Method for producing conductive base material, method for producing electronic device, method for producing electromagnetic shield film, method for producing sheet-like heating element and conductive composition

The method addresses the complexity and inefficiency of existing conductive film manufacturing by using a conductive composition with corrosion-suppressing compounds and optimized particle size distribution to form conductive films with low specific resistance, enhancing conductivity through effective particle bonding.

WO2024204361A1PCT designated stage expired Publication Date: 2024-10-03SATO HLDG CORP

Patent Information

Application Number
PCT/JP2024/012270
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for manufacturing conductive films with low specific resistance are either complex or do not effectively prevent corrosion and aggregation of conductive particles, which impede the formation of highly conductive films.

Method used

A method involving a conductive composition with conductive particles, such as copper or silver, and a compound that suppresses corrosion and aggregation, combined with pressure to form a conductive film, where the compound includes ligands that coordinate with the particles and reducing agents to enhance conductivity, and optimized particle size distribution for improved particle integration.

Benefits of technology

The method achieves a conductive film with low specific resistance by preventing particle oxidation and aggregation, allowing for effective metal bonding and improved conductivity, even with minimal pressure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012270_03102024_PF_FP_ABST
    Figure JP2024012270_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed is a method for producing a conductive base material, the method comprising: a film formation step in which a film that is formed of a conductive composition is provided on a base material; and a conductive film formation step in which a conductive film is formed by at least pressurizing the film. A conductive composition which contains conductive particles (A) that contain at least one element selected from the group consisting of copper and silver, and a compound (B) that suppresses one or both of corrosion and agglomeration of the conductive particles (A) is used in this method for producing a conductive base material.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing conductive substrate, method for manufacturing electronic device, method for manufacturing electromagnetic wave shielding film, method for manufacturing sheet heating element, and conductive composition

[0001] The present invention relates to a method for producing a conductive substrate, a method for producing an electronic device, a method for producing an electromagnetic wave shielding film, a method for producing a sheet heating element, and a conductive composition.

[0002] A technique for forming a conductive substrate having a conductive film is known, in which a conductive composition containing conductive particles is applied to a substrate to form a coating layer, and the coating layer is then heated and pressurized. As an example, Patent Document 1 (JP-A-2005-102626) describes a process in which a dispersion of silver microparticles with an average primary particle size of 7 nm in water / ethylene glycol is applied to a PET film to form a coating film, which is then heated and pressurized at 150°C to form a conductive layer. As another example, Patent Document 2 (JP-A-2005-102626) describes a process in which a copper microparticle dispersion (copper nanoink) containing copper microparticles (copper nanoparticles) with a median diameter of approximately 40 nm, a dispersion medium, and a dispersant is spin-coated onto a glass substrate to form a coating film, which is then baked to form a conductive film. As yet another example, Patent Document 3 (JP-A-2005-102626) describes a process in which a conductive ink composition containing (A) an oxycarboxylic acid, (B) a nitrogen-containing compound, (C) copper particles, and (D) a dispersion medium is applied to a substrate to form a coating film, and the coating film is then treated to form a conductive layer.

[0003] Japanese Patent No. 6181608 Japanese Patent Application Laid-Open No. 2021-044308 Japanese Patent Application Laid-Open No. 2017-191723

[0004] When forming a conductive film using a conductive composition containing conductive particles, it is preferable that the resistivity of the conductive film be as low as possible. It is also more preferable that a conductive film with low resistivity can be produced by a simple and not too complicated process.

[0005] The present invention has been made in view of the above circumstances, and one of its objects is to provide a method for producing a conductive substrate that allows the formation of a conductive film with low resistivity.

[0006] The present inventors have completed the invention provided below and solved the above problems.

