Co2 adsorbent-supporting honeycomb structure, method for manufacturing same, and method for recovering co2

The honeycomb structure with an alkali metal carbonate adsorbent layer on zeolite, alumina, or silica addresses the inefficiencies of conventional CO2 recovery methods by enhancing adsorption and desorption rates and stability, achieving efficient CO2 capture with low energy consumption.

WO2024204110A1PCT designated stage expired Publication Date: 2024-10-03NGK INSULATORS LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011776
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional CO2 recovery technologies, such as temperature swing methods using amine-based materials, face challenges like high energy consumption and material degradation, while humidity swing methods using ion exchange resins or graphite face issues like material instability and low desorption capacity.

Method used

A honeycomb structure with an alkali metal carbonate adsorbent layer supported on zeolite, alumina, or silica, which covers the partition walls, allowing for efficient CO2 adsorption and desorption through humidity changes, reducing energy consumption and enhancing adsorption/desorption capacity.

Benefits of technology

The proposed solution effectively captures CO2 with low energy input, improves adsorption/desorption rates, and extends material lifespan by using a stable and efficient adsorbent layer on the honeycomb structure, suitable for CO2 recovery in various environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011776_03102024_PF_FP_ABST
    Figure JP2024011776_03102024_PF_FP_ABST
Patent Text Reader

Abstract

PROBLEM TO BE SOLVED: To provide a honeycomb structure capable of suitably applying a CO2 recovery method by a humidity swing method. This CO2 adsorbent-supporting honeycomb structure comprises: a honeycomb structure portion including partition walls that extend from a first end surface to a second end surface and partition a plurality of cells forming fluid flow paths; and a CO2 adsorbent layer that at least partially covers the surfaces of the partition walls, the CO2 adsorbent layer containing an alkali metal carbonate supported by a porous material containing at least one selected from zeolite, alumina, and silica, the total content of zeolite, alumina, and silica being 50 mass % or more.
Need to check novelty before this filing date? Find Prior Art

Description

CO2 adsorbent-supported honeycomb structure, its manufacturing method, and CO2 recovery method

[0001] The present invention relates to a CO2 adsorbent-supported honeycomb structure and a method for manufacturing the same, and also to a method for recovering CO2 using a CO2 adsorbent-supported honeycomb structure.

[0002] To realize a decarbonized society, there is a growing need for technologies to capture and utilize carbon dioxide (CO2) from the atmosphere and exhaust gases. A typical conventional CO2 capture technology is the temperature swing method, which uses amine-based materials to adsorb CO2 and then heats the material to desorb it. However, the temperature swing method has problems such as high energy consumption per unit of CO2 captured, high cost, and thermal degradation of the amine.

[0003] To solve these problems, the humidity swing method is being developed, in which CO2 is released by exposing an adsorbent that has adsorbed CO2 to a high-humidity environment. The humidity swing method does not require heating of the CO2 adsorbent, so it consumes less energy and is expected to lead to significant reductions in costs and energy consumption. Prior art documents related to the humidity swing method include the following:

[0004] Patent Document 1 (Japanese Patent No. 6204333) describes a technique in which carbon dioxide is absorbed into an absorbent containing a strongly basic ion exchange resin, and then the humidity of the absorbent is increased to release the carbon dioxide from the absorbent.

[0005] Non-Patent Document 1 (Xiaoyang Shi, Hang Xiao, Kohei Kanamori, Akio Yonezu, Klaus S. Lackner, Xi Chen, "Moisture-Driven CO2 Sorbents", Joule 4, 1823-1837, August 19, 2020) describes the adsorption and desorption of CO2 by humidity swing using an adsorbent powder made of porous carbon material (graphite) carrying carbonate.

[0006] Non-Patent Document 2 (Rafael Rodriguez-Mosqueda, Eddy A. Bramer, Gerrit Brem, “CO capture from ambient air using hydrated NaCO supported on activated carbon honeycombs with application to CO enrichment in greenhouses”, Chem. Eng. Sci. 189(2018) 114-122) describes the production of a honeycomb monolith supported on sodium carbonate by wash-coating an activated carbon honeycomb monolith with an aqueous solution of sodium carbonate, and the subsequent CO adsorption / desorption test using a humidity swing.

[0007] Patent No. 6204333

[0008] Xiaoyang Shi, Hang Xiao, Kohei Kanamori, Akio Yonezu, Klaus S. Lackner, Xi Chen, ”Moisture-Driven CO2 Sorbents”, Joule 4, 1823-1837, August 19, 2020Rafael Rodriguez-Mosqueda, Eddy A. Bramer, Gerrit Brem, “CO2 capture from ambient air using hydrated Na2CO3 supported on activated carbon “honeycombs with application to CO2 enrichment in greenhouses”, Chemical Engineering Science 189(2018) 114-122

[0009] However, the technology described in Patent Document 1 uses an ion exchange resin, and there are concerns that cracks may occur in the resin material if humidity swings are repeated to absorb and release CO. In addition, because the material is a resin, there are concerns that it has low resistance to heat and ultraviolet rays, resulting in a short lifespan.

[0010] Non-Patent Document 1 reports an adsorbent that uses more stable graphite. However, in actual adsorption / desorption tests, the amount of CO2 desorbed was small. This is thought to be because graphite is hydrophobic, so it has poor reactivity with H2O, preventing sufficient CO2 desorption. Furthermore, although the test was conducted using powdered graphite, there is still room for improvement in the CO2 adsorption rate.

[0011] In Non-Patent Document 2, an adsorbent in which sodium carbonate is supported on a honeycomb monolith made of activated carbon is used, but the adsorption / desorption capacity is small, and sufficient desorption capacity is not obtained even at 60° C. This is thought to be due to the fact that activated carbon is hydrophobic, and also because the adsorbent is not able to be used inside the partition walls of the honeycomb monolith.

[0012] In view of the above circumstances, an object of the present invention is to provide a honeycomb structure to which a humidity swing CO2 capture method can be suitably applied in one embodiment.An object of the present invention is to provide a method for manufacturing such a honeycomb structure in another embodiment.

[0013] The present inventors have conducted extensive research to solve the above problems and have found that it is advantageous to at least partially cover the surfaces of the partition walls of a honeycomb structure with a layer of a CO adsorbent material containing an alkali metal carbonate supported on a predetermined porous material. The present invention was completed based on the above findings and is exemplified below.

[0014] [Aspect 1] A CO2 adsorbent-supported honeycomb structure comprising: a honeycomb structure portion including partition walls extending from a first end face to a second end face and defining a plurality of cells forming a fluid flow path; and a CO2 adsorbent layer at least partially covering the surfaces of the partition walls, the CO2 adsorbent layer containing an alkali metal carbonate supported on a porous material containing one or more selected from zeolite, alumina, and silica, wherein the total content of the zeolite, alumina, and silica is 50 mass% or more. [Aspect 2] The CO2 adsorbent-supported honeycomb structure according to Aspect 1, wherein the CO2 adsorbent layer has an average thickness of 30 μm to 250 μm. [Aspect 3] The CO2 adsorbent-supported honeycomb structure according to Aspect 1 or 2, wherein the opening ratios of the first end face and the second end face are 35% to 75%. [Aspect 4] The CO2 adsorbent-supported honeycomb structure according to any one of Aspects 1 to 3, wherein the partition walls have a specific heat of 0.6 kJ / (kg K) or more. [Aspect 5] The partition walls have an average thickness of 40 to 440 μm and a cell density of 20 to 200 cells / cm 2 The CO2 adsorbent-supporting honeycomb structure according to any one of Aspects 1 to 4, wherein the opening ratio of the first end face and the second end face is 35% to 75%, the average thickness of the partition walls is 40 to 440 μm, and the cell density is 20 to 200 cells / cm 2A CO2 adsorbent-supported honeycomb structure according to any one of Aspects 1 to 5. [Aspect 7] The CO2 adsorbent-supported honeycomb structure according to any one of Aspects 1 to 6, wherein the partition walls are made of ceramic. [Aspect 8] A method for recovering CO2, comprising the steps of: causing a first gas having a first humidity to flow into the CO2 adsorbent-supported honeycomb structure according to any one of Aspects 1 to 7 from a first end face or a second end face; capturing CO2 in the first gas by the CO2 adsorbent while the first gas passes through the plurality of cells; and causing the first gas with a reduced CO2 concentration to flow out from the end face opposite the inlet side. A CO2 recovery method according to Aspect 8, comprising the steps of: causing a second gas, water, or a mixture thereof having a second humidity higher than the first humidity to flow into the CO2 adsorbent-supported honeycomb structure from a first end face or a second end face; causing CO2 captured in the CO2 adsorbent to be desorbed from the CO2 adsorbent while the second gas, water, or mixture thereof passes through the plurality of cells; and causing the second gas, water, or mixture thereof with an increased CO2 concentration to flow out from the end face opposite to the inlet side. [Aspect 10] The CO2 recovery method according to Aspect 9, wherein the second gas, water, or mixture thereof flowed into the CO2 adsorbent-supported honeycomb structure from the first end face or the second end face has a temperature of 5 to 90°C. Aspect 11: A method for manufacturing a CO2 adsorbent-supported honeycomb structure, comprising: Step A1: preparing a honeycomb structure member having partition walls extending from a first end face to a second end face and defining a plurality of cells that form fluid flow paths; Step A2: preparing a CO2 adsorbent material containing an alkali metal carbonate supported on a porous material containing one or more selected from zeolite, alumina, and silica, wherein the total content of the zeolite, alumina, and silica is 50 mass% or more; and Step A3: at least partially coating surfaces of the partition walls with the CO2 adsorbent. Aspect 12: The method for manufacturing a CO2 adsorbent-supported honeycomb structure according to Aspect 11, wherein Step A3 includes a step of flowing a slurry containing the CO2 adsorbent into the cells from the first end face or the second end face of the honeycomb structure member.[Aspect 13] A method for manufacturing a CO2 adsorbent-supported honeycomb structure, comprising: Step B1 of preparing a honeycomb structure portion having partition walls extending from a first end face to a second end face and defining a plurality of cells that form fluid flow paths; Step B2 of preparing a porous material containing one or more selected from zeolite, alumina, and silica, wherein the total content of zeolite, alumina, and silica is 50 mass% or more; Step B3 of at least partially coating surfaces of the partition walls with the porous material; and Step B4 of supporting an alkali metal carbonate on the porous material at least partially coating the surfaces of the partition walls. [Aspect 14] The method for manufacturing a CO2 adsorbent-supported honeycomb structure according to Aspect 13, wherein Step B3 comprises a step of flowing a slurry containing the porous material into the cells from the first end face or the second end face of the honeycomb structure portion. [Embodiment 15] The method for manufacturing a CO2 adsorbent-supported honeycomb structure according to embodiment 13 or 14, wherein step B4 includes a step of flowing the aqueous solution of the alkali metal carbonate into the cells from the first end face or the second end face of the honeycomb structure portion.

