Silver-containing zirconia sintered body, silver-containing stabilized zirconia powder, method for producing silver-containing stabilized zirconia powder, and method for producing silver-containing zirconia sintered body

Embedding silver particles with a diameter of 0.5 μm or less within a zirconia sintered body with 0.35 μm or less crystal grain size addresses the durability and mechanical property issues of conventional antibacterial zirconia ceramics, enhancing both mechanical and hydrothermal resistance while maintaining antibacterial effectiveness.

WO2024203828A1PCT designated stage expired Publication Date: 2024-10-03DAIICHI KIGENSO KAGAKU KOGYO CO LTD

Patent Information

Application Number
PCT/JP2024/011255
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional methods for imparting antibacterial properties to zirconia ceramics, such as coating with silver nanoparticles, face issues with durability due to peeling and low mechanical properties when silver is mixed with zirconia and sintered, leading to reduced sinterability and hydrothermal deterioration resistance.

Method used

A silver-containing zirconia sintered body with silver particles and stabilized zirconia, where the average particle diameter of silver particles is 0.5 μm or less and the average crystal grain size of stabilized zirconia is 0.35 μm or less, achieving a relative sintered density of 98% or more, ensuring the silver particles are dispersed within the body for enhanced mechanical and hydrothermal properties.

Benefits of technology

The approach maintains antibacterial efficacy by embedding silver particles within the zirconia sintered body, improving mechanical properties, sinterability, and hydrothermal resistance while preventing the decline in antibacterial action due to wear, and allowing for low-temperature sintering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011255_03102024_PF_FP_ABST
    Figure JP2024011255_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a silver-containing zirconia sintered body comprising silver particles, zirconia, and a stabilizing agent, wherein the silver particles have an average particle diameter of 0.5 μm or less, stabilized zirconia has an average crystal grain diameter of 0.35 μm or less, and the relative sintered density is 98% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Silver-containing zirconia sintered body, silver-containing stabilized zirconia powder, method for producing silver-containing stabilized zirconia powder, and method for producing silver-containing zirconia sintered body

[0001] The present invention relates to a silver-containing zirconia sintered body, a silver-containing stabilized zirconia powder, a method for producing a silver-containing stabilized zirconia powder, and a method for producing a silver-containing zirconia sintered body.

[0002] A common method for imparting antibacterial properties to zirconia ceramics (zirconia sintered bodies) is to coat the ceramic surface with an antibacterial substance, such as silver, which has a wide antibacterial spectrum, or titanium oxide, which functions as a photocatalyst.

[0003] Silver is used in prosthetic devices such as dental implants to suppress the formation of biofilms that cause infections. Non-Patent Documents 1 and 2 disclose that coating prosthetic devices with silver nanoparticles imparts antibacterial properties.

[0004] Furthermore, ceramic knives have traditionally been sold with antibacterial properties imparted by baking a titanium oxide coating onto the surface.

[0005] Kaijin Xu, Ceram. Int., 2011, 37, p2109-2115. "Microorganism adhesion inhibited by silver doped Yttria-stabilized zirconia ceramics" Yamada, R., Mater. Sci. Eng. C, 2017, 78, p1054-1060. "Ag nanoparticle-coated zirconia for antibacterial prosthesis”

[0006] However, such coatings may peel off due to wear, and the antibacterial effect is not long-lasting.

[0007] As a result of extensive research, the present inventors have come to the conclusion that if an antibacterial substance can be incorporated into the system of a zirconia sintered body, it may be possible to suppress the decrease in antibacterial activity due to wear.

[0008] Silver is said to have a broader antibacterial spectrum and stronger antibacterial activity than copper or zinc, which also have antibacterial activity. However, as a result of further investigations by the present inventors, it has become clear that when silver and stabilized zirconia are mixed to form a silver-containing zirconia powder and then sintered to produce a zirconia sintered body, the mechanical properties, sinterability, and hydrothermal degradation resistance are significantly reduced. Furthermore, when copper or zinc is mixed with stabilized zirconia and sintered, the sinterability and hydrothermal degradation resistance are not reduced.

[0009] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a silver-containing zirconia sintered body excellent in mechanical properties, sinterability, and resistance to hydrothermal degradation. It is also an object of the present invention to provide a silver-containing stabilized zirconia powder from which the silver-containing zirconia sintered body can be obtained by sintering. It is also an object of the present invention to provide a method for producing the silver-containing stabilized zirconia powder. It is also an object of the present invention to provide a method for producing the silver-containing zirconia sintered body.

[0010] The present inventors have conducted extensive research into silver-containing zirconia sintered bodies to address the above-mentioned problems, and have found that by employing the following configuration, a silver-containing zirconia sintered body having excellent mechanical properties, sinterability, and resistance to hydrothermal degradation can be provided, thereby completing the present invention.

[0011] That is, the present invention provides the following: [1] A silver-containing zirconia sintered body comprising silver particles and stabilized zirconia containing zirconia and a stabilizer, wherein the silver particles have an average particle size of 0.5 μm or less, the stabilized zirconia has an average crystal grain size of 0.35 μm or less, and the silver-containing zirconia sintered body has a relative sintered density of 98% or more.

[0012] According to the configuration [1], the silver particles are not coated on the surface of the silver-containing zirconia sintered body but are contained in the silver-containing zirconia sintered body itself. Therefore, even if the surface of the silver-containing zirconia sintered body wears, the silver particles are exposed from the inside, and the antibacterial effect can be maintained.

[0013] Furthermore, because silver has excellent ductility and malleability, it is difficult to atomize silver particles by pulverization. However, in the present invention, by employing the manufacturing method described below, it is possible to atomize the silver particles in the silver-containing zirconia sintered body. Specifically, the average particle size of the silver particles can be set to 0.5 μm or less. When the silver particles are fine, segregation of the silver particles within the silver-containing zirconia sintered body can be suppressed. As a result, sintering at low temperatures is possible. Furthermore, deterioration of mechanical properties is suppressed. In other words, by improving the dispersibility of the silver particles in the silver-containing zirconia sintered body, densification becomes possible (the relative sintered density can be increased), and deterioration of the mechanical properties of the silver-containing zirconia sintered body is suppressed. Specifically, by setting the relative sintered density to 98% or more, deterioration of the mechanical properties of the silver-containing zirconia sintered body is suppressed.

[0014] The relative sintered density can also be improved by increasing the sintering temperature (e.g., above 1500°C), but increasing the sintering temperature increases the zirconia crystal grain size, resulting in a decrease in hydrothermal degradation resistance. However, in the present invention, the sintering temperature is relatively low, thereby making the average crystal grain size of the stabilized zirconia 0.35 μm or less. As a result, the decrease in hydrothermal degradation resistance is suppressed.

[0015] According to the above-mentioned configuration [1], by setting the average particle size of the silver particles to 0.5 μm or less, the deterioration of sinterability is suppressed, and densification is possible (relative sintered density is 98% or more), and the deterioration of mechanical properties is suppressed. Furthermore, since the average crystal grain size of the stabilized zirconia is 0.35 μm or less, the deterioration of hydrothermal degradation resistance is suppressed.

[0016] Furthermore, the present invention provides the following: [2] The silver-containing zirconia sintered body according to the above [1], wherein the average crystal grain size of the stabilized zirconia is 0.25 μm or less.

[0017] When the average crystal grain size of the stabilized zirconia is 0.25 μm or less, the sintering temperature can be lowered.

[0018] The present invention further provides the following: [3] When the total amount of zirconia and the stabilizer is 100 mass %, silver particles are Ag 2 The silver-containing zirconia sintered body according to [1] or [2], containing 0.025% by mass or more and 20% by mass or more in terms of O.

[0019] When the content of the silver particles is 0.025% by mass or more, the antibacterial properties are excellent, and when the content of the silver particles is 20% by mass or less, the mechanical properties and sinterability are excellent.

[0020] Furthermore, the present invention provides the following: [4] The silver-containing zirconia sintered body according to any one of [1] to [3] above, which has a three-point bending strength of 600 MPa or more.

[0021] When the three-point bending strength is 600 MPa or more, it can be said that the strength is higher.

[0022] Furthermore, the present invention provides the following: [5] A steel sheet having a toughness value of 5 MPa m according to the IF method. 0.5 The silver-containing zirconia sintered body according to any one of [1] to [4] above.

[0023] The toughness value is 5 MPa m 0.5 If the value is above this, it can be said that the toughness is higher.

[0024] The present invention further provides the following: [6] The silver-containing zirconia sintered body according to any one of [1] to [5] above, which has a monoclinic ratio of 10% or less after hydrothermal treatment at 134°C and 0.3 MPa for 15 hours.

[0025] If the monoclinic ratio after hydrothermal treatment at 134° C. and 0.3 MPa for 15 hours is 10% or less, it can be said that the resistance to hydrothermal deterioration is more excellent.

[0026] Furthermore, the present invention provides the following: [7] The stabilizer is Y 2 O 3 , CeO 2 , Er 2 O 3 The silver-containing zirconia sintered body according to any one of [1] to [6], wherein the silver-containing zirconia sintered body is one or more selected from the group consisting of CaO.

[0027] The stabilizer is Y 2 O 3 , CeO 2 , Er 2 O 3 When the composition contains one or more elements selected from the group consisting of SiO 2 and CaO, the composition has excellent low-temperature sinterability and mechanical strength.

[0028] The present invention further provides the following: [8] The silver-containing zirconia sintered body according to any one of [1] to [7], wherein the content of the stabilizer is 15 mol % or less based on the total amount of zirconia and the stabilizer.

[0029] When the content of the stabilizer is 15 mol % or less, the mechanical strength is superior.

[0030] The present invention further provides the following: [9] A silver-containing stabilized zirconia powder comprising: stabilized zirconia containing zirconia and a stabilizer; and silver and / or silver oxide having an average particle size of 0.5 μm or less.

[0031] When the silver oxide particles are thermally decomposed, they become silver particles. The silver-containing stabilized zirconia powder of [9] contains stabilized zirconia and silver and / or silver oxide having an average particle size of 0.5 μm or less. Therefore, by sintering the silver-containing stabilized zirconia powder, a sintered body containing silver (silver particles) having an average particle size of 0.5 μm or less can be obtained. That is, whether the silver-containing stabilized zirconia powder contains only silver oxide having an average particle size of 0.5 μm or less, the silver-containing stabilized zirconia powder contains both silver and silver oxide having an average particle size of 0.5 μm or less, or the silver-containing stabilized zirconia powder contains only silver having an average particle size of 0.5 μm or less, the silver oxide particles become silver particles when thermally decomposed, and therefore, by sintering the silver-containing stabilized zirconia powder, a sintered body containing silver (silver particles) having an average particle size of 0.5 μm or less can be obtained. In particular, according to the configuration [9], the average particle size of silver and / or silver oxide is reduced to 0.5 μm or less and is highly dispersed in the stabilized zirconia powder, which makes it possible to easily control the crystal grain size of the stabilized zirconia in the zirconia sintered body obtained by sintering to 0.35 μm or less, thereby achieving the desired hydrothermal degradation resistance and mechanical properties.

[0032] The present invention further provides the following:

[10] The silver-containing stabilized zirconia powder according to [9], wherein the peak top diameter of the pore volume distribution is 30 nm to 100 nm, the pore volume is 0.25 ml / g to 0.46 ml / g, and the pore distribution width is 40 nm to 120 nm in the range of 10 nm to 0.5 μm in a pore size distribution determined by mercury intrusion porosimetry.

[0033] By reducing the average particle size of silver and / or silver oxide to 0.5 μm or less, highly dispersing silver and / or silver oxide in the stabilized zirconia powder, and controlling (optimizing) the pore size distribution of the silver-containing stabilized zirconia powder as described in

[10] above, the crystal grain size of the stabilized zirconia in the zirconia sintered body obtained by sintering can be easily controlled to 0.25 μm or less, and desired hydrothermal degradation properties and mechanical properties can be obtained.

[0034] The present invention further provides the following:

[11] A method for producing a silver-containing stabilized zirconia powder, comprising a step of mixing stabilized zirconia containing zirconia and a stabilizer with silver oxide having an average particle size of 0.5 μm or less.

