Method for producing quartz member, device for coating quartz member, and method for regenerating quartz member
By employing an airflow control plate to manage rising air currents and stabilize the oxyhydrogen flame, the method achieves a uniform and dense quartz coating on quartz members, addressing the issue of uneven coatings and enhancing the quality of the coating process for semiconductor applications.
Patent Information
- Application Number
- PCT/JP2024/012799
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for coating quartz members, such as those used in semiconductor manufacturing, face challenges with uneven heat input and unmelted material due to rising air currents interfering with the oxyhydrogen flame, particularly when coating inner surfaces, leading to irregular coatings and reduced film density.
The implementation of an airflow control plate installed within a specific range relative to the burner axis, combined with controlled gas supply and burner positioning, stabilizes the flame and ensures uniform coating by suppressing rising air currents, allowing for a dense and transparent quartz coating film on both flat and curved surfaces.
This approach effectively stabilizes the oxyhydrogen flame, enabling the formation of a uniform, dense, and transparent quartz coating film on quartz members, even on complex shapes, by controlling airflow and flame direction, thereby improving coating consistency and quality.
Smart Images

Figure JP2024012799_03102024_PF_FP_ABST
Abstract
Description
Method for manufacturing quartz member, apparatus for coating quartz member, and method for regenerating quartz member
[0001] The present invention relates to a method for manufacturing a quartz member including a fire processing step, a quartz member coating apparatus, and a quartz member regeneration method.
[0002] Machines, equipment, containers, etc. used in semiconductor manufacturing processes require heat resistance and chemical purity depending on the process used.
[0003] Under any circumstances, it is necessary to suppress reactions with semiconductor materials and element transfer, and silica glass is known to be almost the only material that meets all of these conditions.
[0004] Quartz glass members used in the semiconductor industry are made by processing natural quartz glass material into a desired shape using fire processing or the like, then annealing to remove distortion, cleaning, and finally manufacturing the product.
[0005] Fire processing also includes coating. There are needs for coating quartz glass onto the surface of a substrate, such as suppressing impurities from the substrate that constitutes the device, regenerating thinned quartz components, and increasing the purity of components similar to silicon wafers.
[0006] As a method for coating a substrate surface with quartz glass, Patent Document 1 describes a method for overlay coating a quartz member using a quartz oxyhydrogen burner. The method in Patent Document 1 involves mixing quartz powder with oxygen gas by the so-called Bernoulli method, and since the powder is deposited on the substrate using gravity, the portion to be coated is limited to the upward-facing surface of the substrate.
[0007] Patent Document 2 describes a method for forming a silica glass thermal sprayed film on the side surface of a substrate using a plasma spraying method. In this plasma spraying method, heated and melted particles are sprayed onto the substrate at high speed, so the particles flatten and solidify after impact. For this reason, this method is not suitable for obtaining a dense coating film without bubbles, and is actually used in applications that take advantage of the presence of bubbles that occur in the film.
[0008] When coating quartz components with the aim of restoring them after they have lost thickness, it is necessary to be able to coat them at any angle to suit the component shape. In thermal spray coating of quartz glass, an oxyhydrogen flame is used to heat the substrate to be coated and the quartz powder that is the coating raw material, and the heated air creates an updraft.
[0009] The state of the ascending air currents varies greatly depending on the surrounding environment, but their impact is most pronounced when coating the inner surface of the quartz component rather than the outer surface. Specifically, the ascending air currents interfere with the oxyhydrogen flame, causing the flame to fluctuate irregularly, resulting in uneven heat input to the quartz component and raw quartz powder, and resulting in unmelted powder. Furthermore, the raw quartz powder is supplied while being heated through the center of the oxyhydrogen flame, but flame disturbances cause it to deposit in a position on the order of several millimeters from the target location, resulting in some areas not receiving the heat necessary for melting after deposition. These factors significantly hinder the achievement of a uniform coating.
[0010] Japanese Patent Laid-Open No. 7-126025 Japanese Patent Laid-Open No. 2004-142996
[0011] An object of the present invention is to provide a method for manufacturing a quartz member, a quartz member coating device, and a method for regenerating a quartz member that can suppress disturbance of the flame emitted from a burner when applying quartz coating to a substrate.
