Spherical magnesium oxide, production method for same, thermally conductive filler, and resin composition
Spherical magnesium oxide with tailored titanium and iron content addresses the limitations of existing thermally conductive fillers by enhancing sphericity and resin filling properties, improving heat dissipation and reducing viscosity in semiconductor applications.
Patent Information
- Application Number
- PCT/JP2024/012542
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Current thermally conductive fillers like silica and alumina fail to adequately address heat dissipation in high-integration, high-power semiconductor applications due to insufficient thermal conductivity and excessive wear on manufacturing equipment, respectively.
Spherical magnesium oxide with controlled titanium and iron content, within specific ranges, is produced to enhance sphericity and resin filling properties while minimizing viscosity increase during resin processing.
The resulting spherical magnesium oxide exhibits improved heat dissipation performance, excellent resin filling properties, and reduced viscosity increase, making it suitable as a thermally conductive filler for semiconductor applications.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Spherical magnesium oxide, its manufacturing method, thermally conductive filler, and resin composition
[0001] The present invention relates to spherical magnesium oxide and a method for producing the same, as well as a thermally conductive filler containing the spherical magnesium oxide and a resin composition containing the same.
[0002] Silica, alumina, and the like have traditionally been used as thermally conductive fillers, but silica has low thermal conductivity and is insufficient to dissipate heat in response to the increased heat generated by recent trends toward higher integration, higher power consumption, and higher speeds, potentially resulting in problems with stable semiconductor operation. On the other hand, alumina, which has a higher thermal conductivity than silica, offers improved heat dissipation compared to silica, but its high hardness causes severe wear on kneading machines, molding machines, molds, and the like. Therefore, magnesium oxide, which has a thermal conductivity one order of magnitude higher than silica and approximately twice that of alumina, and is less hard than alumina, and can suppress wear on various manufacturing equipment, is being considered as a thermally conductive filler.
[0003] Various technological developments have been made to obtain magnesium oxide that is more suitable as a thermally conductive filler. Patent Document 1 proposes magnesium oxide in which a boron compound or the like is added to control the aggregation state and particle size distribution. Patent Document 2 proposes spherical magnesium oxide with a smooth surface and fine grain size, which is obtained by adding a lithium compound. Patent Document 3 proposes spherical magnesium oxide with excellent moisture resistance and packing ability, which is obtained by adjusting the boron and iron contents within a certain range.
[0004] JP 2011-020870 A JP 2016-088838 A JP 2018-131378 A
[0005] As shown in Patent Documents 1 to 3, the main objective of technological development for magnesium oxide as a thermally conductive filler has been to improve its fillability. On the other hand, there has also been hope for an improvement in the increase in viscosity that occurs when the filler is filled into a resin, which would facilitate resin processing, but technological development from this perspective has not been sufficient to date. Therefore, an object of the present invention is to provide spherical magnesium oxide that has high sphericity, excellent fillability into a resin, and small increase in viscosity when kneaded into a resin, and a method for producing the same.
[0006] In order to solve the above problems, the present inventors have conducted extensive research and found that by adjusting the titanium and iron contents within a certain range, it is possible to obtain spherical magnesium oxide with high sphericity, excellent fillability into resin, and a small increase in viscosity when filled into resin, and have completed the present invention.The gist of the present invention is as follows.
[0007] [1] A powder containing 0.05 to 2.0% titanium and 100 to 1,500 ppm iron, having a volume-based cumulative 50% particle diameter (D 50 ) is in the range of 3 to 200 μm, and the sphericity as read from an SEM photograph is 1.00 to 1.20.
[0008] [2] Cumulative 50% particle diameter (D 50 The spherical magnesium oxide of [1], wherein the particle size is greater than 25 μm and less than 150 μm.
[0009] [3] A thermally conductive filler containing the spherical magnesium oxide of [1] or [2].
[0010] [4] A resin composition containing the thermally conductive filler according to [3].
