Method for producing polypeptide
The method of solid-phase synthesis and chemical linking of specific sequence blocks in elastin-like polypeptides addresses the challenges of high hydrophobicity and synthesis difficulties, resulting in effective gel-forming polypeptides with enhanced structural integrity and properties.
Patent Information
- Application Number
- PCT/JP2024/011171
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
The production of elastin-like polypeptides is hindered by the difficulty in handling their high hydrophobicity, impurities from genetic recombination technology, and challenges in chemical synthesis due to the length of the polypeptides and potential inhibition of fiber formation by chemical reaction linkages.
A method involving solid-phase synthesis and chemical linking of terminal regions of divided polypeptide fragments using a specific sequence structure, such as (XGGXG)n and (VPGXG)m blocks, to produce elastin-like polypeptides without relying on genetic recombination, utilizing chemical reactions like thiol-maleimide coupling for efficient synthesis and gel formation.
This method enables the production of elastin-like polypeptides with improved gel-forming properties and structural integrity, overcoming the limitations of traditional methods by achieving high storage modulus and maintaining solid properties under strain, while avoiding the drawbacks of genetic recombination and chemical synthesis challenges.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Method for producing polypeptides
[0001] The present invention relates to a method for producing a polypeptide, and the like.
[0002] Elastin is an important functional protein that provides elasticity and stretchability to biological tissues. However, its highly hydrophobic nature makes it difficult to handle, significantly slowing down its use as a material. The present inventors have developed a doubly hydrophobic elastin-like polypeptide (GPG) that forms self-assembling nanofibers in water (Non-Patent Document 1). The resulting fibers can form physical gels, which are expected to be useful in biomaterials such as artificial blood vessels, cell culture substrates, and functional cosmetics.
[0003] Biomacromolecules. 14 (2013) 1028-1034. https: / / doi.org / 10.1021 / bm301887m.Journal of Peptide Science. 2016 May;22(5):334-42.
[0004] In Non-Patent Document 1, GPG is produced intracellularly using genetic engineering technology. However, this production technology is undesirable due to the presence of biological impurities, the difficulty of quality control, and consumer resistance to recombinant technology.
[0005] On the other hand, because elastin-like polypeptides consist of several tens of amino acid residues or more, it has been thought that chemical synthesis is difficult (Non-Patent Document 2). Furthermore, when multiple fragments are linked using a chemical reaction, it has been thought that the linkage sites formed by the chemical reaction within the resulting elastin-like polypeptide would inhibit fiber formation from the elastin-like polypeptide.
[0006] An objective of the present invention is to provide a method for producing an elastin-like polypeptide without relying on genetic recombination technology.
[0007] In view of the above problems, the present inventors have conducted extensive research and have found that (SEQ ID NO: 1:X 1 GGX 2 G) n G sequence block consisting of 1 are the same or different and represent V or L, and X 2are the same or different and represent V or L, and n represents an integer of 2 or more.) and (SEQ ID NO: 2: VPGX 3 G) m P sequence block consisting of 3 are the same or different and represent any amino acid, and m is an integer of 5 or greater.) The inventors have found that the above-mentioned problems can be solved by a method for producing a polypeptide containing an elastin-like block peptide sequence comprising the polypeptide and / or divided fragments of the polypeptide, the method comprising: (a) a step of solid-phase synthesis of the polypeptide and / or divided fragments of the polypeptide; and / or (b) a step of linking the terminal regions of multiple divided fragments of the polypeptide by a chemical reaction. Based on this finding, the inventors have conducted further research and have completed the present invention. Specifically, the present invention encompasses the following aspects.
[0008] Item 1. (SEQ ID NO: 1:X 1 GGX 2 G) n G sequence block consisting of 1 are the same or different and represent V or L, and X 2 are the same or different and represent V or L, and n represents an integer of 2 or more.) and (SEQ ID NO: 2: VPGX 3 G) m P sequence block consisting of 3 are the same or different and represent any amino acid, and m represents an integer of 5 or more.), the method for producing a polypeptide comprising an elastin-like block peptide sequence comprising the polypeptide and / or divided fragments of the polypeptide, the method comprising: (a) a step of solid-phase synthesis of the polypeptide and / or divided fragments of the polypeptide; and / or (b) a step of linking the terminal regions of a plurality of divided fragments of the polypeptide by a chemical reaction.
[0009] Item 2. The production method according to Item 1, wherein the sequence structure of the elastin-like block peptide sequence is, from the N-terminus, G sequence block-P sequence block-G sequence block, G sequence block-P sequence block-P sequence block-G sequence block, P sequence block-G sequence block, or G sequence block-P sequence block.
[0010] Item 3. The production method according to Item 1 or 2, which comprises the step (a) and wherein the number of amino acid residues in the divided fragments of the polypeptide is 30 or more.
[0011] Item 4. The method according to Item 3, wherein the number of amino acid residues in the divided fragments of the polypeptide is 50 or more.
[0012] Item 5. A production method according to any one of Items 1 to 4, comprising the step (a), wherein the divided fragments in the step (a) comprise all or part of the P sequence block.
[0013] Item 6. The production method according to any one of Items 1 to 5, which comprises the step (a), and wherein the polypeptide and / or the divided fragment of the polypeptide comprises a hydrophilic amino acid-rich sequence.
[0014] Item 7. The production method according to any one of Items 1 to 6, which includes the step (b), and wherein the chemical reaction in the step (b) is a reaction between a thiol group of amino acid residue a in the terminal region of one of the cleaved fragments a and a vinyl group or maleimide group added to amino acid residue b in the terminal region of the other cleaved fragment b.
[0015] Item 8. The terminal region of the divided fragment b has the general formula (A):
[0016]
[0017] [In the formula: R 1 represents a vinyl group or a maleimide group. 1 R represents a linker containing an amide bond or an ester bond. 2 indicates an aromatic ring. 2 Item 8. The method for producing according to Item 7, wherein a group represented by the following formula (I) is added to the compound represented by the formula (I):
[0018] Item 9. The production method according to any one of Items 1 to 8, wherein the polypeptide has 80 or more amino acid residues.
[0019] Item 10. The polypeptide is represented by the following sequence: 1 GGX 2 G) n G sequence block consisting of 1 are the same or different and represent V or L, and X 2are the same or different and represent V or L, and n represents an integer of 2 or more.) and (SEQ ID NO: 2: VPGX 3 G) m P sequence block consisting of 3 (c) the sequence structure of the elastin-like block peptide sequence is, from the N-terminus, a G sequence block-P sequence block; and / or (d) m is an integer of 5 to 22.
[0020] Item 11. (SEQ ID NO: 1:X 1 GGX 2 G) n G sequence block consisting of 1 are the same or different and represent V or L, and X 2 are the same or different and represent V or L, and n represents an integer of 4 or more.) and (SEQ ID NO: 2: VPGX 3 G) m P sequence block consisting of 3 (c) the sequence structure of the elastin-like block peptide sequence is, from the N-terminus, a G sequence block-P sequence block; and / or (d) m is an integer of 5 to 22.
[0021] Item 12. The polypeptide according to Item 11, wherein m is 13 to 22.
[0022] Item 13. A gel composition comprising the polypeptide according to Item 11 or 12.
[0023] The present invention provides a method for producing an elastin-like polypeptide without relying on genetic recombination technology, and also provides an elastin-like polypeptide with a novel structure that is suitable for production by the method.
