Oxide sintered compact, sputtering target, oxide thin film, thin film transistor, and electronic device

By adding a positive trivalent X element to the oxide sintered body with specific atomic ratios, the issues of color unevenness and white spots are mitigated, resulting in improved sputtering stability and transistor mobility, addressing the performance limitations in existing oxide sintered bodies containing In, Ga, and Al elements.

WO2024203946A1PCT designated stage expired Publication Date: 2024-10-03IDEMITSU KOSAN CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011471
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Oxide sintered bodies containing In, Ga, and Al elements often exhibit color unevenness and white spots, leading to abnormal discharge during sputtering and reduced mobility in thin film transistors, which compromises in-plane uniformity and device performance.

Method used

Incorporating a positive trivalent X element such as Sc, Y, La, or Lu into the oxide sintered body, with specific atomic ratios of In, Ga, Al, and X, to form a bixbite crystal phase with defined diffraction peaks, which reduces color unevenness and white spots, and improves sputtering stability and thin film transistor mobility.

Benefits of technology

The inclusion of a positive trivalent X element in the oxide sintered body effectively minimizes color unevenness and white spots, enhancing the stability and mobility of thin film transistors and achieving high in-plane uniformity and low bulk resistance, thereby improving the performance of sputtering targets and thin film transistors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011471_03102024_PF_FP_ABST
    Figure JP2024011471_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an oxide sintered compact which contains, as main constituent elements, an In element, a Ga element, an Al element, and a predetermined X element comprising a positive trivalent element, wherein the atomic ratios of the In element, the Ga element, the Al element, and the X element satisfy formulae (1) to (3) ((1): 0.05 ≤ Ga / (In+Ga) ≤ 0.20, (2): 0.015 ≤ (Al+X) / (In+Ga+Al+X) ≤ 0.07, and (3): 0.10 ≤ Al / (Al+X) ≤ 0.90, wherein In, Ga, Al and X respectively represent the number of atoms of the In element, the Ga element, the Al element and the X element in the oxide sintered compact). The oxide sintered compact contains a bixbyite crystal phase represented by In2O3 and a crystal phase having diffraction peak in a incident angle (2θ) range observed by a predetermined X ray (Cu-Kα line) diffraction measurement.
Need to check novelty before this filing date? Find Prior Art

Description

Oxide sintered body, sputtering target, oxide thin film, thin film transistor, and electronic device

[0001] The present invention relates to an oxide sintered body, a sputtering target, an oxide thin film, a thin film transistor, and an electronic device.

[0002] Amorphous oxide semiconductors used in thin film transistors (hereinafter sometimes referred to as TFTs) have higher carrier mobility, a larger optical band gap, and can be deposited at low temperatures compared to general-purpose amorphous silicon (amorphous silicon may be abbreviated as a-Si). Therefore, amorphous oxide semiconductors are expected to be applied to next-generation displays that require large size, high resolution, and high-speed operation, as well as to resin substrates with low heat resistance. Furthermore, in recent years, research has been conducted into applying crystalline oxide semiconductors, rather than amorphous oxide semiconductors, to the channel layer of thin film transistors.

[0003] In forming the oxide semiconductor (thin film), a sputtering method in which a sputtering target is sputtered is preferably used because a thin film formed by the sputtering method has excellent in-plane uniformity of component composition in the film surface direction (within the film surface) and film thickness, etc., compared to a thin film formed by an ion plating method, a vacuum deposition method, or an electron beam deposition method, and has the same component composition as the sputtering target.

[0004] In Patent Document 1, 2 O 3 A bixbyite phase composed of 3 B 5 O 12 The document describes an oxide sintered body containing a ZnO phase (wherein A is one or more elements selected from the group consisting of Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, and B is one or more elements selected from the group consisting of Al and Ga).

[0005] Patent Document 2 describes a compound having the composition formula (In x Ga y Al z ) 2 O3 (wherein 0.47≦x≦0.53, 0.17≦y≦0.43, 0.07≦z≦0.33, and x+y+z=1), and has diffraction peaks in the ranges of incident angles (2θ) observed by X-ray (Cu-Kα ray) diffraction measurement specified in the following (A) to (K): (A): 31° to 34°, (B): 36° to 39°, (C): 30° to 32°, (D): 51° to 53°, (E): 53° to 56°, (F): 62° to 66°, (G): 9° to 11°, (H): 19° to 21°, (I): 42° to 45°, (J): 8° to 10°, and (K): 17° to 19°.

[0006] Patent Document 3 describes a compound formed from indium element (In), gallium element (Ga), aluminum element (Al), and oxygen element (O), having lattice constants of a = 10.07 ± 0.15 Å, b = 10.45 ± 0.15 Å, c = 11.01 ± 0.15 Å, α = 111.70 ± 0.50°, β = 107.70 ± 0.50°, and γ = 90.00 ± 0.50°, and exhibiting a triclinic crystal system.

[0007] International Publication No. 2015 / 098060 International Publication No. 2020 / 027243 International Publication No. 2020 / 027244

[0008] For example, in a target using an oxide sintered body containing In (indium), Ga (gallium), Al (aluminum), and O (oxygen), color unevenness occurs in the oxide sintered body of the target, and white spots that appear white are generated due to the accumulation of small pores on the surface of the oxide sintered body. The presence of color unevenness and white spots in the sintered body of the target makes abnormal discharge more likely to occur during the sputtering process.

[0009] Furthermore, when an oxide thin film is formed using a target including an oxide sintered body having color unevenness and white spots and a TFT element including the oxide thin film is fabricated, the color unevenness and white spots present in the sintered body of the target cause a decrease in mobility. Furthermore, the color unevenness and white spots present in the sintered body of the target cause a decrease in the in-plane uniformity of the TFT element characteristics. For this reason, further improvement has been required for targets using oxide sintered bodies containing In, Ga, Al, and O elements.

[0010] An object of the present invention is to provide an oxide sintered body in which the occurrence of color unevenness and the occurrence of white spots are reduced, a sputtering target including the oxide sintered body, an oxide thin film using the sputtering target, a thin film transistor including the oxide thin film, and an electronic device including the thin film transistor.

[0011] [1] A composition comprising, as main constituent elements, In (indium), Ga (gallium), Al (aluminum), and a positive trivalent X element, wherein the X element is one or more elements selected from the group consisting of Sc (scandium), Y (yttrium), La (lanthanum), Pr (praseodymium), Nd (neodymium), Pm (promethium), Sm (samarium), Eu (europium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium), Yb (ytterbium), and Lu (lutetium), and wherein the atomic ratios of the In element, the Ga element, the Al element, and the X element satisfy the following formulas (1) to (3): 2 O 3and a crystalline phase having a diffraction peak in a range of incident angles (2θ) observed by X-ray (Cu-Kα ray) diffraction measurement specified in the following (A) to (K): 31° to 34°...(A) 36° to 39°...(B) 30° to 32°...(C) 51° to 53°...(D) 53° to 56°...(E) 62° to 66°...(F) 14° to 16°...(G) 19° to 21°...(H) 42° to 45°...(I) 8° to 10°...(J) 17° to 19°...(K) 0.05≦Ga / (In+Ga)≦0.20...(1) 0.015≦(Al+X) / (In+Ga+Al+X)≦0.07...(2) 0.10≦Al / (Al+X)≦0.90 (3) (In the formula, In, Ga, Al, and X represent the number of atoms of indium element, gallium element, aluminum element, and X element in the oxide sintered body, respectively.)

[0012] [2] The oxide sintered body according to [1], wherein 99 atomic % or more of the metal elements contained in the oxide sintered body are the In element, the Ga element, the Al element, and the X element.

[0013] [3] The oxide sintered body according to [1] or [2], wherein the atomic ratio represented by the formula (1) is 0.05 or more and 0.18 or less.

[0014] [4] The oxide sintered body according to any one of [1] to [3], wherein the atomic ratio represented by the formula (1) is 0.05 or more and 0.16 or less.

[0015] [5] The oxide sintered body according to any one of [1] to [4], wherein the atomic ratio represented by the formula (1) is 0.08 or more and 0.10 or less.

[0016] [6] The oxide sintered body according to any one of [1] to [5], wherein the atomic ratio represented by the formula (2) is 0.02 or more and 0.07 or less.

[0017] [7] The oxide sintered body according to any one of [1] to [6], wherein the atomic ratio represented by the formula (2) is 0.02 or more and 0.06 or less.

[0018] [8] The oxide sintered body according to any one of [1] to [7], wherein the atomic ratio represented by the formula (2) is 0.02 or more and 0.05 or less.

[0019] [9] The oxide sintered body according to any one of [1] to [8], wherein the atomic ratio represented by the formula (3) is 0.20 or more and 0.90 or less.

[0020]

[10] The oxide sintered body according to any one of [1] to [9], wherein the atomic ratio represented by the formula (3) is 0.30 or more and 0.60 or less.

[0021]

[11] The oxide sintered body according to any one of [1] to

[10] , having a bulk resistance of 10 mΩ cm or less.

[0022]

[12] A sputtering target comprising the oxide sintered body according to any one of [1] to

[11] .

[0023]

[13] An oxide thin film formed using the sputtering target according to

[12] .

[0024]

[14] A thin film transistor comprising the oxide thin film according to

[13] .

[0025]

[15] An electronic device comprising the thin film transistor according to

[14] .

[0026] According to one aspect of the present invention, it is possible to provide an oxide sintered body in which the occurrence of color unevenness and the occurrence of white spots are reduced, a sputtering target including the oxide sintered body, an oxide thin film using the sputtering target, a thin film transistor including the oxide thin film, and an electronic device including the thin film transistor.

