BEA-type zeolite
The ammonia temperature-programmed desorption method effectively produces BEA type zeolites with high acid strength and crystallinity, addressing the limitations of previous synthesis methods by controlling the SiO2/Al2O3 molar ratio and preserving active acid sites, thus enhancing their catalytic performance.
Patent Information
- Application Number
- PCT/JP2024/013015
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for synthesizing BEA type zeolites, such as acid treatment and steam treatment, often result in decreased acid strength and crystallinity due to aluminum elution from the skeletal structure, leading to suboptimal performance in catalytic applications.
The use of the ammonia temperature-programmed desorption method (NH3-TPD) to produce BEA type zeolites with specific diffraction intensity ratios and Al MAS NMR peak characteristics, ensuring high acid strength and crystallinity by controlling the SiO2/Al2O3 molar ratio and maintaining four-coordinated aluminum as active acid sites.
This approach results in BEA type zeolites with enhanced acid strength and crystallinity, suitable for a wide range of applications including catalysis and exhaust gas purification, by maintaining a high degree of structural integrity and active acid site density.
Smart Images

Figure JPOXMLDOC01-APPB-M000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
BEA type zeolite
[0001] The present invention relates to a BEA-type zeolite.
[0002] Zeolites are crystalline aluminosilicates with uniform pores due to their crystalline structure. Taking advantage of this characteristic, zeolites are industrially used as molecular sieve adsorbents that adsorb only molecules of a specific size, adsorption / separation agents that adsorb molecules with strong affinity, or catalyst substrates. For example, BEA-type zeolites are used as catalysts in the petrochemical industry and as catalysts for purifying exhaust gases.
[0003] BEA-type zeolite has been synthesized using an organic structure directing agent (OSDA). BEA-type zeolite synthesized without using an OSDA has also been proposed. BEA-type zeolite synthesized without using an OSDA contains a large amount of Al in the framework, and SiO 2 / Al 2 O 3 The molar ratio tends to be low. 2 / Al 2 O 3 Zeolites with a low molar ratio are characterized by high ion exchange capacity.
[0004] In order to use zeolite in a wide range of applications, it is necessary to select SiO suitable for the intended purpose, taking into consideration the affinity with the reactants due to differences in hydrophilicity, hydrophobicity, polarity, etc. 2 / Al 2 O 3 It is important that the molar ratio can be adjusted to the desired SiO 2 / Al 2 O 3 There is a need to prepare zeolites with a molar ratio of SiO 2 / Al 2 O 3 When the molar ratio is increased, dealumination is carried out to obtain the desired SiO 2 / Al 2 O 3 It is desired to provide a zeolite having a molar ratio of 0.1 to 0.2.
[0005] US Pat. Nos. 5,999,952 and 5,999,952 disclose a process for dealuminating zeolites by acid treatment and / or steam treatment.
[0006] Special table 2018-506500 publication Special table 2015-536291 publication
[0007] However, when zeolite is dealuminated by acid treatment and / or steam treatment as described in Patent Documents 1 and 2, aluminum in the framework structure of the zeolite is eluted, which may reduce the acid strength of the zeolite. Furthermore, when aluminum in the framework structure of the zeolite is dealuminated, defects may occur in the crystal structure, which may reduce the crystallinity.
[0008] Therefore, the present invention is a wide range of SiO 2 / Al 2 O 3 The object of the present invention is to provide a BEA-type zeolite having high acid strength and crystallinity in a molar ratio.
[0009] The present invention relates to a BEA-type zeolite, and the BEA-type zeolite is obtained by ammonia temperature-programmed desorption (NH 3 -TPD method) when the temperature is increased at 10 ° C / min. 3 The present invention proposes a BEA-type zeolite in which, in a TPD spectrum, the apex of the peak resulting from adsorption to the acid sites of the BEA-type zeolite is in the range of 340°C or higher and 500°C or lower, and in an X-ray diffraction spectrum measured by an X-ray diffraction method using CuKα radiation, the ratio A / B of the maximum diffraction intensity A of the peak of the BEA-type zeolite to the diffraction intensity B of the (111) plane of Si, which is standard material 640c distributed by the National Institute of Standards and Technology, is 25 or higher.
[0010] The present invention relates to a BEA-type zeolite, and the BEA-type zeolite is 27The present invention proposes a BEA zeolite in which, when a peak located in an Al MAS NMR spectrum with a chemical shift value at the peak apex in the range of 55.5 ppm or more and 60.0 ppm or less is defined as Peak 1, and a peak located in the range of 51.0 ppm or more and less than 55.5 ppm with a chemical shift value at the peak apex, the area ratio P1 / (P1+P2) of the area P1 of Peak 1 to the sum of the areas P1 of Peak 1 and P2 of Peak 2 is within the range of 0.4 or more and 1.0 or less, and in an X-ray diffraction spectrum measured by an X-ray diffraction method using CuKα radiation, the ratio A / B of the maximum diffraction intensity A of the peak of the BEA zeolite to the diffraction intensity B of the (111) plane of Si, which is standard material 640c distributed by the National Institute of Standards and Technology, is 25 or more.
[0011] The present invention is based on a wide range of SiO 2 / Al 2 O 3 At this molar ratio, a BEA-type zeolite having high acid strength and high crystallinity can be provided.
[0012] 1 shows the X-ray diffraction spectra of the BEA zeolites obtained in Example 3 and Comparative Example 2. 2 shows the relationship between the acid strength and the acid amount per molar amount of Al of the BEA zeolites obtained in Example 1 and Comparative Example 2. 3 shows the NMR spectrum of the BEA zeolite obtained in Example 3. 4 shows the NMR spectrum of the BEA zeolite obtained in Comparative Example 4. 5 shows the NMR spectrum of the BEA zeolite obtained in Comparative Example 4.
[0013] The embodiments of the present invention may include the following technical ideas: [1] BEA type zeolite, wherein the BEA type zeolite is obtained by ammonia temperature programmed desorption (NH 3 -TPD method) when the temperature is increased at 10 ° C / min. 3[2] A BEA zeolite, wherein in a TPD spectrum, the apex of a peak resulting from adsorption to acid sites of the BEA zeolite is in the range of 340°C or higher and 500°C or lower, and in an X-ray diffraction spectrum measured by an X-ray diffraction method using CuKα radiation, the ratio A / B of the maximum diffraction intensity A of the peak of the BEA zeolite to the diffraction intensity B of the Si (111) plane, which is standard material 640c distributed by the National Institute of Standards and Technology, is 25 or higher. 27 [3] A BEA-type zeolite in which, when a peak located in an Al MAS NMR spectrum with a chemical shift value at the peak apex in the range of 55.5 ppm to 60.0 ppm is defined as Peak 1 and a peak located in the range of 51.0 ppm to less than 55.5 ppm with a chemical shift value at the peak apex in the range of 51.0 ppm to less than 55.5 ppm, the area ratio P1 / (P1+P2) of the area P1 of Peak 1 to the sum of the areas P1 of Peak 1 and P2 of Peak 2 is in the range of 0.4 to 1.0, and in an X-ray diffraction spectrum measured by an X-ray diffraction method using CuKα radiation, the ratio A / B of the maximum diffraction intensity A of the peak of the BEA-type zeolite to the diffraction intensity B of the (111) plane of Si, which is standard material 640c distributed by the National Institute of Standards and Technology, is 25 or more. 2 / Al 2 O 3 [1] The BEA zeolite according to [1] or [2], wherein the molar ratio is within the range of 13 or more and 1000 or less. [4] The BEA zeolite according to any one of [1] to [3], which is a proton-type BEA zeolite ion-exchanged with hydrogen ions, a sodium-type BEA zeolite ion-exchanged with sodium ions, or an ammonium-type BEA zeolite ion-exchanged with ammonium ions. [5] The BEA zeolite according to [1] or [2], wherein the molar ratio is determined by ammonia temperature-programmed desorption (NH 3 The BEA zeolite according to any one of [1] to [4], wherein the total molar amount of ammonium adsorbed to the acid sites of the BEA zeolite is 0.30 mmol / Al-mmol or more when the temperature is raised at 10°C / min by a TPD method.