[0024]
[0033] Figure 1 shows MALDI-TOF MS data and HPLC data for the polypeptide (MG5PPPPP) synthesized in Test Example 1. Figure 2 shows MALDI-TOF MS data for the polypeptide (MG5P) synthesized in Test Example 2. Figure 3 shows MALDI-TOF MS data for the polypeptide (MG5PP) synthesized in Test Example 2. Figure 4 shows MALDI-TOF MS data for the polypeptide (PHis) synthesized in Test Example 2. Figure 5 shows MALDI-TOF MS data for the polypeptide (PPHis) synthesized in Test Example 2. Figure 6 shows MALDI-TOF MS data for the polypeptide (PPPHis) synthesized in Test Example 2. Figure 7 shows HPLC data and MALDI-TOF MS data for the polypeptide (MG5P-PHis) synthesized in Test Example 3. Figure 8 shows HPLC data and MALDI-TOF MS data for the polypeptide (MG5P-PPHis) synthesized in Test Example 3. Figure 9 shows HPLC data and MALDI-TOF MS data for the polypeptide (MG5P-PPPHis) synthesized in Test Example 3. 1 shows HPLC data and MALDI-TOF MS data for the polypeptide (MG5PP-PPPHis) synthesized in Test Example 3. 1 shows an atomic force microscope image of the MG5P-PPPHis gel in Test Example 4. 1 shows the measurement results of the storage modulus (G') in frequency dispersion in Test Example 5. GP2 shows the measurement results of the MG5P-PHis gel, GP3 shows the measurement results of the MG5P-PPHis gel, GP4 shows the measurement results of the MG5P-PPPHis gel, and GP5 shows the measurement results of the MG5PP-PPPHis gel. 1 shows the measurement results of the loss tangent (tanδ) in frequency dispersion in Test Example 5. GP2 shows the measurement results of the MG5P-PHis gel, GP3 shows the measurement results of the MG5P-PPHis gel, GP4 shows the measurement results of the MG5P-PPPHis gel, and GP5 shows the measurement results of the MG5PP-PPPHis gel. 1 shows the measurement results of the loss tangent (tanδ) in strain dispersion in Test Example 5. GP2 shows the measurement results for MG5P-PHis gel, GP3 shows the measurement results for MG5P-PPHis gel, GP4 shows the measurement results for MG5P-PPPHis gel, and GP5 shows the measurement results for MG5PP-PPPHis gel. Figure 1 shows MALDI-TOF MS data for the polypeptide (MPP) synthesized in Test Example 6.1 shows MALDI-TOF MS data for the polypeptide (MPPP) synthesized in Test Example 6. 2 shows MALDI-TOF MS data for the polypeptide (MG4PP) synthesized in Test Example 6. 3 shows MALDI-TOF MS data for the polypeptide (PG5His) synthesized in Test Example 6. 4 shows MALDI-TOF MS data for the polypeptide (PPG4His) synthesized in Test Example 6. 5 shows MALDI-TOF MS data for the polypeptide (PPG5His) synthesized in Test Example 6. 6 shows MALDI-TOF MS data for the polypeptide (MPP-PG5His) synthesized in Test Example 7. 7 shows HPLC data and MALDI-TOF MS data for the polypeptide (MPP-PPG5His) synthesized in Test Example 7. 8 shows HPLC data and MALDI-TOF MS data for the polypeptide (MPPP-PPG5His) synthesized in Test Example 7. 1 shows HPLC data and MALDI-TOF MS data for the polypeptide (MPP-PPG4His) synthesized in Test Example 7. 1 shows HPLC data and MALDI-TOF MS data for the polypeptide (MG4PP-PPHis) synthesized in Test Example 7.
[0025] In this specification, the expressions "contain" and "comprise" include the concepts of "contain," "comprise," "consist essentially of," and "consist only of."
[0026] In this specification, amino acid residues in an amino acid sequence may be referred to simply as the amino acid or by a specific amino acid name (valine, leucine), etc. In addition, amino acid residues in an amino acid sequence may be referred to by a single-letter code for the amino acid.
[0027] In one aspect, the present invention provides a method for the preparation of a nucleic acid sequence comprising the steps of: 1 GGX 2 G) n G sequence block consisting of 1 are the same or different and represent V or L, and X 2 are the same or different and represent V or L, and n represents an integer of 2 or more.) and (SEQ ID NO: 2: VPGX 3 G) m P sequence block consisting of 3are the same or different and represent any amino acid, and m is an integer of 5 or greater.) The present invention relates to a method for producing a polypeptide (sometimes referred to herein as "the polypeptide of the present invention") comprising an elastin-like block peptide sequence comprising the polypeptide and / or divided fragments of the polypeptide, the method comprising: (a) a step of solid-phase synthesis of the polypeptide and / or divided fragments of the polypeptide; and / or (b) a step of linking the terminal regions of multiple divided fragments of the polypeptide by a chemical reaction (sometimes referred to herein as "the production method of the present invention"). This method is described below.
[0028] The polypeptide of the present invention, which is the subject of production, will now be described.
[0029] The G sequence block is an amino acid sequence shown in SEQ ID NO: 1 (X 1 GGX 2 G) repeat sequence (X 1 GGX 2 G) n There are no particular limitations on the G sequence block, as long as it is a block consisting of the following. The G sequence block is usually a block that can adopt a β-sheet structure. The G sequence block can impart the ability to form fibers by self-assembly to the polypeptide.
[0030] X 1 are the same or different and represent V or L, and X 2 are the same or different and represent V or L. X 1 and X 2 is preferably V.
[0031] n represents an integer of 2 or greater. By setting n to 2 or greater, the polypeptide of the present invention can form fibrous self-assemblies. n is preferably 3 or greater, more preferably 4 or greater, even more preferably 4 to 20, still more preferably 4 to 12, particularly more preferably 4 to 8, and particularly even more preferably 4 to 6.
[0032] The P sequence block is the amino acid sequence shown in SEQ ID NO: 2 (VPGX 3 G) repeat sequence (VPGX 3 G) mThe P sequence block is not particularly limited as long as it is a block consisting of the above. The P sequence block is usually a block that can form a β-turn structure. The P sequence block gives the polypeptide a lower critical solution temperature (LCST), and the polypeptide self-assembles and phase-separates from an aqueous solution above the LCST. The presence of the P sequence block, or the P sequence block in combination with other sequence structures of the polypeptide of the present invention, further improves the efficiency of solid-phase synthesis.
[0033] The LCST of the polypeptide of the present invention (solvent: water, concentration: 0.03 wt%) is, for example, 10 to 30°C, preferably 15 to 25°C.
[0034] X 3 X represents any amino acid, whether identical or different. 3 Examples of the amino acid represented by the formula (X) include amino acids having a basic side chain such as lysine, arginine, and histidine; amino acids having an acidic side chain such as aspartic acid and glutamic acid; amino acids having an uncharged polar side chain such as glycine, asparagine, glutamine, serine, threonine, tyrosine, and cysteine; amino acids having a nonpolar side chain such as alanine, valine, leucine, isoleucine, proline, phenylalanine, methionine, and tryptophan; amino acids having a β-branched side chain such as threonine, valine, and isoleucine; and amino acids having an aromatic side chain such as tyrosine, phenylalanine, tryptophan, and histidine. 3 The amino acid represented by is preferably an amino acid other than proline.
