Molded body, downhole tool member, and downhole tool

By integrating a cyclic ester, basic metal oxide, and carboxylic acid anhydride into the glycolic acid polymer composition, the molded articles exhibit enhanced thickness reduction and maintained tensile strength, overcoming the limitations of existing glycolic acid polymer-based downhole tool materials.

WO2024203809A1PCT designated stage expired Publication Date: 2024-10-03KUREHA CORPORATION

Patent Information

Application Number
PCT/JP2024/011213
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing molded articles made from glycolic acid polymers used in downhole tools face challenges in maintaining tensile strength while achieving a higher rate of thickness reduction after the initial thickness has been reduced by 5 mm, as the rate of thickness reduction decreases and tensile strength tends to decrease with increased thickness reduction.

Method used

Incorporating a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride into the glycolic acid polymer composition, with specific mass ratios and particle distributions, to enhance the decomposition rate and maintain tensile strength, particularly by promoting hydrolysis and improving water absorption.

Benefits of technology

The solution achieves a significant thickness reduction rate of 0.080 mm/hour or more after the initial thickness has decreased by 5 mm, while maintaining tensile strength at 52 MPa or more at 49°C, thereby addressing the limitations of existing compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011213_03102024_PF_FP_ABST
    Figure JP2024011213_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a molded body which retains tensile strength and has an improved thickness reduction rate after a reduction of 5 mm or more from the initial thickness. This molded body comprises a glycolic acid polymer, a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride, wherein the content of the cyclic ester is 21 parts by mass or less when the total mass of the glycolic acid polymer, the cyclic ester, the basic metal oxide, and the carboxylic acid anhydride is taken as 100 parts by mass, and the basic metal oxide has a shortest interparticle distance of 9.1 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Compact, downhole tool component and downhole tool

[0001] The present invention relates to a molded article made of a composition containing a glycolic acid polymer, a downhole tool component made of the molded article, and a downhole tool including the downhole tool component.

[0002] Glycolic acid polymers are degradable resin materials that are highly strong yet hydrolyzable and degradable. Taking advantage of these properties, glycolic acid polymers are used as medical materials, such as bone fixation materials and sutures. In recent years, their use has expanded as components for downhole tools used in the recovery of hydrocarbon resources. Some applications require even faster decomposition rates, and various research and development efforts are underway to improve the decomposition rate of glycolic acid polymers.

[0003] For example, Patent Document 1 discloses that the decomposition rate of a molded article can be improved by forming the molded article from a composition containing a glycolic acid polymer, a plasticizer, and a decomposition accelerator.

[0004] International Publication No. 2022 / 209885

[0005] Molded articles made of resin compositions containing glycolic acid polymers are useful as materials for downhole tools or components thereof from the viewpoints of the degradability and strength of the molded articles. When using molded articles containing glycolic acid polymers in downhole tools or components thereof, there is a demand for further improvements in the decomposition rate of the molded articles. In particular, for molded articles with a thickness of more than 5 mm, there is a demand for improvements in the rate of thickness reduction after a thickness reduction of 5 mm or more from the initial thickness while maintaining tensile strength.

[0006] However, according to the investigations of the present inventors, it has been found that in the case of a molded article made of the resin composition disclosed in Patent Document 1, the rate of thickness reduction decreases after the thickness is reduced by 5 mm or more from the initial thickness. Furthermore, from the viewpoint of strength, it has been found that the tensile strength tends to decrease as the rate of thickness reduction increases.

[0007] An object of one aspect of the present invention is to provide a molded article that maintains tensile strength while improving the rate of thickness reduction after the thickness is reduced by 5 mm or more from the initial thickness.

[0008] As a result of extensive research, the present inventors have found that when a composition contains a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride in addition to a glycolic acid polymer, the rate of thickness reduction of a molded article after the thickness has been reduced by 5 mm or more from the initial thickness is improved, and further, that the decrease in tensile strength of the molded article at 49°C is suppressed, leading to the completion of the present invention.

[0009] A molded article according to one embodiment of the present invention is a molded article comprising a glycolic acid polymer, a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride, wherein when the total mass of the glycolic acid polymer, the cyclic ester, the basic metal oxide, and the carboxylic acid anhydride is taken as 100 parts by mass, the content of the cyclic ester is 21 parts by mass or less, the distance between particles of the basic metal oxide is 9.1 μm or less, and the thickness or diameter is greater than 5 mm.

[0010] A molded article according to another embodiment of the present invention comprises a glycolic acid polymer, a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride, and when held in water at 49°C, the rate of thickness reduction after a thickness reduction of 5 mm or more from the initial thickness is 0.080 mm / h or more.

[0011] According to one aspect of the present invention, it is possible to provide a molded article that maintains tensile strength and has an improved rate of thickness reduction after the thickness is reduced by 5 mm or more from the initial thickness.

[0012] FIG. 1 is a graph showing the correlation between the nearest neighbor distance between basic metal oxide particles and the rate of thickness reduction in the later decomposition stage of the molded body in Examples 15 to 18 of the present invention and Comparative Example 15.

[0013] [Molded Article] The molded article according to this embodiment is made of a composition containing a glycolic acid polymer, a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride. In other words, the molded article according to this embodiment is a molded article containing a glycolic acid polymer, a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride.

[0014] (Glycolic Acid Polymer) In this specification, the glycolic acid polymer is a polymer having a repeating unit derived from glycolic acid (—(—O—CH 2 The glycolic acid polymer may be a homopolymer of glycolic acid (polyglycolic acid (PGA)). Alternatively, the glycolic acid polymer may be a copolymer containing repeating units derived from glycolic acid and repeating units derived from other monomers.

[0015] When the glycolic acid polymer is a homopolymer of glycolic acid, the weight-average molecular weight (Mw) of the glycolic acid polymer is preferably 150,000 or more, more preferably 160,000 or more, and even more preferably 170,000 or more, from the viewpoint of maintaining the strength of the molded article and extrusion molding. Furthermore, from the viewpoint of facilitating molding during extrusion molding or injection molding, the Mw of the glycolic acid polymer is preferably 500,000 or less, more preferably 450,000 or less, and even more preferably 400,000 or less.

[0016] Hereinafter, a copolymer containing a repeating unit derived from glycolic acid and a repeating unit derived from another monomer (hereinafter referred to as "glycolic acid copolymer") will be described.

[0017] (Glycolic Acid Copolymer) In order to improve the decomposition rate, the glycolic acid copolymer may be a copolymer in which a linear polymer chain A consisting of repeating units derived from glycolic acid is chemically bonded to two or more polymer chains B different from the polymer chain A. The polymer chain A and the polymer chain B will be described later.

[0018] In the glycolic acid copolymer, it is sufficient that two or more polymer chains A are chemically bonded to polymer chain B, and there are no particular limitations on the bonding positions of polymer chain A in polymer chain B. For example, the copolymer may be a triblock copolymer in which polymer chain A is chemically bonded to both ends of the main chain of polymer chain B (an "ABA block copolymer," where A is polymer chain A and B is polymer chain B), or a graft copolymer in which two or more polymer chains A are graft-bonded to polymer chain B.

[0019] The copolymer is preferably an ABA type block copolymer (where A is polymer chain A and B is polymer chain B) because this has a more excellent effect of improving the rate of thickness reduction during decomposition when the glycolic acid copolymer is formed into a molded article.

