Low-oxygen vanadium carbide and preparation method therefor

The synthesis of low-oxygen vanadium carbide through a carbonization-reduction reaction, high-energy milling, and vacuum heat treatment addresses the challenge of vanadium's oxygen affinity, producing a material with low oxygen content and small particle size, suitable for various applications.

WO2024205148A1PCT designated stage expired Publication Date: 2024-10-03KOREA INSTITUTE OF GEOSCIENCE AND MINERAL RESOURCES
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003637
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Vanadium carbide synthesis is challenging due to vanadium's high affinity for oxygen, leading to the formation of oxycarbides with high oxygen content, making it difficult to produce pure low-oxygen vanadium carbide with a small particle size and excellent physical properties.

Method used

Reducing oxygen content through a carbonization-reduction reaction by mixing vanadium oxide with a carbon compound, refining the particle size via high-energy milling, and performing vacuum heat treatment to produce low-oxygen vanadium carbide with a particle size of 2 nm to 50 μm and a chemical formula of VCx, where 0.3 < x < 1.

Benefits of technology

The method results in low-oxygen vanadium carbide with low oxygen content, small particle size, and excellent physical properties, suitable for use as a precursor, cemented carbide material, catalyst, or semiconductor material, while ensuring process stability and economical mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003637_03102024_PF_FP_ABST
    Figure KR2024003637_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a low-oxygen vanadium carbide and a preparation method therefor, the low-oxygen vanadium carbide having reduced oxygen content and being formed by mixing a vanadium oxide with a carbon compound, and then refining the particle size thereof by means of high-energy milling by using a high-energy milling apparatus, and carbonizing and reducing same by means of a vacuum heat treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Low-oxygen vanadium carbide and method for producing the same

[0001] The present invention relates to a low-oxygen vanadium carbide and a method for producing the same, which is formed by reducing the oxygen content, mixing vanadium oxide and a carbon compound, and then refining the particle size through high-energy milling using a high-energy milling device, followed by vacuum heat treatment and carbonization reduction reaction.

[0002] Vanadium metal is a material that readily forms carbides, nitrides, or oxides due to its high affinity for non-metallic elements such as carbon, nitrogen, or oxygen.

[0003] Therefore, vanadium carbide, which is manufactured through the combination of vanadium and carbon, can be said to be a compound that can be easily manufactured, but due to the characteristic of vanadium having a high affinity for oxygen, it is not easy to synthesize pure carbide (with a low amount of oxygen).

[0004] That is, V(C x O 1-x ), it is not easy to manufacture vanadium carbide with a low oxygen content because the formation of oxycarbide in the form of x < 1 is easy.

[0005] In particular, low-oxygen vanadium carbides, which are considered to be thermodynamically possible to form, are compounds in which vacancies exist in some carbon positions in the form of VCx, and in reality, there are many vacancies in the lattice, and oxygen penetration into the vacancies occurs easily, resulting in V(C x O 1-x ) It is very difficult to synthesize low-oxygen vanadium carbides because they easily change into .

[0006] Accordingly, the applicant, through long-term, painstaking efforts and various studies, has obtained a low-oxygen vanadium carbide and a method for producing the same by reducing the oxygen content, mixing vanadium oxide and carbon compounds, and then refining the particle size through high-energy milling using a high-energy milling device, and then performing a vacuum heat treatment to cause a carbonization-reduction reaction, thereby completing the present invention.

[0007] Accordingly, the purpose of the present invention is to provide a low-oxygen vanadium carbide formed by reducing the oxygen content, mixing vanadium oxide and a carbon compound, and then refining the particle size through high-energy milling using a high-energy milling device, followed by vacuum heat treatment and carbonization reduction reaction.

[0008] In addition, an object of the present invention is to provide a method for producing low-oxygen vanadium carbide by mixing vanadium oxide and a carbon compound, then refining the particle size through high-energy milling using a high-energy milling device, and then performing a vacuum heat treatment to carry out a carbonization reduction reaction.

[0009] In addition, the purpose of the present invention is to provide a use for low-oxygen vanadium carbide formed by mixing vanadium oxide and a carbon compound, then refining the particle size through high-energy milling using a high-energy milling device, and then performing a vacuum heat treatment to undergo a carbonization-reduction reaction.

[0010] In addition, an object of the present invention is to provide low-oxygen vanadium carbide having a particle size of 2 nm to 50 μm, manufactured by the method for manufacturing the above low-oxygen vanadium carbide.

[0011] In addition, an object of the present invention is to provide a low-oxygen vanadium carbide having a chemical formula of VCx manufactured by the method for manufacturing the low-oxygen vanadium carbide, wherein the range of x is 0.3 < x < 1.

[0012] In addition, an object of the present invention is to provide a use of low-oxygen vanadium carbide having a particle size of 2 nm to 50 μm produced by the method for producing low-oxygen vanadium carbide.

[0013] In addition, an object of the present invention is to provide a use of a low-oxygen vanadium carbide having a chemical formula of VCx manufactured by the method for manufacturing the low-oxygen vanadium carbide, wherein the range of x is 0.3 < x < 1.

[0014] The problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the description below.

[0015] In order to solve the above problem, according to one aspect of the present invention,

[0016] As a low-oxygen vanadium carbide,

[0017] It comprises low-oxygen vanadium carbide whose particle size is refined by high-energy milling with reduced oxygen content and high energy input of 0.6 to 2.4 J / g·s.

[0018] The above low-oxygen vanadium carbide is characterized in that it is formed by mixing vanadium oxide and a carbon compound, then refining the particle size through high-energy milling using a high-energy milling device, and then performing a vacuum heat treatment to undergo a carbonization-reduction reaction.

[0019] Provides low-oxygen vanadium carbide.

[0020] According to one embodiment of the present invention, the content of oxygen may be from 10 ppm to 10,000 ppm.

[0021] According to one embodiment of the present invention, the low-oxygen vanadium carbide has a chemical formula of VCx,

[0022] The range of the above x can be 0.3 < x < 1.

[0023] According to one embodiment of the present invention, the molar ratio (B / A) of the carbon compound (B) to the vanadium oxide (A) may be 6.1 to 7.5.

[0024] According to one embodiment of the present invention, the particle size of the mixed powder of the vanadium oxide or the carbon compound may be 2 nm to 50 μm.