[0035] Silver has excellent ductility and malleability, making it difficult to atomize by pulverization. On the other hand, silver oxide, due to its nature, can be atomized by pulverization. According to the configuration of

[10] , silver oxide atomized to an average particle size of 0.5 μm or less is mixed with stabilized zirconia to obtain a zirconia powder containing stabilized zirconia and silver oxide having an average particle size of 0.5 μm or less. Here, the silver oxide particles can be converted into silver particles by heating and thermal decomposition. Therefore, by sintering the silver-containing stabilized zirconia powder obtained by the manufacturing method of

[10] , a sintered body containing silver (silver particles) having an average particle size of 0.5 μm or less can be obtained.

[0036] The present invention further provides the following:

[12] A method for producing a silver-containing zirconia sintered body, comprising: a step X of molding the silver-containing stabilized zirconia powder according to the above item [9] or

[10] to obtain a molded body; and a step Y of sintering the molded body at a temperature of 1250°C or higher and 1500°C or lower for 1 hour or longer and 5 hours or shorter, after the step X.

[0037] According to the configuration

[12] , since the silver-containing stabilized zirconia powder according to the above [9] or

[10] is used, it is possible to obtain a sintered body with a high sintered density under sintering conditions at a low temperature of 1250° C. or higher and 1500° C. or lower. In addition, since the sintering is performed at a low temperature, the obtained sintered body has excellent resistance to hydrothermal degradation.

[0038] According to the present invention, a silver-containing zirconia sintered body having excellent mechanical properties, sinterability, and resistance to hydrothermal degradation can be provided. It is also possible to provide a silver-containing stabilized zirconia powder from which the silver-containing zirconia sintered body can be obtained by sintering. It is also possible to provide a method for producing the silver-containing stabilized zirconia powder. It is also possible to provide a method for producing the silver-containing zirconia sintered body.

[0039] 1 is a schematic diagram for explaining a method for producing a silver-containing stabilized zirconia powder according to an embodiment of the present invention, and FIG. 2 is a schematic diagram for explaining an indentation length and a crack length.

[0040] Hereinafter, embodiments of the present invention will be described. However, the present invention is not limited to these embodiments. In this specification, zirconia (zirconium oxide) is a general term and contains 10 mass % or less of impurity metal compounds including hafnia. In addition, in this specification, the expressions "contain" and "comprise" include the concepts of "contain," "comprise," "substantially consist," and "consist only of."

[0041] [Silver-containing zirconia sintered body] An example of the silver-containing zirconia sintered body according to this embodiment will be described below. However, the silver-containing zirconia sintered body of the present invention is not limited to the following example.

[0042] The silver-containing zirconia sintered body according to this embodiment contains silver particles and stabilized zirconia containing zirconia and a stabilizer, wherein the silver particles have an average particle size of 0.5 μm or less, the stabilized zirconia has an average crystal grain size of 0.35 μm or less, and has a relative sintered density of 98% or more.

[0043] The silver-containing zirconia sintered body contains silver particles. The average particle size of the silver particles is 0.5 μm or less. Because the average particle size of the silver particles is 0.5 μm or less, segregation of the silver particles within the silver-containing zirconia sintered body can be suppressed. As a result, a decrease in sinterability is suppressed. Furthermore, a decrease in mechanical properties is suppressed. In other words, by improving the dispersibility of the silver particles in the silver-containing zirconia sintered body, densification becomes possible (the relative sintered density can be increased), and a decrease in the mechanical properties of the silver-containing zirconia sintered body is suppressed.

[0044] The average particle size of the silver particles is preferably 0.4 μm or less. The smaller the average particle size of the silver particles, the more preferable it is, for example, 0.05 μm or more, 0.1 μm or more, etc. The average particle size of the silver particles is preferably 0.05 μm or more and 0.5 μm or less, more preferably 0.1 μm or more and 0.4 μm or less. The average particle size of the silver particles is measured by the method described in the Examples.

[0045] The content of the silver particles is 100% by mass of the total of zirconia and the stabilizer. 2 The silver content is preferably in the range of 0.025% by mass or more and 20% by mass or less in terms of O. When the content of the silver particles is 0.025% by mass or more, excellent antibacterial properties are achieved. Furthermore, when the content of the silver particles is 20% by mass or less, excellent mechanical properties and sinterability are achieved.

[0046] The content of the silver particles is 100% by mass of the total of zirconia and the stabilizer. 2 The content of the silver particles is more preferably 0.05% by mass or more, further preferably 0.1% by mass or more, and particularly preferably 0.5% by mass or more, calculated as O. When the total amount of zirconia and the stabilizer is 100% by mass, the content of the silver particles is more preferably 0.05% by mass or more, further preferably 0.1% by mass or more, and particularly preferably 0.5% by mass or more, calculated as O. 2 The content of the silver particles is more preferably 16% by mass or less, further preferably 12% by mass or less, and particularly preferably 10% by mass or less, calculated as O. When the total amount of zirconia and the stabilizer is 100% by mass, the content of the silver particles is more preferably 16% by mass or less, further preferably 12% by mass or less, and particularly preferably 10% by mass or less. 2 The O content is more preferably 0.05% by mass or more and 16% by mass or less, even more preferably 0.1% by mass or more and 12% by mass or less, and particularly preferably 0.5% by mass or more and 10% by mass or less, calculated as O.

[0047] The silver-containing zirconia sintered body contains stabilized zirconia containing zirconia and a stabilizer.

[0048] The total content of zirconia and stabilizer (stabilized zirconia content) in the silver-containing zirconia sintered body is preferably 70% by mass or more, and more preferably 80% by mass or more, when the entire silver-containing zirconia sintered body is taken as 100% by mass. The total content of zirconia and stabilizer can be 99.9% by mass or less, 99% by mass or less, when the entire silver-containing zirconia sintered body is taken as 100% by mass. The total content of zirconia and stabilizer in the silver-containing zirconia sintered body is more preferably 70% by mass or more and 99.9% by mass or less, and even more preferably 80% by mass or more and 99.9% by mass or less, when the entire silver-containing zirconia sintered body is taken as 100% by mass.

[0049] The stabilizer is preferably an oxide of one or more elements selected from alkaline earth metals and rare earth elements. The alkaline earth metals are Ca, Sr, Ba, and Ra. The rare earth elements are Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. The stabilizer is preferably an oxide of Y, 2 O 3 , CeO 2 , Er 2 O 3 and CaO. 2 O 3 , CeO 2 , Er 2 O 3 When the composition contains one or more elements selected from the group consisting of SiO 2 and CaO, the composition has excellent low-temperature sinterability and mechanical strength.

[0050] The content of the stabilizer is preferably 15 mol % or less based on the total amount of zirconia and stabilizer, which results in better mechanical strength.

[0051] The content of the stabilizer is preferably 1.4 mol% or more, more preferably 1.5 mol% or more, and even more preferably 1.6 mol% or more. The content of the stabilizer is preferably 14 mol% or less, more preferably 13 mol% or less, and even more preferably 12.5 mol% or less. The content of the stabilizer is more preferably 1.4 mol% or more and 14 mol% or less, more preferably 1.5 mol% or more and 13 mol% or less, and particularly preferably 1.6 mol% or more and 12.5 mol% or less.

[0052] The stabilizer is Y 2 O 3 When the zirconia and the stabilizer are used as a whole, the Y 2 O 3 The content of Y is preferably 1.4 mol % or more and 7.5 mol % or less. 2 O 3 The content of Y is more preferably 1.5 mol % or more, and further preferably 1.6 mol % or more. 2 O 3 The content of Y is more preferably 6.5 mol% or less, further preferably 6 mol%, particularly preferably 5.6 mol% or less, particularly preferably 5 mol% or less, and especially preferably 4.5 mol% or less. 2 O 3 When the content of Y is 1.4 mol % or more and 7.5 mol % or less, the silver-containing zirconia sintered body has better mechanical strength. 2 O 3 When the zirconia and the stabilizer are used as a whole, the Y 2 O 3 The content is more preferably 1.5 mol % or more and 6.5 mol % or less, and further preferably 1.6 mol % or more and 6 mol % or less.

[0053] As the stabilizer, CeO 2 When the zirconia and the stabilizer are used as a whole, the CeO 2 The content of CeO is preferably 10 mol % or more and 15 mol % or less. 2The content of CeO is more preferably 11 mol % or more, and further preferably 11.5 mol % or more. 2 The content of CeO is more preferably 14 mol% or less, further preferably 13 mol% or less, particularly preferably 12.5 mol% or less, particularly preferably 14 mol% or less, and especially preferably 12 mol% or less. 2 When the content of CeO is 10 mol % or more and 15 mol % or less, the silver-containing zirconia sintered body has better mechanical strength. 2 The content of CeO as the stabilizer is preferably 10 mol % or more and 14 mol % or less. 2 When the zirconia and the stabilizer are used as a whole, the CeO 2 The content is more preferably 11 mol % or more and 14 mol % or less, further preferably 11.5 mol % or more and 13 mol % or less, and particularly preferably 11.5 mol % or more and 12.5 mol % or less.

[0054] As the stabilizer, Sc 2 O 3 , Er 2 O 3 , Yb 2 O 3 When any of the above is used, the content of the zirconia and the stabilizer as a whole is preferably 1.4 mol % or more and 7.5 mol % or less. 2 O 3 , Er 2 O 3 , Yb 2 O 3 When any of the above is used, the content is more preferably 1.5 mol % or more, and further preferably 1.6 mol % or more. 2 O 3 , Er 2 O 3 , Yb 2 O 3 When any of the above is used, the content is more preferably 6.5 mol % or less, further preferably 6 mol %, particularly preferably 5.6 mol % or less, particularly preferably 5 mol % or less, and especially preferably 4.5 mol % or less.2 O 3 , Er 2 O 3 , Yb 2 O 3 When any one of the stabilizers is used, if the content is 1.4 mol % or more and 7.5 mol % or less, the silver-containing zirconia sintered body has superior mechanical strength. 2 O 3 , Er 2 O 3 , Yb 2 O 3 When any of the above is used, the content of the zirconia and stabilizer as a whole is more preferably 1.5 mol % or more and 6.5 mol % or less, and even more preferably 1.6 mol % or more and 6 mol % or less.

[0055] When CaO is used as the stabilizer, the CaO content is preferably 3.5 mol% or more and 15 mol% or less, based on the total amount of zirconia and stabilizer. The CaO content is more preferably 3.8 mol% or more, and even more preferably 4.0 mol% or more. The CaO content is more preferably 12.0 mol% or less, and even more preferably 9.0 mol% or less. When the CaO content is 3.5 mol% or more and 15 mol% or less, the silver-containing zirconia sintered body has superior mechanical strength. When CaO is used as the stabilizer, the CaO content is more preferably 3.8 mol% or more and 12 mol% or less, and even more preferably 4 mol% or more and 9 mol% or less, based on the total amount of zirconia and stabilizer.

[0056] CaO and Y are used as the stabilizers. 2 O 3When using zirconia and stabilizers as a whole, the total amount of the stabilizers is preferably 2.5 mol% or more and 6.5 mol% or less in terms of oxides, and the ratio of [CaO amount (mol%)] / [total amount of stabilizers (mol%)] is preferably 50% or more and 98% or less. The ratio of [CaO amount (mol%)] / [total amount of stabilizers (mol%)] is more preferably 55% or more, and even more preferably 60% or more. The ratio of [CaO amount (mol%)] / [total amount of stabilizers (mol%)] is more preferably 90% or less, and even more preferably 80% or less. The ratio of [CaO amount (mol%)] / [total amount of stabilizers (mol%)] is more preferably 55% or more and 90% or less, and even more preferably 60% or more and 80% or less.

