Improved formation electrolyte for tantalum solid electrolyte capacitors
The introduction of inositol derivatives in the electrolyte for forming tantalum oxide dielectric in solid electrolytic capacitors addresses the issue of anomalous charge current, enhancing capacitor performance by stabilizing the dielectric interface and reducing ACC.
Patent Information
- Application Number
- PCT/US2024/018805
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-03
AI Technical Summary
Solid electrolytic capacitors using tantalum anodes and conductive polymer cathodes suffer from anomalous charge current (ACC), which interferes with circuit performance and leads to faulty capacitors due to poor dielectric quality.
An improved formation electrolyte comprising derivatives of inositol is used to form a stable tantalum oxide dielectric on the anode, which reduces ACC by anchoring ions to the tantalum surface and forming a uniform oxide layer, thereby stabilizing the interface between the dielectric and conductive polymer.
The use of inositol derivatives in the electrolyte significantly improves the electrical properties of solid electrolytic capacitors, reducing anomalous charge current and enhancing capacitor performance by forming a stable dielectric interface.
Smart Images

Figure US2024018805_03102024_PF_FP_ABST
Abstract
Description
IMPROVED FORMATION ELECTROLYTE FOR TANTALUM SOLID ELECTROLYTE CAPACITORS FIELD OF THE INVENTION
[0001] The present invention is related to an improved formation(anodization), electrolyte for the formation of tantalum oxide dielectric on a tantalum anode body. More specifically, the present invention is specific to a formation electrolyte comprising compounds derived from inositol which significantly improves oxide formation. BACKGROUND
[0002] Solid electrolytic capacitors comprising oxide formed on sintered tantalum as the anode and conductive polymer as the cathode are now utilized extensively throughout the electronics industry in virtually every application necessitating a capacitive couple in the electronic assembly. As would be fully understood by those of skill in the art, tantalum oxide is formed on the tantalum surface wherein the tantalum oxide functions as the dielectric between the tantalum anode and conductive polymer cathode. The process of forming tantalum oxide by subjecting the anode to voltage in the presence of an electrolyte is referred to as anodization.
[0003] Dielectric quality is a measure of electrical property of a solid electrolytic capacitor. Poor dielectric may cause failure of the part. One factor that contributes to faulty electrical properties is anomalous charge current (ACC). Parts formed in currently available anodization electrolytes exhibit high ACC wherein the high ACC is now known to be detrimental to electrolytic capacitor quality. This has led to a significant effort todevelop an improved forming, or anodizing electrolytewhich provides a more stable dielectric resulting in an improved solid electrolytic capacitor, particularly with a lower ACC.
[0004] Solid electrolytic capacitors using valve metal as anodes, specifically tantalum, and conductive polymer as cathode, display anomalous charge current (ACC) which exceeds the theoretical value {I(t)) calculated as: I(t)=C*dv / dt with C being the capacitance and dV / dt being the voltage ramp}. ACC might interfere with circuit performance thereby leading to faulty capacitors as described in Y. Freeman and P. Lessner Evolution of Polymer Tantalum Capacitors Appl. Sci.2021, 11(12), 5514-5521.
[0005] Provided herein is an improved electrolyte which is particularly suitable for use in the formation of tantalum oxide on tantalum wherein the tantalum oxide functions as an improved dielectric in a solid electrolytic capacitor. SUMMARY OF THE INVENTION
[0006] The present invention is related to an improved formation electrolyte which is particularly suitable for use in the formation of tantalum oxide on tantalum.
[0007] More specifically, the present invention is related to a capacitor with improved electrical properties, comprising a tantalum anode and conductive polymer cathode with an improved tantalum oxide dielectric there between.
[0008] A particular feature of the present invention is the ability to form a dielectric oxide on a tantalum anode without alteration of the manufacturing steps, equipment or procedures.