[0035] X 3 The LCST can be adjusted by the amino acid represented by X. 3 If the amino acid represented by X in the P sequence block is a hydrophilic amino acid, the LCST tends to be too high, which is not preferable. 3It is preferred that some of the amino acids represented by are non-aromatic hydrophobic amino acids such as valine and leucine (preferably valine), and other amino acids are aromatic hydrophobic amino acids such as phenylalanine and tryptophan (preferably phenylalanine). In this case, X in the P sequence block 3 X to the total number of 3 The ratio of the number of non-aromatic hydrophobic amino acids represented by X in the P sequence block is, for example, 60 to 95%, preferably 70 to 90%, more preferably 75 to 85%. 3 X to the total number of 3 The ratio of the number of aromatic hydrophobic amino acids represented by X is, for example, 5 to 40%, preferably 10 to 30%, more preferably 15 to 25%. 3 It is preferable that the aromatic hydrophobic amino acids represented by the formula (VPGX) are present as dispersedly as possible, for example, 1 to 10, preferably 2 to 8, more preferably 3 to 7, further preferably 4 to 6, particularly preferably 5 repeat units. 3 G) at a rate of one for each iteration, x 3 It is preferred that repeat units in which the amino acid is an aromatic hydrophobic amino acid occur.
[0036] m represents an integer of 5 or greater. From the viewpoints of a high storage modulus, a low loss tangent, and the ability of a gel obtained from the polypeptide of the present invention to maintain solid properties against strain, m is preferably 5 to 25, more preferably 8 to 25, even more preferably 13 to 25, still more preferably 13 to 22, particularly more preferably 13 to 20, and particularly preferably 14 to 17. In one embodiment of the present invention, m can be 5 to 22 or 13 to 22.
[0037] The elastin-like block peptide sequence is not particularly limited as long as it contains a G sequence block and a P sequence block. The number of G sequence blocks in the elastin-like block peptide sequence is not particularly limited, but is, for example, 1 to 5, preferably 1 to 4, more preferably 1 to 3, even more preferably 1 to 2, and particularly preferably 1. The number of P sequence blocks in the elastin-like block peptide sequence is not particularly limited, but is, for example, 1 to 5, preferably 1 to 4, more preferably 1 to 3, even more preferably 1 to 2, and particularly preferably 1.
[0038] The blocks (between a G sequence block and a P sequence block, between a G sequence block and a G sequence block, and between a P sequence block and a P sequence block) may be directly linked or may be linked via a linker sequence.
[0039] The linker sequence is not particularly limited as long as it does not significantly reduce the fiber-forming ability of the elastin-like block peptide sequence due to its self-assembly, and generally, any amino acid or amino acid sequence can be used without major limitations. The linker sequence may have a length of, for example, 1 to 20 amino acids, preferably 1 to 15 amino acids, more preferably 1 to 10 amino acids, even more preferably 1 to 8 amino acids, and even more preferably 2 to 8 amino acids. Specific examples of linker sequences include the amino acid sequence represented by SEQ ID NO: 9: LWLGSG and the amino acid sequence represented by KL. Furthermore, amino acid sequences obtained by mutation (e.g., substitution, deletion, insertion, addition, preferably substitution, more preferably conservative substitution) of one or more amino acids (e.g., 1 to 5 amino acids, preferably 1 to 3 amino acids, more preferably 1 to 2 amino acids, and even more preferably 1 amino acid) of these amino acid sequences can also be used.
[0040] As used herein, the term "conservative substitution" refers to the substitution of an amino acid with an amino acid having a similar side chain. For example, substitution between amino acids having basic side chains such as lysine, arginine, and histidine constitutes a conservative substitution. Other examples of conservative substitutions include substitution between amino acids having acidic side chains such as aspartic acid and glutamic acid; amino acids having uncharged polar side chains such as glycine, asparagine, glutamine, serine, threonine, tyrosine, and cysteine; amino acids having nonpolar side chains such as alanine, valine, leucine, isoleucine, proline, phenylalanine, methionine, and tryptophan; amino acids having β-branched side chains such as threonine, valine, and isoleucine; and amino acids having aromatic side chains such as tyrosine, phenylalanine, tryptophan, and histidine.
[0041] From the viewpoint of fiber-forming ability through self-assembly, the sequence structure of the elastin-like block peptide sequence is preferably, from the N-terminus, G sequence block-P sequence block-G sequence block, G sequence block-P sequence block-P sequence block-G sequence block, P sequence block-G sequence block, or G sequence block-P sequence block. The sequence structure is particularly preferably G sequence block-P sequence block. In these structures, "-" indicates a direct bond (between blocks) or another sequence (e.g., a linker sequence, etc.).
[0042] The polypeptides of the present invention preferably contain a hydrophilic amino acid-rich sequence. The hydrophilic amino acid-rich sequence can further improve the efficiency of solid-phase synthesis, the ease of purification due to improved polypeptide solubility, and gel-forming properties. The hydrophilic amino acid-rich sequence is not particularly limited as long as it contains a high proportion of hydrophilic amino acids (amino acids with basic side chains, amino acids with acidic side chains, and amino acids with uncharged polar side chains). Examples of the hydrophilic amino acid-rich sequence include amino acid sequences with a length of 3 to 15 or 5 to 10 amino acids, containing hydrophilic amino acids at a ratio of 50% or more, 60% or more, 70% or more, 80% or more, or 90% or more. A preferred hydrophilic amino acid-rich sequence is a consecutive histidine sequence (His tag sequence). The other amino acid sequence preferably contains an amino acid with a functional group that can be used in a crosslinking reaction (e.g., lysine, cysteine, etc.).
[0043] When the polypeptide of the present invention comprises a hydrophilic amino acid-rich sequence, the cell adhesion sequence is located at the terminus (N-terminus and / or C-terminus) of the polypeptide of the present invention, preferably at the C-terminus. The hydrophilic amino acid-rich sequence may be located at either the N-terminus or the C-terminus, or at both the N-terminus and the C-terminus.
[0044] The polypeptide of the present invention can have a cell adhesive sequence at its terminus. The cell adhesive sequence is not particularly limited, and various sequences can be used. The cell adhesive sequence can be one that does not have cell selectivity, such as RGDS (SEQ ID NO: 10), or one that has cell selectivity (e.g., REDV (SEQ ID NO: 22)). Sequences with cell selectivity include, for example, HHH, VVV, TTT, TGA, NNN, KKK, AAA, RRR, YYY, TTT, GAT, GGG, PGH, GQA, QGD, GIG, EKG, KGK, QGF, GMK, GLS, CAG, CNG, KGT, PLG, NRG, CSG, LGL, AVG, GHP, GLI, GVG, G PS, SPG, GPP, GIS, GYL, GEK, QGE, CNY, FPG, GAP, APG, GEC, LPG, GPR, PCG, GDV, IGG, CDG, AVA, FLM, GFD, GTP, GPY, VSG, DGR, GIT, GFL, ASG, GCP, NQG, SGL, GGA, PDG, QAL, GLK, GSP, GEP, GN Examples include S, AKG, DGY, TGP, VGP, SLW, AAG, AGA, ARG, GRD, EGF, GSC, PGQ, HSQ, EAP, RGP, PGD, CNI, GFG, GPT, GDQ, KGE, PFI, QGP, SYW, LPGFPGLK (SEQ ID NO: 11), LPGFPGTP (SEQ ID NO: 12), GPPGLSGPP (SEQ ID NO: 13), FPGPPGPP (SEQ ID NO: 14), LPGLPGPP (SEQ ID NO: 15), FPGLPGPP (SEQ ID NO: 16), GPPGPPGSPG (SEQ ID NO: 17), LPGPPGPP (SEQ ID NO: 18), FPGSPGFPG (SEQ ID NO: 19), GSPGLPGTP (SEQ ID NO: 20), and IGLSGEKG (SEQ ID NO: 21).