[0014] The present invention will now be described based on embodiments, although the present invention is not limited to the embodiments described below.
[0015] BEA-type zeolite is produced by the ammonia temperature-programmed desorption method (NH 3 -TPD method) when the temperature was raised at 10 ° C. / min. 3 In the -TPD spectrum, the apex of the peak resulting from adsorption to the acid sites of BEA zeolite is in the range of 340°C or higher and 500°C or lower, and in the X-ray diffraction spectrum measured by X-ray diffraction using CuKα radiation, the ratio A / B of the maximum diffraction intensity A of the peak of BEA zeolite to the diffraction intensity B of the (111) plane of Si, which is standard material 640c distributed by the National Institute of Standards and Technology, is 25 or higher.
[0016] BEA-type zeolite is used in ammonia temperature-programmed desorption (NH 3 -TPD method) when the temperature was raised at 10 ° C. / min. 3 When the apex of the peak due to adsorption on the acid sites of BEA-type zeolite in the TPD spectrum is in the range of 340°C or more and 500°C or less, NH is present on the acid sites that exhibit high acid strength. 3 This indicates that BEA zeolite has high acid strength. 3 In the -TPD spectrum, the apex of the peak due to adsorption to the acid sites of BEA zeolite is preferably in the range of 350°C or higher and 500°C or lower, more preferably in the range of 350°C or higher and 450°C or lower.
[0017] In an X-ray diffraction spectrum of BEA zeolite measured by an X-ray diffraction method using CuKα radiation, the ratio A / B of the maximum diffraction intensity A of the peak of BEA zeolite to the diffraction intensity B of the (111) plane of Si, which is standard material 640c distributed by the National Institute of Standards and Technology, is 25 or more. The ratio A / B is an index of the crystallinity of BEA zeolite. When the ratio A / B is 25 or more, a high degree of crystallinity is maintained and the crystal structure is stable. In the X-ray diffraction spectrum of BEA zeolite, the ratio A / B is more preferably 27 or more, even more preferably 33 or more, even more preferably 35 or more, and particularly preferably 40 or more, and may be 200 or less, 150 or less, 100 or less, or 80 or less. The X-ray diffraction spectrum of BEA-type zeolite can be measured by an X-ray diffractometer (for example, RINT-TTR III, manufactured by Rigaku Corporation) using CuKα rays (0.15406 nm, 50 kV, 300 mA) as an X-ray source.
[0018] BEA type zeolite is 27 In an Al MAS NMR spectrum, when Peak 1 has a chemical shift value at the peak apex in the range of 55.5 ppm or more and 60.0 ppm or less, and Peak 2 has a chemical shift value at the peak apex in the range of 51.0 ppm or more and less than 55.5 ppm, the area ratio P1 / (P1+P2) of the area of Peak 1 to the sum of the areas of Peak 1 and Peak 2 is in the range of 0.4 or more and 1.0 or less, and in an X-ray diffraction spectrum measured by an X-ray diffraction method using CuKα radiation, the ratio A / B of the maximum diffraction intensity A of the peak of BEA zeolite to the diffraction intensity B of the (111) plane of Si, which is standard material 640c distributed by the National Institute of Standards and Technology, is 25 or more.
[0019] BEA type zeolite 27 The Al MAS NMR spectrum can be measured, for example, under the following conditions: Magnetic field: 14.1 T ( 1H 600 MHz) Spectrometer: AVANCE NEO600 manufactured by Bruker Measurement and data processing software: TopSpin manufactured by Bruker NMR probe: 3.2 mm MAS probe Sample rotation speed: 20 kHz Standard sample for chemical shift values and radio frequency intensity: potassium alum Chemical shift value reference: The central peak of potassium alum is set to -0.21 ppm. Spectral center (O1 value - SR value (chemical shift notation)): 53.066 ppm Radio frequency pulse intensity: The pulse width that maximizes the potassium alum peak when the spectral center is 51.675 ppm is set to 4.5 μs. Radio frequency pulse width: 2.5 μs Measurement interval: 10.4 μs (5.2 μs when converted to the value indicated by the symbol DW on the software mentioned above) Number of measurement points: 961 points (1922 when converted to the value indicated by the symbol TD on the software mentioned above) Number of spectrum points (symbol SI on the software mentioned above): 4096 points Number of accumulations (symbol NS on the software mentioned above): 3200
[0020] The spectrum obtained as described above is subjected to baseline correction using calculation software, 27 An Al MAS NMR spectrum is obtained. The baseline is created by connecting point Q1, which is the arithmetic mean of the chemical shift values and signal intensities of all points from the point closest to 90 ppm to the point closest to 100 ppm, with point Q2, which is the arithmetic mean of the chemical shift values and signal intensities of all points from the point closest to -50 ppm to the point closest to -40 ppm. The spectrum obtained in this manner is referred to as the "measured Al spectrum." Peak 1 and Peak 2 are peaks obtained by peak separation of the measured Al spectrum. Peak separation is performed by adding two pseudo-Voigt functions to the measured Al spectrum and then calculating a calculated spectrum. 27This is performed by fitting in the range from the point closest to the Al chemical shift value -40 ppm to the point closest to 90 ppm (hereinafter referred to as the "range of -40 ppm to 90 ppm" for convenience). The pseudo-Voigt function is the sum of a Lorentzian function and a Gaussian function with the same full width at half maximum. The pseudo-Voigt function f(x) used in peak separation is shown in Equation (1) below. The peak area of each peak is determined by the sum of the signal intensities of the peaks calculated by the pseudo-Voigt function at points in the range of -40 ppm to 90 ppm in the measured Al spectrum. In addition, the chemical shift value x of the peak apex obtained by fitting with this pseudo-Voigt function is 0 are referred to as the "chemical shift values of the peak apex" of Peak 1 and Peak 2. Fitting is performed until the ratio of the mean square error D0 between the measured spectrum and the calculated spectrum (hereinafter referred to as the "calculated spectrum"), with respect to the maximum value Y0 in the range of -40 ppm to 90 ppm where the chemical shift of the measured spectrum is the sum of all the peaks, D0 / Y0, is 0.01 or less. If D0 / Y0 is not 0.01 or less, one or more peaks whose chemical shift at the peak apex is in the range of more than 59.0 ppm and not more than 90 ppm, and one or more peaks whose chemical shift at the peak apex is in the range of -40 ppm to less than 45 ppm are added. If the addition of this peak makes D0 / Y0 0.01 or less, no peaks are added. If D0 / Y0 is greater than 0.01, the above operation is repeated. The "pseudo-Voigt function" is based on "6. Profile functions and pattern decomposition methods" in "Special feature: New developments in powder diffraction methods," Journal of the Crystallographic Society of Japan, 34, 86 (1992).