[0020] In addition, in the glycolic acid copolymer, it is preferable that the polymer chain A and the polymer chain B are bonded by an ester bond, which has the effect of easily improving the rate of thickness reduction during decomposition when the glycolic acid copolymer composition is formed into a molded article.

[0021] In particular, when polymer chain B is a unit that is more hydrophilic or flexible than polymer chain A, it is particularly preferable that polymer chain A and polymer chain B are bonded by an ester bond. Specifically, when polymer chain B is a unit that is more hydrophilic or flexible than polymer chain A, water penetrates more easily near polymer chain B than near polymer chain A, and the ester bond between polymer chain A and polymer chain B is more easily hydrolyzed than the ester bond within polymer chain A. In other words, the ester bond between polymer chain A and polymer chain B is hydrolyzed, and the glycolic acid copolymer is more likely to be cleaved between polymer chain A and polymer chain B. This results in a significant decrease in molecular weight, which tends to improve the rate of thickness reduction.

[0022] The polymer chains A and B constituting the glycolic acid copolymer will be described below.

[0023] (Polymer Chain A) A linear polymer chain composed of glycolic acid units is an example of the polymer chain A. The number of glycolic acid units constituting one block of the polymer chain A in the glycolic acid copolymer is not particularly limited, and can be appropriately determined within a range in which the glycolic acid copolymer can exhibit the degradability derived from the polymer chain A.

[0024] (Polymer Chain B) Polymer chain B is a polymer chain different from polymer chain A. For example, polymer chain B may be a polymer chain derived from a polymer compound having a glass transition temperature (Tg) of less than 45° C. Furthermore, polymer chain B may be a polymer chain derived from a polymer compound having a weight-average molecular weight of 1,500 or more and 250,000 or less.

[0025] The glass transition temperature of the polymer compound from which polymer chain B is derived (hereinafter referred to as "polymer compound B") is preferably 45°C or lower, more preferably 0°C or lower, from the viewpoint of making the glass transition temperature of the glycolic acid copolymer lower than that of a polymer consisting only of polymer chain A. The glass transition temperature of the polymer compound from which polymer chain B is derived can be measured by differential scanning calorimetry (DSC).

[0026] The weight-average molecular weight of polymer compound B is preferably 2,500 or more, more preferably 3,000 or more, and even more preferably 7,500 or more, from the viewpoint of further improving the rate of thickness reduction during decomposition of the molded article. Furthermore, from the viewpoint of further improving the strength of the molded article, the weight-average molecular weight of polymer compound B is preferably 50,000 or less, more preferably 20,000 or less. A weight-average molecular weight of polymer compound B of 50,000 or less is advantageous from the viewpoint of controlling the solubility in glycolide and copolymerization reactivity during the polymerization of glycolic acid copolymer. The weight-average molecular weight of polymer compound B can be measured using a gel permeation chromatography (GPC) apparatus.

[0027] The polymer compound B is not particularly limited as long as it has functional groups at two or more ends capable of chemically bonding to glycolic acid units constituting the polymer chain A in order to function as a polymerization initiator, and has a weight-average molecular weight and / or glass transition temperature within the specific range, other than polyglycolic acid.

[0028] An example of such a polymer compound B is a polyol having the specific weight-average molecular weight and glass transition temperature. Examples of polyols include polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, polycaprolactone, polydioxanone, polydimethylsiloxane, and polyethylene oxalate. The "polyol" may be a homopolymer consisting of only one type of repeating unit, or a copolymer further containing repeating units derived from other monomers.

[0029] Since the polymer compound B can impart hydrophilicity to the glycolic acid copolymer, it is preferable that the polymer compound B is a hydrophilic polyhydric alcohol polymer having a terminal hydroxy group. Examples of the hydrophilic polyhydric alcohol polymer having a terminal hydroxy group include polyethylene glycol, polypropylene glycol, polyglycerin, polyvinyl alcohol, etc.

[0030] In one embodiment of the present invention, polymer compound B can be a hydrophilic polyhydric alcohol having a terminal hydroxy group and a weight-average molecular weight of 3,000 to 50,000. When polymer compound B is a hydrophilic polyhydric alcohol having a terminal hydroxy group and a weight-average molecular weight of 3,000 to 50,000, the hydrophilicity of polymer chain B is expressed in the glycolic acid copolymer, improving affinity with water during decomposition, and as a result, achieving the effect of further improving the rate of thickness reduction during decomposition in the molded article.

[0031] In another embodiment of the present invention, polymer compound B may be polyethylene glycol or polypropylene glycol having a weight-average molecular weight of 3,000 to 50,000. Polyethylene glycol and polypropylene glycol have particularly low glass transition temperatures and particularly high hydrophilicity. Therefore, when the hydrophilic polyhydric alcohol having a terminal hydroxy group is polyethylene glycol or polypropylene glycol, flexibility and hydrophilicity can be imparted to the glycolic acid copolymer.

[0032] In another embodiment of the present invention, polymer compound B may be polyethylene glycol having a weight-average molecular weight of 7,500 or more and 50,000 or less. When polymer compound B is polyethylene glycol having a weight-average molecular weight of 7,500 or more and 50,000 or less, an effect of further improving the rate of thickness reduction during decomposition of the molded article is achieved.

[0033] The polymer compound B may be a homopolymer consisting of repeating units derived from a single monomer, or may be a copolymer further containing repeating units derived from other monomers.

[0034] Examples of other monomers include ethylene oxalate (1,4-dioxane-2,3-dione), lactides, lactones (e.g., β-propiolactone, β-butyrolactone, β-pivalolactone, γ-butyrolactone, δ-valerolactone, β-methyl-δ-valerolactone, ε-caprolactone, etc.), carbonates (e.g., trimethyline carbonate, etc.), ethers (e.g., 1,3-dioxane, etc.), ether esters (e.g., dioxanone, etc.), amides (e.g., ε-caprolactone, cyclic monomers such as hydroxycarboxylic acids or alkyl esters thereof, such as lactic acid, 3-hydroxypropanoic acid, 3-hydroxybutanoic acid, 4-hydroxybutanoic acid, and 6-hydroxycaproic acid; substantially equimolar mixtures of aliphatic diols such as ethylene glycol, propylene glycol, tetramethylene ether glycol, and 1,4-butanediol with aliphatic dicarboxylic acids or alkyl esters thereof, such as succinic acid and adipic acid; or two or more of these.

[0035] The repeating units derived from other monomers can be employed from the viewpoint of adjusting the physical properties of polymer compound B. For example, by employing other repeating units, it is possible to adjust the affinity of polymer compound B for water. The content of other repeating units in polymer compound B can be appropriately determined within a range in which the expected effect of polymer chain B can be sufficiently obtained. For example, the content of repeating units derived from other monomers in polymer compound B may be 50% by mass or less, preferably 30% by mass or less, and more preferably 10% by mass or less. Polymer compound B may be linear, or may be a graft copolymer in which another polymer compound is graft-bonded.

[0036] The polymer chain B may have an ester bond in the molecule. When the polymer chain B has an ester bond in the molecule, cleavage due to hydrolysis of the ester bond occurs also in the polymer chain B, and the thickness reduction rate is more likely to be improved.

[0037] Since the hydrophilicity of the polymer chains B in the glycolic acid copolymer is fully expressed and the rate of thickness reduction during decomposition of the molded article is improved, the amount of polymer chains B in the glycolic acid copolymer, in mass ratio, is preferably 0.5 or more, more preferably 1.5 or more, per 100 of the total amount of polymer chains A. Furthermore, from the viewpoint of maintaining the strength of the glycolic acid copolymer, the amount of polymer chains B in the glycolic acid copolymer, in mass ratio, is preferably 30 or less, more preferably 20 or less, per 100 of the total amount of polymer chains A.