[0027] 2A is a perspective view showing the shape of a target according to one embodiment of the present invention; FIG. 2B is a perspective view showing the shape of a target according to one embodiment of the present invention; FIG. 2C is a perspective view showing the shape of a target according to one embodiment of the present invention; FIG. 2D is a longitudinal sectional view showing a state in which an oxide semiconductor thin film is formed on a glass substrate; and FIG. 2E is a perspective view showing a state in which an oxide semiconductor thin film is formed on the oxide semiconductor thin film of 21 is a longitudinal sectional view showing a state in which a film has been formed. FIG. 2 is a longitudinal sectional view showing a thin film transistor according to an embodiment of the present invention. FIG. 3 is a longitudinal sectional view showing a thin film transistor according to an embodiment of the present invention. FIG. 4 is a longitudinal sectional view showing a thin film transistor according to an embodiment of the present invention. FIG. 5 is a longitudinal sectional view showing a quantum tunnel field effect transistor according to an embodiment of the present invention. FIG. 6 is a longitudinal sectional view showing another embodiment of a quantum tunnel field effect transistor. FIG. 7 is a longitudinal sectional view showing a manufacturing procedure for a quantum tunnel field effect transistor. FIG. 8 is a longitudinal sectional view showing a manufacturing procedure for a quantum tunnel field effect transistor. FIG. 9 is a longitudinal sectional view showing a manufacturing procedure for a quantum tunnel field effect transistor. FIG. 10 is a longitudinal sectional view showing a manufacturing procedure for a quantum tunnel field effect transistor. FIG. 11 is a longitudinal sectional view showing a manufacturing procedure for a quantum tunnel field effect transistor. FIG. 12 is a top view showing a display device using a thin film transistor according to an embodiment of the present invention. FIG. 13 is a diagram showing a circuit of a pixel portion that can be applied to pixels of a VA-type liquid crystal display device. FIG. 14 is a diagram showing a circuit of a pixel portion of a display device using an organic EL element. FIG. 15 is a diagram showing a circuit of a pixel portion of a solid-state imaging element using a thin film transistor according to an embodiment of the present invention. FIG. 16 is an XRD chart of an oxide sintered body according to an embodiment of the present invention. FIG. 17 is an XRD chart of an oxide sintered body according to Example 1. FIG. 18 is an XRD chart of an oxide sintered body according to Example 3. FIG. 19 is an XRD chart of an oxide sintered body according to Example 5. 10 is an XRD chart of an oxide sintered body according to Example 11. FIG. 11 is an XRD chart of an oxide sintered body according to Example 13.

[0028] Hereinafter, embodiments will be described with reference to the drawings, etc. However, it will be readily understood by those skilled in the art that the embodiments can be implemented in many different ways and that various changes in form and details can be made without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the following description of the embodiments.

[0029] In the drawings, sizes, layer thicknesses, regions, etc. may be exaggerated for clarity. Therefore, the present invention is not limited to the illustrated sizes, layer thicknesses, regions, etc. Note that the drawings are schematic illustrations of ideal examples, and the present invention is not limited to the shapes, values, etc. shown in the drawings.

[0030] The ordinal numbers "first," "second," and "third" used in this specification are used to avoid confusion between components, and components that are not specified numerically are not limited in number.

[0031] In this specification and the like, the terms "film" or "thin film" and the term "layer" can be used interchangeably in some cases.

[0032] In the sintered body and oxide thin film of this specification and the like, the terms "compound" and "crystalline phase" can be interchangeable in some cases.

[0033] In this specification, the “oxide sintered body” may be simply referred to as the “sintered body.” In this specification, the “sputtering target” may be simply referred to as the “target.”

[0034] In this specification, "electrically connected" includes connection via "something that has some kind of electrical function." Here, "something that has some kind of electrical function" is not particularly limited as long as it allows electrical signals to be transmitted and received between the connected objects. For example, "something that has some kind of electrical function" includes electrodes, wiring, switching elements (such as transistors), resistive elements, inductors, capacitors, and other elements with various functions.

[0035] In this specification, the functions of the source and drain of a transistor may be interchanged when transistors of different polarities are used or when the direction of current flow changes during circuit operation, etc. Therefore, in this specification, the terms source and drain may be used interchangeably.

[0036] In this specification, a numerical range expressed using "to" means a range that includes the numerical value written before "to" as the lower limit and the numerical value written after "to" as the upper limit.

[0037] The present inventors have invented the present invention based on the following findings. The present inventors have found that in an oxide sintered body containing the metal elements In, Ga, and Al, the inclusion of a positive trivalent X element can reduce the occurrence of color unevenness in the target and the occurrence of white spots. Furthermore, when a positive trivalent X element is included, the inventors have found that the occurrence of color unevenness in the target and the occurrence of white spots can be reduced by examining the atomic ratio of "the total of the Al element and the positive trivalent X element" to "the total of the In element, the Ga element, the Al element, and the positive trivalent X element," the atomic ratio of "the Al element" to "the total of the Al element and the positive trivalent X element," and the atomic ratio of "the Ga element" to "the total of the In element and the Ga element." Furthermore, when the sintered body contains In 2 O 3 It has been found that the occurrence of color unevenness in the target can be reduced and the occurrence of white spots can be reduced by including a crystalline phase having a specific diffraction peak described later in addition to the bixbyite crystalline phase represented by the formula (1). Here, in this specification, the term "X element having a positive trivalent atom" means an X element exhibiting a positive trivalent atomic valence.

[0038] [Oxide Sintered Body] The oxide sintered body according to this embodiment contains In, Ga, Al, and a positive trivalent X element as main constituent elements. The X element is at least one element selected from the group consisting of Sc (scandium), Y (yttrium), La (lanthanum), Pr (praseodymium), Nd (neodymium), Pm (promethium), Sm (samarium), Eu (europium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium), Yb (ytterbium), and Lu (lutetium). The oxide sintered body according to this embodiment has an atomic ratio of the In element, the Ga element, the Al element, and the X element that satisfies the following formulas (1) to (3), and the In2 O 3 and a crystalline phase having a diffraction peak in the range of incident angles (2θ) observed by X-ray (Cu-Kα ray) diffraction measurement specified in the following (A) to (K). 31° to 34°...(A) 36° to 39°...(B) 30° to 32°...(C) 51° to 53°...(D) 53° to 56°...(E) 62° to 66°...(F) 14° to 16°...(G) 19° to 21°...(H) 42° to 45°...(I) 8° to 10°...(J) 17° to 19°...(K) 0.05≦Ga / (In+Ga)≦0.20...(1) 0.015≦(Al+X) / (In+Ga+Al+X)≦0.07...(2) 0.10≦Al / (Al+X)≦0.90 (3) (In the formula, In, Ga, Al, and X represent the number of atoms of indium element, gallium element, aluminum element, and X element in the oxide sintered body, respectively.)

[0039] The oxide sintered body according to this embodiment may consist essentially of only In, Ga, Al, a positive trivalent X, and O (oxygen). Here, "substantially" means that the oxide sintered body according to this embodiment may contain other components as long as the effects of the present invention resulting from the combination of In, Ga, Al, a positive trivalent X, and O (oxygen) are achieved. In this case, the oxide sintered body according to this embodiment may contain impurity elements. At least 99 atomic % of the elements contained in the oxide sintered body may be In, Ga, Al, a positive trivalent X, and O, or at least 99.9 atomic % of the elements contained in the oxide sintered body may be In, Ga, Al, a positive trivalent X, and O. Furthermore, the oxide sintered body according to this embodiment contains In, Ga, Al, and a positive trivalent X as the main constituent elements as metal elements. 99 atomic % or more of the metal elements contained in the oxide sintered body may be In, Ga, Al, and a positive trivalent X element, or 99.9 atomic % or more of the metal elements contained in the oxide sintered body may be In, Ga, Al, and a positive trivalent X element. In the oxide sintered body according to this embodiment, the metal elements contained in the oxide sintered body may consist essentially of only In, Ga, Al, and a positive trivalent X element. In this specification, atomic % may be expressed as at %.

[0040] Impurities refer to elements that are not intentionally added but are mixed into at least one of the raw materials and the manufacturing process. That is, impurities are inevitable impurities that are inevitably included. The same applies to the following explanation. Examples of impurities include at least one element selected from the group consisting of alkali metal elements (elements such as Li (lithium), Na (sodium), K (potassium), and Rb (rubidium)), alkaline earth metal elements (elements such as Mg (magnesium), Ca (calcium), Sr (strontium), and Ba (barium)), H (hydrogen), B (boron), C (carbon), N (nitrogen), F (fluorine), Si (silicon), and Cl (chlorine).

[0041] <Measurement of Impurity Concentration (H, C, N, F, Si, and Cl)> The impurity concentration (H, C, N, F, Si, and Cl) in the obtained oxide sintered body can be quantitatively evaluated using a sector-type dynamic secondary ion mass spectrometer SIMS analysis (IMS 7f-Auto, manufactured by AMETEK CAMECA). Specifically, first, primary ions Cs + Using a 14.5 kV accelerating voltage, sputtering is performed from the surface of the oxide sintered body to a depth of 20 μm. Thereafter, the mass spectrum intensity of impurities (H, C, N, F, Si, and Cl) is integrated while sputtering with primary ions over a raster of 100 μm, a measurement area of ​​30 μm, and a depth of 1 μm.

[0042] Furthermore, in order to calculate the absolute value of the impurity concentration from the mass spectrum, each impurity is injected into the sintered body by controlling the dose amount through ion implantation to prepare a standard sample with a known impurity concentration. The mass spectrum intensity of the impurities (H, C, N, F, Si, and Cl) is obtained by SIMS analysis of the standard sample, and the relationship between the absolute value of the impurity concentration and the mass spectrum intensity is made into a calibration curve. Finally, the mass spectrum intensity of the oxide sintered body to be measured and the calibration curve are used to calculate the impurity concentration of the measurement target, which is then expressed as the absolute value of the impurity concentration (atom cm -3 )

[0043] <Measurement of Impurity Concentration (B and Na)> The impurity concentration (B and Na) of the obtained oxide sintered body can also be quantitatively evaluated using SIMS analysis (IMS 7f-Auto, manufactured by AMETEK CAMECA). 2 + The absolute value of the impurity concentration (atom cm) of the measurement target was determined by the same evaluation as for the measurements of H, C, N, F, Si, and Cl, except that the acceleration voltage of the primary ions was 5.5 kV and the mass spectrum intensity of each impurity was measured. -3 ) can be obtained.

[0044] The positive trivalent X element contained in the oxide sintered body according to this embodiment is one or more elements selected from the group consisting of Sc, Y, La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. Among these, the positive trivalent X element is preferably one or more elements selected from the group consisting of Y, La, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu.

[0045] In the sintered body according to this embodiment, the atomic ratios of In, Ga, Al, and the positive trivalent X element satisfy all of the following formulas (1) to (3): 0.05≦Ga / (In+Ga)≦0.20 (1) 0.015≦(Al+X) / (In+Ga+Al+X)≦0.07 (2) 0.10≦Al / (Al+X)≦0.90 (3) (where In, Ga, Al, and X represent the number of atoms of indium, gallium, aluminum, and the positive trivalent X element in the oxide sintered body, respectively.)

[0046] When the atomic ratio represented by the formula (1) is 0.05 or more, a crystalline phase having a diffraction peak within the range of incident angles (2θ) observed by X-ray (Cu-Kα ray) diffraction measurement defined in the above (A) to (K) is more likely to be generated, thereby improving the effect of reducing the occurrence of color unevenness and the effect of reducing white spots in the target. On the other hand, when the atomic ratio represented by the formula (1) is 0.20 or less, a crystalline oxide thin film is more likely to be obtained when an oxide thin film formed using a sputtering target including the sintered body according to this embodiment is annealed, and a high-mobility TFT device is obtained. From this perspective, the atomic ratio represented by the formula (1) is preferably 0.05 or more and 0.18 or less, more preferably 0.05 or more and 0.16 or less, and even more preferably 0.08 or more and 0.10 or less.

