Carbon fiber sheet, gas diffusion electrode base material, membrane electrode assembly, and fuel cell
The carbon fiber sheet, with a binder occupying 40% of the volume and specific filling rate distribution, addresses the challenges of high manufacturing costs and mechanical strength by achieving low electrical and thermal resistance while maintaining springiness and compressive strength, suitable for polymer electrolyte fuel cells.
Patent Information
- Application Number
- PCT/JP2024/011827
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Carbon fiber sheets with low electrical and thermal resistance for use in polymer electrolyte fuel cells face challenges such as high manufacturing costs, insufficient springiness, and compressive strength due to the need for increased basis weight and the use of large amounts of conductive fillers, which can lead to weak bonding and increased costs.
A carbon fiber sheet with a binder occupying 40% or more of the volume, having a specific filling rate distribution and open pore volume ratio, and incorporating a conductive filler with a controlled aspect ratio and particle size to achieve low electrical and thermal resistance while maintaining mechanical strength and springiness.
The solution results in a carbon fiber sheet with reduced manufacturing costs, improved springiness, and enhanced compressive strength, enabling efficient gas diffusion and electrical conductivity while maintaining low electrical and thermal resistance.
Smart Images

Figure JP2024011827_03102024_PF_FP_ABST
Abstract
Description
Carbon fiber sheet, gas diffusion electrode substrate, membrane electrode assembly and fuel cell
[0001] The present invention relates to a carbon fiber sheet, a gas diffusion electrode substrate, a membrane electrode assembly, and a fuel cell. More specifically, the present invention relates to a carbon fiber sheet and a gas diffusion electrode suitable for use in an electrochemical unit using a porous electrode that requires electrical conductivity and gas diffusion or liquid passage. Examples of such electrochemical units include fuel cells, water electrolysis cells, redox flow batteries, and air batteries, but the present invention is particularly suitable for use in solid polymer fuel cells. The present invention also relates to a membrane electrode assembly and a fuel cell that use the carbon fiber sheet or gas diffusion electrode substrate.
[0002] Polymer electrolyte fuel cells, which generate electromotive force by supplying a hydrogen-containing fuel gas to the anode and an oxygen-containing oxidizing gas to the cathode through an electrochemical reaction at both electrodes, are generally constructed by stacking a separator, a gas diffusion electrode, a catalyst layer, an electrolyte membrane, a catalyst layer, a gas diffusion electrode, and a separator in this order. The gas diffusion electrode must have high gas diffusivity to diffuse the gas supplied from the separator to the catalyst layer, high drainage properties to discharge water produced by the electrochemical reaction to the separator, and high conductivity to extract the generated current. Furthermore, the operating temperatures of polymer electrolyte fuel cells have been increasing in recent years, creating a demand for carbon fiber sheets with low electrical and thermal resistance.
[0003] However, such carbon fiber sheets with low electrical and thermal resistance have the following problems: (1) the need for a high basis weight to form electrical and thermal conduction paths results in high raw material costs, and (2) they lack other necessary properties such as springiness and sag resistance. Therefore, there is a need to develop a carbon fiber sheet that has low electrical and thermal resistance, while being low in manufacturing cost and offering both high springiness and sag resistance.
[0004] Therefore, for example, a carbon fiber sheet with low electrical and thermal resistance has been proposed, which can be produced by stacking and thermoforming multiple carbon fiber sheet precursors, and then heat treating them at high temperature for a long period of time (Patent Document 1).
[0005] Also, a carbon fiber sheet with low electrical and thermal resistance has been proposed in which a large amount of graphite is added as a conductive filler to a carbon fiber sheet precursor (Patent Document 2).
[0006] Furthermore, a carbon fiber sheet having low electrical and thermal resistance has been proposed in which pulp is mixed into a carbon fiber sheet precursor (Patent Document 3).
[0007] Japanese Patent Laid-Open No. 9-157052 Japanese Patent Laid-Open No. 2007-40040 Japanese Patent Laid-Open No. 2011-195374
[0008] However, the invention described in Patent Document 1 requires a long heating treatment, which results in high manufacturing costs. Furthermore, the invention described in Patent Document 2 uses an extremely large amount of conductive filler, which results in weak bonding between the carbon fibers in the carbon fiber sheet, resulting in insufficient compressive strength and poor sag properties. Furthermore, the invention described in Patent Document 3 requires the processing of gases generated by the decomposition of the pulp contained in the carbon fiber sheet during high-temperature heat treatment, which results in high manufacturing costs.
[0009] In order to solve the above problems, the present invention has the following configuration: (1) A carbon fiber sheet comprising carbon fibers and a binder, in which the proportion of an area occupied by the binder having a cross-sectional area larger than 10 times the cross-sectional area of the carbon fibers is 40 volume % or more of the volume of the entire carbon fiber sheet, and in which, in a section from a surface having a 50% filling rate that is closest to one surface to a surface having a 50% filling rate that is closest to the other surface, the carbon fiber sheet is divided into three equal parts in the direction perpendicular to the surface by planes parallel to the one surface, where, among the layers closest to each surface, the layer with the highest filling rate is called layer X, the layer with the lowest filling rate is called layer Y, and the layer located between layer X and layer Y is called layer Z, the carbon fiber sheet has the highest layer filling rate, and the ratio Z / Y of the layer filling rates of layer Y to layer Z is 1.8 or less. Here, the term "50% filling rate" refers to measuring the surface filling rate at every thickness of one-third of the carbon fiber diameter from one surface of a carbon fiber sheet to the other, then calculating the average of the surface filling rates obtained, and then calculating 50% of the average value obtained. Furthermore, the layer filling rate refers to the average value of the surface filling rates forming a layer. (2) The carbon fiber sheet according to (1), wherein the difference in layer filling rate between the layer Y and the layer Z is 15% or less. (3) The carbon fiber sheet according to any one of (1) to (2), wherein the open pore volume ratio, defined as the ratio of the volume of open pores having a pore diameter of 0.5 μm or more and less than 10 μm to the volume of open pores having a pore diameter of 10 μm or more and 100 μm or less, is 0.02 or more and 0.20 or less. (4) The carbon fiber sheet according to any one of (1) to (3), wherein the springiness upon compression is 4 μm or more and the sag upon compression is 10% or less. (5) The carbon fiber sheet according to any one of (1) to (4), wherein the binder contains a conductive filler having an aspect ratio of 20 to 60 and an average particle size of 2 μm to 8 μm. (6) The carbon fiber sheet according to any one of (1) to (5), which is a single-layer sheet. (7) The carbon fiber sheet according to any one of (1) to (6), wherein the fibrous material contained in the carbon fiber sheet is only carbon fiber. (8) A gas diffusion electrode substrate comprising the carbon fiber sheet according to any one of (1) to (7). (9) A gas diffusion electrode substrate comprising the carbon fiber sheet according to any one of (1) to (7), which has been subjected to a water-repellent treatment.(10) A gas diffusion electrode substrate having a microporous layer formed on at least one surface of the carbon fiber sheet according to any one of (1) to (7). (11) A membrane electrode assembly comprising the carbon fiber sheet according to any one of (1) to (7) or the gas diffusion electrode substrate according to (8). (12) A fuel cell comprising the membrane electrode assembly according to (11).