[0038] The glycolic acid polymer can be produced by a known method. For example, a glycolic acid copolymer can be suitably produced by ring-opening polymerization of glycolide, a dimer of glycolic acid, in the presence of a small amount of catalyst and in the substantial absence of solvent (i.e., bulk polymerization conditions) using polymer compound B, from which polymer chain B is derived, as a polymerization initiator. The reaction temperature for ring-opening polymerization can be appropriately determined within a range in which the ring-opening polymerization of glycolide proceeds appropriately, and is, for example, 140°C. Examples of catalysts include cationic catalysts such as organic tin carboxylates, tin halides, and antimony halides. Commercially available glycolic acid polymers may be used.

[0039] (Glycolic Acid Polymer Content) The content of the glycolic acid polymer in the composition of this embodiment, i.e., the content of the glycolic acid polymer when the total of the glycolic acid polymer, cyclic ester, basic metal oxide, and carboxylic acid anhydride in the molded body of this embodiment is 100 parts by mass, is preferably 50 parts by mass or more and 97 parts by mass or less. A glycolic acid polymer content of 50 parts by mass or more is preferred from the viewpoint of ensuring sufficient tensile strength of the composition. From the viewpoint of improving the tensile strength, the content of the glycolic acid polymer is more preferably 55 parts by mass or more, and even more preferably 60 parts by mass or more. Furthermore, as described below, the cyclic ester, basic metal oxide, and carboxylic acid anhydride have a decomposition-promoting effect on the glycolic acid polymer. Therefore, a glycolic acid polymer content of 97 parts by mass or less is preferred from the viewpoint of increasing the thickness reduction rate, since the content of the compound having a decomposition-promoting effect is relatively increased. From the viewpoint of increasing the thickness reduction rate, a content of 90 parts by mass or less is more preferred, and even more preferably 80 parts by mass or less is more preferred.

[0040] (Cyclic Ester) Examples of cyclic esters contained in the composition according to this embodiment include glycolide, lactide, ε-caprolactone, γ-valerolactone, δ-valerolactone, diglycolic anhydride, and glutaric anhydride. Among these, glycolide or ε-caprolactone, which have a particularly high plasticizing effect, are preferred. One type of cyclic ester may be used alone, or two or more types may be used in combination.

[0041] In the composition according to this embodiment, the absolute value of the difference between the Fedors solubility parameter of the cyclic ester and the Fedors solubility parameter of the glycolic acid polymer is preferably 6.0 (J / cm 3 ) 1/2 More preferably, it is 5.5 (J / cm 3 ) 1/2 and more preferably 5.0 (J / cm 3 ) 1/2Hereinafter, "Fedors solubility parameter" may be abbreviated as "SP value." When the absolute value of the difference between the SP value of the cyclic ester and the SP value of the glycolic acid polymer is within the above range, the composition has sufficient plasticity.

[0042] The SP value can be calculated, for example, by Hideki Yamamoto, "SP Value: Fundamentals, Applications and Calculation Methods" (published by Johokko Co., Ltd. (2005), pp. 66-67). More specifically, the SP value δ ((cal / cm)) of the target compound (glycolic acid polymer or cyclic ester) is calculated according to the following formula (1): 3 ) 1/2 ) is calculated. δ = (ΣEcoh / ΣV) 1/2 ... (1) In formula (1), ΣEcoh is the cohesive energy density (cal / cm) of the structural unit of the target compound. 3 )); ΣV is the sum of V (the molar volume (cm) of the constituent units of the target compound); 3 )) indicates.

[0043] When two or more types of cyclic esters are contained in the composition, the absolute value of the difference between the SP value of at least one type of cyclic ester and the SP value of the glycolic acid polymer is 6.0 (J / cm 3 ) 1/2 It is preferable that:

[0044] The structure of the cyclic ester contained in the composition can be identified, for example, by gas chromatography-mass spectrometry (GCMS analysis) and comparison with known compounds as standard samples. If necessary, the structure can also be identified by combining other analytical methods such as NMR measurement and FT-IR.

[0045] The content of the cyclic ester in the composition is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 7 parts by mass or more, based on 100 parts by mass of the total of the glycolic acid polymer, the cyclic ester, the basic metal oxide, and the carboxylic acid anhydride. Furthermore, this content is 21 parts by mass or less, preferably 20 parts by mass or less, more preferably 18 parts by mass or less, and even more preferably 17 parts by mass or less. When the content of the cyclic ester is within this range, the glass transition temperature (Tg) of the composition can be sufficiently lowered, sufficient plasticity can be imparted to the composition, and sufficient tensile strength of the composition can be ensured. In one aspect of the embodiment of the present invention, the content of the cyclic ester in the composition is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 7% by mass or more, based on 100% by mass of the composition. Furthermore, this content is 21% by mass or less, preferably 20% by mass or less, more preferably 18% by mass or less, and even more preferably 17% by mass or less.

[0046] The content of cyclic ester in the composition can be calculated from the ratio of the materials charged. Alternatively, it can be measured, for example, by GCMS analysis. An example of gas chromatography (GC) measurement is shown below. Sample preparation method: p-chlorobenzophenone-containing dehydrated DMSO (0.4 mg / 2 mL) is added to approximately 100 mg of the composition, and the mixture is heated and dissolved at 160°C for approximately 10 minutes. After cooling to room temperature, the solution is filtered. Gas chromatography (GC) measurement is performed on the obtained filtrate. Measurement conditions: Apparatus: Shimadzu GC-2010 Column: RESTEK Rxi-5ms Column temperature: Hold at 150°C for 5 minutes → Heat at 20°C / min → Hold at 270°C for 3 minutes Injection temperature: 180°C.

[0047] (Basic Metal Oxide) Examples of basic metal oxides contained in the composition according to this embodiment include magnesium oxide, zinc oxide, calcium oxide, sodium oxide, and copper oxide. Among these, magnesium oxide or zinc oxide, which are weakly basic metal oxides or amphoteric metal oxides, are preferred because strong basic metal oxides decompose the matrix polymer itself. Furthermore, compared with cyclic esters and carboxylic acid anhydrides, the basic metal oxides remain in the molded product and are less likely to be eluted, making it possible to maintain a high thickness reduction rate even over a long period of time when the thickness has been reduced by 5 mm or more.

[0048] The interparticle distance of the basic metal oxide in the molded body according to this embodiment is preferably 0.35 μm or more, more preferably 0.50 μm or more. Furthermore, the interparticle distance is 9.1 μm or less, preferably 4.0 μm or less, and more preferably 1.0 μm or less. In this specification, the "interparticle distance" is defined as the average value of the distance between the center of gravity of any metal oxide particle and the center of gravity of another metal oxide particle closest to the center of gravity in any cross section of the molded body. Specifically, this distance can be obtained, for example, by measuring the interparticle distances of particles detected in a 3,000x electron microscope image, with the entire edge of the particle falling within the image, and calculating the average value. For example, a molded body that is a cube with a side length of 5 mm is cut into a 2 mm x 2 mm x 5 mm rectangular parallelepiped, and one of the 2 mm x 2 mm faces is trimmed into a cone shape (e.g., a pyramid), and then frozen in liquid nitrogen. A cross section of the frozen sample is taken using a cryostat ultramicrotome, and the resulting cross section is imaged at 3,000x magnification using a scanning electron microscope. The distance between all particles whose entire edges are within the image and the nearest neighboring particle is measured, and the average value is calculated to obtain the nearest interparticle distance. A basic metal oxide can be identified in a scanning electron microscope image, for example, by mapping the metal elements of the basic metal oxide through elemental analysis using an electron microscope elemental analyzer. The presence of a basic metal oxide within the range of nearest interparticle distance in the molded body promotes hydrolysis of the composition and further improves the rate of thickness reduction of the molded body. Furthermore, the addition of a basic metal oxide with a high decomposition acceleration effect can reduce the amount of cyclic ester added, which plasticizes the base material and promotes decomposition, resulting in improved strength of the base material.