[0015] A CO2 adsorbent-supported honeycomb structure according to one embodiment of the present invention has a layer of CO2 adsorbent containing an alkali metal carbonate supported on a predetermined porous material provided on the surface of the partition walls. This is useful for improving CO2 adsorption and desorption capacity and enabling a high CO2 adsorption rate. Furthermore, the honeycomb structure reduces pressure loss compared to ion exchange resins, which fill the gas flow channels. Therefore, this CO2 adsorbent-supported honeycomb structure is suitable for use in a humidity swing CO2 capture method.

[0016] FIG. 1 is a schematic perspective view of a CO2 adsorbent-supported honeycomb structure according to one embodiment of the present invention. FIG. 2 is a schematic diagram of a cross section parallel to the height direction (cell extension direction) of a CO2 adsorbent-supported honeycomb structure according to one embodiment of the present invention. FIG. 3 is a schematic partially enlarged view of the partition walls and CO2 adsorbent layer of a CO2 adsorbent-supported honeycomb structure according to one embodiment of the present invention, observed in a cross section perpendicular to the cell extension direction. FIG. 4 is a graph showing the relationship between elapsed time and the amount of CO2 desorption when a CO2 adsorbent containing zeolite, silica gel, or activated carbon is used as the porous material. FIG. 5 is a graph showing the relationship between elapsed time and the amount of CO2 adsorption when CO2 is adsorbed using a honeycomb structure supported on a CO2 adsorbent and a powdered CO2 adsorbent. FIG. 6 is a graph showing the relationship between the average thickness of the CO2 adsorbent layer and the amount of CO2 adsorption. FIG. 7 is a graph showing the relationship between the opening ratio of a first end face and a second end face and the amount of CO2 adsorption.

[0017] Next, an embodiment of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiment, and that appropriate design changes and improvements may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0018] (1. CO2 adsorbent material-supported honeycomb structure) Fig. 1 shows a schematic perspective view of a CO2 adsorbent material-supported honeycomb structure according to one embodiment of the present invention. Fig. 2 shows a schematic view of a cross section parallel to the height direction (cell extension direction) of the CO2 adsorbent material-supported honeycomb structure shown in Fig. 1.

[0019] The CO2 adsorbent-supported honeycomb structure 100 according to the embodiment of FIG. 1 includes an outer peripheral sidewall 102 and a honeycomb structure portion including partition walls 112 disposed inside the outer peripheral sidewall 102, extending from a first end face 104 to a second end face 106, and partitioning a plurality of cells 108 that form fluid flow paths. The plurality of cells 108 are arranged parallel to one another. The CO2 adsorbent-supported honeycomb structure 100 according to this embodiment also includes a CO2 adsorbent layer 114 that at least partially covers the surface of the partition walls 112. The CO2 adsorbent-supported honeycomb structure 100 according to this embodiment is a flow-through type in which both ends of each cell 108 are open to the first end face 104 and the second end face 106, and a fluid that flows in through an inlet of a cell passes through the cell and flows out through an outlet of the cell.

[0020] The end face shape of the CO2 adsorbent material-supporting honeycomb structure is not particularly limited, and may be, for example, a circular shape, an elliptical shape, a round shape such as a racetrack shape or an oval shape, a polygonal shape such as a triangular shape or a square shape, or other irregular shapes. The overall outer shape of the CO2 adsorbent material-supporting honeycomb structure may typically be a columnar shape. The CO2 adsorbent material-supporting honeycomb structure 100 shown in Figure 1 has a circular end face shape and is cylindrical as a whole.

[0021] When the CO2 adsorbent-supported honeycomb structure is a columnar structure, its height (the length from the first end face to the second end face) is not particularly limited and may be set appropriately depending on the application and required performance. There is also no particular limit on the relationship between the height of the CO2 adsorbent-supported honeycomb structure and the maximum diameter of each end face (the maximum length of the diameters passing through the center of gravity of each end face of the columnar honeycomb structure). Therefore, the height of the CO2 adsorbent-supported honeycomb structure may be longer than the maximum diameter of each end face, or the height of the CO2 adsorbent-supported honeycomb structure may be shorter than the maximum diameter of each end face.

[0022] There is no particular limitation on the length in the cell extension direction (height direction) of the CO2 adsorbent-supported honeycomb structure. However, while a longer length allows for a larger amount of CO2 adsorbent to be supported, if the length is too long it becomes difficult to coat the cells with the CO2 adsorbent. Therefore, the length is preferably 50 to 300 mm, more preferably 60 to 270 mm, and even more preferably 70 to 250 mm.

[0023] There is no particular limitation on the maximum diameter of each end face of the CO2 adsorbent-supported honeycomb structure. However, while a larger maximum diameter allows for a larger amount of CO2 adsorbent to be supported, if the maximum diameter is too large it becomes difficult to coat with the CO2 adsorbent. Therefore, the maximum diameter is preferably 50 to 250 mm, more preferably 60 to 230 mm, and even more preferably 70 to 200 mm.

[0024] (1-1. Honeycomb Structure Portion) Materials constituting the partition walls and outer peripheral side walls of the honeycomb structure portion of the CO2 adsorbent-supported honeycomb structure include, but are not limited to, ceramics. Examples of ceramics include cordierite, mullite, zircon, zirconium phosphate, aluminum titanate, silicon carbide (SiC), silicon-silicon carbide composites (e.g., Si-bonded SiC), cordierite-silicon carbide composites, zirconia, spinel, indialite, sapphirine, corundum, titania, silicon nitride, alumina, and silica-alumina. These ceramics may be contained singly or in combination of two or more types.

[0025] In a preferred embodiment, the honeycomb structure portion is formed of ceramics containing 90 mass% or more of cordierite. This means that the total mass percentage of cordierite (2MgO.2Al2O3.5SiO2) in 100 mass% of the material constituting the honeycomb structure portion is 90 mass% or more. The mass percentage of cordierite in 100 mass% of the material constituting the honeycomb structure portion is more preferably 95 mass% or more, and even more preferably 99 mass% or more. Excluding unavoidable impurities, it is also possible for 100 mass% of the material constituting the honeycomb structure portion to be cordierite.

[0026] The specific heat of the partition walls and outer peripheral side walls of the honeycomb structure is preferably high. This is because, after supplying moisture into the cells in the CO2 desorption process, when attempting to dry the CO2 adsorbent-supported honeycomb structure, the temperature of the honeycomb structure is lowered by the heat of vaporization, which tends to prolong the drying time. Specifically, the specific heat of the partition walls and outer peripheral side walls of the honeycomb structure is preferably 0.6 kJ / (kg·K) or more, more preferably 0.61 kJ / (kg·K) or more, and even more preferably 0.62 kJ / (kg·K) or more. While no particular upper limit is set for the specific heat of the partition walls and outer peripheral side walls of the honeycomb structure, from the viewpoint of ease of manufacture, it is usually 1 kJ / (kg·K) or less, typically 0.95 kJ / (kg·K) or less, and more typically 0.9 kJ / (kg·K) or less. Therefore, the specific heat of the partition walls and outer peripheral side wall of the honeycomb structure part is preferably 0.6 to 1 kJ / (kg·K), more preferably 0.61 to 0.95 kJ / (kg·K), and even more preferably 0.62 to 0.9 kJ / (kg·K). A method for increasing the specific heat of the partition walls and outer peripheral side wall of the honeycomb structure part includes, for example, using alumina as the material. For example, the partition walls and outer peripheral side wall of a honeycomb structure part made of cordierite can have a specific heat of about 0.7 to 0.8 kJ / (kg·K). The partition walls and outer peripheral side wall of a honeycomb structure part made of a silicon-silicon carbide composite can have a specific heat of about 0.63 to 0.73 kJ / (kg·K). In this specification, the specific heat of the partition walls and outer peripheral side wall of the honeycomb structure part refers to the specific heat at 25°C measured by a differential scanning calorimeter (DSC).

[0027] Although there is no particular limitation on the average thickness of the partition walls, from the viewpoint of ensuring strength, it is preferably 40 μm or more, more preferably 45 μm or more, and even more preferably 50 μm or more. Furthermore, from the viewpoint of suppressing pressure loss and increasing the amount of CO adsorbent supported, the average thickness of the partition walls is preferably 440 μm or less, more preferably 390 μm or less, and even more preferably 310 μm or less. Therefore, the average thickness of the partition walls is, for example, preferably 40 to 440 μm, more preferably 45 to 390 μm, and even more preferably 50 to 310 μm.