[0045] When the polypeptide of the present invention comprises a cell adhesion sequence, the cell adhesion sequence is located at the termini (N-terminus and / or C-terminus) of the polypeptide of the present invention, preferably at the C-terminus. The cell adhesion sequence may be located at either the N-terminus or the C-terminus, or at both. In a preferred embodiment of the present invention, the cell adhesion sequence is located at only one terminus.
[0046] The number of amino acid residues in the elastin-like block peptide sequence is preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, even more preferably 80% or more, and particularly preferably 90% or more of the total number of amino acid residues in the polypeptide of the present invention (100%).
[0047] The polypeptide of the present invention may have, for example, 80 or more amino acid residues, preferably 80 to 250, more preferably 90 to 200, and even more preferably 100 to 180 amino acid residues.
[0048] The polypeptides of the present invention can be composed solely of polymers in which amino acids are linked by amide bonds (typical polypeptides), or can be linked polypeptides in which the terminal amino acid residues of the typical polypeptides are linked together by a chemical reaction. In the latter case, a linker (having, for example, 2-25, 5-20, or 7-15 main chain atoms) containing a bond formed by a chemical reaction is disposed between multiple typical polypeptides (e.g., 2-5, 2-4, 2-3, or 2). The main chain refers to the chain connecting the terminal amino acid residues of the typical polypeptides, and in the case of an intervening ring, refers to the chain obtained by tracing the atoms in the ring so as to obtain the shortest chain length.
[0049] The polypeptide of the present invention may be chemically modified as long as its gel-forming property is not significantly impaired. The presence or absence of the gel-forming property can be evaluated according to Test Examples 4 and 5 described below.
[0050] The polypeptide of the present invention has a C-terminus containing a carboxyl group (-COOH), a carboxylate group (-COO - ), amide (-CONH2) or ester (-COOR).
[0051] Here, R in the ester is, for example, C such as methyl, ethyl, n-propyl, isopropyl, n-butyl, etc. 1-6 Alkyl groups; for example, C groups such as cyclopentyl and cyclohexyl 3-8 Cycloalkyl groups such as phenyl and α-naphthyl 6-12Aryl groups; for example, phenyl-C such as benzyl and phenethyl 1-2 Alkyl group: α-naphthyl-C such as α-naphthylmethyl 1-2 C such as alkyl group 7-14 Aralkyl groups, pivaloyloxymethyl groups, etc. are used.
[0052] In the polypeptide of the present invention, a carboxyl group (or carboxylate) other than that at the C-terminus may be amidated or esterified. In this case, the ester may be, for example, the C-terminal ester described above.
[0053] Furthermore, in the polypeptide of the present invention, the amino group of the N-terminal amino acid residue is protected by a protecting group (e.g., a C group such as a formyl group or an acetyl group). 1-6 C such as alkanoyl 1-6 those in which the N-terminal glutamine residue that can be generated by cleavage in vivo is pyroglutamated; those in which the substituents on the side chains of amino acids in the molecule (e.g., -OH, -SH, amino group, imidazole group, indole group, guanidino group, etc.) are protected by an appropriate protecting group (e.g., C group such as formyl group, acetyl group, etc.); 1-6 C such as alkanoyl group 1-6 Also included are those protected by an acyl group or the like, or conjugated proteins such as so-called glycoproteins to which sugar chains are bound.
[0054] The polypeptides of the present invention may be in the form of a pharmaceutically acceptable salt with an acid or base. The salt is not particularly limited as long as it is pharmaceutically acceptable, and both acidic and basic salts can be used. Examples of acidic salts include inorganic acid salts such as hydrochloride, hydrobromide, sulfate, nitrate, and phosphate; organic acid salts such as acetate, propionate, tartrate, fumarate, maleate, malate, citrate, methanesulfonate, and paratoluenesulfonate; and amino acid salts such as aspartate and glutamate. Examples of basic salts include alkali metal salts such as sodium salt and potassium salt; and alkaline earth metal salts such as calcium salt and magnesium salt.
[0055] The polypeptide of the present invention may be in the form of a solvate. The solvent is not particularly limited as long as it is pharmaceutically acceptable, and examples thereof include water, ethanol, glycerol, and acetic acid.
[0056] In step (a), the polypeptide of the present invention and / or a fragment of the polypeptide of the present invention is synthesized by solid phase synthesis.
[0057] The fragments of the polypeptide of the present invention are polypeptides consisting of a part of the amino acid sequence of the polypeptide of the present invention, and are not particularly limited insofar as they are so.
[0058] The number of amino acid residues in the divided fragments is, for example, 30 or more, preferably 40 or more, and more preferably 50 or more. As long as the divided fragments are of the polypeptide of the present invention, even such long polypeptides can be subjected to solid phase synthesis.
[0059] The divided fragments preferably contain all or part of the P sequence block of the polypeptide of the present invention. This can further improve the efficiency of solid-phase synthesis. 3 G) The number of repeats is preferably 3 or more, more preferably 5 or more, and the upper limit is not particularly limited and can be the upper limit of the number of repeats of the P sequence block in the polypeptide of the present invention. The number of amino acid residues in the P sequence block is preferably 25% or more, more preferably 30% or more, even more preferably 35% or more, even more preferably 40% or more, particularly preferably 50% or more, especially more preferably 60% or more, and particularly preferably 70% or more, relative to the number of amino acid residues in the divided fragment (100%).
[0060] In one embodiment of the present invention, the split fragments preferably do not contain the G sequence block of the polypeptide of the present invention, which can further improve the efficiency of solid-phase synthesis.
[0061] In one aspect of the present invention, the split fragments preferably contain a hydrophilic amino acid-rich sequence of the polypeptide of the present invention, which can further improve the efficiency of solid-phase synthesis, the ease of purification due to improved solubility of the polypeptide, gel-forming properties, etc.
[0062] In one embodiment of the present invention, the amino acid residues in the terminal regions of the split fragments may be amino acid residues having side chains that can be used in the chemical reaction for linkage in the step (b) described below, or may be amino acid residues to which a group that can be used in the chemical reaction has been added.
[0063] The amino acid residues in the terminal region are, for example, amino acid residues in a region of 1 to 5 amino acids from the terminal, preferably amino acid residues in a region of 1 to 3 amino acids, more preferably amino acid residues in a region of 1 to 2 amino acids, and particularly preferably amino acid residues in the terminal amino acids.
[0064] The amino acid residue having a side chain that can be used in a chemical reaction is preferably a cysteine residue, the thiol group of which can be used for linkage via a thiol-ene reaction or a Michael addition reaction.
[0065] Groups that can be used in chemical reactions are preferably vinyl groups and maleimide groups, and particularly preferably vinyl groups. The vinyl group can be used in a thiol-ene reaction with a thiol group, and the maleimide group can be used in a Michael addition reaction with a thiol group. From the viewpoint of the reaction efficiency of the step (b) described below, the terminal region of the split fragment is preferably provided with a group represented by the general formula (A):
[0066]
[0067] [In the formula: R 1 represents a vinyl group or a maleimide group. 1 R represents a linker containing an amide bond (-C(=O)-NH-) or an ester bond (-C(=O)-O-). 2 indicates an aromatic ring. 2 represents a linker.] is preferably added.
[0068] R 1 The maleimide group represented by formula (B):
[0069]
[0070] It is a group represented by the following formula:
[0071] L1 The number of atoms constituting the main chain of the linker represented by is preferably 2 to 5, more preferably 2 to 4, even more preferably 2 to 3, and particularly preferably 2. 1 The linker represented by L is a chain structure that does not contain a ring structure. 1 The linker represented by is particularly preferably an amide bond (-C(=O)-NH-).