[0047] When the atomic ratio represented by the formula (2) is 0.015 or more, the effect of reducing the occurrence of color unevenness in the target and the effect of reducing white spots are improved, allowing for stable sputtering. Furthermore, the in-plane variation of a TFT element including an oxide thin film formed using a sputtering target including the sintered body according to this embodiment is suppressed. On the other hand, when the atomic ratio represented by the formula (2) is 0.07 or less, an increase in the resistance value of the sintered body is suppressed, abnormal discharge is less likely to occur, and a TFT element with high mobility can be obtained. From this perspective, the atomic ratio represented by the formula (2) is preferably 0.02 or more and 0.07 or less, more preferably 0.02 or more and 0.06 or less, and even more preferably 0.02 or more and 0.05 or less.

[0048] When the atomic ratio represented by the formula (3) is 0.10 or more and 0.90 or less, the effect of reducing the occurrence of color unevenness in the target and the effect of reducing white spots are improved, and stable sputtering is possible. From this viewpoint, the atomic ratio represented by the formula (3) is preferably 0.20 or more and 0.90 or less, and more preferably 0.30 or more and 0.60 or less.

[0049] In the sintered body according to this embodiment, the atomic ratio of In, Ga, Al, and the positive trivalent X element preferably satisfies all of the above formulas (1) to (3) and also satisfies the following formula (4): 0.01≦Al / (In+Ga+Al+X)≦0.05 (4) (where In, Ga, Al, and X represent the number of atoms of indium, gallium, aluminum, and the positive trivalent X element in the oxide sintered body, respectively.)

[0050] When the atomic ratio represented by the formula (4) is 0.01 or more, a crystalline phase having a diffraction peak within the range of incident angles (2θ) observed by X-ray (Cu-Kα ray) diffraction measurement defined in the above (A) to (K) is easily generated. Furthermore, when the atomic ratio represented by the formula (4) is 0.01 or more and 0.05 or less, stable sputtering is easily achieved. Furthermore, when the atomic ratio represented by the formula (4) is 0.01 or more and 0.05 or less, in-plane variations in a TFT element including an oxide thin film formed using a sputtering target including the sintered body according to this embodiment are easily suppressed.

[0051] The content (atomic ratio) of each metal element in the sintered body according to this embodiment can be measured by an inductively coupled plasma atomic emission spectrometer (ICP-AES).

[0052] The sintered body according to this embodiment is made of In 2 O 3 and a crystalline phase having diffraction peaks in the ranges of incident angles (2θ) observed by X-ray (Cu-Kα ray) diffraction measurement specified in the following (A) to (K): 31° to 34° (A), 36° to 39° (B), 30° to 32° (C), 51° to 53° (D), 53° to 56° (E), 62° to 66° (F), 14° to 16° (G), 19° to 21° (H), 42° to 45° (I), 8° to 10° (J), and 17° to 19° (K).

[0053] In the sintered body according to this embodiment, In 2 O 3 The bixbyite crystal phase represented by the formula (I) may contain at least one element selected from the group consisting of Ga element, Al element, and X element having a positive trivalent atom. 2 O 3 The bixbyite crystal phase represented by the formula (I) contains at least one element selected from the group consisting of Ga, Al, and a positive trivalent X element, and examples of such a solid solution include substitutional solid solution and interstitial solid solution. 2 O 3In the bixbyite crystal phase represented by the formula (I), at least one element selected from Ga element, Al element, and X element having a positive trivalent is preferably dissolved in solid solution.

[0054] It can be confirmed by X-ray diffraction (XRD) measurement that the sintered body according to this embodiment contains a crystalline phase having a diffraction peak within the range of the incident angle (2θ) defined in (A) to (K). The criteria for determining whether a sintered body has a diffraction peak by X-ray diffraction (XRD) measurement are as follows:

[0055] <X-ray diffraction (XRD) measurement conditions> Scanning mode: 2θ / θ Scanning type: continuous scan X-ray intensity: 45 kV / 200 mA Entrance slit: 1.000 mm Receiving slit 1: 1.000 mm Receiving slit 2: 1.000 mm IS length: 10.0 mm Step width: 0.02° Speed ​​counting time: 2.0° / min The XRD pattern obtained under the above measurement conditions using SmartLab (Rigaku Corporation) was analyzed for peaks using JADE6's "Peak Search and Labeling" function, with the threshold σ set to 2.1, the cutoff peak intensity set to 0.19%, the background determination range set to 0.5, and the number of background averaging points set to 7. The peak positions were defined using the centroid method.

[0056] In the sintered body according to this embodiment, the crystalline phases having a diffraction peak within the range of the incident angle (2θ) defined in (A) to (K) each independently have a diffraction peak within the range of the incident angle (2θ) defined in (A) to (K). For example, when the peak within the range defined in (A) has a diffraction peak at 31°, the diffraction peak within the range defined in (C) has a diffraction peak at an incident angle (2θ) lower than 31°, and when the peak within the range defined in (E) has a diffraction peak at 53°, the diffraction peak within the range defined in (D) has a diffraction peak at an incident angle (2θ) lower than 53°.

[0057] When analyzed by JADE6, the crystalline phase having a diffraction peak within the range of incident angles (2θ) defined in (A) to (K) was found to be a compound with an unknown crystal structure, not matching any known compound. The crystalline phase having a diffraction peak within the range of incident angles (2θ) defined in (A) to (K) is a novel compound. For example, FIG. 12A shows an X-ray diffraction pattern of a sintered body according to one embodiment of the present invention. As shown in FIG. 12A, the sintered body used in the target according to one embodiment of the present invention contains a crystalline phase having a diffraction peak within the range of incident angles (2θ) defined in (A) to (K).

[0058] The sintered body according to this embodiment is made of In 2 O 3 As a main component (main phase), it is preferable that the sintered body contains a bixbyite crystalline phase represented by the formula (I) and contains, as a subcomponent (subphase), a crystalline phase having a diffraction peak in the range of incident angle (2θ) observed by X-ray (Cu-Kα ray) diffraction measurement specified in (A) to (K). 2 O 3 It is preferable that the bixbyite crystalline phase represented by the formula (I) is contained in a larger amount than the crystalline phase having a diffraction peak in the range of incident angles (2θ) observed by X-ray (Cu-Kα ray) diffraction measurement specified in (A) to (K) above.

[0059] The bulk resistance of the sintered body according to this embodiment is preferably 10 mΩ cm or less. If the bulk resistance of the sintered body is 10 mΩ cm or less, the sintered body has a sufficiently low resistance, and the sintered body according to this embodiment can be more suitably used as a sputtering target. If the bulk resistance of the sintered body is low, the resistance of the resulting target will be low, and stable plasma will be generated. Furthermore, if the bulk resistance of the sintered body is low, arc discharge, also known as fireball discharge, will be less likely to occur, and melting of the target surface and cracking of the target can be suppressed. The bulk resistance can be measured by the method described in the examples.

[0060] [Method for manufacturing sintered body] The oxide sintered body according to this embodiment can be manufactured by mixing raw material powders, molding, and sintering. Examples of raw materials include indium compounds, gallium compounds, aluminum compounds, and compounds of a positive trivalent X element, and oxides of these compounds are preferred. That is, indium oxide (In 2 O 3 ), gallium oxide (Ga 2 O 3 ), aluminum oxide (Al 2 O 3 ) and an oxide of a positive trivalent X element.

[0061] The indium oxide powder is not particularly limited, and commercially available indium oxide powder can be used. The indium oxide powder preferably has a high purity, for example, 4N (0.9999) or higher. Indium compounds may be indium salts such as chlorides, nitrates, or acetates, in addition to oxides.

[0062] The gallium oxide powder is not particularly limited, and commercially available gallium oxide powder can be used. The gallium oxide powder is preferably high purity, for example, 4N (0.9999) or higher. In addition, as the gallium compound, not only oxides but also gallium salts such as chlorides, nitrates, or acetates can be used.

[0063] The aluminum oxide powder is not particularly limited, and commercially available aluminum oxide powders can be used. The aluminum oxide powder preferably has a high purity, for example, 4N (0.9999) or higher. Furthermore, the aluminum compound may be not only an oxide but also an aluminum salt such as a chloride, a nitrate, or an acetate.

[0064] The raw material powder of the compound of the positive trivalent X element is not particularly limited, and at least one raw material powder selected from the group consisting of scandium oxide, yttrium oxide, lanthanum oxide, praseodymium oxide, neodymium oxide, promethium oxide, samarium oxide, europium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, holmium oxide, erbium oxide, thulium oxide, ytterbium oxide, and lutetium oxide can be used, which are commercially available industrially. The raw material powder of the compound of the positive trivalent X element preferably has a high purity, for example, 4N (0.9999) or higher. Furthermore, the compound of the positive trivalent X element may be not only an oxide but also a chloride, nitrate, acetate, or the like.

[0065] The raw material powders used may be mixed by wet mixing or dry mixing, and a mixing method in which wet mixing is performed after dry mixing is preferred.

[0066] The mixing step is not particularly limited, and can be carried out by mixing and grinding the raw material powders once or twice or more times. As the mixing and grinding means, known devices such as a ball mill, a bead mill, a jet mill, or an ultrasonic device can be used. As the mixing and grinding means, wet mixing using a bead mill is preferred.

[0067] The raw materials prepared in the above mixing step are molded by a known method to obtain a molded body, and this molded body is sintered to obtain an oxide sintered body. In the molding step, the mixed powder obtained in the mixing step is molded, for example, by pressure molding to obtain a molded body. This process molds the powder into the shape of the product (for example, a shape suitable for a sputtering target). Examples of molding processes include mold molding, slip casting, and injection molding. In order to obtain a sintered body with a high sintered density, it is preferable to use cold isostatic pressing (CIP) or the like for the molding process. A molding aid may be used during the molding process. Examples of molding aids include polyvinyl alcohol, methyl cellulose, polywax, and oleic acid.

[0068] In the sintering step, the compact obtained in the molding step is fired. Sintering conditions are atmospheric pressure, an oxygen gas atmosphere, or pressurized oxygen gas, typically at 1200°C to 1550°C for 30 minutes to 360 hours, preferably 8 hours to 180 hours, and more preferably 12 hours to 96 hours. If the sintering temperature is less than 1200°C, it may be difficult to increase the target density or the sintering time may be too long. On the other hand, if the sintering temperature exceeds 1550°C, the vaporization of components may cause compositional deviation or damage to the furnace. A sintering time of 30 minutes or more makes it easier to increase the target density. Sintering times longer than 360 hours are not practically feasible due to the excessive manufacturing time and high costs. A sintering time within the above range makes it easier to improve the relative density and reduce the bulk resistance.