[0012] The present inventors have conducted extensive research to solve the above problems based on an understanding of phenomenology through thermal flow analysis, and have found that the above problems can be solved by installing an airflow control plate below the burner that generates the oxyhydrogen flame, which prevents the updraft (hot air current) from flowing into the flame.
[0013] [1] A method for manufacturing a quartz member, comprising a fire processing step of applying heat to the surface of a workpiece containing quartz using a burner, and positioning an airflow control plate within a range of ±45° from a position parallel to the axis of the burner during the fire processing step. [2] The method for manufacturing a quartz member according to [1], wherein the fire processing step includes a process of spraying molten silica powder onto the surface of the workpiece to form a coating. [3] The method for manufacturing a quartz member according to [1] or [2], wherein the shape of the airflow control plate is line-symmetrical with respect to the axis of the burner. [4] The method for manufacturing a quartz member according to any of [1] to [3], wherein the distance between the surface of the airflow control plate facing the burner and the axis of the burner is 20 mm or more and 500 mm or less. [5] The method for manufacturing a quartz member according to any of [1] to [4], wherein the angle between the axial direction of the burner and the vertical direction is 30° or more and 150° or less. [6] The method for manufacturing a quartz member according to any one of [1] to [5], wherein the airflow control plate is installed in a position in the gravity direction of the burner. [7] The method for manufacturing a quartz member according to any one of [1] to [6], wherein the airflow control plate is installed within ±20° of a position parallel to the axis of the burner. [8] The method for manufacturing a quartz member according to any one of [1] to [7], wherein the burner has a plurality of supply pipes for supplying gas or powder. [9] The method for manufacturing a quartz member according to any one of [1] to [8], wherein the burner has supply pipes for silica powder, oxygen gas, and hydrogen gas.
[10] The method for manufacturing a quartz member according to any one of [2] to [9], wherein a gas having a volume ratio of oxygen of 80% or less is used as a carrier gas for silica powder.
[11] The method for manufacturing a quartz member according to any one of [1] to
[10] , wherein the processing surface of the workpiece is a curved surface.
[0014]
[12] A quartz member coating apparatus having a burner and an airflow control plate, the airflow control plate being installed within a range of ±45° from a position parallel to the axis of the burner.
[13] The quartz member coating apparatus according to
[12] , wherein the distance between the surface of the airflow control plate facing the burner and the axis of the burner is 20 mm or more and 500 mm or less.
[14] The quartz member coating apparatus according to
[12] or
[13] , wherein the airflow control plate is installed in a position in the gravity direction of the burner.
[15] The quartz member coating apparatus according to any of
[12] to
[14] , wherein the angle between the axial direction of the burner and the vertical direction is 30° or more and 150° or less.
[16] The quartz member coating apparatus according to any of
[12] to
[15] , wherein the airflow control plate is installed within a range of ±20° from a position parallel to the flame blowing direction.
[0015]
[17] A method for regenerating a quartz member, comprising providing a quartz coating film on the quartz member using the quartz member coating device according to any one of
[12] to
[16] .
[0016] According to the present invention, it is possible to prevent the inflow of ascending air currents (hot air currents) into the burner flame, stabilize the burner flame, and form a transparent and dense coating film.
[0017] 1(a) is a front view of a burner according to an embodiment, and FIG. 1(b) is a cross-sectional view taken along line B-B in FIG. 1(a). FIG. 1(b) is a diagram illustrating the configuration of a hopper. FIG. 1(c) is a diagram illustrating an example of the installation of an airflow control plate. FIG. 1(d) is a plan view of the airflow control plate and the burner.
[0018] The following describes in detail the embodiments of the present invention, but the present invention is not limited to the following embodiments and can be practiced in various modified forms within the scope of the gist thereof.
[0019] "Method for manufacturing a quartz member" First, the method for manufacturing a quartz member of the present invention will be described. The method for manufacturing a quartz member of the present invention includes a fire processing step in which heat is applied to the surface of a workpiece containing quartz by a burner, and is characterized in that an airflow control plate is positioned within a range of ±45° from a position parallel to the axis of the burner during the fire processing step.
[0020] [Burner (quartz burner, hereinafter sometimes simply referred to as "burner")] FIG. 1 shows a burner 1 according to an embodiment, where (a) is a front view and (b) is a cross-sectional view taken along line BB of (a).