[0072] R 2 The aromatic ring represented by the formula (I) can be, for example, an aromatic ring having 5 to 20 carbon atoms, preferably 5 to 12, and more preferably 5 to 7. A particularly preferred example of the aromatic ring is a benzene ring.
[0073] L 2 The number of atoms constituting the main chain of the linker represented by L is preferably 1 to 5, more preferably 1 to 3, and even more preferably 2. 2 The linker represented by L is a chain structure that does not contain a ring structure. 2 The linker represented by is particularly preferably —CH2—C(═O)—.
[0074] The solid phase synthesis is not particularly limited and can be carried out according to or in accordance with a known method.
[0075] The general steps of solid-phase synthesis are as follows: An amino acid (protected amino acid) whose N-terminus is protected with a protecting group (typically Fmoc or Boc) is bound to a solid, insoluble support (typically polystyrene resin beads) at the C-terminus of the protected amino acid, optionally via a linker. Next, unreacted protected amino acids, i.e., protected amino acids not bound to the support, are removed. Next, the protecting group of the protected amino acid is removed under conditions that do not cause the support-bound protected amino acid to be released from the support. Separately, a second protected amino acid is prepared in which the N-terminus of the amino acid to be bound to the support-bound amino acid is protected with a protecting group. The second protected amino acid is added to the support-bound amino acid, and the N-terminus of the support-bound amino acid and the C-terminus of the second protected amino acid are condensed. Next, the unreacted second protected amino acid is removed, and then the protecting group of the second protected amino acid is removed. A third amino acid whose N-terminus is protected with a protecting group is added, and the N-terminus of the second amino acid and the C-terminus of the third protected amino acid are condensed. This procedure is repeated to synthesize a peptide having the desired amino acid sequence bound to the carrier, which is then separated from the carrier to obtain the desired peptide.
[0076] Examples of protecting groups for amino groups on the main chain include 9-fluorenylmethyloxycarbonyl (Fmoc), tertiary-butoxycarbonyl (Boc), benzyloxycarbonyl (Z), tertiary-amyloxycarbonyl, isobornyloxycarbonyl, 4-methoxybenzyloxycarbonyl, 2-chlorobenzyloxycarbonyl (Cl-Z), 2-bromobenzyloxycarbonyl (Br-Z), adamantyloxycarbonyl, trifluoroacetyl, phthalyl, formyl, 2-nitrophenylsulfenyl, diphenylphosphinothioyl, etc. Among these, from the viewpoint of peptide synthesis efficiency and the like, preferred are F-moc and Boc, and particularly preferred is Fmoc.
[0077] If an amino acid contains another group (reactive side chain) that is not desired to react under condensation reaction conditions, a protected amino acid in which this reactive side chain is protected with an appropriate protecting group can be used. Examples of carboxyl-protecting groups include alkyl esters (e.g., methyl, ethyl, propyl, butyl, tert-butyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, 2-adamantyl, etc.), benzyl esters, 2-nitrobenzyl esters, 4-methoxybenzyl esters, 4-chlorobenzyl esters, benzhydryl esters, phenacyl esters, benzyloxycarbonyl hydrazide, tert-butoxycarbonyl hydrazide, and trityl hydrazide. The hydroxyl group of serine can be protected, for example, by esterification or etherification. Examples of groups suitable for this esterification include lower alkanoyl groups such as acetyl (preferably alkanoyl groups having 1 to 3 carbon atoms), aroyl groups such as benzoyl, and groups derived from carbonic acid such as benzyloxycarbonyl and ethoxycarbonyl. Examples of groups suitable for etherification include benzyl, tetrahydropyranyl, and tert-butyl. Examples of protecting groups for the phenolic hydroxyl group of tyrosine include benzyl (Bzl), 2,6-dichlorobenzyl (Cl2-Bzl), 2-nitrobenzyl, Br-Z, and tert-butyl (tBu). Examples of protecting groups for the imidazole group of histidine include paratoluenesulfonyl (Tos), 4-methoxy-2,3,6-trimethylbenzenesulfonyl, dinitrophenyl (DNP), benzyloxymethyl, tert-butoxymethyl (Bum), Boc, trityl (Trt), and Fmoc.
[0078] Examples of carriers include, but are not limited to, styrene resin, acrylamide resin, polyethylene glycol-acrylamide composite resin, and polyoxyethylene-grafted styrene resin. These may be crosslinked with divinylbenzene and may be used alone or in combination. A wide variety of known linkers can be used. Examples of linkers include, but are not limited to, chloromethyl, hydroxymethyl, benzhydrylamine, aminomethyl, 4-benzyloxybenzyl alcohol, 4-methylbenzhydrylamine, phenylacetamidomethyl, 4-hydroxymethylphenylacetamidomethyl, 4-(2',4'-dimethoxyphenyl-hydroxymethyl)phenoxy, 2-chlorotrityl chloride resin, 4-hydroxymethylphenoxyacetic acid (HMPA), 4-hydroxymethylbenzoic acid (HMBA), and 2,4-dimethoxy-4-hydroxybenzophenone.
[0079] The protecting group removal agent may be appropriately selected taking into consideration the protecting group, solid phase support, linker, etc. used. For example, an N,N-dimethylformamide (DMF) solution containing 20% v / v piperidine can be used to remove Fmoc. To reduce the amount of organic solvent used in this step from the perspective of environmental load reduction, an aqueous protecting group removal agent, such as aqueous ethanol containing sodium hydroxide (e.g., 90% aqueous ethanol containing 0.1 M NaOH), can be used. Other protecting group removal agents include a 25% v / v hydrogen bromide / acetic acid solution, anhydrous hydrogen fluoride, methanesulfonic acid, trifluoromethanesulfonic acid, and trifluoroacetic acid (TFA). Furthermore, the 2,4-dinitrophenyl group used as the imidazole-protecting group of histidine can be removed by treatment with thiophenol, and the formyl group used as the indole-protecting group of tryptophan can be removed by alkali treatment with dilute sodium hydroxide, dilute ammonia, etc., in addition to the above-mentioned deprotection by acid treatment in the presence of 1,2-ethanedithiol, 1,4-butanedithiol, etc. Furthermore, the protection and protecting groups of functional groups that should not be involved in the condensation reaction, as well as the elimination of the protecting groups, the activation of functional groups involved in the reaction, the reaction conditions, and the like, can also be appropriately selected from known groups or known means.
[0080] The separated peptide is purified, if necessary, by conventional methods such as extraction, partitioning, reprecipitation, recrystallization, column chromatography, or high performance liquid chromatography.
[0081] In step (b), the terminal regions of the divided fragments of the polypeptide of the present invention are linked together by a chemical reaction.
[0082] The number of fragments to be ligated in step (b) is not particularly limited, and can be, for example, 2 to 5, 2 to 4, 2 to 3, or 2. When the number of fragments is 3 or more, the 3 or more fragments may be ligated simultaneously, or the 3 or more fragments may be ligated sequentially (two fragments are ligated, and the resulting fragment is ligated to another fragment).
[0083] The chemical reaction in step (b) is not particularly limited as long as it is a reaction that can link two molecules via a covalent bond, but is preferably a click reaction from the viewpoints of reaction efficiency, regioselectivity, etc. Among click reactions, from the viewpoint of the safety of the components used in the reaction to living organisms, for example, a thiol-ene reaction, a Michael addition reaction, or a Huisgen cycloaddition reaction is preferred, with the thiol-ene reaction and the Michael addition reaction being preferred, and the thiol-ene reaction being particularly preferred.