[0069] According to the oxide sintered body of this embodiment, the atomic ratio of the In element, the Ga element, the Al element, and the X element having a positive trivalent valence satisfies all of the formulas (1) to (3), and In 2 O 3 and a crystalline phase having a diffraction peak within the range of the incident angle (2θ) defined in (A) to (K). Therefore, stable sputtering can be achieved by using a sputtering target including the oxide sintered body. Furthermore, a TFT having an oxide thin film obtained by sputtering a sputtering target including the oxide sintered body can be achieved, which has high mobility and excellent in-plane uniformity.

[0070] [Sputtering Target] The sputtering target according to this embodiment can be obtained by using the oxide sintered body according to this embodiment. That is, the sputtering target according to this embodiment includes the oxide sintered body according to this embodiment.

[0071] For example, the sputtering target according to this embodiment can be obtained by cutting and polishing an oxide sintered body and bonding it to a backing plate. The bonding rate between the sintered body and the backing plate is preferably 95% or more. The bonding rate can be confirmed by X-ray CT.

[0072] In one aspect, the sputtering target according to this embodiment includes the oxide sintered body according to this embodiment and a backing plate. In one aspect, the sputtering target according to this embodiment may be a target consisting only of the oxide sintered body. The sputtering target according to this embodiment preferably includes the oxide sintered body according to this embodiment and a cooling and holding member such as a backing plate that is provided on the sintered body as needed. The oxide sintered body (target material) constituting the sputtering target according to this embodiment is obtained by grinding the oxide sintered body according to this embodiment. Therefore, the target material is the same as the oxide sintered body according to this embodiment in terms of substance. Therefore, the description of the oxide sintered body according to this embodiment also applies to the target material.

[0073] 1A to 1D show perspective views showing the shape of a sputtering target. The sputtering target may be plate-shaped as shown by reference numeral 1 in FIG. 1A. The sputtering target may be cylindrical as shown by reference numeral 1A in FIG. 1B. When the sputtering target is plate-shaped, the planar shape may be rectangular as shown by reference numeral 1 in FIG. 1A, or circular as shown by reference numeral 1B in FIG. 1C. The oxide sintered body may be integrally molded, or may be a multi-piece type in which multiple divided oxide sintered bodies (reference numeral 1C) are each fixed to a backing plate 3 as shown in FIG. 1D. The backing plate 3 is a member for holding and cooling the oxide sintered body. It is preferable that the material be a material with excellent thermal conductivity, such as copper. The shape of the oxide sintered body constituting the sputtering target is not limited to the shapes shown in FIGS. 1A to 1D.

[0074] The sputtering target is manufactured, for example, by the following steps: A step of grinding the surface of the oxide sintered body (grinding step) A step of bonding the oxide sintered body to a backing plate (bonding step) Each step will be specifically described below.

[0075] <Grinding step> In the grinding step, the oxide sintered body is cut into a shape suitable for installation in a sputtering device. The surface of the oxide sintered body often has sintered portions in a highly oxidized state or is uneven. In addition, it is necessary to cut the oxide sintered body to a predetermined size. The surface of the oxide sintered body is preferably ground to a depth of 0.3 mm or more. The grinding depth is preferably 0.5 mm or more, and more preferably 2 mm or more. By grinding to a depth of 0.3 mm or more, it is possible to remove portions of the oxide sintered body with a fluctuating crystal structure near the surface.

[0076] The oxide sintered body is preferably made into a material having an average surface roughness Ra of 5 μm or less by, for example, grinding the surface of the oxide sintered body with a surface grinder. Furthermore, the sputtering surface of the sputtering target is subjected to mirror finishing to make the average surface roughness Ra of 1000×10 -10 The polishing method may be set to 0.05 mm or less. Mirror finishing (polishing) can be performed using known polishing techniques such as mechanical polishing, chemical polishing, and mechanochemical polishing (a combination of mechanical polishing and chemical polishing). For example, polishing to #2000 or higher may be performed using a fixed abrasive polisher (using water as the polishing liquid), or lapping may be performed using a free abrasive lap (using SiC paste or the like as the abrasive), followed by lapping using a diamond paste as the abrasive. The polishing method is not limited to these methods. Examples of abrasives include #200, #400, and #800 abrasives.

[0077] After the grinding process, the oxide sintered body is preferably cleaned by air blowing, running water washing, or the like. When removing foreign matter by air blowing, removal can be more effective if a dust collector is used to suck air from the opposite side of the nozzle. Note that, since air blowing and running water washing have limitations in their cleaning power, ultrasonic cleaning or the like can also be performed. An effective ultrasonic cleaning method is to use multiple oscillations at a frequency between 25 kHz and 300 kHz. For example, it is recommended to perform ultrasonic cleaning by multiple oscillations at 12 different frequencies in 25 kHz increments between 25 kHz and 300 kHz.

[0078] <Bonding step> In the bonding step, the ground oxide sintered body is bonded to a backing plate using a low-melting-point metal. Metallic indium is preferably used as the low-melting-point metal. Metallic indium containing at least one of metal gallium and metal tin can also be preferably used as the low-melting-point metal.

[0079] According to the sputtering target of this embodiment, the atomic ratios of the In element, the Ga element, the Al element, and the X element having a positive trivalent valence satisfy all of the formulas (1) to (3). 2 O 3 and a crystalline phase having a diffraction peak within the range of the incident angle (2θ) defined in (A) to (K) above, stable sputtering can be achieved by using this sputtering target. Furthermore, in a TFT having an oxide thin film obtained by sputtering a sputtering target containing this oxide sintered body, a TFT with high mobility and excellent in-plane uniformity can be achieved.

[0080] [Oxide Thin Film] The oxide thin film according to this embodiment is an oxide thin film formed using the sputtering target according to this embodiment. The oxide thin film according to this embodiment is obtained by forming a film by a sputtering method using the sputtering target according to this embodiment. The oxide thin film according to this embodiment can be formed by a method other than the sputtering method, for example, selected from the group consisting of a vapor deposition method, an ion plating method, and a pulsed laser vapor deposition method. The oxide thin film according to this embodiment is preferably formed by a sputtering method using the sputtering target according to this embodiment. The oxide thin film according to this embodiment may be an amorphous oxide semiconductor thin film or a crystalline oxide semiconductor thin film. The oxide thin film according to this embodiment may be either amorphous or crystalline. The oxide thin film according to this embodiment is preferably a crystalline oxide semiconductor thin film.

[0081] The oxide thin film according to this embodiment is formed using a target having the same atomic composition (atomic ratio) as the sintered body according to this embodiment, and therefore the atomic composition of the oxide thin film according to this embodiment usually reflects the atomic composition of the oxide sintered body included in the sputtering target according to this embodiment used for film formation. Therefore, the oxide thin film according to this embodiment allows for the production of TFTs with high mobility and excellent in-plane uniformity.

[0082] Whether an oxide thin film is amorphous or crystalline can be confirmed by subjecting each oxide thin film to X-ray diffraction (XRD) measurement. When an oxide thin film is subjected to XRD measurement, if no clear peak is observed but a broad pattern is, the oxide thin film can be determined to be amorphous, and if a clear peak is observed, the oxide thin film can be determined to be crystalline.

[0083] 99 atomic % or more of the elements contained in the oxide thin film according to this embodiment may be In, Ga, Al, a positive trivalent X element, and O, or 99.9 atomic % or more of the elements contained in the oxide thin film may be In, Ga, Al, a positive trivalent X element, and O. Furthermore, 99 atomic % or more of the metal elements contained in the oxide thin film may be In, Ga, Al, and a positive trivalent X element, or 99.9 atomic % or more of the metal elements contained in the oxide thin film may be In, Ga, Al, and a positive trivalent X element. The metal elements contained in the oxide thin film according to this embodiment may consist essentially of In, Ga, Al, and a positive trivalent X element.

[0084] In this specification, the atomic ratio of the oxide thin film (crystalline oxide thin film and amorphous oxide thin film) can be determined by measuring the amount of each element present by inductively coupled plasma atomic emission spectroscopy (ICP-AES) or X-ray fluorescence spectroscopy (XRF). An inductively coupled plasma atomic emission spectroscopy analyzer can be used for the ICP measurement. A thin film X-ray fluorescence analyzer (AZX400, manufactured by Rigaku Corporation) can be used for the XRF measurement.

[0085] Furthermore, the content (atomic ratio) of each metal element in an oxide thin film can be analyzed with the same accuracy as in inductively coupled plasma optical emission spectroscopy (ICP-AES). A standard material is prepared by forming source and drain electrodes of the same material as the TFT element on the top surface of a standard oxide thin film whose atomic ratio of metal elements is known, as measured by an ICP-AES or thin film X-ray fluorescence analyzer. The oxide semiconductor layer is analyzed using a SIMS sector dynamic secondary ion mass spectrometer (IMS 7f-Auto, manufactured by AMETEK Corporation) to obtain the mass spectral intensity of each element, and a calibration curve of the known element concentration and mass spectral intensity is prepared. Next, the atomic ratio of the oxide semiconductor film portion of an actual TFT element is calculated from the spectral intensity obtained by the SIMS sector dynamic secondary ion mass spectrometer analysis using the calibration curve. It can be confirmed that the calculated atomic ratio is within 2 atomic % of the atomic ratio of the oxide semiconductor film separately measured by a thin film X-ray fluorescence analyzer or an ICP-AES.

[0086] [Method for forming oxide thin film] The oxide thin film according to this embodiment is preferably obtained by a production method including, for example, a step of forming an oxide thin film by sputtering using the sputtering target according to this embodiment, and a step of subjecting the oxide thin film to a heat treatment (annealing treatment) as necessary.

[0087] Hereinafter, a case where an oxide thin film is formed on a substrate by sputtering a sputtering target obtained from the oxide sintered body according to this embodiment will be described. Referring to Fig. 2A, Fig. 2A shows a state where an oxide thin film 83 is formed on a glass substrate 81.

[0088] The sputtering may be performed by a method selected from the group consisting of DC sputtering, RF sputtering, AC sputtering, and pulsed DC sputtering. Any of these methods can perform sputtering without abnormal discharge. A mixed gas of argon and an oxidizing gas can be used as the sputtering gas. The oxidizing gas may be O. 2 , CO 2 , O 3, and H 2 The gas may be selected from the group consisting of O and the like.

[0089] The sputtering gas used is a gas that is substantially free of impurity gases. The phrase "substantially free of impurity gases" means that no impurity gases other than the sputtering gas used as the sputtering gas are actively introduced, excluding adsorbed water brought in with the gas introduction and gases that cannot be eliminated (unavoidable impurity gases) such as gases leaking from the chamber or adsorbed gases. The proportion of impurity gases in the sputtering gas is preferably 0.1% by volume or less, and more preferably 0.05% by volume or less.