[0021] Burner 1 has a multiple-layer structure with multiple supply pipes for supplying gas or powder. In other words, burner 1 is a so-called quartz burner for processing quartz glass, and as shown in Figure 1, has a body 5 with a multiple-layer structure of three or more pipes, in order from the center in the radial direction: raw silica powder supply pipe 2, oxygen gas supply pipe 3, and hydrogen gas supply pipe 4. The rear ends of oxygen gas supply pipe 3 and hydrogen gas supply pipe 4 are closed by closing members (not shown). Oxygen gas supply pipe 3 and hydrogen gas supply pipe 4 are provided with gas inlets 3a and 4a.
[0022] A tapered portion that narrows toward the tip is provided from the body 5 to the tip.
[0023] This tapered section has oxygen gas nozzles 6 arranged concentrically at equal circumferential positions, and has a structure in which some of the hydrogen gas is introduced into the gaps between the oxygen gas nozzles 6. The tip side of the oxygen gas supply pipe 3 communicates only with the oxygen gas nozzles 6. Six oxygen gas nozzles 6 are shown, but this is not limited to this.
[0024] A convergence point of the blown flows of raw material silica powder, oxygen gas, and hydrogen gas is formed in front of the burner 1. The axial direction of each oxygen gas nozzle 6 is directed toward this convergence point.
[0025] The raw silica powder blown out from the central silica powder supply pipe 2 together with the carrier gas is guided by the surrounding combustion flames of oxygen and hydrogen gas, and while receiving the heat required for melting, it efficiently gathers near the convergence point, melts, and is sprayed onto the surface of the target material to form a quartz coating.
[0026] [Raw Silica Powder] The raw silica powder is preferably of high purity (for example, greater than 5N) since the purity of the resulting film is higher. However, depending on the application, powder with a purity of 5N or less, such as natural quartz powder, may also be used.
[0027] The particle size of the raw material silica powder is usually 20 μm to 400 μm, preferably 40 μm to 200 μm, and more preferably 50 μm to 80 μm. In the present invention, the particle size of the silica powder is determined by sieving.
[0028] If the particle size of the raw silica powder is 20 μm or more, the silica powder is less likely to vaporize when sprayed from the nozzle, is less likely to become fumed silica, and the film formation yield increases.If the particle size of the raw silica powder is 400 μm or less, the silica powder is more likely to be subjected to the guiding action of the oxyhydrogen combustion flame, and a film is formed on the target surface without variation.
[0029] [Subject Material for Forming a Quartz Component] The subject material for forming a quartz component, more specifically, the subject material for forming a coating by melting silica powder in a pyrolytic processing process, is preferably a quartz component. Examples include etching rings in plasma etching apparatuses, quartz plates, rectangular cleaning tanks, and furnace tubes used in semiconductor wafer oxide coating apparatuses. The processing surface of the subject material may have any shape, but the present manufacturing method and apparatus are particularly effective when the processing surface is curved. When the processing surface is curved, the burner flame is more susceptible to the influence of updrafts than when the processing surface is flat. Even in such a situation, the manufacturing method of the quartz component of this embodiment can sufficiently suppress the influence of updrafts.
[0030] To prevent stress from occurring due to differences in linear expansion after film formation, it is desirable for the target material to have a linear expansion coefficient close to that of the raw material silica powder. Specifically, the average linear expansion coefficient of the coating surface is 0.5 × 10 -6 ~0.6 × 10 -6 [K -1 In addition, when a primary layer having an average linear expansion close to the above-mentioned value is formed on the surface to be coated of the target member, the material of the target member itself may be a material other than quartz.
[0031] 2, the silica powder feeding device 10 uses a quartz tube in the suction line 11 of the raw silica powder hopper. The raw silica powder is sucked into the suction line 11 together with the carrier gas by the negative pressure generated by the ejection of oxygen gas and hydrogen gas from the burner 1. The member (scraper 12) that smooths the surface of the silica powder in the hopper 13 is made of quartz.
[0032] The carrier gas is introduced into the hopper 13 from near the center of the bottom of the hopper 13, as indicated by arrow C. Nitrogen gas, oxygen, air, or the like can be used as the carrier gas. It is preferable to use a gas with an oxygen volume ratio of 80% or less as the carrier gas. If the oxygen ratio is 80% or less, it is possible to prevent the raw material powder to be sprayed from turning into fumes after being ejected from the nozzle tip.