[0084] The chemical reaction in step (b) is particularly preferably a reaction between a thiol group in amino acid residue a in the terminal region of one of the fragments a and a vinyl group or maleimide group added to amino acid residue b in the terminal region of the other fragment b. In this embodiment, from the viewpoint of the reaction efficiency of step (b), it is preferable that a group represented by the above-mentioned general formula (A) is added to the terminal region of the fragment b. Furthermore, it is preferable that amino acid residue a is an amino acid residue in the C-terminal region, and amino acid residue b is an amino acid residue in the N-terminal region.
[0085] In step (b), the amount of one of the fragments to be linked relative to 1 mole of the other fragment is, for example, 0.5 to 3 moles, preferably 0.8 to 2 moles.
[0086] The solvent used in step (b) is not particularly limited as long as it dissolves the polypeptide, but water is particularly preferred.
[0087] The reaction solution in step (b) preferably contains a buffer such as a sodium carbonate buffer, and the pH of the reaction solution is preferably 8 to 12, more preferably 9 to 11, and particularly preferably 9.5 to 10.5.
[0088] The reaction liquid may contain additives such as a catalyst, a polymerization initiator, etc. as needed and depending on the type of chemical reaction. During the reaction, radicals can be generated by irradiation with light or heating, and the reaction can proceed.
[0089] The reaction can be carried out under heating, at room temperature, or under cooling, preferably at 30 to 80° C., more preferably 40 to 60° C. The reaction time is not particularly limited, and can usually be 30 minutes to 30 hours.
[0090] After the reaction is completed, the solvent is distilled off, and the product is purified, if necessary, by a conventional method such as extraction, distribution, reprecipitation, recrystallization, column chromatography, or high performance liquid chromatography.
[0091] Step (b) is an efficient and preferred convergent synthetic route. Furthermore, by purifying the synthetic intermediate fragments, the purification procedure for the target polypeptide of the present invention can be facilitated.
[0092] Step (b) can be used for combinatorial synthesis. That is, by preparing multiple types of fragments in advance, these fragments can be combined in any combination and subjected to step (b) to easily produce a variety of polypeptides of the present invention. By using the library of polypeptides of the present invention thus obtained, it becomes possible to more easily and efficiently screen for polypeptides of the present invention that are optimal for a desired purpose.
[0093] By using step (a) and / or step (b) (particularly preferably by using steps (a) and (b) from the viewpoints of production efficiency, safety to living organisms, etc.), it is possible to produce an elastin-like polypeptide without relying on genetic engineering. The polypeptide of the present invention obtained by the production method of the present invention can maintain and / or exhibit the gelling ability of the polypeptide.
[0094] The production method of the present invention is to produce an elastin-like polypeptide having a novel structure (novel polypeptide): (SEQ ID NO: 1:X 1 GGX 2 G) n G sequence block consisting of 1 are the same or different and represent V or L, and X 2 are the same or different and represent V or L, and n represents an integer of 4 or more.) and (SEQ ID NO: 2: VPGX 3G) m P sequence block consisting of 3 (a) a polypeptide comprising an elastin-like block peptide sequence containing, from the N-terminus, a G sequence block and a P sequence block; and (b) a polypeptide comprising an elastin-like block peptide sequence containing, from the N-terminus, a G sequence block and a P sequence block; and (c) a polypeptide comprising an elastin-like block peptide sequence containing, from the N-terminus, a G sequence block and a P sequence block; and (d) a polypeptide comprising an elastin-like block peptide sequence containing, from the N-terminus
[0095] The novel polypeptide is superior to conventional elastin-like polypeptides in that the resulting gel has a high storage modulus and a low loss tangent, and is able to maintain solid properties against strain. From this perspective, it is preferable that the novel polypeptide satisfies the above requirement (d), and it is particularly preferable that the novel polypeptide satisfies both requirements (c) and (d). From the same perspective, m is more preferably 8 to 22, even more preferably 13 to 22, even more preferably 13 to 17, and particularly preferably 14 to 16.
[0096] A gel composition containing the polypeptide of the present invention can be obtained by dissolving the polypeptide of the present invention in a solvent at a temperature below the LCST (e.g., 0-15°C, 2-10°C), and then heating the resulting solution to a temperature above the LCST (e.g., 30-50°C, 30-45°C, 30-40°C) and allowing it to stand for a certain period of time (e.g., 1-300 hours, preferably 8-120 hours, more preferably 12-80 hours). Water is used as the solvent, but a mixed solvent of water and an organic solvent can also be used.
[0097] The concentration of the polypeptide of the present invention in the gel composition of the present invention is, from the viewpoint of gel-forming properties, for example, 0.2 w / v% or more, preferably 0.3 w / v% or more, and more preferably 0.35 w / v% or more. From the viewpoint of facilitating the penetration of other components (e.g., components necessary or suitable for cell culture) into the gel composition of the present invention, the concentration is, for example, 3.0 w / v% or less, preferably 2.0 w / v% or less, more preferably 1.5 w / v% or less, even more preferably 1.0 w / v% or less, and even more preferably 0.8 w / v% or less.
[0098] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples.
[0099] Test Example 1. Polypeptide synthesis 1 (solid phase synthesis) A polypeptide with the following amino acid sequence and structure was synthesized by solid phase synthesis. Amino acid residues are represented by single letter codes.
[0100]
[0101] The details of the synthesis method are as follows.
[0102] <1-1. Abbreviations> DMF: N,N-dimethylformamide HATU: O-(7-azabenzotriazol-1-yl)-N,N,N',N'-tetramethyluronium hexafluorophosphate HCTU: O-(1H-6-chlorobenzotriazol-1-yl)-N,N,N',N'-tetramethyluronium hexafluorophosphate HPLC: High-performance liquid chromatography.
[0103] <1-2. Synthesis Reagents and Solvents> Fmoc-amino acids, HCTU, and HATU were purchased from Merck (Germany). HPLC-grade acetonitrile used for analysis and purification was purchased from Kanto Chemical Co., Ltd. (Tokyo, Japan) and Fujifilm Wako Pure Chemical Co., Ltd. (Osaka, Japan). DMF from Fujifilm Wako Pure Chemical Co., Ltd. was used as is for solid-phase peptide synthesis. Other commercially available reagents were purchased from Merck (Germany), Kanto Chemical Co., Ltd. (Tokyo, Japan), Fujifilm Wako Pure Chemical Co., Ltd. (Osaka, Japan), and Tokyo Chemical Industry Co., Ltd. (Tokyo, Japan) and were used without purification.
[0104] <1-3. Solid-Phase Peptide Synthesis> Solid-phase peptide synthesis was performed using the Fmoc method either automatically or manually. The amino acid reagents used were Fmoc-Cys(Trt)-OH, Fmoc-Glu(OtBu)-OH, Fmoc-Gly-OH, Fmoc-His(l-Trt)-OH, Fmoc-Leu-OH, Fmoc-Lys(Boc)-OH, Fmoc-Phe-OH, Fmoc-Pro-OH, Fmoc-Ser(tBu)-OH, Fmoc-Trp(Boc)-OH, and Fmoc-Val-OH. The solid phase used was 2-chlorotrimethylsilyl polystyrene resin, and the first amino acid residue was manually loaded onto the resin. Peptide elongation was then performed according to the following standard protocol. Fmoc-deprotection was performed with 20% piperidine in DMF (8 min × 2). Coupling was performed in DMF for 60 minutes using Fmoc-amino acid (4 molar equivalents relative to the amino acid loading on the resin), HCTU or HATU (4 molar equivalents), and N-methylmorpholine (8 molar equivalents). Double coupling (repeated coupling steps) was performed as needed. After coupling, unreacted free amino groups were capped by treatment with 20% acetic anhydride and 10% N-methylmorpholine in DMF for 10 minutes. Epimerization-prone amino acid residues were coupled using 1-hydroxybenzotriazole esters prepared in advance using N,N'-diisopropylcarbodiimide.