[0009] These and other advantages, as will be realized, are provided in a formation electrolyte suitable for formation of an oxide on a valve metal anode comprising a derivative of inositol is defined by Formula 1:Formula 1 wherein: each of R1^R6is independently selected from H, substituted or unsubstituted carbon chain of up to 20 carbon atoms, ^PO3R7R8; ^SiR93,^C(O)R10; and ; or adjacent groups may be^P(O)OH^O^P(O)OH^; each R7and R8are independently selected from H, a cation; saturated or unsaturated carbon chain of up 35 carbon atoms; or ^CH2CHR12CH2R13each R9is independently an alkyl of 1 to 10 carbon atoms; each R10is independently an alkyl of 1 to 10 carbon atoms; each R11represents a bond to an oxygen of the derivative of inositol of Formula 1; and R12and R13are esters terminated with H, saturated or unsaturated carbon chain of 1 to 35 carbon atoms
[0010] Yet another embodiment is provided in a method of forming a solid electrolytic capacitor comprising: forming a dielectric oxide on a tantalum anode by: applying a formation electrolyte on said anode wherein said formation electrolyte comprises a derivative of inositol is defined by Formula 1:wherein: each of R1^R6is independently selected from H, substituted or unsubstituted carbon chain of up to 20 carbon atoms, ^PO3R7R8; ^SiR93, ^C(O)R10; and or adjacent groups may be^P(O)OH^O^P(O)OH^; each R7and R8are independently selected from H, a cation; saturated or unsaturated carbon chain of up 35 carbon atoms; or ^CH2CHR12CH2R13; each R9is independently an alkyl of 1 to 10 carbon atoms; each R10is independently an alkyl of 1 to 10 carbon atoms;each R11represents a bond to an oxygen of the derivative of inositol of Formula 1; and R12and R13are esters terminated with H, saturated or unsaturated carbon chain of 1 to 35 carbon atoms; and forming a conductive polymer cathode on said dielectric oxide. DESCRIPTION
[0011] The present invention is related to improved solid electrolytic capacitor comprising an improved tantalum oxide dielectric wherein the properties of the solid electrolytic capacitor, and particularly ACC, are significantly improved relative to the art. More specifically, the present invention is related to an improved formation electrolyte suitable for use in the formation of an improved tantalum oxide on a tantalum anode that yields low wet leakage. The capacitor formed with the improved tantalum oxide provides an improved solid electrolytic capacitor, particularly, when used with solid conductive polymer cathodes.
[0012] High ACC in solid electrolytic capacitors is solved by formation of tantalum oxide on a tantalum anode in an electrolyte that comprises derivatives of inositol. Without being limited to theory, it is hypothesized that the derivatives of inositol are capable of bonding with the free hydroxyl groups present on the surface of tantalum or with tantalum oxide thereby stabilizing the interface of the growing dielectric and anode which facilitates improved tantalum oxide growth.
[0013] The present invention is related to improved electrical properties in solid electrolytic capacitors and more specifically anomalous charge current (ACC). This invention provides a method of forming a dielectric oxide film on a tantalum anode and of making a solid electrolytic capacitor therewith. Formation in theinventive forming electrolyte, having free terminal O^ion upon ionization, in aqueous solution, forms an improved dielectric oxide layer. Without being limited to theory, it is hypothesized that the geometry of the ions of the inventive forming electrolyte anchor to the tantalum surface, which has free hydroxyl groups. The bonding / anchoring of the ions, facilitates more electrolyte molecule access and in effect forms uniform oxide. Another hypothesis is that a portion of the inventive forming electrolyte remains on the surface of the tantalum oxide and forms a stable interface between dielectric and conductive polymer at the p-n junction. This assists in possible tunneling and significantly reduces anomalous charge current (ACC) in solid electrolytic capacitors.
[0014] Forming a stable dielectric interface is crucial for having stable electrical properties. The dielectric is formed by anodically oxidizing the metal anode in the electrolyte that contains the inventive forming electrolyte. Through selective control over a voltage range, the anodization process leads to a dielectric having better electrical properties which in turn leads to a capacitor having improved ACC exhibiting less anomalous charge current when charged at a constant voltage slew rate such as 100 volts / second.
