Fine copper particles and method for producing fine copper particles

Copper fine particles with glycol polymer coatings address the limitations of solder and existing copper bonding materials by providing high conductivity, heat dissipation, and improved workability for bonding semiconductor devices at elevated temperatures, enhancing the reliability and efficiency of die attach applications.

WO2024204241A1PCT designated stage expired Publication Date: 2024-10-03NISSHIN SEIFUN GROUP INC +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012027
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional solder-based bonding materials for semiconductor devices are limited by their melting temperature, restricting the operating conditions of power semiconductor devices with high temperature applications, and existing plate-shaped or sheet-shaped copper bonding materials have poor workability and require precise alignment.

Method used

Copper fine particles with a coating layer made of glycol or glycol polymer, having specific thermal and weight loss properties, are used for die attach applications, offering excellent heat dissipation and conductivity while maintaining high temperature stability and ease of use.

Benefits of technology

The copper fine particles provide effective bonding with high thermal and electrical conductivity, excellent heat dissipation, and improved workability, enabling reliable die attach and bonding of semiconductor elements even at high temperatures without the need for precise alignment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012027_03102024_PF_FP_ABST
    Figure JP2024012027_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: fine copper particles usable for die attach (die bonding) and the like and having excellent heat dissipation properties; and a method for producing the fine copper particles. The fine copper particles have a coating layer made of a glycol or a glycol polymer. The glycol or glycol polymer preferably has a molecular weight of 300 or less. The fine copper particles have a particle diameter, as determined by the BET method, of 20-400 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Copper microparticles and method for producing copper microparticles

[0001] The present invention relates to copper microparticles used for bonding semiconductor elements, high frequency devices, light emitting diodes, semiconductor lasers, etc. to substrates, etc., and a method for producing copper microparticles.

[0002] Currently, power semiconductor elements using wide bandgap semiconductors such as silicon carbide (SiC), gallium nitride (GaN), gallium oxide, or diamond are being developed. Compared to semiconductor elements using Si or GaAs, power semiconductor elements have lower on-resistance, enable high-speed switching, and can be miniaturized. Furthermore, power semiconductor elements have high heat resistance and can operate at high temperatures of 250-300°C. Solder has traditionally been used to bond semiconductor elements to substrates, etc. However, power semiconductor elements have higher operating temperatures than conventional semiconductor elements using Si or GaAs, and solder bonding requires them to be used at temperatures at which the solder does not melt. When solder is used as a bonding material, the power semiconductor elements must be used at temperatures at which the solder does not melt, which places limitations on their use. Thus, bonding materials are also required to be able to be used at high temperatures.

[0003] As a bonding material other than solder, Patent Document 1 describes a plate- or sheet-shaped bonding material containing copper as a main component and copper fine particles having an average particle size of 300 nm or less. The bonding material further contains a reducing agent that reduces the copper fine particles, and the reducing agent contains either or both of a polyol solvent and an organic acid.

[0004] Japanese Patent Application Laid-Open No. 2019-203172

[0005] The plate- or sheet-shaped bonding material of Patent Document 1 bonds components together under predetermined bonding conditions of pressure, temperature, and time in an inert atmosphere. However, because the bonding material of Patent Document 1 is in plate or sheet form, it needs to be adjusted to a size appropriate for the size of the bonding location. Furthermore, the bonding material needs to be positioned and installed at the bonding location, resulting in poor workability. Therefore, a simple method for bonding, such as coating, is desired, and particles that can be used as a bonding material are desired. Furthermore, when the bonding material is used for die attach (die bonding), excellent heat dissipation properties are required.

[0006] An object of the present invention is to provide copper microparticles that can be used for die attach (die bonding) and the like and have excellent heat dissipation properties, and a method for producing the copper microparticles.

[0007] In order to achieve the above-mentioned object, one aspect of the present invention is copper microparticles that have a coating layer made of a glycol or a glycol polymer and exist as particles alone. The glycol or glycol polymer preferably has a molecular weight of 300 or less. Another aspect of the present invention is copper microparticles that have a coating layer made of a glycol or a glycol polymer and exist as particles alone, and in a nitrogen atmosphere, a coating layer removal rate of 30% by mass or more at 200°C as measured by simultaneous differential thermal analysis and thermogravimetry. Another aspect of the present invention is copper microparticles that have a coating layer made of a glycol or a glycol polymer and exist as particles alone, and in a nitrogen atmosphere, a weight loss rate of 0.25% by mass or more at 200°C as measured by simultaneous differential thermal analysis and thermogravimetry. Another aspect of the present invention is copper microparticles that have a coating layer made of a glycol or a glycol polymer and exist as particles alone, and in an air atmosphere, a weight increase rate of 5% by mass or less at 200°C as measured by simultaneous differential thermal analysis and thermogravimetry.

[0008] One aspect of the present invention is copper microparticles having a coating layer made of glycol or a glycol polymer, existing as particles alone, which have a particle growth rate of particle diameter based on the BET method of 105% or more after being heated in a particle state at a temperature of 200°C for 1 hour in a nitrogen atmosphere. -4 One aspect of the present invention is copper fine particles having a coating layer made of a glycol or a glycol polymer, existing as particles alone, and having a volume shrinkage rate of 20% or less after being fired in a pellet state in a nitrogen atmosphere at a temperature of 200°C for 1 hour. The particle size measured by the BET method is preferably 20 to 400 nm.

[0009] One aspect of the present invention is a method for producing copper microparticles having a coating layer composed of glycol or a glycol polymer, the method comprising the steps of: supplying a carrier gas in which copper powder is dispersed into a thermal plasma flame to generate microparticles; and supplying a surface treatment agent containing glycol or a glycol polymer to the microparticles in an air-dispersed state before the microparticles are collected, in a temperature range in which the surface treatment agent does not denature. The plasma gas in the thermal plasma flame is preferably argon gas, helium gas, hydrogen gas, or nitrogen gas.

[0010] According to the present invention, copper microparticles that can be used for die attach (die bonding) and the like and have excellent heat dissipation properties, and a method for producing copper microparticles can be provided.

[0011] FIG. 1 is a schematic diagram showing an example of a utilization form of copper microparticles of the present invention. FIG. 2 is a schematic diagram showing another example of a utilization form of copper microparticles of the present invention. FIG. 3 is a schematic diagram showing an example of an apparatus for producing copper microparticles of the present invention. FIG. 4 is a schematic diagram showing an SEM image of copper microparticles of Example 1. FIG. 5 is a schematic diagram showing an SEM image of copper microparticles of Example 2. (a) is a schematic diagram showing an SEM image of copper microparticles of Example 1 before calcination, and (b) is a schematic diagram showing an SEM image of copper microparticles of Example 1 after calcination. (a) is a schematic diagram showing an SEM image of copper microparticles of Example 2 before calcination, and (b) is a schematic diagram showing an SEM image of copper microparticles of Example 2 after calcination. (a) is a schematic diagram showing an SEM image of a pellet of copper microparticles of Example 1 before calcination, and (b) is a schematic diagram showing an SEM image of a pellet of copper microparticles of Example 1 after calcination. 1 is a graph showing the results of an analysis of the crystal structure of copper microparticles of Examples 1 and 2 of the present invention by X-ray diffraction. (a) is a schematic diagram showing an SEM image of a pellet of copper microparticles of Example 2 before calcination, and (b) is a schematic diagram showing an SEM image of a pellet of copper microparticles of Example 2 after calcination. (b) is a graph showing the results of an analysis of the crystal structure of copper microparticles of Examples 1 and 2 of the present invention by X-ray diffraction. (c) is a graph showing the change over time in the volume resistivity of copper microparticles of Examples 1 and 2 of the present invention.