[0057] CaO and Y are used as the stabilizers. 2 O 3 When using the stabilizer, the total amount of the stabilizer, based on the zirconia and stabilizer as a whole, is preferably 2.5 mol% or more and 6.5 mol% or less in terms of oxide. When the total amount of the stabilizer is 2.5 mol% or more in terms of oxide, the monoclinic phase fraction in the resulting zirconia sintered body can be reduced, thereby preventing cracks from occurring in the zirconia sintered body obtained by sintering the zirconia powder. Furthermore, when the total amount of the stabilizer is 6.5 mol% or less in terms of oxide, the cubic phase fraction, which has poor mechanical properties (strength, toughness), can be reduced and the tetragonal phase fraction, which has good mechanical properties, can be increased. The total amount of the stabilizer is preferably 2.7 mol% or more in terms of oxide, more preferably 2.9 mol% or more, and even more preferably 3.0 mol% or more. The total amount of the stabilizer is preferably 6.0 mol% or less in terms of oxide, more preferably 5.5 mol% or less, even more preferably 5.0 mol% or less, and particularly preferably 4.5 mol% or less. The total amount of the stabilizer is preferably 2.7 mol % or more and 6.0 mol % or less, more preferably 2.9 mol % or more and 5.5 mol % or less, still more preferably 3.0 mol % or more and 5.0 mol % or less, and particularly preferably 3.0 mol % or more and 4.5 mol % or less, calculated as oxide.

[0058] The stabilized zirconia has an average crystal grain size of 0.35 μm or less. Since the stabilized zirconia has an average crystal grain size of 0.35 μm or less, it has excellent resistance to hydrothermal degradation. Note that, although a high sintering temperature would increase the crystal grain size of the stabilized zirconia, since the average crystal grain size of the stabilized zirconia is 0.35 μm or less, the sintering temperature can be said to be low.

[0059] The average crystal grain size of the stabilized zirconia is preferably 0.3 μm or less, more preferably 0.25 μm or less, and even more preferably 0.2 μm or less. The smaller the average crystal grain size of the stabilized zirconia, the better, and is, for example, 0.05 μm or more, 0.1 μm or more, etc. The average crystal grain size of the stabilized zirconia is preferably 0.05 μm or more and 0.3 μm or less, more preferably 0.05 μm or more and 0.25 μm or less. The average crystal grain size of the stabilized zirconia is measured by the method described in the Examples.

[0060] The silver-containing zirconia sintered body contains Al when the total amount of zirconia and the stabilizer is 100 mass %. 2 O 3 The silver-containing zirconia sintered body may contain 25% by mass or less of alumina. When the silver-containing zirconia sintered body contains 25% by mass or less of alumina, the alumina acts as a sintering aid when the zirconia powder is sintered to obtain the silver-containing zirconia sintered body.

[0061] The silver-containing zirconia sintered body is Al 2 O 3 When the Al 2 O 3 From the viewpoint of suitably functioning as a sintering aid, the content of Al is more preferably 10% by mass or less, and even more preferably 1% by mass or less. 2 O 3 When the Al 2 O 3 From the viewpoint of suitably functioning as a sintering aid, the content of Al is more preferably 0.1 mass % or more, and even more preferably 0.25 mass % or more. 2 O 3 When the Al 2 O 3The content is more preferably 0.1% by mass or more and 10% by mass or less, and further preferably 0.25% by mass or more and 1% by mass or less.

[0062] The silver-containing zirconia sintered body may contain, in addition to alumina, sinterable ceramics, thermosetting resins, etc., for the purpose of improving properties such as strength.

[0063] The silver-containing zirconia sintered body may contain one or more elements selected from the group consisting of Fe, V, Mn, Co, Zn, Cu, and Ti. When the silver-containing zirconia sintered body contains one or more elements selected from the group consisting of Fe, V, Mn, Co, Zn, Cu, and Ti, it can be suitably colored.

[0064] <Monoclinic fraction before hydrothermal treatment> The monoclinic fraction contained in the crystalline phase of the silver-containing zirconia sintered body (monoclinic fraction before hydrothermal treatment) is preferably 0% or more and 10% or less. The monoclinic fraction is preferably 0%, but may be 0.1% or more, 0.5% or more, etc. The monoclinic fraction is more preferably 5% or less, and even more preferably 1% or less. The monoclinic fraction is more preferably 0% or more and 10% or less, and even more preferably 0% or more and 1% or less. When the monoclinic fraction is 0% or more and 10% or less, the mechanical properties (flexural strength, fracture toughness) are more excellent. The monoclinic fraction can be controlled, for example, by the average particle size of the silver particles, the content of the silver particles, the content and content ratio of the stabilizer, the sintering temperature, etc. The monoclinic fraction is determined according to the method described in the Examples.

[0065] <Hydrothermal Degradation Resistance> The silver-containing zirconia sintered body preferably has a monoclinic fraction of 80% or less after hydrothermal treatment at 134°C and 0.3 MPa (absolute pressure 0.3 MPa) for 15 hours. A monoclinic fraction of 80% or less after hydrothermal treatment can be said to have better hydrothermal degradation resistance. The monoclinic fraction after hydrothermal treatment can be controlled by, for example, the average particle size of the silver particles, the content of the silver particles, the content and content ratio of the stabilizer, the sintering temperature, etc.

[0066] The monoclinic fraction after the hydrothermal treatment is more preferably 50% or less, and even more preferably 10% or less. The smaller the monoclinic fraction after the hydrothermal treatment, the more preferable it is, for example, 0.1% or more, 0.5% or more. The monoclinic fraction after the hydrothermal treatment is more preferably 0% or more and 50% or less, and even more preferably 0% or more and 10% or less.

[0067] <Mechanical Strength> The silver-containing zirconia sintered body preferably has a three-point bending strength of 600 MPa or more.

[0068] The three-point bending strength is more preferably 700 MPa or more, and even more preferably 800 MPa or more. The higher the three-point bending strength, the better, but it can be, for example, 1500 MPa or less, 1200 MPa or less, etc. The three-point bending strength is more preferably 700 MPa or more and 1500 MPa or less, and even more preferably 800 MPa or more and 1500 MPa or less.

[0069] When the three-point bending strength is 600 MPa or more, it can be said that the strength is higher. The three-point bending strength is determined by the method described in the examples.

[0070] <Toughness> The silver-containing zirconia sintered body has a toughness value of 5 MPa m 0.5 It is preferable that this is equal to or greater than this.

[0071] The toughness value is more preferably 6 MPa m 0.5 More preferably, 10 MPa m 0.5 The higher the toughness value, the better. 0.5 Below, 25MPa・m 0.5 The toughness value is more preferably 6 MPa m 0.5 20MPa・m or more 0.5 More preferably, 10 MPa m 0.5 20MPa・m or more 0.5 The following is the result.

[0072] The toughness value is 5 MPa m 0.5 The toughness value is determined by the method described in the Examples.

[0073] <Relative sintered density> The relative sintered density of the silver-containing zirconia sintered body is preferably 98% or more, and more preferably 98.5% or more. When the relative sintered density is 98% or more, it can be said that the silver-containing zirconia sintered body is sufficiently sintered. Furthermore, when the relative sintered density is 98% or more, it can be said that the silver-containing zirconia sintered body has higher strength.

[0074] <Method for measuring relative sintered density of silver-containing zirconia sintered body> The relative sintered density is expressed by the following formula (1): Relative sintered density (%) = (sintered density / theoretical sintered density) × 100 (1) Here, the theoretical sintered density (ρ 0 ) is a value calculated by the following formula (2-1): 0 = (100 + Y + Z) / [(100 / ρz) + (Y / 3.987) + (Z / 10.49)] ... (2-1) where Y is the alumina concentration (wt%) and Z is the silver concentration (wt%). When silver oxide is used as the raw material, the silver concentration (wt%) is calculated from formula (2-2). Z = [107.868 × (silver oxide concentration (wt%))] / (231.736 × 2) ... (2-2) ρz is a value calculated from the following formula (2-3). ρz = [124.25 (100 - X) + [molecular weight of stabilizer] × X] / 150 [150.5 (100 + X)A 2 C] ... (2-3) Here, the molecular weight of the stabilizer is determined by the following formula: 2 O 3 In the case of 225.81, Er 2 O 3 382.52 in the case of Yb 2 O 3In this case, 394.11 is used. X is the stabilizer concentration (mol %). A and C are values ​​calculated by the following formulas (2-4) and (2-5), respectively. A = 0.5080 + 0.06980X / (100 + X) ... (2-4) C = 0.5195 - 0.06180X / (100 + X) ... (2-5) In formula (1), the theoretical sintered density varies depending on the powder composition. For example, the theoretical sintered density of yttria-containing zirconia is 6.117 g / cm when the yttria content is 2 mol %. 3 , 3 mol% is 6.098 g / cm 3 , 5.5 mol% is 6.051 g / cm 3 (Al 2 O 3 = 0 wt %). 2 O 3 In this case, ρz is a value calculated by the following formula (3): ρz = -0.0402(Sc 2 O 3 (molar concentration of CaO) + 6.1294 ... (3) When the stabilizer is CaO, ρz is a value calculated by the following formula (3-1): ρz = -0.0400 (molar concentration of CaO) + 6.1700 ... (3-1) When a colorant is included, the theoretical sintered density (denoted as ρ1) is: ρ1 = 100 / [(Z / V) + (100 - Z) / ρ0] ... (2-5) Furthermore, Z is the colorant concentration (wt %), V is the colorant theoretical density (g / cm 3 The theoretical density of the colorant is Fe 2 O 3 is 5.24 g / cm 3 , ZnO is 5.61 g / cm 3 , MnO 2 is 5.03 g / cm 3 , CoO is 6.10 g / cm 3 , Cr 2 O 3 is 5.22 g / cm 3 , TiO 2 is 4.23 g / cm 3 , Tb 4 O 7 is 7.80 g / cm 3 , CuO is 6.31 g / cm 3 , V 2 O5 is 3.36 g / cm 3 The sintered density is measured by the Archimedes method.

[0075] The silver-containing zirconia sintered body according to this embodiment can be obtained, for example, by the method for producing a silver-containing zirconia sintered body described below.

[0076] The silver-containing zirconia sintered body according to this embodiment can be used as an industrial part, an aesthetic part, or a dental material. More specifically, it can be used for jewelry, watch parts, watch dials, artificial teeth, molding components, wear-resistant components, chemical-resistant components, and the like. In particular, when a blade is made from the silver-containing zirconia sintered body, the decrease in antibacterial activity due to wear and sharpening associated with use can be suppressed. Furthermore, since the resistance to hydrothermal degradation is improved by low-temperature sintering, stable mechanical properties can be exhibited even under conditions that cause hydrothermal degradation, such as in a dishwasher.

[0077] [Silver-Containing Stabilized Zirconia Powder] The silver-containing stabilized zirconia powder according to this embodiment contains stabilized zirconia containing zirconia and a stabilizer, and silver and / or silver oxide having an average particle size of 0.5 μm or less.

[0078] The silver-containing stabilized zirconia powder contains primary particles of stabilized zirconia containing zirconia as a primary component. All or part of the primary particles aggregate to form secondary particles. That is, the silver-containing stabilized zirconia powder contains non-aggregated primary particles of stabilized zirconia and secondary particles formed by aggregation of the primary particles. However, in the silver-containing stabilized zirconia powder, the amount of primary particles that do not form secondary particles and exist in the form of non-aggregated primary particles is extremely small, for example, less than 1 mass% of the total primary particles (the sum of non-aggregated primary particles and primary particles that have aggregated to form secondary particles). That is, the silver-containing stabilized zirconia powder may contain a very small amount of non-aggregated primary particles, but is mostly composed of secondary particles. Note that "containing zirconia as a primary component" means that the primary particles contain 70 mass% or more of zirconia when the primary particles are 100 mass%. That is, in this specification, primary particles containing zirconia as a primary component refer to primary particles containing 70 mass% or more of zirconia. The content of zirconia contained in the primary particles is preferably 74% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass or more.

[0079] <Composition> The silver-containing stabilized zirconia powder according to this embodiment contains silver and / or silver oxide having an average particle size of 0.5 μm or less.

[0080] When the silver oxide particles are thermally decomposed, they become silver particles. The silver-containing stabilized zirconia powder contains stabilized zirconia and silver and / or silver oxide having an average particle size of 0.5 μm or less. Therefore, by sintering the silver-containing stabilized zirconia powder, a sintered body containing silver (silver particles) having an average particle size of 0.5 μm or less can be obtained. That is, whether the silver-containing stabilized zirconia powder contains only silver oxide having an average particle size of 0.5 μm or less, the silver-containing stabilized zirconia powder contains both silver and silver oxide having an average particle size of 0.5 μm or less, or the silver-containing stabilized zirconia powder contains only silver having an average particle size of 0.5 μm or less, the silver oxide particles become silver particles when thermally decomposed, and therefore, by sintering the silver-containing stabilized zirconia powder, a sintered body containing silver (silver particles) having an average particle size of 0.5 μm or less can be obtained.