[0010] According to the present invention, it is possible to obtain a carbon fiber sheet having low electrical resistance, high spring properties, and high sag resistance, which has been difficult to achieve with conventional methods, at low production costs.
[0011] FIG. 1 is a schematic cross-sectional view illustrating surfaces A, B, and C in the three-dimensional structure of the carbon fiber sheet of the present invention. FIG. 2 is a schematic cross-sectional view of the structure of the carbon fiber sheet of the present invention as viewed from the surface B side. FIG. 3 is a cross-sectional view of the carbon fiber sheet of the present invention. FIG. 4 is a schematic view illustrating cross sections B1 and Bn in the three-dimensional structure of the carbon fiber sheet of the present invention. FIG. 5 is a schematic view illustrating cross sections C1 and Cn in the three-dimensional structure of the carbon fiber sheet of the present invention.
[0012] Explaining with reference to FIG. 3 , in the carbon fiber sheet of the present invention, in a carbon fiber sheet 1 made of carbon fibers and a binder, the proportion of an area occupied by binder having a cross-sectional area larger than 10 times the cross-sectional area of the carbon fibers is 40 volume % or more of the volume of the entire carbon fiber sheet, and in a section from a surface 11 having a 50% filling rate and closest to one surface 8 to a surface 12 having a 50% filling rate and closest to the other surface 9, the carbon fiber sheet 1 is divided into three equal parts in the direction perpendicular to the surface by planes parallel to the one surface 8, and among the layers close to each surface, the layer with the highest layer filling rate is layer X13, the layer with the lowest layer filling rate is layer Y15, and the layer located between layer X and layer Y is layer Z14, the layer Z14 has the highest layer filling rate, and the ratio Z / Y of the layer filling rates of layer Y15 to layer Z14 is 1.8 or less. Here, the 50% filling rate refers to a value obtained by measuring the surface filling rate at each thickness of 1 / 3 of the carbon fiber diameter from one surface 8 to the other surface 9 of the carbon fiber sheet, calculating the average value of the surface filling rates obtained, and then 50% of the average value obtained. Furthermore, the layer filling rate refers to the average value of the surface filling rates that form the layer.
[0013] The carbon fiber sheet, gas diffusion electrode, membrane electrode assembly, and fuel cell of the present invention will be described in detail below.
[0014] [Carbon Fiber Sheet] The carbon fiber sheet of the present invention includes carbon fibers and a binder. The binder is a component other than the carbon fibers in the carbon fiber sheet that serves to bind the carbon fibers together, and includes a carbide of a resin composition, etc.
[0015] To obtain the carbon fiber sheet of the present invention, it is preferable to use a carbon fiber porous body containing carbon fibers. Examples of the carbon fiber porous body that can be used include carbon fiber paper, carbon fiber woven fabric, and carbon fiber nonwoven fabric. However, carbon fiber paper is preferred because of its excellent "springiness," i.e., its ability to absorb dimensional changes in the thickness direction of the electrolyte membrane. In other words, a preferred embodiment of the carbon fiber sheet is carbon paper obtained by binding carbon fiber paper with a binder.
[0016] Examples of carbon fibers that can be used in the present invention include polyacrylonitrile (PAN)-based, pitch-based, and rayon-based carbon fibers. Among these, PAN-based carbon fibers and pitch-based carbon fibers are preferably used because of their excellent mechanical strength.
[0017] The carbon fiber of the present invention preferably has an average diameter of single fibers in the range of 3 to 20 μm, more preferably in the range of 5 to 10 μm. When the average diameter of single fibers is 3 μm or more, the diameter of the pores in the carbon fiber sheet becomes large, improving drainage and making it easier to suppress flooding. On the other hand, when the average diameter of single fibers is 20 μm or less, it is preferable because it is easy to control the thickness of the carbon fiber sheet to the preferred range described below.
[0018] When a carbon fiber paper sheet is used as the carbon fiber porous body, the average length of the carbon fibers used in the carbon fiber paper sheet is preferably in the range of 3 to 20 mm, more preferably in the range of 5 to 15 mm. When the average length of the single fibers is 3 mm or more, a carbon fiber sheet with excellent mechanical strength, electrical conductivity, and thermal conductivity can be obtained. On the other hand, when the average length of the single fibers is 20 mm or less, the dispersion of the carbon fibers during papermaking is excellent, and a homogeneous carbon fiber sheet can be obtained.
[0019] The average diameter and average length of single fibers in carbon fibers, and the cross-sectional area of carbon fibers described below are usually measured by directly observing the carbon fibers that are raw materials, but they can also be measured by observing a carbon fiber sheet.
[0020] The carbon fiber porous body may be mixed with natural fibers such as pulp or synthetic fibers as fibers other than carbon fiber, but this may increase the amount of decomposition gas from fibers other than carbon fiber during firing. Using a carbon fiber porous body that does not contain fibers other than carbon fiber can suppress an increase in production costs due to an increase in decomposition gas, and also makes it easier to control the distribution of the resin composition in the pre-impregnated body described below, making it easier to realize the structure of the present invention. However, flame-resistant yarns such as polyacrylonitrile, which are precursors of carbon fiber, emit little decomposition gas and can be suitably used as fibers other than carbon fiber to be mixed into the carbon fiber porous body.
[0021] When a carbon fiber paper sheet is used as the carbon fiber porous body, it is preferable that the carbon fibers be in the form of a sheet in which they are randomly dispersed in a two-dimensional plane in order to maintain isotropic in-plane electrical and thermal conductivities.
[0022] Furthermore, when obtaining a carbon fiber paper sheet, the carbon fiber papermaking may be performed only once or may be performed by laminating multiple times, but in order to prevent internal peeling of the carbon fiber sheet, it is preferable to form the carbon fiber sheet continuously in one step. Forming a thick carbon fiber sheet by a method of performing papermaking steps multiple times may result in discontinuous surfaces being formed in the thickness direction, which may cause stress concentration when the carbon fiber sheet is bent, resulting in internal peeling.
[0023] The binder contained in the carbon fiber sheet of the present invention is preferably a resin carbide, and the resin carbide may contain a filler. In particular, it is preferable to contain a conductive filler such as carbon powder as the filler, since this can reduce the electrical and thermal resistance of the carbon fiber sheet.