[0015] The derivative of inositol is defined by Formula 1wherein:each of R1^R6is independently selected from H, substituted or unsubstituted carbon chain of up to 20 carbon atoms, ^PO3R7R8, ^SiR93, C(O)R10; andor adjacent groups may be taken together to represent ^P(O)OH^O^P(O)OH^; each R7and R8are independently selected from H, a cation; saturated or unsaturated carbon chain of up 35 carbon atoms; or ^CH2CHR12CH2R13each R9is independently an alkyl of 1 to 10 carbon atoms and preferably 1 to 3 carbon atoms with ^CH3being particularly preferred; each R10is independently an alkyl of 1 to 10 carbon atoms and preferably 1 to 3 carbon atoms with ^CH3being particularly preferred; Each R11represents a bond to an oxygen of the derivative of inositol of Formula 1; and R12and R13are esters terminated with H, saturated or unsaturated carbon chain of 1 to 35 carbon atoms.
[0016] In a preferred embodiment at least one of R1^R6is PO3R7R8with at least one of R7or R8being H and preferably R7and R8are both H. In a more preferred embodiment at least two of R1^R6is ^PO3R7R8with at least one of R7or R8being H and preferably R7or R8are both ^H. In a more preferred embodiment at least three of R1R6is PO3R7R8with at least one of R7or R8being H and preferably R7and R8are both H. In a more preferred embodiment at least four of R1^R6is PO3R7R8with at least one of R7or R8being ^H and preferably R7and R8are both H. In a more preferred embodiment at least five of R1-R6is PO3R7R8with at least one ofR7or R8being H and preferably R7and R8are both H. In a more preferred embodiment each of R1-R6 is PO3R7R8with at least one of R7or R8being ^H and preferably R7and R8are both H.
[0017] R7and R8can be a cation preferably selected from quaternary amines, ammonium; metal cation, saturated or unsaturated carbon chain of up 35 carbon atoms, preferably 10-17 carbon atoms.
[0018] Substituted or unsubstituted carbon chains include alkyl chains and alkene chains which are straight chains, branched chains or cyclic which may be substituted or unsubstituted. Substitutions include ethers, ^OH, carboxylic acids, phosphonic acids, phosphinic acids, esters, amines and amides.
[0019] Particularly preferred derivatives of inositol are selected from the group consisting of myo-inoViWol and iW¶V iVomeUV and their respective derivatives namely myo-inositol hexakis- phosphate (phytic acid); pentakis-, tri-, di-phosphates and their isomers; and myo-inositol mono phosphate, myo-inositol trispyrophosphate, 1- phosphatidyl-myo-inositol , 1-phosphatidyl-myo-inositol 3-phosphate, derivatives of ononitol, sequoytol, dombonitol, viscumitol, pinitol, quebrachitol, pinpollitol and brahol, myo-inositol 1,3,4,5,6-pentakis-O-(trimethylsilyl)-, bis(trimethylsilyl) phosphate, phosphatidylinositol 5-phosphate PI(5) diC8 ammonium salt, phosphatidylinositol 5-phosphate diC16 (PI(5)P diC16) sodium salt, 1,2 -ciacyl-sn- glycero-3-phospho-(1-D-myo-inositol 4,5^biphosphate), phosphatidylinositol, phosphatidylinositol 3-phosphate, phosphatidylinositol 4-phosphate, phosphatidylinositol 4,5^phosphate, di-myo-inositol-phosphate, ciceritol phosphate, fagopyritol phosphate, glycosylinositol phosphryl ceramide, C25,25- Archeditylinositol, ceramide phosphoinositol, D-myo-inositol-4-hydrogen phosphate monoammonium salt and phosphatidylinositol phosphate.
[0020] The formation electrolyte may further comprise additives selected from metal salts, salts of organic acids, salts of inorganic acids, organic acids, inorganic acids, organometallic compounds, inorganic solvents, organic solvents, crosslinking agents, surface active agents, buffers and the like.