[0081] In this specification, the average particle size of silver and / or silver oxide refers to the overall average particle size of silver and silver oxide, without distinguishing between silver and silver oxide. The method for measuring the average particle size of silver and / or silver oxide is the method described in the Examples.

[0082] The average particle size of the silver and / or silver oxide is preferably 0.4 μm or less, more preferably 0.3 μm or less. The smaller the average particle size of the silver and / or silver oxide, the better, and is, for example, 0.01 μm or more, 0.05 μm or more, etc. The average particle size of the silver and / or silver oxide is preferably 0.01 μm or more and 0.4 μm or less, more preferably 0.01 μm or more and 0.3 μm or less.

[0083] The content of the silver and / or silver oxide is, when the total of the zirconia and the stabilizer is 100 mass %, Ag 2 The silver and / or silver oxide content is preferably in the range of 0.025% by mass or more and 20% by mass or less, calculated as O. When the silver and / or silver oxide content is 0.025% by mass or more, excellent antibacterial properties are obtained. Furthermore, when the silver and / or silver oxide content is 20% by mass or less, excellent sinterability is obtained. Furthermore, when the silver and / or silver oxide content is 20% by mass or less, the mechanical properties of the resulting sintered body are excellent.

[0084] The content of the silver and / or silver oxide is, when the total of the zirconia and the stabilizer is 100 mass %, Ag 2 The content of silver and / or silver oxide is more preferably 0.05% by mass or more, further preferably 0.1% by mass or more, and particularly preferably 0.5% by mass or more, calculated as O. When the total of zirconia and the stabilizer is taken as 100% by mass, the content of silver and / or silver oxide is more preferably 0.05% by mass or more, further preferably 0.1% by mass or more, and particularly preferably 0.5% by mass or more. 2 The content of silver and / or silver oxide is more preferably 16% by mass or less, further preferably 12% by mass or less, and particularly preferably 10% by mass or less, calculated as O. When the total of zirconia and the stabilizer is taken as 100% by mass, the content of silver and / or silver oxide is more preferably 16% by mass or less, further preferably 12% by mass or less, and particularly preferably 10% by mass or less. 2 The O content is more preferably 0.05% by mass or more and 16% by mass or less, even more preferably 0.1% by mass or more and 12% by mass or less, and particularly preferably 0.5% by mass or more and 10% by mass or less, calculated as O.

[0085] The silver-containing stabilized zirconia powder contains stabilized zirconia containing zirconia and a stabilizer.

[0086] The stabilized zirconia contains a stabilizer. The stabilizer is contained in the primary particles in the form of a solid solution, etc. Because the stabilizer is contained, the silver-containing stabilized zirconia powder can be suitably sintered at a low temperature.

[0087] The stabilizer is preferably an oxide of one or more elements selected from alkaline earth metals and rare earth elements. The alkaline earth metals are Ca, Sr, Ba, and Ra. The rare earth elements are Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. The stabilizer is preferably an oxide of Y, 2 O 3 , CeO 2 , Er 2 O 3 and CaO. 2 O 3 , CeO 2 , Er 2 O 3When the content of the SiO 2 -containing SiO 3 is at least one selected from the group consisting of SiO 2 and CaO, the low-temperature sintering property is excellent and the mechanical strength of the resulting sintered body is excellent.

[0088] The content of the stabilizer is preferably 15 mol % or less based on the total amount of zirconia and stabilizer, and when the content of the stabilizer is 15 mol % or less, the mechanical strength of the resulting sintered body is superior.

[0089] The content of the stabilizer is preferably 1.4 mol% or more, more preferably 1.5 mol% or more, and even more preferably 1.6 mol% or more. The content of the stabilizer is preferably 14 mol% or less, more preferably 13 mol% or less, and even more preferably 12.5 mol% or less. The content of the stabilizer is more preferably 1.4 mol% or more and 14 mol% or less, more preferably 1.5 mol% or more and 13 mol% or less, and particularly preferably 1.6 mol% or more and 12.5 mol% or less.

[0090] The stabilizer is Y 2 O 3 When the zirconia and the stabilizer are used as a whole, the Y 2 O 3 The content of Y is preferably 1.4 mol % or more and 7.5 mol % or less. 2 O 3 The content of Y is more preferably 1.5 mol % or more, and further preferably 1.6 mol % or more. 2 O 3 The content of Y is more preferably 6.5 mol% or less, further preferably 6 mol%, particularly preferably 5.6 mol% or less, particularly preferably 5 mol% or less, and especially preferably 4.5 mol% or less. 2 O 3 When the content of Y as the stabilizer is 1.4 mol % or more and 7.5 mol % or less, the zirconia sintered body obtained by sintering the silver-containing stabilized zirconia powder has better mechanical strength. 2 O 3 When the zirconia and the stabilizer are used as a whole, the Y 2 O 3The content is more preferably 1.5 mol % or more and 6.5 mol % or less, and further preferably 1.6 mol % or more and 6 mol % or less.

[0091] As the stabilizer, CeO 2 When the zirconia and the stabilizer are used as a whole, the CeO 2 The content of CeO is preferably 10 mol % or more and 15 mol % or less. 2 The content of CeO is more preferably 11 mol % or more, and further preferably 11.5 mol % or more. 2 The content of CeO is more preferably 14 mol% or less, further preferably 13 mol% or less, particularly preferably 12.5 mol% or less, and particularly preferably 12 mol% or less. 2 When the content of CeO is 10 mol % or more and 15 mol % or less, the zirconia sintered body obtained by sintering the silver-containing stabilized zirconia powder has excellent mechanical strength. 2 The content of CeO as the stabilizer is preferably 10 mol % or more and 14 mol % or less. 2 When the zirconia and the stabilizer are used as a whole, the CeO 2 The content is more preferably 11 mol % or more and 14 mol % or less, further preferably 11.5 mol % or more and 13 mol % or less, and particularly preferably 11.5 mol % or more and 12.5 mol % or less.

[0092] As the stabilizer, Sc 2 O 3 , Er 2 O 3 , Yb 2 O 3 When any of the above is used, the content of the zirconia and the stabilizer as a whole is preferably 1.4 mol % or more and 7.5 mol % or less. 2 O 3 , Er 2 O 3 , Yb 2 O 3When any of the above is used, the content is more preferably 1.5 mol % or more, and further preferably 1.6 mol % or more. 2 O 3 , Er 2 O 3 , Yb 2 O 3 When any of the above is used, the content is more preferably 6.5 mol % or less, further preferably 6 mol %, particularly preferably 5.6 mol % or less, particularly preferably 5 mol % or less, and especially preferably 4.5 mol % or less. 2 O 3 , Er 2 O 3 , Yb 2 O 3 When the content of any one of the stabilizers is 1.4 mol % or more and 7.5 mol % or less, the zirconia sintered body obtained by sintering the silver-containing stabilized zirconia powder has better mechanical strength. 2 O 3 , Er 2 O 3 , Yb 2 O 3 When any of the above is used, the content of the zirconia and stabilizer as a whole is more preferably 1.5 mol % or more and 6.5 mol % or less, and even more preferably 1.6 mol % or more and 6 mol % or less.

[0093] When CaO is used as the stabilizer, the CaO content, based on the total amount of zirconia and stabilizer, is preferably 3.5 mol% or more and 15 mol% or less. The CaO content is more preferably 3.8 mol% or more, and even more preferably 4.0 mol% or more. The CaO content is more preferably 12.0 mol% or less, and even more preferably 9.0 mol% or less. When the CaO content is 3.5 mol% or more and 15 mol% or less, the zirconia sintered body obtained by sintering the silver-containing stabilized zirconia powder has superior mechanical strength. When CaO is used as the stabilizer, the CaO content, based on the total amount of zirconia and stabilizer, is more preferably 3.8 mol% or more and 12 mol% or less, and even more preferably 4 mol% or more and 9 mol% or less.

[0094] CaO and Y are used as the stabilizers. 2 O 3 When using zirconia and stabilizers as a whole, the total amount of the stabilizers is preferably 2.5 mol% or more and 6.5 mol% or less in terms of oxides, and the ratio of [CaO amount (mol%)] / [total amount of stabilizers (mol%)] is preferably 50% or more and 98% or less. The ratio of [CaO amount (mol%)] / [total amount of stabilizers (mol%)] is more preferably 55% or more, and even more preferably 60% or more. The ratio of [CaO amount (mol%)] / [total amount of stabilizers (mol%)] is more preferably 90% or less, and even more preferably 80% or less. The ratio of [CaO amount (mol%)] / [total amount of stabilizers (mol%)] is more preferably 55% or more and 90% or less, and even more preferably 60% or more and 80% or less.

[0095] CaO and Y are used as the stabilizers. 2 O 3When using the stabilizer, the total amount of the stabilizer, based on the zirconia and stabilizer as a whole, is preferably 2.5 mol% or more and 6.5 mol% or less in terms of oxide. When the total amount of the stabilizer is 2.5 mol% or more in terms of oxide, the monoclinic phase fraction in the resulting zirconia sintered body can be reduced, thereby preventing cracks from occurring in the zirconia sintered body obtained by sintering the zirconia powder. Furthermore, when the total amount of the stabilizer is 6.5 mol% or less in terms of oxide, the cubic phase fraction, which has poor mechanical properties (strength, toughness), can be reduced and the tetragonal phase fraction, which has good mechanical properties, can be increased. The total amount of the stabilizer is preferably 2.7 mol% or more in terms of oxide, more preferably 2.9 mol% or more, and even more preferably 3.0 mol% or more. The total amount of the stabilizer is preferably 6.0 mol% or less in terms of oxide, more preferably 5.5 mol% or less, even more preferably 5.0 mol% or less, and particularly preferably 4.5 mol% or less. The total amount of the stabilizer is preferably 2.7 mol % or more and 6.0 mol % or less, more preferably 2.9 mol % or more and 5.5 mol % or less, still more preferably 3.0 mol % or more and 5.0 mol % or less, and particularly preferably 3.0 mol % or more and 4.5 mol % or less, calculated as oxide.

[0096] The silver-containing zirconia powder contains Al when the total amount of zirconia and the stabilizer is 100 mass %. 2 O 3 The zirconia powder may contain 25% by mass or less of alumina. When the zirconia powder contains 25% by mass or less of alumina, the alumina acts as a sintering aid when the zirconia powder is sintered to obtain a silver-containing zirconia sintered body.

[0097] The silver-containing zirconia powder is Al 2 O 3 When the Al 2 O 3 From the viewpoint of suitably functioning as a sintering aid, the content of Al is more preferably 10% by mass or less, and further preferably 1% by mass or less. 2 O 3 When the Al 2 O 3From the viewpoint of suitably functioning as a sintering aid, the content of Al is more preferably 0.1 mass % or less, and even more preferably 0.25 mass % or less. 2 O 3 When the Al 2 O 3 The content of is more preferably 0.1% by mass or more and 10% by mass or less, and even more preferably 0.25% by mass or more and 1% by mass or less. When the alumina in the silver-containing stabilized zirconia powder is in the form of a powder, there are no particular restrictions on the average particle size of the primary particles of the alumina, but it is, for example, 0.02 to 0.4 μm, preferably 0.05 to 0.3 μm, and more preferably 0.07 to 0.2 μm. Note that when the silver-containing stabilized zirconia powder has the following pore volume distribution, low-temperature sintering is possible. Therefore, low-temperature sintering is possible even when the powder does not contain a sintering aid.

[0098] The silver-containing stabilized zirconia powder may contain, in addition to alumina, sinterable ceramics, thermosetting resins, etc., for the purpose of improving properties such as strength.

[0099] The silver-containing stabilized zirconia powder may contain one or more elements selected from the group consisting of Fe, V, Mn, Co, Cr, Tb, Zn, Cu, and Ti. When the silver-containing stabilized zirconia powder contains one or more elements selected from the group consisting of Fe, V, Mn, Co, Cr, Tb, Zn, Cu, and Ti as a coloring element, the zirconia sintered body obtained by sintering the silver-containing stabilized zirconia powder can be suitably colored.