[0011] [5] A method for producing spherical magnesium oxide, comprising: 1) a step of reacting an aqueous magnesium chloride solution with an aqueous alkali solution to prepare a magnesium hydroxide slurry; 2) a step of drying and firing the magnesium hydroxide slurry to prepare magnesium oxide; 3) a step of dispersing the magnesium oxide in a solvent to prepare a dispersion, followed by wet-pulverization; 4) a step of spray-drying the magnesium oxide dispersion after wet-pulverization; and 5) a step of firing the spherical magnesium oxide granulated by spray drying, wherein in at least one of steps 1) to 5), the titanium and / or iron contents are adjusted so that the titanium content in the fired spherical magnesium oxide is 0.05 to 2.0% and the iron content is 100 to 1,500 ppm.
[0012] It should be noted that any two or more of the configurations [1] to [5] above can be selected and combined.
[0013] According to the present invention, there can be provided spherical magnesium oxide having high sphericity, excellent fillability into resin, and a small increase in viscosity when filled into resin, and a method for producing the same.
[0014] The spherical magnesium oxide of the present invention contains 0.05 to 2.0% of titanium and 100 to 1,500 ppm of iron, and has a volume-based cumulative 50% particle diameter (D 50 ) is in the range of 3 to 200 μm, and the sphericity as read from an SEM photograph is 1.00 to 1.20. In the description of the content throughout the specification, unless otherwise specified, % means % by mass, and ppm means ppm by mass. The spherical magnesium oxide of the present invention is intended to be magnesium oxide powder.
[0015] First, the spherical magnesium oxide obtained in the present invention has a volume-based cumulative 50% particle diameter (D 50 ) is in the range of 3 to 200 μm, preferably 15 to 180 μm, and more preferably greater than 25 μm and not greater than 150 μm, which is a relatively large particle size range that can improve heat dissipation performance, and also has high sphericity and excellent filling properties.
[0016] In the present invention, sphericity refers to the sphericity that can be read from a scanning electron microscope (SEM) photograph, and is preferably 1.00 to 1.20, preferably 1.00 to 1.15, and more preferably 1.00 to 1.10. Such a sphericity results in excellent fillability into resin. In the present invention, the major axis and minor axis lengths passing through the center of 100 particles in an electron microscope photograph taken using an SEM are measured, the major axis / minor axis ratio is calculated, and the average value is used as the sphericity.
[0017] In the present invention, by adjusting the titanium and iron contents of the spherical magnesium oxide within a certain range, it is possible to obtain spherical magnesium oxide with high sphericity and small increase in viscosity when filled with resin. Here, the titanium content is 0.05 to 2.0%, preferably 0.08 to 1.5%, and more preferably 0.1 to 1.0%. At the same time, the iron content is 100 to 1,500 ppm, preferably 150 to 1,300 ppm, and more preferably 200 to 1,000 ppm. By blending titanium and iron in appropriate amounts and in a balanced manner, spherical magnesium oxide with high sphericity and small increase in viscosity when filled with resin can be obtained.
[0018] The method for producing spherical magnesium oxide of the present invention is not particularly limited, and can be, for example, produced by the following production method: 1) a step of reacting an aqueous magnesium chloride solution with an aqueous alkali solution to prepare a magnesium hydroxide slurry; 2) a step of drying and firing the magnesium hydroxide slurry to prepare magnesium oxide; 3) a step of dispersing the magnesium oxide in a solvent to form a dispersion, which is then wet-pulverized; 4) a step of spray-drying the magnesium oxide dispersion after wet-pulverization; and 5) a step of firing the spherical magnesium oxide granulated by spray drying, wherein in at least one or more of steps 1) to 5), the titanium and / or iron content is adjusted so that the titanium content in the spherical magnesium oxide after firing is 0.05 to 2.0% and the iron content is 100 to 1,500 ppm.