[0049] The content of the basic metal oxide is preferably 0.5 parts by mass or more, more preferably 5 parts by mass or more, and particularly preferably 10 parts by mass or more, and is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and particularly preferably 20 parts by mass or less, based on 100 parts by mass of the total of the glycolic acid polymer, the cyclic ester, the basic metal oxide, and the carboxylic acid anhydride. By using such a content, the thickness reduction rate of the molded article can be increased. Furthermore, the molecular weight reduction during molding can be reduced, making it easier to obtain a molded article with a preferred molecular weight.

[0050] The average particle diameter of the basic metal oxide is preferably 5.0 μm or less, more preferably 2.0 μm or less, and particularly preferably 1.5 μm or less. By setting such a particle diameter, the dispersibility in the molded body is improved, and a preferable interparticle closest distance is easily obtained. In this specification, the particle diameter of the basic metal oxide refers to the particle diameter in the molded body. For example, a method for measuring the particle diameter is to perform elemental analysis using a scanning electron microscope elemental analyzer, and obtain an image by mapping the metal elements of the basic metal oxide. The particle diameter can be obtained by subjecting this image to image analysis processing. In the case of a shape that can exhibit multiple diameter sizes, such as an oval, the maximum length of the straight line is taken as the particle diameter. Note that the average particle diameter in this specification refers to a value calculated as the median diameter. There are no particular limitations on the method of image analysis processing after mapping, and commercially available image analysis software may be used. For example, a method may be used in which commercially available image analysis software is used to convert an image obtained by mapping metal elements of a basic metal oxide using a scanning electron microscope elemental analyzer into a monochrome image, and then the contrast of the monochrome image is adjusted by calibration so that it is closest to the original image in terms of contrast, and the particle diameter is then measured from the binarized image.

[0051] The basic metal oxide contained in the composition can be identified from the peak pattern of the basic metal oxide, for example, by XRD measurement. If necessary, a combination of multiple analytical methods, such as elemental analysis using an elemental analyzer for an electron microscope and FT-IR, may also be used.

[0052] (Carboxylic Acid Anhydride) Examples of carboxylic acid anhydrides contained in the composition according to this embodiment include hexanoic anhydride, octanoic anhydride, decanoic anhydride, lauric anhydride, myristic anhydride, palmitic anhydride, stearic anhydride, benzoic anhydride, succinic anhydride, maleic anhydride, phthalic anhydride, trimellitic anhydride, tetrahydrophthalic anhydride, butanetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, diphenylsulfonetetracarboxylic dianhydride, biphenyltetracarboxylic dianhydride, ethylene glycol bisanhydrotrimellitate, and glycerin bisanhydrotrimellitate monoacetate, with benzene-1,2,4,5-tetracarboxylic anhydride (pyromellitic anhydride) and 3,3',4,4'-benzophenonetetracarboxylic dianhydride being particularly preferred. One type of carboxylic acid anhydride may be used alone, or two or more types may be used in combination.

[0053] The structure of the carboxylic acid anhydride contained in the composition can be identified, for example, by GCMS analysis and comparison with a known compound as a standard. If necessary, the structure can also be identified by combining the results with other analytical methods such as NMR spectroscopy.

[0054] The content of the carboxylic acid anhydride in the composition is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, based on 100 parts by mass of the total of the glycolic acid polymer, the cyclic ester, the basic metal oxide, and the carboxylic acid anhydride. Furthermore, this content is preferably 10 parts by mass or less, more preferably 8 parts by mass or less. When the content of the carboxylic acid anhydride is within this range, the carboxylic acid anhydride is less likely to bleed out of the composition, thereby accelerating the decomposition rate of the composition while maintaining the thermal stability of the composition, and facilitating molding and processing. In one aspect of the embodiment of the present invention, the content of the carboxylic acid anhydride in the composition is preferably 0.5% by mass or more, more preferably 1% by mass or more, based on 100% by mass of the composition. Furthermore, this content is preferably 10% by mass or less, more preferably 8% by mass or less.

[0055] The content of carboxylic acid anhydride in the composition can be calculated from the proportions of the materials charged. Alternatively, it can be measured, for example, by GCMS analysis. An example of gas chromatography (GC) measurement is shown below. Sample preparation method: p-chlorobenzophenone-containing dehydrated DMSO (0.4 mg / 2 mL) is added to approximately 100 mg of the composition and heated to 160°C for approximately 10 minutes to dissolve. After cooling to room temperature, the solution is filtered. Gas chromatography (GC) measurement is performed on the obtained filtrate. Measurement conditions: Apparatus: Shimadzu GC-2010 Column: RESTEK Rxi-5ms Column temperature: Hold at 180°C for 4 minutes → Heat to 210°C at 10°C / min → Heat to 330°C at 40°C / min → Hold at 330°C for 3 minutes Injection temperature: 250°C.

[0056] (Weight-average molecular weight of composition) The weight-average molecular weight (Mw) of the composition, which is a material for forming a molded body, is preferably 150,000 or more, more preferably 160,000 or more, and even more preferably 170,000 or more, in terms of maintaining the strength of the molded body and extrusion molding, etc. Furthermore, in terms of facilitating molding during extrusion molding or injection molding, etc., the Mw of the composition is preferably 500,000 or less, more preferably 450,000 or less, and even more preferably 400,000 or less.

[0057] The weight-average molecular weight of the composition can be measured, for example, by the following method: Approximately 10 mg of the composition is dissolved in 0.5 mL of DMSO by heating at 150°C and then cooled to room temperature. The cooled solution is made up to 10 mL with hexafluoroisopropanol (HFIP), and the weight-average molecular weight of the composition is measured using a gel permeation chromatography (GPC) device. Polymethyl methacrylate (PMMA) is used as the standard substance. An example of a GPC device is a Shodex GPC-104 (detector: RI, column: two HFIP-606M columns). Furthermore, 5 mM CF as the solvent is used. 3 HFIP containing COONa may also be used.

[0058] (Other Components) In addition to the glycolic acid polymer, cyclic ester, basic metal oxide, and carboxylic acid anhydride, the composition may contain other components as long as they do not contradict the object of the present invention.

[0059] Examples of other components include various additives such as decomposition accelerators, heat stabilizers, light stabilizers, inorganic fillers, moisture-proofing agents, waterproofing agents, water-repellent agents, lubricants, hydrophilic agents, water-absorbing agents, nucleating agents, pore-forming agents, etc. The composition may also contain a polymerization initiator, a catalyst, etc. that are used in preparing the polymer.

[0060] The composition can be prepared by mixing a glycolic acid polymer, a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride. The cyclic ester may be added during the preparation of the glycolic acid polymer. Furthermore, when a glycolic acid polymer is obtained by ring-opening polymerization of glycolide, the remaining glycolide may be used as the cyclic ester. That is, the composition may be prepared by mixing a glycolic acid polymer composition containing glycolide and a glycolic acid polymer obtained by the preparation of the glycolic acid polymer with a basic metal oxide, a carboxylic acid anhydride, and optionally a cyclic ester.