[0024] Examples of carbon powder that can be used include carbon black, such as furnace black, acetylene black, lamp black, and thermal black; graphite, such as flake graphite, phosphorus graphite, amorphous graphite, artificial graphite, expanded graphite, and flake graphite; carbon nanotubes, linear carbon, and milled carbon fiber fibers. The binder constituting the carbon fiber sheet of the present invention preferably contains a conductive filler having an aspect ratio of 20 to 60 and an average particle size of 2 μm to 8 μm. The inclusion of such a conductive filler can adjust the distribution of the filling rate in the carbon fiber sheet and more effectively form open pores. This allows the carbon fiber sheet of the present invention to be realized with a wide range of carbon fiber sheet material blends. If the average particle size of the conductive filler is greater than 8 μm or the aspect ratio of the conductive filler is greater than 60, the conductive filler may not be uniformly attached to the carbon fiber porous body when producing the pre-impregnated body described below. On the other hand, when the average particle diameter of the conductive filler is smaller than 2 μm or the aspect ratio of the conductive filler is smaller than 20, the particles may be densely packed together, making it impossible to form open pores. The aspect ratio of the conductive filler can be determined by observing the graphite particles in a magnified state using a scanning electron microscope. When the length of the graphite particle in the major axis direction in the magnified image (the length of the longest line segment connecting two points on the periphery of the graphite particle in the image) is a and the length of the minor axis direction (the length of the longest line segment connecting two points on the periphery of the graphite particle in the image that is perpendicular to the major axis direction) is b, a / b is measured for 50 random graphite particles, and the average value is used as the aspect ratio in the present invention. In the case of a thin, sheet-like shape such as flake graphite, the length in the major axis direction a is the length in the major axis direction in a plane perpendicular to the thickness direction, and the length in the minor axis direction b is the thickness.
[0025] The carbon fiber sheet of the present invention includes a region occupied by a binder having a cross-sectional area that is more than 10 times the cross-sectional area of the carbon fibers. By including a region occupied by a binder having a cross-sectional area that is more than 10 times the cross-sectional area of the carbon fibers, the carbon fibers can be firmly bonded together, resulting in a carbon fiber sheet with excellent sag resistance.
[0026] In the carbon fiber sheet of the present invention, the proportion of the region occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fibers is 40% by volume or more relative to the volume of the entire carbon fiber sheet. By making the proportion of the region occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fibers 40% by volume or more relative to the volume of the entire carbon fiber sheet, conductive paths can be formed between the binders, resulting in a carbon fiber sheet with low electrical resistance. When the proportion of the region occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fibers is 60% by volume or more relative to the volume of the entire carbon fiber sheet, the formation of conductive paths becomes stronger, resulting in a carbon fiber sheet with lower electrical and thermal resistance, which is preferable. On the other hand, when the proportion of the region occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fibers is 90% by volume or less, the gas diffusion properties required for the carbon fiber sheet are more easily achieved, which is preferable. In other words, it is preferable to make the proportion of the region occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fibers 60 to 90% by volume relative to the volume of the entire carbon fiber sheet.
[0027] Here, the cross-sectional area of the binder is confirmed using an X-ray CT image described later. In this image, when the cross-sectional area of the portion where the binder is continuous is defined as the cross-sectional area of the binder, the ratio of the region occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fiber to the volume of the entire carbon fiber sheet is defined as the ratio of the region occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fiber. Note that regions occupied by binders whose cross-sectional area is 10 times or less than the cross-sectional area of the carbon fiber are not included in the cross-sectional area of the binder. Furthermore, the cross-sectional area of the carbon fiber here refers to the cross-sectional area of a cross section perpendicular to the longitudinal direction of the carbon fiber. In the cross section of the carbon fiber sheet, carbon fibers, binders, and binders containing carbon fibers are present, and any region whose cross-sectional area is greater than 10 times the cross-sectional area of the carbon fiber is considered to be a binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fiber. The binder adheres to the carbon fiber, and the carbon fiber is encapsulated in the binder to form a composite structure, so the carbon fiber encapsulated in the binder is also calculated as the binder. Note that the binder may contain voids, but because voids do not contribute to electronic conduction or mechanical properties, they are not included in the cross-sectional area of the carbon fiber and binder, or the binder encapsulating the carbon fiber.
[0028] In the present invention, the filling rate of the surface of a carbon fiber sheet refers to the proportion of the constituent components (carbon fibers and binder) of the carbon fiber sheet to the total area of a surface obtained by slicing the carbon fiber sheet in a direction perpendicular to the surface by a plane parallel to one surface, at thicknesses of 1 / 3 of the carbon fiber diameter of the surface forming a layer. In other words, it is the area occupancy rate of the part excluding voids inside the carbon fiber sheet. The method for measuring the filling rate will be described in detail later.
[0029] The area occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fiber is calculated by image processing of an X-ray CT image of the carbon fiber sheet. This will be explained with reference to FIGS. 1, 4, and 5. In a three-dimensional image of the carbon fiber sheet, one surface 2 of the carbon fiber sheet is designated as plane A, one surface 3 perpendicular to plane A is designated as cross section B, and a surface 4 perpendicular to cross section B is designated as cross section C. Since the three-dimensional image of the carbon fiber sheet obtained by X-ray CT is a laminate of surfaces, the three-dimensional image of the carbon fiber sheet has cross sections from cross section B1, which is one surface, to cross section Bn, which is the opposite surface. Similarly, for cross section C, it has cross sections from cross section C1, which is one surface, to cross section Cn, which is the opposite surface. In this two-dimensional image of the carbon fiber sheet from cross section B1 to cross section Bn, an area (carbon fiber and binder) having an area less than 10 times the cross-sectional area of the carbon fiber is removed from the three-dimensional image of the carbon fiber sheet by image processing. Furthermore, in the two-dimensional images from cross section C1 to cross section Cn of cross section C, regions having an area of 10 times or less the cross-sectional area of the carbon fiber are removed from the three-dimensional image of the carbon fiber sheet by image processing. After removing the areas having an area of 10 times or less the cross-sectional area of the carbon fiber in cross sections B and C from the three-dimensional image of the carbon fiber sheet by image processing as described above, the region remaining after the above processing in the image sliced along a plane parallel to plane A is defined as the region occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fiber. Here, the start point and end point in the thickness direction of the carbon fiber sheet when calculating the region occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fiber refer to one surface and the other surface, and are different from the surface having a 50% filling rate used when determining layer X, layer Y, and layer Z, which will be described later. In addition, since the carbon fibers contained within the binder are included in the area occupied by the binder, the ratio of the area occupied by the binder having a cross-sectional area larger than 10 times the cross-sectional area of the carbon fibers to the entire carbon fiber sheet differs from the blending ratio of the materials. The image analysis is performed using image analysis software "TRI / 3D-VOL-FCS64 (manufactured by Ratoc System Engineering Co., Ltd.)".