[0021] BEA type zeolite 27In an Al MAS NMR spectrum, the sum (P1+P2) of the peak areas P1 and P2 of the two peaks, Peak 1 and Peak 2, is positively correlated with the amount of aluminum in BEA zeolite. , "Effective fabrication of catalysts from large-pore, multi-dimensional zeolites synthesized without using organic structure-directing agents," Chemistry of Materials, 2014, 26(2), 1250-1259 (hereinafter sometimes referred to as "Non-Patent Document Yoshihiro"). As shown in this document, T1 to T9 silicon sites are present.
[0022] BEA type zeolite 27 In the Al MAS NMR spectrum, Peak 1 is located in the range of 55.5 ppm to 60.0 ppm in chemical shift value of the peak apex. The area P1 of Peak 1 is positively correlated with the amount of aluminum substituted at the silicon sites T3 to T9 among the nine silicon sites T1 to T9 that exist equivalently in the crystal structure of BEA-type zeolite. When multiple peaks are observed in the range of 55.5 ppm to 60.0 ppm, the area P1 of Peak 1 is taken as the total area of the multiple peaks. It is presumed that the reason multiple peaks are observed is that aluminum is detected in the process of being desorbed. Note that when the area P1 of Peak 1 is large, it is difficult to determine the amount of aluminum substituted at the silicon sites T3 to T9 among the nine silicon sites T1 to T9 that exist equivalently in the crystal structure of BEA-type zeolite. 3 -TPD method) 3) adsorption amount increases, and therefore, it is thought that oxygen (O) bonded to aluminum substituted at silicon sites T3 to T9 among silicon sites T1 to T9 in the crystal structure of BEA zeolite is likely to become a strong acid site. Peak 1 represents a peak derived from aluminum substituted at silicon sites T3 to T9 among nine silicon sites T1 to T9 that exist equivalently in the crystal structure of BEA zeolite. When aluminum (Al) is substituted at silicon (Si) sites T3 to T9 in the crystal structure of BEA zeolite, ammonia (NH 3 The amount of ammonia adsorbed increases, and when ammonia is adsorbed on zeolite and then desorbed by calcination, acid sites are formed by the tetracoordinated aluminum. The acid sites formed by the tetracoordinated aluminum in BEA zeolite are Bronsted acid sites. The acid sites of the tetracoordinated aluminum in BEA zeolite serve as active sites for oxidation reactions when purifying adsorbed hydrocarbons (HC).
[0023] BEA type zeolite 27 In the Al MAS NMR spectrum, Peak 2 has a peak apex chemical shift value in the range of 51.0 ppm or more and less than 55.5 ppm. Peak 2 represents a peak derived from aluminum substituted at the T1 and / or T2 silicon sites among the nine silicon sites T1 to T9 that exist equivalently in the crystal structure of BEA zeolite. The aluminum substituted at the T1 and / or T2 silicon sites is a tetrahedral aluminum that is relatively unlikely to function as an acid site, and the acid site adjacent to the Al atom formed by the four ranges of aluminum that are relatively unlikely to function as an acid site is a relatively weak acid, resulting in low acid strength. When multiple peaks are observed in the range of 51.0 ppm or more and less than 55.5 ppm, the area P2 of Peak 2 is the sum of the areas of the multiple peaks. It is speculated that the reason multiple peaks are observed is because aluminum is detected in the process of being desorbed.
[0024] The obtained BEA type zeolite 27In the Al MAS NMR spectrum, peaks whose peak apex chemical shift values are in the range of −10.0 ppm to 10.0 ppm are peaks derived from hexacoordinated aluminum present outside the framework structure of the zeolite.
[0025] The obtained BEA type zeolite 27 In an Al MAS NMR spectrum, the area ratio P1 / (P1+P2) is a value that shows a positive correlation with the abundance ratio of aluminum that is substituted at silicon sites T3 to T9 and that is likely to become strong acid sites that exhibit high acid strength, relative to the total amount of aluminum substituted at nine silicon sites T1 to T9 in a BEA zeolite sample. The number of silicon sites T1 to T9 in one unit cell of BEA zeolite is 4 sites for T7 and T9, respectively, and 8 sites for T1 to T6 and T8, respectively. In one unit cell of BEA zeolite, the total number of sites T3 to T9 is 48, and the total number of sites T1 and T2 is 16. BEA zeolite 27 In the Al MAS NMR spectrum, when the area ratio P1 / (P1+P2) of the area of peak 1 P1 to the sum of the area P1 of peak 1 and the area P2 of peak 2 is in the range of 0.4 to 1.0, a high acid strength is maintained and a large number of Bronsted acid sites are present. 27 The relationship with Al MAS NMR spectra is described in the aforementioned non-patent document Yoshihiro.
[0026] The aluminum substituted at the silicon sites T1 to T9 in the BEA zeolite sample is tetrahedral coordinated aluminum and functions as an acid site, as reported in J. A. van Bokhoven et al., "Stepwise Dealumination of Zeolite Beta at Specific T-Sites Observed with 27 Al MAS and 27 Al MQ MAS NMR," J. Am. Chem. Soc., 2000, 122, 12842-12847. Aluminum substituted at the silicon sites of T3 to T9 is H 2It is described that by attracting O, octahedrally coordinated aluminum is formed, and the cations are delocalized. From this, the inventors speculate that aluminum substituted at the silicon sites T3 to T9 functions as a strong acid site because the charge imbalance is greater than that of aluminum substituted at the silicon sites T1 and T2. Conversely, aluminum substituted at the silicon sites T1 and T2 functions as a relatively weak acid site because the charge imbalance is smaller than that of aluminum substituted at the silicon sites T3 to T9.
[0027] A wide range of SiO 2 / Al 2 O 3 In terms of obtaining a BEA zeolite having a high crystallinity and a high acid strength, the molar ratio of BEA zeolite is 27 The area ratio P1 / (P1+P2) in the Al MAS NMR spectrum is in the range of 0.4 to 1.0, preferably in the range of 0.5 to 0.95, more preferably 0.6 or more, and may be 0.90 or less, or 0.85 or less.
[0028] The pseudo-Voigt function f(x) used in peak separation of the pseudo-Voigt spectrum can be derived from the following equation (1).