[0028] 3 shows a schematic partial enlarged view of the partition walls 112 and the CO2 adsorbent layer 114 of the CO2 adsorbent material-supported honeycomb structure 100 when observed in a cross section perpendicular to the extension direction of the cells 108. In this specification, the thickness of the partition walls 112 refers to the length D of a line segment L that crosses the partition walls 112 when the line segment L connects the centers of gravity C of adjacent cells 108 in a cross section perpendicular to the extension direction of the cells 108 (the height direction if the CO2 adsorbent material-supported honeycomb structure is a columnar shape). In this specification, the average thickness of the partition walls 112 refers to the average value of the thicknesses of all the partition walls 112 of the CO2 adsorbent material-supported honeycomb structure.

[0029] The partition walls can be porous. When the partition walls are porous, the average pore diameter thereof is preferably 0.5 μm or more, more preferably 0.7 μm or more, and even more preferably 1 μm or more, from the viewpoint of improving adhesion with the CO adsorbent layer. Furthermore, the average pore diameter of the partition walls is preferably 60 μm or less, more preferably 55 μm or less, and even more preferably 50 μm or less, from the viewpoint of ensuring strength. Therefore, the average pore diameter of the partition walls is, for example, preferably 0.5 to 60 μm, more preferably 0.7 to 55 μm, and even more preferably 1 to 50 μm.

[0030] In this specification, the average pore diameter is measured by mercury intrusion porosimetry in accordance with JIS R1655:2003 using a mercury porosimeter. Mercury intrusion porosimetry is a method in which a sample is immersed in mercury under vacuum and a uniform pressure is applied, mercury is forced into the sample while the pressure is gradually increased, and the pore size distribution is calculated from the pressure and the volume of mercury forced into the pores. As the pressure is gradually increased, mercury is forced into pores starting from the larger diameter pores, increasing the cumulative volume of mercury. When all pores are finally filled with mercury, the cumulative volume reaches an equilibrium amount. The cumulative volume at this time is called the total pore volume (cm 3 / g), and the pore diameter (D50) at the time when mercury is intruded into the pores at a volume that is 50% of the total pore volume is defined as the average pore diameter.

[0031] When the partition walls are porous, the porosity of the partition walls is preferably 5% or more, more preferably 10% or more, and even more preferably 15% or more, from the viewpoint of ensuring the amount of CO adsorbent supported and from the viewpoint of keeping the pressure loss low when a fluid is passed through the cells. Furthermore, the porosity of the partition walls is preferably 75% or less, more preferably 70% or less, and even more preferably 65% ​​or less, from the viewpoint of ensuring the strength of the honeycomb structure. Therefore, the porosity of the partition walls is, for example, preferably 5 to 75%, more preferably 10 to 70%, and even more preferably 15 to 65%. In this specification, the porosity is measured by mercury intrusion porosimetry using a mercury porosimeter in accordance with JIS R1655:2003.

[0032] There is no particular restriction on the cell density (the number of cells per unit cross-sectional area), but from the viewpoint of improving the contact area between the adsorbent on the partition wall and the gas being vented, it is preferable that the cell density be 20 cells / cm. 2 Preferably, the number of cells is 25 or more. 2 More preferably, 30 cells / cm or more. 2 From the viewpoint of ensuring a gas flow path and reducing pressure loss, the cell density is preferably 200 cells / cm. 2 Preferably, the number of cells per square centimeter is 195 cells / cm or less. 2 More preferably, it is 190 cells / cm or less.2 Therefore, the cell density is, for example, 20 to 200 cells / cm. 2 Preferably, the density is 25 to 195 cells / cm 2 More preferably, it is 30 to 190 cells / cm 2 In this specification, the cell density is calculated by dividing the number of cells in the honeycomb structure part by the area of ​​one end face of the honeycomb structure part excluding the outer peripheral side wall.

[0033] Although there are no limitations on the shape of the cells in a cross section perpendicular to the cell extension direction (height direction of the honeycomb structure), a quadrangle, a hexagon, an octagon, or a combination thereof is preferred. Among these, a square and a hexagon are preferred. By using such a cell shape, pressure loss when a fluid is passed through the honeycomb structure is reduced.

[0034] From the viewpoint of increasing the utilization rate of the CO2 adsorbent, a larger open area ratio (OFA) of the first end face and the second end face is advantageous. Therefore, the lower limit of the open area ratio of the first end face and the second end face of the CO2 adsorbent-supported honeycomb structure is preferably 35% or more, more preferably 40% or more, even more preferably 50% or more, and even more preferably 60% or more. Furthermore, by increasing the open area ratio (OFA), it is possible to reduce pressure loss when a fluid is flowed through the cells. However, from the viewpoint of ensuring the strength of the CO2 adsorbent-supported honeycomb structure and ensuring the CO2 adsorption / desorption capacity per volume, the upper limit of the open area ratio of the first end face and the second end face is preferably 75% or less, more preferably 70% or less. Therefore, the open area ratio of the first end face and the second end face is preferably 35 to 75%, more preferably 40 to 75%, even more preferably 50 to 70%, and even more preferably 60 to 70%. In this specification, the aperture ratio of the first end face and the second end face of a CO2 adsorbent-supported honeycomb structure is determined by the following method. Optical microscope photographs (field of view size: 6.1 mm × 4.6 mm, magnification: 50x) of the first end face and the second end face of the CO2 adsorbent-supported honeycomb structure are taken at five locations on each end face without bias. Each optical microscope photograph is binarized by image processing, and the area of ​​only the cell openings is calculated. This is then divided by the area of ​​one field of view to determine the aperture ratio for each microscope photograph. The average aperture ratio for all microscope photographs is taken as the measured value. Note that the aperture ratio is measured taking into account the adsorbent layer. Therefore, for example, as the thickness of the adsorbent layer increases, the cell openings become smaller and the aperture ratio also decreases.

[0035] (1-2. CO2 Adsorbent Layer) In one embodiment, the CO2 adsorbent layer 114, which at least partially covers the surface of the partition wall 112, contains one or more selected from zeolite, alumina, and silica, and contains an alkali metal carbonate supported on a porous material having a total content of zeolite, alumina, and silica of 50% by mass or more. Zeolite, alumina, and silica have a higher affinity for water than carbon, which promotes the CO2 desorption reaction even at low temperatures. Therefore, the CO2 adsorbent layer 114 contains a porous material having a total content of zeolite, alumina, and silica of 50% by mass or more, which contributes to improving the adsorption and desorption capacity during humidity swings. The porous material may contain only one of zeolite, alumina, and silica, or a combination of two or three of them.

[0036] The total content of zeolite, alumina, and silica in the porous material is more preferably 70% by mass or more, even more preferably 90% by mass or more, and can be 99% by mass or more (e.g., 100% by mass excluding unavoidable impurities).

[0037] The composition of the CO2 adsorbent layer can be determined based on the material composition when the material composition used to form the adsorbent layer is known. However, if the material composition is unknown, approximately 0.1 to 0.5 g of a powdered sample of the adsorbent layer is collected and analyzed using an X-ray diffractometer (XRD, X-ray source: CuKα radiation), and identified and quantified using ICDD data. Zeolite is analyzed by XRD using a standard sample prepared by mixing 90% by mass of the powdered adsorbent layer sample with 10% by mass of Si powder. The XRD analysis results are compared with the results of XRD analysis of a powder sample (90% by mass of pure zeolite + 10% by mass of Si powder) prepared separately for comparison. Aluminum and silicon are quantitatively analyzed using a calibration curve method with inductively coupled plasma atomic emission spectroscopy (ICP-AES), quantifying aluminum as alumina and silicon as silica (excluding the amount of zeolite previously quantified).

[0038] Specific examples of alkali metal carbonates include one or more selected from potassium carbonate, sodium carbonate, lithium carbonate, rubidium carbonate, cesium carbonate, and francium carbonate. Among these, it is preferable to use one or two selected from potassium carbonate and sodium carbonate because they have high solubility in water and a small ionic radius, making them less likely to clog the pores of the base material even when the loading is increased. Alkali metal carbonates can efficiently chemically adsorb CO2 in the presence of water vapor. For example, when sodium carbonate (Na2CO3) is used as the alkali metal carbonate, CO2 is chemically adsorbed according to the reaction formula: Na2CO3 + H2O + CO2 → 2NaHCO3. Furthermore, the equilibrium of NaHCO3 shifts in the presence of a large amount of water vapor or water, releasing CO2 according to the reaction formula: 2NaHCO3 → Na2CO3 + H2O + CO2, allowing for concentrated recovery of CO2.

[0039] The average thickness of the CO2 adsorbent layer 114 is not limited, but is preferably 30 μm or more, more preferably 35 μm or more, and even more preferably 40 μm or more, from the viewpoint of increasing the amount of CO2 adsorbent per volume of the CO2 adsorbent-supported honeycomb structure. However, if the CO2 adsorbent layer is too thick, gas diffusion within the adsorbent layer takes time, which tends to decrease the CO2 adsorption rate per unit mass of the CO2 adsorbent and the CO2 adsorption rate per unit volume of the honeycomb structure. For this reason, the average thickness of the CO2 adsorbent layer 114 is preferably 250 μm or less, more preferably 230 μm or less, and even more preferably 200 μm or less. Therefore, the average thickness of the CO2 adsorbent layer 114 is preferably 30 μm to 250 μm, more preferably 35 μm to 230 μm, and even more preferably 40 μm to 200 μm.

[0040] In this specification, the average thickness of the CO2 adsorbent layer 114 is measured by the following method. First, cross sections perpendicular to the cell extension direction of the CO2 adsorbent-supported honeycomb structure 100 are cut out at 1 / 4, 1 / 2, and 3 / 4 of the length in the cell extension direction. Cutting out one section results in two cross sections, and either one of the cross sections can be used. Next, three locations near the center of gravity of each of the three cross sections cut out at 1 / 4, 1 / 2, and 3 / 4 of the length in the cell extension direction are photographed using an optical microscope (field of view size: 6.1 mm × 4.6 mm, magnification: 50x). The thickness of the CO2 adsorbent layer 114 is measured at five random locations in each field of view. The thickness T of the CO2 adsorbent layer 114 at one location is defined as the length of either of the CO2 adsorbent layer 114 at two locations intersected by a line segment L when the line segment L connects the centers of gravity C of adjacent cells 108 ( FIG. 3 ). The average value of the thicknesses of all the CO2 adsorbent layer 114 measured at the three cross sections is defined as the measured value.