[0030] In the carbon fiber sheet of the present invention, in a section from surface 11, which has a filling rate of 50% and is closest to one surface 8, to surface 12, which has a filling rate of 50% and is closest to the other surface 9, the carbon fiber sheet 1 is divided into three equal parts in the direction perpendicular to the surface by planes parallel to one of the surfaces, and among the layers close to each surface, the layer with the highest filling rate is called layer X13, the layer with the lowest filling rate is called layer Y15, and the layer located between layer X13 and layer Y15 is called layer Z14. Layer Z14 has the highest layer filling rate, and the ratio Z / Y of the layer filling rates of layer Y15 to layer Z14 is 1.8 or less.
[0031] The 50% filling rate in the carbon sheet of the present invention refers to a value that is obtained by measuring the surface filling rate at thicknesses of 1 / 3 of the carbon fiber diameter from one surface 8 (plane A) of the carbon fiber sheet toward the other surface 9, calculating the average value of the surface filling rates obtained, and then 50% of the obtained average value.
[0032] For the layers X, Y, and Z defined above, layer Z having the highest layer packing ratio allows for the formation of a uniform conductive path in the thickness direction of the carbon fiber sheet, and by setting the layer packing ratio ratio Z / Y between layer Y, which has the lowest layer packing ratio, and layer Z located between layers X and Y, to be 1.8 or less, the contact resistance between both surfaces of the carbon fiber sheet and adjacent members can be reduced. A layer packing ratio Z / Y of 1.5 or less is even more effective and is therefore preferable. In this case, the layer packing ratio refers to the average value of the packing ratios of all surfaces forming the layer.
[0033] It is preferable that the difference in packing ratio between Layer Y and Layer Z is 15% or less, because uniform conductive paths can be formed in the thickness direction of the carbon fiber sheet. It is even more preferable that the difference in packing ratio between Layer Y and Layer Z is 10% or less, because uniform conductive paths can be more significantly formed in the thickness direction of the carbon fiber sheet.
[0034] Furthermore, in the carbon fiber sheet of the present invention, the ratio (open pore volume ratio) of the open pore volume with a pore diameter of 0.5 μm or more and less than 10 μm to the open pore volume with a pore diameter of 10 μm or more and 100 μm or less is preferably 0.02 or more and 0.20 or less. By setting the open pore volume ratio to 0.02 or more, the mobility of the binder is increased, and the springiness during compression can be enhanced. By setting the open pore volume ratio to 0.20 or less, the presence of weak points that could be the starting point for fracture of the binder during compression can be suppressed, and the sag characteristics are improved. An open pore volume ratio of 0.05 or more and 0.15 or less is more preferable because these effects are more pronounced.
[0035] The open pore volume in the present invention is measured by mercury porosimetry, which will be described later in the Examples section.
[0036] The thickness of the carbon fiber sheet of the present invention is preferably 50 to 250 μm, and more preferably 70 to 180 μm. By making the thickness of the carbon fiber sheet 250 μm or less, more preferably 180 μm or less, gas diffusibility is likely to be increased and generated water is also likely to be discharged more easily. Furthermore, the size of the fuel cell as a whole is likely to be reduced. On the other hand, by making the thickness of the carbon fiber sheet 50 μm or more, more preferably 70 μm or more, gas diffusion in the in-plane direction within the carbon sheet is efficient, and power generation performance is likely to be improved. The thickness of the carbon fiber sheet is the thickness when pressurized at 1 MPa.
[0037] Furthermore, the carbon fiber sheet of the present invention preferably has a springiness of 4 μm or more when compressed and a sag characteristic of 10% or less when compressed. A gas diffusion electrode using a carbon fiber sheet having properties in these ranges can easily absorb deformation of components such as an electrolyte membrane and can be used for a long period of time, making it particularly suitable for use in fuel cells. It is more preferable that the springiness of the carbon fiber sheet when compressed is 6 μm or more and the sag characteristic of 5% or less when compressed.
[0038] In the present invention, the springiness of the carbon fiber sheet during compression refers to the difference between the thickness at 1.5 MPa and the thickness at 0.5 MPa during the process of releasing the pressure from the carbon fiber sheet after it has been pressurized at 2 MPa. The higher the springiness of the carbon fiber sheet during compression, the more excellent the restoring force of the carbon fiber sheet after compression, and this is preferable.
[0039] The settling property of a carbon fiber sheet during compression in the present invention is the rate of decrease in thickness at 1 MPa during the first compression cycle and the third compression cycle when the carbon fiber sheet is pressurized three times at 2 MPa. The smaller the settling property during compression, the less irreversible deformation occurs due to pressure cycles, making the carbon fiber sheet less susceptible to breakage, and is therefore preferable.
[0040] Furthermore, a preferred embodiment of the carbon fiber sheet of the present invention is a carbon fiber sheet consisting of a single layer sheet. By using a single layer sheet, the production cost can be reduced compared to a carbon fiber sheet formed by laminating multiple precursor sheets. From the viewpoint of reducing the production cost, continuous production by roll-to-roll is also a preferred embodiment.
[0041] [Method for Producing Carbon Fiber Sheet] Next, a preferred method for producing the carbon fiber sheet of the present invention will be described.
[0042] [Impregnation with Resin Composition] When obtaining the carbon fiber sheet of the present invention, one preferred method is to impregnate the carbon fiber porous body with a resin composition that serves as a binder.
[0043] In the present invention, methods for impregnating a porous carbon fiber body with a resin composition that serves as a binder include a method of immersing the porous carbon fiber body in a solution containing the resin composition, a method of applying a solution containing the resin composition to the porous carbon fiber body, and a method of laminating and bonding the porous carbon fiber body to a film made of the resin composition. Among these, the method of immersing the porous carbon fiber body in a solution containing the resin composition is particularly preferred because of its excellent productivity. Note that a porous carbon fiber body impregnated with a resin composition that serves as a binder may be referred to as a "pre-impregnated body."
[0044] The resin composition used in producing the pre-impregnated body is preferably a resin composition that carbonizes upon firing to form a binder that is a conductive carbide, and contains additives such as the above-mentioned conductive filler and surfactant as needed. Examples of resins that constitute the resin component in the resin composition used in producing the pre-impregnated body include thermosetting resins such as phenolic resins, epoxy resins, melamine resins, and furan resins. Among these, phenolic resins are preferably used because of their high carbonization yield.
[0045] When producing a pre-impregnated body, the resin composition obtained by the above-mentioned method can be used for impregnation as is, or various solvents can be added as needed to improve the impregnation ability into the carbon fiber porous body. Examples of solvents that can be used here include methanol, ethanol, and isopropyl alcohol.
[0046] During impregnation, the resin composition is preferably impregnated so that the resin component is 30 to 400 parts by mass, more preferably 50 to 300 parts by mass, per 100 parts by mass of carbon fibers in the pre-impregnated body. When the resin component is 30 parts by mass or more per 100 parts by mass of carbon fibers in the pre-impregnated body, the carbon fiber sheet has excellent mechanical properties, electrical conductivity, and thermal conductivity. On the other hand, when the resin component is 400 parts by mass or less per 100 parts by mass of carbon fibers in the pre-impregnated body, the carbon fiber sheet has excellent gas diffusivity in the in-plane direction and through-thickness direction.