[0033] [Airflow Control Plate] As shown in Figure 3, the airflow control plate 20 is placed below the flame emitted from the burner 1 when coating the target material 30, and is a component that prevents the updraft generated by the heated air from flowing into the flame. The material of the airflow control plate 20 is preferably quartz glass, but it may also be made of metal as long as it does not affect the target material 30. The thickness of the airflow control plate 20 is, for example, 3 mm to 10 mm. Updrafts are particularly likely to occur during processing in a closed space, such as when coating the inner surface of a cylindrical target material.
[0034] The airflow control plate 20 is installed within a range of ±45° from a position parallel to the burner axis. Within this range, it is possible to sufficiently prevent the updraft from interfering with the burner flame. If the angle is less than -45° or more than +45°, it is not possible to sufficiently prevent the updraft from interfering with the burner flame.
[0035] It is more preferable to install the airflow control plate 20 within ±20° of the position parallel to the burner axis. Within this range, the updraft can be more effectively prevented from interfering with the burner flame. If the angle is less than −20° or more than +20°, the updraft cannot be effectively prevented from interfering with the burner flame.
[0036] It is more preferable that the airflow control plate 20 is installed parallel to the burner axis, which is the direction in which the burner flame is blown. By installing the airflow control plate 20 parallel to the burner axis, the distance between the airflow control plate 20 and the burner flame becomes constant over the entire burner flame, compared to when the plate is installed non-parallel, and it is possible to suppress fluctuations of the flame and stabilize the flame.
[0037] The burner is preferably positioned so that the angle between the axial direction of the burner and the vertical direction is 30° or more and 150° or less. When the airflow control plate 20 is installed within a range of ±45° based on a position parallel to the axis of the burner, by positioning the burner so that the angle between the axial direction of the burner and the vertical direction is 30° or more and 150° or less, interference of the rising air current with the burner flame can be more reliably suppressed.
[0038] The airflow control plate 20 is preferably installed in a position in the direction of gravity of the burner. By arranging the airflow control plate 20 in this position, it is possible to more sufficiently suppress the rising air current from interfering with the burner flame.
[0039] The airflow control plate 20 is preferably disposed in an area where the distance L from the center of the burner flame to the surface facing the burner flame is 20 mm or more and 500 mm or less, and more preferably 30 mm or more and 100 mm or less. If the distance between the airflow control plate 20 and the burner flame is 20 mm or more, thermal deformation of the airflow control plate 20 due to radiant heat during long-term coating can be suppressed. If the distance between the airflow control plate 20 and the burner flame is 500 mm or less, the flow of rising air currents into the flame can be effectively suppressed.
[0040] The distance D between the edge of the airflow control plate 20 in the blowing direction of the burner flame and the coated surface of the target member 30 (for example, the inner peripheral surface of the target member 30) is preferably 5 mm or more and 20 mm or less, and the airflow control plate 20 is installed so that the distance D is, for example, 10 mm. This makes it possible to prevent the rising air current from flowing through the gap between the airflow control plate 20 and the coated surface of the target member 30 from interfering with the burner flame.
[0041] When the burner 1 moves, the airflow control plate 20 moves in accordance with the movement of the burner 1. For example, the airflow control plate 20 may be attached integrally with the quartz burner.
[0042] The shape of the airflow control plate 20 is not particularly limited, but it is preferable that the end of the airflow control plate 20 in the blowing direction of the burner flame has a shape that follows the coating surface of the target member 30. This makes it possible to prevent the rising air current from flowing through the gap between the airflow control plate 20 and the coating surface of the target member 30 from interfering with the burner flame.
[0043] It is also preferable that the airflow control plate 20 is line-symmetrical about the axis of the projection line of the burner flame onto the airflow control plate 20. In other words, it is preferable that the shape of the airflow control plate 20 is line-symmetrical with respect to the axis of the burner 1. This allows the airflow control plate 20 to divide the ascending air currents symmetrically, thereby suppressing the fluctuation of the burner flame.