[0021] The metal salts, salts of inorganic acids and salts of organic acids included in the formation electrolyte may comprise halides, nitrides, sulfides, amides, nitrates, sulfates, phosphates, carbonates, chromates, chlorates, perchlorates, oxides, oxychlorides, peroxides, carboxylates, amides and esters.
[0022] The organic and inorganic acids included in the formation electrolyte may comprise carboxylic acids, phosphonic acids, phosphinic acids, pyrophosphoric acids, phosphoric acid, phthalic acid, maleic acid, malonic acid and trimesic acid and the like.
[0023] The organometallic compounds included in the formation electrolyte may comprise organosilanes, organoboranes, carbonyls, phosphines, crosslinking agents, surface active agents and buffers.
[0024] The solvent included in the formation electrolyte may be selected from the group consisting of water, alcohol, ethylene glycol, polyethylene glycol, tetraglyme, propylene glycol, glycol ether and alkanolamines.
[0025] The solid electrolytic capacitor comprises an anode, a cathode and a dielectric oxide between the anode and cathode. The anode is a sintered porous tantalum metal which is anodized to form the dielectric oxide. The dielectric oxide layer is covered by solid electrolyte, which is preferably a conductive polymer, which acts as cathode. The dielectric oxide is formed by subjecting the anode to voltage, in the presence of an inventive forming electrolyte in a process referred to in the art as anodization.
[0026] The solid electrolytic capacitor comprises an anode, a cathode and a dielectric oxide between the anode and cathode. The anode is a sintered porous tantalum metal which is anodized to form the dielectric oxide. The dielectric oxide layer is covered by solid electrolyte, which is preferably a conductive polymer, which acts as cathode. The dielectric oxide is formed by subjecting the anode to voltage, in the presence of an inventive forming electrolyte in a process referred to in the art as anodization.
[0027] After formation (anodization) of the anode, with a dielectric thereon can be washed. In one embodiment the anode, with a dielectric thereon is not washed which allows residual formation electrolyte to remain anchored to the surface which facilitates bonding with the cathode layer.
[0028] Formation temperatures of about 60-125oC are suitable for demonstration of the invention. More preferably an anodization temperature of about 75-90oC is suitable for demonstration of the invention.
[0029] The anomalous charging current (ACC) refers to the ideal current (I ideal) in milliamps (mA) for charging a capacitor Iideal= 1000*C(dv / dt), C is the capacitance in Farads and dv / dt is the instantaneous rate of voltage change which is typically about 100V / S. Thus, the actual charging current remains the same or is greater than the ideal charging current (Iideal). Iactual / Iideal=1 or greater than 1.
[0030] The structure of a solid electrolytic capacitor is well understood by those of skill in the art and further elaboration is not necessary herein.
[0031] The conductive polymer is preferably selected from a group consisting of polyanilines, polypyrroles and polythiophenes each of which may be substituted. A particularly preferred polymer comprises conjugated groups having the structure of Formula 2:R1R2nwherein: R1and R2independently represent linear or branched C1C16 alkyl or C2C18 alkoxyalkyl; or are C3^C8cycloalkyl, phenyl or benzyl which are unsubstituted or substituted by C1C6 alkyl, C1^C6 alkoxy, halogen or OR3; or R1and R2, taken together, are linear C1^C6alkylene which is unsubstituted or substituted by C1^C6alkyl, C1^C6alkoxy, halogen, C3^C8cycloalkyl, phenyl, benzyl, C1^C4alkylphenyl, C1-C4 alkoxyphenyl, halophenyl, C1^C4 alkylbenzyl, C^^C4 alkoxybenzyl or halobenzyl, 5-, 6-, or 7- membered heterocyclic structure containing two oxygen elements. R3preferably represents hydrogen, linear or branched C1^C16 alkyl or C2^C18alkoxyalkyl; or are C3^C8cycloalkyl, phenyl or benzyl which are unsubstituted or substituted by C1^C6 alkyl; X is S, N or O and most preferable X is S; R1and R2of Formula 2 are preferably chosen to prohibit polymerization aW Whe ȕ^site of the ring as iW iV moVW pUefeUUed WhaW onl\ Į-site polymerization be allowed to proceed; it is more preferred that R1and R2are not hydrogen and more preferably, R1and R2aUe Į-directors with ether linkages being preferable over alkyl linkages; it is most preferred that the R1and R2are small to avoid steric interferences.