[0029]
[0030] In formula (1), x is the value on the horizontal axis of the NMR spectrum (chemical shift value), x 0 is the chemical shift value of the peak apex, S is a scaling coefficient to fit the actual measurement, η is the peak area ratio of the Lorentz function (first term) in the range from -∞ (minus infinity) to +∞ (plus infinity), H and Δ are the full width at half maximum of the peak, π is the ratio of the circumference of a circle to its diameter, ln is the natural logarithm function, and exp is the natural exponential function. In peak separation, the x of each of the two pseudo-Voigt functions is 0、Fitting is performed using the solver function of the calculation software so that the mean square deviation between the chemical shift values of the measured spectrum and the calculated spectrum in the range of -40 ppm to 90 ppm is minimized, with Δ, η, and S as variables. The scaling coefficient S is a normalized value so that the sum of S for all peaks is 1.
[0031] The BEA zeolite of the present invention is SiO 2 / Al 2 O 3 The molar ratio is preferably in the range of 13 to 1000. BEA-type zeolite has a wide range of SiO 2 / Al 2 O 3 In this molar ratio, it has high acid strength and high crystallinity, and the desired SiO 2 / Al 2 O 3 It is possible to provide a BEA zeolite having a molar ratio of SiO 2 / Al 2 O 3 The molar ratio may be in the range of 14 or more and 800 or less, or may be 700 or less, 600 or less, 500 or less, or 400 or less. 2 / Al 2 O 3 Zeolites with a high molar ratio have high hydrothermal durability. Hydrothermal durability indicates the resistance of the crystalline structure to destruction when exposed to high temperatures in the presence of water vapor. 2 / Al 2 O 3 Zeolites with a low molar ratio have a large amount of Al in the zeolite framework. Therefore, the charge of the zeolite framework becomes negative, which makes it easier for cations to be introduced from outside the framework, thereby increasing the ion exchange capacity. 2 / Al 2 O 3 The molar ratio can be evaluated from the Si amount and Al amount obtained by measuring the Si amount and Al amount by elemental analysis using an X-ray fluorescence analyzer (e.g., ZSX Primus II, manufactured by Rigaku Corporation) or ICP emission spectroscopic analysis.
[0032] The BEA zeolite may be at least one type of zeolite selected from the group consisting of proton-type BEA zeolite ion-exchanged with hydrogen ions, sodium-type BEA zeolite ion-exchanged with sodium ions, and ammonium-type BEA zeolite ion-exchanged with ammonium ions. The obtained BEA zeolite may be brought into contact with water or an aqueous solution containing sodium ions or ammonium ions to obtain a BEA zeolite of each cation type, or ammonium ion-type BEA zeolite may be heated to obtain a proton-type BEA zeolite.
[0033] The amount of Al contained in BEA-type zeolite was measured by ammonia temperature-programmed desorption (NH 3 It is preferable that the total molar amount of ammonium adsorbed on the acid sites of the BEA zeolite when the temperature is raised at 10°C / min by the TPD method is 0.30 mmol / Al-mmol or more. If the total molar amount of ammonium adsorbed on the acid sites relative to the molar amount of Al of the BEA zeolite is 0.30 mmol / Al-mmol or more, NH 3 The total molar amount of ammonium adsorbed at the acid sites relative to the molar amount of Al in the BEA zeolite is more preferably 0.35 mmol / Al-mmol or more, even more preferably 0.38 mmol / Al-mmol or more, and is 1.8 mmol / Al-mmol or less, preferably 1.0 mmol / Al-mmol or less, more preferably 0.95 mmol / Al-mmol or less, and may be 0.90 mmol / Al-mmol or less, or may be 0.85 mmol / Al-mmol or less.
[0034] The BEA zeolite of the present invention can be produced by the following production method. The production method for BEA zeolite preferably includes the steps of preparing zeolite, mixing zeolite with water to prepare a zeolite mixed solution, and continuously supplying a solution containing an inorganic acid to the zeolite mixed solution.
[0035] In a method for producing zeolite, a solution containing an inorganic acid is continuously supplied to a zeolite mixture, whereby the zeolite reacts gently with the inorganic acid. As a result, Al not contained in the framework structure and tetracoordinated Al contained in the framework structure, which are relatively difficult to function as acid sites, are preferentially dissolved, while tetracoordinated Al, which is relatively easy to function as acid sites, tends to remain in the framework structure. For tetracoordinated Al, the acid sites adjacent to the Al atoms in the framework structure of the zeolite become Brønsted acid sites. The acid sites formed by tetracoordinated Al in zeolite have strong acid strength and, for example, when hydrocarbons are adsorbed, serve as active sites for reactions in purifying the adsorbed hydrocarbons. Tricoordinated Al serves as Lewis acid sites, and are acid sites other than the acid sites that are the center of catalytic activity. Tetracoordinated aluminum, which serves as Brønsted acid sites with strong acid strength, remains in the framework structure and becomes the center of catalytic activity. The tetracoordinated aluminum, which is relatively difficult to function as acid sites, is dissolved from the framework structure, resulting in a decrease in Al while maintaining high acid strength, resulting in the formation of, for example, SiO 2 / Al 2 O 3 From low molar ratio zeolite to SiO 2 / Al 2 O 3 Zeolites with a high molar ratio of SiO can be prepared. 4 and AlO 4 In the crystalline structure of zeolite, which is composed of repeating tetrahedral units, even if Al, which is relatively difficult to function as an acid site, is dissolved, Al, which is relatively easy to function as an acid site, remains, so that SiO 2 / Al 2 O 3 Zeolites with adjusted molar ratios can be obtained.
[0036] The solution containing an inorganic acid preferably has a pH of 5 or less at room temperature (for example, 25° C.). By continuously supplying a solution containing an inorganic acid having a pH of 5 or less to the zeolite mixed solution, the inorganic acid and zeolite react gently, and Al that is not contained in the framework structure or Al that does not easily function as an acid site is preferentially eluted from the framework structure, thereby forming SiO while maintaining high acid strength. 2 / Al 2 O 3The molar ratio can be adjusted. The solution containing the inorganic acid to be continuously supplied to the zeolite mixed solution preferably has a pH of 5 or less, but may also have a pH of 3 or less, 1 or less, −2 or more, or −1.5 or more, so that the zeolite and the inorganic acid contained in the solution react slowly.
[0037] The rate at which the solution containing an inorganic acid is continuously supplied per 1000 g of zeolite contained in the zeolite mixture is preferably 3.0 mL / min or less, more preferably 2.5 mL / min or less, even more preferably 2.0 mL / min or less, and even more preferably 1.8 mL / min or less. There is no lower limit, but from the viewpoint of production efficiency, it may be, for example, 0.05 mL / min or more, 0.10 mL / min or more, 0.12 mL / min or more, 0.15 mL / min or more, or 0.20 mL / min or more. When the rate at which the solution containing an inorganic acid is continuously supplied per 1000 g of zeolite contained in the zeolite mixture is 3.0 mL / min or less, the zeolite and the inorganic acid react slowly, and SiO is formed while maintaining high acid strength and high crystallinity. 2 / Al 2 O 3 The molar ratio can be adjusted.