[0047] In the carbon fiber sheet of the present invention, the distribution of the layer packing rate can be adjusted by controlling the single fiber diameter of the carbon fibers constituting the carbon fiber sheet, the density of the carbon fiber sheet, and the distribution of the binder in the thickness direction of the carbon fiber sheet. Of these, the method of controlling the distribution of the binder in the thickness direction of the carbon fiber sheet is more preferred. Controlling the distribution of the binder in the thickness direction of the carbon fiber sheet makes it easier to control the conduction path through the binder, which has a cross-sectional area greater than 10 times the cross-sectional area of the carbon fiber.
[0048] Examples of methods for controlling the binder distribution in the thickness direction of a carbon fiber sheet include a method of preparing three pre-impregnated bodies, each with an adjusted amount of resin composition impregnated therein, and stacking these bodies, and a method of controlling the binder distribution by preparing a single pre-impregnated body having a distribution in the amount of resin composition adhered thereto using a resin application method that forms a distribution in the amount of resin composition adhered thereto when impregnating a porous carbon fiber body with the resin composition. Of these methods, the method of preparing a single pre-impregnated body having a distribution in the amount of resin adhered thereto using a resin application method that forms a distribution in the amount of resin composition adhered thereto is preferred because it does not require a supply device that supplies multiple pre-impregnated bodies at once, which is required when obtaining carbon fiber sheets by stacking pre-impregnated bodies, and therefore can suppress increases in production costs. Furthermore, the method of preparing a single pre-impregnated body is also suitable for adjusting the thickness to a preferred range because it is easy to reduce the thickness of the resulting carbon fiber sheet.
[0049] Examples of resin application methods that form a distribution in the amount of resin composition applied include mixing a conductive filler into the resin composition, adjusting the viscosity of the impregnation liquid by combining different types of solvents when applying the resin composition, and controlling the evaporation rate by adjusting the drying conditions.
[0050] Methods for forming open pores with a pore diameter of 0.5 μm or more and less than 10 μm in a carbon fiber sheet include appropriately adjusting the amount and size of the conductive filler mixed into the resin composition, and combining the amount and size of the pore-forming material that disappears during the carbonization process. Of these methods, the method of adjusting the amount and size of the conductive filler mixed in combination is preferred because it can suppress the increase in decomposition gas during the carbonization process. Here, size specifically refers to the particle size and aspect ratio.
[0051] [Heat Treatment] After the pre-impregnated body is formed, it is possible to laminate the pre-impregnated body or to subject the pre-impregnated body to a heat treatment under pressure before carbonization.
[0052] A plurality of pre-impregnated bodies can be bonded together. In this case, a plurality of pre-impregnated bodies having the same properties can be bonded together, or a plurality of pre-impregnated bodies having different properties can be bonded together. Bonding can also be performed by stacking a plurality of pre-impregnated bodies and subjecting them to a heat treatment under pressure. However, bonding can result in the formation of a discontinuous surface in the thickness direction, which can lead to internal isolation. Therefore, in the present invention, it is more preferable to use only one pre-impregnated body and subject it to a heat treatment under pressure.
[0053] By carrying out the heat treatment under pressure, it is possible to more accurately control the thickness of the carbon fiber sheet and the distribution of the packing ratio in the thickness direction.
[0054] [Carbonization] After impregnating a carbon fiber porous body with a resin composition to form a pre-impregnated body, calcining the resin composition in an inert atmosphere is one preferred embodiment for producing the carbon fiber sheet of the present invention. For this calcination, a batch-type heating furnace or a continuous heating furnace can be used, but using a continuous heating furnace increases the carbonization treatment speed and reduces production costs.
[0055] The maximum firing temperature is preferably within the range of 1,300 to 3,000°C. If the maximum temperature is 1,300°C or higher, the carbonization of the resin component in the pre-impregnated body proceeds, resulting in a carbon fiber sheet with excellent electrical and thermal conductivity. On the other hand, if the maximum temperature is 3,000°C or lower, the operating cost of the heating furnace is reduced.
[0056] [Gas diffusion electrode substrate] Next, the gas diffusion electrode substrate of the present invention will be described. In one preferred embodiment, the gas diffusion electrode substrate of the present invention is a gas diffusion electrode substrate made of the carbon fiber sheet described above. In addition, it is also preferred that the gas diffusion electrode substrate is made of the carbon fiber sheet described above that has been subjected to a water-repellent treatment for the purpose of improving drainage. It is also preferred that the gas diffusion electrode substrate has a microporous layer on at least one side of the carbon fiber sheet described above. Note that a carbon fiber sheet that has been subjected to a water-repellent treatment and then formed with a microporous layer may be used as the gas diffusion electrode substrate.
[0057] The water-repellent treatment can be carried out by coating or impregnating the carbon fiber sheet with a water-repellent material and then heat treating it.
[0058] As the water-repellent material, it is preferable to use a fluorine-based polymer because of its excellent corrosion resistance, such as polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA).
[0059] The microporous layer can be formed by applying a coating liquid to the surface of a carbon fiber sheet. The microporous layer is composed of conductive fine particles and a microporous layer resin that binds them. The conductive fine particles are preferably nanocarbon powder such as acetylene black, and the microporous layer resin is preferably a fluororesin such as PTFE or FPE. Microcarbon powder such as graphite may be mixed as conductive fine particles to improve the conductivity of the microporous layer, or non-conductive fine particles may be mixed to improve the durability of the catalyst.
[0060] The coating liquid may contain a dispersion medium such as water or an organic solvent, and may also contain a dispersion aid such as a surfactant. Water is preferred as the dispersion medium, and a nonionic surfactant is preferred as the dispersion aid.
[0061] The microporous layer is obtained by applying the coating liquid to a carbon fiber sheet. Coating methods such as screen printing, rotary screen printing, spraying, intaglio printing, gravure printing, die coater coating, bar coating, and blade coating can be used for the coating. It is also preferable to subsequently dry the coating at a temperature of 80 to 180°C. Furthermore, after drying, it is also preferable to heat the coating at a temperature of about 300 to 400°C, preferably 340 to 390°C, to melt the water-repellent material.
[0062] The upper limit of the basis weight of the microporous layer is not particularly limited, but is preferably 50 g / m 2 It is preferable that the content is 30 g / m or less, and more preferably 30 g / m 2 More preferably, it is 25 g / m or less. 2 The lower limit is 10 g / m 2It is preferable that the content is 14 g / m or more. 2 More preferably, it is 16 g / m or more, and even more preferably, it is 16 g / m or more. 2 The basis weight of the microporous layer is 10 g / m 2 When the microporous layer has a mass per unit area of 50 g / m or more, the entire surface of the carbon fiber sheet can be covered with the microporous layer, the back diffusion of the generated water is further promoted, and drying-up can be further suppressed. 2 If the ratio is less than 1 / 2, the drainage property is further improved and flooding can be further suppressed.