[0007] 1. A method for producing a conductive substrate, comprising: a film-forming step of providing a film made of a conductive composition on a substrate; and a conductive film-forming step of applying at least pressure to the film to form a conductive film, wherein the conductive composition comprises: conductive particles (A) containing at least any element selected from the group consisting of copper and silver; and a compound (B) that suppresses one or both of corrosion and aggregation of the conductive particles (A). 2. A method for producing a conductive substrate according to 1., wherein the substrate is flexible. 3. A method for producing a conductive substrate according to 1. or 2., wherein the conductive film-forming step involves applying pressure while heating the film. 4. A method for producing a conductive substrate according to any one of 1. to 3., wherein the compound (B) contains a ligand (B1) capable of coordinating to copper or silver in the conductive particles (A). 5. 4. 6. A method for producing a conductive substrate according to item 4 or 5, wherein the ligand (B1) comprises at least one compound selected from the group consisting of amines, imines, phosphines, azoles, and carboxylic acids. 7. A method for producing a conductive substrate according to any one of items 1 to 6, wherein the compound (B) comprises a reducing agent (B2). 8. A method for producing a conductive substrate according to item 7, wherein the reducing agent (B2) comprises at least one compound selected from the group consisting of ascorbic acid, oxalic acid, and formic acid. 9. A method for producing a conductive substrate according to any one of items 1 to 9, wherein the compound (B) comprises a nitrile compound (B3). 10. A method for producing a conductive substrate according to any one of items 1 to 9. 2. The method for producing a conductive substrate according to claim 1, wherein the conductive particles (A) have a particle diameter D at which a cumulative frequency of 50% is obtained in a volume-based cumulative particle diameter distribution curve obtained by measuring the particle diameters of the conductive particles (A) by a laser diffraction scattering method. 50is 0.6 to 50 μm. 11. A method for producing a conductive substrate according to any one of 1. to 10., wherein the amount of binder in all non-volatile components of the conductive composition is 5 mass % or less. 12. A method for producing a conductive substrate according to any one of 1. to 11., wherein the conductive film forming step includes a roll press step of transporting the substrate on which the film has been provided between two opposing rolls. 13. A method for producing a conductive substrate according to 12., wherein in the roll press step, the roll of the two rolls that comes into contact with the film is not heated or is heated to 400° C. or less. 14. A method for producing a conductive substrate according to 12. or 13., wherein in the roll press step, a pressure of 10 to 150 MPa is applied to the substrate on which the film has been provided. 15. A method for producing a conductive substrate according to 1. to 14. 16. A method for producing a conductive substrate according to any one of 1. to 15., wherein the conductive film has a patterned structure. 16. A method for producing an electronic device, comprising producing an electronic device using a conductive substrate obtained by the method for producing a conductive substrate according to any one of 1. to 15. 17. A method for producing an electronic device according to 16., wherein the electronic device is an RF tag. 18. A method for producing an electromagnetic wave shielding film, comprising producing an electromagnetic wave shielding film using a conductive substrate obtained by the method for producing a conductive substrate according to any one of 1. to 15. 19. A method for producing a planar heating element, comprising producing a planar heating element using a conductive substrate obtained by the method for producing a conductive substrate according to any one of 1. to 15. 20. A conductive composition containing conductive particles, used in applications in which a film is formed on a substrate and the film is at least pressed to form a conductive film, the conductive composition comprising: conductive particles (A) containing at least one element selected from the group consisting of copper and silver, and a compound (B) that suppresses one or both of corrosion and aggregation of the conductive particles (A).21. The conductive composition according to 20., wherein the compound (B) comprises a ligand (B1) capable of coordinating with copper or silver in the conductive particles (A). 22. The conductive composition according to 21., wherein the ligand (B1) comprises at least one compound selected from the group consisting of amines, imines, phosphines, azoles, and carboxylic acids. 23. The conductive composition according to 21. or 22., wherein the ligand (B1) comprises at least one selected from the group consisting of monodentate ligands and bidentate ligands. 24. The conductive composition according to any one of 20. to 23., wherein the compound (B) comprises a reducing agent (B2). 25. The conductive composition according to 24., wherein the reducing agent (B2) comprises at least one selected from the group consisting of ascorbic acid, oxalic acid, and formic acid. 26. The conductive composition according to 20. 27. The conductive composition according to any one of 20. to 25., wherein the compound (B) comprises a nitrile compound (B3). 27. The conductive composition according to any one of 20. to 26., wherein the conductive particles (A) have a particle diameter D at which a cumulative frequency of 50% is obtained in a volume-based cumulative particle diameter distribution curve obtained when the particle diameters of the conductive particles (A) are measured by a laser diffraction scattering method. 50 28. The conductive composition according to any one of 20. to 27., wherein the amount of the binder in the total non-volatile components is 5 mass % or less.

[0008] According to the present invention, it is possible to form a conductive film with low resistivity.

[0009] It is a figure for demonstrating a film forming step, a figure for demonstrating a conductive film forming step, a figure for demonstrating a conductive film forming step, and a figure for demonstrating a conductive film forming step.

[0010] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. In all drawings, similar components are given the same reference numerals, and descriptions thereof will be omitted where appropriate. To avoid complexity, (i) when multiple identical components are present in the same drawing, only one of the components is given a reference numeral, and not all of the components are given a reference numeral, or (ii) particularly in Figure 2 and subsequent figures, components similar to those in Figure 1 are not given a reference numeral again. All drawings are for illustrative purposes only. The shapes and dimensional ratios of each component in the drawings do not necessarily correspond to actual objects.

[0011] In this specification, unless otherwise specified, the expression "X to Y" in the description of a numerical range means at least X and at most Y. For example, "1 to 5% by mass" means "at least 1% by mass and at most 5% by mass."

[0012] <Method for manufacturing conductive substrate> The method for manufacturing a conductive substrate of this embodiment includes a film forming step of providing a film made of a conductive composition containing conductive particles on a substrate, and a conductive film forming step of applying at least pressure to the film to form a conductive film. Each step will be specifically described below with reference to the drawings.

[0013] (FIG. 1: Film Forming Step) In the film forming step, a conductive composition containing conductive particles is applied, printed, or otherwise applied to the substrate 1 (on at least one surface of the substrate 1) to provide a film 3. Here, the conductive composition contains conductive particles (A) containing at least one element selected from the group consisting of copper and silver, and a compound (B) that suppresses either or both of corrosion and aggregation of the conductive particles (A).

[0014] Through their own investigations, the present inventors have concluded that when forming a conductive film by a conventional method, (i) an oxide film present on the surface of conductive particles may prevent the formation of a conductive film with high conductivity, or (ii) unintended aggregation of conductive particles may prevent the formation of a conductive film with high conductivity. Based on this idea, the present inventors have decided to use, as the conductive particles contained in a conductive composition, "conductive particles containing at least one element selected from the group consisting of copper and silver" (conductive particles (A)), which have high conductivity and are suitable for forming a conductive film by pressing, in combination with a compound (B) that suppresses one or both of the corrosion and aggregation of the conductive particles (A). Then, by forming a conductive film by at least pressing using a conductive composition containing conductive particles (A) and compound (B), the conductivity of the conductive film could be improved.

[0015] Incidentally, in the conductive film forming process, if the compound (B) is present on or near the surface of the conductive particles (A), it seems that the metallic bond between the conductive particles (A) is hindered. However, according to the findings of the present inventors, it is likely that at least a portion of the compound (B) present on or near the surface of the conductive particles (A) is "detached" from the surface or near the conductive particles (A) due to the pressure applied in the conductive film forming process. Therefore, even if the compound (B) is present on or near the surface of the conductive particles (A), it is believed that the conductive particles (A) can be bonded to each other, and a conductive film with good conductivity can be obtained.

[0016] The film forming step will be described in more detail below.

[0017] Particle size distribution of conductive particles (A) In the volume-based cumulative particle size distribution curve obtained when the particle size of the conductive particles (A) is measured by a laser diffraction scattering method, the particle size (median size) at which the cumulative frequency is 50% is defined as D 50 The particle diameter at which the cumulative frequency is 10% is D 10 The particle diameter at which the cumulative frequency is 90% is D 90 Let's say.