[0038] The concentration of the inorganic acid in the solution containing the inorganic acid to be continuously supplied to the zeolite mixed liquid may be 50% by mass or more, 60% by mass or more, 70% by mass or more, 75% by mass or more, 100% by mass or less, or 98% by mass or less.
[0039] The total mass of inorganic acid added per 1000 g of zeolite is preferably in the range of 200 g or more, more preferably in the range of 250 g or more, even more preferably in the range of 300 g or more, and even more preferably in the range of 325 g or more. The total mass of inorganic acid is determined based on the SiO of the target zeolite. 2 / Al 2 O 3Since the amount can be adjusted depending on the molar ratio and the supply rate, there is no upper limit, but it may be, for example, 1500 g or less, 1250 g or less, or 1150 g or less. When the total mass of the inorganic acid relative to 1000 g of zeolite is within the range of 200 g or more, by continuously supplying a solution containing the inorganic acid to the zeolite mixed solution, the inorganic acid and the zeolite react gently, and SiO is produced while maintaining high acid strength and high crystallinity. 2 / Al 2 O 3 Zeolites with adjusted molar ratios can be obtained.
[0040] The temperature of the zeolite mixed solution when the solution containing an inorganic acid is continuously supplied is preferably 80° C. or higher, and may be 90° C. or higher, or may be 100° C. If the temperature of the zeolite mixed solution when the solution containing an inorganic acid is continuously supplied is 80° C. or higher, the zeolite and the inorganic acid tend to react more gently.
[0041] It is preferable to continuously supply the solution containing an inorganic acid while stirring the zeolite mixture. Continuously supplying the solution containing an inorganic acid while stirring the zeolite mixture facilitates the reaction between the zeolite and the inorganic acid. There are no particular limitations on the method for continuously supplying the solution containing an inorganic acid, and examples include methods such as constant volume feeding and dropwise addition. The stirring speed of the zeolite mixture is preferably changed depending on the volume of the zeolite mixture and the amount of zeolite in the zeolite mixture, and can be, for example, 5 rpm or more and 300 rpm or less.
[0042] The time for continuously supplying the solution containing an inorganic acid depends on the supply rate, but may be 1 hour or more, 2 hours or more, 3 hours or more, 3.5 hours or more, 40 hours or less, or 38 hours or less. If the time for continuously supplying the solution containing an inorganic acid is 1 hour or more or less and 40 hours or less, the inorganic acid and the zeolite react gently, and Al, which is relatively difficult to function as an acid site, is preferentially eluted from the framework structure, and high acid strength and high crystallinity are maintained, and SiO 2 / Al 2 O 3 Zeolites with adjusted molar ratios can be obtained.
[0043] The inorganic acid can be any known acid used for dealumination of zeolites without any particular limitation, for example, at least one selected from the group consisting of phosphoric acid, sulfuric acid, hydrochloric acid, nitric acid, and a mixture of two or more thereof.
[0044] It is preferable to continuously supply a solution containing an inorganic acid to the zeolite mixture, and then maintain the zeolite and the inorganic acid without separating the solution containing the inorganic acid from the zeolite. By continuously supplying the solution containing the inorganic acid and then keeping the zeolite and the inorganic acid in contact without separating them, the reaction between the inorganic acid and the zeolite progresses further, and Al, which is relatively difficult to function as an acid site, can be preferentially eluted from the framework structure. As a result, SiO can be obtained while maintaining high acid strength and high crystallinity. 2 / Al 2 O 3 It is possible to obtain zeolite with an adjusted molar ratio. After continuously supplying a solution containing an inorganic acid to a zeolite mixture, the zeolite and the inorganic acid are maintained without separating the solution containing the inorganic acid from the zeolite, which is also called "aging."
[0045] After continuously supplying the solution containing the inorganic acid to the zeolite mixed solution, the time for which the zeolite and the inorganic acid are kept without separating the solution containing the inorganic acid from the zeolite is determined by the amount of SiO2 of the target zeolite. 2 / Al 2 O 3 The time can be adjusted according to the molar ratio. For example, the time for which the zeolite and the inorganic acid are maintained may be 1 hour or more, 2 hours or more, 3 hours or more, 15 hours or less, or 12 hours or less. The time for which the zeolite and the inorganic acid are maintained without separating the inorganic acid-containing solution from the zeolite after the inorganic acid-containing solution is continuously supplied to the zeolite mixed solution is also referred to as the "aging time."
[0046] In the aging step, stirring may or may not be performed. When stirring is performed, the stirring speed may be, for example, 5 rpm or more and 300 rpm or less.
[0047] A solution containing an inorganic acid may be continuously supplied to the zeolite mixed solution, and after aging, a second step of continuously supplying a solution containing an inorganic acid may be performed. The second step of continuously supplying a solution containing an inorganic acid may be performed under the same conditions (concentration, amount, rate, time) as the first continuous supply, or may not be the same conditions. After the second step of continuously supplying a solution containing an inorganic acid, an aging step may be further performed.
[0048] The zeolite to be prepared is SiO 2 / Al 2 O 3 The molar ratio is preferably 3 or more. 2 / Al 2 O 3 When the molar ratio is 3 or more, a solution containing an inorganic acid is continuously supplied to the zeolite mixed solution, and the zeolite and the inorganic acid are reacted to produce SiO 2 / Al 2 O 3 The molar ratio of SiO 2 / Al 2 O 3 The molar ratio of SiO of the prepared zeolite can be adjusted. 2 / Al 2 O 3 The molar ratio may be 5 or more, 8 or more, or 9 or more. 2 / Al 2 O 3 There is no particular upper limit to the molar ratio, but by removing aluminum contained in zeolite, a wide range of SiO 2 / Al 2 O 3 From the viewpoint of adjusting the molar ratio of zeolite, it is preferable that aluminum is contained in a large amount. For example, SiO 2 / Al 2 O 3 The molar ratio may be 500 or less, 400 or less, or 350 or less.
[0049] The zeolite to be prepared is preferably one synthesized without using an organic structure directing agent (OSDA). Zeolite synthesized without using an OSDA does not require removal of the OSDA, and the energy and cost required for removing the OSDA can be reduced. In addition, zeolite synthesized without using an OSDA has few defects and SiO 2 / Al 2 O 3 The molar ratio of aluminum is 3 or more, and the zeolite contains a large amount of aluminum. Therefore, by continuously supplying a solution containing an inorganic acid to the zeolite mixture, the inorganic acid and the zeolite react gently, and Al, which is relatively difficult to function as an acid site, is preferentially eluted from the framework structure, leaving Al, which is relatively easy to function as an acid site and contributes to the formation of acid sites in the framework structure. This allows the SiO 2 / Al 2 O 3 The molar ratio can be adjusted to be higher. Zeolite synthesized without using OSDA is also called OSDA-free zeolite. BEA zeolite synthesized without using OSDA is also called OSDA-free BEA zeolite. OSDA-free BEA zeolite can be produced, for example, by referring to the description in WO 2021 / 002322.