[0063] [Membrane Electrode Assembly] The membrane electrode assembly of the present invention includes the carbon fiber sheet or the gas diffusion electrode substrate. A specific method for producing the membrane electrode assembly of the present invention is to bond the carbon fiber sheet or the gas diffusion electrode substrate to at least one side of a solid polymer electrolyte membrane having catalyst layers on both sides to form the membrane electrode assembly. The catalyst layer comprises a layer containing a solid polymer electrolyte and catalyst-supported carbon. Platinum is typically used as the catalyst. In fuel cells in which a reformed gas containing carbon monoxide is supplied to the anode side, platinum and ruthenium are preferably used as the anode-side catalyst. The solid polymer electrolyte is preferably a perfluorosulfonic acid-based polymer material with high proton conductivity, oxidation resistance, and heat resistance. When a gas diffusion electrode substrate having a microporous layer is used, arranging the microporous layer of the gas diffusion electrode substrate on the catalyst layer side facilitates back diffusion of generated water and increases the contact area between the catalyst layer and the gas diffusion electrode substrate, thereby reducing contact electrical resistance.
[0064] [Fuel Cell] The fuel cell of the present invention includes the above-described membrane electrode assembly. That is, the fuel cell of the present invention has separators on both sides of the above-described membrane electrode assembly. That is, a fuel cell is constructed by disposing separators on both sides of the above-described membrane electrode assembly. Usually, a polymer electrolyte fuel cell is constructed by stacking a plurality of such membrane electrode assemblies, each sandwiched between separators via a gasket.
[0065] Next, the carbon fiber sheet of the present invention will be specifically described with reference to examples.
[0066] Regarding the measurement method for carbon fiber sheets described below, when measuring a water-repellent treated carbon fiber sheet or a carbon fiber sheet used in a gas diffusion electrode substrate having a microporous layer, the carbon fiber sheet was heated in an air atmosphere at 500°C for 1 hour to burn off the water-repellent material and the fluororesin in the microporous layer, and then air was blown to remove carbon powder such as carbon black contained in the microporous layer before measurement.
[0067] <Measurement of filling ratio> A carbon fiber sheet (dimensions: 10 mm length × 5 mm width) was set upright in a three-dimensional measuring X-ray CT (manufactured by Yamato Scientific Co., Ltd., product name TDM1000H-CF), and a 360° scan was performed with the vertical axis of the sheet sample as the rotation axis to create a three-dimensional image with a field of view diameter of 2.39 mmΦ × sheet thickness [mm]. In the examples described below, imaging was performed at a tube voltage of 40 kV and a tube current of 60 μA. At this time, the field of view diameter dimensions were determined so that the thickness of each slice image constituting the three-dimensional image was 1 / 3 of the carbon fiber diameter, and the image was reconstructed with 1024 pixels. First, all slice images constituting the three-dimensional image were output from the image analysis software attached to the X-ray CT. Next, each obtained slice image was subjected to binarization processing to distinguish the carbon fiber sheet from the background area where the carbon fiber sheet was not present. In the binarization process, the image analysis software "TRI / 3D-VOL-FCS64 (manufactured by Ratoc Systems Engineering Co., Ltd.)" was used. The point at which the degree of separation between the two peaks obtained when drawing a grayscale histogram of each obtained slice image was the highest was used as the brightness threshold for binarization (Otsu's binarization method). That is, the image was divided into a dark side (background) and a bright side (carbon fiber sheet components such as carbon fiber and binder). The percentage of the area of the binarized bright side out of the total area per slice image was taken as the filling rate [%]. Next, the filling rate of each slice image was plotted from one surface (hereinafter sometimes referred to as the first surface) of the carbon fiber sheet to the other surface (hereinafter sometimes referred to as the second surface) to confirm the distribution of the filling rate. From the filling rate distribution thus obtained, the average value of the area with a filling rate of 0.1% or more was calculated, and 50% of that average value was taken as the 50% filling rate. In the carbon fiber sheet, the surface having a 50% filling rate and closest to the first surface and the surface having a 50% filling rate and closest to the second surface were determined, and then the section between the two determined surfaces was divided into three equal parts by surfaces parallel to the first surface to form three layers.
[0068] In order to evaluate the filling rate of the carbon fiber sheet, measurements were taken multiple times and the average value was calculated. In the examples described later, six samples were taken at different positions on the carbon fiber sheet, and measurements were taken, and the average value was calculated.
[0069] Furthermore, for layers obtained by dividing a section from a surface having a 50% packing rate that is closest to the first surface (one surface) to a surface having a 50% packing rate that is closest to the second surface (the other surface) into thirds in the thickness direction and in the direction perpendicular to the surface by planes parallel to the first surface, the layer with the highest packing rate among the layers close to each surface was designated Layer X, the layer with the lowest packing rate among the layers was designated Layer Y, and the layer located between Layer X and Layer Y was designated Layer Z. Note that in Comparative Examples 1 to 4 described below, for the layers obtained by dividing the section into thirds as described above, the two layers close to each surface had the same packing rate, and therefore it was not possible to determine which was Layer X by definition; however, for convenience, one of the two layers close to each surface was designated Layer X and the other Layer Y.
[0070] <Measurement of Carbon Fiber Diameter and Cross-Sectional Area> To measure the carbon fiber diameter, photographs of the carbon fibers on both surfaces of the carbon fiber sheet were taken at 1,000x magnification using a microscope such as a scanning electron microscope. Thirty different single fibers were randomly selected on each surface, and their diameters were measured, and the average value for a total of 60 single fibers on both surfaces was calculated. When measuring the diameter of each single fiber, the width of the single fiber (the length in the direction perpendicular to the fiber length direction) was measured, and this length was used as the diameter of the single fiber. The scanning electron microscope used was an SU8010 manufactured by Hitachi, Ltd.
[0071] The cross-sectional area of a single carbon fiber was determined by calculating the cross-sectional area of the single carbon fiber when it was made into a perfect circle from the average diameter determined in this manner.
[0072] <Measurement of the proportion of the area occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fiber> The proportion of the area occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fiber was calculated by image processing of the X-ray CT image of the carbon fiber sheet. For the binarized image (three-dimensional image) of the carbon fiber sheet used in the above measurement, in the thickness direction range of the thickness direction surface area where the surface filling rate determined by the surface filling rate measurement was 0.1% or more, in the two-dimensional image from surface B1 to surface Bn of cross section B of the carbon fiber sheet, a region having an area of 10 times or less the cross-sectional area of the carbon fiber was removed from the three-dimensional image of the carbon fiber sheet by image processing. Furthermore, in the two-dimensional image from surface C1 to surface Cn of cross section C, a region having an area of 10 times or less the carbon fiber diameter was removed from the three-dimensional image of the carbon fiber sheet by image processing. The filling rate of each surface was calculated for the three-dimensional image of the carbon fiber sheet after the above removal. The filling rate of each surface in the region of the carbon fiber sheet before the removal operation where the filling rate was 0.1% or more was calculated, and the region occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fiber was divided by the volume of the entire carbon fiber sheet and multiplied by 100 to obtain the average value of the proportion (expressed in %) of each layer. This was taken as the proportion (volume %) of the region occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fiber in the carbon fiber sheet. The image analysis was performed using image analysis software "TRI / 3D-VOL-FCS64 (manufactured by Ratoc System Engineering Co., Ltd.)." Six samples were taken from different parts of the carbon fiber sheet and measured, and the average value was calculated.