[0061] The molded article according to this embodiment is a polyglycolic acid molded article made of the composition, and has a thickness or diameter of more than 5 mm.

[0062] When a molded article according to one embodiment of the present invention is kept in water at 49°C, the rate of thickness reduction of the molded article after the thickness has decreased by 5 mm from the initial thickness (the thickness of the molded article before being kept in water) is preferably 0.080 mm / hour or more, more preferably 0.088 mm / hour or more, and even more preferably 0.10 mm / hour or more. Hereinafter, a "molded article after the thickness has decreased by 5 mm or more from the initial thickness when kept in water at 49°C" may be referred to as a "molded article in the late decomposition stage."

[0063] When the molded article according to one embodiment of the present invention is held in water at 49°C, and the rate of thickness reduction after a thickness reduction of 5 mm or more from the initial thickness is 0.080 mm / hour or more, the tensile strength at 49°C is preferably 52 MPa or more, more preferably 55 MPa or more, and even more preferably 57 MPa or more. The tensile strength value in this specification is a value measured in accordance with ISO 527-1. Specifically, a test piece (No. 5 test piece) having a shape specified in ISO 527-1 is subjected to a tensile test at 49°C (temperature 49°C ± 1°C) at a speed of 20 mm / min, and the maximum point stress exhibited until the test piece breaks is calculated, and the maximum point stress is calculated as the average of five measurements.

[0064] As described above, the molded article according to this embodiment contains a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride. The cyclic ester improves the water absorption capacity of the glycolic acid polymer and accelerates the decomposition of the molded article. The basic metal oxide and the carboxylic acid anhydride improve the hydrolysis rate of the glycolic acid polymer and accelerate the decomposition of the molded article. The carboxylic acid anhydride also stabilizes moldability. Specifically, it suppresses the molecular weight reduction of the glycolic acid polymer caused by heat and the basic metal oxide during molding. A molded article containing a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride improves the water absorption capacity and hydrolysis rate of the glycolic acid polymer, synergistically accelerating the decomposition of the molded article. As shown in the examples, compared to a molded article lacking any of the cyclic ester, the basic metal oxide, and the carboxylic acid anhydride, the molded article according to this embodiment exhibits a higher thickness reduction rate due to the synergistic effect of the cyclic ester, the basic metal oxide, and the carboxylic acid anhydride.

[0065] In this specification, the thickness reduction rate refers to the rate at which the thickness of the non-embrittled portion of the molded body decreases. "Embrittlement" refers to the hydrolysis of the glycolic acid polymer, which reduces the molecular weight of the glycolic acid polymer, resulting in the molded body becoming brittle. The embrittled portion of the molded body is also referred to as an embrittled layer. Embrittlement progresses from the surface to the center of the molded body, and the thickness of the non-embrittled portion decreases from the surface side. Therefore, the rate at which embrittlement progresses shows a positive correlation with the thickness reduction rate. Therefore, in this specification, the embrittlement progression rate of the molded body is defined as the thickness reduction rate.

[0066] The thickness reduction rate can be measured, for example, by the following method: A required number of cubic test pieces with sides of 40 mm are prepared from the molded body. The test pieces are placed in a 1 L autoclave at 49°C, and the autoclave is filled with water (deionized water) to perform an immersion test. After immersion, the test pieces are removed at predetermined time intervals and left to dry overnight in a dry room (dew point -65°C, temperature 23°C), after which the thickness of the core (hard part) of the test piece is measured. The thickness reduction is calculated from the difference between the thickness of the core and the thickness of the test piece before immersion (initial thickness, specifically 40 mm). The time change in the thickness reduction of the test piece is determined based on the measured values ​​of the thickness reduction of the test piece measured at different immersion times. Here, the period from the initial thickness until the thickness reduction is 5 mm is defined as the initial decomposition period, and the period from the initial thickness until the thickness reduction is 5 mm or more is defined as the later decomposition period. The thickness reduction rate of a 40 mm thick test piece is calculated from the time change in the thickness reduction of the test piece within the range of the initial decomposition period or the later decomposition period (unit: mm / h). The core can be identified, for example, by scraping off the embrittled layer on the surface of the test piece with a cutter or the like, and identifying the surface of each surface after scraping as the core surface. Alternatively, since the color of the embrittled layer changes due to a decrease in molecular weight caused by hydrolysis of the glycolic acid polymer, a molded product containing the embrittled layer can be cut to expose the cross section, and the part with a color different from that of the surface layer can be identified as the core. The thickness can be measured using any method as long as it can measure the thickness, and examples of such methods include using a vernier caliper or a microscope.

[0067] (Method for Producing Molded Article) The molded article according to this embodiment can be obtained by molding the composition. The molding method is not limited, and examples include injection molding, melt extrusion molding, solidification extrusion molding, compression molding (press molding), and centrifugal molding.

[0068] An example of producing a molded product by solidification extrusion molding is shown below. Pellets made of the composition are fed into an extruder with a cylinder set at a temperature above the melting point of the composition and below 255°C (usually 200-255°C) and melt-kneaded. The molten mixture is then extruded from the extrusion die at the tip of the extruder into the flow path of a forming die, cooled to below the crystallization temperature of the composition in the flow path of the forming die to solidify, and extruded out from the tip of the forming die at a rate of 5-50 mm / 10 min. This extrudate is pressurized and withdrawn in the direction of the forming die while applying a back pressure of 1,500-8,500 kg, to produce a molded product that is a solidified extrusion molded product. This molded product may be annealed by heat-treating it at a temperature of 150-230°C for 3-24 hours.

[0069] An example of producing a molded article by injection molding is shown below. Pellets made of the composition are fed into an injection molding machine equipped with an injection mold. The cylinder temperature is set to a temperature between the melting point of the composition and 255°C (usually 200-255°C), and the mold temperature is set to a temperature between 0°C and the melting point of the composition (usually 0-190°C). An injection-molded article is then produced by injection molding at an injection pressure of 1-104 MPa (preferably 10-104 MPa). This molded article may be annealed at a temperature between the crystallization temperature of the composition and the melting point (usually 70-220°C) for 1 minute to 10 hours.

[0070] There is no particular upper limit to the thickness or diameter of the molded article, but it is preferably 500 mm or less, more preferably 400 mm or less.

[0071] [Downhole Tool Component] A downhole tool component according to one embodiment of the present invention is a component used in underground excavation to recover hydrocarbon resources such as oil and gas from the earth, and is made of the compact. The compact may be used as a downhole tool component as is, or may be subjected to conventionally known machining (secondary processing) to manufacture a downhole tool component. An example of machining is cutting.

[0072] The shape and size of the downhole tool component according to one embodiment of the present invention are not particularly limited, but may be, for example, 5 to 500 mm in thickness or diameter, preferably 20 to 300 mm, and more preferably 30 to 200 mm. The downhole tool component may have various shapes, such as a round bar, a flat plate, a hollow product such as a pipe, or an irregularly shaped product. A round bar, a hollow product, or a flat plate is preferred because they facilitate extrusion molding and subsequent densification treatment, and are often suitable for extrusion-molded products, which are raw materials for machining. A round bar is more preferred for forming a downhole tool component for oil drilling, particularly a core rod for a plug.