[0012] The copper microparticles and the method for producing copper microparticles of the present invention will be described in detail below based on preferred embodiments shown in the accompanying drawings. Note that the drawings described below are illustrative for explaining the present invention and are simplified for explaining the present invention. Therefore, the present invention is not limited to the drawings shown below. Note that in the following, the term "to" indicating a numerical range includes the numerical values ​​written on both sides. For example, when ε is a numerical value ε α ~Number ε β That is, the range of ε is the number ε α and the number ε β The range includes ε α ≦ε≦ε β In addition, unless otherwise specified, various numerical values ​​include error ranges generally accepted in the relevant technical field. Copper microparticles and a method for producing copper microparticles will be described below.

[0013] [First Example of Copper Particles] The copper particles have a coating layer made of glycol or glycol polymer. The glycol referred to here is a dehydration condensation product of ethylene glycol, i.e., a di-, tri-, or tetra-molecule ethylene glycol (HOCH 2 CH 2 Examples of suitable glycols include diethylene glycol, triethylene glycol, and tetraethylene glycol, which are dehydration condensates of ethylene glycol (OH). Furthermore, glycol polymers include polyethylene glycol, which is a polymer of ethylene glycol. Glycols or glycol polymers exhibit reducing properties. A coating layer composed of glycol or glycol polymer must be present, entirely or partially covering the surface of the copper microparticles when the copper microparticles are heated. If the coating layer does not entirely or partially cover the surface of the copper microparticles, the reducing action is not exerted, and sintering of the copper microparticles does not proceed, which may prevent bonding such as die attach. For this reason, it is necessary for the glycol or glycol polymer not to completely evaporate (volatilize) at temperatures below the bonding temperature.

[0014] As the molecular weight of the ethylene glycol polymer increases, the temperature at which the mass begins to rapidly decrease due to evaporation or thermal decomposition tends to shift toward a higher temperature, and the temperature at which the weight loss rate reaches 100%, i.e., the temperature at which all of the ethylene glycol polymer evaporates or thermally decomposes, tends to shift toward a higher temperature. For this reason, the glycol or glycol polymer preferably has a molecular weight of 300 or less. Examples of glycols or glycol polymers having a molecular weight of 300 or less include ethylene glycol, diethylene glycol, triethylene glycol, and tetraethylene glycol. Other examples include polyethylene glycols having a molecular weight of 300 or less. The molecular weight of the glycol or glycol polymer can be selected based on the bonding temperature, for example, the temperature at which a predetermined weight loss rate is achieved, such as the temperature at which the weight loss rate reaches 100% or 50%. In other words, the glycol or glycol polymer can be selected depending on the bonding temperature during die attachment. As described above, the surfaces of the copper microparticles are coated with glycol or glycol polymer. The presence or absence of a coating layer on the copper microparticles and the composition of the coating layer can be determined, for example, using FT-IR (Fourier transform infrared spectrophotometer).

[0015] Furthermore, the copper microparticles preferably have a particle size of 20 to 400 nm as measured by the BET method. A particle size of 20 to 400 nm is preferable because it allows for good handling. The particle size of the copper microparticles described above is an average particle size measured using the BET method. In the BET method, the particle size is calculated from the specific surface area, assuming that the particles are spherical. A Macsorb HM-1208 (trade name) manufactured by Mountech Co., Ltd. is used to measure the particle size of the copper microparticles.

[0016] Copper microparticles have a coating layer composed of glycol or glycol polymer, which provides excellent oxidation suppression on the particle surface during firing and excellent reduction of existing oxides on the particle surface, thereby facilitating sintering. Furthermore, sintered copper microparticles have a higher melting point and better heat resistance than solder and other materials. Therefore, they can be used for die attachment (die bonding), and when used as a bonding material, they can achieve excellent electrical conductivity and heat dissipation while still satisfying heat resistance requirements. It is known that the ratio of thermal conductivity to electrical conductivity in metals is proportional to temperature (Wiedemann-Franz law). Therefore, in copper metal, increased electrical conductivity means increased thermal conductivity. Therefore, excellent electrical conductivity in copper microparticles means excellent heat dissipation. The copper microparticles are not dispersed in a solvent or the like, but exist alone without the solvent or the like. Therefore, when using copper microparticles, a sintered body can be obtained using only the copper microparticles. For this reason, copper microparticles are also suitable for die attachment (die bonding), etc. Furthermore, since the copper microparticles exist alone, when the copper microparticles are used in combination with a solvent, the combination of the copper microparticles and the solvent is not particularly limited, and the degree of freedom in selecting the solvent is high. As described above, the copper microparticles exist alone without a solvent or the like. In other words, the copper microparticles exist alone as particles, but the presence of copper microparticles alone also includes a state in which the copper microparticles are dispersed in a gas.

[0017] [Second Example of Copper Microparticles] The copper microparticles have a coating layer composed of a glycol or a glycol polymer, and the coating layer removal rate at 200°C in a nitrogen atmosphere, as measured by simultaneous differential thermal analysis and thermogravimetry (TG-DTA), is 30% by mass or more. The coating layer removal rate is a value defined by dividing the weight loss rate at 200°C by the weight loss rate at 700°C when performing simultaneous differential thermal analysis and thermogravimetry (TG-DTA) in a nitrogen atmosphere. If the coating layer removal rate at 200°C in a nitrogen atmosphere, as measured by simultaneous differential thermal analysis and thermogravimetry, is 30% by mass or more, sintering of the copper microparticles progresses due to the suppression of oxidation and reduction of the copper microparticles during firing, thereby allowing the copper microparticles to be bonded together well. Moreover, because the bonding between the copper microparticles is good, the copper microparticles have high conductivity and high heat dissipation. The upper limit of the coating layer removal rate at 200°C, as measured by simultaneous differential thermal analysis and thermogravimetry, is 100% by mass. For the simultaneous differential thermal analysis-thermogravimetry (TG-DTA), an STA7200 (trade name) manufactured by Hitachi High-Tech Science Corporation is used.

[0018] In the present invention, a nitrogen atmosphere refers to an atmosphere in which nitrogen gas with a purity of 99.99 (99.99% by volume of nitrogen) is constantly flowing, and refers to an atmosphere in which the oxygen concentration is 3 ppm by volume or less. Therefore, in a nitrogen atmosphere, the oxygen concentration can be 3 ppm by volume or less, and a gas such as a rare gas that does not react with copper or its decomposition products may be mixed with the nitrogen. The oxygen concentration can be measured, for example, using a low-concentration oxygen analyzer PS-820-L (trade name) manufactured by Iijima Electronics Co., Ltd.

[0019] As described above, when copper microparticles have a coating layer removal rate of 30% by mass or more at 200°C in a nitrogen atmosphere as measured by simultaneous differential thermal and thermogravimetric analysis, oxidation during firing is suppressed and even if copper oxide is present on the surface of the copper microparticles during firing, it can be reduced, thereby allowing the copper microparticles to be bonded together well. Moreover, since the bonding between the copper microparticles is good, electrical conductivity and heat dissipation can be improved. Furthermore, sintered copper microparticles have a higher melting point and better heat resistance than solder, etc. Therefore, they can be used for die attach (die bonding), etc., and when copper microparticles are used as a bonding material, they can be made to have excellent electrical conductivity and heat dissipation while still satisfying heat resistance.

[0020] [Third Example of Copper Microparticles] These copper microparticles have a coating layer made of a glycol or a glycol polymer, and exhibit a weight loss rate of 0.25% by mass or more at 200°C measured by simultaneous differential thermal analysis and thermogravimetry in a nitrogen atmosphere. The weight loss rate at 200°C measured by simultaneous differential thermal analysis and thermogravimetry in a nitrogen atmosphere is an index showing the degree of thermal decomposition of the glycol or glycol polymer constituting the coating layer. When the weight loss rate at 200°C measured by simultaneous differential thermal analysis and thermogravimetry in a nitrogen atmosphere is 0.25% by mass or more, the coating layer undergoes thermal decomposition, which not only suppresses oxidation during firing but also reduces copper oxide, even if present on the surface of the copper microparticles, during firing, thereby enabling good bonding of the copper microparticles to each other. The upper limit of the weight loss rate at 200°C measured by simultaneous differential thermal analysis and thermogravimetry in a nitrogen atmosphere is 10% by mass. The weight loss rate is the weight loss rate obtained by simultaneous differential thermal analysis and thermogravimetry (TG-DTA). The nitrogen atmosphere is as described above.