[0019] More specifically, the above-mentioned production method can be carried out as follows: 1) reacting an aqueous alkali solution with an aqueous magnesium chloride solution to obtain a magnesium hydroxide slurry, 2) filtering, washing with water, drying, and then calcining the slurry to obtain magnesium oxide, 3) dispersing the magnesium oxide in a solvent, preferably an organic solvent, to obtain a dispersion, which is then wet-pulverized, 4) spray-dried, and 5) calcining the obtained spherical magnesium oxide to obtain the desired spherical magnesium oxide. Before the final calcination, a titanium source and / or an iron source are mixed and / or added so that the titanium content of the spherical magnesium oxide after final calcination is 0.05 to 2.0% and the iron content is 100 to 1,500 ppm. Specifically, the titanium content and / or iron source are adjusted by, for example, a) adding a boron source and / or an iron source to an aqueous magnesium chloride solution and / or an alkaline aqueous solution, b) adding a titanium source and / or an iron source to the produced magnesium hydroxide slurry, c) mixing a titanium source and / or an iron source with magnesium oxide obtained by calcining magnesium hydroxide, d) adding a titanium source and / or an iron source during wet-pulverization of magnesium oxide, e) mixing a titanium source and / or an iron source with spherical magnesium oxide granulated by spray drying, etc. The titanium content and iron content in the finally obtained spherical magnesium oxide may be adjusted in the same step or in different steps.
[0020] The titanium source is not particularly limited as long as it is a compound containing titanium, and examples thereof include titanium oxide (anatase type, rutile type), titanium chloride, titanium hydroxide, titanium bromide, titanium fluoride, magnesium titanate, and the like.
[0021] The iron source is not particularly limited as long as it is a compound containing iron, and examples thereof include iron (II) oxide, iron (III) oxide, iron tetroxide, iron hydroxide, iron chloride, iron nitride, iron bromide, and iron fluoride.
[0022] The titanium source is adjusted so that the titanium content of the spherical magnesium oxide after final firing is 0.05 to 2.0%. If the titanium content is less than 0.05%, the viscosity reduction effect is not sufficiently obtained. If the titanium content exceeds 2.0%, excessive particle growth and adhesion between particles are likely to occur, making it impossible to obtain spherical magnesium oxide with high sphericity. Then, the iron source is adjusted so that the iron content of the spherical magnesium oxide after final firing is 100 to 1,500 ppm. If the iron content is in the range of 100 to 1,500 ppm in addition to the above titanium content, spherical magnesium oxide with high sphericity tends to be obtained.
[0023] The magnesium chloride aqueous solution can be selected from, for example, magnesium chloride hexahydrate, magnesium chloride dihydrate, anhydrous magnesium chloride, bittern, seawater, and combinations thereof.
[0024] The alkaline aqueous solution may be selected from, for example, an aqueous sodium hydroxide solution, an aqueous calcium hydroxide solution, aqueous ammonia, and combinations thereof.
[0025] The magnesium hydroxide slurry obtained by reacting an aqueous magnesium chloride solution with an aqueous alkali solution is filtered, washed with water, dried, and then calcined, for example, by a method common in the art, to form magnesium oxide. The obtained magnesium oxide is then dispersed in a solvent to form a dispersion (e.g., a slurry), which is wet-pulverized and spray-dried to form granules. The solvent used here is not particularly limited, but known solvents can be used, such as aqueous systems, aqueous-organic solvent mixtures, alcohols such as methanol and ethanol, ketones such as acetone, esters such as ethyl acetate, ethers such as diethyl ether, and aromatic compound solvents such as tetrahydrofuran and toluene.
[0026] The spray drying method is not particularly limited, but it is preferable to use, for example, a spray drying method in which a magnesium oxide dispersion (e.g., a slurry) after wet milling is sprayed from a rotating disk or nozzle to obtain magnesium oxide particles. The operating conditions are appropriately adjusted depending on the slurry viscosity, the particle size of the powder in the slurry, the target particle diameter, etc. A dispersant may also be added to the slurry as appropriate. The operating conditions are not particularly limited, but in the case of the spray drying method, for example, a slurry with a viscosity adjusted to 10 to 3000 cps is sprayed from a rotating disk or nozzle into an airflow at 80°C to 250°C while appropriately adjusting the flow rate, thereby producing particles of approximately 1 to 200 μm. Furthermore, it is preferable to adjust the concentration of the dispersion during wet milling and spraying so that the magnesium oxide is 50 to 70 wt %, for example. Here, by appropriately setting the spray conditions, it is possible to adjust the sphericity of the obtained spherical magnesium oxide. Furthermore, by appropriately setting the spray conditions, it is possible to adjust the cumulative 50% particle diameter (D 50 The spray drying method is preferred because it allows for the stable production of particles with large particle sizes.