[0100] <Pore Distribution> 1. Peak Top Diameter of Primary Particle Gaps The silver-containing stabilized zirconia powder preferably has a peak top diameter of 20 nm to 200 nm in the pore volume distribution in the range of 10 nm to 0.5 μm in the pore distribution measured by mercury intrusion porosimetry. The peak top diameter is preferably 25 nm or more, more preferably 30 nm or more, even more preferably 32 nm or more, and particularly preferably 35 nm or more. The peak top diameter is preferably 150 nm or less, more preferably 120 nm or less, even more preferably 100 nm or less, and particularly preferably 85 nm or less. The peak top diameter is preferably 25 nm to 150 nm, more preferably 30 nm to 120 nm. In addition, when there are multiple peaks in the range of 10 nm or more and 0.5 μm or less in the pore distribution, the phrase "the peak top diameter of the pore volume distribution is 20 nm or more and 200 nm or less" in this specification means that all peak top diameters in the range of 10 nm or more and 0.5 μm or less in the pore distribution are within the range of 20 nm or more and 200 nm or less.

[0101] 2. Pore Distribution Width of Primary Particle Gaps The silver-containing stabilized zirconia powder preferably has a pore distribution width of 40 nm to 200 nm in the range of 10 nm to 0.5 μm in the pore size distribution measured by mercury intrusion porosimetry. The pore distribution width is preferably 43 nm or more, more preferably 46 nm or more, even more preferably 50 nm or more, and particularly preferably 55 nm or more. The pore distribution width is preferably 150 nm or less, more preferably 120 nm or less, even more preferably 110 nm or less, particularly preferably 100 nm or less, and especially preferably 80 nm or less. The pore distribution width is preferably 43 nm to 150 nm, more preferably 46 nm to 120 nm. Here, the pore distribution width refers to the width of the peak at which the log differential pore volume is 0.1 ml / g or more. In addition, when there are multiple peaks in the pore distribution in the range of 10 nm or more and 0.5 μm or less, the term "pore distribution width is 40 nm or more and 200 nm or less" as used herein means that, in a graph showing the pore distribution with pore diameter on the horizontal axis and log differential pore volume on the vertical axis, the point at which, viewed from the smaller pore diameter side, the smallest diameter is defined as the point at which the smallest diameter first intersects with the log differential pore volume of 0.1 mL / g (the point at which the intersects while ascending), and the point at which the smallest diameter again intersects with the log differential pore volume of 0.1 mL / g (the point at which the intersects while descending) is defined as the maximum diameter, and the difference between the largest diameter and the smallest diameter is 40 nm or more and 200 nm or less.

[0102] 3. Pore Volume of Primary Particle Gaps The silver-containing stabilized zirconia powder preferably has a pore volume of 0.2 ml / g or more but less than 0.5 ml / g in the pore size range of 10 nm to 0.5 μm in a pore size distribution determined by mercury intrusion porosimetry. The pore volume is preferably 0.22 ml / g or more, more preferably 0.25 ml / g or more, even more preferably 0.3 ml / g or more, particularly preferably 0.35 ml / g or more, and especially preferably 0.4 ml / g or more. The pore volume is preferably 0.48 ml / g or less, more preferably 0.46 ml / g or less, and particularly preferably 0.44 ml / g or less. The pore volume is preferably 0.22 ml / g or more but less than 0.48 ml / g, more preferably 0.25 ml / g or more but less than 0.46 ml / g.

[0103] The "range of 10 nm to 0.5 μm in the pore size distribution determined by mercury intrusion porosimetry" is the range in which pores can exist as gaps between primary particles in the silver-containing stabilized zirconia powder. When the peak-top diameter of the pore volume distribution is 20 nm to 200 nm and the pore distribution width is 40 nm to 200 nm in the range of 10 nm to 0.5 μm in the pore size distribution determined by mercury intrusion porosimetry, the size of each pore (the gaps between primary particles) is small and uniform (the distribution is sharp). Therefore, the primary particles constituting the secondary particles are uniformly and densely agglomerated, and no large pores are present. Zirconia particles (including primary and secondary particles) are characterized by the fact that a large pore volume makes them difficult to sinter. In other words, to sinter at low temperatures, not only must the size of the pores originating from the gaps between primary particles in the secondary particles be small and the distribution be sharp, but the pore volume originating from the gaps between primary particles must also be reduced. Therefore, if the pore volume in the range of 10 nm to 0.5 μm in the pore size distribution based on mercury intrusion porosimetry is 0.2 ml / g or more and less than 0.5 ml / g, the pore volume derived from the gaps between primary particles will be small and large pores will not be present, making it possible to obtain a sintered body with a high sintered density. In this way, by controlling the pore size, pore distribution, and pore volume of the gaps between primary particles, low-temperature sintering is possible and a sintered body with a high sintered density can be obtained.

[0104] <Particle diameter D 50 > Particle diameter D of the silver-containing stabilized zirconia powder 50 The particle diameter D is preferably 0.1 μm or more and 1.5 μm or less. 50 is preferably 0.1 μm or more, more preferably 0.20 μm or more, even more preferably 0.25 μm or more, and particularly preferably 0.30 μm or more. 50 is preferably 1.2 μm or less, more preferably 1.0 μm or less, even more preferably 0.8 μm or less, particularly preferably 0.7 μm or less, especially preferably 0.6 μm or less, and especially preferably less than 0.5 μm. 50The particle diameter D is preferably 0.1 μm or more and 1.5 μm or less, and more preferably 0.20 μm or more and 1.0 μm or less. 50 The particle diameter D 50 When measuring the particle diameter D, not only secondary particles but also non-aggregated primary particles may be included, but the amount of non-aggregated primary particles that may be contained in the silver-containing stabilized zirconia powder is extremely small. 50 is the particle diameter D of the secondary particles 50 , that is, it can be considered to represent the average particle size of the secondary particles. 50 When the particle size is 1.5 μm or less, the particle size of the secondary particles is relatively small, so that the gaps between the secondary particles can be made small. As a result, the low-temperature sintering property is excellent. In addition, since the gaps between the secondary particles are small, a sintered body with a high sintering density can be obtained.

[0105] <Specific surface area> The specific surface area of ​​the silver-containing stabilized zirconia powder is 5 m 2 / g or more 60m 2 The specific surface area is preferably 5 m / g or less. 2 / g or more, more preferably 9m 2 / g or more, more preferably 13m 2 / g or more, particularly preferably 15m 2 The specific surface area is preferably 50 m / g or more. 2 / g or less, more preferably 40m 2 / g or less, more preferably 35m 2 / g or less, particularly preferably 30m 2 The specific surface area of ​​the silver-containing stabilized zirconia powder is 9 m / g or less. 2 / g or more 40m 2 / g or less is more preferable, and 13m 2 / g or more 35m 2 / g or less, and more preferably 15m 2 / g or more 30m 2 / g or less is particularly preferred. In order to sinter stabilized zirconia powder at a temperature of about 1300°C to 1500°C, which is lower than conventional temperatures, it is effective to increase the specific surface area. However, conventionally, it has been difficult to control the grain growth rate during the production of stabilized zirconia powder, and in order to minimize the number of pores remaining in the stabilized zirconia powder, it has been necessary to increase the specific surface area to 15 m 2 On the other hand, if the gap between primary particles is controlled as described above, it is possible to make the specific surface area 15 m 2 / g or more, not many pores remain in the silver-containing stabilized zirconia powder. 2 / g or more, the low-temperature sintering property can be improved. The specific surface area is a value obtained by the method described in the examples.

[0106] The silver-containing stabilized zirconia powder according to this embodiment has been described above.

[0107] [Method for Producing Silver-Containing Stabilized Zirconia Powder] An example of a method for producing a silver-containing stabilized zirconia powder will be described below, although the method for producing a silver-containing stabilized zirconia powder is not limited to the following example.

[0108] The method for producing a silver-containing stabilized zirconia powder according to this embodiment includes a step of mixing stabilized zirconia containing zirconia and a stabilizer with silver oxide having an average particle size of 0.5 μm or less.

[0109] The method for producing the silver-containing stabilized zirconia powder preferably includes: Step 1 of separately heating a zirconium salt solution and a sulfating agent solution to 95° C. or higher and 100° C. or lower; Step 2 of contacting the heated zirconium salt solution and the heated sulfating agent solution so that the concentration of the mixed solution does not change from the start to the end of contact, thereby obtaining a basic zirconium sulfate-containing reaction solution as a mixed solution; Step 3 of aging the basic zirconium sulfate-containing reaction solution obtained in Step 2 at 95° C. or higher for 3 hours or more; Step 4 of adding a stabilizer to the basic zirconium sulfate-containing reaction solution after aging obtained in Step 3; Step 5 of adding an alkali to the basic zirconium sulfate-containing reaction solution obtained in Step 4, thereby obtaining a zirconium-containing hydroxide; Step 6 of heat-treating the zirconium-containing hydroxide obtained in Step 5, thereby obtaining stabilized zirconia; and Step 7 of mixing the stabilized zirconia obtained in Step 6 with silver oxide having an average particle size of 0.5 μm or less. In Step 2, SO in the mixed solution is maintained at 95° C. or higher from the start to the end of the contact. 4 2- / ZrO 2 The weight ratio is maintained in the range of 0.3 to 0.8, and the temperature of the mixed liquid is maintained at 95° C. or higher. Each step will be explained in detail below.

[0110] <Step 1> In step 1, the starting materials, the zirconium salt solution and the sulfating agent solution, are each separately heated to 95°C or higher and 100°C or lower. The zirconium salt used to prepare the zirconium salt solution may be any zirconium salt that supplies zirconium ions, and examples thereof include zirconium oxynitrate, zirconium oxychloride, and zirconium nitrate. These may be used alone or in combination of two or more. Among these, zirconium oxychloride is preferred because of its high productivity on an industrial scale.

[0111] The solvent used to prepare the zirconium salt solution may be selected depending on the type of zirconium salt, etc. Generally, water (pure water, ion-exchanged water, the same applies hereinafter) is preferred.

[0112] The concentration of the zirconium salt solution is not particularly limited, but is generally 1000 g of zirconium oxide (ZrO 2 The content is preferably 5 to 250 g, more preferably 20 to 150 g, calculated as 100 g of cellulose esters.

[0113] The sulfating agent may be any agent that reacts with zirconium ions to produce a sulfate (i.e., a sulfating reagent), and examples thereof include sodium sulfate, potassium sulfate, ammonium sulfate, potassium hydrogen sulfate, sodium hydrogen sulfate, potassium disulfate, sodium disulfate, and sulfur trioxide. The sulfating agent may be in any form, such as a powder or a solution, but a solution (particularly an aqueous solution) is preferred. The solvent may be the same as the solvent used to prepare the zirconium salt solution.

[0114] The acid concentration of the zirconium salt solution is preferably 0.1 to 2.0 N. By setting the acid concentration within this range, the aggregation state of the particles constituting the silver-containing stabilized zirconia powder can be controlled to a suitable state. The acid concentration can be adjusted by using, for example, hydrochloric acid, nitric acid, sodium hydroxide, etc.

[0115] The concentration of the sulfating agent (sulfating agent solution) is not particularly limited, but it is generally preferred that the sulfating agent be used in an amount of 5 to 250 g, particularly 20 to 150 g, per 1000 g of solvent.

[0116] The materials of the containers for preparing the zirconium salt solution and the sulfating agent solution are not particularly limited as long as they have a capacity that allows sufficient stirring of the zirconium salt solution and the sulfating agent solution, respectively. However, it is preferable that the containers have equipment that can appropriately heat the solutions so that the temperatures do not fall below 95°C. The heating temperatures of the zirconium salt solution and the sulfating agent solution may be 95°C or higher and 100°C or lower, and preferably 97°C or higher. If step 2 is performed while the temperatures of the zirconium salt solution and the sulfating agent solution are below 95°C, the zirconium salt solution and the sulfating agent will not react sufficiently, resulting in a reduced yield.

[0117] <Step 2> In step 2, the heated zirconium salt solution and the heated sulfating agent solution are brought into contact with each other so that the concentration of the mixed solution does not change from the start to the end of the contact, thereby obtaining a basic zirconium sulfate-containing reaction solution as a mixed solution. 4 2- / ZrO 2 The weight ratio is maintained in the range of 0.3 to 0.8, and the temperature of the mixed liquid is maintained at 95° C. or higher. Step 2 will now be described with reference to the drawings.