[0021] The copper microparticles have a weight loss rate of 0.25% by mass or more at 200°C as measured by simultaneous differential thermal and thermogravimetric analysis in a nitrogen atmosphere, so that the coating layer composed of glycol or glycol polymer is thermally decomposed at 200°C, thereby bonding the copper microparticles together well, thereby improving electrical conductivity and heat dissipation. Furthermore, sintered copper microparticles have a higher melting point and superior heat resistance than solder, etc. Therefore, they can be used for die attach (die bonding), etc., and when used as a bonding material, they can achieve excellent electrical conductivity and heat dissipation while satisfying heat resistance requirements.

[0022] [Fourth Example of Copper Microparticles] Copper microparticles having a coating layer composed of a glycol or a glycol polymer, and having a weight gain rate of 5% by mass or less at 200°C measured by simultaneous differential thermal analysis and thermogravimetry in an air atmosphere. The weight gain rate at 200°C measured by simultaneous differential thermal analysis and thermogravimetry in an air atmosphere is an index showing the degree of oxidation of the copper microparticles. When the weight gain rate at 200°C measured by simultaneous differential thermal analysis and thermogravimetry in an air atmosphere is 5% by mass or less, oxidation of the copper microparticles is suppressed when sintered at 200°C in a nitrogen atmosphere, allowing the copper microparticles to be bonded well. The lower limit of the weight gain rate at 200°C measured by simultaneous differential thermal analysis and thermogravimetry in an air atmosphere is 0% by mass. The upper limit of the weight gain rate at 200°C measured by simultaneous differential thermal analysis and thermogravimetry in an air atmosphere is 25% by mass. The weight gain rate is the weight gain rate obtained by simultaneous differential thermal analysis and thermogravimetry (TG-DTA).

[0023] The atmospheric atmosphere is generally referred to as air. The composition of the atmospheric atmosphere, i.e., the composition of air, is 78.08% by volume of nitrogen, 20.95% by volume of oxygen, 0.93% by volume of argon, and 0.03% by volume of carbon dioxide. Note that a general measurement error is allowed for the composition of air.

[0024] The copper microparticles have a weight increase rate of 5% by mass or less at 200°C in an air atmosphere as measured by simultaneous differential thermal and thermogravimetric analysis, thereby suppressing oxidation, allowing the copper microparticles to be well bonded together, and improving electrical conductivity. Furthermore, sintered copper microparticles have a higher melting point and superior heat resistance than solder, etc. Therefore, they can be used for die attach (die bonding), etc., and when used as a bonding material, they can achieve excellent electrical conductivity and heat dissipation while satisfying heat resistance requirements.

[0025] [Fifth Example of Copper Microparticles] These copper microparticles have a coating layer made of glycol or glycol polymer, and after heating in a particulate state at 200°C for 1 hour in a nitrogen atmosphere, have a particle growth rate of 105% or more in particle size based on the BET method. The particle growth rate can be determined from the particle sizes before and after firing. The particle growth rate is obtained using the following formula: Particle growth rate (%) = ((particle size after firing) / (particle size before firing)) x 100 If the above particle growth rate is 105% or more, the particles can be sintered by firing in a nitrogen atmosphere at 200°C for 1 hour. The upper limit of the particle growth rate is, for example, 500%. The nitrogen atmosphere is as described above.

[0026] Copper microparticles have a particle growth rate of 105% or more based on the BET method after being heated in a nitrogen atmosphere at 200°C for 1 hour in a particle state. This allows the copper microparticles to be sintered by heating in a nitrogen atmosphere at 200°C for 1 hour, thereby improving electrical conductivity and heat dissipation. Furthermore, the sintered copper microparticles have a higher melting point and excellent heat resistance than solder, etc. Therefore, they can be used for die attach (die bonding), etc., and when used as a bonding material, they can achieve excellent electrical conductivity and heat dissipation while satisfying heat resistance requirements.

[0027] Sixth Example of Copper Microparticles: Copper microparticles having a coating layer made of glycol or glycol polymer, and having a volume resistivity of 1.0×10 after being baked in a pellet state in a nitrogen atmosphere at a temperature of 200° C. for 1 hour -4 The copper fine particles have a volume resistivity of 1.6 × 10 Ω cm or less. -6 The volume resistivity is 1.0×10 -4 When the resistivity is Ω·cm or less, the electrical conductivity is excellent and the heat dissipation is excellent.

[0028] When determining the volume resistivity, copper fine particles are formed into a cylindrical pellet, which is placed in an electric furnace and fired in a nitrogen atmosphere at 200°C for 1 hour. The pellet is prepared by holding the copper fine particles in a press at a pressure of 127 MPa for 10 seconds. The volume resistivity is a value obtained by measuring the above-mentioned pellet using the four-terminal method. For example, a Loresta EP ((instrument name), MCP-T360 (model)) manufactured by Mitsubishi Chemical Corporation is used as the measuring device. By measuring the volume resistivity of the pellet before and after firing, the change in volume resistivity after firing can be measured.

[0029] The copper fine particles were fired in a pellet state in a nitrogen atmosphere at a temperature of 200° C. for 1 hour, and the volume resistivity was 1.0×10 -4 The sintered copper particles have a high electrical conductivity of Ω cm or less. Furthermore, the sintered copper particles have a higher melting point and excellent heat resistance compared to solder and the like. Therefore, they can be used for die attach (die bonding) and the like. When the copper particles are used as a bonding material, they can have excellent electrical conductivity and heat dissipation properties while satisfying heat resistance requirements.

[0030] [Seventh Example of Copper Microparticles] Copper microparticles having a coating layer composed of glycol or a glycol polymer, and having a volume shrinkage rate of 20% or less after being fired in a pellet state in a nitrogen atmosphere at a temperature of 200°C for 1 hour. The lower limit of the volume shrinkage rate is 0%. When the volume shrinkage rate is 20% or less, the occurrence of cracks and the like due to volume shrinkage can be suppressed.

[0031] The volumetric shrinkage rate was calculated from the volumes of the pellets before and after firing by using a press machine as described above to prepare cylindrical pellets by holding the copper fine particles at a pressure of 127 MPa for 10 seconds, measuring the thickness and diameter of the cylindrical pellets with calipers, and then calcining the pellets. The volumetric shrinkage rate was calculated using the following formula. The pellets were fired in an electric furnace. The nitrogen atmosphere was as described above. Volumetric shrinkage rate (%) = 100 - ((volume after firing / volume before firing) x 100)

[0032] The copper microparticles have a volume shrinkage rate of 20% or less after being fired in a nitrogen atmosphere in the form of pellets at 200°C for 1 hour, thereby suppressing volume shrinkage and increasing conductivity. Furthermore, the sintered copper microparticles have a higher melting point and excellent heat resistance than solder and the like. Therefore, they can be used for die attach (die bonding), etc., and when used as a bonding material, they can achieve excellent conductivity and heat dissipation while satisfying heat resistance. The lower limit of the volume shrinkage rate after being fired in a nitrogen atmosphere in the form of pellets at 200°C for 1 hour is, for example, 0%.