[0050] The BEA zeolite to be prepared may be at least one type of zeolite selected from the group consisting of proton-type BEA zeolite ion-exchanged with hydrogen ions, sodium-type BEA zeolite ion-exchanged with sodium ions, and ammonium-type BEA zeolite ion-exchanged with ammonium ions. Regarding the BEA zeolite to be prepared, BEA zeolite of each cation type may be obtained by contacting BEA zeolite with water or an aqueous solution containing sodium ions or ammonium ions, or proton-type BEA zeolite may be obtained by heating ammonium ion-type BEA zeolite.
[0051] The water to be mixed with the zeolite is preferably deionized water or pure water. The concentration of the zeolite mixture is not particularly limited and can be adjusted appropriately depending on the amount of zeolite to be prepared, the scale of the production equipment, etc.
[0052] A solution containing an inorganic acid is continuously supplied to the zeolite mixed solution, and then separated from the resulting treated mixed solution. The zeolite separated from the mixed solution may be washed, dried, or calcined. Separation of the zeolite can be performed by methods such as filtration, ultrafiltration, diafiltration, or centrifugation. The separated zeolite may be washed with water, alcohol such as methanol, ethanol, or propanol, or a mixture thereof. The washed zeolite may be dried, and the drying may be performed as long as moisture is removed. For example, the zeolite may be dried in an air atmosphere at a temperature of 50°C to 120°C for 3 hours to 25 hours. Drying may be performed using a dryer such as a fluidized bed dryer or a spray dryer.
[0053] Desired SiO 2 / Al 2 O 3 Zeolites having high acid strength and high crystallinity in a molar ratio can be used, for example, as catalysts in the petrochemical industry, hydrocarbon adsorbents, and catalyst compositions for purifying exhaust gases containing hydrocarbon adsorbents. Exhaust gas purifying catalysts formed using the exhaust gas purifying compositions can be used as catalysts for purifying exhaust gases from internal combustion engines such as gasoline engines and diesel engines.
[0054] Catalysts in the petrochemical industry, hydrocarbon adsorbents, and exhaust gas purifying compositions containing BEA-type zeolite can be used in any form, such as powder, paste, or granules. For example, the exhaust gas purifying composition can be used as a catalyst layer formed on a catalyst support. The catalyst support can be made of, for example, ceramics or metal materials. Ceramics used as catalyst supports include alumina (Al 2 O 3 ), mullite (3Al 2 O 3 -2SiO 2 ), cordierite (2MgO-2Al2 O 3 -5SiO 2 ), aluminum titanate (Al 2 TiO 5 ), silicon carbide (SiC), etc. Examples of metal materials used as catalyst supports include stainless steel, etc. The shape of the catalyst support is not particularly limited, but examples include a honeycomb shape, a plate shape, and a pellet shape.
[0055] A catalyst structure including an exhaust gas purifying catalyst using an exhaust gas purifying composition in a catalyst layer may include a catalyst layer made of a conventionally known catalyst material other than the exhaust gas purifying composition. Also, a catalyst structure using an exhaust gas purifying composition in a catalyst layer can be used as a DPF (Diesel Particulate Filter) or a GPF (Gasoline Particulate Filter).
[0056] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0057] Preparation of Zeolite Used in Examples 1 to 5 According to the method described in the examples of WO 2021 / 002322, specifically, an OSDA-free BEA zeolite is prepared as follows. (1) Preparation of Seed Crystals Tetraethylammonium hydroxide was used as the OSDA, sodium aluminate was used as the alumina source, and finely divided silica (P707, manufactured by Mizusawa Industrial Chemicals) was used as the silica source. These were stirred and heated at 165 ° C. for 96 hours to synthesize a BEA zeolite having a Si / Al molar ratio of 12. The obtained BEA zeolite was calcined in an electric furnace at 550 ° C. for 10 hours while circulating air to produce seed crystals that did not contain organic matter. The seed crystals did not contain OSDA.
[0058] (2) Preparation of OSDA-Free Sodium-Type BEA-Type Zeolite (Na-BEA) OSDA-free BEA-type zeolite was prepared in accordance with the method described in the examples of Japanese Patent No. 4904417, specifically as follows. An aqueous solution was obtained by dissolving 2.35 g of sodium aluminate and 18.28 g of 36 mass % sodium hydroxide in 139 g of deionized water. A mixture of 20.24 g of finely powdered silica (M-5, manufactured by CABOT Corporation) and 2.02 g of the seed crystals was added little by little to the aqueous solution and stirred to obtain SiO 2 / Al 2 O 3 A reaction mixture having a composition with the molar ratios shown in Table 1 was obtained. This reaction mixture was placed in a 60 mL stainless steel sealed container and, without aging or stirring, was allowed to stand and heated under autogenous pressure at 140°C for 46 hours. After the sealed container was cooled, the product was filtered and washed with warm water to obtain a white powder. By the X-ray diffraction measurement described below, it was confirmed that the white powder product obtained was OSDA-free sodium BEA zeolite (Na-BEA) containing no impurities. The SiO of the obtained OSDA-free BEA zeolite 2 / Al 2 O 3 The molar ratios were measured using a scanning X-ray fluorescence analyzer described below. The results are shown in Table 1. In Tables 1, 2, and 3 shown below, "-" indicates that the corresponding item was not treated or that the corresponding value does not exist.
[0059] (3) OSDA free ammonium type BEA type zeolite (NH 3 10 g of the obtained OSDA-free sodium-type BEA-type zeolite was dispersed in 300 mL of a 2 mol / L aqueous ammonium nitrate solution. This dispersion was kept at 80°C for 24 hours. Thereafter, the dispersion was filtered, washed with a sufficient amount of distilled water, and dried overnight at 100°C. In this way, OSDA-free ammonium-type BEA-type zeolite (NH 3 -BEA) was obtained.
[0060] (4) Preparation of OSDA-free proton-type BEA zeolite (H-BEA) The obtained OSDA-free ammonium-type BEA zeolite was calcined at 600° C. for 2 hours in an ammonia atmosphere to obtain OSDA-free proton-type BEA zeolite (H-BEA).
[0061] Preparation of Zeolite Used in Reference Example 1 The same OSDA-free proton type BEA type zeolite (H-BEA) as used in Examples 1 and 2 was used.
[0062] Preparation of Zeolite Used in Comparative Example 1 The zeolite used in Comparative Example 1 was obtained in the same manner as in the preparation of the seed crystals used in the Examples.
[0063] Preparation of Zeolite Used in Comparative Examples 2 to 4 The same OSDA-free proton type BEA type zeolite (H-BEA) as used in Examples 1 and 2 was used.