[0073] [Downhole Tool] A downhole tool according to one embodiment of the present invention includes a downhole tool component. In this specification, a downhole tool refers to a device or component thereof that is used for various well treatments, such as well drilling, well plugging, and fracturing, and that is installed in a well. The shape of the downhole tool is not particularly limited, and may be, for example, a conventionally known shape. Examples of downhole tools include a frac plug, a bridge plug, a cement retainer, a perforation gun, a ball sealer, a plugging plug, and a packer.

[0074] [Summary] The molded article according to aspect 1 of the present invention is a molded article comprising a glycolic acid polymer, a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride, wherein when the total mass of the glycolic acid polymer, the cyclic ester, the basic metal oxide, and the carboxylic acid anhydride is taken as 100 parts by mass, the content of the cyclic ester is 21 parts by mass or less, the distance between particles of the basic metal oxide is 9.1 μm or less, and the thickness or diameter is greater than 5 mm.

[0075] The molded article according to Aspect 2 of the present invention may be, in Aspect 1 above, such that when held in water at 49°C, the thickness reduction rate after the thickness has decreased by 5 mm or more from the initial thickness is 0.080 mm / hour or more.

[0076] The molded article according to Aspect 3 of the present invention may be the molded article of Aspect 2 above, having a tensile strength at 49°C of 52 MPa or more.

[0077] A molded article according to a fourth aspect of the present invention is a molded article comprising a glycolic acid polymer, a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride, and when held in water at 49°C, the rate of thickness reduction after a thickness reduction of 5 mm or more from the initial thickness is 0.080 mm / h or more.

[0078] A molded article according to a fifth aspect of the present invention may be the molded article of any one of the first to fourth aspects, wherein the cyclic ester is glycolide or ε-caprolactone.

[0079] A molded article according to a sixth aspect of the present invention may be the molded article of any one of the first to fifth aspects, wherein the basic metal oxide is magnesium oxide or zinc oxide.

[0080] A molded article according to a seventh aspect of the present invention may be the molded article of any one of the first to sixth aspects, wherein the carboxylic acid anhydride is benzene-1,2,4,5-tetracarboxylic acid anhydride or 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride.

[0081] A molded article according to an eighth aspect of the present invention is the article of any one of the first to seventh aspects, wherein the glycolic acid polymer is a copolymer in which a linear polymer chain A composed of repeating units derived from glycolic acid is chemically bonded to a polymer chain B different from the polymer chain A, and the polymer chain B may be derived from a polymer compound having a glass transition temperature of less than 45°C.

[0082] A ninth aspect of the present invention provides a molded article according to the eighth aspect, wherein the glycolic acid polymer is a block copolymer of the polymer chain A and the polymer chain B.

[0083] A molded article according to a tenth aspect of the present invention may be the molded article of any one of the first to ninth aspects, wherein the glycolic acid polymer is a homopolymer of glycolic acid.

[0084] The molded article according to an eleventh aspect of the present invention may be the molded article of any one of the first to tenth aspects, wherein the weight average molecular weight of the material forming the molded article is 150,000 or more and 500,000 or less.

[0085] A downhole tool component according to a twelfth aspect of the present invention comprises the molded article according to any one of the first to eleventh aspects.

[0086] A downhole tool according to a thirteenth aspect of the present invention includes the downhole tool member of the twelfth aspect.

[0087] Another aspect of the molded article according to the first aspect of the present invention is a molded article that is made of a composition containing a glycolic acid polymer, a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride, wherein the content of the cyclic ester in the composition is 21 mass% or less, the interparticle distance of the basic metal oxide is 9.1 μm or less, and the thickness or diameter is greater than 5 mm.

[0088] The following examples are provided to further explain the embodiments of the present invention. It goes without saying that the present invention is not limited to the following examples, and various modifications are possible in detail. Furthermore, the present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. Furthermore, all of the documents cited in this specification are incorporated by reference.

[0089] Hereinafter, the glycolic acid polymer composition obtained by polymerization will be referred to as a "polymer composition." Furthermore, a composition containing a glycolic acid polymer (or polymer composition), a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride will be referred to as a "molding composition."

[0090] In the following examples, unless otherwise specified, % represents % by mass.

[0091] [Measurement of SP Values ​​of Glycolic Acid Polymers and Cyclic Esters] The SP values ​​were measured with reference to "SP Values: Fundamentals, Applications and Calculation Methods" by Yamamoto Hideki (published by Johokko Co., Ltd. (2005), pp. 66-67). More specifically, the SP value δ ((cal / cm)) of the target compound (glycolic acid polymer or cyclic ester) was calculated according to the following formula (1): 3 ) 1/2 ) was calculated. δ = (ΣEcoh / ΣV) 1/2... (1) In formula (1), ΣEcoh is the cohesive energy density (cal / cm) of the structural unit of the target compound. 3 )); ΣV is the sum of V (the molar volume (cm) of the constituent units of the target compound); 3 )) indicates.

[0092] The SP value measurement results, the difference between the SP value of the cyclic ester and the SP value of the glycolic acid polymer, and the glass transition temperature of the mixture are shown in Table 1. The SP value of the glycolic acid polymer is 26.8. When two types of cyclic esters are contained in the mixture, the difference between the SP value of each cyclic ester and the SP value of the glycolic acid polymer is the one with the largest absolute value of the difference in SP value.

[0093]

[0094] [Evaluation of molding compositions and molded articles] The molding compositions and molded articles obtained in the examples and comparative examples were evaluated as follows.

[0095] (Measurement of weight-average molecular weight of molded product) Approximately 10 mg of sample was dissolved in 0.5 mL of DMSO by heating at 150°C and cooled to room temperature. The cooled solution was made up to 10 mL with hexafluoroisopropanol (HFIP), and the weight-average molecular weight of the composition was measured using a GPC device. Polymethyl methacrylate (PMMA) was used as the standard substance. The measurement conditions are as follows: Device: Shodex GPC-104 (Detector: RI, Column: HFIP-606M (2 columns)) Solvent: 5 mM CF 3 HFIP containing COONa

[0096] (Measurement of glycolide content in molded body) p-Chlorobenzophenone-containing DMSO (0.4 mg / 2 mL) was added to approximately 100 mg of sample, and the mixture was heated and dissolved at 150°C for approximately 10 minutes. After cooling to room temperature, the solution was filtered. The obtained filtrate was subjected to gas chromatography (GC) measurement. The measurement conditions are as follows: Apparatus: Shimadzu GC-2010 Column: RESTEK Rxi-5ms Column temperature: 150°C for 5 minutes → (heated at 20°C / min) → 270°C for 3 minutes Injection temperature: 180°C

[0097] (Measurement of Thickness Reduction Rate of Molded Articles) The required number of cubic test pieces, each 40 mm on a side, were prepared from the molded articles. The test pieces were then placed in a 1 L autoclave at 49°C. The autoclave was then filled with water (deionized water) and an immersion test was performed. After immersion, the test pieces were removed at predetermined time intervals and cut to expose the cross section. After leaving the test pieces to dry overnight in a dry room, the thickness of the core (hard part) of each test piece was measured. The thickness reduction was measured as the difference from the thickness before immersion (initial thickness, specifically, 40 mm). The time change in thickness reduction of the test pieces was calculated based on the measured values ​​of the thickness reduction of the test pieces measured for different immersion times. The period from the initial thickness until a thickness reduction of 5 mm was defined as the initial decomposition period, and the period from the initial thickness until a thickness reduction of 5 mm or more was defined as the later decomposition period. The thickness reduction rate of a 40 mm thick test piece was calculated (unit: mm / h) from the time change in thickness reduction of the test piece within the range of the initial or later decomposition period.