[0041] It is sufficient that the CO adsorbent layer 114 at least partially covers the surface of the partition wall 112. However, from the viewpoint of increasing the amount of CO adsorbent per volume of the CO adsorbent-supported honeycomb structure, it is preferable that the surface area ratio of the partition wall 112 covered with the CO adsorbent material is large. Specifically, this area ratio is preferably 40% or more, more preferably 60% or more, even more preferably 80% or more, and most preferably 100%.

[0042] In this specification, the surface area ratio of the partition walls 112 coated with the CO adsorbent is measured by the following method. First, cross sections perpendicular to the cell extension direction of the CO adsorbent-supported honeycomb structure 100 are cut out at ¼, ½, and ¾ of the length in the cell extension direction. Cutting out one section results in two cross sections, and either one of the cross sections can be used. Next, three locations near the centers of gravity of each of the three cross sections cut out at ¼, ½, and ¾ of the length in the cell extension direction are photographed using an optical microscope (field size: 6.1 mm × 4.6 mm, magnification: 50x). In each field of view, the total length of the sides of the surface of the partition walls 112 that partition any five cells 108 is measured, and the total value (total partition wall side length) is calculated. Next, of the surfaces of the partition walls 112 that separate the five cells 108, the lengths of all the sides of the surfaces of the partition walls 112 that are coated with a CO adsorbent layer are measured, and the total value (total coated partition wall side length) is calculated. Next, the total coated partition wall side length / total partition wall side length × 100 (%) is calculated, and this is regarded as the area ratio of the partition wall surface that is coated with the CO adsorbent material in each field of view. Then, the average value of the area ratio in all fields of view measured in the three cross sections is taken as the measured value for the entire CO adsorbent-supported honeycomb structure.

[0043] (2. CO2 Capture Method) According to one embodiment of the present invention, there is provided a CO2 capture method using the CO2 adsorbent material-supported honeycomb structure according to the embodiment described above. The CO2 adsorbent material-supported honeycomb structure according to the embodiment described above includes a layer of CO2 adsorbent material containing alkali metal carbonate supported on a porous material, as described above. The alkali metal carbonate supported on the porous material has the property of adsorbing CO2 in a low-humidity environment and desorbing CO2 in a high-humidity environment, and therefore the CO2 adsorbent material-supported honeycomb structure is suitably applicable to a CO2 capture method using a humidity swing system.

[0044] Therefore, according to one embodiment of the present invention, there is provided a CO2 recovery method including the steps of: causing a first gas having a first humidity to flow in from the first end face 104 or the second end face 106 of the CO2 adsorbent-supported honeycomb structure 100 according to the embodiment described above; capturing CO2 in the first gas by the CO2 adsorbent while the first gas passes through a plurality of cells 108; and causing the first gas with a reduced CO2 concentration to flow out from the end face opposite the inlet side.

[0045] The first gas is not particularly limited as long as it contains CO2, and examples thereof include environmental air (outdoor air as well as indoor air), factory exhaust gas, ship exhaust gas, and power plant exhaust gas.

[0046] From the viewpoint of efficiently adsorbing CO2, the first humidity of the first gas is preferably 0 to 50% relative humidity (RH), more preferably 3 to 45%, and even more preferably 5 to 40%. Also, from the viewpoint of efficiently adsorbing CO2, the temperature of the first gas is preferably 0 to 90°C, more preferably 5 to 85°C, and even more preferably 10 to 80°C.

[0047] Furthermore, according to one embodiment of the present invention, the process includes a step of allowing a second gas, water, or a mixture thereof having a second humidity higher than the first humidity to flow into the first end face 104 or the second end face 106 of the CO2 adsorbent-supported honeycomb structure 100 according to the embodiment described above, desorbing the CO2 captured in the CO2 adsorbent from the CO2 adsorbent while the second gas, water, or mixture thereof passes through the multiple cells 108, and allowing the second gas, water, or mixture thereof with an increased CO2 concentration to flow out from the end face opposite the inlet side.

[0048] The second gas having a second humidity higher than the first humidity is not particularly limited, and examples thereof include inert gases such as nitrogen, argon, and helium containing water vapor. The inert gas containing water vapor can be obtained by passing the inert gas through water. Because O inhibits the reaction when CO is used, the O concentration in the second gas is preferably 2% by volume or less, more preferably 1% by volume or less, and even more preferably 0% by volume. Examples of water include liquid water, water vapor, or a combination thereof. For example, low-temperature waste steam from a factory, such as waste steam at 90°C or less, can be used. The second gas and water may be used in combination.

[0049] From the viewpoint of sufficiently desorbing CO2, the second humidity of the second gas is preferably 50 to 100% relative humidity (RH), more preferably 55 to 100%, and even more preferably 60 to 100%. Furthermore, from the viewpoint of increasing the saturated vapor pressure and efficiently desorbing CO2, the temperature of the second gas, water, or a mixture thereof is preferably 5°C or higher, more preferably 10°C or higher, and even more preferably 15°C or higher. Furthermore, from the viewpoint of energy conservation, the temperature of the second gas, water, or a mixture thereof is preferably 90°C or lower, more preferably 85°C or lower, and even more preferably 80°C or lower. Therefore, the temperature of the second gas, water, or a mixture thereof is preferably 5 to 90°C, more preferably 10 to 85°C, and even more preferably 15 to 85°C.

[0050] Although the CO2 recovery method using the humidity swing method has been described in detail here, the CO2 adsorbent-supported honeycomb structure according to the above-described embodiment can also be applied to a CO2 recovery method using the temperature swing method, and there is no problem in implementing a CO2 recovery method using the temperature swing method.

[0051] (3. Manufacturing Method of CO2 Adsorbent Material-Supported Honeycomb Structure) A preferred example of a manufacturing method of a CO2 adsorbent material-supported honeycomb structure according to the present invention will be described below. In one embodiment, the manufacturing method of a CO2 adsorbent material-supported honeycomb structure according to the present invention includes the steps of: Step A1 of preparing a honeycomb structure part having partition walls extending from a first end face to a second end face and defining a plurality of cells that form fluid flow paths; Step A2 of preparing a CO2 adsorbent material containing an alkali metal carbonate supported on a porous material that contains one or more selected from zeolite, alumina, and silica, and has a total content of zeolite, alumina, and silica of 50 mass% or more; and Step A3 of at least partially coating the surfaces of the partition walls with the CO2 adsorbent material.

[0052] (Step A1) In step A1, a honeycomb structure part is prepared, which includes partition walls extending from a first end face to a second end face and partitioning a plurality of cells that form a fluid flow path. Such a honeycomb structure part itself may be manufactured by any known manufacturing method, but below, a manufacturing method for a ceramic honeycomb structure part will be described as an example.

[0053] In one embodiment, a method for manufacturing a ceramic honeycomb structure includes a step of manufacturing a honeycomb formed body having an outer peripheral side wall and partition walls arranged inside the outer peripheral side wall and dividing a plurality of cells extending from a first end face to a second end face, and a step of sequentially drying, degreasing, and firing the honeycomb formed body.

[0054] The honeycomb molded body can be produced by kneading a raw material composition containing ceramic raw materials, a dispersion medium, a pore-forming material, and a binder to form a puddle, and then extruding the puddle. Additives such as dispersants can be blended into the raw material composition as needed. During extrusion molding, a die having the desired overall shape, cell shape, partition wall thickness, cell density, etc. can be used.

[0055] The ceramic raw material is the raw material for the portion remaining after firing that constitutes the skeleton of the honeycomb structure as ceramic. The ceramic raw material can be provided, for example, in the form of a powder. Examples of the ceramic raw material include raw materials for obtaining ceramics, such as cordierite, mullite, zircon, zirconium phosphate, aluminum titanate, silicon carbide (SiC), silicon-silicon carbide composites (e.g., Si-bonded SiC), cordierite-silicon carbide composites, zirconia, spinel, indialite, sapphirine, corundum, titania, silicon nitride, alumina, and silica-alumina. Specific examples include, but are not limited to, silica, talc, aluminum hydroxide, alumina, kaolin, serpentine, pyroferrite, brucite, boehmite, mullite, and magnesite. The ceramic raw material may be used singly or in combination of two or more types.

[0056] The pore-forming material is not particularly limited as long as it forms pores after firing, and examples thereof include wheat flour, starch, foamed resin, water-absorbent resin, silica gel, carbon (e.g., graphite), ceramic balloons, polyethylene, polystyrene, polypropylene, nylon, polyester, acrylic, and phenol. One type of pore-forming material may be used alone, or two or more types may be used in combination. From the viewpoint of increasing the porosity of the honeycomb structure, the content of the pore-forming material is preferably 0.5 parts by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass, per 100 parts by mass of the ceramic raw materials. From the viewpoint of ensuring the strength of the honeycomb structure, the content of the pore-forming material is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 4 parts by mass or less, per 100 parts by mass of the ceramic raw materials.

[0057] Examples of binders include organic binders such as methyl cellulose, hydroxypropoxyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, and polyvinyl alcohol. In particular, it is preferable to use a combination of methyl cellulose and hydroxypropoxyl cellulose. Furthermore, from the viewpoint of increasing the strength of the honeycomb formed body, the binder content is preferably 4 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 6 parts by mass or more, per 100 parts by mass of the ceramic raw materials. From the viewpoint of suppressing cracks due to abnormal heat generation during the firing process, the binder content is preferably 9 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 7 parts by mass or less, per 100 parts by mass of the ceramic raw materials. The binder may be used alone or in combination of two or more types.