[0018] D 50is preferably 0.6 to 30 μm, more preferably 0.7 to 20 μm, and even more preferably 0.7 to 15 μm. By using conductive particles (A) having an appropriate median diameter, a good balance is achieved between the ease of particle integration when pressure is applied and the reduction in resistance due to fewer boundaries between particles, thereby further increasing the conductivity of the resulting conductive film.

[0019] Also, (D 90 -D 50 ) / D 50 is preferably 0.55 to 3.0, more preferably 0.55 to 2.5, and even more preferably 0.55 to 2.0. (D 90 -D 50 ) / D 50 The value of D is 3.0 or less. 50 Based on this, relatively D 90 This means that the ratio of coarse particles is small and the amount of coarse particles is relatively small. A small ratio of coarse particles in the conductive particles (A) makes it difficult for "gaps" to form between the conductive particles (A), and further improvement in the conductivity of the conductive film can be expected. Incidentally, the lower limit of 0.6 was set in consideration of the particle size distribution of conductive particles that are easily available industrially.

[0020] Furthermore, (D 50 -D 10 ) / D 50 is preferably 0.4 to 0.8, more preferably 0.4 to 0.7, and even more preferably 0.5 to 0.7. In order to improve the conductivity of the conductive film obtained by at least pressurizing a film containing the conductive particles (A), it is preferable to increase the density of the conductive particles (A) in the film. One possible method for achieving this is to adjust and optimize the particle size distribution of the conductive particles (A) so that an appropriate amount of particles with relatively small particle sizes are present in the "gaps" between particles with relatively large diameters. (D 50 -D 10 ) / D 50 is the particle diameter D 50This can be interpreted as meaning that an appropriate amount of particles having a particle size smaller than that of nearby particles are present in the conductive particles (A). It is also thought that the inclusion of a "certain amount" of submicron-sized conductive particles (A) has a certain degree of sintering-promoting effect.

[0021] D of a certain conductive particle (A) 50 When the conductive particles (A) are purchased and the supplier provides a volume-based cumulative particle size distribution curve for the conductive particles (A), the values ​​of D etc. are calculated based on the curve. 50 You can get the value of D from the supplier. 50 If the value itself is provided, such as 50 When values ​​such as σ cannot be known, the particle size of the conductive particles (A) is measured by a laser diffraction scattering method to obtain a volume-based cumulative particle size distribution curve. Measurement is usually performed wet. In this case, examples of the dispersion medium include water containing a surfactant and isopropanol (an appropriate dispersion medium can be selected taking into consideration the state of the surface treatment agent on the conductive particles (A)). Examples of measurement devices include the SALD series (SALD-2300, etc.) from Shimadzu Corporation. When using the SALD series as the device, it is preferable to measure the particle size while circulating the dispersion medium and generating ultrasonic waves using the attached ultrasonic unit.

[0022] Chemical Composition of Conductive Particles (A) As mentioned above, the conductive particles (A) preferably contain at least one element selected from the group consisting of silver and copper. Specifically, the conductive particles (A) preferably contain at least one element selected from the group consisting of particles primarily composed of silver and particles primarily composed of copper. Here, the expression "mainly composed of silver" means that the ratio of silver element to all constituent elements in the particle is preferably 50 mol% or more, more preferably 75 mol% or more, even more preferably 90 mol% or more, and particularly preferably 95 mol% or more. Similarly, the expression "mainly composed of copper" means that the ratio of copper element to all constituent elements in the particle is preferably 50 mol% or more, more preferably 75 mol% or more, even more preferably 90 mol% or more, and particularly preferably 95 mol% or more. Just to be clear, as long as the desired conductivity is obtained, the conductive particles (A) may contain elements other than silver and copper, or may be substantially free of them. Examples of elements other than silver and copper include gold, aluminum, platinum, palladium, iridium, tungsten, nickel, tantalum, lead, zinc, etc. Here, "substantially free" means that the ratio of elements other than silver and copper in the conductive particles (A) is, for example, 1% by mass or less, specifically 0.5% by mass or less, and more specifically 0.1% by mass or less.

[0023] The conductive particles (A) may contain only one element, or may contain two or more elements. For example, conductive particles in which the surface of copper particles is silver-plated (silver-coated copper particles) are preferably used in this embodiment. The silver-coated copper particles are particles containing copper as the main component, and for example, up to 35 mass% of silver based on the total mass of the particles is plated on the surface of the copper particles.

[0024] - Method for Obtaining Conductive Particles (A) The conductive particles (A) that can be used in this embodiment can be purchased from, for example, Dowa Electronics Co., Ltd., Fukuda Metal Foil and Powder Co., Ltd. Incidentally, two or more different conductive particles (A) may be mixed and used in order to adjust and optimize the particle size distribution.

[0025] Proportion of the conductive particles (A) in the conductive composition: From the viewpoint of further reducing the specific resistance of the conductive film, it is preferable that the proportion of the conductive particles (A) in the conductive composition is large. Specifically, the proportion of the conductive particles (A) in the total non-volatile components of the conductive composition is preferably 95% by mass or more, more preferably 97% by mass or more, even more preferably 98% by mass or more, and particularly preferably 99% by mass or more.

[0026] Compound (B) As the compound (B), any compound having a function of suppressing either or both of corrosion and aggregation of the conductive particles (A) can be used without any particular limitation.

[0027] An example of a preferred compound (B) is a ligand (B1) that can coordinate to copper or silver in the conductive particles (A). When the ligand (B1) coordinates to copper or silver in the conductive particles (A), oxidation of the surface of the conductive particles (A) can be suppressed. This can further increase the conductivity of the conductive film that is formed. In the conductive film formation step described below, it is believed that at least a portion of the ligand (B1) coordinated to the conductive particles (A) is detached from the surface of the conductive particles (A) by the action of pressure, resulting in the formation of "unoxidized portions" on the surface of the conductive particles (A). It is believed that bonding of these "unoxidized portions" forms a conductive film with high conductivity.