[0032] In a particularly preferred embodiment the R1and R2of Formula 1 are taken together to represent ^O-(CHR4)n-O^ wherein:n is an integer from 1 to 5 and most preferably 2; R4is independently selected from hydrogen; a linear or branched C1 to C18 alkyl radical C5to C12cycloalkyl radical, C6to C14aryl radical C7to C18aralkyl radical or C1to C4hydroxyalkyl radical, optionally substituted with a functional group selected from carboxylic acid, hydroxyl, amine, substituted amines, alkene, acrylate, thiol, alkyne, azide, sulfate, sulfonate, sulfonic acid, imide, amide, epoxy, anhydride, silane, and phosphate; hydroxyl radical; or R4is selected from ^(CHR5)a-R16; ^O(CHR5)aR16; ^CH2O(CHR5)aR16;±CH2O(CH2CHR5O)aR16, or R4is a functional group selected from the group consisting of hydroxyl, carboxyl, amine, epoxy, amide, imide, anhydride, hydroxymethyl, alkene, thiol, alkyne, azide, sulfonic acid, benzene sulfonic sulfonate, SO3M, anhydride, silane, acrylate and phosphate; R5is H or alkyl chain of 1 to 5 carbon atoms optionally substituted with a functional group selected from carboxylic acid, hydroxyl, amine, alkene, thiol, alkyne, azide, epoxy, acrylate and anhydride; R16is H or SO3M or an alkyl chain of 1 to 5 carbon atoms optionally substituted with a functional group selected from carboxylic acid, hydroxyl, amine, substituted amines, alkene, thiol, alkyne, azide, amide, imide, sulfate, SO3M, amide, epoxy, anhydride, silane, acrylate and phosphate; a is integer from 0 to 10; and M is a H or cation preferably selected from ammonia, sodium or potassium.
[0033] The conducting polymer can be either a water-soluble or water- diVpeUVible compoXnd. E[ampleV of VXch a ʌ conjXgaWed condXcWiYe pol\meU inclXde polypyrrole or polythiophene. Particularly preferred conductive polymers include poly(3,4-ethylenedioxythiophene), poly(4-(2,3-dihydrothieno-[3,4-b][1,4]dioxin-2-yl)methoxy)-1-butane-sulphonic acid, salt), poly(4-(2,3-dihydrothieno-[3,4- b][1,4]dioxin-2-yl)methoxy)-1-propane-sulphonic acid, salt), poly(4-(2,3- dihydrothieno-[3,4-b][1,4]dioxin-2-yl)methoxy)-1-methyl-1-propane-sulphonic acid, salt), poly(4-(2,3-dihydrothieno-[3,4-b][1,4]dioxin-2-yl)methoxy alcohol, poly(N- methylpyrrole), poly(3-methylpyrrole), poly(3-octylpyrrole), poly(3-decylpyrrole), poly(3-dodecylpyrrole), poly(3,4-dimethylpyrrole), poly(3,4-dibutylpyrrole), poly(3- carboxypyrrole), poly(3-methyl-4-carboxypyrrole), poly(3-methyl-4- carboxyethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), poly(3-hydroxypyrrole), poly(3-methoxypyrrole), polythiophene, poly(3-methylthiophene), poly(3- hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3- decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3- bromothiophene), poly(3,4-dimethylthiophene), poly(3,4-dibutylthiophene), poly(3- hydroxythiophene), poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3- butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3- octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), poly(3- octadecyloxythiophene), poly(3,4-dihydroxythiophene), poly(3,4- dimethoxythiophene), poly(3,4-ethylenedioxythiophene), poly(3,4- propylenedioxythiophene), poly(3,4-butenedioxythiophene), poly(3- carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4- carboxyethylthiophene), poly(3-methyl-4-carboxybutylthiophene), polyaniline, poly(2- methylaniline), poly(3-isobutylaniline), poly(2-aniline sulfonate), poly(3-aniline sulfonate), and the like.