[0073] <Measurement of open pore volume ratio> A carbon fiber sheet was placed in a 6 cm 2 Five measurement samples cut into 1 / 4" were prepared and measured by mercury intrusion porosimetry at a measurement pressure of 6 kPa to 123 MPa (pore diameter of 10 nm to 200 μm) to determine the pore size distribution. The measurement device used was an Autopore 9520 manufactured by Shimadzu Corporation.
[0074] The pore volume (open pore volume) of each region was calculated by subtracting the integrated data of the smaller pore diameters from the integrated data of the larger pore diameters of the pores to be measured in the logarithmic differential pore volume distribution graph. For example, the volume in the region of pore diameters of 0.5 μm or more and less than 10 μm was calculated by subtracting the integrated data of the smaller pore diameters from the integrated data of the smaller pore diameters.
[0075] Using the above method, the ratio of the open pore volume of pores with a pore diameter of 0.5 μm or more and less than 10 μm to the open pore volume present in the pore diameter range of 10 μm or more and 100 μm or less was measured as the open pore volume ratio of the carbon fiber sheet.
[0076] <Measurement of basis weight> The carbon fiber sheet to be measured was cut into a 10 cm square to prepare a sample, and its mass [g] was calculated by multiplying the area of the sample (0.01 m 2 ) to find the answer.
[0077] <Measurement of Electrical Resistance of Carbon Fiber Sheet> The electrical resistance under pressure was measured using an "Autograph" (registered trademark) AGS-X manufactured by Shimadzu Corporation. A carbon fiber sheet cut into a 22.4 mm square was placed on two upper and lower electrical resistance measuring jigs attached at an interval of 20.0 cm. The upper electrical resistance measuring jig was lowered, and a load was applied until it reached 1.0 MPa. After the predetermined load was reached, a current of 1.0 ampere was applied using a DC power supply connected to the electrical resistance measuring jig. 20 seconds after the current application, the voltage value of the digital multimeter was read, and the electrical resistance value was calculated from the measurement value and the measured area.
[0078] <Measurement of Springiness and Sagging Properties of Carbon Fiber Sheet> The springiness and sagging properties of the carbon fiber sheet were measured by a surface pressure cycle test at 0.03 MPa and 2 MPa for the compressed thickness of the carbon fiber sheet. Two upper and lower flat metal jigs attached to an "Autograph" (registered trademark) AGS-X manufactured by Shimadzu Corporation were equipped with a digital micrometer to measure the distance between the upper and lower jigs. A carbon fiber sheet cut into a 30 mm square was placed in the center of the flat metal jig, and a surface pressure cycle test at 0.03 MPa and 2 MPa was performed. During this test, the distance between the upper and lower jigs was continuously measured at each pressure, and this value was used as the compressed thickness of the carbon fiber sheet at that pressure. Measurements were performed on five carbon fibers, and the average values were used to calculate the springiness and sagging properties of the carbon fiber sheet below.
[0079] The springiness of the carbon fiber sheet was determined as the difference between the thickness at 1.5 MPa and the thickness at 0.5 MPa during decompression in the first cycle.
[0080] The settling property of the carbon fiber sheet was determined as the reduction rate of thickness at 1 MPa in the third cycle of pressure relative to the thickness at 1 MPa in the first cycle of pressure.
[0081] (Example 1) Toray Industries, Inc.'s polyacrylonitrile carbon fiber "TORAYCA" (registered trademark) T300 (average single fiber diameter: 7 μm) was cut into short fibers with an average length of 12 mm, dispersed in water, and continuously made into paper by a wet papermaking method. Furthermore, a 10% by mass aqueous solution of polyvinyl alcohol was applied as a binder to the paper body, and the paper was dried to obtain a paper body with a basis weight of carbon fiber of 30.0 g / m. 2 The amount of polyvinyl alcohol applied was 20 parts by mass per 100 parts by mass of the carbon fiber paper body.
[0082] Next, a resin composition in which a resol-type phenolic resin and a novolac-type phenolic resin were mixed in a mass ratio of 1:1 as the thermosetting resin, graphite (average particle size 5 μm, aspect ratio 38) as the carbon powder, and a mixture of methanol and butanol in a mass ratio of 3:1 as the solvent were used, and these were mixed in a compounding ratio of thermosetting resin / carbon powder / solvent = 35 parts by mass / 15 parts by mass / 50 parts by mass, and the mixture was stirred for 1 minute using an ultrasonic dispersing device to obtain a uniformly dispersed resin composition.
[0083] Next, the long carbon fiber paper sheet was continuously immersed in an impregnation solution of the resin composition filled in a tank and sandwiched between two rolls to adjust the amount of resin attached. At this time, a certain clearance was left between the two rolls to allow the pre-impregnated body to pass through, thereby adjusting the overall amount of resin composition attached. The pre-impregnated body was then heated and dried at a temperature of 100°C for 5 minutes to produce a pre-impregnated body. Next, the pre-impregnated body was continuously heated and pressurized at a temperature of 180°C for a total of 5 minutes while being conveyed in stages and pressurized with parallel hot plates. Here, the thickness of the pre-impregnated body after heating and pressurization was adjusted by the thickness of the spacer so that the carbonized carbon fiber sheet would have the desired thickness.
[0084] The pre-impregnated body thus subjected to the heat and pressure treatment was introduced into a heating furnace maintained in a nitrogen gas atmosphere at a maximum temperature of 2,400° C., to obtain a carbon fiber sheet.
[0085] The obtained carbon fiber sheet was measured for the layer packing ratio of Layer X, Layer Y, and Layer Z, the proportion of the area occupied by the binder having a cross-sectional area larger than 10 times the cross-sectional area of the carbon fiber, the open pore volume ratio, the electrical resistance, the spring property, and the sag property using the above-mentioned measurement methods, and the results are shown in Table 1.
[0086] (Example 2) A carbon fiber sheet was obtained in the same manner as in Example 1, except that graphite (average particle size: 5 μm, aspect ratio: 18) was used as the carbon powder and a mixture of methanol and butanol in a 1:1 (mass ratio) was used as the solvent, and various evaluations were performed.
[0087] Example 3 A carbon fiber sheet was obtained in the same manner as in Example 1, except that the compounding ratio of thermosetting resin / carbon powder / solvent was 30 parts by mass / 20 parts by mass / 50 parts by mass, and various evaluations were carried out.