[0028] The ligand (B1) is preferably at least one compound selected from the group consisting of amines, imines, phosphines, azoles, and carboxylic acids. Specific examples of amines include 2-{[(2-dimethylamino)ethyl]methylamino}ethanol, 1,2-propanediamine, 1,2-cyclohexanediamine, monoethanolamine, diethanolamine, and triethanolamine. Specific examples of imines include diimines, ethyleneimine, propyleneimine, hexamethyleneimine, benzophenoneimine, and methyl ethyl ketoneimine. Specific examples of phosphines include phosphinic acid and various compounds known as phosphine ligands in the field of organometallic chemistry. Phosphine ligands are represented, for example, by the general formula PRR'R''. In this general formula, R, R', and R'' each independently represent a hydrogen atom or a monovalent organic group, and examples of the monovalent organic group include an alkyl group and an aryl group. Specific examples of azoles include triazole, tetrazole, benzotriazole, tolyltriazole, aminotriazole, aminobenzimidazole, pyrazole, imidazole, aminotetrazole, and derivatives thereof. Specific examples of carboxylic acids include adipic acid, gluconic acid, lactic acid, citric acid, tartaric acid, malic acid, glycolic acid, malonic acid, acetic acid, propionic acid, succinic acid, lactic acid, and derivatives thereof. Of course, compounds other than those listed above that can be coordinated to the conductive particles (A) can also be used as the ligand (B1) without any particular limitation.

[0029] Particularly preferred examples of the ligand (B1) include at least one selected from the group consisting of monodentate ligands and bidentate ligands. As described above, in the conductive film-forming process described below, it is believed that at least a portion of the ligand (B1) coordinated to the conductive particles (A) is detached from the conductive particles (A) by the action of pressure, resulting in the formation of "unoxidized or slightly oxidized portions" on the surfaces of the conductive particles (A). These "unoxidized or slightly oxidized portions" are then bonded together by pressure, forming a conductive film with high conductivity. Monodentate and bidentate ligands do not have too strong an interaction with the conductive particles (A), and are therefore likely to detach from the surfaces of the conductive particles (A) when pressure is applied in the conductive film-forming process. This is believed to make it easier for the surfaces of the unoxidized conductive particles (A) to come into contact with each other. Due to this mechanism, it is believed that using a monodentate or bidentate ligand as the ligand (B1) can further increase the conductivity of the conductive film and sufficiently bond the conductive particles (A) together even when a relatively small pressure is applied.

[0030] Specific examples of monodentate and bidentate ligands include those corresponding to monodentate or bidentate ligands from among the examples given above as the ligand (B1). Incidentally, in coordination involving π electrons, whether a certain ligand is monodentate or multidentate is determined based on its "hapto number." That is, a ligand with a hapto number of 1 is classified as a monodentate ligand. Furthermore, a ligand with a hapto number of 3 is classified as a tridentate ligand, which is a type of multidentate ligand.

[0031] Another example of the compound (B) is a reducing agent (B2). It is believed that the action of the reducing agent (B2) leaves at least a portion of the surface of the conductive particle (A) unoxidized or only slightly oxidized. The reducing agent (B2) can be ascorbic acid, oxalic acid, formic acid, or the like. Here, carboxylic acids with reducing properties are classified as reducing agents (B2) rather than ligands (B1). Other specific examples of reducing agents include hydrazine, hydrazine hydrate, sodium, carbon, potassium iodide, iron (II) sulfide, sodium thiosulfate, tin (II) chloride, diisobutylaluminum hydride, sodium borohydride, and sulfites.

[0032] Another example of compound (B) is a nitrile compound (B3), i.e., a compound having a nitrile group. It is believed that the nitrile compound (B3) inhibits oxidation of the conductive particles (A) by adsorbing the nitrile group to the surface of the conductive particles (A). Examples of the nitrile compound (B3) include various organic compounds having a nitrile group. Specifically, alkanenitriles are preferred. The alkanenitrile may have, for example, 1 to 20 carbon atoms. From another perspective, the boiling point of the nitrile compound (B3), such as alkanenitrile, under normal pressure is preferably 340°C or lower. It is believed that nitrile compounds (B3) with low boiling points are more likely to detach from or near the surface of the conductive particles (A) due to the pressure in the conductive film formation process. This is believed to enable the production of a conductive film with even better conductivity.

[0033] Another example of the compound (B) is the dispersant (B4). The use of the dispersant (B4) can suppress unintended aggregation of the conductive particles (A) before the conductive film-forming step. As a result, it is possible to reduce the "gaps" between the conductive particles (A) in the conductive film-forming step, which is thought to further increase the conductivity of the resulting conductive film.

[0034] Examples of the dispersant (B4) include polyolefin resins, polyvinyl alcohol resins, polyalkylene glycol resins, polyvinylpyrrolidone resins, polyester resins, polyamide resins, acrylic resins, urethane resins, and epoxy resins. The dispersant (B4) may be selected from known surfactants that can function as a dispersant.

[0035] The conductive composition may contain only one compound (B) or two or more compounds (B). By using two or more different compounds (B), some synergistic or complementary action may be exerted, further enhancing the oxidation suppression effect on the surface of the conductive particles (A), and the resulting conductive film may have even higher conductivity. For example, a preferred embodiment is the combined use of the nitrile compound (B3) with the ligand (B1) and / or the reducing agent (B2).

[0036] Optimizing the amount of compound (B) used can further increase the conductivity of the final conductive film. Using a relatively large amount of compound (B) can sufficiently suppress oxidation of the surfaces of the conductive particles (A) and sufficiently suppress aggregation of the conductive particles (A). On the other hand, using an inappropriate amount of compound (B) increases the ratio of the "conductive components" (copper, silver) in the conductive composition, thereby further increasing the conductivity of the final conductive film. Furthermore, during the conductive film formation process, unoxidized or slightly oxidized portions of the surfaces of the conductive particles (A) are more likely to be exposed, thereby further increasing the conductivity of the final conductive film. Specifically, the amount of compound (B) (the total amount when two or more compounds (B) are used) is preferably 0.01 to 10 parts by mass, more preferably 0.03 to 5 parts by mass, per 100 parts by mass of the conductive particles (A).