[0034] Co-polymers composed at least two different copolymerized monomers are contemplated. Co-polymers comprise at least one polymerized monomer selected from the group consisting of polypyrrole, polythiophene, poly(4-(2,3-dihydrothieno-[3,4-b][1,4]dioxin-2-yl)methoxy)-1-butane-sulphonic acid, salt), poly(4-(2,3-dihydrothieno-[3,4-b][1,4]dioxin-2-yl)methoxy)-1-methyl-1-propane- sulphonic acid, salt), poly(N-methylpyrrole), poly(3-methylthiophene), poly(3- methoxythiophene), and poly(3,4-ethylenedioxythiophene).
[0035] A particularly preferred conductive polymer is poly-3,4-polyethylene dioxythiophene (PEDOT).
[0036] The conductive polymer layer can be formed on the dielectric by any technique commonly employed in the art. The conductive polymer can be formed into a slurry and deposited onto the surface. Alternatively, the conductive polymer can be added as monomer and polymerized in-situ as well known in the art.
[0037] It is known in the art to additional layers to the cathode to facilitate soldering of the cathode to a lead frame or circuitry. Carbon containing layers and metal containing layers are well known and well documented in the art and further discussion is not warranted herein.
[0038] Organofunctional silanes and organic compounds with more than one crosslinking group, especially more than one epoxy group, are particularly suitable for use in combination with the inventive formation electrolyte. The formation electrolyte may include the organofunctional silanes and organic compounds with more than one crosslinking group as additive in combination with inositol derivative. After formation of the dielectric oxide the anode with dielectric thereon can be washed. In an embodiment the anode with dielectric thereon is not washed which allows residual organofunctional silanes and organic compounds with more than one crosslinking group together with inositol derivative to be present during formation of the cathode.
[0039] An exemplary organofunctional silane is defined by the formula: XR1Si(R3)3-n(R2)n wherein X is an organic functional group such as amino, epoxy, anhydride, hydroxy, mercapto, sulfonate, carboxylate, phosphonate, halogen, vinyl, methacryloxy, ester, alkyl etc; R1 is an aryl or alkyl (CH2)m wherein m can be 0 to 14; R2 is individually a hydrolysable functional group such as alkoxy, acyloxy, halogen, amine or their hydrolyzed product; R3is individually an alkyl functional group of 1-6 carbon atoms; n is 1 to 3.
[0040] The organofunctional silane can also be dipodal, define by the formula: Y(Si(R3)3-n(R2)n)2 wherein Y is any organic moiety that contains reactive or nonreactive functional groups, such as alkyl, aryl, sulfide or melamine; R3, R2 and n are defined above. The organofunctional silane can also be multi-functional or polymeric silanes, such as silane modified polybutadiene, or silane modified polyamine, etc.
[0041] Examples of organofunctional silane include 3^glycidoxypropyltrimethoxysilane, 3-aminopropytriethoxysilane, aminopropylsilanetriol, (triethoxysilyl)propylsuccinic anhydride, 3- mercaptopropyltrimethoxysilane, vinyltrimethoxysilane, 3- methacryloxypropyltrimethoxysilane, 3-trihydroxysilyl-1-propane sulfonic acid, octyltriethyoxysilane, bis(triethoxysilyl)octane, etc. The examples are used to illustrate the invention and should not be regarded as conclusiveExamples of organofunctional silane include 3-glycidoxypropyltrimethoxysilane, 3- aminopropytriethoxysilane, aminopropylsilanetriol, (triethoxysilyl)propylsuccinic anhydride, 3-mercaptopropyltrimethoxysilane, vinyltrimethoxysilane, 3- methacryloxypropyltrimethoxysilane, 3-trihydroxysilyl-1-propane sulfonic acid,octyltriethyoxysilane, bis(triethoxysilyl)octane, etc. The examples are used to illustrate the invention and should not be regarded as conclusive.