[0118] FIG. 1 is a schematic diagram illustrating a method for producing a silver-containing stabilized zirconia powder according to this embodiment. As shown in FIG. 1 , a container 10 is connected to one upper end (left side in FIG. 1 ) of a T-shaped tube 20 via a valve 12. A container 30 is connected to the other upper end (right side in FIG. 1 ) of the T-shaped tube 20 via a valve 32. A zirconium solution heated to 95°C or higher and 100°C or lower is stored in the container 10. A sulfating agent solution heated to 95°C or higher and 100°C or lower is stored in the container 30. In step 2, the zirconium solution and the sulfating agent solution are brought into contact by opening both the valve 12 and the valve 32. The resulting mixture (basic zirconium sulfate-containing reaction solution) flows immediately from the bottom of the T-shaped tube 20 into the aging container 40. In step 2, this technique prevents the concentration of the reaction solution (the concentration of the reaction solution in the T-shaped tube 20) from changing between the start and end of contact between the zirconium solution and the sulfating agent solution. In step 2, the SO 4 2- / ZrO 2 Since the change in concentration of SO is suppressed, a uniform reaction product can be obtained. By adopting such a step (step 2), the peak top diameter, pore volume, and pore distribution width of the primary particles can be controlled. That is, the size of the pores originating from the gaps between primary particles in the secondary particles can be made small and the distribution can be made sharp, and further, the pore volume originating from the gaps between primary particles can also be made small. 4 2- / ZrO 2The weight ratio is preferably in the range of 0.3 to 0.8, more preferably 0.4 to 0.7, and even more preferably 0.45 to 0.65. 4 2- / ZrO 2 By setting the weight ratio to 0.3 or more, the yield of the reaction product, basic zirconium sulfate, can be increased. 4 2- / ZrO 2 By setting the weight ratio to 0.8 or less, it is possible to suppress the generation of soluble salts of zirconium sulfate and to suppress a decrease in the yield of basic zirconium sulfate. In step 2, in order to maintain the temperature of the mixed solution at 95° C. or higher, it is preferable to install a heater in the pipes (e.g., T-pipe 20) that supply each solution.

[0119] An example of step 2 will be specifically described below. A T-shaped tube 20 having a tube diameter L1 of 10 mm at one end (left side in FIG. 1 ), a tube diameter L2 of 10 mm at the other end (right side in FIG. 1 ), and a lower tube diameter L3 of 15 mm was used. 213 g of a 25% by mass aqueous solution of sodium sulfate and ZrO 2 When the aqueous solution of zirconium oxychloride is brought into contact with 450 g of a 16% by mass equivalent aqueous solution of zirconium oxychloride, the time (contact time) from the start of the contact to the end of the contact (until the aqueous zirconium chloride solution in vessel 10 and the sulfating agent solution in vessel 30 are exhausted) is preferably 30 to 300 seconds, more preferably 60 to 200 seconds, and even more preferably 90 to 150 seconds.

[0120] <Step 3> In step 3, the basic zirconium sulfate-containing reaction solution obtained in step 2 is aged at 95°C or higher for 3 hours or more. In step 3, for example, the basic zirconium sulfate-containing reaction solution flowing into the aging vessel 40 is aged at 95°C or higher for 3 hours or more while being stirred with the agitator 42. The upper limit of the aging time is not particularly limited, but is, for example, 7 hours or less. The temperature (aging temperature) of the mixed solution (basic zirconium sulfate-containing reaction solution) in step 3 is preferably 95°C or higher, more preferably 97°C or higher and 100°C or lower. By setting the aging temperature to 95°C or higher and the aging time to 3 hours or longer, basic zirconium sulfate can be sufficiently produced and the yield can be increased. The mixed solution contains basic zirconium sulfate as a main component and is a basic zirconium sulfate slurry.

[0121] <Step 4> In step 4, a stabilizer is added to the aged reaction liquid containing basic zirconium sulfate obtained in step 3.

[0122] <Step 5> In step 5, an alkali is added to the basic zirconium sulfate-containing reaction solution obtained in step 4 to carry out a neutralization reaction. Neutralization produces a zirconium-containing hydroxide. The alkali is not particularly limited, and examples include caustic soda, sodium carbonate, ammonia, and hydrazine ammonium bicarbonate. The alkali concentration is not particularly limited, but an alkali diluted with water is typically used at a concentration of 5 to 30%. There are two methods for adding the alkali: (1) adding an alkali solution to the basic zirconium sulfate-containing reaction solution; and (2) adding the basic zirconium sulfate-containing reaction solution to the alkali solution. Either method is not particularly limited, and either method may be used. After neutralization, the slurry is filtered to obtain a zirconium-containing hydroxide. If necessary, the zirconium-containing hydroxide is preferably washed with pure water or the like to remove impurities. After washing, drying or other procedures may be performed as needed.

[0123] <Step 6> In step 6, the zirconium-containing hydroxide obtained in step 5 is heat-treated (calcined) to oxidize the zirconium-containing hydroxide and obtain stabilized zirconia. The heat treatment temperature (calcination temperature) and heat treatment time (calcination time) of the zirconium-containing hydroxide are not particularly limited, but are usually performed at about 600 to 1050°C for 1 to 10 hours. The calcination temperature is more preferably 650°C or higher and 1000°C or lower, and even more preferably 700°C or higher and 980°C or lower. The calcination temperature is more preferably 2 to 6 hours, and even more preferably 2 to 4 hours. By setting the heat treatment temperature to 600°C or higher and 1200°C or lower, the specific surface area of ​​the obtained stabilized zirconia can be made within a suitable range (for example, 5 m 2 / g or more 60m 2 The heat treatment atmosphere is not particularly limited, but is usually carried out in air or an oxidizing atmosphere.

[0124] <Step 7> In step 7, the stabilized zirconia obtained in step 6 is mixed with silver oxide having an average particle size of 0.5 μm or less. During mixing, the stabilized zirconia powder and silver oxide may be slurried to homogenize them. This produces a silver-containing stabilized zirconia powder.

[0125] <Step 8> After step 7, the silver-containing stabilized zirconia powder obtained may be pulverized to form a slurry, if necessary. A binder may be added to improve moldability. If the slurry is not formed (pulverized), the binder and the silver-containing stabilized zirconia powder may be uniformly mixed in a kneader. An organic binder is preferred as the binder. Organic binders are easily removed from the molded body in a heating furnace under an oxidizing atmosphere, allowing a degreased body to be obtained, reducing the likelihood of impurities remaining in the final sintered body. Examples of the organic binder include those soluble in alcohol or in a mixture of two or more selected from the group consisting of alcohol, water, aliphatic ketones, and aromatic hydrocarbons. Examples of the organic binder include at least one selected from the group consisting of polyethylene glycol, glycol fatty acid ester, glycerin fatty acid ester, polyvinyl butyral, polyvinyl methyl ether, polyvinyl ethyl ether, and vinyl propionate. The organic binder may further include one or more thermoplastic resins insoluble in alcohol or the mixture. After the addition of the organic binder, the target silver-containing stabilized zirconia powder can be obtained by applying a known method to treatments such as drying and pulverization. 50 For example, the silver-containing stabilized zirconia powder obtained in step 5 may be pulverized depending on its state, and the particle diameter D of the silver-containing stabilized zirconia powder may be controlled. 50 can be controlled.

[0126] The silver-containing stabilized zirconia powder immediately after step 7 is a silver-containing stabilized zirconia powder containing stabilized zirconia and silver oxide, and usually does not contain silver. By heating after step 7, all or part of the silver oxide is decomposed to form silver. For example, by the heat generated during drying after step 7, all or part of the silver oxide is decomposed to form silver. Thus, according to the method for producing a silver-containing stabilized zirconia powder of this embodiment, (1) if heating is not performed after step 7, a silver-containing stabilized zirconia powder containing stabilized zirconia and silver oxide having an average particle size of 0.5 μm or less but not containing silver is obtained; (2) if heating is performed after step 7 to an extent that some of the silver oxide decomposes, a silver-containing stabilized zirconia powder containing stabilized zirconia, silver, and silver oxide having an average particle size of 0.5 μm or less is obtained; and (3) if heating is performed after step 7 to an extent that all of the silver oxide decomposes, a silver-containing stabilized zirconia powder containing stabilized zirconia and silver having an average particle size of 0.5 μm or less but not containing silver oxide is obtained.

[0127] When a sintering aid, a colorant, or the like is added, it is possible to obtain a silver-containing stabilized zirconia powder containing the sintering aid, the colorant, or the like by adding and mixing in the step 7. As a more detailed mixing method, it is preferable to disperse the sintering aid, the colorant, or the like in pure water to form a slurry and then wet mix the slurry. Furthermore, when the step 7 is performed, the sintering aid, the colorant, or the like may be added during the step 7.

[0128] The silver-containing stabilized zirconia powder according to this embodiment has been described above.

[0129] [Method for producing zirconia sintered body] An example of a method for producing a zirconia sintered body will be described below, however, the method for producing a zirconia sintered body of the present invention is not limited to the following example.

[0130] The method for producing a zirconia sintered body according to this embodiment includes: a step X of molding the silver-containing stabilized zirconia powder to obtain a molded body; and a step Y of sintering the molded body at a temperature of 1250°C or higher and 1500°C or lower for 1 hour or higher and 5 hours or lower, after the step X.

[0131] In the method for producing a zirconia sintered body according to this embodiment, first, a silver-containing stabilized zirconia powder is prepared. As the silver-containing stabilized zirconia powder, the powder described in the section [Silver-containing stabilized zirconia powder] can be used.

[0132] Next, the silver-containing stabilized zirconia powder is molded to obtain a molded body (Step X). For molding, a commercially available molded body or cold isostatic pressing (CIP) can be used. Alternatively, the silver-containing stabilized zirconia powder may be temporarily molded using a molded body and then finally molded by press molding. Press molding is usually performed at a pressure of 0.1 t to 3 t / cm. 2 Preferably, the range is 0.5t to 2.5t / cm 2 , more preferably 0.8t to 2.2t / cm 2 , more preferably 1t to 2t / cm 2 is.

[0133] Next, the molded body is sintered under conditions of 1250°C to 1500°C for 1 hour to 5 hours (Step Y). In this embodiment, because the silver-containing stabilized zirconia powder is used, the sintering temperature can be set low, at 1250 to 1500°C. The sintering temperature is more preferably 1300°C to 1450°C, and particularly preferably 1350°C to 1400°C. The holding time during sintering is also not particularly limited, but is preferably, for example, about 1 to 5 hours, more preferably 1 to 3 hours. The sintering atmosphere can be air or an oxidizing atmosphere. Sintering can be performed under normal pressure; pressurization is not particularly required. Note that if silver oxide remains in the silver-containing stabilized zirconia powder, all of the silver oxide will be thermally decomposed to silver by this sintering step (Step Y). Note that depending on the sintering conditions, some (e.g., a very small amount) silver oxide may remain.

[0134] As a result of the above, a silver-containing zirconia sintered body can be obtained which contains silver particles, zirconia, and a stabilizer, wherein the silver particles have an average particle size of 0.5 μm or less, the stabilized zirconia has an average crystal grain size of 0.35 μm or less, and has a relative sintered density of 98% or more.

[0135] The method for producing a zirconia sintered body according to this embodiment has been described above.

[0136] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. Note that the silver-containing stabilized zirconia powders and silver-containing zirconia sintered bodies in the examples and comparative examples contain 1 to 3 mass % of hafnium as an unavoidable impurity relative to zirconium (calculated using the following formula (X)). <Formula (X)> ([mass of hafnium oxide] / ([mass of zirconium oxide]+[mass of hafnium oxide]))×100(%)

[0137] The maximum and minimum values ​​of the content of each component shown in the following examples should be considered as the preferred minimum and maximum values ​​of the present invention, regardless of the content of other components. Also, the maximum and minimum values ​​of the measured values ​​shown in the following examples should be considered as the preferred minimum and maximum values ​​of the present invention, regardless of the content (composition) of each component.