[0044] For example, as shown in Figure 4, when the inner circumferential surface of a cylindrical target member 30 is coated with a burner 1 disposed at the center, it is preferable to use a fan-shaped airflow control plate 20. The projection line of the burner flame projected onto the airflow control plate 20 bisects the central angle of the fan shape. The central angle of the fan shape is preferably 30° to 225°, and more preferably 45° to 90°. By making the central angle 30° or more, it is possible to prevent the rising air current from interfering with the burner flame. By making the central angle 225° or less, it is possible to reduce the cost of the airflow control plate 20. If the central angle is 180°, it becomes a semicircle.
[0045] [Regarding the steps of the method for manufacturing a quartz component] When manufacturing a quartz component, i.e., when coating a target component 30, the tip of the burner 1 is positioned toward the target component 30, and the distance from the tip of the burner 1 to the target component 30 is adjusted. An airflow control plate is also positioned between the tip of the burner 1 and the target component 30, below the burner 1. Without supplying raw silica powder, the burner 1 is ignited, and the distance between the burner 1 and the target component 30 is adjusted so that the surface of the target component 30 reaches 1800°C or higher and becomes incandescent. This distance adjustment facilitates the formation of a transparent and dense coating film. The angle of the airflow control plate is also adjusted so that it is parallel to the burner flame.
[0046] Thereafter, while maintaining the burner 1 in an ignited state, the supply of raw material silica powder is started, and while maintaining a constant distance from the target member 30, the burner 1 is moved or the target member 30 is moved while coating the surface of the target member 30. The coating does not necessarily have to be formed on the entire surface of the target member, and only a portion may be coated.
[0047] Moving the burner includes moving the tip of the burner horizontally or vertically to change the direction of the flame. For example, the direction of the burner flame is 30° to 150° from the vertical direction (a range of +60° to -60° from the horizontal), preferably 45° to 135°, and more preferably 70° to 100°. By moving the direction of the burner flame, it is possible to coat a desired area.
[0048] It is not necessary to constantly supply the raw silica powder. After a predetermined coating thickness is obtained, the coating surface may be flattened by heating with only an oxyhydrogen flame.
[0049] "Quartz Component Coating Apparatus" The quartz component coating apparatus of the present invention comprises a burner and an airflow control plate, the airflow control plate being installed within a ±45° range relative to the axis of the burner. The burner and airflow control plate of the quartz component coating apparatus of the present invention can be the burner 1 and airflow control plate 20 used in the quartz component manufacturing method described above. Furthermore, the preferred position of the airflow control plate 20 relative to the burner 1 can also be the preferred position described in the quartz component manufacturing method described above. The quartz component coating apparatus of the present invention can also incorporate the silica powder feed device and other coating support equipment depending on the desired characteristics. Furthermore, the target components and coating surfaces that the quartz component coating apparatus of the present invention preferably coat are curved, similar to the quartz component manufacturing method described above. The quartz component coating apparatus of the present invention can form a transparent and dense coating film on a quartz component.
[0050] "Method for Regenerating Quartz Members" The method for regenerating quartz members of the present invention is characterized in that a quartz coating film is provided on the quartz member using the quartz coating device described above. According to the method for regenerating quartz members of the present invention, a transparent and dense coating film can be provided on the quartz member, thereby allowing the quartz member to be regenerated.
[0051] [Example 1] A cylindrical quartz jig with a thickness of 7 mm and an inner diameter of 500 mm was used as the target member. This quartz jig was fixed vertically, and a burner 1 was placed horizontally inside the quartz jig. The distance between the inner peripheral surface of the quartz jig and the tip of the burner was set to 160 mm.
[0052] An airflow control plate 20 consisting of a fan-shaped quartz plate with a thickness of 5 mm, a radius of 240 mm, and a central angle of 60° was installed symmetrically 50 mm below the tip of the burner, so that it was horizontal to the axis of the burner and the distance between the edge of the fan shape (arc portion) and the inner surface of the quartz jig was 10 mm.
[0053] Silica powder with an average particle size (D50) of 80 μm (metal impurity content of 0.1 ppm or less) was supplied at a rate of 1.2 g / min with a carrier gas flow rate of 2 L / min, and fusion coating of the silica powder was carried out using an oxyhydrogen flame under conditions of a hydrogen gas flow rate of 90 L / min and an oxygen gas flow rate of 25 L / min. Nitrogen was used as the carrier gas.