[0042] A particularly preferred organofunctional silane is glycidyl silane defined by the formula:wherein R1 is an alkyl of 1 to 14 carbon atoms and more preferably selected from methyl ethyl and propyl; and each R2 is independently an alkyl or substituted alkyl of 1 to 6 carbon atoms.
[0043] A particularly preferred glycidyl silane is 3- glycidoxypropyltrimethoxysilane defined by the formula:Zhich iV UefeUUed Wo heUein aV ³Silane A´ foU conYenience.
[0044] A particularly suitable organometallic is neoalkoxy titanate with titanium IV 2,2(bis 2-propenolatomethyl)butanolato, tris neodecanoato-O; titanium IV 2,2(bis 2-propenolatomethyl)butanolato, iris(dodecyl)benzenesulfonato-O; titanium IV 2,2(bis 2-propenolatomethyl)butanolato, tris(dioctyl)phosphato-O; titanium IV 2,2(bis 2-propenolatomethyl)tris(dioctyl)pyrophosphatobutanolato-O;titanium IV 2,2(bis 2- propenolatomethyl)butanolato, tris(2-ethylenediamino)ethylato; and titanium IV 2,2(bis 2-propenolatomethyl)butanolato, tris(3-amino)phenylato being representative neoalkoxy titanates and derivatives thereof.
[0045] A crosslinker with at least two epoxy groups is referred to herein as an epoxy crosslinking compound and is defined by the formula:wherein the X is an alkyl or substituted alkyl of 0-14 carbon atoms, preferably 0-6 carbon atoms; an aryl or substituted aryl, an ethylene ether or substituted ethylene ether, polyethylene ether or substituted polyethylene ether with 2-20 ethylene ether groups or combinations thereof. A particularly preferred substitute is an epoxy group.
[0046] Examples of epoxy crosslinking compounds having more than one epoxy groups include ethylene glycol diglycidyl ether (EGDGE), propylene glycol diglycidyl ether (PGDGE), 1,4-butanediol diglycidyl ether (BDDGE), pentylene glycol diglycidyl ether, hexylene glycol diglycidyl ether, cyclohexane dimethanol diglycidyl ether, resorcinol glycidyl ether, glycerol diglycidyl ether (GDGE), glycerol polyglycidyl ethers, diglycerol polyglycidyl ethers, trimethylolpropane polyglycidyl ethers, sorbitol diglycidyl ether (Sorbitol-DGE), sorbitol polyglycidyl ethers, polyethylene glycol diglycidyl ether (PEGDGE), polypropylene glycol diglycidyl ether, polytetramethylene glycol diglycidyl ether, di(2,3-epoxypropyl)ether, 1,3-butadiene diepoxide, 1,5- hexadiene diepoxide, 1,2,7,8-diepoxyoctane, 1,2,5,6-diepoxycyclooctane, 4-vinyl cyclohexene diepoxide, bisphenol A diglycidyl ether, maleimide-epoxy compounds, etc. EXAMPLES
[0047] Wet capacitance and leakage are measured by an LCR meter in 25wt% Phosphoric acid in water under a test frequency of 120Hz and test voltage of 70% of formation voltage. For wet leakage, the parts have been tested after a charge time of 120 seconds and DC bias voltage of 2V. ACC (anomalous charging current) is measured at the end of the production process. The finished parts are mounted on a circuit board and measurement is done at 0oC and 80%Vr and expressed as times theoretical value (xTLV).
[0048] Comparative Example: Tantalum anodes (330 microfarads, 16V rated voltage) are prepared by sintering of tantalum powder. First, the anodes are anodized in an electrolyte that works as a control {phosphoric acid about (2-5wt%), ethylene glycol (50-70wt%) and water having resistivity of about (100-370) ohm-cm measured at 80oC} at 35V and 80oC to form a dielectric oxide on the tantalum anode (1stanodization). The anodes are rinsed, heat-treated at 450oC for 30 minutes and re-anodized in the original electrolytes. Wet leakage after 1stanodization is given in Table 1. The anodes are then covered in conductive polymer that served as cathode, followed by carbon and silver coatings. Parts get assembled and molded into surface mount finished capacitors using known techniques. ACC is measured at 0oC on mount parts and reported as current in mA at 12.8V {80% of the rated voltage (Vr)}. Cap and ESR (equivalent series resistance) of the finished part are also reported along with ACC in Table 1.