[0138] [Preparation of Silver-Containing Stabilized Zirconia Powder] (Example 1) 213 g of a 25 mass % aqueous solution of sodium sulfate and ZrO 2 450 g of an aqueous solution of zirconium oxychloride (acid concentration: 1N) equivalent to 16% by mass was separately heated to 95°C (step 1). 4 2- / ZrO 2 The heated aqueous solutions were contacted with each other for 2 minutes so that the mass ratio was 0.50 (Step 2). Next, the obtained reaction solution containing basic zirconium sulfate was kept at 95°C for 4 hours for aging, and basic zirconium sulfate was obtained (Step 3). Next, the aged solution was cooled to room temperature, and then Y 2 O 3 A 10 mass % yttrium chloride aqueous solution was 2 O 3The resulting mixture was mixed uniformly to a concentration of 3.2 mol% (Step 4). Next, a 25% by mass aqueous solution of sodium hydroxide was added to the resulting mixed solution, neutralizing it to a pH of 13 or higher, thereby forming a hydroxide precipitate (Step 5). Specifically, the above procedure was performed using the apparatus described with reference to FIG. 1. The resulting hydroxide precipitate was filtered and thoroughly washed with water. The resulting hydroxide was heat-treated in air at 1000°C (the calcination temperature) for 4 hours to obtain unground stabilized zirconia (yttria-stabilized zirconia powder) (Step 6). Silver oxide powder (manufactured by Mitsuwa Chemical Co., Ltd., product name: silver(I) oxide, average particle size: 20 μm) was added to the resulting unground stabilized zirconia in an amount of 1% by mass relative to the stabilized zirconia. Furthermore, alumina powder with an average primary particle size of 0.1 μm was added in an amount of 0.5% by mass relative to the stabilized zirconia. The mixture was then ground and mixed in a wet ball mill using water as a dispersion medium for 40 hours (Step 7). Zirconia beads having a diameter of 5 mm were used for the pulverization. The zirconia slurry obtained after pulverization was dried at 110° C. to obtain the silver-containing stabilized zirconia powder described in Example 1.

[0139] (Examples 2 to 5) Silver-containing stabilized zirconia powders according to Examples 2 to 5 were obtained in the same manner as in Example 1, except that the amount of silver oxide added was changed as shown in Table 1, no alumina powder was added, and the firing temperature was changed to 850°C.

[0140] Example 6 A silver-containing stabilized zirconia powder according to Example 6 was obtained in the same manner as in Example 1, except that no alumina powder was added and the firing temperature was changed to 1150°C.

[0141] Example 7 A silver-containing stabilized zirconia powder according to Example 7 was obtained in the same manner as in Example 1, except that no alumina powder was added and the firing temperature was changed to 830°C.

[0142] Example 8 The same powder as the silver-containing stabilized zirconia powder of Example 3 was used as the silver-containing stabilized zirconia powder of Example 8.

[0143] (Examples 9-10) Y 2 O 3The silver-containing stabilized zirconia powders according to Examples 9 and 10 were obtained in the same manner as in Example 1, except that the amounts of the additives were changed as shown in Table 1 and the firing temperature was changed to 850°C.

[0144] Example 11 Instead of adding an aqueous solution of yttrium chloride, Er 2 O 3 A 10 mass % erbium chloride aqueous solution was prepared by converting 2 O 3 A silver-containing stabilized zirconia powder according to Example 11 was obtained in the same manner as in Example 1, except that the amount of Zn was 3.2 mol % and the firing temperature was changed to 850°C.

[0145] (Example 12) Instead of adding an aqueous solution of yttrium chloride, CeO 2 A 12% by mass aqueous solution of cerium chloride in terms of CeO 2 A silver-containing stabilized zirconia powder according to Example 12 was obtained in the same manner as in Example 1, except that the amount of the alumina powder added was changed to 0.25 mass %.

[0146] (Example 13) Y 2 O 3 A 10% by mass yttrium chloride aqueous solution was used as Y 2 O 3 Instead of adding yttrium chloride solution to make the amount of yttrium chloride 3.2 mol %, 2 O 3 was added so that the amount was 0.9 mol%, and calcium carbonate (CaCO 3 A silver-containing stabilized zirconia powder according to Example 13 was obtained in the same manner as in Example 1, except that 2.1 mol % of the alumina powder was added in terms of CaO, no alumina powder was added, and the firing temperature was changed to 950°C.

[0147] Example 14 A silver-containing stabilized zirconia powder according to Example 14 was obtained in the same manner as in Example 1, except that the amount of alumina powder added was changed to 20 mass % and the firing temperature was changed to 850°C.

[0148] Comparative Example 1: 213 g of a 25% by mass aqueous solution of sodium sulfate and ZrO 2450 g of an aqueous solution of zirconium oxychloride (acid concentration: 1N) equivalent to 16% by mass was separately heated to 95°C (step 1). 4 2- / ZrO 2 The heated aqueous solutions were contacted with each other for 2 minutes so that the mass ratio was 0.50 (Step 2). Next, the obtained reaction solution containing basic zirconium sulfate was kept at 95°C for 4 hours for aging, and basic zirconium sulfate was obtained (Step 3). Next, the aged solution was cooled to room temperature, and then Y 2 O 3 A 10 mass % yttrium chloride aqueous solution was 2 O 3 The resulting mixture was mixed uniformly to a concentration of 3.2 mol% (Step 4). Next, a 25% by mass aqueous solution of sodium hydroxide was added to the resulting mixed solution, neutralizing it to a pH of 13 or higher, thereby forming a hydroxide precipitate (Step 5). Specifically, the above procedure was performed using the apparatus described with reference to FIG. 1. The resulting hydroxide precipitate was filtered and thoroughly washed with water. The resulting hydroxide was heat-treated in air at 850°C (calcination temperature) for 4 hours to obtain unground stabilized zirconia (yttria-stabilized zirconia powder) (Step 6). Silver powder (manufactured by Mitsuwa Chemical Co., Ltd., product name: silver (particles), particle size: 2-4 μm) was added to the resulting unground stabilized zirconia in an amount of 1% by mass relative to the stabilized zirconia, and the mixture was ground and mixed in a wet ball mill using water as a dispersion medium for 40 hours (Step 7). Zirconia beads with a diameter of 5 mm were used for grinding. The zirconia slurry obtained after grinding was dried at 110°C to obtain the silver-containing stabilized zirconia powder of Example 1.

[0149] Comparative Example 2: 99% silver (powder) (up to 525 mesh) manufactured by Mitsuwa Chemical Co., Ltd. was heat-treated at 400°C for 2 hours. This coarsened the particle size. A silver-containing stabilized zirconia powder according to Comparative Example 2 was obtained in the same manner as in Example 3, except that the obtained silver powder was used.

[0150] [Measurement of composition of silver-containing stabilized zirconia powder] The compositions (oxide equivalent) of the silver-containing stabilized zirconia powders of the examples and comparative examples were analyzed using an ICP-AES ("ULTIMA-2" manufactured by HORIBA). The results are shown in Table 1.

[0151] [Measurement of particle size of silver particles and / or silver oxide particles in silver-containing stabilized zirconia powder] For the silver-containing stabilized zirconia powders of the Examples and Comparative Examples, COMPO images were obtained using an SEM "Phenom Pro-x" (manufactured by Phenom World). The Heywood diameter of the silver oxide particles or silver particles was measured using image analysis software "Image-Pro" (manufactured by Media Cybernetics). Specifically, the outline of the silver particle was manually surrounded (traced) on the image analysis software, the area of ​​the surrounded silver particle was measured, and the result was converted into a Heywood diameter. A total of 10 Heywood diameters were measured, and the average particle size was calculated. The results are shown in Table 1.

[0152] [Measurement of specific surface area of ​​silver-containing stabilized zirconia powder] The specific surface area of ​​the silver-containing stabilized zirconia powders of the examples and comparative examples was measured by the BET method using a specific surface area meter ("Macsorb" manufactured by Mountec). The results are shown in Table 1.

[0153] [Particle diameter D of silver-containing stabilized zirconia powder 50 0.15 g of the silver-containing stabilized zirconia powder of each of the Examples and Comparative Examples and 40 ml of a 0.2% aqueous solution of sodium hexametaphosphate were placed in a 50 ml beaker and dispersed for 5 minutes using an ultrasonic homogenizer "Sonifier S-450D" (Emerson Japan, Ltd.), and then the beaker was placed in an apparatus (a laser diffraction particle size distribution analyzer ("SALD-2300" manufactured by Shimadzu Corporation)) and measured. The results are shown in Table 1.

[0154] [Measurement of pore volume of silver-containing stabilized zirconia powder] For the zirconia powders of the examples and comparative examples, the pore size distribution was measured by mercury intrusion porosimetry using a pore size distribution measuring device ("Autopore IV9500" manufactured by Micromeritics). The measurement conditions were as follows. <Measurement conditions> Measuring device: pore size distribution measuring device (Autopore IV9500 manufactured by Micromeritics) Measurement range: 0.0036 to 10.3 μm Number of measurement points: 120 Mercury contact angle: 140 degrees Mercury surface tension: 480 dyne / cm

[0155] Using the obtained pore distribution, the peak top diameter, pore volume, and pore distribution width in the range of 10 nm to 0.5 μm were determined. The results are shown in Table 1. Here, the pore distribution width refers to the width of the peak where the log differential pore volume is 0.1 ml / g or more.

[0156] [Preparation of Zirconia Sintered Body] First, the zirconia powders of the examples and comparative examples were subjected to cold isostatic pressing (CIP) to obtain a molded body. The molding pressure was 2 t / cm. 2 The relative molded density of the molded body was determined as follows. The results are shown in Table 2. Next, the molded body was sintered for 2 hours at the "sintering temperature" shown in Table 2 to obtain a silver-containing zirconia sintered body. The silver-containing zirconia sintered body of Comparative Example 3 is a silver-containing zirconia sintered body obtained by sintering the silver-containing stabilized zirconia powder of Comparative Example 2 at a sintering temperature of 1550°C. When the silver particles are large, as in the silver-containing stabilized zirconia powder of Comparative Example 2, sintering at 1550°C is necessary for densification. However, it can be seen that the silver-containing zirconia sintered body of Comparative Example 3, obtained by sintering the silver-containing stabilized zirconia powder of Comparative Example 2 at a sintering temperature of 1550°C, has deteriorated hydrothermal degradation resistance due to the increased sintering temperature.

[0157] <Relative sintered density> The relative sintered density is expressed by the following formula (1): Relative sintered density (%)=(sintered density / theoretical sintered density)×100 (1) Here, the theoretical sintered density (ρ 0 ) is a value calculated by the following formula (2-1): 0= (100 + Y + Z) / [(100 / ρz) + (Y / 3.987) + (Z / 10.49)] ... (2-1) where Y is the alumina concentration (wt%) and Z is the silver concentration (wt%). When silver oxide is used as the raw material, the silver concentration (wt%) is calculated using formula (2-2). Z = [107.868 × silver oxide concentration (wt%)] / (231.736 × 2) ... (2-2) ρz is a value calculated using the following formula (2-3). ρz = [124.25 (100 - X) + [molecular weight of stabilizer] × X] / 150 [150.5 (100 + X)A 2 C] ... (2-3) Here, the molecular weight of the stabilizer is determined by the following formula: 2 O 3 In the case of 225.81, Er 2 O 3 382.52 in the case of Yb 2 O 3 In this case, 394.11 is used. X is the stabilizer concentration (mol %). A and C are values ​​calculated by the following formulas (2-4) and (2-5), respectively. A = 0.5080 + 0.06980X / (100 + X) ... (2-4) C = 0.5195 - 0.06180X / (100 + X) ... (2-5) In formula (1), the theoretical sintered density varies depending on the powder composition. For example, the theoretical sintered density of yttria-containing zirconia is 6.117 g / cm when the yttria content is 2 mol %. 3 , 3 mol% is 6.098 g / cm 3 , 5.5 mol% is 6.051 g / cm 3 (Al 2 O 3 = 0 wt %). 2 O 3 In this case, ρz is a value calculated by the following formula (3): ρz = -0.0402(Sc 2 O 3(molar concentration of CaO) + 6.1294 ... (3) When the stabilizer is CaO, ρz is a value calculated by the following formula (3-1): ρz = -0.0400 (molar concentration of CaO) + 6.1700 ... (3-1) When a colorant is included, the theoretical sintered density (denoted as ρ1) is: ρ1 = 100 / [(Z / V) + (100 - Z) / ρ0] ... (2-5) Furthermore, Z is the colorant concentration (wt %), V is the colorant theoretical density (g / cm 3 The theoretical density of the colorant is Fe 2 O 3 is 5.24 g / cm 3 , ZnO is 5.61 g / cm 3 , MnO 2 is 5.03 g / cm 3 , CoO is 6.10 g / cm 3 , Cr 2 O 3 is 5.22 g / cm 3 , TiO 2 is 4.23 g / cm 3 , Tb 4 O 7 is 7.80 g / cm 3 , CuO is 6.31 g / cm 3 , V 2 O 5 is 3.36 g / cm 3 The sintered density was measured by the Archimedes method.