[0037] Other Components The conductive composition may contain components other than the conductive particles (A) and the compound (B).

[0038] The conductive composition may contain a solvent. When the conductive composition contains a solvent, the film-forming properties of the conductive composition on a substrate are improved. The solvent typically contains an organic solvent. The type of solvent is not particularly limited. Any solvent may be used as long as it does not substantially alter the components in the conductive composition. The amount of solvent used may be adjusted appropriately depending on the application / printing method of the conductive composition, etc. The amount of solvent used is, for example, 3 to 35 mass %, preferably 5 to 30 mass %, and more preferably 10 to 30 mass % of the total conductive composition.

[0039] The conductive composition may or may not contain a binder, depending on factors such as adhesion to the substrate 1, film-forming properties, and printability. When a binder is used, the type of binder is not particularly limited, but preferred examples include polyvinylpyrrolidone, polyester, epoxy resin, (meth)acrylic resin, polyvinyl acetal, cellulose-based resin (e.g., ethyl cellulose), and phenolic resin. From the viewpoint of maintaining the conductivity of the conductive film, the amount of binder in the total non-volatile components of the conductive composition is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less. The lower limit of the binder amount may be 0. However, when actively obtaining effects such as improved adhesion by using a binder, the amount of binder is preferably 1% by mass, and more preferably 2% by mass or more, of the total non-volatile components of the conductive composition. That is, from the viewpoint of balancing various performances, the amount of binder is preferably 1 to 5% by mass, more preferably 2 to 5% by mass, of the total non-volatile components of the conductive composition.

[0040] The conductive composition may or may not contain various additive components found in conventional ink compositions and conductive pastes.

[0041] Substrate 1 The substrate 1 is usually in the form of a film, sheet, or plate. From the viewpoint of industrial productivity, the shape of the substrate 1 is preferably one of these. The substrate 1 is preferably flexible. By employing a flexible substrate 1, a flexible printed circuit (FPC) can be manufactured. In addition, a flexible substrate 1 has the advantage that it is easy to form a conductive film by a roll press process in the conductive film forming process described later. Just to be clear, the substrate 1 may be a rigid substrate that does not have flexibility.

[0042] Considering cost and end use, the substrate 1 is preferably at least one selected from the group consisting of polyesters such as PET (polyethylene terephthalate) and PEN (polyethylene naphthalate), polyolefins such as polyethylene and polypropylene, polyimide, and paper. Here, the paper may be coated paper (paper whose surface is coated with a coating agent) or ordinary uncoated paper. Furthermore, the substrate 1 is not limited to PET and other materials, and general resin films can also be used. As will be described later, in this embodiment, a conductive film with sufficiently low resistivity can be obtained without heating or even with heating at a relatively low temperature in the conductive film formation process. Therefore, substrates 1 with low heat resistance, such as polyester, polyolefin, and paper, can also be suitably used as the substrate. Furthermore, when a highly heat-resistant substrate 1, such as polyimide, is used, high-temperature heating in the conductive film formation process can further reduce the resistivity.

[0043] -Film Formation Method The method for forming a film of the conductive composition is not particularly limited. The conductive composition may be formed as a film over the entire surface of the substrate, or may be formed as a film only over a portion of the surface of the substrate. In the former case, film formation (application) can be performed using devices such as a blade coater, air knife coater, doctor coater, roll coater, bar coater (rod coater), or curtain coater. In the latter case, various printing methods, such as screen printing, gravure printing, letterpress printing, lithographic printing (offset printing), and inkjet printing, can be applied. By appropriately designing the "pattern" for film formation, it is possible to produce a substrate with a pattern structure, such as a conductive film that can function as a circuit (circuit pattern) or a mesh pattern with electromagnetic wave shielding properties. When forming a film of the conductive composition over only a portion of the surface of the substrate, it is preferable that the "pattern" for film formation be appropriately designed depending on the intended use of the final conductive film. To prevent the conductive composition from being formed in areas other than the desired location, for example, a process may be performed in which a film with holes is placed on the substrate 1, a film of the conductive composition is formed on top of it, and then the film is removed.

[0044] From the viewpoint of obtaining sufficient conductivity when formed into a conductive film and from the viewpoint of ease of film formation, the thickness of the film 3 (dry thickness when the conductive composition contains a solvent) is preferably 5 to 100 μm, more preferably 10 to 50 μm.

[0045] In particular, when the conductive composition contains a solvent, it is preferable to perform a heat treatment to dry the solvent. The conditions for the heat treatment are not particularly limited as long as the solvent is sufficiently dried, but from the viewpoint of sufficiently drying the solvent and preventing the conductive particles from being altered by excessive heating, the heat treatment temperature is preferably 50 to 150°C, more preferably 80 to 120°C. The heat treatment time is preferably 1 to 60 minutes, more preferably 3 to 30 minutes. Specifically, the heat treatment to dry the solvent can be performed by applying hot air to the film 3. Of course, the heat treatment may be performed by other methods.

[0046] (FIG. 2: Conductive film forming process) In the conductive film forming process, at least pressure is applied to the film 3 to form a conductive film. FIG. 2 schematically shows a case where a roll press is used as the pressure applying means. When a roll press is used as the pressure applying means, in the conductive film forming process, the substrate 1 provided with the film 3 is sandwiched between two opposing rolls 10A and 10B. The sandwiched substrate 1 is transported from left to right in FIG. 2 by the force of the rotation of the rolls 10A and 10B (indicated by arrows in FIG. 2 ), etc.

[0047] In the roll press process, a pressure of 10 MPa or more is preferably applied to the substrate 1 on which the film 3 is provided. This pressure is more preferably 10 to 5000 MPa, even more preferably 20 to 300 MPa, and particularly preferably 30 to 250 MPa. A pressure of 10 MPa or more can further reduce the resistivity of the resulting conductive film. Furthermore, a pressure of 5000 MPa or less can suppress damage to the substrate 1 and the film 3. Incidentally, if the substrate 1 has sufficient strength, the pressure can be increased to further reduce the resistivity of the conductive film.