[0058] The dispersant may be a surfactant such as ethylene glycol, dextrin, fatty acid soap, or polyalcohol. One type of dispersant may be used alone, or two or more types may be used in combination. The content of the dispersant is preferably 0 to 2 parts by mass per 100 parts by mass of the ceramic raw material.

[0059] Examples of the dispersion medium include water and a mixed solvent of water and an organic solvent such as alcohol, with water being particularly preferred.

[0060] The water content of the honeycomb formed body before the drying step is preferably 20 to 90 parts by mass, more preferably 60 to 85 parts by mass, and even more preferably 70 to 80 parts by mass, per 100 parts by mass of the ceramic raw materials. When the water content of the honeycomb formed body is 20 parts by mass or more per 100 parts by mass of the ceramic raw materials, the advantage of the quality of the honeycomb formed body being easily stabilized is easily obtained. When the water content of the honeycomb formed body is 90 parts by mass or less per 100 parts by mass of the ceramic raw materials, the amount of shrinkage during drying is small, and deformation can be suppressed. In this specification, the water content of the honeycomb formed body refers to the value measured by the loss on drying method.

[0061] After drying the honeycomb formed body, degreasing and firing are performed to obtain a honeycomb structure part. The conditions for the drying process, degreasing process and firing process may be well known conditions depending on the material composition of the honeycomb formed body, and no particular explanation is required, but specific examples of conditions are given below.

[0062] In the drying step, a conventionally known drying method can be used, for example, hot air drying, microwave drying, dielectric drying, reduced pressure drying, vacuum drying, freeze drying, etc. Among them, a drying method that combines hot air drying with microwave drying or dielectric drying is preferred, since it can dry the entire molded body quickly and uniformly.

[0063] Next, the degreasing step will be described. The combustion temperature of the binder is about 200°C, and the combustion temperature of the pore-forming material is about 300 to 1000°C. Therefore, the degreasing step can be carried out by heating the honeycomb formed body to a temperature in the range of about 200 to 1000°C. The heating time is not particularly limited, but is usually about 10 to 100 hours. The honeycomb formed body after the degreasing step is called a calcined body.

[0064] The firing step may be carried out by heating the calcined body to 1350 to 1600° C. and holding the calcined body for 3 to 10 hours, although this depends on the material composition of the honeycomb formed body.

[0065] (Step A2) In step A2, a CO2 adsorbent containing an alkali metal carbonate supported on a porous material containing one or more selected from zeolite, alumina, and silica, with the total content of zeolite, alumina, and silica being 50 mass% or more, is prepared. The porous material may contain only one of zeolite, alumina, and silica, or may contain two or three of these in combination. The porous zeolite may be provided in the form of, but is not limited to, a powder, having an average pore diameter of 0.1 to 2 nm and a BET specific surface area of ​​30 to 1500 m. 2 / g, and a median diameter (D50) of 0.1 to 200 μm. The average pore diameter is 0.15 to 1.8 nm, and the BET specific surface area is 40 to 1400 m. 2 / g, and a median diameter (D50) of 0.5 to 100 μm are more preferably used. The average pore diameter is 0.2 to 1.5 nm, and the BET specific surface area is 50 to 1300 m 2 The porous alumina may be provided in the form of, for example, a powder, and has an average pore size of 0.5 to 100 nm and a BET specific surface area of ​​1 to 1000 m. 2 / g, and a median diameter (D50) of 0.1 to 200 μm. The average pore diameter is 0.7 to 90 nm, and the BET specific surface area is 3 to 950 m. 2 / g, and a median diameter (D50) of 0.5 to 100 μm are more preferably used. The average pore diameter is 1 to 80 nm, and the BET specific surface area is 5 to 900 m. 2 The porous silica may be provided in the form of, for example, a powder, and has an average pore size of 0.5 to 100 nm and a BET specific surface area of ​​30 to 1500 m. 2 / g, and a median diameter (D50) of 0.1 to 200 μm. The average pore diameter is 0.7 to 90 nm, and the BET specific surface area is 40 to 1400 m. 2 / g, and a median diameter (D50) of 0.5 to 100 μm are more preferably used. The average pore diameter is 1 to 80 nm, and the BET specific surface area is 50 to 1300 m. 2 / g and a median diameter (D50) of 0.7 to 80 μm can be used even more preferably. Silica gel is preferably used as the porous silica.

[0066] In this specification, the average pore diameter (L) of a porous material is calculated from the BET specific surface area (A) calculated by a multipoint method using the BET equation from the nitrogen gas adsorption isotherm and the pore volume (V) calculated by BJH analysis, using the relational equation L = 4V / A. In this specification, the BET specific surface area of ​​a porous material is calculated from the nitrogen gas adsorption isotherm by a multipoint method using the BET equation. In this specification, the median diameter (D50) of a porous material is determined from the volume-based cumulative particle size distribution obtained by laser diffraction / scattering method.

[0067] One method for supporting an alkali metal carbonate on a porous material is, for example, to stir and mix a powder of the porous material with an aqueous solution of the alkali metal carbonate to form a slurry, and then dry the resulting slurry. Examples of drying methods include vacuum drying. The drying temperature is not particularly limited, but can be set to 20 to 200°C. After drying, a CO2 adsorbent containing the alkali metal carbonate supported on the porous material is obtained.

[0068] The mass ratio of the alkali metal carbonate to the porous material in the CO adsorbent can be, for example, alkali metal carbonate:porous material = 0.5:10 to 7:10, preferably 0.7:10 to 6.5:10, and more preferably 1:10 to 6:10.

[0069] (Step A3) In step A3, the partition wall surfaces of the honeycomb structure section are at least partially coated with a CO2 adsorbent. Examples of such coating methods include preparing a slurry containing the CO2 adsorbent by dispersing the CO2 adsorbent in a solvent, contacting the slurry with the partition wall surfaces, and then drying the slurry. Alcohols such as ethanol, isopropanol, and butanol, as well as other organic solvents, can be suitably used as the solvent. Examples of methods for contacting the slurry with the partition wall surfaces include immersing the honeycomb structure section in the slurry, causing the slurry to flow into the cells from the first end face or the second end face of the honeycomb structure section. Examples of drying methods include vacuum drying. The drying temperature is not particularly limited, but can be set to 20 to 200°C.

[0070] In another embodiment, the method for manufacturing a CO2 adsorbent-supported honeycomb structure according to the present invention includes the steps of: step B1 of preparing a honeycomb structure portion having partition walls extending from a first end face to a second end face and separating a plurality of cells that form a fluid flow path; step B2 of preparing a porous material containing one or more selected from zeolite, alumina, and silica, wherein the total content of zeolite, alumina, and silica is 50 mass% or more; step B3 of at least partially coating the surfaces of the partition walls with the porous material; and step B4 of loading an alkali metal carbonate onto the porous material at least partially coating the surfaces of the partition walls.

[0071] (Step B1) Step B1 is the same as step A1 described above, and therefore a description thereof will be omitted.

[0072] (Step B2) In step B2, a porous material containing one or more selected from zeolite, alumina, and silica, and having a total content of zeolite, alumina, and silica of 50 mass% or more is prepared. The porous material can be suitably the porous material described in step A2.

[0073] (Step B3) In step B3, the surfaces of the partition walls of the honeycomb structure section are at least partially coated with a porous material. Examples of such coating methods include a method in which the porous material is stirred and dispersed in a solvent to prepare a slurry containing the porous material, and the slurry is brought into contact with the surfaces of the partition walls, and then the slurry is dried. Suitable solvents include alcohols such as ethanol, isopropanol, and butanol, as well as other organic solvents, and water. Examples of methods for bringing the slurry into contact with the surfaces of the partition walls include a method in which the honeycomb structure section is immersed in the slurry, and the slurry flows into the cells from the first end face or the second end face of the honeycomb structure section. Examples of drying methods include vacuum drying. The drying temperature is not particularly limited, but can be set to 20 to 200°C.

[0074] (Step B4) In step B4, an alkali metal carbonate is supported on the porous material at least partially covering the surfaces of the partition walls of the honeycomb structure section. For example, a method of supporting the alkali metal carbonate on the porous material includes contacting the surfaces of the partition walls with an aqueous solution of the alkali metal carbonate and then drying the aqueous solution. For example, a method of contacting the surfaces of the partition walls with the aqueous solution includes immersing the honeycomb structure section in the aqueous solution, causing the aqueous solution to flow into the cells from the first end face or the second end face of the honeycomb structure section. For example, a vacuum drying method is used as the drying method. The drying temperature is not particularly limited, but can be set to 20 to 200°C. After drying, a CO2 adsorbent containing the alkali metal carbonate supported on the porous material is obtained.

[0075] The mass ratio of the alkali metal carbonate to the porous material in the CO adsorbent can be, for example, alkali metal carbonate:porous material = 0.5:10 to 7:10, preferably 0.7:10 to 6.5:10, and more preferably 1:10 to 6:10.

[0076] The following examples are provided to provide a better understanding of the present invention and its advantages, but the present invention is not limited to these examples.

[0077] <Test I. Test on the effect of the type of porous material on the amount of CO desorption> (1. Preparation of honeycomb structure) For laboratory tests, a sufficient number of flow-through honeycomb structures, each of which was made of cordierite and had a rectangular parallelepiped shape of 20 mm x 20 mm x height (cell extension length) of 10 mm and open at both ends, were prepared for use in each of the following tests. The honeycomb structure had an average partition wall thickness of 10 mil (254 μm), an average pore diameter of 11 μm, a partition wall porosity of 56%, and a cell density of 300 cells / in. 2 (47 cells / cm 2 The cross-sectional shape of the cells of the honeycomb structure part was square. The specific heat of the honeycomb structure part was 0.76 kJ / (kg·K).