[0025] According to one embodiment of the present invention, the vanadium oxide may be at least one selected from vanadium pentoxide (V2O5), sodium metavanadate (NaVO3), vanadium trioxide (V2VO3), vanadium oxychloride (VOCl3), and ammonium metavanadate (H4NVO3).

[0026] According to one embodiment of the present invention, the carbon compound

[0027] It may be at least one selected from industrial carbon powder, coke, coal, coal tar, activated carbon, graphite, natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, industrial diamond, and carbon fiber.

[0028] According to one embodiment of the present invention, the high-energy milling

[0029] After mixing the above vanadium oxide and carbon compound, the mixed powder is fed into a rotating container in a high-energy milling device together with steel balls.

[0030] In an atmosphere of air, vacuum, nitrogen or argon, high energy of 0.6 to 2.4 J / g·s is input, the rotating shaft rotates at 500 to 1500 rpm, and the rotating container rotates at 2000 to 3500 rpm in the direction opposite to the rotation direction of the rotating shaft, so that high-energy milling can be performed for a short time of 10 to 100 minutes.

[0031] According to one embodiment of the present invention, the high-energy milling device

[0032] It could be a ball mill, a specs mill, or an attritor.

[0033] According to one embodiment of the present invention, the vacuum heat treatment

[0034] The heat treatment temperature can be from 800 ℃ to 1600 ℃,

[0035] Heat treatment times can range from 10 minutes to 24 hours.

[0036] According to one embodiment of the present invention, the carbon reduction reaction is

[0037] By refining the above vanadium oxide and carbon compound through the high-energy milling, the contact area can be increased and the carbon reduction reaction rate can be increased.

[0038] In addition, according to another aspect of the present invention,

[0039] A method for producing low-oxygen vanadium carbide,

[0040] (a-1) A step of preparing a mixed powder by mixing vanadium oxide and a carbon compound;

[0041] (a-2) A step of putting the above mixed powder together with a ball into a rotating container in a high-energy milling device;

[0042] (a-3) A step of manufacturing a fine powder by applying high energy of 0.6 to 2.4 J / g·s in an atmosphere of air, vacuum, nitrogen or argon, and rotating the rotating shaft and the rotating container in different directions to perform high-energy milling; and

[0043] (a-4) A step of manufacturing low-oxygen vanadium carbide by subjecting the above fine powder to a vacuum heat treatment and carbonization reduction reaction.

[0044] A method for producing low-oxygen vanadium carbide can be provided.

[0045] According to one embodiment of the present invention, in the step of preparing a mixed powder by mixing vanadium oxide and a carbon compound (a-1),

[0046] The mixing ratio of the above vanadium oxide and the above carbon compound may be 1:0.2 to 1:0.7 by weight.

[0047] According to one embodiment of the present invention, in the step of introducing the mixed powder (a-2) into a rotating container in a high-energy milling device together with a steel ball,

[0048] The above-mentioned ball may be at least one selected from among a ceramic ball, a metal ball, and a superalloy ball.

[0049] According to one embodiment of the present invention, in the step of manufacturing a fine powder by applying high energy of 0.6 to 2.4 J / g·s in an atmosphere of air, vacuum, nitrogen or argon, and rotating the rotating shaft and the rotating container in different directions to perform high-energy milling,

[0050] The above-mentioned rotary shaft rotates at 500 to 1500 rpm, and the rotary container rotates at 2000 to 3500 rpm in the direction opposite to the rotation direction of the rotary shaft, so that high-energy milling can be performed for a short time of 10 to 100 minutes.

[0051] According to one embodiment of the present invention, in the step of manufacturing low-oxygen vanadium carbide by subjecting the (a-4) fine powder to vacuum heat treatment and carbonization reduction reaction,

[0052] The above vacuum heat treatment

[0053] The heat treatment temperature can be from 800 ℃ to 1600 ℃,

[0054] Heat treatment times can range from 10 minutes to 24 hours.

[0055] According to one embodiment of the present invention, the high-energy milling device

[0056] It could be a ball mill, a specs mill, or an attritor.

[0057] In addition, according to another aspect of the present invention, a low-oxygen vanadium carbide can be provided, the use of which is a max precursor, a raw material for a superalloy material, a catalyst, or a semiconductor material.

[0058] In addition, according to another aspect of the present invention, low-oxygen vanadium carbide having a particle size of 2 nm to 50 μm can be provided by the method for producing low-oxygen vanadium carbide.

[0059] In addition, according to another aspect of the present invention, a low-oxygen vanadium carbide having the chemical formula of VCx manufactured by the method for manufacturing the low-oxygen vanadium carbide, wherein the range of x is 0.3 < x < 1, can be provided.

[0060] In addition, according to another aspect of the present invention, the use of the low-oxygen vanadium carbide manufactured by the method for manufacturing the low-oxygen vanadium carbide can provide a low-oxygen vanadium carbide as a max precursor, a raw material for a superalloy material, a catalyst, or a semiconductor material.

[0061] According to the present invention, a low-oxygen vanadium carbide is provided by reducing the oxygen content, mixing vanadium oxide and a carbon compound, and then refining the particle size through high-energy milling using a high-energy milling device, and then vacuum heat-treating to perform a carbonization-reduction reaction, so that the low-oxygen vanadium carbide has a low oxygen content, small particle size, excellent physical properties, and can be used for various purposes such as a max precursor, a raw material for cemented carbide materials, a catalyst, or a semiconductor material.

[0062] In addition, the present invention provides a method for producing low-oxygen vanadium carbide by mixing vanadium oxide and a carbon compound, then refining the particle size through high-energy milling using a high-energy milling device, and then performing a vacuum heat treatment to carry out a carbonization reduction reaction, so that the process stability is excellent and mass production is possible, making it economical.

[0063] In addition, the present invention provides low-oxygen vanadium carbide having a particle size of 2 nm to 50 μm manufactured by the method for manufacturing the low-oxygen vanadium carbide, so that the low-oxygen vanadium carbide has a low oxygen content, a small particle size, excellent physical properties, and can be used for various purposes such as a max precursor, a raw material for a superalloy material, a catalyst, or a semiconductor material.

[0064] In addition, the present invention provides a low-oxygen vanadium carbide having the chemical formula of VCx manufactured by the method for manufacturing the low-oxygen vanadium carbide, wherein the range of x is 0.3 < x < 1, so that the low-oxygen vanadium carbide has a low oxygen content, a small particle size, excellent physical properties, and can be used for various purposes such as a max precursor, a raw material for a superalloy material, a catalyst, or a semiconductor material.