[0105] <1-4. Automatic Peptide Synthesizer> CS Bio 136X (CSBio) or Syro I (Biotage) was used as the automatic peptide synthesizer.
[0106] <1-5. Manual Peptide Synthesis> Each monomer (1 molar equivalent) was dissolved in a minimum amount of DMF, and HATU (1 molar equivalent) and N-methylmorpholine (2 molar equivalents) were added to prepare a reaction solution. After preactivation for 2 minutes, this solution was added to the resin in a filter-equipped reaction column (Kokusan Chemical, Tokyo), and the reaction was carried out at room temperature for 2 hours. If necessary, the coupling was repeated to complete the reaction.
[0107] <1-6. Cleavage from Resin and Deprotection> Cleavage solution (triisopropylsilane:water:TFA = 1:2:98 v / v solution) was added to the resulting resin and shaken at room temperature for 2 hours. After the reaction, the resin was removed by filtration, and the filtrate was concentrated under reduced pressure. Ice-cold diethyl ether was added to the resulting solid, which was then vortexed and centrifuged, and the supernatant was removed. This diethyl ether washing was repeated twice to obtain the crude product. The crude product was dissolved in aqueous acetonitrile containing 0.1 v / v% TFA, filtered through a 0.45 μm membrane filter, and then purified by preparative HPLC. The resulting fraction was lyophilized to obtain the target peptide.
[0108] <1-7. Analysis and Purification by HPLC> Analysis and purification of peptide and protein segments were performed using an HPLC system from JASCO Corporation (Tokyo, Japan) or a Gilson HPLC system (USA) equipped with a dual pump, mixer, in-line degasser, and tunable UV detector. The mobile phase was monitored for absorption at wavelengths of 220 nm, 254 nm, and 301 nm. If necessary, the column was heated using a column heater or water bath. The mobile phase used was an aqueous solution of acetonitrile supplemented with 0.1 v / v% TFA.
[0109] Before sample injection, the column was typically pre-equilibrated for 10 minutes with the starting solvent composition. After sample injection, the column was run for 10 minutes with the starting solvent composition, followed by a gradient run to the final solvent composition (e.g., 50% acetonitrile). After reaching the final solvent composition, the solvent composition was changed to 95% acetonitrile within 1 minute, and the column was washed for 10 minutes. The solvent composition was then changed to 10% acetonitrile within another 1 minute.
[0110] <1-8. Analytical HPLC> Analytical HPLC was performed using Capcell Pak MG-II (Shiseido, 5 μm, pore size 120 Å, inner diameter 4.6 mm x 250 mm), Jupiter C18 (Phenomenex, 5 μm, pore size 300 Å, inner diameter 4.6 mm x 250 mm), or Jupiter C4 (Phenomenex, 5 μm, 300 Å, inner diameter 4.6 mm x 250 mm) at a flow rate of 1 mL / min.
[0111] <1-9. Preparative HPLC > Preparative HPLC is Capcell pak C18 UG80 (Shiseido, 5 μm, pore size 80 Å, inner diameter 50 mm x 250 mm), Jupiter C18 (Phenomenex, 5 μm, pore size 300 Å, inner diameter 30 mm x 250 mm), Jupiter C18 (Phenomenex, 5 μm, pore size 300 Jupiter C4 (Phenomenex, 5 μm, 300 Å pore size, 30 mm x 250 mm i.d.), or Jupiter C4 (Phenomenex, 5 μm, 300 Å pore size, 21.2 mm x 250 mm i.d.).
[0112] <1-10. Mass spectrometry> Mass spectrometry of the compounds was measured using α-cyano-4-hydroxycinnamic acid (CHCA) as a matrix and a Microflex MALDI-TOF spectrometer (Bruker, Germany).
[0113] <Results> Mass spectrometry confirmed that the target polypeptide (MG5PPPPP) was synthesized (Figure 1). The yield was 1.2%.
[0114] Test Example 2. Polypeptide Synthesis 2 (Solid-Phase Synthesis) Polypeptides with the following amino acid sequences and structures were synthesized by solid-phase synthesis in the same manner as in Test Example 1. Only the C-terminal cysteine residue in MG5P and MG5PP is represented by a three-letter code, and other amino acid residues are represented by a one-letter code. In Phis, PPHis, and PPPHis, the -NH- group to the left of the N-terminal V (valine residue) is a group derived from the valine residue.
[0115]
[0116] Mass spectrometry confirmed that the target polypeptides (MG5P, MG5PP, Phis, PPHis, and PPPHis) were synthesized (Figures 2 to 6). The yields were as follows: MG5P: 19% yield; MG5PP: 16% yield; Phis: 27% yield; PPHis: 15% yield; and PPPHis: 6% yield.
[0117] Test Example 3. Polypeptide synthesis 3 (linking by chemical reaction) A polypeptide having the following amino acid sequence and structure was synthesized.
[0118]
[0119] MG5P-PHis was synthesized by linking MG5P and PHis via a thiol-ene reaction. MG5P-PPHis was synthesized by linking MG5P and PPHis via a thiol-ene reaction. MG5P-PPPHis was synthesized by linking MG5P and PPPHis via a thiol-ene reaction. MG5PP-PPPHis was synthesized by linking MG5PP and PPPHis via a thiol-ene reaction.
[0120] The thiol-ene reaction was carried out as follows: 1.5 molar equivalents of peptide segment 1 (MG5P or MG5PP) and 1.0 molar equivalent of peptide segment 2 (PHis, PPHis, or PPPHis) were weighed into a vial, and sodium carbonate buffer (pH 10) was added to adjust the concentration of peptide segment 2 to 10 mM. Dissolved oxygen was removed from the buffer by bubbling nitrogen gas through it. The reaction solution was heated to 50°C with stirring for 18 hours. The reaction was monitored by analytical HPLC. The mixture was then diluted with 50% acetonitrile aqueous solution containing 0.1 v / v% TFA and purified by preparative HPLC.
[0121] Mass spectrometry confirmed that the target polypeptides (MG5P, MG5PP, Phis, PPHis, and PPPHis) were synthesized (Figures 7 to 10). The yields were as follows: MG5P-PHis: 24% yield; MG5P-PPHis: 24% yield; MG5P-PPPHis: 21% yield; and MG5PP-PPPHis: 15% yield.
[0122] Test Example 4. Gelation of Polypeptide Solution MG5P-PHis, MG5P-PPHis, MG5P-PPPHis, and MG5PP-PPPHis were each dissolved in a 10 wt% aqueous sucrose solution to a final concentration of 0.5 wt%. The resulting polypeptide solution was heated to 37°C and allowed to stand. After 7 days, the polypeptide solution had turned into a transparent gel.
[0123] Furthermore, MG5P-PPHis was dissolved in a 10 wt% sucrose aqueous solution to a final concentration of 0.1 wt%, and the resulting dispersion was kept at 37°C for 7 days. The resulting solution was then dropped onto a mica substrate and dried at 37°C. When the sample was observed with an atomic force microscope (AFM), an entangled nanofiber structure was observed (Figure 11).