[0027] The conditions for firing the granulated magnesium oxide are not particularly limited as long as they are within a range in which the magnesium oxide particles are sintered, but the temperature is preferably 1000°C to 1800°C, more preferably 1100°C to 1700°C, and particularly preferably 1200°C to 1600°C. The firing time depends on the firing temperature, but is preferably 0.5 to 10 hours. If the firing temperature is less than 1000°C, the particles will not be sufficiently sintered, and if it exceeds 1800°C, the particles will sinter together and form coarse aggregates, so it is adjusted to be within the above range.
[0028] The spherical magnesium oxide of the present invention can be surface-treated using a known method in order to improve moisture resistance. When surface-treating the spherical magnesium oxide of the present invention, the surface treatment agent used is not particularly limited, but for example, colloidal silica, silane-based coupling agents, titania sol, titanate-based coupling agents, phosphorus compounds, alumina sol, aluminate-based coupling agents, zirconium-based coupling agents, etc. can be used. These may be used alone or in combination of two or more.
[0029] Examples of the silane coupling agent include vinyltrichlorosilane, vinyltrialkoxysilane, glycidoxypropyltrialkoxysilane, and methachloroxypropylmethyldialkoxysilane.
[0030] Examples of titanate coupling agents include tetraisopropyl titanate, tetra-normal-butyl titanate, tetraoctyl titanate, tetrastearyl titanate, isopropyl triisostearoyl titanate, tetraoctylbis(ditridecylphosphite)titanate, and bis(dioctylpyrophosphate)oxyacetate titanate.
[0031] The phosphorus compound is not particularly limited as long as it is a compound capable of reacting with magnesium oxide to form a magnesium phosphate-based compound, and examples thereof include phosphoric acid, phosphates, and acidic phosphate esters. Examples of acidic phosphate esters include isopropyl acid phosphate, 2-ethylhexyl acid phosphate, oleyl acid phosphate, methyl acid phosphate, ethyl acid phosphate, propyl acid phosphate, butyl acid phosphate, lauryl acid phosphate, and stearyl acid phosphate.
[0032] Examples of the aluminate coupling agent include aluminum isopropylate, monosec-butoxyaluminum diisopropylate, aluminum sec-butylate, aluminum ethylacetoacetate diisopropylate, aluminum tris(ethylacetoacetate), and aluminum alkylacetoacetate diisopropylate.
[0033] Examples of zirconium-based coupling agents include normal propyl zirconate and normal butyl zirconate.
[0034] The spherical magnesium oxide of the present invention has the advantages of high sphericity, excellent filling properties, and a small increase in viscosity when filled into a resin, making it suitable for incorporation into resins as a filler and useful as a thermally conductive filler. The thermally conductive filler of the present invention may contain the spherical magnesium oxide of the present invention alone, or may contain the spherical magnesium oxide of the present invention together with other thermally conductive filler materials. The resin composition of the present invention contains the thermally conductive filler of the present invention, and examples of resins that can be used in the present invention include thermosetting resins and thermoplastic resins. Thermosetting resins are not particularly limited, but include, for example, phenolic resins, urea resins, melamine resins, alkyd resins, polyester resins, epoxy resins, diallyl phthalate resins, polyurethane resins, and silicone resins. The thermoplastic resin is not particularly limited, but examples thereof include polyamide resin, polyacetal resin, polycarbonate resin, polybutylene terephthalate resin, polyolefin resin, polysulfone resin, polyamideimide resin, polyetherimide resin, polyarylate resin, polyphenylene sulfide resin, polyether ether ketone resin, fluororesin, and liquid crystal polymer.
[0035] The amount of spherical magnesium oxide to be added to the resin composition of the present invention is not particularly limited and may be determined appropriately depending on the properties required of the resin composition, but as an example, the amount of spherical magnesium oxide may be in the range of 0.1 to 100 parts by mass per 100 parts by mass of the resin.