[0065] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the detailed description of the present invention or the composition of the invention described in the claims.

[0066] FIG. 1 is a reaction schematic diagram of a low-oxygen vanadium carbide produced through a carbon reduction reaction of vanadium oxide and a carbon compound according to one embodiment of the present invention.

[0067] Figure 2 is a process flow diagram of a method for manufacturing low-oxygen vanadium carbide according to one embodiment of the present invention.

[0068] Figure 3 is a schematic diagram of a rotating plate of a high-energy milling device according to one embodiment of the present invention.

[0069] FIG. 4 is a TEM image of a vanadium oxide-graphite mixture refined by high-energy milling according to one embodiment of the present invention.

[0070] Figure 5 is a graph of the crystal structure of low-oxygen vanadium carbide according to one embodiment of the present invention.

[0071] Hereinafter, a preferred embodiment according to the present invention will be described in detail with reference to the attached drawings.

[0072] The advantages and features of the present invention and the method for achieving them will become clear with reference to the embodiments described in detail below together with the attached drawings.

[0073] However, the present invention is not limited to the embodiments disclosed below, but may be implemented in various different forms, and these embodiments are provided only to make the disclosure of the present invention complete and to fully inform a person having ordinary skill in the art to which the present invention pertains of the scope of the invention, and the present invention is defined only by the scope of the claims.

[0074] In addition, when describing the present invention, if it is determined that related known technologies, etc. may obscure the gist of the present invention, a detailed description thereof will be omitted.

[0075] Hereinafter, the present invention will be described in detail.

[0076]

[0077] low-oxygen vanadium carbide

[0078] The present invention provides a low-oxygen vanadium carbide formed by reducing the oxygen content, mixing vanadium oxide and a carbon compound, then refining the particle size through high-energy milling using a high-energy milling device, and performing a vacuum heat treatment to cause a carbonization-reduction reaction.

[0079] The present invention is a low-oxygen vanadium carbide,

[0080] It comprises low-oxygen vanadium carbide whose particle size is refined by high-energy milling with reduced oxygen content and high energy input of 0.6 to 2.4 J / g·s.

[0081] The above low-oxygen vanadium carbide is formed by mixing vanadium oxide and a carbon compound, then refining the particle size through high-energy milling using a high-energy milling device, vacuum heat treatment, and carbonization-reduction reaction.

[0082] The present invention provides a low-oxygen vanadium carbide formed by reducing the oxygen content, mixing vanadium oxide and a carbon compound, and then refining the particle size through high-energy milling using a high-energy milling device, and then performing a vacuum heat treatment to cause a carbonization-reduction reaction. Therefore, the low-oxygen vanadium carbide has a low oxygen content, small particle size, excellent physical properties, and can be used for various purposes such as a max precursor, a raw material for cemented carbide materials, a catalyst, or a semiconductor material.

[0083]

[0084] Vanadium metal is a material that readily forms carbides, nitrides, or oxides due to its high affinity for non-metallic elements such as carbon, nitrogen, or oxygen.

[0085] Therefore, vanadium carbide, which is manufactured through the combination of vanadium and carbon, can be said to be a compound that can be easily manufactured, but due to the characteristic of vanadium having a high affinity for oxygen, it is not easy to synthesize pure carbide (with a low amount of oxygen).

[0086] That is, V(C x O 1-x ), it is not easy to manufacture vanadium carbide with a low oxygen content because the formation of oxycarbide in the form of x < 1 is easy.

[0087] In particular, low-oxygen vanadium carbides, which are considered to be thermodynamically possible to form, are compounds in which vacancies exist in some carbon positions in the form of VCx, and in reality, there are many vacancies in the lattice, and oxygen penetration into the vacancies occurs easily, resulting in V(C x O 1-x) It is very difficult to synthesize low-oxygen vanadium carbides because they easily change into .

[0088] Accordingly, the applicant, through long-term, painstaking efforts and various studies, has obtained a low-oxygen vanadium carbide and a method for producing the same by reducing the oxygen content, mixing vanadium oxide and carbon compounds, and then refining the particle size through high-energy milling using a high-energy milling device, and then performing a vacuum heat treatment to cause a carbonization-reduction reaction, thereby completing the present invention.

[0089]

[0090] In addition, the low-oxygen vanadium carbide of the present invention can be formed by mixing vanadium oxide and a carbon compound, then refining the particle size through high-energy milling using a high-energy milling device, and then performing a vacuum heat treatment to cause a carbonization-reduction reaction.

[0091] At this time, the oxygen content may be 10 ppm to 10,000 ppm.

[0092] Here, if the content of oxygen is within the above range, V(C) with a high oxygen content x O 1-x ) may not be easily formed in the form of carbonates.

[0093] At this time, the oxygen content may preferably be 30 ppm to 8,000 ppm, and more preferably 100 ppm to 2,000 ppm.

[0094] And, the above low-oxygen vanadium carbide has a chemical formula of VCx,

[0095] The range of the above x can be 0.3 < x < 1.

[0096] Here, when the range of the above x is within the above range, the low-oxygen vanadium carbide is V(C) with a high oxygen content. x O 1-x ) may not be easily formed in the form of carbonates.

[0097] At this time, the range of x may preferably be 0.4 < x < 0.9, and more preferably 0.45 < x < 0.8.

[0098] Additionally, the molar ratio (B / A) of the carbon compound (B) to the vanadium oxide (A) may be 6.1 to 7.5.

[0099] Here, when the molar ratio (B / A) of the carbon compound (B) to the vanadium oxide (A) is within the above range, the low-oxygen vanadium carbide is V(C) with a high oxygen content. x O 1-x ) may not be easily formed in the form of carbonates.

[0100] At this time, the molar ratio (B / A) of the carbon compound (B) to the vanadium oxide (A) may preferably be 6.3 to 7.0, and more preferably 6.45 to 6.8.

[0101] And, the particle size of the mixed powder of the vanadium oxide or the carbon compound may be 2 nm to 50 μm.

[0102] Here, when the particle size of the mixed powder of the vanadium oxide or the carbon compound is within the above range, the contact area between the vanadium oxide and the carbon compound increases, so that the carbon reduction reaction rate can increase.

[0103] At this time, the particle size of the mixed powder of the vanadium oxide or the carbon compound may preferably be 2 nm to 48 μm, and more preferably 2 nm to 45 μm.