[0098] (Measurement of Tensile Strength of Molded Article) A molded article having a thickness of 5 mm or more can be said to have a tensile strength sufficient for practical use if the tensile strength measured using a specified test piece is 52 MPa or more. The tensile strength of the test piece can be measured in accordance with ISO 527-1. A tensile test was performed on a test piece (No. 5 test piece) having a shape specified in ISO 527-1 at 49°C (temperature 49°C ± 1°C) at a speed of 20 mm / min, and the maximum point stress exhibited until the test piece broke was calculated and used as the tensile strength of the test piece (average value of n = 5, unit: MPa).

[0099] (Calculation of the nearest neighbor distance between particles of basic metal oxide in the molded body) The molded body was cut into a size of 2 mm x 2 mm x 5 mm with a razor, trimmed into a pyramidal shape on one side, and then frozen in liquid nitrogen. The frozen sample was cross-sectioned using a cryo-ultramicrotome (knife temperature: 100°C, sample temperature: 120°C, chamber temperature: 120°C). The sample was then metal-deposited and observed using a Hitachi High-Technologies field-emission scanning electron microscope "SU8220" and elemental analysis was performed using a Bruker electron microscope elemental analyzer "QUANTAX Flat QUAD" at 3000x magnification. The elemental mapping image of the metal oxide obtained by elemental analysis was binarized using LightStone's image analysis software "MIPAR," and metal oxide particles were extracted as white images. Furthermore, the distance from the center of gravity of the extracted metal oxide particle to the center of gravity of the closest other extract was calculated as the nearest neighbor distance between the particles. The closest inter-particle distances were calculated for all the extracted particles as described above, and the average value was calculated.

[0100] (Comparison of the Presence and Absence of Glycolic Acid Polymer, Cyclic Ester, Basic Metal Oxide, and Carboxylic Acid Anhydride) Example 1 Polyglycolic acid (PGA, manufactured by Kureha Corporation) was blended with glycolide (GL) as a cyclic ester, magnesium oxide (MgO) as a basic metal oxide, benzene-1,2,4,5-tetracarboxylic acid anhydride (PMDA) as a carboxylic acid anhydride, and a mixture of distearyl acid phosphate and monostearyl acid phosphate ("ADK STAB AX-71" manufactured by ADEKA Corporation) as a heat stabilizer to obtain a molding composition. The contents of the cyclic ester, basic metal oxide, and carboxylic acid anhydride contained in the molding composition, as well as the nearest neighbor distance between particles of the basic metal oxide, are shown in Table 2. Note that the parts by mass in each Example and Comparative Example are expressed as parts by mass when the total of the polyglycolic acid (or polyglycolic acid-polyethylene glycol polymer), cyclic ester, basic metal oxide, and carboxylic acid anhydride (or N,N-diisopropylcarbodiimide) is taken as 100 parts by mass.

[0101] The molding composition was supplied to the feed section of a twin-screw extrusion kneader ("2D25S" manufactured by Toyo Seiki Co., Ltd.) with a screw temperature set to 190 to 240°C, melt-kneaded, and extrusion-molded to obtain pellets of the molding composition. The pellets of the molding composition were then supplied to the feed section of an injection molding machine ("EC-100N" manufactured by Toshiba Machine Co., Ltd.) with a cylinder temperature set to 190 to 240°C, and injection-molded to obtain a molded article. The mold temperature during injection molding was set to 80 to 100°C.

[0102] Examples 2 to 11 Except for changing the amounts of the cyclic ester, basic metal oxide, and carboxylic acid anhydride, molding compositions and molded articles were obtained in the same manner as in Example 1. The contents of the cyclic ester, basic metal oxide, and carboxylic acid anhydride, as well as the nearest neighbor distance between particles of the basic metal oxide, for Examples 2 to 11 are shown in Table 2.

[0103] Example 12 A molding composition and a molded article were obtained in the same manner as in Example 1, except that 7 parts by mass of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) was added as the carboxylic acid anhydride and the amounts of the cyclic ester and basic metal oxide were changed. The contents of the cyclic ester, basic metal oxide, and carboxylic acid anhydride, as well as the nearest neighbor distance between particles of the basic metal oxide, for Example 12 are shown in Table 2.

[0104] Example 13 A molding composition and a molded article were obtained in the same manner as in Example 1, except that 7.3 parts by mass of ε-caprolactone (ε-CL) was added as the cyclic ester and the amounts of the basic metal oxide and carboxylic acid anhydride were changed. The contents of the cyclic ester, basic metal oxide, and carboxylic acid anhydride, as well as the nearest neighbor distance between particles of the basic metal oxide in Example 13, are shown in Table 2.

[0105] Example 14 A molding composition and a molded body were obtained in the same manner as in Example 1, except that 14 parts by mass of zinc oxide (ZnO) was added as the basic metal oxide and the amounts of the cyclic ester and carboxylic acid anhydride were changed. The contents of the cyclic ester, basic metal oxide, and carboxylic acid anhydride, as well as the nearest neighbor distance between particles of the basic metal oxide in Example 14, are shown in Table 2.

[0106] Comparative Example 1 A molding composition and a molded article were obtained in the same manner as in Example 1, except that none of the cyclic ester, basic metal oxide, and carboxylic acid anhydride was added.

[0107] [Comparative Examples 2 and 3] Except for not adding the cyclic ester and the basic metal oxide and for changing the amount of carboxylic acid anhydride, molding compositions and molded articles were obtained in the same manner as in Example 1. The contents of carboxylic acid anhydride in Comparative Examples 2 and 3 are shown in Table 3.

[0108] [Comparative Examples 4 and 5] A molding composition and a molded article were obtained in the same manner as in Example 1, except that the basic metal oxide and the carboxylic acid anhydride were not added and the amount of the cyclic ester was changed. The contents of the cyclic ester in Comparative Examples 4 and 5 are shown in Table 3.

[0109] Comparative Examples 6-8: 100 parts by weight of glycolide were charged to a polymerization vessel with 0.03 parts by weight of tin dichloride as a catalyst, 1 part by weight of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] as a heat stabilizer, and 2 parts by weight of polyethylene glycol (PEG, Mw 7500) as a polymerization initiator. The charged contents were heated at 140°C for 6 hours to obtain a polyglycolic acid-polyethylene glycol polymer (PGA-PEG). The polyglycolic acid-polyethylene glycol polymer (PGA-PEG) obtained by the above process did not contain glycolide. Molding compositions and molded articles were obtained in the same manner as in Example 1, except that no basic metal oxide was added, the polyglycolic acid-polyethylene glycol polymer (PGA-PEG) obtained by the above process was used instead of polyglycolic acid, and the amounts of cyclic ester and carboxylic acid anhydride were changed. The cyclic ester and carboxylic acid anhydride contents of Comparative Examples 6-8 are shown in Table 3.

[0110] Comparative Example 9 A molding composition was obtained in the same manner as in Example 1, except that the carboxylic acid anhydride was not added and the amounts of the cyclic ester and basic metal oxide were changed. The contents of the cyclic ester and basic metal oxide in Comparative Example 9 are shown in Table 3. This molding composition was unable to be injection molded due to thermal decomposition.