[0033] [Use of Copper Microparticles] FIG. 1 is a schematic diagram showing an example of a use of copper microparticles of the present invention, and FIG. 2 is a schematic diagram showing another example of a use of copper microparticles of the present invention. Copper microparticles are used, for example, as a bonding material. More specifically, copper microparticles are used as a bonding material to bond a substrate 50 and a power semiconductor element 52 shown in FIG. 1. Copper microparticles are used for die attachment. The copper microparticles form a bonding portion 54 that bonds the substrate 50 and the power semiconductor element 52. The bonding portion 54 is formed by firing the copper microparticles, for example, at a temperature of 200°C for 1 hour in a nitrogen atmosphere. The bonding portion 54 bonds the substrate 50 and the power semiconductor element 52, physically fixing the substrate 50 and the power semiconductor element 52. The copper microparticles can also be used to bond a single substrate 50 and multiple semiconductor elements as shown in FIG. 2. Three semiconductor elements 53a, 53b, and 53c are shown as an example in FIG. 2. The three semiconductor elements 53a, 53b, and 53c are different in size. The three semiconductor elements 53a, 53b, and 53c are bonded to the substrate 50 via a bonding portion 54. Since the three semiconductor elements 53a, 53b, and 53c are different in size, when the bonding material forming the bonding portion 54 is plate-shaped or sheet-shaped, it is necessary to match the size of the bonding material to the sizes of the three semiconductor elements 53a, 53b, and 53c, and it is also necessary to align the positions of the bonding material, which results in poor workability. In contrast, when copper fine particles are used, it is not necessary to match the size of the bonding material to the sizes of the three semiconductor elements 53a, 53b, and 53c, and there is no need to align the positions of the bonding material, and bonding can be performed in a simple manner.

[0034] Sintered copper microparticles have a higher melting point and higher heat resistance than solder. Furthermore, as described above, the copper microparticles exhibit a volumetric shrinkage rate of 20% or less after being fired in pellet form in a nitrogen atmosphere at 200°C for 1 hour. Therefore, even when temperature changes occur during operation of the power semiconductor element 52, the volumetric fluctuation of the joint 54 is small, suppressing the occurrence of cracks and the like. As a result, even when the ambient temperature exceeds the melting point of the solder, the bond between the power semiconductor element 52 and the substrate 50, and the bond between the semiconductor elements 53a, 53b, and 53c and the substrate 50 are maintained, resulting in high durability. Furthermore, because the copper microparticles have a low volume resistivity after firing, they also have excellent thermal conductivity, allowing the joint 54 to efficiently conduct heat generated by the power semiconductor element 52 to the substrate 50.

[0035] The substrate 50 is, for example, Si 3 N 4 The power semiconductor element 52 is a semiconductor element using a semiconductor such as silicon carbide (SiC), gallium nitride (GaN), gallium oxide, or diamond. The semiconductor elements 53a, 53b, and 53c are semiconductor elements using a general silicon substrate. The semiconductor elements 53a, 53b, and 53c may also be power semiconductor elements. The copper microparticles are not limited to bonding with the power semiconductor element 52 or the semiconductor elements 53a, 53b, and 53c, but can also be used to bond high-frequency devices, light-emitting diodes, semiconductor lasers, and the like. As described above, copper microparticles have excellent thermal conductivity and are suitable for bonding with items that generate a large amount of heat or have a high operating temperature. In addition to the bonding between the power semiconductor element and the substrate and the bonding between the semiconductor element and the substrate, the copper microparticles can also be used for various types of wiring, such as signal wiring and conductive wiring.

[0036] [Method for producing copper microparticles] Next, an example of a method for producing copper microparticles will be described with reference to Fig. 3, but the method for producing copper microparticles of the present invention is not limited to a production method using the copper microparticle production apparatus 10 shown in Fig. 3. Fig. 3 is a schematic diagram showing an example of the copper microparticle production apparatus of the present invention. The copper microparticles described above can be obtained by the copper microparticle production apparatus 10 shown in Fig. 3 (hereinafter simply referred to as the production apparatus 10).

[0037] The manufacturing apparatus 10 includes a plasma torch 12 that generates a thermal plasma flame, a material supply device 14 that supplies raw powder of copper microparticles into the plasma torch 12, a chamber 16 that functions as a cooling tank for generating primary copper microparticles 15, a cyclone 19 that removes coarse particles having a particle size equal to or larger than a specified particle size from the primary copper microparticles 15, and a recovery unit 20 that recovers secondary copper microparticles 18 having a desired particle size classified by the cyclone 19. The chamber 16 and the cyclone 19 are connected by a connecting pipe 21a. The cyclone 19 and the recovery unit 20 are also connected by a connecting pipe 21b that is connected to an inner pipe 19e. The manufacturing apparatus 10 further includes a supply unit 40 that supplies a surface treatment agent to the primary copper microparticles 15 or the secondary copper microparticles 18. The primary copper microparticles 15 and the secondary copper microparticles 18 are both microparticles in the process of being produced as microparticles of the present invention. The copper microparticles of the present invention are obtained by surface-treating the primary copper microparticles 15 or the secondary copper microparticles 18, i.e., surface-treated copper microparticles 30. The surfaces of the copper microparticles 30 are coated with glycol or a glycol polymer, and have a coating layer made of glycol or a glycol polymer. For the material supply device 14, chamber 16, cyclone 19, and recovery section 20, various devices described in JP 2007-138287 A can be used, for example.

[0038] In this embodiment, for example, copper powder is used as a raw material for producing the microparticles. The copper powder has an average particle size appropriately set so that it can easily evaporate in the thermal plasma flame. The average particle size of the copper powder is measured using a laser diffraction method and is, for example, 100 μm or less, preferably 50 μm or less, and more preferably 15 μm or less.

[0039] The plasma torch 12 is composed of a quartz tube 12a and a high-frequency oscillation coil 12b surrounding it. A supply pipe 14a (described later) is provided at the center of the upper portion of the plasma torch 12 for supplying fine particle raw material powder into the plasma torch 12. A plasma gas supply port 12c is formed around the supply pipe 14a (on the same circumference) and has a ring shape. A power supply (not shown) that generates a high-frequency voltage is connected to the high-frequency oscillation coil 12b. When a high-frequency voltage is applied to the high-frequency oscillation coil 12b, a thermal plasma flame 24 is generated. The raw material (not shown) is evaporated by the thermal plasma flame 24, becoming a gaseous mixture. The plasma torch 12 is a processing unit that uses a gas-phase method to turn the raw material into a gaseous mixture.

[0040] The plasma gas supply unit 22 supplies plasma gas into the plasma torch 12. The plasma gas supply unit 22 is connected to the plasma gas supply port 12c via a pipe 22a. Although not shown, the plasma gas supply unit 22 is provided with a supply amount adjustment unit such as a valve for adjusting the supply amount. The plasma gas is supplied from the plasma gas supply unit 22 through the ring-shaped plasma gas supply port 12c into the plasma torch 12 in the directions indicated by arrows P and S.

[0041] The plasma gas used may be, for example, a mixture of hydrogen gas and argon gas. In this case, hydrogen gas and argon gas are stored in the plasma gas supply unit 22. Hydrogen gas and argon gas are supplied from the plasma gas supply unit 22 through the piping 22a and the plasma gas supply port 12c into the plasma torch 12 in the directions indicated by arrows P and S. Argon gas alone may be supplied in the direction indicated by arrow P. Since the plasma gas used may be a gas appropriate for the copper fine particles, such as argon gas, helium gas, hydrogen gas, or nitrogen gas, it is not necessary to use a mixture of gases as the plasma gas, as described above, and a single type of gas may be used as the plasma gas. When a high-frequency voltage is applied to the high-frequency oscillation coil 12b, a thermal plasma flame 24 is generated in the plasma torch 12.