[0104] That is, the present invention increases the reaction rate by reducing the particle size of the mixed powder of vanadium oxide and carbon compound as raw materials to 2 nm to 50 ㎛ through a high-energy milling process, thereby producing a low-oxygen vanadium carbide having a particle size of 2 nm to 50 ㎛ and a low oxygen content.

[0105] Additionally, the vanadium oxide may be at least one selected from vanadium pentoxide (V2O5), sodium metavanadate (NaVO3), vanadium trioxide (V2VO3), vanadium oxychloride (VOCl3), and ammonium metavanadate (H4NVO3).

[0106] Here, when vanadium oxide (V2O5) is used as a raw material for synthesizing vanadium carbide, vanadium carbide is formed through the reaction of vanadium oxide with carbon, i.e., carbonization reduction, as shown in the following chemical formula 1.

[0107]

[0108] V2O5+ 7C → 2VC + 5CO ----- (Chemical Formula 1)

[0109]

[0110] In this process, theoretically, if the amount of carbon is adjusted to less than 7 moles per mole of vanadium oxide, low-oxygen vanadium carbide in the form of VCx can be synthesized.

[0111] However, in the actual process, if the amount of carbon that acts as a reducing agent is lowered, the reaction rate for reduction decreases, and V(C) with a high amount of oxygen x O 1-x ) form of carbonates are easily formed.

[0112] In addition, in order to form vanadium carbide, treatment is required to increase the speed of the carbon reduction reaction as well as adjust the carbon amount.

[0113] In the present invention, the particle size of the mixed powder of vanadium oxide and carbon, which is a raw material, was reduced to the above range through a high-energy milling process to increase the reaction rate, thereby synthesizing a low-oxygen vanadium carbide with a low oxygen content.

[0114] In addition, the above carbon compound

[0115] It may be at least one selected from industrial carbon powder, coke, coal, coal tar, activated carbon, graphite, natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, industrial diamond, and carbon fiber.

[0116] Here, the carbon compound may further include biomass selected from at least one of coffee grounds, fallen leaves, and waste wood.

[0117] Additionally, the carbon compound may further comprise a reducing gas containing carbon, at least one selected from carbon monoxide, methane, and hydrocarbons.

[0118] And, the high energy milling

[0119] After mixing the above vanadium oxide and carbon compound, the mixed powder is fed into a rotating container in a high-energy milling device together with steel balls.

[0120] In an atmosphere of air, vacuum, nitrogen or argon, high energy of 0.6 to 2.4 J / g·s is input, the rotating shaft rotates at 500 to 1500 rpm, and the rotating container rotates at 2000 to 3500 rpm in the direction opposite to the rotation direction of the rotating shaft, so that high-energy milling can be performed for a short time of 10 to 100 minutes.

[0121] Additionally, the high-energy milling device may be a planetary ball mill, a spectrometer, or an attritor.

[0122] Here, the planetary ball mill can reduce the particle size of the mixed powder of the vanadium oxide and the carbon compound to the above range by loading steel balls into a container together with raw materials and causing the container to rotate and revolve at high speed.

[0123] In addition, the above specsmill can reduce the particle size of the mixed powder of the vanadium oxide and the carbon compound to the above range by loading the raw material into a container and causing the container to vibrate up and down and left and right at high speed.

[0124] And, the above-mentioned attritor can reduce the particle size of the mixed powder of the vanadium oxide and the carbon compound to the above range by loading the raw material into the container and transmitting energy by the rotational force of the rotor.

[0125] In addition, the high-energy milling device can reduce the particle size of the mixed powder of the vanadium oxide and the carbon compound to the above range by rotating the rotating direction of the rotating container containing the mixed powder of the vanadium oxide and the carbon compound in the opposite direction to the rotating direction of the rotating axis of the rotating plate.

[0126] And, the vacuum heat treatment

[0127] The heat treatment temperature can be from 800 ℃ to 1600 ℃,

[0128] Heat treatment times can range from 10 minutes to 24 hours.

[0129] Here, when the heat treatment temperature of the vacuum heat treatment is within the above range, the low-oxygen characteristics and manufacturing efficiency of the low-oxygen vanadium carbide can be excellent.

[0130] That is, the mixed powder of the vanadium oxide and the carbon compound produced by the high-energy milling device can be vacuum-heat treated at the heat treatment temperature of the vacuum heat treatment to produce low-oxygen vanadium carbide with excellent low-oxygen characteristics and manufacturing efficiency.

[0131] At this time, the heat treatment temperature of the vacuum heat treatment may preferably be 850°C to 1600°C, and more preferably 900°C to 1600°C.

[0132] And, when the heat treatment time of the vacuum heat treatment is within the above range, the low-oxygen characteristics and manufacturing efficiency of the low-oxygen vanadium carbide can be excellent.

[0133] That is, the mixed powder of the vanadium oxide and the carbon compound produced by the high-energy milling device is subjected to vacuum heat treatment during the heat treatment time of the vacuum heat treatment, thereby producing low-oxygen vanadium carbide having excellent low-oxygen characteristics and manufacturing efficiency.

[0134] At this time, the heat treatment time of the vacuum heat treatment may preferably be 20 minutes to 24 hours, and more preferably 30 minutes to 24 hours.

[0135] In addition, the above carbon reduction reaction

[0136] By refining the above vanadium oxide and carbon compound through the high-energy milling, the contact area can be increased and the carbon reduction reaction rate can be increased.

[0137]

[0138] FIG. 1 is a reaction schematic diagram of a low-oxygen vanadium carbide produced through a carbon reduction reaction of vanadium oxide and a carbon compound according to one embodiment of the present invention.

[0139] Referring to Figure 1, the reaction formula of low-oxygen vanadium carbide manufactured through a carbon reduction reaction of vanadium oxide and a carbon compound is as shown in Chemical Formula 2 below.

[0140]

[0141] VOa + (x + a)C → VCx +aCO ------ (Formula 2)

[0142]

[0143] And, for example, when vanadium oxide (V2O5) is used as a raw material for synthesizing low-oxygen vanadium carbide, vanadium carbide is formed as shown in the following chemical formula 3 through the reaction of vanadium oxide with carbon, i.e., carbonization reduction.

[0144]

[0145] V2O5+ (5+2x)C → 2VCx + 5CO ----- (Chemical Formula 3)

[0146]

[0147] Here, the chemical formula 3 is a combination of the two chemical formulas described in Fig. 1.