[0036] The resin composition containing the spherical magnesium oxide of the present invention can be used in various fields depending on the properties of the resin. However, since the spherical magnesium oxide of the present invention has excellent thermal conductivity, it can be suitably used in applications that require heat dissipation. For example, the resin composition of the present invention can be used as a semiconductor encapsulation material with excellent thermal conductivity.
[0037] The present invention will be described in detail with reference to the following examples, but these examples are not intended to limit the present invention in any way.
[0038] [Measurement and Evaluation Methods] (1) Measurement Method of Iron Content The iron content was measured by ICP atomic emission spectroscopy. The measurement sample was added to 12N hydrochloric acid (special reagent grade) and heated to completely dissolve it, and then the iron content was measured using an ICP measurement device (PS3520 VDD, manufactured by Hitachi High-Tech Science Corporation).
[0039] (2) Measurement method of titanium content The titanium content was measured using an X-ray fluorescence analyzer (device name: ZSX Primus4, manufactured by Rigaku Corporation). First, the magnesium oxide to be measured was placed in an aluminum ring (φ35 mm), clamped between dies, and pelletized using a press (surface pressure 250 MPa) to obtain a measurement sample. This sample was measured in SQX analysis (EZ scan) mode (bulb: Rh (4 kW), atmosphere: vacuum, analysis window: Be (30 μm), measurement diameter: 30 mmφ, measurement range F to U) to determine the titanium content in the magnesium oxide.
[0040] (3) Volume-based cumulative 50% particle diameter (D 50 ) Measurement sample 0.1 x 10 -3 kg was precisely weighed, dispersed in 40 mL of methanol, and measured using a laser diffraction scattering particle size distribution measuring device (MT3300, manufactured by Nikkiso Co., Ltd.).
[0041] (4) Sphericity as Read from SEM Photographs Magnesium oxide samples to be evaluated were photographed using a scanning electron microscope (SEM) (JSM6510LA, manufactured by JEOL Ltd.) For 100 randomly selected particles in the electron microscope photographs, the lengths of the major and minor axes passing through the center of the particle were measured, the ratio of the major axis to the minor axis was calculated, and the average value was taken as the sphericity.
[0042] (5) Viscosity Evaluation During Resin Filling Spherical magnesium oxide to be evaluated and alumina particles (Denka's "DAW-05" (average particle size: 5 μm)) were mixed at 50% by volume, and this mixture was added to silicone oil (Shin-Etsu Chemical Co., Ltd.'s "KF96-100cs") so that the total filling rate of the spherical magnesium oxide and alumina particles was 75% by volume. This mixture was mixed using a rotation / revolution mixer at a rotation speed of 2,200 rpm for 30 seconds, and then vacuum degassed to obtain a resin composition. The viscosity of the obtained resin composition was measured using a Brookfield viscometer (TOKIMEC's BL model, measurement conditions: sample temperature 25°C, 6 rpm, rotor No. 4, container dimensions φ26 mm × h46 mm, sample volume 20 mL).
[0043] [Examples and Comparative Examples] (Example 1) Anhydrous magnesium chloride (MgCl 2 ) was dissolved in ion-exchanged water to prepare an approximately 3.5 mol / L aqueous magnesium chloride solution. 2 MgCl 2The solution and 25% NaOH solution were each pumped into a reactor using a metering pump, and a continuous reaction was carried out to obtain a magnesium hydroxide slurry. Subsequently, titanium oxide / anatase type (JA-20, manufactured by Teika Corporation) was added to the magnesium hydroxide slurry so that the titanium content in the finally obtained spherical magnesium oxide was 0.7%, and iron (II) oxide (manufactured by Hayashi Pure Chemical Industries, Ltd.) was added so that the iron content was 250 ppm. The mixture was then filtered, washed with water, and dried to obtain magnesium hydroxide. The obtained magnesium hydroxide was calcined at 900°C for 1 hour to obtain magnesium oxide. The obtained magnesium oxide was dispersed in an organic solvent to obtain a slurry with a magnesium oxide concentration of 65 wt%. Subsequently, wet pulverization was carried out using a ball mill for 4 hours, followed by spray drying using a spray drying method. The obtained spray-dried spherical magnesium oxide was finally calcined at 1400°C for 1 hour in an electric furnace to obtain the desired spherical magnesium oxide.