[0090] The oxide thin film formed on the substrate by sputtering is annealed as necessary. The crystallinity of the oxide thin film on the substrate is improved by annealing after sputtering, resulting in a crystalline oxide thin film. Even when the oxide thin film on the substrate is annealed, the oxide thin film is likely to maintain an amorphous state if the annealing conditions are as follows: The annealing temperature is, for example, 500°C or less, preferably 100°C or more and 500°C or less, more preferably 150°C or more and 400°C or less, and particularly preferably 250°C or more and 400°C or less. The annealing time is usually 0.01 hours or more and 5.0 hours or less, preferably 0.1 hours or more and 3.0 hours or less, and more preferably 0.5 hours or more and 2.0 hours or less.

[0091] The heating atmosphere during the annealing treatment is not particularly limited, and an air atmosphere or an oxygen-flowing atmosphere is preferred from the viewpoint of carrier controllability, and an air atmosphere is more preferred. In the annealing treatment, an apparatus selected from the group consisting of a lamp annealing apparatus, a laser annealing apparatus, a thermal plasma apparatus, a hot air heating apparatus, and a contact heating apparatus can be used in the presence or absence of oxygen.

[0092] The oxide thin film according to this embodiment can also be manufactured as part of a laminate including, for example, an oxide thin film and a protective film. For example, referring to FIG. 2B, a SiO 2 thin film 83 is laminated on the oxide thin film 83 as a protective film. 2The protective film 85 is formed on the substrate 10. The protective film 85 may be made of, for example, SiO 2 , SiON, Al 2 O 3 , Ta 2 O 5 , TiO 2 , MgO, ZrO 2 , CeO 2 , K. 2 O, Li 2 O, Na 2 O, Rb 2 O, Sc 2 O 3 , Y 2 O 3 , Hf 2 O 3 , CaHfO 3 , PbTiO 3 ,BaTa 2 O 6 , and SrTiO 3 Among these, the protective film is preferably a film made of SiO 2 , SiON, Al 2 O 3 , Y 2 O 3 , Hf 2 O 3 , and CaHfO 3 and more preferably, SiO 2 or Al 2 O 3 The number of oxygen atoms in these oxides does not necessarily have to match the stoichiometric ratio (for example, SiO 2 (The formula "x" is a real number greater than 0.) These protective films can function as protective insulating films. The protective film can be formed using plasma CVD or sputtering, and is preferably formed by sputtering in an oxygen-containing rare gas atmosphere. The thickness of the protective film can be set appropriately, and is, for example, 50 nm or more and 500 nm or less.

[0093] When a protective film is formed on an oxide thin film, the annealing treatment can be performed (1) after the oxide thin film is formed on the substrate but before the protective film is formed, (2) after the protective film is formed so as to cover the oxide thin film on the substrate, or (3) in either of (1) and (2).

[0094] The oxide thin film according to this embodiment can be applied to various integrated circuits such as logic circuits, memory circuits, and differential amplifier circuits, and can be applied to electronic devices, etc. The oxide thin film according to this embodiment can also be applied as a part of a layer in a solar cell, and a part of a layer in a display device such as a liquid crystal device, an organic electroluminescence device, an inorganic electroluminescence device, a micro organic EL display, a micro LED (Light Emitting Diode) display, and a mini LED display. Furthermore, the oxide thin film according to this embodiment can be applied as a part of a layer in a solid-state imaging device, an X-ray sensor, a power semiconductor device, a touch panel, an LSI (Large Scale Integrated Circuit), a resistance change type memory, a DRAM (Dynamic Random Access Memory), a ferroelectric memory, a BEOL (Back End of Line), and a microprocessor. The oxide thin film according to this embodiment can also be used as a semiconductor layer of a field-effect transistor, a static induction transistor, a quantum tunnel field-effect transistor, a Schottky barrier transistor, a Schottky diode, a PN diode, and a resistor element, or as a part of any of these layers.

[0095] [Thin Film Transistor and Electronic Device] The thin film transistor according to this embodiment includes a thin film transistor including the oxide thin film according to this embodiment. The thin film transistor according to this embodiment may be a thin film transistor including an amorphous oxide thin film, a thin film transistor including a crystalline oxide thin film, or a thin film transistor including both an amorphous oxide thin film and a crystalline oxide thin film. The oxide thin film included in the thin film transistor according to this embodiment is preferably a crystalline oxide semiconductor thin film.

[0096] It is preferable to use the oxide thin film according to this embodiment as the channel layer of a thin film transistor.

[0097] When the thin film transistor according to this embodiment has the oxide thin film according to this embodiment as a channel layer, other element configurations in the thin film transistor are not particularly limited, and known element configurations can be adopted.

[0098] The thin film transistor according to this embodiment can be suitably used in electronic devices. Specifically, the thin film transistor according to this embodiment can be suitably used in display devices such as liquid crystal displays and organic EL displays.

[0099] The thickness of the channel layer in the thin film transistor according to this embodiment is usually 10 nm or more and 300 nm or less, and preferably 20 nm or more and 250 nm or less.

[0100] The channel layer in the thin film transistor according to this embodiment is usually used in an N-type region, but can also be used in various semiconductor devices such as a PN junction transistor in combination with various P-type semiconductors, such as a P-type Si-based semiconductor, a P-type oxide semiconductor, and a P-type organic semiconductor.

[0101] The thin film transistor according to this embodiment can be applied to various integrated circuits such as field-effect transistors, logic circuits, memory circuits, and differential amplifier circuits. Furthermore, in addition to field-effect transistors, the thin film transistor can also be applied to static induction transistors, Schottky barrier transistors, Schottky diodes, and resistor elements. That is, the thin film transistor according to this embodiment can be applied to the applications exemplified in the "Applications of Thin Film Transistors" section described later.

[0102] The structure of the thin film transistor according to this embodiment can be selected from known structures such as bottom gate, bottom contact, and top contact, without any restrictions. The bottom gate structure is particularly advantageous because it provides higher performance than amorphous silicon or ZnO thin film transistors. The bottom gate structure is preferred because it can easily reduce the number of masks used during manufacturing and thus reduce manufacturing costs for applications such as large displays.

[0103] The shape of the thin film transistor according to this embodiment is not particularly limited, and is preferably a back channel etch type transistor, an etch stopper type transistor, a top gate type transistor, a double gate type transistor, etc. Each transistor may have a self-aligned structure.

[0104] Specific examples of thin film transistors are shown in Figures 3, 4, 5, and 6. As shown in Figure 3, a thin film transistor 100 includes a silicon wafer 20, a gate insulating film 30, an oxide thin film 40, a source electrode 50, a drain electrode 60, and interlayer insulating films 70 and 70A.

[0105] The silicon wafer 20 is a gate electrode. The gate insulating film 30 is an insulating film that blocks electrical conduction between the gate electrode and the oxide thin film 40, and is provided on the silicon wafer 20. The oxide thin film 40 is a channel layer and is provided on the gate insulating film 30. The oxide thin film 40 is made of the oxide thin film according to this embodiment.

[0106] The source electrode 50 and the drain electrode 60 are conductive terminals for passing source current and drain current through the oxide thin film 40, and are provided so as to be in contact with the vicinity of both ends of the oxide thin film 40. The interlayer insulating film 70 is an insulating film that blocks conduction between the source electrode 50 and the drain electrode 60 and the oxide thin film 40 except at the contact portions between the source electrode 50 and the drain electrode 60 and the oxide thin film 40. The interlayer insulating film 70A is an insulating film that blocks conduction between the source electrode 50 and the drain electrode 60 and the oxide thin film 40 except at the contact portions between the source electrode 50 and the drain electrode 60 and the oxide thin film 40. The interlayer insulating film 70A is also an insulating film that blocks conduction between the source electrode 50 and the drain electrode 60. The interlayer insulating film 70A also functions as a channel layer protective layer.

[0107] 4, the structure of the thin-film transistor 100A is similar to that of the thin-film transistor 100, except that the source electrode 50 and the drain electrode 60 are provided so as to be in contact with both the gate insulating film 30 and the oxide thin film 40. Another difference is that an interlayer insulating film 70B is provided integrally so as to cover the gate insulating film 30, the oxide thin film 40, the source electrode 50, and the drain electrode 60.

[0108] There are no particular limitations on the materials forming the drain electrode 60, the source electrode 50, and the gate electrode, and any commonly used material can be selected. In the examples shown in Figures 3 and 4, a silicon wafer is used as the substrate, and the silicon wafer also functions as the electrode, but the electrode material is not limited to silicon. For example, indium tin oxide (ITO), indium zinc oxide (IZO), ZnO, and SnO 2 3, 4, 5, and 6, a gate electrode may be formed on a substrate such as glass.

[0109] There is no particular limitation on the material for forming the interlayer insulating films 70, 70A, and 70B, and any commonly used material can be selected. x , M.N. x , and M.N. x O y (where M is a metal element, and x and y are real numbers greater than 0. The same applies to x and y in the compounds exemplified below.) Specific examples of the material include SiO 2 , SiO x , SiN x , and SiN x O y Furthermore, the material may be, for example, Al 2 O 3 , Ta 2 O 5 , TiO 2 , MgO, ZrO 2 , CeO 2 , K. 2 O, Li 2 O, Na 2 O, Rb 2 O, Sc 2 O 3 , Y 2 O 3 , HfO 2 , CaHfO 3 , PbTiO3 ,BaTa 2 O 6 , SrTiO 3 , Sm 2 O 3 Compounds such as AlN can also be used. The valence of the anions (oxygen anions and nitrogen anions) in these oxide compounds and nitride compounds is not particularly limited as long as it is a real number greater than 0.

[0110] When the thin film transistor according to this embodiment is a back channel etch type (bottom gate type), it is preferable to provide a protective film on the drain electrode, the source electrode, and the channel layer. By providing a protective film, the durability of the TFT is likely to be improved even when the TFT is driven for a long time. In the case of a top gate type TFT, for example, a gate insulating film is formed on the channel layer.

[0111] When the thin-film transistor according to this embodiment is a top-gate TFT, for example, it has a structure in which an interlayer insulating film is formed as a buffer layer on a substrate and a gate insulating film is formed on a channel layer. As shown in FIG. 5 , the thin-film transistor 100B includes a substrate 21, a buffer layer 22, a channel layer (oxide thin film) 11, a first low-resistance region 11A-1, a second low-resistance region 11A-2 (oxide thin film), a semiconductor region 11B (oxide thin film), a gate insulating film 24, a gate electrode 25, an interlayer insulating film 26, a source electrode 27, a drain electrode 28, and a protective film 29. In the thin-film transistor 100B, the first low-resistance region 11A-1 and the second low-resistance region 11A-2 are formed, for example, by ion implantation, a dry process such as plasma treatment, or the like. Furthermore, an electrode layer may be provided between the substrate 21 and the buffer layer 22 as a write shield layer.