[0148]

[0149] Method for producing low-oxygen vanadium carbide

[0150] The present invention provides a method for producing low-oxygen vanadium carbide, which comprises mixing vanadium oxide and a carbon compound, then refining the particle size through high-energy milling using a high-energy milling device, and then performing a vacuum heat treatment to carry out a carbonization-reduction reaction.

[0151] The present invention is a method for producing low-oxygen vanadium carbide,

[0152] (a-1) A step of preparing a mixed powder by mixing vanadium oxide and a carbon compound;

[0153] (a-2) A step of putting the above mixed powder together with a ball into a rotating container in a high-energy milling device;

[0154] (a-3) A step of manufacturing a fine powder by applying high energy of 0.6 to 2.4 J / g·s in an atmosphere of air, vacuum, nitrogen or argon, and rotating the rotating shaft and the rotating container in different directions to perform high-energy milling; and

[0155] (a-4) It includes a step of manufacturing low-oxygen vanadium carbide by vacuum heat-treating the above fine powder and performing a carbonization-reduction reaction.

[0156] The present invention provides a method for producing low-oxygen vanadium carbide by mixing vanadium oxide and a carbon compound, then refining the particle size through high-energy milling using a high-energy milling device, and then performing a vacuum heat treatment to carry out a carbonization-reduction reaction. Therefore, the process stability is excellent, and mass production is possible, making it economical.

[0157] In addition, in the step of manufacturing a mixed powder by mixing the vanadium oxide and carbon compound (a-1),

[0158] The mixing ratio of the above vanadium oxide and the above carbon compound may be 1:0.2 to 1:0.7 by weight.

[0159] Here, when the mixing ratio of the vanadium oxide and the carbon compound is within the above range by weight ratio, V(C) with a high oxygen content x O 1-x ) may not be easily formed in the form of carbonates.

[0160] At this time, the mixing ratio of the vanadium oxide and the carbon compound may preferably be 1:0.4 to 1:0.6 by weight, and more preferably 1:0.45 to 1:0.55 by weight.

[0161] And, in the step of putting the above (a-2) mixed powder together with the steel ball into the rotating container in the high-energy milling device,

[0162] The above-mentioned ball may be at least one selected from among a ceramic ball, a metal ball, and a superalloy ball.

[0163] Specifically, the material of the above-mentioned ball may be steel, tungsten, or zirconia.

[0164] Here, the shape of the ball may be at least one selected from a sphere, a star, a horn, and a columnar shape.

[0165] In addition, in the step of manufacturing fine powder by high energy milling by applying high energy of 0.6 to 2.4 J / g·s in the atmosphere of (a-3) air, vacuum, nitrogen or argon and rotating the rotating shaft and the rotating container in different directions,

[0166] The above-mentioned rotary shaft rotates at 500 to 1500 rpm, and the rotary container rotates at 2000 to 3500 rpm in the direction opposite to the rotation direction of the rotary shaft, so that high-energy milling can be performed for a short time of 10 to 100 minutes.

[0167] Here, the high-energy milling may be a process of applying energy of 0.6 to 2.4 J / g·s, rotating the rotating shaft and the rotating container in opposite directions, and milling the mixed powder of vanadium oxide and carbon compound by friction between the steel balls placed in the rotating container and the mixed powder of vanadium oxide and carbon compound, thereby pulverizing the particles of the mixed powder of vanadium oxide and carbon compound and reducing the average particle size of the mixed powder to 2 nm to 50 ㎛.

[0168] Additionally, the high-energy milling device may be a planetary ball mill, a spectrometer, or an attritor.

[0169] Here, the planetary ball mill can reduce the particle size of the mixed powder of the vanadium oxide and the carbon compound to the above range by loading steel balls into a container together with raw materials and causing the container to rotate and revolve at high speed.

[0170] In addition, the above specsmill can reduce the particle size of the mixed powder of the vanadium oxide and the carbon compound to the above range by loading the raw material into a container and causing the container to vibrate up and down and left and right at high speed.

[0171] And, the above-mentioned attritor can reduce the particle size of the mixed powder of the vanadium oxide and the carbon compound to the above range by loading the raw material into the container and transmitting energy by the rotational force of the rotor.

[0172] In addition, the high-energy milling device can reduce the particle size of the mixed powder of the vanadium oxide and the carbon compound to the above range by rotating the rotating direction of the rotating container containing the mixed powder of the vanadium oxide and the carbon compound in the opposite direction to the rotating direction of the rotating axis of the rotating plate.

[0173] And, in the step of manufacturing low-oxygen vanadium carbide by performing a carbonization reduction reaction by vacuum heat treatment of the above (a-4) fine powder,

[0174] The above vacuum heat treatment

[0175] The heat treatment temperature can be from 800 ℃ to 1600 ℃,

[0176] Heat treatment times can range from 10 minutes to 24 hours.

[0177] Here, when the heat treatment temperature of the vacuum heat treatment is within the above range, the low-oxygen characteristics and manufacturing efficiency of the low-oxygen vanadium carbide can be excellent.

[0178] That is, the mixed powder of the vanadium oxide and the carbon compound produced by the high-energy milling device can be vacuum-heat treated at the heat treatment temperature of the vacuum heat treatment to produce low-oxygen vanadium carbide with excellent low-oxygen characteristics and manufacturing efficiency.

[0179] At this time, the heat treatment temperature of the vacuum heat treatment may preferably be 850°C to 1600°C, and more preferably 900°C to 1600°C.

[0180] And, when the heat treatment time of the vacuum heat treatment is within the above range, the low-oxygen characteristics and manufacturing efficiency of the low-oxygen vanadium carbide can be excellent.

[0181] That is, the mixed powder of the vanadium oxide and the carbon compound produced by the high-energy milling device is subjected to vacuum heat treatment during the heat treatment time of the vacuum heat treatment, thereby producing low-oxygen vanadium carbide having excellent low-oxygen characteristics and manufacturing efficiency.

[0182] At this time, the heat treatment time of the vacuum heat treatment may preferably be 20 minutes to 24 hours, and more preferably 30 minutes to 24 hours.

[0183]

[0184] Figure 2 is a process flow diagram of a method for manufacturing low-oxygen vanadium carbide according to one embodiment of the present invention.

[0185] Referring to Fig. 2, first, a mixed powder is prepared by mixing vanadium oxide and a carbon compound (S110).