[0064] Examples 1 to 5 Each prepared BEA zeolite was mixed with pure water to obtain a zeolite mixture having the concentration shown in Table 1. The weight of each BEA zeolite shown in Table 1 is the weight in a dry state. Here, the "dry state" refers to a state in which the change (fluctuation range) in moisture content when measured with a moisture meter (MX-50, manufactured by A&D Co., Ltd.) is 0.01% or less. Using sulfuric acid or nitric acid as the inorganic acid, aqueous sulfuric acid or nitric acid solutions were prepared at the concentrations and pHs shown in Table 2. The zeolite mixture was set to the temperature shown in Table 2 and placed in a flask. While stirring, the aqueous sulfuric acid or nitric acid solution was continuously supplied (dropwise) to the zeolite mixture in the amount, addition rate, and addition time shown in Table 2. After the aqueous sulfuric acid or nitric acid solution was continuously supplied to the zeolite mixture, the zeolite was aged by continuously contacting it with sulfuric acid or nitric acid for the time shown in Table 2 without separating the aqueous sulfuric acid or nitric acid solution from the zeolite. Table 2 also shows the total time for continuously supplying the aqueous sulfuric acid or nitric acid solution and the aging time.
[0065] Reference Example 1 and Comparative Example 1 The prepared zeolites used in Reference Example 1 and Comparative Example 1 were evaluated as described below. Note that Reference Example 1 and Comparative Example 1 were not treated with an inorganic acid.
[0066] Comparative Examples 2 and 3 Each of the prepared zeolites was mixed with pure water to obtain a zeolite mixture having the concentration shown in Table 1. Sulfuric acid was used as the inorganic acid, and aqueous sulfuric acid solutions were prepared at the concentrations and pHs shown in Table 2. The zeolite mixture was set to the temperature shown in Table 2, placed in a flask, and, while stirring, an aqueous sulfuric acid solution in the amount shown in Table 2 was supplied all at once to the zeolite mixture. After the entire amount of the aqueous sulfuric acid solution was supplied all at once to the zeolite mixture, the zeolite was kept in contact with sulfuric acid without separating the aqueous sulfuric acid solution from the zeolite, and aged for the time shown in Table 2. Because the entire amount of the aqueous sulfuric acid solution was supplied all at once to the zeolite mixture, the time during which the aqueous sulfuric acid solution was continuously supplied was 0 hours, and the total time during which the aqueous sulfuric acid solution was continuously supplied and the aging time was the same as the aging time.
[0067] Comparative Example 4 The prepared zeolite was calcined at 800°C, and then the same procedure as in Comparative Example 2 was carried out.
[0068] The zeolites obtained by the production methods of Examples 1 to 5, and the zeolites of the Reference Examples and Comparative Examples were evaluated as follows. The results are shown in Table 1 or Table 3.
[0069] Zeolite Framework Structure The X-ray diffraction spectrum of the prepared zeolite and the zeolites according to the Examples, Reference Examples, and Comparative Examples was confirmed to be BEA-type zeolite by measuring the X-ray diffraction spectrum of the obtained zeolite using a powder X-ray diffractometer. If the X-ray diffraction spectrum using CuKα radiation obtained using a powder X-ray diffractometer has diffraction peaks at diffraction angles 2θ of 8±1.5° and 22.8±1°, it can be confirmed that the zeolite is BEA-type zeolite. The positions of the diffraction angles 2θ (°) of the diffraction peaks in the X-ray diffraction spectrum are the same as the positions of the diffraction angles 2θ (°) of the diffraction peaks in the X-ray diffraction spectrum published by the International Zeolite Society. Figure 1 shows the X-ray diffraction spectra of Example 3 and Comparative Example 2.
[0070] Zeolite SiO 2 / Al 2 O 3Molar ratio: The Si content and Al content in each zeolite sample were measured by elemental analysis using a scanning X-ray fluorescence analyzer (ZSX Primus II, manufactured by Rigaku Corporation), and the SiO content was calculated from the measured Si content and Al content. 2 / Al 2 O 3 The molar ratio of SiO was calculated from the Si content and Al content in the measurement sample of each zeolite. 2 / Al 2 O 3 The molar ratio was calculated.
[0071] Ammonia temperature-programmed desorption (NH 3 -TPD method) For each zeolite, ammonia temperature programmed desorption (NH 3 -TPD method) and NH 3 The TPD spectrum was obtained. The measurement was carried out according to the following procedure. As a pretreatment, approximately 0.05 g of zeolite was heated to 500°C in He gas, held at 500°C for 10 minutes, and then cooled to 100°C and held there for 10 minutes. Next, at a sample temperature of 100°C, ammonia gas diluted with He gas (the concentration of ammonia in He is 5 vol%, hereinafter referred to as "5% NH 3 -He). Ammonia was adsorbed onto the zeolite at a flow rate of 50 sccm for 30 minutes. Thereafter, the sample was purged in He gas for 30 minutes to remove the physically adsorbed ammonia. The temperature was then increased from 100°C to 610°C at a rate of 10°C / min, and the amount of ammonia desorbed was measured. The measurement equipment used was a catalyst analyzer BELCAT-II (manufactured by Microtrac-Bell Corporation) and an online gas analyzer BELMass (manufactured by Microtrac-Bell Corporation). The area of the TCD signal obtained by the measurement was calculated using waveform separation software ChemMaster (manufactured by Microtrac-Bell Corporation). 5% NH 3The area value of the TCD signal was converted to the amount of ammonia desorption using a calibration curve that utilizes the relationship between the flow rate and area when -He gas was flowed at a specified flow rate. Furthermore, peak separation was performed on the obtained TCD signal using the above-mentioned software. Peak separation was performed using the waveform decomposition function of the software. The TCD signal may have two or three peaks. The inventors speculate that, from the low-temperature side, each peak represents physical adsorption, adsorption to acid sites, and desorption of structural water. The peak representing desorption of structural water may not appear.
[0072] Amount of acid (mmol) NH 3 The TCD signal obtained by the measurement by the TPD method was analyzed, and the area of the peak corresponding to adsorption to the acid sites (corresponding to the total molar amount of ammonium adsorbed to the acid sites of the BEA zeolite) was calculated, and this was taken as the amount of acid.
[0073] Acid amount per mole of Al (mmol / Al-mmol) was calculated by dividing the above-mentioned acid amount value by the mole amount of Al contained in the zeolite. The mole amount of Al was calculated based on the SiO 2 / Al 2 O 3 The calculation was made using the results of the molar ratio measurements.
[0074] Acid strength (°C) NH 3 The TCD signal obtained by the measurement using the TPD method was analyzed, and the peak apex temperature of the peak due to adsorption to the acid sites of BEA zeolite was taken as the acid strength. Figure 2 shows the relationship between the acid strength and the amount of acid per mole of Al for Example 1 and Comparative Example 2.
[0075] Ratio A / B (Crystallinity) X-ray diffraction spectra were measured by XRD using an X-ray diffractometer (Rigaku Corporation, RINT-TTR III) and CuKα radiation (0.15406 nm, 50 kV, 300 mA) as the X-ray source. Measurement conditions included a diffraction angle 2θ of 5° to 80°, a scan rate of 20° / min, and a scan step width of 0.02°. The software "PDXL2" was used to analyze the diffraction intensity. After removing the background, the Kα1 position was used as the peak position and fitted with a split pseudo-Voigt function to obtain the diffraction peak intensity. The peak intensity B of the (111) plane was determined from the X-ray diffraction spectrum measured for Si, the standard material 640c distributed by the National Institute of Standards and Technology. The maximum diffraction intensity A of the peak was determined from the X-ray diffraction spectrum measured for each zeolite in the Examples, Reference Examples, and Comparative Examples. The ratio A / B of the maximum diffraction intensity A of the peak to the peak intensity B was calculated.