[0078] (2. Preparation of CO2 adsorbent) The following three types of porous materials (commercially available products) were prepared: (a) Zeolite: average pore diameter of 0.9 nm, BET specific surface area of ​​630 m 2 / g, median diameter (D50) is 6 μm, content is 95 wt% or more (b) Silica gel: average pore diameter is 6.0 nm, BET specific surface area is 500 m 2 / g, median diameter (D50) 10 μm, content 100 wt% (c) Activated carbon: average pore diameter 3.0 nm, BET specific surface area 1500 m 2 / g, median diameter (D50) not measured, content 100% by weight

[0079] [2-1. Preparation of CO2 adsorbent A] 12 mL of a 1 M Na2CO3 aqueous solution was added dropwise to 10 g of the above zeolite, and the mixture was stirred to form a slurry, which was then vacuum-dried at room temperature for 72 hours to obtain a powdered CO2 adsorbent A. The mass ratio of Na2CO3 to zeolite in CO2 adsorbent A was Na2CO3:zeolite = 1.3:10.

[0080] [2-2. Preparation of CO2 adsorbent B] 12 mL of a 1 M aqueous Na2CO3 solution was added dropwise to 10 g of the above silica gel, and the mixture was stirred to form a slurry, which was then vacuum dried at room temperature for 72 hours to obtain a powdered CO2 adsorbent B. The mass ratio of Na2CO3 to silica gel in CO2 adsorbent B was Na2CO3:silica gel = 1.3:10.

[0081] [2-3. Preparation of CO2 adsorbent C] 12 mL of a 1 M Na2CO3 aqueous solution was added dropwise to 10 g of the above activated carbon, and the mixture was stirred to form a slurry, which was then vacuum dried at room temperature for 72 hours to obtain a powdered CO2 adsorbent C. The mass ratio of Na2CO3 to activated carbon in the CO2 adsorbent C was Na2CO3:silica gel = 1.3:10.

[0082] (3. Fabrication of a honeycomb structure supporting a CO2 adsorbent) [3-1. Fabrication of a honeycomb structure A supporting a CO2 adsorbent A] The CO2 adsorbent A prepared above was added to ethanol to a concentration of 20% by mass, and the mixture was stirred to form a slurry. The honeycomb structure obtained above was immersed in the slurry, removed after 1 minute, and vacuum dried at room temperature for 24 hours. The same immersion and drying process was then repeated to fabricate a honeycomb structure A supporting a CO2 adsorbent A. The average thickness of the CO2 adsorbent A layer was 46 μm. The surface area ratio of the partition walls covered with the CO2 adsorbent A was 97%. The amount of CO2 adsorbent A supported by the honeycomb structure A was approximately 0.5 g. The honeycomb structure A had an opening ratio of 58% at the first end face and the second end face. [3-2.

[0046] 3-3. Preparation of Honeycomb Structure B Supporting CO2 Adsorbent B] The CO2 adsorbent B prepared above was added to ethanol to a concentration of 20% by mass, and the mixture was stirred to form a slurry. The honeycomb structure obtained above was immersed in the slurry, removed after 1 minute, and vacuum-dried at room temperature for 24 hours. The same immersion and drying process was then repeated to prepare a honeycomb structure B supporting CO2 adsorbent B. The average thickness of the CO2 adsorbent B layer was 52 μm. The surface area ratio of the partition walls covered with CO2 adsorbent B was 96%. The amount of CO2 adsorbent B supported on the honeycomb structure B was approximately 0.5 g. The honeycomb structure B had an opening ratio of 57% at the first end face and the second end face.

[0047] 3-3. Preparation of Honeycomb Structure C Supporting CO2 Adsorbent C] The CO2 adsorbent C prepared above was added to ethanol to a concentration of 20% by mass, and the mixture was stirred to form a slurry. The honeycomb structure part obtained above was immersed in the slurry, pulled out after 1 minute, and vacuum dried at room temperature for 24 hours. The same immersion and drying process was then repeated to produce a honeycomb structure C supporting CO2 adsorbent C. The average thickness of the CO2 adsorbent C layer was 56 μm. The area ratio of the partition wall surface covered by CO2 adsorbent C was 95%. The amount of CO2 adsorbent C supported on the honeycomb structure C was approximately 0.5 g. The honeycomb structure C had an opening ratio of 56% at the first end face and the second end face.

[0083] (4. CO2 adsorption / desorption test) A CO2 adsorption / desorption test was performed on each of the honeycomb structures A, B, and C obtained above using the following test equipment. The test equipment had a 12-liter chamber equipped with an air inlet, an air outlet, a fan, a CO2 concentration meter, and a thermo-hygrometer. An air circulation system was connected to this chamber, and the piping was configured so that air flowing into the chamber from the air inlet passed through the chamber, then flowed out from the air outlet, and was then pumped back into the chamber by a circulation pump. A humidifier and a dehumidifier were installed in parallel in the circulation system, making it possible to switch the humidity of the air flowing into the chamber.

[0084] The test procedure was as follows: A honeycomb structure to be tested was placed in a chamber. With a fan rotating at 5 W to agitate the air in the chamber, humidified air with a relative humidity of 90% or higher and a temperature of approximately 27°C was circulated through the chamber at a flow rate of 12 L / min using a circulation pump, allowing CO2 to be desorbed from the honeycomb structure for 30 minutes (first desorption treatment). Next, with a fan rotating at 5 W to agitate the air in the chamber, dry air with a relative humidity of approximately 5% and a temperature of approximately 28°C was circulated through the air inlet using a circulation pump at a flow rate of 12 L / min, allowing CO2 to be adsorbed into the honeycomb structure for 120 minutes. After CO2 adsorption, with a fan rotating at 5 W to agitate the air in the chamber, humidified air with a relative humidity of 90% or higher and a temperature of approximately 27°C was circulated through the chamber at a flow rate of 12 L / min using a circulation pump, allowing CO2 to be desorbed from the honeycomb structure for 30 minutes (second desorption treatment). When the second CO2 desorption process was performed, the relationship between the elapsed time during CO2 desorption and the amount of CO2 desorbed was calculated from the change in CO2 concentration in the chamber.

[0085] The relationship between the elapsed time during the second desorption treatment and the amount of CO2 desorption (moles) per unit mass of adsorbent is shown in Figure 4. The amount of CO2 desorption was normalized by setting the amount of CO2 desorption after 30 minutes for honeycomb structure A, which supported CO2 adsorbent A using zeolite as the porous material, at 1. Table 1 also shows the amount of CO2 desorption after 10 minutes from the start of desorption (10-minute desorption amount) and the ratio of the amount of CO2 desorption after 10 minutes from the start of desorption to the amount of CO2 desorption after 30 minutes from the start of desorption (10-minute / 30-minute desorption amount ratio). These results demonstrate that honeycomb structure C, which supported CO2 adsorbent C using activated carbon as the porous material, had a significantly slower desorption rate than honeycomb structure A (zeolite porous material) and honeycomb structure B (silica gel porous material).

[0086]

[0087] <Test II. Verification of the effect of supporting a CO2 adsorbent material on a honeycomb structure> (1. Measurement of CO2 adsorption rate by honeycomb structure B supporting CO2 adsorbent material B) As described in Test I, a honeycomb structure B supporting CO2 adsorbent material B using silica gel as the porous material was prepared. A CO2 adsorption test was conducted using honeycomb structure B and the same test equipment as in Test I. The test procedure was as follows. Honeycomb structure B was placed in a chamber. With a fan rotating at 5 W to agitate the air in the chamber, humidified air with a relative humidity of 90% or more and a temperature of approximately 27°C was circulated into the chamber at a flow rate of 12 L / min using a circulation pump, and CO2 was desorbed from honeycomb structure B for 30 minutes (desorption treatment). Next, with the fan rotating at 5 W to agitate the air in the chamber, dry air with a relative humidity of about 5% and a temperature of about 28°C was circulated from the air inlet into the chamber at a flow rate of 12 L / min, and CO2 was adsorbed into the honeycomb structure B for 120 minutes (adsorption treatment). The change in the amount of CO2 adsorbed over time during the adsorption treatment was calculated from the change in CO2 concentration in the chamber.

[0088] (2. Measurement of CO2 adsorption rate by powdered CO2 adsorbent B) Powdered CO2 adsorbent B containing silica gel, as described in Test I, was prepared. A CO2 adsorption test was conducted on CO2 adsorbent B using the same test equipment as in Test I. The test procedure was as follows. Powder of CO2 adsorbent B (approximately 0.5 g) was placed in a petri dish with an inner diameter of 50 mm and tapped several times. The petri dish was then placed in a chamber. With a fan rotating at 5 W to agitate the air in the chamber, humidified air with a relative humidity of 90% or higher and a temperature of approximately 27°C was circulated into the chamber at a flow rate of 12 L / min using a circulation pump, and CO2 was desorbed from CO2 adsorbent B for 30 minutes (desorption treatment). Next, with the fan rotating at 5 W to agitate the air in the chamber, dry air with a relative humidity of approximately 5% and a temperature of approximately 28°C was circulated from the air inlet into the chamber at a flow rate of 12 L / min, and CO was adsorbed into CO adsorbent B for 120 minutes (adsorption treatment). The change in the amount of CO adsorption over time during the adsorption treatment was calculated from the change in CO concentration in the chamber.

[0089] The results are shown in Figure 5. The CO2 adsorption amount (number of moles) per unit mass of the adsorbent was normalized by setting the CO2 adsorption amount of honeycomb structure B after 120 minutes as 1. Table 2 also shows the time required to reach 80% of the CO2 adsorption amount 120 minutes after the start of adsorption (80% adsorption time). These results show that the CO2 adsorption rate of honeycomb structure B carrying CO2 adsorbent B is significantly higher than that of powdered CO2 adsorbent B.