[0186] Afterwards, the above mixed powder is fed into a rotating container in a high-energy milling device together with a steel ball (S120).

[0187] Then, high energy of 0.6 to 2.4 J / g·s is applied in an atmosphere of air, vacuum, nitrogen or argon, and the rotating shaft and the rotating container are rotated in different directions to perform high-energy milling to produce a fine powder (S130).

[0188] Afterwards, the above fine powder is vacuum heat-treated to undergo a carbonization-reduction reaction to produce low-oxygen vanadium carbide (S140).

[0189]

[0190] Figure 3 is a schematic diagram of a rotating plate of a high-energy milling device according to one embodiment of the present invention.

[0191] Referring to FIG. 3, the rotational direction of the main axis of the rotary plate of the high-energy milling device and the rotational direction of the rotary container containing the mixed powder of the vanadium oxide and the carbon compound are opposite to each other, and the particle size of the mixed powder of the vanadium oxide and the carbon compound can be reduced to 2 nm to 50 ㎛ by the rotational force in the opposite directions.

[0192]

[0193] Uses of low-oxygen vanadium carbide

[0194] The present invention provides a use for low-oxygen vanadium carbide formed by mixing vanadium oxide and a carbon compound, then refining the particle size through high-energy milling using a high-energy milling device, and then performing a vacuum heat treatment to undergo a carbonization-reduction reaction.

[0195] The present invention can provide a low-oxygen vanadium carbide, the use of which is a max precursor, a raw material for a superalloy material, a catalyst, or a semiconductor material.

[0196]

[0197] Low-oxygen vanadium carbide with particle size of 2 nm to 50 μm

[0198] The present invention provides low-oxygen vanadium carbide having a particle size of 2 nm to 50 μm, manufactured by the above method for manufacturing low-oxygen vanadium carbide.

[0199] The present invention can provide low-oxygen vanadium carbide having a particle size of 2 nm to 50 μm, manufactured by the above method for manufacturing low-oxygen vanadium carbide.

[0200] The present invention provides low-oxygen vanadium carbide having a particle size of 2 nm to 50 μm, manufactured by the method for manufacturing the low-oxygen vanadium carbide, so that the low-oxygen vanadium carbide has a low oxygen content, a small particle size, excellent physical properties, and can be used for various purposes such as a max precursor, a raw material for a superalloy material, a catalyst, or a semiconductor material.

[0201] The present invention can provide a low-oxygen vanadium carbide manufactured by the method for manufacturing the low-oxygen vanadium carbide, which is used as a max precursor, a raw material for a superalloy material, a catalyst, or a semiconductor material.

[0202] The present invention increases the reaction rate by reducing the particle size of a mixed powder of vanadium oxide and carbon compound as raw materials to 2 nm to 50 ㎛ through a high-energy milling process, thereby producing a low-oxygen vanadium carbide having a particle size of 2 nm to 50 ㎛ and a low oxygen content.

[0203]

[0204] Low-oxygen vanadium carbide having a chemical formula of VCx, wherein x is in the range of 0.3 < x < 1

[0205] The present invention provides a low-oxygen vanadium carbide having the chemical formula of VCx manufactured by the above method for manufacturing the low-oxygen vanadium carbide, wherein the range of x is 0.3 < x < 1.

[0206] The present invention can provide a low-oxygen vanadium carbide having the chemical formula of VCx manufactured by the above method for manufacturing the low-oxygen vanadium carbide, wherein the range of x is 0.3 < x < 1.

[0207] The use of the low-oxygen vanadium carbide produced by the method for producing the low-oxygen vanadium carbide of the present invention can provide a low-oxygen vanadium carbide that is a max precursor, a raw material for a superalloy material, a catalyst, or a semiconductor material.

[0208] The present invention provides a low-oxygen vanadium carbide having the chemical formula of VCx manufactured by the method for manufacturing the low-oxygen vanadium carbide, wherein the range of x is 0.3 < x < 1, so that the low-oxygen vanadium carbide has a low oxygen content, a small particle size, excellent physical properties, and can be used for various purposes such as a max precursor, a raw material for a superalloy material, a catalyst, or a semiconductor material.

[0209] The present invention increases the reaction rate by reducing the particle size of a mixed powder of vanadium oxide and carbon compound as raw materials to 2 nm to 50 ㎛ through a high-energy milling process, thereby producing a low-oxygen vanadium carbide having a chemical formula of VCx and in which x is in the range of 0.3 < x < 1.

[0210]

[0211] Hereinafter, the present invention will be described in more detail through examples. However, the following examples are intended to further illustrate the present invention, and the scope of the present invention is not limited by these examples. Those skilled in the art may appropriately modify or alter the following examples within the scope of the present invention.

[0212]

[0213] <Example>

[0214] <Examples 1 to 7> Preparation of low-oxygen vanadium carbide

[0215] A mixed powder of vanadium oxide and carbon compound was prepared with the components and contents shown in Table 1 below.

[0216] Afterwards, the mixed powder was fed into a rotating container in a high-energy milling device as shown in Table 1 below together with the steel balls.

[0217] Then, in the high-energy milling device of Table 1 below, high energy of Table 1 below was applied in a gaseous condition of air, vacuum, nitrogen or argon when grinding particles, and the rotating shaft and the rotating container were rotated in different directions to perform high-energy milling to produce fine powder.

[0218] Afterwards, the above fine powder was subjected to vacuum heat treatment under the conditions shown in Table 1 below to undergo a carbonization-reduction reaction to produce low-oxygen vanadium carbide.

[0219]

[0220] <Comparative Example> Manufacture of vanadium carbide

[0221] Vanadium carbide of the comparative example was manufactured in the same manner as in Example 1, except that a high-energy milling device was used in Example 1.