[0054] The quartz jig was rotated at an angular velocity of 2 mm / sec on its inner circumferential surface while spraying the coating. The burner flame remained stable during the coating process, and a 5 mm wide, uniformly thick quartz member (molten coating film) was formed on the inner circumferential surface of the quartz jig.
[0055] Comparative Example 1 A quartz member was formed (fusion coating) on the inner peripheral surface of a quartz jig in the same manner as in Example 1, except that no airflow control plate was provided.
[0056] During the formation of the quartz component (coating), the burner flame was occasionally disturbed in the vertical direction, and irregular sounds thought to be caused by air currents were confirmed. Although a 5 mm wide coating film was formed on the inner surface of the quartz jig, adhesion of silica powder and undissolved silica powder were observed at positions 2.5 mm to 5 mm from the center of the coating.
[0057] REFERENCE SIGNS LIST 1 burner 2 silica powder supply pipe 3 oxygen gas supply pipe 4 hydrogen gas supply pipe 5 barrel 6 oxygen gas nozzle 10 silica powder feed device 11 suction line 12 scraper 13 hopper 20 airflow control plate 30 target member
Claims
1. A method for manufacturing a quartz component, comprising a fire processing process in which heat is applied to the surface of a workpiece containing quartz using a burner, and an airflow control plate is installed within a range of ±45° based on a position parallel to the axis of the burner during the fire processing process.
2. The method for manufacturing a quartz member according to claim 1, wherein the fire processing step includes a process of spraying molten silica powder onto the surface of the workpiece to form a coating.
3. The method for manufacturing a quartz member according to claim 1 or 2, wherein the shape of the airflow control plate is linearly symmetrical with respect to the axis of the burner.
4. The method for manufacturing a quartz member according to claim 1 or 2, wherein the distance between the surface of the airflow control plate corresponding to said burner and the axis of said burner is 20 mm or more and 500 mm or less.
5. A method for manufacturing a quartz member according to claim 1 or 2, wherein the angle between the axial direction of the burner and the vertical direction is 30° or more and 150° or less.
6. The method for manufacturing a quartz member according to claim 1 or 2, wherein the airflow control plate is disposed at a position in the direction of gravity of the burner.
7. The method for manufacturing a quartz member according to claim 1 or 2, wherein the airflow control plate is installed within ±20° of a position parallel to the axis of the burner.
8. The method for manufacturing a quartz member according to claim 1 or 2, wherein the burner has a plurality of supply pipes for supplying gas or powder.
9. The method for manufacturing a quartz member according to claim 1 or 2, wherein the burner has supply pipes for silica powder, oxygen gas, and hydrogen gas.
10. The method for manufacturing a quartz member according to claim 2, wherein a gas having a volume ratio of oxygen of 80% or less is used as a carrier gas for the silica powder.
11. The method for manufacturing a quartz member according to claim 1 or 2, wherein the surface to be processed of the workpiece is a curved surface.
12. A quartz component coating apparatus having a burner and an airflow control plate, the airflow control plate being installed within a range of ±45° with respect to a position parallel to the axis of the burner.
13. The quartz member coating apparatus according to claim 12, wherein the distance between said airflow control plate and the axis of said burner is 20 mm or more and 500 mm or less.
14. The quartz member coating apparatus according to claim 12, wherein the airflow control plate is disposed at a position in the gravity direction of the burner.
15. The apparatus for coating a quartz member according to claim 12, wherein the angle between the axial direction of the burner and the vertical direction is equal to or greater than 30° and equal to or less than 150°.
16. The quartz member coating apparatus according to claim 12, wherein the airflow control plate is installed within ±20° of a position parallel to the direction of the flame blowing.
17. A method for regenerating a quartz member, comprising providing a quartz coating film on the quartz member by using the quartz member coating apparatus according to any one of claims 12 to 16.
Citation Information
Patent Citations
Quartz glass article and production thereof
JP1995126025A
Quartz glass thermal sprayed componentt and method for producing the same
JP2004142996A
Burner for generating glass soot
JP1992238820A
Production of porous glass preform for optical fiber and apparatus therefor
JP1997030829A
Device for manufacturing quartz glass
JP2002234746A