[0090]

[0091] <Test III. Relationship between thickness of CO2 adsorbent layer and CO2 adsorption amount> (1. Fabrication of CO2 adsorbent-supported honeycomb structure using honeycomb structure X) [1-1. Fabrication of honeycomb structure X] For laboratory tests, a sufficient number of flow-through honeycomb structure X, each of which was made of cordierite and had a rectangular parallelepiped shape measuring 20 mm x 20 mm x height (cell extension length) of 10 mm and open at both ends, was fabricated for use in each of the following tests. The honeycomb structure X had an average partition wall thickness of 2.5 mil (64 μm), an average pore diameter of 5 μm, a partition wall porosity of 47%, and a cell density of 900 cells / in2 (140 cells / cm 2 The cross-sectional shape of the cells of the honeycomb structure section X was square. The specific heat of the honeycomb structure section X was 0.76 kJ / (kg·K).

[0092] [1-2. Fabrication of a honeycomb structure supporting CO2 adsorbent B] The CO2 adsorbent B described in Test I was prepared and added to ethanol to a concentration of 20% by mass, followed by stirring to form a slurry. The honeycomb structure part X obtained above was immersed in the slurry, removed after 1 minute, and vacuum-dried at room temperature for 24 hours. The same immersion and drying process was then repeated to fabricate a honeycomb structure supporting CO2 adsorbent B. The average thickness of the CO2 adsorbent B layer was 20 μm. The surface area ratio of the partition walls covered with CO2 adsorbent B was 93%. Approximately 0.3 g of CO2 adsorbent B was supported on the honeycomb structure. This honeycomb structure had an opening ratio of 77% at the first end face and the second end face.

[0093] Furthermore, honeycomb structures supporting CO2 adsorbent B with average layer thicknesses of 30 μm, 40 μm, and 70 μm were fabricated under the same conditions as above except for varying the number of times the immersion and drying process was repeated. Table 3 shows the average thickness of the CO2 adsorbent B layer (average thickness), the surface area ratio of the partition walls covered with CO2 adsorbent B (coverage rate), the amount of CO2 adsorbent B supported (adsorbent amount), and the opening rate at the first end face and the second end face (opening rate) for the honeycomb structures fabricated above.

[0094]

[0095] (2. Fabrication of a CO2 adsorbent-supporting honeycomb structure using honeycomb structure Y) [2-1. Fabrication of honeycomb structure Y] For laboratory tests, a sufficient number of flow-through honeycomb structure Y, each of which was made of cordierite and had a rectangular parallelepiped shape of 20 mm x 20 mm x height (cell extension length) of 10 mm and open at both ends, was fabricated for use in each of the following tests. The honeycomb structure Y had an average partition wall thickness of 2.5 mil (64 μm), an average pore diameter of 5 μm, a partition wall porosity of 47%, and a cell density of 300 cells / in 2(47 cells / cm 2 The cross-sectional shape of the cells of the honeycomb structure portion was square. The specific heat of the honeycomb structure portion was 0.76 kJ / (kg·K). The honeycomb structure had an opening ratio of 86% at the first end face and the second end face.

[0096] [2-2. Fabrication of a honeycomb structure supporting CO2 adsorbent B] The CO2 adsorbent B described in Test I was prepared and added to ethanol to a concentration of 20% by mass, followed by stirring to form a slurry. The honeycomb structure Y obtained above was immersed in the slurry, removed after 1 minute, and vacuum-dried at room temperature for 24 hours. The same immersion and drying process was then repeated to fabricate a honeycomb structure supporting CO2 adsorbent B. The average thickness of the CO2 adsorbent B layer was 100 μm. The surface area ratio of the partition wall covered by CO2 adsorbent B was 95%. The amount of CO2 adsorbent B supported by the honeycomb structure was approximately 1.0 g. This honeycomb structure had an opening ratio of 67% at the first end face and the second end face.

[0097] Furthermore, under the same conditions as above except for varying the number of times the immersion and drying process was repeated, honeycomb structures supporting CO2 adsorbent B with average layer thicknesses of CO2 adsorbent B of 200 μm, 250 μm, 300 μm, and 350 μm were fabricated. Table 4 shows the average thickness of the CO2 adsorbent B layer (average thickness), the surface area ratio of the partition wall covered with CO2 adsorbent B (coverage rate), the amount of CO2 adsorbent B supported (adsorbent amount), and the opening rate at the first end face and the second end face (opening rate) for the honeycomb structures fabricated above.

[0098]

[0099] (3. Measurement of CO2 Adsorption Rate by CO2 Adsorbent-Supported Honeycomb Structure) Using each of the CO2 adsorbent-supported honeycomb structures fabricated above, a CO2 adsorption test was conducted using the same test equipment as in Test I. The test procedure was as follows: The honeycomb structure was placed in a chamber. With a fan rotating at 5 W to agitate the air in the chamber, humidified air with a relative humidity of 90% or higher and a temperature of approximately 27°C was circulated through the chamber at a flow rate of 12 L / min using a circulation pump, allowing CO2 to be desorbed from the honeycomb structure for 30 minutes (desorption treatment). Next, with a fan rotating at 5 W to agitate the air in the chamber, dry air with a relative humidity of approximately 5% and a temperature of approximately 28°C was circulated through the air inlet at a flow rate of 12 L / min, allowing CO2 to be adsorbed into the honeycomb structure for 60 minutes (adsorption treatment). The amount of CO2 adsorbed during the adsorption treatment was calculated from the change in CO2 concentration in the chamber.

[0100] The results are shown in Figure 6. The CO2 adsorption amount (number of moles) per unit volume of the honeycomb structure was normalized by setting the value of a honeycomb structure in which the average thickness of the layer of CO2 adsorbent material B was 100 μm as 1. Figure 6 shows that the CO2 adsorption amount per unit volume of the honeycomb structure increases when the average thickness of the layer of CO2 adsorbent material B is in the range of 30 to 250 μm.

[0101] <Test IV. Relationship between Opening Ratio of Honeycomb Structure and CO2 Adsorption Amount> (1. Fabrication of Honeycomb Structure) [1-1. Fabrication of Honeycomb Structure 1] For laboratory testing, a flow-through honeycomb structure 1 was fabricated from cordierite in the shape of a rectangular parallelepiped, measuring 20 mm x 20 mm x height (cell extension length) of 10 mm, with both ends open. The honeycomb structure 1 had an average partition wall thickness of 4.0 mil (102 μm), an average pore diameter of 5 μm, a partition wall porosity of 47%, and a cell density of 400 cells / in 2 (62 cells / cm 2 The cross-sectional shape of the cells of the honeycomb structure part 1 was square. The specific heat of the honeycomb structure part 1 was 0.76 kJ / (kg·K).

[0102] [1-2. Preparation of honeycomb structure 2] For laboratory testing, a rectangular parallelepiped cordierite honeycomb structure 2 measuring 20 mm x 20 mm x height (cell extension length) 10 mm and open at both ends was prepared. The honeycomb structure 2 had an average partition wall thickness of 3.5 mil (89 μm), an average partition wall pore diameter of 5 μm, a partition wall porosity of 47%, and a cell density of 400 cells / in 2 (62 cells / cm 2 The cross-sectional shape of the cells of the honeycomb structure part 2 was square. The specific heat of the honeycomb structure part 2 was 0.76 kJ / (kg·K).

[0103] [1-3. Preparation of honeycomb structure 3] For laboratory testing, a rectangular parallelepiped cordierite honeycomb structure 3 measuring 20 mm x 20 mm x height (cell extension length) 10 mm and open at both ends was prepared. The honeycomb structure 3 had an average partition wall thickness of 2.5 mil (64 μm), an average partition wall pore diameter of 5 μm, a partition wall porosity of 47%, and a cell density of 200 cells / in 2 (31 cells / cm 2 The cross-sectional shape of the cells of the honeycomb structure section 3 was square. The specific heat of the honeycomb structure section 3 was 0.76 kJ / (kg·K).

[0104] [1-4. Fabrication of honeycomb structure 4] For laboratory testing, a rectangular parallelepiped cordierite honeycomb structure 4 measuring 20 mm x 20 mm x height (cell extension length) 10 mm and open at both ends was fabricated. The honeycomb structure 4 had an average partition wall thickness of 2.5 mil (64 μm), an average partition wall pore diameter of 5 μm, a partition wall porosity of 47%, and a cell density of 300 cells / in 2 (47 cells / cm 2 The cross-sectional shape of the cells of the honeycomb structure part 4 was square. The specific heat of the honeycomb structure part 4 was 0.76 kJ / (kg·K).

[0105] [1-5. Fabrication of honeycomb structure 5] For laboratory testing, a rectangular parallelepiped cordierite honeycomb structure 5 measuring 20 mm x 20 mm x height (cell extension length) 10 mm and open at both ends was fabricated. The honeycomb structure 5 had an average partition wall thickness of 2.5 mil (64 μm), an average partition wall pore diameter of 5 μm, a partition wall porosity of 47%, and a cell density of 400 cells / in 2 (62 cells / cm 2 The cross-sectional shape of the cells of the honeycomb structure section 5 was square. The specific heat of the honeycomb structure section 5 was 0.76 kJ / (kg·K).

[0106] [1-6. Fabrication of honeycomb structure 6] For laboratory testing, a rectangular parallelepiped cordierite honeycomb structure 6 measuring 20 mm x 20 mm x height (cell extension length) 10 mm and open at both ends was fabricated. The honeycomb structure 6 had an average partition wall thickness of 2.5 mil (64 μm), an average partition wall pore diameter of 5 μm, a partition wall porosity of 47%, and a cell density of 600 cells / in 2 (93 cells / cm 2 The cross-sectional shape of the cells of the honeycomb structure section 6 was square. The specific heat of the honeycomb structure section 6 was 0.76 kJ / (kg·K).