[0222]

[0223] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Comparative Example Vanadium oxide (A) Vanadium pentoxide (V2O5) Vanadium pentoxide (V2O5) Vanadium pentoxide (V2O5) Vanadium pentoxide (V2O5) Vanadium pentoxide (V2O5) Vanadium pentoxide (V2O5) Vanadium pentoxide (V2O5) Vanadium pentoxide (V2O5) Carbon compound (B) Graphite Graphite Graphite Graphite Graphite Graphite Graphite Graphite Molar ratio of B / A 6.3 0 6.4 0 6.5 0 7.0 0 7.0 5 7.1 0 7.1 5 7.0 0 Average particle size of mixed powder 20 nm 20 nm 20 nm 20 nm 20 nm 20 nm 45 ㎛ High energy Milling devicePlanetary ball millPlanetary ball millPlanetary ball millPlanetary ball millPlanetary ball millPlanetary ball millHorizontal ball millEnergy (J / g·s)0.6 ~ 2.40.6 ~ 2.40.6 ~ 2.40.6 ~ 2.40.6 ~ 2.40.6 ~ 2.40.1 ~ 0.2Steel ball materialCemented carbideCemented carbideCemented carbideCemented carbideCemented carbideCemented carbideCemented carbideRotational speed of rotating shaft (rpm)250250250250250250250150Rotational speed of rotating vessel (rpm)500500500500500500500500150Particle crushing in high-energy milling deviceGate conditionAirAirAirAirAirAirVacuum heat treatment Temperature (℃) 1500 1500 1500 1500 1500 1500 1500 1500 Vacuum heat treatment time 3 hours 3 hours 3 hours 3 hours 3 hours 3 hours Oxygen content of low-oxygen vanadium carbide (ppm) 368 0 226 0 367 0 387 0 337 0 184 0 144 0 12000 Chemical formula of low-oxygen vanadium carbide (VCx) x = 0.52 x = 0.62 x = 0.64 x = 0.80 x = 0.81 x = 0.86 x = 0.90 x = 0.80 Average particle size of low-oxygen vanadium carbide 20 nm 20 nm 20 nm 20 nm 20 nm 20 nm 10 ㎛

[0224]

[0225] Referring to Table 1 above, the low-oxygen vanadium carbides of Examples 1 to 7 had oxygen contents of 1440 ppm to 3870 ppm, which was significantly lower than the oxygen content of 12,000 ppm of the vanadium carbide of the comparative example.

[0226] Therefore, the low-oxygen vanadium carbides of Examples 1 to 7 were found to contain less oxygen.

[0227] In addition, the average particle size of the low-oxygen vanadium carbide of Examples 1 to 7 was 20 nm, which was a very small average particle size compared to the average particle size of 10 μm of the vanadium carbide of the comparative example.

[0228] Accordingly, it was confirmed that the low-oxygen vanadium carbides of Examples 1 to 7 have a significantly lower oxygen content and a significantly smaller average particle size than the comparative examples.

[0229]

[0230] <Examples 8 to 13> Preparation of low-oxygen vanadium carbide

[0231] A mixed powder of vanadium oxide and carbon compound was prepared with the components and contents shown in Table 2 below.

[0232] Afterwards, the mixed powder was fed into a rotating container in a high-energy milling device as shown in Table 2 below together with the steel balls.

[0233] Then, in the high-energy milling device of Table 2 below, high energy of Table 2 below was applied in a gaseous condition of air, vacuum, nitrogen or argon when grinding particles, and the rotating shaft and the rotating container were rotated in different directions to perform high-energy milling to produce fine powder.

[0234] Afterwards, the above fine powder was subjected to vacuum heat treatment under the conditions shown in Table 2 below to undergo a carbonization-reduction reaction to produce low-oxygen vanadium carbide.

[0235]

[0236] Example 8 Example 9 Example 10 Example 11 Example 12 Example 13 Vanadium oxide (A) Vanadium pentoxide (V2O5) Sodium metavanadate (NaVO3) Vanadium pentoxide (V2O5) Vanadium trioxide (V2VO3) Vanadium oxychloride (VOCl3) Ammonium metavanadate (H4NVO3) Carbon compound (B) Carbon powder for coke coal industry Graphite Carbon powder for graphite industry Molar ratio of B / A 6.5 6.8 7.5 7.0 6.2 6.1 Average particle size of mixed powder 20 nm 2 nm 100 nm 50 nm 20 ㎛ 50 ㎛ High-energy milling device Planetary ball mill Planetary ball mill Specs Mill Planetary ball mill Attritor Planetary ball mill Energy (J / g·s) 0.6 ~ 2.4 0.6 ~ 2.4 0.6 ~ 2.40.6 ~ 2.40.6 ~ 2.40.6 ~ 2.4Steel ball materialSteelZirconiaZirconiaSteelTungstenTungstenRotational speed of rotating shaft (rpm)1000200015001500500500Rotational speed of rotating vessel (rpm)300025003500350020002000Particle crushing in high-energy milling deviceCondition of gasVacuumNitrogenNitrogenNitrogenArgonArgonVacuum heat treatment temperature (℃)13001000800110015001600Vacuum heat treatment time1 hour4 hours24 hours2 hours30 minutes10 minutes

[0237]

[0238] <Experimental Example>

[0239] <Experimental Example 1> TEM image of a vanadium oxide-graphite mixture refined by high-energy milling.

[0240] A TEM image of the vanadium oxide-graphite mixture refined by high-energy milling manufactured in Example 1 is shown in Fig. 4.

[0241]

[0242] Figure 4 is a TEM image of a vanadium oxide-graphite mixture refined by high-energy milling according to Example 1.

[0243] Referring to FIG. 4, the vanadium oxide-graphite mixture refined by high-energy milling according to Example 1 was confirmed to have a vanadium oxide nano-crystal grain size of about 20 nm and an amorphous carbon (derived from graphite) particle size of about 100 nm.

[0244]

[0245] Experimental Example 2

[0246] The crystal structure (XRD) graph of the low-oxygen vanadium carbide manufactured in Example 1 above is shown in Fig. 5.

[0247]

[0248] Figure 5 is a graph of the crystal structure of low-oxygen vanadium carbide according to Example 1.

[0249] Referring to FIG. 5, the crystal structure of the low-oxygen vanadium carbide according to Example 1 was confirmed to be low-oxygen vanadium carbide at all at 1500°C, with the oxygen content decreasing and the carbide content increasing as the vacuum heat treatment temperature increased from 1000°C to 1500°C.

[0250]

[0251] Although specific examples of the low-oxygen vanadium carbide and the method for producing the low-oxygen vanadium carbide according to the present invention have been described so far, it is obvious that various modifications are possible within the scope of the present invention.

[0252] Therefore, the scope of the present invention should not be limited to the described embodiments, but should be defined not only by the claims described below but also by equivalents of the claims.

[0253] That is, it should be understood that the above-described embodiments are exemplary in all respects and not restrictive, and the scope of the present invention is indicated by the claims to be described later rather than the detailed description, and all changes or modified forms derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.