[0048] In the conductive film formation process, it is preferable to heat and pressurize the film 3. When heating the film 3, the heating temperature can be appropriately set depending on the heat resistance of the substrate 1, the type of conductive particles used, and other factors. For example, when the substrate 1 is made of a low-heat-resistant material such as polyester, polyolefin, or paper, the heating temperature is preferably set within the range of, for example, 50 to 200°C, more preferably 70 to 180°C, even more preferably 70 to 150°C, and particularly preferably 80 to 125°C, taking into account the heat resistance temperature of the substrate used, at a temperature at which the substrate does not substantially soften or melt. However, if the heating time is short, heating at a higher temperature (e.g., 400°C) may be acceptable. On the other hand, when the substrate 1 is made of a highly heat-resistant material such as polyimide, the heating temperature can be set to 50 to 400°C. In other words, when heating the film 3, the temperature is preferably adjusted appropriately to 400°C or less. The heating time can also be appropriately set depending on the heat resistance of the substrate 1 and the type of conductive particles used. The heating time is, for example, 0.01 to 1 second, preferably 0.04 to 0.6 seconds. Incidentally, when a roll press is used in the conductive film formation process, the "heating time" refers to the time during which the film 3 is heated while being in contact with the roll and pressurized. As an example, assuming that the contact width between two opposingly rotating rolls is 1 mm and the speed at which the substrate passes between the two rolls is v, the heating time (equivalent to the time during which pressure is applied) is 0.59 seconds when v = 0.1 m / min, 0.04 seconds when v = 1.5 m / min, 0.06 seconds when v = 1.0 m / min, and 0.012 seconds when v = 5.0 m / min.

[0049] When a roll press is used in the conductive film formation process, it is preferable that at least the roll 10A, which is closest to the film 3, be heated, in order to heat and press the film 3. As explained above, the heating temperature of the roll 10A can be appropriately set to 400°C or less depending on the heat resistance of the substrate 1, the type of conductive particles used, and other factors. The heating time can be adjusted by changing the rotation speed (i.e., the conveying speed) of the rolls 10A and 10B. The conveying speed may be adjusted, for example, between 0.1 and 10 m / min, taking into consideration factors such as ensuring sufficient heating and pressurizing time and mass productivity. In addition, not only the roll 10A but also the roll 10B may be heated to achieve uniform heating and shorten the heating time.

[0050] On the other hand, if a conductive film with a sufficiently low resistivity can be obtained, the roll 10A and the roll 10B do not need to be heated.

[0051] Incidentally, if a conductive film with sufficiently low resistivity can be obtained, it is not necessary to heat the film 3 in the conductive film forming step. Specifically, when the conductive film forming step includes a roll pressing step, the roll 10A and the roll 10B do not need to be heated. In particular, when particles containing silver as a main component are used as the conductive particles, a conductive film with sufficiently low resistivity can be easily obtained by pressurization alone.

[0052] Although not shown in FIG. 2 , in the roll press process, for example, rolls 10A and 10B may be rotated while a resin film is sandwiched between the membrane 3 and roll 10A. By interposing a resin film between the membrane 3 and roll 10A, it is possible to prevent the membrane 3 from peeling off and adhering to the roll 10A. Furthermore, by interposing a resin film between the membrane 3 and roll 10A, the pressure applied to the membrane 3 is appropriately distributed, which tends to make it easier to obtain a conductive film that is more uniform and has consistent performance. The material of the resin film sandwiched between the membrane 3 and roll 10A is not particularly limited. In terms of heat resistance and durability, a polyimide film or the like can be preferably used.

[0053] (FIGS. 3 and 4: Modified Examples of the Conductive Film Forming Step) Although the roll press step has been described above as a specific method of the conductive film forming step, it should be noted that the conductive film forming step may be carried out by a method other than roll press as long as sufficient pressure (and heat in some cases) is applied to the film 3. However, in consideration of ease of mass production, it is preferable that the conductive film forming step include a roll press step.

[0054] For completeness, steps other than the roll press step that can be applied to the conductive film forming process will be described below.

[0055] As shown in Fig. 3, the conductive film forming step may include a step of placing the substrate 1 provided with the film 3 on a flat surface 20A of a table 20 having a flat surface, and at least pressurizing the film 3 from above using a roll 12. Note that the table 20 having a flat surface may not be a table but a flat plate, as long as appropriate pressure can be applied. The key is that the substrate 1 is placed on a flat surface and appropriate pressure can be applied with the roll 12.

[0056] 4, the conductive film forming step may include a step of sandwiching the substrate 1 on which the film 3 is provided between a first flat surface 31A of a first pressing member 31 having a first flat surface 31A and a second flat surface 32A of a second pressing member 32 having a second flat surface 32A. An example of an apparatus preferably used for carrying out such a step is a pressing apparatus "CYPF-400" manufactured by Sintokogyo Co., Ltd.

[0057] <Method for manufacturing electronic device> An electronic device can be manufactured using the conductive substrate obtained through the above-mentioned film formation step and conductive film formation step. For example, by appropriately designing the "pattern" of coating or printing in the film formation step, a substrate having a conductive film (circuit pattern) that can function as a circuit can be manufactured, and an electronic device can be manufactured by combining this substrate with other electronic elements.