[0042] The temperature of the thermal plasma flame 24 must be higher than the boiling point of the raw material powder. A higher temperature of the thermal plasma flame 24 is preferable because it facilitates the transition of the raw material powder to a gaseous state, but the temperature is not particularly limited. For example, the temperature of the thermal plasma flame 24 can be set to 6000°C, and theoretically it is believed to reach approximately 10000°C. The pressure atmosphere within the plasma torch 12 is preferably below atmospheric pressure. While the pressure of the below-atmospheric atmosphere is not particularly limited, it is, for example, 0.5 to 100 kPa.

[0043] The outside of the quartz tube 12a is surrounded by a concentric tube (not shown), and cooling water is circulated between this tube and the quartz tube 12a to water-cool the quartz tube 12a and prevent the quartz tube 12a from becoming too hot due to the thermal plasma flame 24 generated within the plasma torch 12.

[0044] The material supply device 14 is connected to the upper part of the plasma torch 12 via a supply pipe 14a. The material supply device 14 supplies the raw material into the thermal plasma flame 24 inside the plasma torch 12. The material supply device 14 is not particularly limited as long as it can supply the raw material into the thermal plasma flame 24. For example, the material supply device 14 supplies the raw material into the thermal plasma flame 24 in a particulate dispersed state.

[0045] When the raw material is a powder, for example, the material supply device 14 that supplies copper powder in powder form can be, as described above, for example, the one disclosed in Japanese Patent Application Laid-Open No. 2007-138287. In this case, the material supply device 14 has, for example, a storage tank (not shown) that stores the raw material, a screw feeder (not shown) that transports a fixed amount of the raw material, a dispersing section (not shown) that disperses the raw material transported by the screw feeder into primary particles before it is finally sprayed, and a carrier gas supply source (not shown).

[0046] The raw material is supplied from a carrier gas supply source under extrusion pressure to a thermal plasma flame 24 in the plasma torch 12 via a supply pipe 14a. The material supply device 14 is not particularly limited in configuration as long as it can prevent the raw material from agglomerating and disperse the raw material into the plasma torch 12 while maintaining a dispersed state. An inert gas such as argon gas is used as the carrier gas. The carrier gas flow rate can be controlled using a flow meter such as a float flow meter. The flow rate value of the carrier gas refers to the scale value of the flow meter.

[0047] The chamber 16 is provided adjacent to and below the plasma torch 12. In the chamber 16, primary copper particles 15, which are particles, are generated from the gaseous mixture without using a cooling gas. The chamber 16 also functions as a cooling tank. The cooling gas is also called a quenching gas, and argon gas or the like is used.

[0048] For example, a gas supply unit 28 that supplies a temperature regulating gas containing an inert gas is provided in the connecting pipe 21a or the connecting pipe 21b. The gas supply unit 28 supplies the temperature regulating gas containing an inert gas to the copper primary particles 15 or the copper secondary particles 18. The gas supply unit 28 has, for example, a valve 28a, and a first gas supply pipe 28b and a second gas supply pipe 28c connected to the valve 28a. The first gas supply pipe 28b is connected to the connecting pipe 21a, and the second gas supply pipe 28c is connected to the connecting pipe 21b. By switching the valve 28a, the temperature regulating gas is supplied to either the first gas supply pipe 28b or the second gas supply pipe 28c, and the temperature regulating gas is supplied into the connecting pipe 21a or the connecting pipe 21b.

[0049] The gas supply unit 28 further includes a pressure applying device (not shown) that applies extrusion pressure to the temperature adjustment gas supplied to the first gas supply pipe 28b or the second gas supply pipe 28c. The pressure applying device is, for example, a compressor or a blower. The gas supply unit 28 also includes a storage unit (not shown) that stores the temperature adjustment gas and a pressure control valve (not shown) that controls the amount of gas supplied. The temperature adjustment gas is, for example, argon gas. The temperature adjustment gas supplied from the gas supply unit 28 to the connecting pipe 21a or the connecting pipe 21b can be used to adjust the gas temperature to a desired level.

[0050] As shown in Fig. 3, the chamber 16 is provided with a cyclone 19 for classifying the copper primary particles 15 into particles of a desired particle size. The cyclone 19 includes an inlet pipe 19a for supplying the primary particles 15 from the chamber 16, a cylindrical outer cylinder 19b connected to the inlet pipe 19a and located at the top of the cyclone 19, a truncated cone section 19c extending downward from the bottom of the outer cylinder 19b and gradually decreasing in diameter, a coarse particle recovery chamber 19d connected to the bottom of the truncated cone section 19c for recovering coarse particles having a particle size equal to or larger than the desired particle size, and an inner pipe 19e protruding from the outer cylinder 19b and connected to a recovery section 20 (described later in detail). The chamber 16 and the inlet pipe 19a are connected by a connecting pipe 21a, and the primary particles 15 move to the cyclone 19 through the connecting pipe 21a. The connecting pipe 21a is a transport path for the primary particles 15.

[0051] An airflow containing primary fine particles 15 is blown from the inlet pipe 19a of the cyclone 19 along the inner peripheral wall of the outer cylinder 19b, and as a result, this airflow flows from the inner peripheral wall of the outer cylinder 19b toward the truncated cone portion 19c as shown by arrow T in Figure 3, forming a downward swirling flow. When the downward swirling flow reverses and becomes an upward flow, the balance between centrifugal force and drag forces prevents coarse particles from joining the upward flow, and they descend along the side surface of the truncated cone portion 19c and are collected in the coarse particle collection chamber 19d. Furthermore, fine particles that are more affected by drag than centrifugal force are discharged out of the cyclone 19 along with the upward flow on the inner wall of the truncated cone portion 19c via the inner pipe 19e and connecting pipe 21b.

[0052] Furthermore, a negative pressure (suction force) is generated from the recovery unit 20, which will be described later in detail, through the inner pipe 19e and the connecting pipe 21b. This negative pressure (suction force) causes the fine particles separated from the swirling airflow to be sucked in as indicated by the symbol U, and is sent to the recovery unit 20 through the inner pipe 19e and the connecting pipe 21b.

[0053] A recovery section 20 for recovering copper microparticles 30 having a desired nanometer-order particle size is provided on the extension of inner tube 19e, which is the outlet of the airflow within cyclone 19. Recovery section 20 includes recovery chamber 20a, filter 20b provided within recovery chamber 20a, and vacuum pump 29 connected via tube 20c provided below recovery chamber 20a. Copper microparticles 30 sent from cyclone 19 are sucked by vacuum pump 29 into recovery chamber 20a, where they are collected and remain on the surface of filter 20b. Note that the number of cyclones used in the above-described manufacturing apparatus 10 is not limited to one, and may be two or more, or no cyclone may be used.

[0054] The supply unit 40 supplies the surface treatment agent St to the copper fine particles downstream of the first gas supply pipe 28b in the connecting pipe 21a or downstream of the second gas supply pipe 28c in the connecting pipe 21b. The surface treatment agent St forms copper fine particles whose surfaces are coated with glycol or a glycol polymer. Here, the chamber 16 side with respect to the connecting pipe 21a is referred to as the upstream side, and the cyclone 19 side is referred to as the downstream side. The supply unit 40 has, for example, a valve 41, and a first supply pipe 41b and a second supply pipe 41c connected to the valve 41. The first supply pipe 41b is connected to the connecting pipe 21a downstream of the first gas supply pipe 28b, and the second supply pipe 41c is connected to the connecting pipe 21b downstream of the second gas supply pipe 28c. The connection position of the first supply pipe 41b on the connecting pipe 21a is referred to as P. 1 The connection position of the second supply pipe 41c on the connection pipe 21b is P 2 The connection position P of the second supply pipe 41c 2 is the connection position P of the first supply pipe 41b 1 It is further downstream than

[0055] The supply unit 40 supplies the surface treatment agent St in a temperature range where the surface treatment agent St does not denature, and to the microparticles (primary copper microparticles 15 or secondary copper microparticles 18) in a state of dispersion in the air before they are collected. More specifically, the supply unit 40 supplies the surface treatment agent St to the primary copper microparticles 15 passing through the connecting pipe 21a or the secondary copper microparticles 18 passing through the connecting pipe 21b. The primary copper microparticles 15 passing through the connecting pipe 21a or the secondary copper microparticles 18 passing through the connecting pipe 21b are microparticles in a state of dispersion in the air before they are collected. The surface treatment agent St is supplied by the supply unit 40 in a temperature range where the surface treatment agent St does not denature, and the surface treatment agent St adheres to the primary copper microparticles 15 or the secondary copper microparticles 18. This surface-treats the primary copper microparticles 15 or the secondary copper microparticles 18, forming copper microparticles 30 whose surfaces are coated with glycol or a glycol polymer. The coating of glycol or glycol polymer also prevents fusion between the copper particles 30. The surface condition of the surface-treated copper particles 30 can be examined using, for example, an FT-IR (Fourier transform infrared spectrophotometer).