[0112] 6 shows another example of a top-gate thin-film transistor according to the present embodiment. The thin-film transistor 100C has a similar structure to the thin-film transistor 100B, except that the interlayer insulating film 26 has a two-layer structure (a first interlayer insulating film 26-1 and a second interlayer insulating film 26-2). In the thin-film transistor 100C, the first low-resistance region 11A-1 and the second low-resistance region 11A-2 are formed by, for example, ion implantation.

[0113] The protective film or insulating film can be formed by, for example, CVD, which may require high-temperature processes. Furthermore, the protective film or insulating film often contains impurity gases immediately after deposition, so it is preferable to subject it to a heat treatment (annealing treatment). Removing the impurity gases through the heat treatment results in a stable protective film or insulating film, which facilitates the formation of highly durable TFT elements.

[0114] By using the oxide thin film according to this embodiment, the film is less susceptible to the effects of temperature in the CVD process and subsequent heat treatment, and therefore the stability of the TFT characteristics can be improved even when a protective film or an insulating film is formed.

[0115] In the characteristics of the thin film transistor according to this embodiment, the On / Off ratio is 10 6 That's it, 10 12 Preferably, it is 10 7 That's it, 10 11 More preferably, it is 10 8 That's it, 10 10 It is more preferable that the On / Off ratio is 10 or less. 6 An On / Off ratio of 10 or more is preferable for driving liquid crystal and OLED displays. 12 If the On / Off ratio is 10 or less, an organic EL display with high contrast can be driven. 12 If the off-state current is 10 -11 A or less, and when the thin film transistor is used as a transfer transistor or reset transistor in a CMOS image sensor, it is possible to extend the image retention time and improve the sensitivity. The On / Off ratio can be calculated by determining the ratio [On current value / Off current value], where the value of Id when Vg = -10 V is the Off current value and the value of Id when Vg = 20 V is the On current value.

[0116] The mobility of the TFT according to this embodiment is 5 cm 2 / Vs or more, and 2The linear mobility is expressed by the transconductance (Gm) for each Vg calculated from a graph of transfer characteristics, and the maximum mobility in the Vg range from -15 V to 20 V can be defined as the linear mobility.

[0117] In the characteristics of the thin film transistor according to this embodiment, the threshold voltage (Vth) is preferably −3.0 V or more and 3.0 V or less, more preferably −2.0 V or more and 2.0 V or less, and even more preferably −1.0 V or more and 1.0 V or less. When the threshold voltage (Vth) is −3.0 V or more, a thin film transistor with high mobility can be obtained. When the threshold voltage (Vth) is 3.0 V or less, a thin film transistor with a small off-current and a large on-off ratio can be obtained. Furthermore, when the threshold voltage (Vth) is −3.0 V or more and 3.0 V or less, a Vth correction circuit can be installed in the TFT to correct Vth to 0 V. When the TFT thus obtained is installed in a panel, it can drive a display without uneven brightness or burn-in. From the transfer characteristic graph, the threshold voltage (Vth) is determined by the current value Id between the source and drain = 10 -9 It can be defined as the gate voltage Vg at A.

[0118] <Quantum Tunnel Field Effect Transistor> The oxide thin film according to this embodiment can also be used in a quantum tunnel field effect transistor (FET), which may also be referred to as a quantum tunnel field effect transistor.

[0119] 7 is a schematic diagram (longitudinal cross-sectional view) of a quantum tunnel field effect transistor (FET) according to one embodiment. The quantum tunnel field effect transistor 501 includes a p-type semiconductor layer 503, an n-type semiconductor layer 507, a gate insulating film 509, a gate electrode 511, a source electrode 513, and a drain electrode 515.

[0120] A p-type semiconductor layer 503, an n-type semiconductor layer 507, a gate insulating film 509, and a gate electrode 511 are stacked in this order. A source electrode 513 is provided on the p-type semiconductor layer 503. A drain electrode 515 is provided on the n-type semiconductor layer 507. The p-type semiconductor layer 503 is a p-type Group IV semiconductor layer, and in this case is a p-type silicon layer. In this case, the n-type semiconductor layer 507 is an n-type oxide thin film according to the above embodiment. The source electrode 513 and the drain electrode 515 are conductive films.

[0121] 7, an insulating layer may be formed on the p-type semiconductor layer 503. In this case, the p-type semiconductor layer 503 and the n-type semiconductor layer 507 are connected via a contact hole, which is a region where the insulating layer is partially opened. Although not shown in FIG. 7, the quantum tunnel field effect transistor 501 may also have an interlayer insulating film covering its upper surface.

[0122] The quantum tunnel field effect transistor 501 is a quantum tunnel field effect transistor (FET) that switches current by controlling the current tunneling through the energy barrier formed by the p-type semiconductor layer 503 and the n-type semiconductor layer 507 using the voltage of the gate electrode 511. In this structure, the band gap of the oxide thin film that constitutes the n-type semiconductor layer 507 is large, making it possible to reduce the off-current.

[0123] FIG. 8 is a schematic diagram (longitudinal cross-sectional view) of a quantum tunnel field-effect transistor 501A according to another embodiment. The quantum tunnel field-effect transistor 501A has the same configuration as the quantum tunnel field-effect transistor 501, except that a silicon oxide layer 505 is formed between a p-type semiconductor layer 503 and an n-type semiconductor layer 507. The presence of the silicon oxide layer reduces the off-state current. The thickness of the silicon oxide layer 505 is preferably 10 nm or less. By making the thickness of the silicon oxide layer 505 10 nm or less, it is possible to prevent tunneling current from flowing, energy barriers from being formed, and changes in barrier height, thereby preventing a decrease or change in the tunneling current. The thickness of the silicon oxide layer 505 is preferably 8 nm or less, more preferably 5 nm or less, even more preferably 3 nm or less, and even more preferably 1 nm or less.

[0124] In the quantum tunnel field effect transistors 501 and 501A, the n-type semiconductor layer 507 is also an n-type oxide semiconductor.

[0125] The oxide thin film constituting the n-type semiconductor layer 507 may be amorphous. When the oxide thin film constituting the n-type semiconductor layer 507 is amorphous, it can be etched with an organic acid such as oxalic acid, the difference in etching rate with other layers becomes large, and etching can be performed satisfactorily without affecting metal layers such as wiring.

[0126] The oxide thin film constituting the n-type semiconductor layer 507 may be crystalline. When the oxide thin film constituting the n-type semiconductor layer 507 is crystalline, the band gap becomes larger than in the case of an amorphous material, and the off-current can be reduced. Since the work function can also be increased, it becomes easier to control the current tunneling through the energy barrier formed by the p-type Group IV semiconductor material and the n-type semiconductor layer 507.

[0127] The method for manufacturing the quantum tunnel field effect transistor 501 is not particularly limited, but the following method can be exemplified. First, as shown in Fig. 9A, an insulating film 505A is formed on a p-type semiconductor layer 503, and a part of the insulating film 505A is opened by etching or the like to form a contact hole 505B. Next, as shown in Fig. 9B, an n-type semiconductor layer 507 is formed on the p-type semiconductor layer 503 and the insulating film 505A. At this time, the p-type semiconductor layer 503 and the n-type semiconductor layer 507 are connected via the contact hole 505B.

[0128] 9C, a gate insulating film 509 and a gate electrode 511 are formed in this order on the n-type semiconductor layer 507. Next, as shown in FIG. 9D, an interlayer insulating film 519 is provided so as to cover the insulating film 505A, the n-type semiconductor layer 507, the gate insulating film 509, and the gate electrode 511.

[0129] Next, as shown in Fig. 9E, a contact hole 519A is formed by opening a portion of the insulating film 505A and interlayer insulating film 519 on the p-type semiconductor layer 503, and a source electrode 513 is provided in the contact hole 519A. Furthermore, as shown in Fig. 9E, a contact hole 519B is formed by opening a portion of the gate insulating film 509 and interlayer insulating film 519 on the n-type semiconductor layer 507, and a drain electrode 515 is formed in the contact hole 519B. Through the above procedure, the quantum tunnel field effect transistor 501 can be manufactured.

[0130] After forming n-type semiconductor layer 507 on p-type semiconductor layer 503, heat treatment is performed at a temperature of 150° C. or higher and 600° C. or lower, thereby forming silicon oxide layer 505 between p-type semiconductor layer 503 and n-type semiconductor layer 507. By adding this step, quantum tunnel field effect transistor 501A can be manufactured.

[0131] The thin film transistor according to this embodiment is preferably a channel-doped thin film transistor, which is a transistor in which carriers in the channel are appropriately controlled by n-type doping rather than by oxygen deficiency, which is susceptible to fluctuations in response to external stimuli such as atmosphere and temperature, and which has the effect of achieving both high mobility and high reliability.

[0132] <Applications of Thin Film Transistor> The thin film transistor according to this embodiment can be suitably used in solar cells, display elements (liquid crystal elements, organic electroluminescence elements, inorganic electroluminescence elements, etc.), and power semiconductor elements. The thin film transistor according to this embodiment can be suitably used as a transistor in active matrix devices such as display devices (liquid crystal displays, organic electroluminescence (EL) displays, micro organic EL displays, micro light-emitting diode (LED) displays, mini LED displays, etc.), solid-state imaging elements, and touch panels. The thin film transistor according to this embodiment can also be applied to various integrated circuits such as field-effect transistors, logic circuits, memory circuits, and differential amplifier circuits, which can be applied to electronic devices, etc. The electronic device according to this embodiment preferably includes a thin film transistor. Furthermore, the thin film transistor according to this embodiment can be applied to static induction transistors and Schottky barrier transistors in addition to field-effect transistors. The thin film transistor according to this embodiment can also be applied as a transistor for sensors such as image sensors, X-ray sensors, and biosensors.

[0133] Hereinafter, the case where the thin film transistor according to this embodiment is used in a display device and a solid-state image sensor will be described.

[0134] First, a case where the thin film transistor according to this embodiment is used in a display device will be described with reference to Figures 10A to 10C. Figure 10A is a top view of the display device according to this embodiment. Figure 10B is a circuit diagram for explaining the circuit of the pixel portion when a liquid crystal element is applied to the pixel portion of the display device according to this embodiment. Also, Figure 10C is a circuit diagram for explaining the circuit of the pixel portion when an organic EL element is applied to the pixel portion of the display device according to this embodiment.