[0058] Here, several examples of "electronic devices" are described, but electronic devices including a conductive substrate obtained by the method for producing a conductive substrate of this embodiment are not limited to these. Sensors: For example, the conductive substrate obtained by the method for producing a conductive substrate of this embodiment can be applied to the conductive members / circuits in sensors such as pressure-sensitive sensors and vital signs sensors. Solar cells: For example, the conductive substrate obtained by the method for producing a conductive substrate of this embodiment can be applied to the current collecting wiring of solar cells. Membrane switches: A membrane switch is a thin sheet-like switch in which circuits and contacts are printed on a film and then laminated. The method for producing a conductive substrate of this embodiment can be applied to form the circuits and contacts. Touch sensors / touch panels: For example, the method for producing a conductive substrate of this embodiment can be applied to form lead wiring in touch sensors / touch panels. It is also conceivable to apply the method for producing a conductive substrate of this embodiment to form transparent electrodes in touch sensors / touch panels. Flexible substrates: Conventionally, a circuit is formed by first coating the entire surface of a flexible film with a metal film, and then using a chemical to remove unnecessary portions of the metal film. Instead of this conventional method, it is conceivable to form a circuit using the method for producing a conductive substrate of this embodiment.

[0059] In particular, in electronic devices where circuits have conventionally been formed using conductive paste, by using the method for manufacturing a conductive substrate of this embodiment for circuit formation, the specific resistance of the circuit can be reduced, and improved performance of the electronic device can be expected.

[0060] A particularly preferred electronic device is an RF tag. That is, the method for manufacturing a conductive substrate of this embodiment is preferably used to manufacture a conductive circuit such as an antenna portion in an RF tag. For the specific structure of the RF tag, see, for example, JP-A-2003-332714 and JP-A-2020-46834.

[0061] <Method for producing electromagnetic wave shielding film> As an application other than electronic devices, it is conceivable to produce an electromagnetic wave shielding film by the method for producing a conductive substrate of the present embodiment. Specifically, in the film formation step, the conductive composition is formed into a film in a pattern specific to the electromagnetic wave shielding film (e.g., a mesh pattern), thereby producing an electromagnetic wave shielding film.

[0062] <Method for manufacturing a sheet heating element> As another application, the method for manufacturing a conductive substrate according to this embodiment may be used to manufacture a sheet heating element. A sheet heating element is an element that has electrical wiring provided on a substrate and generates heat by passing an electric current through the wiring. A specific example of a sheet heating element is a sheet heating element for preventing fogging or cold weather, such as on the rear window of a passenger vehicle.

[0063] <Conductive Composition> In the above, embodiments of the present invention have been described focusing on the "methods" of manufacturing a conductive substrate and manufacturing an electronic device. Separately, embodiments of the present invention can also be understood as conductive compositions. That is, the following conductive compositions are preferably used for forming conductive films with low resistivity. "A conductive composition containing conductive particles, which is used for forming a conductive film by forming a film on a substrate and at least pressurizing the film, the conductive composition comprising: conductive particles (A) containing at least one element selected from the group consisting of copper and silver; and a compound (B) that inhibits one or both of corrosion and aggregation of the conductive particles (A)."

[0064] Specific embodiments of the composition have been explained in the section <Method for producing conductive substrate>, so further explanation will be omitted.

[0065] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations may be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the object of the present invention are included in the present invention.

[0066] The embodiments of the present invention will be described in detail based on examples and comparative examples. It should be noted that the present invention is not limited to the examples. In the following, exponential notation may be indicated by the symbol "E". For example, 1.3.E-06 is 1.3 x 10 -6 means.

[0067] <Preparation of Conductive Composition> The components shown in Table 1 below were mixed using a planetary mixer. This resulted in a uniform paste-like conductive composition. In Table 1, the amount of each component is expressed in parts by mass.

[0068] Additional information on some of the components in Table 1 is provided below. Copper particles 1: median diameter 10.3 μm Silver particles 1: median diameter 6.1 μm Alkanenitrile: a mixture of several alkanenitriles having carbon atoms ranging from 1 to 18 (boiling point 340°C or less)

[0069] (Film Forming Process and Conductive Film Forming Process) The film forming process and conductive film forming process were performed according to the following procedure to produce a conductive substrate with a conductive film. (1) A 15 mm x 5 mm coating film (solid film) was formed on the substrate using the conductive composition. Specifically, 3M Scotch tape was first applied to the substrate to create a 15 mm x 5 mm "cutout" on the substrate. Then, a squeegee was used to squeeze the conductive composition onto the cutout, filling it with the conductive composition. The Scotch tape was then removed. The thickness of the coating film at this time was approximately 40 μm. A polyimide film was used as the substrate. (2) The substrate with the coating film was placed in a hot air circulating atmospheric oven and heated at 100°C for 15 minutes. This allowed the solvent to dry. (3) The coated film from which the solvent had dried was roll-pressed together with the substrate using a load-adjustable roll press (manufactured by Tester Sangyo Co., Ltd., the general structure of which is shown schematically in Figure 2) under the following conditions: Temperature of roll 10A: heated to 200°C Pressure: 121 MPa Conveying speed: 0.1 m / min

[0070] The pressure above is calculated as follows: Roll width: 165 mm, contact width between rolls: 1 mm, and the area to which pressure is applied is 165 mm. 2The pressure was 20 kN. 2 Since a force of 20 kN was applied to the area, 20 kN ÷ 165 mm 2 The pressure was calculated to be 121 MPa.

[0071] (Measurement of specific resistance) The resistance value of the conductive film obtained above was measured using a four-terminal resistance measuring device, and the film thickness was measured using a film thickness meter. The specific resistance was calculated from the measured resistance value and film thickness.

[0072] The composition information and evaluation results of the conductive compositions are summarized in Table 1.

[0073]

[0074] As shown in Table 1, a conductive composition containing conductive particles (A) containing at least one element selected from the group consisting of copper and silver and a compound (B) that inhibits one or both of the corrosion and aggregation of the conductive particles (A) was used to form a film on a substrate, and pressure was applied to the film, thereby producing a conductive substrate having a conductive film with good conductivity. A more detailed analysis of the examples showed that, in the examples using the same copper particles 1, the resistivity of Examples 3 to 11, which used a combination of a nitrile compound (B3) and a ligand (B1) and / or a reducing agent (B2) as the compound (B), was lower than the resistivity of Example 1, which used only the nitrile compound (B3) as the compound (B). This demonstrates that the conductivity of the resulting conductive film can be further enhanced by using two or more different compounds (B).

