles 3 of the first conductive film 4. The average particle size and crushing manner of the conductive particles are as described in the light-emitting device repair method of the present invention. Note that when the second conductive particles have a larger particle size than the first conductive particles, the height from the translucent substrate surface to the surface of the repaired μLED is higher than the height of the surrounding unrepaired μLEDs. A light-emitting device of the present invention having such a structure can achieve stable conduction between the opposing electrodes to be connected, eliminating or greatly reducing the need for re-repair of a repaired μLED.

[0053] The present invention will be specifically described below with reference to examples and comparative examples.

[0054] Reference Example <Relationship between degree of crushing of conductive particles and whether LED lights up or not> (Preparation of conductive film) A thermosetting insulating resin composition was prepared by uniformly mixing 50 parts by mass of phenoxy resin (PKHH, Tomoe Engineering Co., Ltd.), 40 parts by mass of liquid epoxy resin (YL980, Mitsubishi Chemical Corporation), 5 parts by mass of fumed silica (RY200, Nippon Aerosil Co., Ltd.), and 5 parts by mass of a cationic polymerization initiator (Sanaid SI-60L, Sanshin Chemical Industry Co., Ltd.).

[0055] The obtained insulating resin composition was applied to a transparent glass substrate having a thickness of 0.7 mm, and dried at 60°C for 3 minutes to form a 4 μm-thick thermosetting insulating resin layer. Conductive particles 1 to 7 (Micropearl Series AU, Sekisui Chemical Co., Ltd.) having the average particle diameters and 20% compressive moduli (20% K values) shown in Table 1 were added to this insulating resin layer at a particle density of 58,000 particles / mm. 2 A conductive film was fabricated on the light-transmitting substrate by regularly arranging the ITO electrodes in a hexagonal lattice pattern such that: A transparent ITO electrode pattern with a thickness of 200 nm was formed on the conductive film side of the light-transmitting substrate, corresponding to the electrodes of the μLED to be mounted.

[0056] (Creation of Light-Emitting Device) μLEDs (number of electrodes: 2, electrode dimensions: length 15 μm × width 12 μm, electrode height: 2 μm) with a size of 60 μm length × 30 μm width × 10 μm height (including electrodes) with electrodes formed on one side of the conductive film were placed at a density of 2518 pieces / cm 2 The μLEDs on the μLED wafer, arranged with a vertical pitch of 216 μm and a horizontal pitch of 192 μm, were placed side-by-side with their respective μLEDs facing each other, and the μLEDs were transferred using the laser lift-off method under the following conditions. A light-emitting device was then fabricated by thermocompression bonding (main bonding) using a heat tool (160°C, constant 60 MPa, 30 seconds). This allowed the crushing rate of conductive particles 1 to 7 before and after bonding to be compared in approximately 5% increments, enabling the relationship between the crushing rate and whether the particles lit up or not to be examined.

[0057] Laser lift-off device used: Invisi LUM-XTR manufactured by Shin-Etsu Engineering Co., Ltd. Laser: Excimer laser with an oscillation wavelength of 248 nm Laser light pulse energy: 600 J Fluence: 150 J / cm 2 Pulse width (irradiation time): 30,000 picoseconds Pulse frequency: 0.01 kHz Number of irradiation pulses: 1 pulse for each μLED

[0058] The results of the on / off operation of the obtained light-emitting device are shown in Table 1. The results in Table 1 indicate that it is difficult to light up the μLED unless the conductive particles break through the surface oxide film of the transparent electrode of the translucent substrate and ensure a certain contact area with the counter electrode. For example, Conductive Particle 2 has a 20% higher K value and is harder than Conductive Particle 1, but because the size of the conductive particles is too small, the contact area with the electrode is insufficient, and it is believed that its superiority could not be confirmed. Therefore, when repairing the μLED of a light-emitting device, it is necessary to consider the size of the conductive particles and the amount of crushing of the conductive particles after repair.

[0059]

[0060] Light-emitting devices were produced in the same manner as in Examples 1-6 and Comparative Examples 1-5. However, the conductive particles in the pressure-bonding conductive film had the average conductive particle diameter (particle diameter [μm]) and 20% K value [MPa] shown in Table 2, and the insulating resin layer thickness (resin thickness [μm]) of the conductive film was set to the thickness shown in Table 2. In addition, the particle diameter (particle crushing [μm]) in the thickness direction (crushing direction) of the conductive particles after thermocompression bonding and the distance from the translucent substrate surface to the μLED surface after thermocompression bonding (μLED outermost surface height [μm]) were set as shown in Table 2.

[0061] Next, for the unlit μLEDs of the light-emitting device, the μLEDs were peeled off together with the heat-cured conductive film directly below them by a laser lift-off method under the following conditions.

[0062] Laser lift-off device used: Invisi LUM-XTR manufactured by Shin-Etsu Engineering Co., Ltd. Laser: Excimer laser with an oscillation wavelength of 248 nm Laser light pulse energy: 600 J Fluence: 150 J / cm 2 Pulse width (irradiation time): 30,000 picoseconds Pulse frequency: 0.01 kHz Number of irradiation pulses: 1 pulse for each μLED

[0063] Next, a repair conductive film shown in Table 2 was transferred to the exposed portion of the translucent substrate from which the unlit μLED and the thermally cured conductive film directly below it had been removed, following the laser lift-off method described above. Then, a repair μLED identical to the μLED used during the actual bonding was transferred and further thermocompression bonded. However, the conductive particles in the repair conductive film had the average particle diameter (particle diameter [μm]) and 20% K value [MPa] shown in Table 2, and the insulating resin layer thickness of the conductive film (resin thickness [μm]) was set to the thickness shown in Table 2. Furthermore, the particle diameter (particle crushing [μm]) in the thickness direction (crushing direction) of the conductive particles after thermocompression bonding during repair, and the distance from the surface of the translucent substrate to the μLED light-emitting surface after thermocompression bonding (μLED outermost surface height [μm]) were set as shown in Table 2. The results of the operation confirmation of the light-emitting device after repair are shown in Table 2.