[0056] The method for supplying the surface treatment agent St by the supply unit 40 is not particularly limited, and an example is a method in which the surface treatment agent St is formed into droplets and sprayed onto the copper secondary microparticles 18. As described above, the surface treatment agent St is supplied in a temperature range in which the surface treatment agent St does not denature. Specifically, the temperature range in which the surface treatment agent St does not denature is a temperature range in which glycol or glycol polymers do not denature. The temperature range in which the surface treatment agent St does not denature is a temperature range determined based on the temperature measured by simultaneous differential thermal analysis-thermogravimetry (TG-DTA). The temperature range in which the surface treatment agent St does not denature is a temperature range in which the weight loss rate of the surface treatment agent St in simultaneous differential thermal analysis-thermogravimetry is 50% by mass or less. The weight loss rate is more preferably 30% by mass or less, and even more preferably 10% by mass or less. For the simultaneous differential thermal analysis-thermogravimetry, an STA7200 (product name) from Hitachi High-Tech Science Corporation is used.

[0057] The surface treatment agent St includes glycol or glycol polymer that forms a coating layer (not shown). More specifically, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, etc. The surface treatment agent St may contain an organic solvent.

[0058] (Organic solvent) The organic solvent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the organic solvent include alcohols such as ethanol and methanol, ketones such as acetone, alkyl halides, amides such as formamide, sulfoxides such as dimethyl sulfoxide, heterocyclic compounds, hydrocarbons, esters such as ethyl acetate, and ethers. These may be used alone or in combination of two or more.

[0059] The manufacturing apparatus 10 may have a sensor (not shown) that measures the temperature of the transport path of the copper primary particles 15 or the copper secondary particles 18. The temperature measurement result of this sensor is used to determine whether or not the temperature range is within which the surface treatment agent St will not denature. In this case, the temperature measurement result is output to, for example, the supply unit 40. The supply unit 40 can determine whether or not the temperature range is within which the surface treatment agent St will not denature based on the temperature measurement result of the transport path of the copper primary particles 15 or the temperature measurement result of the transport path of the copper secondary particles 18 by the sensor. If the temperature of the transport path of the copper primary particles 15 or the copper secondary particles 18 is within the temperature range within which the surface treatment agent St will denature, for example, the flow rate of the temperature adjustment gas supplied from the gas supply unit 28 is changed. As described above, the temperature measurement result of the sensor is used to determine whether or not the temperature range is within which the surface treatment agent St will not denature. 1 It is preferable to provide the sensor upstream of the connecting pipe 21a. For this reason, the sensor is provided, for example, in the connecting pipe 21a. The configuration of the sensor is not particularly limited as long as it can measure temperature, but it is preferable that the measurement time be short. For this reason, for example, a resistance thermometer, a radiation thermometer, an infrared radiation temperature sensor, a thermistor, etc. can be used as the sensor.

[0060] Next, an example of a method for producing copper microparticles using the above-described production apparatus 10 will be described. First, copper powder having an average particle size of 15 μm or less is fed into the material supply device 14 as raw powder for the copper microparticles. Using argon gas and hydrogen gas, for example, as the plasma gas, a high-frequency voltage is applied to the high-frequency oscillation coil 12b to generate a thermal plasma flame 24 in the plasma torch 12. Next, the copper powder is gas-transported using argon gas, for example, as the carrier gas, and supplied into the thermal plasma flame 24 in the plasma torch 12 via the supply pipe 14a. The supplied copper powder evaporates in the thermal plasma flame 24 to form a gaseous mixture, and primary copper microparticles 15 are generated from the gaseous mixture in the chamber 16 without using a cooling gas.

[0061] The primary copper particles 15 obtained in the chamber 16 then pass through the connecting pipe 21a and are blown into the inlet pipe 19a of the cyclone 19 along the inner circumferential wall of the outer cylinder 19b, along with the airflow. As a result, the airflow flows along the inner circumferential wall of the outer cylinder 19b, forming a swirling flow and descending, as indicated by arrow T in FIG. 3 . When the descending swirling flow reverses and becomes an ascending flow, the balance between centrifugal force and drag forces prevents coarse particles from joining the ascending flow, causing them to descend along the side of the truncated cone portion 19c and be collected in the coarse particle collection chamber 19d. Furthermore, particles affected more by drag than centrifugal force are discharged from the inner wall of the truncated cone portion 19c along with the ascending flow and out of the cyclone 19. The discharged secondary copper particles 18 are sucked in the direction indicated by symbol U in FIG. 3 by the negative pressure (suction force) from the collection section 20 generated by the vacuum pump 29, passing through the inner pipe 19e and the connecting pipe 21b.

[0062] When the copper primary particles 15 pass through the connecting pipe 21a or the copper secondary particles 18 pass through the connecting pipe 21b, a temperature-adjusting gas is supplied from the gas supply unit 28 through the first gas supply pipe 28b into the connecting pipe 21a to cool the copper primary particles 15, or through the second gas supply pipe 28c into the connecting pipe 21b to cool the copper secondary particles 18. After the temperature-adjusting gas adjusts the copper primary particles 15 or the copper secondary particles 18 to a temperature range where the surface treatment agent St does not denature, the surface treatment agent St is further supplied from the supply unit 40 into the connecting pipe 21a in the form of, for example, a spray to the copper primary particles 15, thereby surface-treating the copper primary particles 15. Furthermore, the surface treatment agent St is supplied from the supply unit 40 into the connecting pipe 21b in the form of, for example, a spray to the copper secondary particles 18, thereby surface-treating the copper secondary particles 18. The surface-treated primary copper particles 15 or secondary copper particles 18, i.e., copper particles 30, are sent to the recovery section 20, and the copper particles 30 are recovered by the filter 20b of the recovery section 20. In this manner, the copper particles 30 are obtained.

[0063] When the copper microparticles 30 are collected in the collection section 20, the internal pressure in the cyclone 19 is preferably equal to or lower than atmospheric pressure. The particle size of the copper microparticles 30 is specified to any particle size on the order of nanometers depending on the purpose. While the present invention uses a thermal plasma flame as a heat source to form the primary copper microparticles, other gas phase methods can also be used to form the primary copper microparticles. Therefore, the gas phase method is not limited to using a thermal plasma flame, and may be, for example, a flame method for forming the primary copper microparticles. The method for producing primary microparticles using a thermal plasma flame is called a thermal plasma method.

[0064] Here, the flame method is a method of synthesizing fine particles by passing a copper-containing raw material through a flame using a flame as a heat source. In the flame method, the copper-containing raw material is supplied to the flame, and copper fine particles are generated in the flame to obtain primary copper fine particles 15. Furthermore, a surface treatment agent St is supplied to the primary copper fine particles 15 or the secondary copper fine particles 18 to produce copper fine particles. Note that the same surface treatment agent as that used in the thermal plasma method can also be used in the flame method.