[0107] [1-7. Fabrication of honeycomb structure 7] For laboratory testing, a rectangular parallelepiped cordierite honeycomb structure 7 measuring 20 mm x 20 mm x height (cell extension length) 10 mm and open at both ends was fabricated. The honeycomb structure 7 had an average partition wall thickness of 2.5 mil (64 μm), an average partition wall pore diameter of 5 μm, a partition wall porosity of 47%, and a cell density of 900 cells / in 2 (140 cells / cm 2 The cross-sectional shape of the cells of the honeycomb structure section 7 was square. The specific heat of the honeycomb structure section 7 was 0.76 kJ / (kg·K).

[0108] [1-8. Fabrication of honeycomb structure 8] For laboratory testing, a rectangular parallelepiped cordierite honeycomb structure 8 measuring 20 mm x 20 mm x height (cell extension length) 10 mm and open at both ends was fabricated. The honeycomb structure 8 had an average partition wall thickness of 2.5 mil (64 μm), an average partition wall pore diameter of 5 μm, a partition wall porosity of 47%, and a cell density of 1200 cells / in 2 (186 cells / cm 2 The cross-sectional shape of the cells of the honeycomb structure section 8 was square. The specific heat of the honeycomb structure section 8 was 0.76 kJ / (kg·K).

[0109] (2. Fabrication of Honeycomb Structure Supporting CO2 Adsorbent B) The CO2 adsorbent B described in Test I was prepared and added to ethanol to a concentration of 20% by mass, followed by stirring and mixing to form a slurry. Each of the honeycomb structure sections 1 to 8 obtained above was immersed in the slurry, removed after 1 minute, and vacuum-dried at room temperature for 24 hours. The same immersion and drying process was then repeated to fabricate a honeycomb structure supporting CO2 adsorbent B. The average thickness of the CO2 adsorbent B layer in each honeycomb structure was standardized to 100 μm. Based on the cell structure of the honeycomb structure section, the mass required for the CO2 adsorbent B layer to reach an average thickness of 100 μm was calculated, assuming a porosity of 50%. The immersion and drying process was repeated until the average thickness reached 100 μm. The surface area of ​​the partition walls covered with CO2 adsorbent B was 94%. Table 5 shows the mass of the CO2 adsorbent B supported on each honeycomb structure and the opening ratio at the first end face and the second end face of each honeycomb structure.

[0110] (3. Measurement of CO2 Adsorption Amount by Honeycomb Structure Supporting CO2 Adsorbent B) A CO2 adsorption test was conducted using the honeycomb structure supporting CO2 adsorbent B prepared above, using the same test equipment as in Test I. The test procedure was as follows. The honeycomb structure was placed in a chamber. With a fan rotating at 5 W to agitate the air in the chamber, humidified air with a relative humidity of 90% or higher and a temperature of approximately 27°C was circulated through the chamber at a flow rate of 12 L / min using a circulation pump, allowing CO2 to be desorbed from the honeycomb structure for 30 minutes (desorption treatment). Next, with a fan rotating at 5 W to agitate the air in the chamber, dry air with a relative humidity of approximately 5% and a temperature of approximately 28°C was circulated through the air inlet at a flow rate of 12 L / min, allowing CO2 to be adsorbed into the honeycomb structure for 60 minutes (adsorption treatment). The CO2 adsorption amount during the adsorption treatment was measured from the change in CO2 concentration in the chamber.

[0111] The results are shown in Table 5 and Figure 7. The "CO2 adsorption amount (moles) per unit mass of the CO2 adsorbent" and the "CO2 adsorption amount (moles) per unit volume of the honeycomb structure" were each normalized to the value of 1 for a test example using a honeycomb structure part 5 in which the opening ratio of the layer of CO2 adsorbent B was 63%. It can be seen that the CO2 adsorption amount per unit mass of the CO2 adsorbent, i.e., the utilization rate of the CO2 adsorbent supported on the honeycomb structure, increases as the opening ratio of the first end face and the second end face of the honeycomb structure part increases. On the other hand, it can be seen that the CO2 adsorption amount per unit volume of the honeycomb structure increases with the opening ratio up to about 65%, but decreases when the opening ratio becomes too high.

[0112]

[0113] While a high utilization rate of the CO2 adsorbent material supported on the honeycomb structure contributes to reducing manufacturing costs, the actual CO2 adsorption performance is determined by the amount of CO2 adsorbed per unit volume of the honeycomb structure. From the above results, it can be seen that the range of opening ratio that provides an excellent balance between the utilization rate of the CO2 adsorbent material and CO2 adsorption performance is 60% to 70%, particularly 62% to 68%.

[0114] 100: CO2 adsorbent-carrying honeycomb structure 102: Peripheral side wall 104: First end face 106: Second end face 108: Cell 112: Partition wall 114: CO2 adsorbent layer

Claims

1. A honeycomb structure carrying a CO2 adsorbent, comprising: a honeycomb structure portion having partition walls extending from a first end face to a second end face and partitioning a plurality of cells which form a fluid flow path; and a layer of a CO2 adsorbent at least partially covering a surface of the partition walls, the layer of the CO2 adsorbent containing an alkali metal carbonate supported on a porous material which contains one or more selected from zeolite, alumina and silica, and in which the total content of zeolite, alumina and silica is 50 mass% or more.

2. A CO2 adsorbent-supporting honeycomb structure according to claim 1, wherein the average thickness of the layer of the CO2 adsorbent is 30 μm to 250 μm.

3. A CO2 adsorbent-supporting honeycomb structure according to claim 1 or 2, wherein the opening ratio of the first end face and the second end face is 35% to 75%.

4. A CO2 adsorbent-supporting honeycomb structure according to claim 1 or 2, wherein the specific heat of said partition walls is 0.6 kJ / (kg·K) or more.

5. The average thickness of the partition walls is 40 to 440 μm, and the cell density is 20 to 200 cells / cm 2 3. The CO2 adsorbent-supporting honeycomb structure according to claim 1 or 2, 6. The opening ratio of the first end surface and the second end surface is 35% to 75%, the average thickness of the partition walls is 40 to 440 μm, and the cell density is 20 to 200 cells / cm 2 3. The CO2 adsorbent-supporting honeycomb structure according to claim 1 or 2, 7. A CO2 adsorbent-supporting honeycomb structure according to claim 1 or 2, wherein the partition walls are made of ceramics.

8. A method for recovering CO2, comprising the steps of: causing a first gas having a first humidity to flow into a first end face or a second end face of a honeycomb structure carrying a CO2 adsorbent as described in claim 1 or 2; capturing CO2 in the first gas by the CO2 adsorbent as the first gas passes through the plurality of cells; and causing the first gas with a reduced CO2 concentration to flow out from the end face opposite the inlet side.

9. A method for recovering CO2 as described in claim 8, comprising the steps of: causing a second gas, water or a mixture thereof having a second humidity higher than the first humidity to flow in from a first end face or a second end face of the honeycomb structure supporting the CO2 adsorbent; causing the CO2 captured in the CO2 adsorbent to be desorbed from the CO2 adsorbent while the second gas, water or a mixture thereof passes through the plurality of cells; and causing the second gas, water or a mixture thereof with an increased CO2 concentration to flow out from the end face opposite the inlet side.

10. A method for recovering CO2 as described in claim 9, wherein the second gas, water or a mixture thereof flowed into the first end face or the second end face of the CO2 adsorbent-supporting honeycomb structure has a temperature of 5 to 90°C.

11. A method for manufacturing a honeycomb structure supported on a CO2 adsorbent, comprising: step A1 of preparing a honeycomb structure portion having partition walls extending from a first end face to a second end face and partitioning a plurality of cells which form a fluid flow path; step A2 of preparing a CO2 adsorbent containing an alkali metal carbonate supported on a porous material which contains one or more selected from zeolite, alumina and silica, and in which the total content of zeolite, alumina and silica is 50 mass% or more; and step A3 of at least partially covering the surface of the partition walls with the CO2 adsorbent.

12. A method for manufacturing a honeycomb structure supporting a CO2 adsorbent as described in claim 11, wherein step A3 includes a step of flowing a slurry containing the CO2 adsorbent into the cells from a first end face or a second end face of the honeycomb structure portion.

13. A method for manufacturing a honeycomb structure supporting a CO2 adsorbent, comprising: step B1 of preparing a honeycomb structure portion having partition walls extending from a first end face to a second end face and partitioning a plurality of cells which form a fluid flow path; step B2 of preparing a porous material containing one or more selected from zeolite, alumina and silica, the total content of zeolite, alumina and silica being 50 mass% or more; step B3 of at least partially covering a surface of the partition wall with the porous material; and step B4 of supporting an alkali metal carbonate on the porous material at least partially covering the surface of the partition wall.

14. A method for manufacturing a honeycomb structure supporting a CO2 adsorbent as described in claim 13, wherein step B3 includes a step of flowing a slurry containing the porous material into the cells from a first end face or a second end face of the honeycomb structure portion.

15. A method for manufacturing a honeycomb structure supporting a CO2 adsorbent as described in claim 13, wherein step B4 includes a step of flowing an aqueous solution of the alkali metal carbonate into the cells from the first end face or the second end face of the honeycomb structure portion.

Citation Information

Patent Citations

  • Method and apparatus for extracting carbon dioxide from air

    JP6204333B2

  • Absorbing body for gas and air purifier using same

    JP1998337434A

  • Gaseous carbon dioxide absorption member

    JP1999262632A

  • Method of applying an sorbent onto a substrate, a carrier, and / or a carrier-coated substrate.

    JP2014533195A

  • Material for carbon dioxide recovery, method for producing material for carbon dioxide recovery, and recovery method of carbon dioxide

    JP2016059917A