[0044] (Example 2) Spherical magnesium oxide was obtained using the same production method as in Example 1, except that titanium oxide was added to the reaction solution so that the titanium content in the spherical magnesium oxide was 0.39% and iron (II) oxide was added so that the iron content was 330 ppm.
[0045] (Example 3) Spherical magnesium oxide was obtained using the same production method as in Example 1, except that titanium oxide was added to the reaction solution so that the titanium content in the spherical magnesium oxide was 0.11% and iron (II) oxide was added so that the iron content was 330 ppm.
[0046] (Example 4) Spherical magnesium oxide was obtained using the same manufacturing method as in Example 1, except that titanium oxide was added to the reaction solution so that the titanium content in the spherical magnesium oxide was 0.75% and iron (II) oxide was added so that the iron content was 240 ppm, and the firing temperature in the final firing was set to 1300°C.
[0047] Comparative Example 1 Spherical magnesium oxide was obtained using the same production method as in Example 1, except that no titanium source was added to the reaction solution and iron (II) oxide was added so that the iron content was 240 ppm.
[0048] The above measurements and evaluations were carried out for Examples 1 to 4 and Comparative Example 1. The results are shown in Table 1.
[0049]
[0050] As is clear from Table 1, the spherical magnesium oxides of Examples 1 to 4 had high sphericity and showed low viscosity increase when filled with resin. On the other hand, the spherical magnesium oxide of Comparative Example 1 showed high sphericity but showed a large viscosity increase when filled with resin, and its performance as a filler was poor.
[0051] This indicates that the spherical magnesium oxide of the present invention exhibits a small increase in viscosity when filled into resin, has high sphericity, and is excellent in fillability into resin, and is therefore useful as an excellent resin filler.
[0052] According to the present invention, it is possible to provide spherical magnesium oxide which exhibits a small increase in viscosity when filled into resin, has high sphericity, and is excellent in fillability into resin, and a method for producing the same.
Claims
1. Contains 0.05-2.0% titanium and 100-1,500 ppm iron, and has a cumulative 50% particle diameter (D) based on volume as measured by laser diffraction scattering particle size distribution measurement 50 ) is in the range of 3 to 200 μm, and the sphericity as read from an SEM photograph is 1.00 to 1.
20.
2. Cumulative 50% particle size (D 50 2. The spherical magnesium oxide according to claim 1, wherein the diameter of the particle is greater than 25 μm and less than 150 μm.
3. A thermally conductive filler containing the spherical magnesium oxide according to claim 1 or 2.
4. A resin composition containing the thermally conductive filler according to claim 3.
5. A method for producing spherical magnesium oxide comprising the steps of: 1) reacting an aqueous magnesium chloride solution with an aqueous alkali solution to prepare a magnesium hydroxide slurry; 2) drying and calcining the magnesium hydroxide slurry to prepare magnesium oxide; 3) dispersing the magnesium oxide in a solvent to prepare a dispersion, followed by wet-grinding; 4) spray-drying the magnesium oxide dispersion after wet-grinding; and 5) calcining the spherical magnesium oxide granulated by spray drying, wherein in at least one of steps 1) to 5), the titanium and / or iron content is adjusted so that the spherical magnesium oxide after calcination has a titanium content of 0.05 to 2.0% and an iron content of 100 to 1,500 ppm.
Citation Information
Patent Citations
Spherical magnesium hydroxide particle, spherical magnesium oxide particle, and method for producing them
JP2012201511A
Magnesium hydroxide particle having slow growth late and low aspect ratio method for producing the same
JP2017122029A
Magnesium oxide powder, filler composition, resin composition, and heat dissipating component
JP2022048542A
Magnesium oxide powder, filler composition, resin composition, and heat dissipating component
JP2022048558A
Magnesium oxide powder, filler composition, resin composition, and heat dissipating component
JP2022048574A
Cited By
Magnesium oxide granules and production method therefor
WO2026205431A1