[0254] The present invention can be used to produce vanadium carbide with a low oxygen content.

Claims

1. As a low-oxygen vanadium carbide, It comprises low-oxygen vanadium carbide whose particle size is refined by high-energy milling with reduced oxygen content and high energy input of 0.6 to 2.4 J / g·s. The above low-oxygen vanadium carbide is characterized in that it is formed by mixing vanadium oxide and a carbon compound, then refining the particle size through high-energy milling using a high-energy milling device, and then performing a vacuum heat treatment to undergo a carbonization-reduction reaction. Low-oxygen vanadium carbide.

2. In paragraph 1, The oxygen content is characterized by being 10 ppm to 10,000 ppm. Low-oxygen vanadium carbide.

3. In paragraph 1, The above low-oxygen vanadium carbide has the chemical formula VCx, The above range of x is characterized in that 0.3 < x < 1. Low-oxygen vanadium carbide.

4. In paragraph 1, The molar ratio (B / A) of the carbon compound (B) to the vanadium oxide (A) is characterized in that it is 6.1 to 7.

5. Low-oxygen vanadium carbide.

5. In paragraph 1, The particle size of the mixed powder of the vanadium oxide or the carbon compound is characterized in that it is 2 nm to 50 ㎛. Low-oxygen vanadium carbide.

6. In paragraph 1, The above vanadium oxide is characterized in that at least one selected from vanadium pentoxide (V2O5), sodium metavanadate (NaVO3), vanadium trioxide (V2VO3), vanadium oxychloride (VOCl3), and ammonium metavanadate (H4NVO3). Low-oxygen vanadium carbide.

7. In paragraph 1, The above carbon compound is characterized by at least one selected from industrial carbon powder, coke, coal, coal tar, activated carbon, graphite, natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, industrial diamond, and carbon fiber. Low-oxygen vanadium carbide.

8. In paragraph 1, The above high energy milling After mixing the above vanadium oxide and carbon compound, the mixed powder is fed into a rotating container in a high-energy milling device together with steel balls. In an atmosphere of air, vacuum, nitrogen or argon, high energy of 0.6 to 2.4 J / g·s is input, the rotating shaft rotates at 500 to 1500 rpm, and the rotating vessel rotates at 2000 to 3500 rpm in the direction opposite to the rotation direction of the rotating shaft, thereby performing high-energy milling for a short time of 10 to 100 minutes. Low-oxygen vanadium carbide.

9. In paragraph 1, The above high-energy milling device Characterized by a ball mill, specs mill, or attritor Low-oxygen vanadium carbide.

10. In paragraph 1, The above vacuum heat treatment The heat treatment temperature is 800 ℃ to 1600 ℃, The heat treatment time is characterized by being 10 minutes to 24 hours. Low-oxygen vanadium carbide.

11. In paragraph 1, The above carbon reduction reaction is The above vanadium oxide and carbon compound are refined by the high-energy milling, thereby increasing the contact area and increasing the carbon reduction reaction rate. Low-oxygen vanadium carbide.

12. A method for producing low-oxygen vanadium carbide, (a-1) A step of preparing a mixed powder by mixing vanadium oxide and a carbon compound; (a-2) A step of putting the above mixed powder together with a ball into a rotating container in a high-energy milling device; (a-3) A step of manufacturing a fine powder by applying high energy of 0.6 to 2.4 J / g·s in an atmosphere of air, vacuum, nitrogen or argon, and rotating the rotating shaft and the rotating container in different directions to perform high-energy milling; and (a-4) A step of manufacturing low-oxygen vanadium carbide by subjecting the above fine powder to a vacuum heat treatment and carbonization reduction reaction. Method for producing low-oxygen vanadium carbide.

13. In paragraph 12, In the step of manufacturing a mixed powder by mixing vanadium oxide and carbon compound (a-1), The mixing ratio of the vanadium oxide and the carbon compound is characterized in that it is 1:0.2 to 1:0.7 by weight. Method for producing low-oxygen vanadium carbide.

14. In paragraph 12, In the step of feeding the above (a-2) mixed powder together with the steel ball into the rotating container in the high-energy milling device, The above-mentioned ball is characterized by being at least one selected from among a ceramic ball, a metal ball, and a superalloy ball. Method for producing low-oxygen vanadium carbide.

15. In paragraph 12, In the step of manufacturing fine powder by high energy milling by applying high energy of 0.6 to 2.4 J / g·s in an atmosphere of air, vacuum, nitrogen or argon (a-3) and rotating the rotating shaft and the rotating container in different directions, The above-mentioned rotary shaft rotates at 500 to 1500 rpm, and the rotary container rotates at 2000 to 3500 rpm in the opposite direction to the rotation direction of the rotary shaft, so that high-energy milling is performed for a short time of 10 to 100 minutes. Method for producing low-oxygen vanadium carbide.

16. In paragraph 12, In the step of manufacturing low-oxygen vanadium carbide by performing a carbonization reduction reaction by vacuum heat treatment of the above (a-4) fine powder, The above vacuum heat treatment The heat treatment temperature is 800 ℃ to 1600 ℃, The heat treatment time is characterized by being 10 minutes to 24 hours. Method for producing low-oxygen vanadium carbide.

17. Low-oxygen vanadium carbide according to any one of claims 1 to 11, which is used as a max precursor, a raw material for cemented alloy materials, a catalyst, or a semiconductor material.

18. Low-oxygen vanadium carbide having a particle size of 2 nm to 50 μm, manufactured by a method for manufacturing low-oxygen vanadium carbide according to any one of claims 12 to 16.

19. A low-oxygen vanadium carbide having the chemical formula VCx, manufactured by a method for manufacturing a low-oxygen vanadium carbide according to any one of claims 12 to 16, wherein the range of x is 0.3 < x < 1.

20. The use of the low-oxygen vanadium carbide manufactured by the method for manufacturing low-oxygen vanadium carbide according to any one of claims 12 to 16 is as a low-oxygen vanadium carbide as a max precursor, a raw material for a superalloy material, a catalyst, or a semiconductor material.

Citation Information

Patent Citations

  • The preparing method of alloy / metal powder dispersed with nano ceramic using the high-speed milling machine and the resultant alloy / metal powder dispersed with nano ceramic

    KR1020110010987A

  • Low-oxygen vanadium carbide and method for manufacturing the same

    KR102611243B1

  • Sinterable carbides from oxides using high energy milling

    US6214309B1