[0064] In addition, Examples 1-2 and Comparative Examples 1-3 are examples that focus on the importance of the size of the conductive particles, Examples 3-4 and Comparative Examples 4-5 are examples that focus on the importance of the resistance of the conductive particles to crushing, and Examples 5-6 are examples that focus on the importance of both the size of the conductive particles and the resistance of the conductive particles to crushing.

[0065]

[0066] The results of Example 1-2 in Table 2 show that repair was successful when the size of the conductive particles in the repair conductive film was larger than that of the conductive particles in the conductive film used for the final pressure bonding. In contrast, the results of Comparative Example 1-3 show that repair was unsuccessful when the size of the conductive particles in the repair conductive film was the same as or smaller than that of the conductive particles in the conductive film used for the final pressure bonding.

[0067] Furthermore, the results of Example 3-4 in Table 2 show that repair was successful when the conductive particles in the repair conductive film were more difficult to crush (harder) than the conductive particles in the conductive film used for the final pressure bonding. In contrast, the results of Comparative Example 4-5 show that repair was unsuccessful when the conductive particles in the repair conductive film were the same in crush resistance (hardness) as or softer than the conductive particles in the conductive film used for the final pressure bonding.

[0068] From the results of Example 5-6 in Table 2, it can be seen that the size and crush resistance (hardness) of the conductive particles in the repair conductive film were larger and more crush-resistant (harder) than the conductive particles in the conductive film used for the actual pressure bonding, and the repair was successful.

[0069] 10 Light-emitting device 1 μLED 1a Electrode of μLED 1x Unlit μLED to be removed 1y Repair μLED 1ya Electrode of repair μLED 1y 2 First insulating resin layer 3 First conductive particle 4 First conductive film 5 Translucent substrate 20 Second insulating resin layer 30 Second conductive particle 40 Second conductive film for repair 100 μLED 100a Electrode of μLED 100 101 Insulating resin layer 102 Conductive particle 102a Conductive particle between electrode of translucent substrate 104 and electrode 100Ra of repair μLED 100R 103 Conductive film 103a Repair conductive film 104 Translucent substrate 100R Repair μLED 100Ra Electrode of repair μLED 100R H, 105 Heat tool L Laser

Claims

1. A method for repairing a light-emitting device in which a plurality of μLEDs are mounted on a translucent substrate by thermocompression via a first conductive film in which first conductive particles are held in a first insulating resin layer, the method comprising the following steps (A) to (F): (Step A) identifying a μLED to be repaired from the plurality of mounted μLEDs; (Step B) removing the μLED to be repaired from the translucent substrate by a laser lift-off method; (Step C) providing a repair conductive film in which second conductive particles are held in a second insulating resin layer in an individual piece on a portion of the translucent substrate from which the μLED has been removed; (Step D) providing the repair μLED on the repair conductive film provided on the translucent substrate; (Step E) mounting the repair μLED on the translucent substrate by thermocompression; and (Step F) confirming the operation of the light-emitting device in which the repair μLED is provided, A repair method, in which the second conductive particles of the second conductive film for repair have a larger particle size than the first conductive particles of the first conductive film, or the second conductive particles of the second conductive film for repair are more difficult to crush than the first conductive particles of the first conductive film.

2. A repair method according to claim 1, wherein the average particle diameter D1 of the first conductive particles is 1 μm or more and 5 μm or less, and the average particle diameter D2 of the second conductive particles is 1.1 times or more and 2 times or less than D1.

3. A repair method as described in claim 1, wherein the 20% compressive elastic modulus E1 (20% K value) of the first conductive particles is 2000 MPa or more and 6000 MPa or less, and the 20% compressive elastic modulus E2 (20% K value) of the second conductive particles is 1.1 times or more and 2.5 times or less than E1.

4. The repair method according to claim 1, wherein the first conductive film and the second repair conductive film each have anisotropic conductivity.

5. A repair method as described in claim 1, in which in step A, a μLED that does not light up when the light-emitting device is operated is identified as a μLED to be repaired.

6. The repair method according to claim 1, wherein in step B, the μLED to be repaired is removed together with the first conductive film directly below it by a laser lift-off method.

7. A repair method according to claim 1, wherein in step C, the repair conductive film is provided in the form of individual pieces by a laser lift-off method.

8. The repair method according to claim 1, wherein in step D, the repair LED is installed by a laser lift-off method.

9. A light-emitting device having a plurality of μLEDs mounted on a translucent substrate, wherein a majority of the μLEDs are mounted on the translucent substrate by thermocompression via a first conductive film in which first conductive particles are held in a first insulating resin layer, and a remaining small number of μLEDs are mounted on the translucent substrate by thermocompression via a repair second conductive film in which second conductive particles are held in a second insulating resin layer, wherein the second conductive particles of the repair second conductive film have a larger particle size than the first conductive particles of the first conductive film, or the second conductive particles of the repair second conductive film are not crushed more than the first conductive particles of the first conductive film.

Citation Information

Patent Citations

  • Repairing device and repairing method

    CN112993091A

  • Micro LED display module and method of manufacturing the same

    US20210005588A1

  • Repair component having micro LED chip, method for manufacturing the same, repair method, method for manufacturing light-emitting device, and light-emitting device

    WO2021182139A1