[0065] The present invention is basically configured as described above. While the copper microparticles and the method for producing copper microparticles of the present invention have been described in detail above, the present invention is not limited to the above-described embodiments, and various improvements and modifications may be made without departing from the spirit and scope of the present invention.

[0066] The copper microparticles of the present invention will be described in more detail below. In the examples, copper microparticles of Examples 1 and 2 and copper microparticles of Comparative Example 1 were produced. The copper microparticles of Examples 1 and 2 and the copper microparticles of Comparative Example 1 were produced using a production apparatus 10 shown in Figure 3. The production conditions are shown below.

[0067] Example 1 In Example 1, copper powder with an average particle size of 5 μm was used as the raw material powder. The average particle size of the copper powder was measured using a particle size distribution analyzer. The particle size distribution analyzer used was an MT3300 (product name) manufactured by Microtrac Bell Co., Ltd. The production conditions for the copper microparticles were a constant plasma input of 18 kW and a fixed plasma torch internal pressure of 60 kPa. Argon gas was used as the carrier gas. The flow rate of the argon gas was 5 liters / minute (standard state equivalent). Argon gas and hydrogen gas were used as the plasma gas. The flow rate of the argon gas was 200 liters / minute (standard state equivalent), and the flow rate of the hydrogen gas was 5 liters / minute (standard state equivalent). Argon gas was used as the temperature adjustment gas. The flow rate of the argon gas was 200 liters / minute (standard state equivalent). In Example 1, triethylene glycol (molecular weight 150.17, boiling point 276°C) was used as the surface treatment agent. A solution containing ethanol as a solvent and triethylene glycol (triethylene glycol concentration: 5 W / W%) was sprayed onto the copper secondary particles 18 (see FIG. 3) from the second supply pipe 41c (see FIG. 3) using a spray gas. Argon gas was used as the spray gas. Triethylene glycol manufactured by Tokyo Chemical Industry Co., Ltd. was used. Ethanol manufactured by Junsei Chemical Co., Ltd. (product code 17065-1283) was used.

[0068] Example 2 Example 2 differs from Example 1 in that polyethylene glycol (molecular weight approximately 200, boiling point 250°C) was used as the surface treatment agent. In Example 2, ethanol was used as the solvent, and a solution containing polyethylene glycol (polyethylene glycol concentration 5 W / W%) was sprayed onto the copper secondary microparticles 18 (see FIG. 3) from the second supply pipe 41c (see FIG. 3) using a spray gas. Argon gas was used as the spray gas. In Example 2, the flow rate of argon gas used as the temperature adjustment gas was 380 liters / minute (standard condition equivalent). The polyethylene glycol used was manufactured by Tokyo Chemical Industry Co., Ltd. The ethanol used was manufactured by Junsei Chemical Co., Ltd. (product code 17065-1283).

[0069] Comparative Example 1 Comparative Example 1 differs from Example 1 in that terpineol (molecular weight 154.25, boiling point 219°C) was used as the surface treatment agent. In Comparative Example 1, ethanol was used as the solvent, and a solution containing terpineol (terpineol concentration 5 W / W%) was sprayed onto the copper secondary microparticles 18 (see FIG. 3) from the second supply pipe 41c (see FIG. 3) using a spray gas. Argon gas was used as the spray gas. In Comparative Example 1, the flow rate of argon gas used as the temperature adjusting gas was 200 liters / minute (standard condition equivalent). The terpineol used was manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. The ethanol used was manufactured by Junsei Chemical Co., Ltd. (product code 17065-1283).

[0070] Scanning electron microscope (SEM) images were obtained for the copper microparticles of Examples 1 and 2. The SEM images were obtained using a Regulus (registered trademark) 8220 (product name) manufactured by Hitachi High-Technologies Corporation. An SEM image of the copper microparticles of Example 1 is shown in FIG. 4, and an SEM image of the copper microparticles of Example 2 is shown in FIG. 5. A Macsorb HM-1208 (product name) manufactured by Mountec Co., Ltd. was used to measure the particle size of the copper microparticles of Examples 1 and 2 and the copper microparticles of Comparative Example 1 by the BET method.

[0071] For the copper microparticles of Examples 1 and 2, SEM images were obtained after calcination at a temperature of 200 ° C. for 1 hour in a nitrogen atmosphere. The SEM images were obtained using a Regulus (registered trademark) 8220 (trade name) manufactured by Hitachi High-Technologies Corporation. Figure 6 (a) is a schematic diagram showing an SEM image of the copper microparticles of Example 1 before calcination, and (b) is a schematic diagram showing an SEM image of the copper microparticles of Example 1 after calcination. Figure 7 (a) is a schematic diagram showing an SEM image of the copper microparticles of Example 2 before calcination, and (b) is a schematic diagram showing an SEM image of the copper microparticles of Example 2 after calcination.

[0072] The copper microparticles of Examples 1 and 2 and the copper microparticles of Comparative Example 1 were calcined in a particulate state in a nitrogen atmosphere at a temperature of 200°C for 1 hour, and then their particle sizes were measured based on the BET method. The results are shown in Table 1 below. The particle growth rate was calculated from the particle sizes before and after calcination. The particle growth rate was calculated using the following formula: Particle growth rate (%) = ((particle size after calcination) / (particle size before calcination)) x 100

[0073] For the copper microparticles of Examples 1 and 2 and the copper microparticles of Comparative Example 1, the coating layer removal rate at a temperature of 200°C by simultaneous differential thermal analysis and thermogravimetry, the weight loss rate at a temperature of 200°C by simultaneous differential thermal analysis and thermogravimetry, and the weight increase rate at a temperature of 200°C by simultaneous differential thermal analysis and thermogravimetry were measured. The results are shown in Table 1 below. The coating layer removal rate at a temperature of 200°C by simultaneous differential thermal analysis and thermogravimetry (TG-DTA) was measured in a nitrogen atmosphere, and is defined as the weight loss rate at a temperature of 200°C divided by the weight loss rate at a temperature of 700°C. The coating layer removal rate at a temperature of 200°C, as well as the weight loss rate and weight increase rate at a temperature of 200°C were measured by simultaneous differential thermal analysis and thermogravimetry. The weight increase rate was determined by simultaneous differential thermal analysis and thermogravimetry (TG-DTA) in an air atmosphere. Further, for the simultaneous differential thermal analysis-thermogravimetry (TG-DTA), STA7200 (trade name) manufactured by Hitachi High-Tech Science Corporation was used.

[0074] Furthermore, for the copper microparticles of Examples 1 and 2 and the copper microparticles of Comparative Example 1, cylindrical pellets were formed and calcined in a nitrogen atmosphere at 200°C for 1 hour, after which the volume resistivity and volume shrinkage were measured. The results are shown in Table 1 below. The nitrogen atmosphere was a state in which nitrogen gas with a purity of 99.99 (99.99% by volume of nitrogen) was constantly flowing, and the oxygen concentration was 3 ppm by volume or less. The oxygen concentration was measured using a low-concentration oxygen analyzer PS-820-L (trade name) manufactured by Iijima Electronics Co., Ltd. In measuring the volume resistivity, the copper microparticles were first pressed into a cylindrical pellet by holding it at a pressure of 127 MPa for 10 seconds using a press. The volume resistivity of the pellets before and after calcination was measured by the four-terminal method using a Loresta EP (instrument name, MCP-T360 (model)) manufactured by Mitsubishi Chemical Corporation. The pellets were placed in an electric furnace and calcined in a nitrogen atmosphere at 200°C for 1 hour.