[0111] Comparative Example 10 A molding composition was obtained in the same manner as in Example 1, except that 1 part by mass of N,N-diisopropylcarbodiimide (CDI) was added instead of the carboxylic acid anhydride and the amounts of the cyclic ester and basic metal oxide were changed. The contents of the cyclic ester and basic metal oxide in Comparative Example 10 are shown in Table 3. This molding composition was unable to be injection molded due to thermal decomposition.

[0112] [Comparative Example 11] A molding composition and a molded body were obtained in the same manner as in Example 1, except that the amounts of the cyclic ester, basic metal oxide, and carboxylic acid anhydride were changed. The contents of the cyclic ester and basic metal oxide in Comparative Example 11 are shown in Table 3.

[0113] [Comparative Example 12] A molding composition and a molded article were obtained in the same manner as in Example 1, except that the cyclic ester was not added and the amounts of the basic metal oxide and carboxylic acid anhydride were changed. The contents of the basic metal oxide and carboxylic acid anhydride in Comparative Example 12 are shown in Table 3.

[0114] [Comparative Examples 13 and 14] Except for not adding a basic metal oxide and changing the amount of cyclic ester, molding compositions and molded articles were obtained in the same manner as in Example 1. The contents of cyclic ester in Comparative Examples 13 and 14 are shown in Table 3.

[0115] As shown in Table 2, the molded articles made from the molding compositions of Examples 1 to 14 had thickness reduction rates in the later stage of decomposition of 0.080 mm / h or more and tensile strengths of 52 MPa or more at 49°C, showing good results in both thickness reduction rates and tensile strengths in the later stage of decomposition. On the other hand, as shown in Table 3, the molded articles made from the molding compositions of Comparative Examples 1 to 14, which did not contain any of the cyclic ester, basic metal oxide, or carboxylic acid anhydride, or in which the nearest neighbor distance between basic metal oxide particles was large, had thickness reduction rates in the later stage of decomposition of less than 0.080 mm / h or tensile strengths of less than 52 MPa at 49°C.

[0116]

[0117]

[0118] (Comparison Based on Interparticle Distance of Basic Metal Oxide) [Examples 15-18, Comparative Example 15] In Examples 15-18 and Comparative Example 15, basic metal oxides of various average particle sizes were used to compare the effects on decomposition rate and tensile strength of the basic metal oxide particles, which depend solely on the size of the nearest neighbor distance between particles. Molding compositions and molded articles were obtained using the same procedures as in Example 1. The types and contents of the cyclic ester, basic metal oxide, and carboxylic acid anhydride, as well as the average particle sizes and nearest neighbor distances of the basic metal oxides, are shown in Table 4.

[0119]

[0120] As shown in Table 4, the molded bodies made from the molding compositions of Examples 15 to 18 showed good results in both the rate of thickness reduction in the later stage of decomposition and tensile strength at 49°C. On the other hand, Comparative Example 15, which had a large interparticle distance, showed a slow rate of thickness reduction in the later stage of decomposition. Furthermore, based on these results, when the correlation between the interparticle distance of the basic metal oxide and the rate of thickness reduction in the later stage of decomposition of the molded body is considered (Figure 1), it is suggested that when the interparticle distance of the basic metal oxide is 9.1 µm or less, the rate of thickness reduction in the later stage of decomposition of the molded body will be 0.080 mm / h or more.

[0121] (Comparison of the Presence and Absence of the Thermal Stabilizing Effect of Carboxylic Acid Anhydride) [Examples 19-21, Comparative Examples 16-20] In Examples 19-21 and Comparative Examples 16-20, various hydroxyl group capping agents (CDI, silane coupling agents) were used in addition to carboxylic acid anhydrides to compare the effects on thermal stability of the presence of carboxylic acid anhydrides and other hydroxyl group capping agents. The silane coupling agents used were KBM-4803 manufactured by Shin-Etsu Silicones, KBE-9007N manufactured by Shin-Etsu Silicones, and X-12-967C manufactured by Shin-Etsu Silicones. Molding compositions and molded articles were obtained using the same procedures as in Example 1. The types and contents of the cyclic esters, basic metal oxides, carboxylic acid anhydrides, and hydroxyl group capping agents are shown in Table 5.

[0122]

[0123] As shown in Table 5, Examples 19 to 21 showed good results in terms of the retention of weight-average molecular weight after injection molding compared to before injection molding. On the other hand, Comparative Examples 16 to 19, which contained a hydroxyl group-capping agent other than a carboxylic acid anhydride, and Comparative Example 20, which contained neither a carboxylic acid anhydride nor any other hydroxyl group-capping agent, showed a low retention of weight-average molecular weight after injection molding compared to before injection molding, indicating lower thermal stability compared to the compositions of Examples 19 to 21.

[0124] The compacts of the present invention have a high decomposition rate and can be used, for example, in downhole tools for well drilling.

Claims

1. A molded body comprising a glycolic acid polymer, a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride, wherein when the total mass of the glycolic acid polymer, the cyclic ester, the basic metal oxide, and the carboxylic acid anhydride is 100 parts by mass, the content of the cyclic ester is 21 parts by mass or less, the closest interparticle distance of the basic metal oxide is 9.1 μm or less, and the thickness or diameter of the molded body is more than 5 mm.

2. The molded article according to claim 1, which, when held in water at 49°C, exhibits a thickness reduction rate of 0.080 mm / h or more after the thickness has decreased by 5 mm or more from the initial thickness.

3. The molded body described in claim 2, having a tensile strength of 52 MPa or more at 49°C.

4. A molded article comprising a glycolic acid polymer, a cyclic ester, a basic metal oxide, and a carboxylic acid anhydride, which, when held in water at 49°C, exhibits a thickness reduction rate of 0.080 mm / h or more after the thickness has decreased by 5 mm or more from the initial thickness.

5. The molded article according to claim 1 or 4, wherein the cyclic ester is glycolide or ε-caprolactone.

6. The molded body according to claim 1 or claim 4, wherein the basic metal oxide is magnesium oxide or zinc oxide.

7. The molded article according to claim 1 or 4, wherein the carboxylic acid anhydride is benzene-1,2,4,5-tetracarboxylic acid anhydride or 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride.

8. The molded article according to claim 1 or claim 4, wherein the glycolic acid polymer is a copolymer in which a linear polymer chain A consisting of repeating units derived from glycolic acid is chemically bonded to a polymer chain B different from the polymer chain A, and the polymer chain B is derived from a polymer compound having a glass transition temperature of less than 45°C.

9. The molded article according to claim 8, wherein the glycolic acid polymer is a block copolymer of the polymer chain A and the polymer chain B.

10. The molded article according to claim 1 or 4, wherein the glycolic acid polymer is a homopolymer of glycolic acid.

11. A molded body according to claim 1 or claim 4, wherein the weight average molecular weight of the material forming the molded body is 150,000 or more and 500,000 or less.

12. A downhole tool component comprising the molded article according to any one of claims 1 to 11.

13. A downhole tool comprising the downhole tool component of claim 12.

Citation Information

Patent Citations

  • Method for producing polyglycolic acid resin composition

    JP2020002189A

  • Polyglycolic acid copolymer composition and method for producing same

    JP2022512906A

  • Method for controlling water resistance of polyglycolic acid resin

    WO2007060981A1

  • Polyglycolic acid resin composition, moldings of polyglycolic acid resin, and laminates

    WO2011024653A1

  • Molded body, downhole tool member, and downhole tool

    WO2022209885A1

Cited By

  • Molded body, downhole tool member, and downhole tool

    WO2026211807A1

  • Resin composition, molded body, downhole tool member, downhole tool, and method for producing resin composition

    WO2026211808A1