[0075] This application claims priority based on Japanese Patent Application No. 2023-054831, filed March 30, 2023, the disclosure of which is incorporated herein in its entirety by reference.

[0076] REFERENCE SIGNS LIST 1 Substrate 3 Film 10A Roll 10B Roll 12 Roll 20 Platform having flat surface 20A Flat surface 31 First pressing member 31A First flat surface 32 Second pressing member 32A Second flat surface

Claims

1. A method for producing a conductive substrate, comprising: a film-forming step of providing a film made of a conductive composition on a substrate; and a conductive film-forming step of applying at least pressure to the film to form a conductive film, wherein the conductive composition comprises: conductive particles (A) containing at least any element selected from the group consisting of copper and silver; and a compound (B) that inhibits one or both of corrosion and aggregation of the conductive particles (A).

2. A method for producing a conductive substrate according to claim 1, wherein the substrate is flexible.

3. A method for producing a conductive substrate according to claim 1 or 2, wherein in the conductive film forming step, the film is pressurized while being heated.

4. A method for producing a conductive substrate according to claim 1 or 2, wherein the compound (B) contains a ligand (B1) capable of coordinating with copper or silver in the conductive particles (A).

5. A method for producing a conductive substrate according to claim 4, wherein the ligand (B1) contains at least one compound selected from the group consisting of amines, imines, phosphines, azoles and carboxylic acids.

6. A method for producing a conductive substrate according to claim 4, wherein the ligand (B1) includes at least one selected from the group consisting of monodentate ligands and bidentate ligands.

7. A method for producing a conductive substrate according to claim 1 or 2, wherein the compound (B) contains a reducing agent (B2).

8. A method for producing a conductive substrate according to claim 7, wherein the reducing agent (B2) contains at least one selected from the group consisting of ascorbic acid, oxalic acid and formic acid.

9. A method for producing a conductive substrate according to claim 1 or 2, wherein the compound (B) includes a nitrile compound (B3).

10. The method for producing a conductive substrate according to claim 1 or 2, wherein the conductive particles (A) are measured for particle diameter by a laser diffraction scattering method, and a particle diameter D at which a cumulative frequency of 50% is obtained in a volume-based cumulative particle diameter distribution curve. 50 The method for producing a conductive substrate, 11. A method for producing a conductive substrate according to claim 1 or 2, wherein the amount of binder in the total non-volatile components of the conductive composition is 5 mass % or less.

12. A method for producing a conductive substrate as described in claim 1 or 2, wherein the conductive film forming process includes a roll press process in which the substrate having the film formed thereon is transported between two opposing rolls.

13. A method for producing a conductive substrate as described in claim 12, wherein in the roll press process, the roll of the two rolls with which the film comes into contact is not heated or is heated to 400°C or less.

14. A method for producing a conductive substrate according to claim 12, wherein in the roll press step, a pressure of 10 to 150 MPa is applied to the substrate on which the film is provided.

15. A method for producing a conductive substrate according to claim 1 or 2, wherein the conductive film has a pattern structure.

16. A method for producing an electronic device, comprising the steps of: producing an electronic device using a conductive substrate obtained by the method for producing a conductive substrate according to claim 1 or 2.

17. A method for manufacturing an electronic device according to claim 16, wherein the electronic device is an RF tag.

18. A method for producing an electromagnetic wave shielding film, comprising the steps of: producing an electromagnetic wave shielding film using a conductive substrate obtained by the method for producing a conductive substrate according to claim 1 or 2.

19. A method for producing a sheet heating element, comprising producing a sheet heating element using a conductive substrate obtained by the method for producing a conductive substrate according to claim 1 or 2.

20. A conductive composition containing conductive particles, which is used in applications in which a film is formed on a substrate and the film is at least pressed to form a conductive film, the conductive composition comprising: conductive particles (A) containing at least any element selected from the group consisting of copper and silver; and a compound (B) that inhibits one or both of the corrosion and aggregation of the conductive particles (A).

21. The conductive composition according to claim 20, wherein the compound (B) contains a ligand (B1) capable of coordinating with copper or silver in the conductive particles (A).

22. The conductive composition according to claim 21, wherein the ligand (B1) contains at least one compound selected from the group consisting of amines, imines, phosphines, azoles and carboxylic acids.

23. The conductive composition according to claim 21 or 22, wherein the ligand (B1) includes at least one selected from the group consisting of monodentate ligands and bidentate ligands.

24. The conductive composition according to claim 20 or 21, wherein the compound (B) includes a reducing agent (B2).

25. The conductive composition according to claim 24, wherein the reducing agent (B2) includes at least one selected from the group consisting of ascorbic acid, oxalic acid, and formic acid.

26. The conductive composition according to claim 20 or 21, wherein the compound (B) comprises a nitrile compound (B3).

27. The conductive composition according to claim 20 or 21, wherein the conductive particles (A) have a particle diameter D at which a cumulative frequency of 50% is obtained in a volume-based cumulative particle diameter distribution curve obtained by measuring the particle diameter of the conductive particles (A) by a laser diffraction scattering method. 50 The conductive composition has a particle size of 0.6 to 50 μm.

28. The conductive composition according to claim 20 or 21, wherein the amount of the binder in the total non-volatile components is 5 mass % or less.

Citation Information

Patent Citations

  • Media equipped with conductive circuit and method of manufacturing same

    JP2003332714A

  • Manufacturing method of conductive member

    JP2017191723A

  • RF tag label

    JP2020046834A

  • Conductive film forming method

    JP2021044308A

  • Personal authentication system

    JP2023054831A

Cited By

  • Conductive film-equipped substrate, electronic device, electromagnetic wave shielding sheet, planar heating element, and method for manufacturing conductive film-equipped substrate

    WO2026205157A1

  • Conductive-film-equipped substrate, electronic device, electromagnetic wave shielding sheet, planar heating element, and method for manufacturing conductive-film-equipped substrate

    WO2026205160A1