[0124] Test Example 5. Dynamic Viscoelasticity Measurement The polypeptide gel obtained in Test Example 4 was set in a rheometer MCR302 adjusted to 37°C and subjected to dynamic viscoelasticity measurement. The measured dynamic viscoelasticity was measured by frequency dispersion, and the storage modulus (G') and loss tangent (tanδ) were measured. The frequency dispersion measurement was performed at a constant strain of 0.1% in the angular frequency range of 100-0.1 rad / s.
[0125] The results of measuring the storage modulus are shown in Figure 12, and the results of measuring the loss tangent are shown in Figure 13. Figure 12 shows that MG5P-PHis, MG5P-PPHis, and MG5P-PPPHis have higher storage moduli than MG5PP-PPPHis. Figure 13 shows that tanδ ≦ 1 for all samples, regardless of the angular frequency ω. Furthermore, Figures 12 and 13 show that MG5P-PPHis has the largest G' and the smallest tanδ, i.e., it forms the hardest and most solid gel.
[0126] Furthermore, when the loss tangent (tanδ) was measured using strain dispersion, it was found that MG5P-PPHis had solid-like properties even under 100% strain, and that with increasing strain, the properties became liquid in the following order: MG5PP-PPPHis, MG5P-PHis, MG5P-PPPHis, and MG5P-PPHis (Figure 14).
[0127] Test Example 6. Polypeptide Synthesis 4 (Solid-Phase Synthesis) Polypeptides with the following amino acid sequences and structures were synthesized by solid-phase synthesis in the same manner as Test Example 1. Only the C-terminal cysteine residue in MPP, MPPP, and MG4PP is represented by a three-letter code, and other amino acid residues are represented by a one-letter code. In Phis, PPHis, and PPPHis, the -NH- to the left of the N-terminal V (valine residue) is a group derived from the valine residue.
[0128]
[0129] Mass spectrometry confirmed that the target polypeptides (MPP, MPPP, MG4PP, PG5His, PPG4His, and PPG5His) were synthesized (Figures 15 to 20). The yields were as follows: MPP: 52% yield; MPPP: 29% yield; MG4PP: 20% yield; PG5His: 17% yield; PPG4His: 10% yield; and PPG5His: 6% yield.
[0130] Test Example 7. Synthesis of Polypeptide 5 (Linking by Chemical Reaction) A polypeptide having the following amino acid sequence and structure was synthesized.
[0131]
[0132] MPP-PG5His was synthesized by linking MPP and PG5His via a thiol-ene reaction. MPP-PPG5His was synthesized by linking MPP and PPG5His via a thiol-ene reaction. MPPP-PPG5His was synthesized by linking MPPP and PPG5His via a thiol-ene reaction. MPP-PPG4His was synthesized by linking MPP and PPG4His via a thiol-ene reaction. MG4PP-PPHis was synthesized by linking MG4PP and PPHis via a thiol-ene reaction.
[0133] The thiol-ene reaction was carried out as follows: 1.5 molar equivalents of peptide segment 1 (MPP, MPPP, or MG4PP) and 1.0 molar equivalent of peptide segment 2 (PG5His, PPG4His, and PPG5His or PPHis) were weighed into a vial, and sodium carbonate buffer (pH 10) was added to adjust the concentration of peptide segment 2 to 10 mM. Dissolved oxygen was removed from the buffer by bubbling nitrogen gas through it. The reaction solution was heated to 50°C with stirring for 18 hours. The reaction was monitored by analytical HPLC. The mixture was then diluted with 50% acetonitrile aqueous solution containing 0.1 v / v% TFA and purified by preparative HPLC.
[0134] Mass spectrometry confirmed that the target polypeptides (MPP-PG5His, MPP-PPG5His, MPPP-PPG5His, MPP-PPG4His, and MG4PP-PPHis) were synthesized (Figures 21 to 25). The yields were as follows: MPP-PG5His: 30% yield. MPP-PPG5His: 23% yield. MPPP-PPG5His: 20% yield. MPP-PPG4His: 20% yield. MG4PP-PPHis: 20% yield.
Claims
1. (SEQ ID NO:1:X 1 GGX 2 G) n A G sequence block consisting of 1 are the same or different and represent V or L, and X 2 are the same or different and represent V or L, and n represents an integer of 2 or more.) and (SEQ ID NO: 2: VPGX 3 G) m P sequence block consisting of 3 and m is an integer of 5 or more. A method for producing a polypeptide comprising an elastin-like block peptide sequence comprising:
2. The manufacturing method described in claim 1, wherein the sequence structure of the elastin-like block peptide sequence is, from the N-terminus, G sequence block-P sequence block-G sequence block, G sequence block-P sequence block-P sequence block-G sequence block, P sequence block-G sequence block, or G sequence block-P sequence block.
3. The method according to claim 1, which comprises the step (a) and wherein the number of amino acid residues in the divided fragments of the polypeptide is 30 or more.
4. The method according to claim 3, wherein the number of amino acid residues in the divided fragments of the polypeptide is 50 or more.
5. The method according to claim 1, comprising the step (a), wherein the split fragment in the step (a) comprises all or a part of the P sequence block.
6. The method according to claim 1, comprising the step (a) and wherein the polypeptide and / or the divided fragment of the polypeptide comprises a hydrophilic amino acid-rich sequence.
7. The method according to claim 1, further comprising the step (b), wherein the chemical reaction in the step (b) is a reaction between a thiol group of an amino acid residue a in the terminal region of one of the split fragments a and a vinyl group or a maleimide group added to an amino acid residue b in the terminal region of the other of the split fragments b.
8. The terminal region of the divided fragment b has the general formula (A): [In the formula: R 1 represents a vinyl group or a maleimide group. 1 R represents a linker containing an amide bond or an ester bond. 2 indicates an aromatic ring. 2 The method according to claim 7 , wherein a group represented by the following formula (I) is added to the compound represented by the formula (I):
9. The method according to any one of claims 1 to 8, wherein the polypeptide has 80 or more amino acid residues.
10. The polypeptide is 1 GGX 2 G) n A G sequence block consisting of 1 are the same or different and represent V or L, and X 2 are the same or different and represent V or L, and n represents an integer of 2 or more.) and (SEQ ID NO: 2: VPGX 3 G) m P sequence block consisting of 3 (a) a G sequence block-P sequence block from the N-terminus side of the elastin-like block peptide sequence, and (b) m is an integer of 5 to 22.
11. (SEQ ID NO:1:X 1 GGX 2 G) n A G sequence block consisting of 1 are the same or different and represent V or L, and X 2 are the same or different and represent V or L, and n represents an integer of 4 or more.) and (SEQ ID NO: 2: VPGX 3 G) m P sequence block consisting of 3(a) a polypeptide comprising an elastin-like block peptide sequence including, from the N-terminus, a G sequence block-P sequence block, and (b) a P sequence block, and (c) an N-terminus of the elastin-like block peptide sequence including, from the N-terminus, a G sequence block-P sequence block, and / or (d) an integer of 5 to 22.
12. The polypeptide of claim 11, wherein m is 13 to 22.
13. A gel composition comprising the polypeptide according to claim 11 or 12.
Citation Information
Patent Citations
Temperature-responsive composite polymer
JP2012232961A
Decomposable thiol-ene polymer and method for producing the same
JP2018507908A
polypeptide
WO2021090787A1
Cited By
composition
WO2025089316A1