[0088] Example 4 A carbon fiber sheet was obtained in the same manner as in Example 1, except that the compounding ratio of thermosetting resin / carbon powder / solvent was 42.5 parts by mass / 7.5 parts by mass / 50 parts by mass, and various evaluations were carried out.
[0089] (Comparative Example 1) A carbon fiber sheet was obtained and various evaluations were carried out in the same manner as in Example 1, except that graphite (average particle size 5 μm, aspect ratio 17) was used as the carbon powder and only methanol was used as the solvent. This carbon fiber sheet had high electrical resistance and was therefore inferior.
[0090] (Comparative Example 2) A carbon fiber sheet was obtained in the same manner as in Comparative Example 1, except that the amount of resin composition applied was adjusted by widening the clearance between the two rolls so that the carbon fiber sheet had a higher basis weight, and various evaluations were carried out. This carbon fiber sheet had poor spring properties.
[0091] (Comparative Example 3) A carbon fiber sheet was obtained and various evaluations were carried out in the same manner as in Comparative Example 1, except that the compounding ratio of thermosetting resin / carbon powder / solvent was 20 parts by mass / 30 parts by mass / 50 parts by mass. This carbon fiber sheet was significantly inferior in sag resistance.
[0092] Comparative Example 4 A pre-impregnated body was obtained in which the resin composition was biased toward the lower surface by applying a resin composition to a porous carbon fiber body from the lower surface using a roll coater and drying the body. Two pre-impregnated bodies were prepared, and the two were stacked with their lower surfaces facing each other. While transporting the pre-impregnated bodies in a stepwise manner, the pre-impregnated bodies were continuously subjected to a heating and pressurizing treatment at a temperature of 180°C for a total of 5 minutes while being pressurized and heated with parallel hot plates. A carbon fiber sheet was obtained in the same manner as in Example 1, and various evaluations were performed. This carbon fiber sheet had a low layer filling rate in Layer X and Layer Y, and therefore had high electrical resistance, insufficient bonding on the carbon fiber sheet surface, and poor sag properties.
[0093] Comparative Example 5 A carbon fiber sheet was obtained in the same manner as in Example 1, except that graphite (average particle size 5 μm, aspect ratio 17) and carbon black (average particle size 0.01 μm, aspect ratio 1) were used in a 1:1 (mass ratio) ratio as the carbon powder, and various evaluations were carried out. This carbon fiber sheet had a high electrical resistance and poor sag resistance because the proportion of the area occupied by the binder having a cross-sectional area more than 10 times that of the carbon fiber was low.
[0094]
[0095] LIST OF SYMBOLS 1 Carbon fiber sheet 2 One surface of carbon fiber sheet (plane A) 3 Surface seen from one side perpendicular to plane A (cross section B) 4 Surface seen from the side perpendicular to cross section B (cross section C) 5 Cross section of carbon fiber oriented perpendicular to cross section B 6 Carbon fiber oriented perpendicular to cross section C 7 Binder having a cross section area 10 times the cross section area of carbon fiber 8 One surface of carbon fiber sheet 9 Other surface of carbon fiber sheet 10 Region consisting of surfaces with less than 50% filling rate 11 Surface with 50% filling rate that is closest to one surface 12 Surface with 50% filling rate that is closest to the other surface 13 Layer X 14 Layer Z 15 Layer Y 16 Cross section B1 17 Cross section Bn 18 Cross section C1 19 Cross section Cn
[0096] The present invention can be used in electrochemical units that use porous electrodes, such as fuel cells, water electrolysis cells, redox flow batteries, and air batteries, and is particularly suitable for use in polymer electrolyte fuel cells.
Claims
1. A carbon fiber sheet comprising carbon fibers and a binder, the proportion of the area occupied by the binder having a cross-sectional area greater than 10 times the cross-sectional area of the carbon fibers is 40 volume % or more of the total volume of the carbon fiber sheet, and the carbon fiber sheet is divided into three equal parts in the direction perpendicular to the surface by a plane parallel to one surface in a section from a surface having a 50% filling rate that is closest to one surface to a surface having a 50% filling rate that is closest to the other surface, and among the layers obtained by dividing the carbon fiber sheet into three equal parts in the direction perpendicular to the surface by a plane parallel to the one surface, the layer with the highest layer filling rate among the layers closest to each surface is called layer X, the layer with the lowest layer filling rate is called layer Y, and the layer located between layer X and layer Y is called layer Z, the layer Z has the highest layer filling rate, and the ratio Z / Y of the layer filling rates of layer Y to layer Z is 1.8 or less. Here, the 50% filling rate refers to a value obtained by measuring the filling rate of the surface at a thickness of 1 / 3 of the carbon fiber diameter from one surface of the carbon fiber sheet to the other surface, then calculating the average value of the obtained filling rates of the surfaces, and then calculating 50% of the obtained average value. Furthermore, the packing rate of the layer refers to the average packing rate of the surfaces forming the layer.
2. The carbon fiber sheet according to claim 1, wherein the difference in packing ratio between said layer Y and said layer Z is 15% or less.
3. The carbon fiber sheet according to claim 1, wherein the open pore volume ratio, defined as the ratio of the open pore volume having a pore diameter of 0.5 μm or more and less than 10 μm to the open pore volume having a pore diameter of 10 μm or more and 100 μm or less, is 0.02 or more and 0.20 or less.
4. The carbon fiber sheet according to claim 1, which has a springiness when compressed of 4 μm or more and a sag property when compressed of 10% or less.
5. The carbon fiber sheet according to claim 1, wherein the binder contains a conductive filler having an aspect ratio of 20 or more and 60 or less and an average particle size of 2 μm or more and 8 μm or less.
6. The carbon fiber sheet according to claim 1, which consists of a single layer sheet.
7. The carbon fiber sheet according to claim 1, wherein the fibrous material contained in the carbon fiber sheet is only carbon fiber.
8. A gas diffusion electrode substrate comprising the carbon fiber sheet according to claim 1.
9. A gas diffusion electrode substrate comprising the carbon fiber sheet according to claim 1 which has been subjected to a water repellent treatment.
10. A gas diffusion electrode substrate having a microporous layer formed on at least one surface of the carbon fiber sheet according to claim 1.
11. A membrane electrode assembly comprising the carbon fiber sheet according to claim 1 or the gas diffusion electrode substrate according to claim 8.
12. A fuel cell comprising the membrane electrode assembly of claim 11.
Citation Information
Patent Citations
Porous carbon sheet and its production
JP1997157052A
Ceiling structure and ceiling construction method
JP2007040040A
Porous carbon sheet and method for producing the same
JP2011195374A
Carbon electrode material assembly and manufacturing method thereof
JP2001196071A
Carbon sheet, gas diffusion electrode base material, and fuel cell
JP2017202948A
Cited By
Porous carbon sheet and water electrolysis device
WO2025182758A1