[0075] In measuring the volumetric shrinkage rate, copper fine particles were first pressed using a press machine at a pressure of 127 MPa for 10 seconds to produce a cylindrical pellet. The thickness and diameter of the cylindrical pellet were measured with a vernier caliper, and the volumetric shrinkage rate was calculated from the volume of the pellet before and after firing. The following formula was used to calculate the volumetric shrinkage rate. The pellet was placed in an electric furnace and fired at a temperature of 200°C in a nitrogen atmosphere for 1 hour. Volumetric shrinkage rate (%) = 100 - ((volume after firing / volume before firing) x 100)

[0076] For the copper microparticles of Examples 1 and 2, cylindrical pellets were formed and SEM images were obtained before and after firing. The results are shown in Figures 8(a) and (b) and Figures 9(a) and (b). Figure 8(a) is a schematic diagram showing an SEM image of the pellet of copper microparticles of Example 1 before firing, and (b) is a schematic diagram showing an SEM image of the pellet of copper microparticles of Example 1 after firing. Figure 9(a) is a schematic diagram showing an SEM image of the pellet of copper microparticles of Example 2 before firing, and (b) is a schematic diagram showing an SEM image of the pellet of copper microparticles of Example 2 after firing. From Figures 8(a) and (b) and Figures 9(a) and (b), it can be seen that the copper microparticles are bonded to each other as shown in Figures 8(b) and 9(b), and sintering of the copper microparticles was confirmed. Although not shown, a cylindrical pellet was also formed for Comparative Example 1, and SEM images were obtained before and after firing. In Comparative Example 1, sintering of the copper microparticles was not confirmed. The sintering of the copper fine particles was confirmed by observation using SEM images in this way, and the results are shown in Table 1 below.

[0077] Furthermore, the crystal structure of the copper microparticles of Examples 1 and 2 and the copper microparticles of Comparative Example 1 was analyzed by X-ray diffraction. FIG. 10 shows the results of the crystal structure analysis of the copper microparticles of Examples 1 and 2 of the present invention by X-ray diffraction. FIG. 10 shows a diffraction pattern 60 of Example 1 and a diffraction pattern 62 of Example 2. As shown in FIG. 10, it has been confirmed that Examples 1 and 2 are copper microparticles. Although not shown, when the crystal structure of the copper microparticles of Examples 1 and 2 was analyzed by X-ray diffraction after 3 weeks, it was confirmed that the crystal structure analysis results were similar to those of FIG. 10. Furthermore, for the copper microparticles of Examples 1 and 2, pellets were prepared again 1 week and 2 weeks after the preparation of the copper microparticles, and the pellets were baked in a nitrogen atmosphere at a temperature of 200 ° C. for 1 hour, and the volume resistivity was measured. The results shown in FIG. 11 were obtained. No significant change in volume resistivity was observed in either Example 1 or Example 2. FIG. 11 is a graph showing the change over time in the volume resistivity of the copper microparticles of Examples 1 and 2 of the present invention.

[0078]

[0079] As shown in Table 1, the copper microparticles of Examples 1 and 2 had a larger particle growth rate, calculated from the particle size before calcination and the particle size after heating in a particle state at 200°C for 1 hour in a nitrogen atmosphere, than the copper microparticles of Comparative Example 1, and sintering was also confirmed. For the copper microparticles of Examples 1 and 2, sintering was confirmed after forming cylindrical pellets and calcining them at 200°C for 1 hour in a nitrogen atmosphere. Furthermore, the copper microparticles of Examples 1 and 2 had a lower volume resistivity and a larger volume shrinkage rate than the copper microparticles of Comparative Example 1 after forming cylindrical pellets and calcining them at 200°C for 1 hour in a nitrogen atmosphere. Note that in Comparative Example 1, the coating layer removal rate at 200°C measured by simultaneous differential thermal and thermogravimetry was less than 30% by mass. This indicates that the copper microparticles of Comparative Example 1 cannot be bonded together well. Furthermore, the weight loss rate at 200°C measured by simultaneous differential thermal and thermogravimetry was less than 0.25% by mass, indicating that the copper microparticles of Comparative Example 1 cannot be bonded together well. Furthermore, in Comparative Example 1, the weight increase rate at 200° C. measured by simultaneous differential thermal and thermogravimetric measurements exceeded 5% by mass, and therefore the copper fine particles could not be bonded together satisfactorily.

[0080] DESCRIPTION OF SYMBOLS 10 Copper microparticle manufacturing apparatus (manufacturing apparatus) 12 Plasma torch 12a Quartz tube 12b High frequency oscillation coil 12c Plasma gas supply port 14 Material supply device 14a Supply pipe 15 Primary microparticles 16 Chamber 18 Secondary microparticles 19 Cyclone 19a Inlet pipe 19b Outer cylinder 19c Circular truncated cone portion 19d Coarse particle recovery chamber 19e Inner pipe 20 Recovery section 20a Recovery chamber 20b Filter 21a, 21b Connecting pipe 22 Plasma gas supply section 22a Piping 24 Thermal plasma flame 28 Gas supply section 28a Valve 28b First gas supply pipe 28c Second gas supply pipe 29 Vacuum pump 30 Copper microparticles 40 Supply section 41 Valve 41b First supply pipe 41c Second supply pipe 50: Substrate 52: Power semiconductor element 53: Semiconductor element 54: Joint 60, 62: Diffraction patterns St: Surface treatment agent

Claims

1. Copper particles that have a coating layer made of glycol or glycol polymer and exist as individual particles.

2. The copper microparticles according to claim 1, wherein the glycol or the glycol polymer has a molecular weight of 300 or less.

3. Copper microparticles having a coating layer composed of glycol or a glycol polymer, existing as particles alone, and having a removal rate of the coating layer of 30% by mass or more at 200°C in a nitrogen atmosphere as determined by simultaneous differential thermal and thermogravimetric measurements.

4. Copper microparticles having a coating layer composed of glycol or glycol polymer, existing as particles alone, and exhibiting a weight loss rate of 0.25% or more at 200°C in a nitrogen atmosphere as determined by simultaneous differential thermal and thermogravimetric measurements.

5. Copper particles having a coating layer composed of glycol or glycol polymer, existing as particles alone, and exhibiting a weight increase of 5% or less at 200°C in an air atmosphere as determined by simultaneous differential thermal and thermogravimetric measurements.

6. Copper particles that have a coating layer composed of glycol or glycol polymer, exist as particles alone, and have a particle growth rate of 105% or more based on the BET method after being heated in a nitrogen atmosphere at 200°C for 1 hour.

7. A coating layer made of glycol or glycol polymer, which exists as a single particle, and has a volume resistivity of 1.0 x 10 after baking in a pellet state in a nitrogen atmosphere at a temperature of 200°C for 1 hour. -4 Copper particles having a resistivity of Ω·cm or less.

8. Copper microparticles having a coating layer composed of glycol or glycol polymer, existing as individual particles, and having a volume shrinkage rate of 20% or less after being fired in a pellet state in a nitrogen atmosphere at a temperature of 200°C for one hour.

9. The copper fine particles according to any one of claims 1 to 8, having a particle size of 20 to 400 nm as measured by the BET method.

10. A method for producing copper microparticles having a coating layer composed of glycol or a glycol polymer, comprising the steps of: supplying a carrier gas in which copper powder is dispersed into a thermal plasma flame to generate microparticles; and supplying a surface treatment agent containing glycol or a glycol polymer to the microparticles in a temperature range in which the surface treatment agent is not denatured, and to the microparticles in an air-dispersed state before the microparticles are recovered.

11. A method for producing copper microparticles as described in claim 10, wherein the plasma gas of the thermal plasma flame is argon gas, helium gas, hydrogen gas or nitrogen gas.

Citation Information

Patent Citations

  • Copper particulate for paste for firing and method for forming fired copper film

    JP2012243655A

  • Copper cluster, mixed particles, conductive paste, and conductive ink

    JP2020100893A

  • Paste composition, semiconductor device, and electrical / electronic component

    WO2019093119A1