[0158] <Relative Molded Density> Relative molded density (%) = (molded density / theoretical sintered density) × 100 (4) Here, the theoretical sintered density (ρ 0 ) is a value calculated by the above formula (2-1).

[0159] [Particle diameter of silver particles in silver-containing zirconia sintered body] The surfaces of the sintered bodies of the Examples and Comparative Examples were ground and polished to expose the silver-containing portions, and COMPO images were obtained using an SEM "Phenom Pro-x" (manufactured by Phenom World). The Heywood diameter of the silver particles was measured using image analysis software "Image-Pro" (manufactured by Media Cybernetics). Specifically, the outlines of the silver particles were manually surrounded (traced) on the image analysis software, the area of ​​the surrounded silver particles was measured, and this was converted into a Heywood diameter. A total of 100 Heywood diameters were measured, and the average particle diameter of the silver particles was calculated. The results are shown in Table 2.

[0160] [Average Crystal Grain Size of Stabilized Zirconia in Silver-Containing Zirconia Sintered Body] The crystal grain size of stabilized zirconia in the zirconia sintered bodies of the Examples and Comparative Examples was determined as follows. The results are shown in Table 2. SEM images of the sintered body samples obtained by scanning electron microscopy were obtained. Samples for SEM observation were prepared based on JIS R1633. The SEM images were prepared so that the number of stabilized zirconia crystal grains in one field of view was 150 or more. A rectangle of any size was drawn in the SEM image, and the number of particles present on the sides and diagonals of the rectangle was calculated. In the Examples and Comparative Examples, a magnification of 30,000x was used, and a rectangle measuring 3.497 μm × 2.375 μm was drawn. Each side of the rectangle was set to a length that covered at least 80% of the field of view. The average crystal grain size was calculated from the number of particles and the lengths of the four sides and diagonals of the rectangle. Specifically, the average crystal grain size was calculated using the following formula. (Average crystal grain size) = {[X / (x1 + x2)] + [Y / (y1 + y2)] + [D / (d1 + d2)]} × 2 / 3 In the formula, X, x1, x2, Y, y1, y2, D, d1, and d2 represent the following: X (μm): Length of the long side of the rectangle Y (μm): Length of the short side of the rectangle D (μm): Length of the diagonal of the rectangle x1 (particles): Number of particles on one long side x2 (particles): Number of particles on the other long side y1 (particles): Number of particles on one short side y2 (particles): Number of particles on the other short side d1 (particles): Number of particles on one diagonal d2 (particles): Number of particles on the other diagonal Similar operations were performed on three visual fields for each level, and the average crystal grain size of the three visual fields was taken as the final average crystal grain size. The results are shown in Table 2. Prior to the measurement, the sintered body samples were pretreated by mirror polishing and then thermal etching. The mirror polishing was carried out by grinding the surface of the sintered body with a surface grinder, and then polishing it with diamond abrasive grains having average grain sizes of 9 μm, 6 μm, and 3 μm in a mirror polishing machine.

[0161] [Monoclinic fraction of silver-containing zirconia sintered body after hydrothermal treatment at 134°C and 0.3 MPa for 15 hours] First, the silver-containing zirconia sintered body of each Example and Comparative Example obtained above was hydrothermally treated at 134°C and an absolute pressure of 0.3 MPa (in an aqueous atmosphere) for 15 hours. The monoclinic fraction contained in the crystalline phase of the silver-containing zirconia sintered body after hydrothermal treatment was then determined. The silver-containing zirconia sintered bodies of each Example and Comparative Example after hydrothermal treatment were mirror-polished to determine the monoclinic fraction contained in the crystalline phase. For mirror polishing, the surface of the sintered body was ground using a surface grinder, and then polished using diamond abrasive grains with average particle sizes of 9 μm, 6 μm, and 3 μm in a mirror polishing machine in that order. The results are shown in Table 2. Specifically, the monoclinic fraction of the silver-containing zirconia sintered body of each Example and Comparative Example was determined as described in the following [Crystalline Phase Identification].

[0162] [Identification of crystalline phase] An X-ray diffraction spectrum of the silver-containing zirconia sintered body was obtained using an X-ray diffractometer (RINT2500, manufactured by Rigaku). The measurement conditions were as follows. <Measurement conditions> Measurement device: X-ray diffractometer (RINT2500, manufactured by Rigaku) ​​Radiation source: CuKα radiation source Sampling interval: 0.02° Scan speed: 2θ=1.0° / min Divergence slit (DS): 1° Divergence vertical limiting slit: 5 mm Scattering slit (SS): 1° Receiving slit (RS): 0.3 mm Monochrome receiving slit: 0.8 mm Tube voltage: 50 kV Tube current: 300 mA Scan speed: 2θ=26 to 36°: 4° / min 2θ=72 to 76°: 1° / min

[0163] Thereafter, the crystalline phases were identified from the X-ray diffraction spectrum. The proportion of each crystalline phase contained in the silver-containing zirconia sintered body was calculated using the following formulas. Monoclinic phase proportion (%) = (Im(111) + Im(11-1)) / (Im(111) + Im(11-1) + It(101) + Ic(111)) × 100 Tetragonal phase proportion (%) = (100% - monoclinic phase (%)) × ((It(004) + It(220) / (It(004) + It(220) + Ic(004)) × 100 Cubic phase proportion (%) = (100% - monoclinic phase (%)) × ((Ic(004) / (It(004) + It(220) + Ic(004)) × 100 Here, Im(111) is the diffraction intensity of (111) in the monoclinic phase, Im(11-1) is the diffraction intensity of (11-1) in the monoclinic phase, It(101) is the diffraction intensity of (101) in the tetragonal phase, It(220) is the diffraction intensity of (220) in the tetragonal phase, and It(004) is the diffraction intensity of (004) in the tetragonal phase, Ic(004) is the diffraction intensity of (004) in the cubic phase, and Ic(111) is the diffraction intensity of (111) in the cubic phase. The monoclinic phase of zirconia was distinguished from the tetragonal and cubic phases at 2θ=26 to 36° in the XRD spectrum. The tetragonal and cubic phases were distinguished at 2θ=72 to 76° in the XRD spectrum. The cubic phase may be distorted depending on the amount of stabilizer added and the manufacturing method, and the peak position may shift. In this example, the peak between (004) and (220) of the tetragonal phase was considered to be the peak of the cubic phase, and calculations were performed.

[0164] [Toughness] The toughness of the silver-containing zirconia sintered bodies obtained above in the Examples and Comparative Examples was determined as follows. The toughness measurement by the IF method was performed under a load of 30 kgf (294.2 N) in accordance with JIS R1607 (Room Temperature Fracture Toughness (Toughness) Test Method for Fine Ceramics). Using a Vickers hardness tester, seven square indentations were selected and the toughness was determined. The toughness value was calculated by averaging the toughness values ​​of five of these, excluding the smallest and largest values. However, indentations where no cracks extended from the indentation were considered invalid, and only indentations where cracks extended from the tip of the square were used. Each toughness value was calculated using the following formula: Kc = 0.018 × Hv × a 0.5× [(c−a) / a] -0.5 × (Hv / E) -0.4 Kc, Hv, a, c, and E have the following meanings. The indentation length on the X and Y axes and the crack length on the X and Y axes when determining a and c are as shown in Figure 2. Kc: Toughness value [MPa m 0.5 ] Hv: Vickers hardness [GPa] a: Half the average value of the indentation length along the X and Y axes [μm] c: Half the average value of the crack length along the X and Y axes [μm] E: Young's modulus [GPa] The Vickers hardness was determined in accordance with JIS R 1610 (testing method for hardness of fine ceramics). The Vickers hardness was calculated using the following formula: Hv = 0.001854 × [F / d 2 Sv] F and d have the following meanings. The X-axis indentation length and Y-axis indentation length used to determine d are as shown in Figure 2. Hv: Vickers hardness [GPa] F: Test force [N] d: Average value of X-axis indentation length and Y-axis indentation length [mm] The Young's modulus used was 210 GPa, which is known as the value for general yttria-stabilized zirconia.

[0165] [Three-Point Bending Strength] The three-point bending strength of the silver-containing zirconia sintered bodies of the Examples and Comparative Examples obtained above was measured in accordance with the three-point bending strength standard of JIS R 1601. The results are shown in Table 2.

[0166]

[0167]

Claims

1. A silver-containing zirconia sintered body comprising silver particles and stabilized zirconia containing zirconia and a stabilizer, the silver particles having an average particle size of 0.5 μm or less, the stabilized zirconia having an average crystal grain size of 0.35 μm or less, and a relative sintered density of 98% or more.

2. The silver-containing zirconia sintered body according to claim 1, characterized in that the average crystal grain size of the stabilized zirconia is 0.25 μm or less.

3. When the total amount of zirconia and the stabilizer is 100 mass%, the silver particles are Ag 2 The silver-containing zirconia sintered body according to claim 1 or 2, characterized in that it contains, in terms of O, in a range of 0.025 mass% or more and 20 mass% or less.

4. The silver-containing zirconia sintered body according to claim 1 or 2, characterized in that it has a three-point bending strength of 600 MPa or more.

5. Toughness value by IF method is 5MPa・m 0.5 The silver-containing zirconia sintered body according to claim 1 or 2, characterized in that 6. A silver-containing zirconia sintered body according to claim 1 or 2, characterized in that the monoclinic ratio after hydrothermal treatment at 134°C, 0.3 MPa for 15 hours is 10% or less.

7. The stabilizer is Y 2 O 3 , CeO 2 , Er 2 O 3 3. The silver-containing zirconia sintered body according to claim 1, characterized in that the silver-containing zirconia sintered body is one or more selected from the group consisting of CaO.

8. A silver-containing zirconia sintered body as described in claim 1 or 2, characterized in that the content of the stabilizer is 15 mol % or less when the zirconia and stabilizer are taken as the whole.

9. A silver-containing stabilized zirconia powder comprising: stabilized zirconia containing zirconia and a stabilizer; and silver and / or silver oxide having an average particle size of 0.5 μm or less.

10. The silver-containing stabilized zirconia powder according to claim 9, characterized in that, in the range of 10 nm or more and 0.5 μm or less in the pore distribution based on mercury intrusion porosimetry, the peak top diameter of the pore volume distribution is 30 nm or more and 100 nm or less, the pore volume is 0.25 ml / g or more and 0.46 ml / g or less, and the pore distribution width is 40 nm or more and 120 nm or less.

11. A method for producing a silver-containing stabilized zirconia powder, comprising the step of mixing stabilized zirconia containing zirconia and a stabilizer with silver oxide having an average particle size of 0.5 μm or less.

12. A method for producing a silver-containing zirconia sintered body, comprising: a step X of molding the silver-containing stabilized zirconia powder according to claim 9 or 10 to obtain a molded body; and a step Y of sintering the molded body under conditions of 1250°C to 1500°C and 1 hour to 5 hours after step X.

Citation Information

Patent Citations

  • Method for preparing zirconia ceramic granulation powder

    CN105367056A

  • Antibacterial agent and its production

    JP1999228320A

  • Yellow coloring composite fine particle and method for producing the yellow coloring composite fine particle

    JP2007063530A

  • Osseointegrative surgical implant

    US20160015483A1

  • Implant with ceramic coating, method of forming an implant, and method of applying a ceramic coating

    WO2020049299A1

Cited By

  • Recycling methods for sintered bodies

    JP2026159615A

  • Dental workpiece and method for producing same

    WO2026141681A1

  • Method for recycling sintered object

    WO2026197190A1