[0135] The thin film transistor according to this embodiment can be used as a transistor disposed in a pixel portion. Since the thin film transistor according to this embodiment can be easily made into an n-channel type, part of a driver circuit that can be configured with an n-channel transistor is formed over the same substrate as the transistor in the pixel portion. By using the thin film transistor described in this embodiment for the pixel portion or the driver circuit, a highly reliable display device can be provided.

[0136] 10A shows an example of a top view of an active matrix display device. A pixel portion 301, a first scanning line driver circuit 302, a second scanning line driver circuit 303, and a signal line driver circuit 304 are formed on a substrate 300 of the display device. A plurality of signal lines are arranged in the pixel portion 301, extending from the signal line driver circuit 304, and a plurality of scanning lines are arranged in the pixel portion 301, extending from the first scanning line driver circuit 302 and the second scanning line driver circuit 303. Pixels each having a display element are provided in a matrix at the intersections of the scanning lines and the signal lines. The substrate 300 of the display device is connected to a timing control circuit (also referred to as a controller or a control IC) via a connection portion such as an FPC (Flexible Printed Circuit).

[0137] 10A , the first scanning line driver circuit 302, the second scanning line driver circuit 303, and the signal line driver circuit 304 are formed on the same substrate 300 as the pixel portion 301. This reduces the number of components, such as driver circuits, that are provided externally, thereby reducing costs. Furthermore, if the driver circuits are provided externally to the substrate 300, it becomes necessary to extend the wiring, which increases the number of connections between the wiring. If the driver circuits are provided on the same substrate 300, the number of connections between the wiring can be reduced, thereby improving reliability and yield.

[0138] 10B shows an example of a circuit configuration of a pixel, which is applicable to the pixel portion of a VA-type liquid crystal display device.

[0139] This pixel circuit can be applied to a configuration in which one pixel has multiple pixel electrodes. Each pixel electrode is connected to a different transistor, and each transistor is configured to be driven by a different gate signal. This allows the signals applied to each pixel electrode of a multi-domain pixel to be controlled independently.

[0140] The gate wiring 312 of the transistor 316 and the gate wiring 313 of the transistor 317 are separated so as to receive different gate signals. On the other hand, the source or drain electrode 314 functioning as a data line is used in common by the transistors 316 and 317. The thin film transistors according to this embodiment can be used for the transistors 316 and 317. This makes it possible to provide a highly reliable liquid crystal display device.

[0141] The transistor 316 is electrically connected to a first pixel electrode, and the transistor 317 is electrically connected to a second pixel electrode. The first pixel electrode and the second pixel electrode are separated from each other. The shapes of the first pixel electrode and the second pixel electrode are not particularly limited. For example, the first pixel electrode may be V-shaped.

[0142] The gate electrode of the transistor 316 is connected to the gate wiring 312, and the gate electrode of the transistor 317 is connected to the gate wiring 313. By applying different gate signals to the gate wiring 312 and the gate wiring 313, the operation timing of the transistors 316 and 317 can be made different, thereby controlling the alignment of the liquid crystal.

[0143] Furthermore, a storage capacitor may be formed by the capacitor wiring 310, a gate insulating film that functions as a dielectric, and a capacitor electrode that is electrically connected to the first pixel electrode or the second pixel electrode.

[0144] The multi-domain structure has one pixel having a first liquid crystal element 318 and a second liquid crystal element 319. The first liquid crystal element 318 is composed of a first pixel electrode, a counter electrode, and a liquid crystal layer therebetween, and the second liquid crystal element 319 is composed of a second pixel electrode, a counter electrode, and a liquid crystal layer therebetween.

[0145] The pixel portion is not limited to the configuration shown in Fig. 10B, and may include a switch, a resistor, a capacitor, a transistor, a sensor, or a logic circuit.

[0146] Another example of the circuit configuration of a pixel is shown in Fig. 10C, which shows the structure of a pixel portion of a display device using an organic EL element.

[0147] 10C is a diagram showing an example of an applicable circuit for the pixel portion 320. Here, an example is shown in which two n-channel transistors are used in one pixel. The oxide thin film according to this embodiment can be used in the channel formation region of the n-channel transistor. Digital time grayscale driving can be applied to the circuit for the pixel portion.

[0148] The thin film transistor according to this embodiment can be used for the switching transistor 321 and the driving transistor 322. This makes it possible to provide a highly reliable organic EL display device.

[0149] The configuration of the circuit in the pixel portion is not limited to the configuration shown in Fig. 10C. A switch, a resistor, a capacitor, a sensor, a transistor, or a logic circuit may be added to the circuit in the pixel portion shown in Fig. 10C. The above is a description of the case where the thin film transistor according to this embodiment is used in a display device.

[0150] Next, a case where the thin film transistor according to this embodiment is used in a solid-state imaging device will be described with reference to FIG.

[0151] A CMOS (Complementary Metal Oxide Semiconductor) image sensor is a solid-state imaging device that holds a potential in a signal charge storage section and outputs that potential to a vertical output line via an amplification transistor. If a leak current occurs in the reset transistor and / or transfer transistor included in the CMOS image sensor, the leak current causes charging or discharging, changing the potential of the signal charge storage section. When the potential of the signal charge storage section changes, the potential of the amplification transistor also changes, resulting in a value that deviates from the original potential, degrading the captured image.

[0152] The operational effect when the thin film transistor according to this embodiment is applied to the reset transistor and transfer transistor of a CMOS image sensor will be described. Either a thin film transistor or a bulk transistor may be applied to the amplifying transistor.

[0153] 11 is a diagram showing an example of the pixel configuration of a CMOS image sensor. A pixel is composed of a photodiode 3002, which is a photoelectric conversion element, a transfer transistor 3004, a reset transistor 3006, an amplifier transistor 3008, and various wirings, and a plurality of pixels are arranged in a matrix to form a sensor. A selection transistor electrically connected to the amplifier transistor 3008 may be provided. The transistor symbols "OS" and "Si" represent oxide semiconductor and silicon, respectively, and represent materials that are preferable for use in the respective transistors. This also applies to the subsequent drawings.

[0154] The photodiode 3002 is connected to the source side of the transfer transistor 3004, and a signal charge storage region 3010 (also called FD: floating diffusion) is formed on the drain side of the transfer transistor 3004. The source of the reset transistor 3006 and the gate of the amplification transistor 3008 are connected to the signal charge storage region 3010. As an alternative configuration, the reset power supply line 3110 can be eliminated. For example, the drain of the reset transistor 3006 can be connected to the power supply line 3100 or the vertical output line 3120 instead of the reset power supply line 3110. Note that the oxide thin film according to this embodiment may be used for the photodiode 3002, and the same material as the oxide thin films used for the transfer transistor 3004 and the reset transistor 3006 may be used.

[0155] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples.

[0156] [Production of Oxide Sintered Body] (Examples 1 to 14) Gallium oxide powder, aluminum oxide powder, indium oxide powder, and a powder of an oxide of a positive trivalent X element were weighed out so as to have the composition (at %) shown in Tables 1 and 2, placed in a polyethylene pot, and mixed and pulverized for 72 hours using a dry ball mill to produce a mixed powder. The powder of the oxide of a positive trivalent X element was any powder selected from the group consisting of yttrium oxide, lanthanum oxide, neodymium oxide, promethium oxide, samarium oxide, europium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, holmium oxide, erbium oxide, thulium oxide, ytterbium oxide, and lutetium oxide. This mixed powder was placed in a mold and subjected to a pressure of 500 kg / cm. 2 This press-molded body was subjected to a pressure of 2000 kg / cm. 2 The compact was densified by CIP at a pressure of 100°C. Next, this densified press-molded body was placed in an atmospheric pressure sintering furnace and held at 350°C for 3 hours. Thereafter, the temperature was increased at a rate of 100°C / hour, sintered at 1350°C for 24 hours, and allowed to cool to obtain an oxide sintered body. The obtained oxide sintered body was evaluated as follows. The evaluation results are shown in Tables 1 and 2.

[0157] (Comparative Examples 1 to 7) Oxide sintered bodies were produced in the same manner as in Example 1, etc., except that gallium oxide powder, aluminum oxide powder, indium oxide powder, and powder of oxide of positive trivalent X element were weighed so as to obtain the compositions (at %) shown in Table 3. Note that in Comparative Examples 1 and 2, powder of oxide of positive trivalent X element was not used. The obtained oxide sintered bodies were evaluated as follows in the same manner as in Example 1, etc. The evaluation results are shown in Table 3.

[0158] In Tables 1 to 3, the numerical values ​​shown as "at %" indicate the atomic composition ratio of indium element, gallium element, aluminum element, and X element expressed as a percentage.

[0159] Evaluation of Properties of Oxide Sintered Body (1) Composition (at %) of Oxide Sintered Body The compositions of In element, Ga element, Al element, and positive trivalent X element in the sintered bodies obtained in each of the above examples and comparative examples were measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES, manufactured by Shimadzu Corporation).

[0160] (2) Crystal structure The X-ray diffraction (XRD) of the oxide sintered bodies obtained in each of the above examples and comparative examples was measured using an X-ray diffraction measuring device SmartLab under the following conditions. The obtained XRD chart was analyzed using JADE6 to confirm the crystalline phase in the oxide sintered body. Device: SmartLab (manufactured by Rigaku Corporation) X-ray: Cu-Kα ray (wavelength 1.5418 × 10 -10 m) 2θ-θ reflection method, continuous scan (2.0° / min) Sampling interval: 0.02° Slits DS (divergence slit), SS (scattering slit), RS (receiving slit): 1 mm

[0161] In Tables 1 to 3, In 2 O 3 The bixbyite crystalline phase represented by the formula (I) is referred to as "bixbyite", and the crystalline phase of the novel compound having a diffraction peak in the range of incident angles (2θ) observed by X-ray (Cu-Kα ray) diffraction measurement specified in (A) to (K) above is referred to as "crystalline phase A".

[0162] (3) Bulk Resistivity (mΩ cm) The bulk resistance (mΩ cm) of the oxide sintered bodies obtained in the above-mentioned respective Examples and Comparative Examples was measured using a resistivity meter Loresta (manufactured by Mitsubishi Chemical Corporation) based on the four-probe method (JIS R 1637:1998). The measurement points were five points in total, namely the center of the oxide sintered body and four points midpoints between the four corners and the center of the oxide sintered body, and the average value of the five points was taken as the bulk resistance value.

[0163] (4) Color Unevenness The color unevenness of the oxide sintered bodies obtained in each of the above Examples and Comparative Examples was evaluated by visually inspecting the sintered bodies from a distance of 50 cm under daylight from a north window. If the sintered body has color unevenness, it may be difficult to determine the state of color unevenness, for example, when using the target.

[0164] (5) White Spots The white spots of the oxide sintered bodies obtained in the above-mentioned respective Examples and Comparative Examples were visually observed after surface grinding to a predetermined thickness by grinding processing, and the number of white spots having a diameter of 0.5 mmφ or more was counted.