[0076] 27 Al MAS NMR spectrum of each zeolite 27 The Al MAS NMR spectrum was measured to determine the structure of each zeolite. 27 In the Al MAS NMR spectrum, Peak 1, whose peak apex has a chemical shift value in the range of 55.5 ppm to 60.0 ppm, and Peak 2, whose peak apex has a chemical shift value in the range of 51.0 ppm to less than 55.5 ppm, were calculated. The area P1 of Peak 1, the area P2 of Peak 2, the sum of the areas P1 and P2 (P1+P2), and the area ratio P1 / (P1+P2) of the area P1 to the sum of the areas P1 and P2 were calculated and are shown in Table 3. 27 In the Al MAS NMR spectrum, the area of the peak whose chemical shift value at the peak apex was in the range of −10.0 ppm to 10.0 ppm was calculated. 27 In the Al MAS NMR spectrum, peaks whose peak apex chemical shift values are in the range of -10.0 ppm to 10.0 ppm are peaks derived from hexacoordinated aluminum present outside the framework structure of the zeolite. In Table 3, peaks derived from hexacoordinated aluminum present outside the framework structure of the zeolite are described as "hexacoordinated." Figures 3 and 4 show the NMR spectrum of the BEA zeolite obtained in Example 3 and an enlarged view of the peak derived from tetracoordinated aluminum, respectively. Figures 5 and 6 show the NMR spectrum of the BEA zeolite obtained in Comparative Example 4 and an enlarged view of the peak derived from tetracoordinated aluminum, respectively.
[0077]
[0078]
[0079]
[0080] The BEA zeolites according to Examples 1 to 5 were tested for acid strength (NH 3 The temperature at the top of the peak in the -TPD spectrum) was in the range of 340°C or more and 500°C or less. The BEA zeolites according to Examples 1 to 5 had a ratio A / B of 25 or more and had a higher degree of crystallinity than the BEA zeolites according to Comparative Examples 1 to 3, which were not subjected to dropwise addition of an inorganic acid. In addition, the BEA zeolites according to Examples 1 to 5 had a ratio A / B of 25 or more and had a higher degree of crystallinity than the BEA zeolites according to Comparative Examples 1 to 3, which were not subjected to dropwise addition of an inorganic acid. 2 / Al 2 O 3 The molar ratio is in the range of 13 to 1000, specifically, SiO 2 / Al 2 O 3 The molar ratio is in the range of 14 to 500, and a wide range of SiO 2 / Al 2 O 3 A BEA-type zeolite having the following molar ratio was obtained.
[0081] The BEA zeolites according to Examples 1 to 5 had an area ratio P1 / (P1+P2) of 0.4 or more and 1.0 or less, and contained a large amount of tetrahedral Al that easily functioned as an acid site, and thus had high acid strength. In addition, the ratio A / B was 25 or more, and thus had a high degree of crystallinity.
[0082] The BEA zeolites according to Examples 1 to 5 can be proton-type BEA zeolites, sodium-type BEA zeolites, or ammonium-type BEA zeolites, and can be used in a wide range of SiO 2 / Al 2 O 3 At this molar ratio, a zeolite with high acid strength and high crystallinity was obtained.
[0083] The BEA zeolites according to Examples 1 to 5 were purified by ammonia temperature programmed desorption (NH 3 The acid amount (total ammonium mole amount adsorbed to the acid sites of the zeolite) when the temperature was raised at 10°C / min by the TPD method was 0.30 mmol / Al-mmol or more relative to the Al mole amount contained in the BEA zeolite, and the zeolite had acid sites that exhibited high acid strength.
[0084] The BEA-type zeolites of the present disclosure are zeolites having a wide range of SiO 2 / Al 2 O 3 In this molar ratio, it has high acid strength and high crystallinity, and can be used as a catalyst in the petrochemical industry, a hydrocarbon adsorbent, an exhaust gas purification catalyst, etc.
Claims
1. BEA type zeolite, the BEA type zeolite being produced by ammonia temperature programmed desorption (NH 3 -TPD method) when the temperature is increased at 10 ° C / min NH 3 A BEA-type zeolite, in which in a -TPD spectrum, the apex of a peak resulting from adsorption to acid sites of the BEA-type zeolite is in the range of 340°C or higher and 500°C or lower, and in an X-ray diffraction spectrum measured by an X-ray diffraction method using CuKα radiation, the ratio A / B of the maximum diffraction intensity A of the peak of the BEA-type zeolite to the diffraction intensity B of the Si (111) plane, which is standard material 640c distributed by the National Institute of Standards and Technology, is 25 or higher.
2. BEA type zeolite, the BEA type zeolite being: 27 A BEA-type zeolite, in which, when a peak located in an Al MAS NMR spectrum with a chemical shift value at the peak apex in the range of 55.5 ppm or more and 60.0 ppm or less is defined as Peak 1, and a peak located in the range of 51.0 ppm or more and less than 55.5 ppm is defined as Peak 2, an area ratio P1 / (P1+P2) of the area P1 of Peak 1 to the sum of the areas P1 of Peak 1 and P2 of Peak 2 is within the range of 0.4 or more and 1.0 or less, and a ratio A / B of the maximum diffraction intensity A of the peak of the BEA-type zeolite to the diffraction intensity B of the (111) plane of Si, which is standard material 640c distributed by the National Institute of Standards and Technology, in an X-ray diffraction spectrum measured by an X-ray diffraction method using CuKα radiation, is 25 or more.
3. SiO 2 / Al 2 O 3 3. The BEA zeolite according to claim 1 or 2, wherein the molar ratio is in the range of 13 or more and 1,000 or less.
4. A BEA type zeolite according to claim 1 or 2, which is a proton type BEA type zeolite ion-exchanged with hydrogen ions, a sodium type BEA type zeolite ion-exchanged with sodium ions, or an ammonium type BEA type zeolite ion-exchanged with ammonium ions.
5. The amount of Al contained in the BEA zeolite is calculated by ammonia temperature programmed desorption method (NH 3 3. The BEA zeolite according to claim 1, wherein the total molar amount of ammonium adsorbed to the acid sites of the BEA zeolite is 0.30 mmol / Al-mmol or more when the temperature is raised at 10° C. / min by a TPD method.
Citation Information
Patent Citations
Post-treatment of zeolite materials
JP2015536291A
Method for producing dealuminated zeolitic material with bea framework structure
JP2018506500A
Beta-type zeolite and method for producing the same
JP4904417B2
Beta-type zeolite and catalyst containing same
WO2021002322A1
Beta zeolite and method for producing the same
JP2011126768A