[0165] [Production of sputtering targets] The oxide sintered bodies obtained in each of the examples and comparative examples were ground and polished to produce sputtering targets of 4 inches diameter x 5 mm thickness. Specifically, the cut and polished oxide sintered bodies were bonded to a backing plate to produce the sputtering targets. In all targets, the bonding rate was 98% or higher. Furthermore, almost no warping was observed. The bonding rate (bonding rate) was confirmed by X-ray CT.

[0166] Evaluation of sputtering target characteristics (1) Abnormal discharge (sputtering stability) Using the prepared sputtering target, a 400 W (power density: 4.9 W / cm 2 DC sputtering of the sample was carried out continuously for 5 hours. During sputtering, an arcing counter (μ Arc Monitor, manufactured by Landmark Technology Co., Ltd.) was used to determine whether or not abnormal discharge occurred. The arcing counter had the following settings: detection mode: energy, arc detection voltage: 100 V, large-medium energy boundary: 50 mJ, and minimum hard arc time: 100 μs.

[0167] [Manufacturing of Thin Film Transistors] (1) Film Formation Step The oxide sintered bodies obtained in each Example and Comparative Example were ground and polished to manufacture sputtering targets measuring 4 inches in diameter and 5 mm thick. Using the manufactured sputtering targets, a 50 nm thin film (oxide semiconductor layer) was formed on a silicon wafer with a thermal oxide film (gate insulating film) via a metal mask under the following film formation conditions. In this case, sputtering was performed using a mixed gas of high-purity argon and 1% high-purity oxygen as the sputtering gas. A sample in which only a 50 nm thick oxide semiconductor layer was formed on a glass substrate was also manufactured under the same conditions. The glass substrate used was ABC-G manufactured by Nippon Electric Glass Co., Ltd.

[0168] <Film formation conditions> Substrate temperature during film formation: room temperature Back pressure before film formation: 5×10 -4 Pa or less Atmosphere gas: Ar (argon) + O 2 (Oxygen) Oxygen partial pressure during film formation: 1% Sputtering pressure (total pressure) during film formation: 0.5 Pa Direct current (DC) output: 300 W

[0169] (2) Formation of Source and Drain Electrodes Next, titanium metal was sputtered using a metal mask in the shape of source and drain contact holes so that the ratio of the distance to the width (W / L) between the two electrodes of the source electrode and the drain electrode was 200 / 1000, and titanium electrodes were formed as source and drain electrodes. The obtained laminate was heated to 350°C at a heating rate of 10°C / min in the atmosphere, and then heat-treated at 350°C for 60 minutes to produce a thin film transistor (TFT) before the formation of a protective insulating film.

[0170] <Evaluation of TFT characteristics> (1) Linear mobility The protective insulating film (SiO 2 The linear mobility was evaluated for the TFT before the formation of the thin film. The linear mobility was determined from the transfer characteristics when a drain voltage of 0.1 V was applied. Specifically, a graph of the transfer characteristics Id-Vg was created, the transconductance (Gm) for each Vg was calculated, and the mobility was derived using the linear region equation. Gm is expressed as ∂(Id) / ∂(Vg), and Vg was applied from -10 V to 20 V, with the maximum mobility within that range defined as the linear mobility. Unless otherwise specified in the present invention, the linear mobility was evaluated using this method. Id is the current value between the source electrode and the drain electrode, and Vg is the gate voltage when a voltage Vd is applied between the source electrode and the drain electrode.

[0171] (2) Threshold voltage (Vth) The threshold voltage (Vth) is determined by applying Vd = 0.1 V, measuring the Id-Vg characteristics, and determining from the graph of the transfer characteristics Id-Vg that Id = 10 -9 Vg at A was defined.

[0172]

[0173]

[0174]

[0175] 12B, 12C, 12D, 12E, and 12F show the X-ray diffraction patterns of the sintered bodies used in the targets produced in Examples 1, 3, 5, 11, and 13, respectively. As shown in FIGS. 12B to 12F, it can be seen that the sintered bodies contain a crystalline phase having a diffraction peak in the range of incident angle (2θ) observed by X-ray (Cu-Kα ray) diffraction measurement defined in (A) to (K) above.

[0176] From the results shown in Tables 1 to 3, the sintered bodies according to Examples 1 to 14 have atomic ratios of In, Ga, Al, and X elements that satisfy the atomic ratios expressed by formula (1), the atomic ratios expressed by formula (2), and the atomic ratios expressed by formula (3), and further, In 2 O 3 and a crystalline phase (crystalline phase A in the table) having a diffraction peak in the range of incident angles (2θ) observed by X-ray (Cu-Kα ray) diffraction measurement defined in (A) to (K). Therefore, it can be seen that in Examples 1 to 14, oxide sintered bodies were obtained in which the occurrence of color unevenness was reduced and the occurrence of white spots was reduced. On the other hand, the sintered bodies according to Comparative Examples 1 to 7 were unable to achieve both the reduction in the occurrence of color unevenness and the reduction in the occurrence of white spots. Furthermore, from the results shown in Tables 1 to 3, the TFTs according to Examples 1 to 14 had higher linear mobilities than the TFTs according to Comparative Examples 1 to 7, and had threshold voltages in the range of −1.0 V or more and 1.0 V or less. Therefore, it can be seen that the TFTs according to Examples 1 to 14 had high mobility and excellent in-plane uniformity.

[0177] 1, 1A, 1B: oxide sintered body (sputtering target), 1C: oxide sintered body, 3: backing plate, 20: silicon wafer, 30: gate insulating film, 40: oxide thin film, 50: source electrode, 60: drain electrode, 70: interlayer insulating film, 70A: interlayer insulating film, 70B: interlayer insulating film, 81: glass substrate, 83: oxide thin film, 85: SiO 2film, 100: thin film transistor, 100A: thin film transistor, 11: channel layer (oxide thin film), 11A-1: first low resistance region, 11B: semiconductor region, 11A-2: second low resistance region, 21: substrate, 22: buffer layer, 24: gate insulating film, 25: gate electrode, 26: interlayer insulating film, 27: source electrode, 28: drain electrode, 29: protective film, 100B: thin film transistor, 100C: thin film transistor, 300: substrate, 301: pixel portion, 302: first scanning line driving circuit, 303: second scanning line driving circuit, 304: signal line driving circuit, 310: capacitance wiring, 312: gate wiring, 313: gate wiring, 314: drain electrode, 316: transistor, 317: transistor, 318: first liquid crystal element, 319: second Liquid crystal element, 320: pixel portion, 321: switching transistor, 322: driving transistor, 3002: photodiode, 3004: transfer transistor, 3006: reset transistor, 3008: amplification transistor, 3010: signal charge storage portion, 3100: power line, 3110: reset power line, 3120: vertical output line, 501: quantum tunnel field effect transistor, 501A: quantum tunnel field effect transistor, 503: p-type semiconductor layer, 505: silicon oxide layer, 505A: insulating film, 505B: contact hole, 507: n-type semiconductor layer, 509: gate insulating film, 511: gate electrode, 513: source electrode, 515: drain electrode, 519: interlayer insulating film, 519A, 519B: contact holes.

Claims

1. A semiconductor device comprising In (indium), Ga (gallium), Al (aluminum), and a positive trivalent X element as main constituent elements, wherein the X element is one or more elements selected from the group consisting of Sc (scandium), Y (yttrium), La (lanthanum), Pr (praseodymium), Nd (neodymium), Pm (promethium), Sm (samarium), Eu (europium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium), Yb (ytterbium), and Lu (lutetium), and wherein the atomic ratios of the In element, the Ga element, the Al element, and the X element satisfy the following formulas (1) to (3), 2 O 3 and a crystalline phase having a diffraction peak in a range of incident angles (2θ) observed by X-ray (Cu-Kα ray) diffraction measurement specified in the following (A) to (K). 31° to 34°...(A) 36° to 39°...(B) 30° to 32°...(C) 51° to 53°...(D) 53° to 56°...(E) 62° to 66°...(F) 14° to 16°...(G) 19° to 21°...(H) 42° to 45°...(I) 8° to 10°...(J) 17° to 19°...(K) 0.05≦Ga / (In+Ga)≦0.20...(1) 0.015≦(Al+X) / (In+Ga+Al+X)≦0.07...(2) 0.10≦Al / (Al+X)≦0.90 (3) (In the formula, In, Ga, Al, and X represent the number of atoms of indium element, gallium element, aluminum element, and X element in the oxide sintered body, respectively.) 2. The oxide sintered body according to claim 1, wherein 99 atomic % or more of the metal elements contained in the oxide sintered body are the In element, the Ga element, the Al element, and the X element.

3. The oxide sintered body according to claim 1 or 2, wherein the atomic ratio represented by the formula (1) is 0.05 or more and 0.18 or less.

4. The oxide sintered body according to any one of claims 1 to 3, wherein the atomic ratio represented by the formula (1) is 0.05 or more and 0.16 or less.

5. The oxide sintered body according to any one of claims 1 to 4, wherein the atomic ratio represented by the formula (1) is 0.08 or more and 0.10 or less.

6. The oxide sintered body according to any one of claims 1 to 5, wherein the atomic ratio represented by the formula (2) is 0.02 or more and 0.07 or less.

7. The oxide sintered body according to any one of claims 1 to 6, wherein the atomic ratio represented by the formula (2) is 0.02 or more and 0.06 or less.

8. The oxide sintered body according to any one of claims 1 to 7, wherein the atomic ratio represented by the formula (2) is 0.02 or more and 0.05 or less.

9. The oxide sintered body according to any one of claims 1 to 8, wherein the atomic ratio represented by the formula (3) is 0.20 or more and 0.90 or less.

10. The oxide sintered body according to any one of claims 1 to 9, wherein the atomic ratio represented by the formula (3) is 0.30 or more and 0.60 or less.

11. The oxide sintered body according to any one of claims 1 to 10, having a bulk resistivity of 10 mΩ·cm or less.

12. A sputtering target comprising the oxide sintered body according to any one of claims 1 to 11.

13. An oxide thin film formed by using the sputtering target according to claim 12.

14. A thin film transistor comprising the oxide thin film of claim 13.

15. An electronic device comprising the thin film transistor according to claim 14.

Citation Information

Patent Citations

  • Oxide sintered body and sputtering target

    JP2017178740A

  • Oxide sintered body, method for producing same and sputtering target

    WO2015098060A1

  • Novel garnet compound, sintered body containing same, and sputtering target

    WO2018043323A1

  • Amorphous oxide semiconductor film, oxide sintered body, and thin film transistor

    WO2018143280A1

  • Garnet compound, oxide sintered compact, oxide semiconductor thin film, thin film transistor, electronic device and image sensor