[0049] Inventive Example 1: A series of solid electrolytic capacitors have been prepared in a similar manner to that in comparative example 1 using 300 microfarad parts with rated voltage 16V except that the electrolyte is (5-10wt%) inositol-6-phosphate in water having resistivity (7-15) ohm-cm at 80oC. Wet leakageafter 1stanodization, cap and ESR of finished part are also reported along with ACC as current (mA) at 12.8V (80% of Vr) are given in Table 1.
[0050] Inventive Example 2: A series of solid electrolytic capacitors are prepared in similar manner to that in inventive example 1 using 300 microfarad parts with rated voltage 16V except that the anodization electrolyte is a mixture of (5- 10wt%) inositol-6-phosphate and epoxy silane (1:1) in water having resistivity (9-17) ohm-cm at 80oC. Wet leakage after 1stanodization, cap and ESR of finished part are also reported along with ACC as current (mA) at 12.8V (80% of Vr) are given in Table 1.
[0051] Inventive Example 3: In this example, a series of solid electrolytic capacitors are prepared in similar manner to that in inventive example 1 using 300 microfarad parts with rated voltage 16V except that the electrolyte has ethylene glycol (EG) added to it. Inositol-6-phosphate (5-10wt%) is added to ethylene glycol (50-70wt%) in water having resistivity (75-100) ohm-cm at 80oC. Wet leakage after 1stanodization, cap and ESR of finished part are also reported along with ACC as current (mA) at 12.8V (80% of Vr) are given in Table 1.
[0052] Inventive Example 4: In this example, a series of solid electrolytic capacitors are prepared in similar manner using 300 microfarad parts with rated voltage 16V to that in inventive example 2 except that the polymer also has the same electrolyte used in inventive example 2 along with conductive polymer. Wet leakage after 1stanodization, cap and ESR of finished part are also reported along with ACC as current (mA) at 12.8V (80% of Vr) are given in Table 1.
[0053] Inventive Example 5: In this example, a series of solid electrolytic capacitors using 300 microfarad parts with rated voltage 16V are prepared in similar manner to that in inventive example 1 except that the electrolyte has inositol (1-6wt%) and phosphoric acid (1-6wt%) in water having resistivity of about (10-30) ohm-cm. Wet leakage after 1stanodization, cap and ESR of finished part are also reported along with ACC as current (mA) at 12.8V (80% of Vr) are given in Table 1. Table 1 Wet leakage Capacitance Equivalent Series Current(mA) at Example (nano resistance compliance
[0054] The inventive examples demonstrated the ability to form a capacitor, using the inventive formation electrolyte, having an anomalous charge current less than 4 times the theoretical value. This is otherwise not available in the art.
[0055] The invention has been described with reference to preferred embodiments without limit thereto. One of skill in the art would realize additional embodiments which are described and set forth in the claims appended hereto.
Claims
Claimed is 1. A formation electrolyte suitable for formation of an oxide on a valve metal anode comprising a derivative of inositol is defined by Formula 1:wherein: each of R1^R6is independently selected from H, substituted or unsubstituted carbon chain of up to 20 carbon atoms, ^PO3R7R8; ^SiR93,^C(O)R10; and ; or adjacent groups mayrepresent ^P(O)OH^O^P(O)OH^; each R7and R8are independently selected from H, a cation; saturated or unsaturated carbon chain of up 35 carbon atoms; or ^CH2CHR12CH2R13each R9is independently an alkyl of 1 to 10 carbon atoms;each R10is independently an alkyl of 1 to 10 carbon atoms; each R11represents a bond to an oxygen of the derivative of inositol of Formula 1; and R12and R13are esters terminated with H, saturated or unsaturated carbon chain of 1 to 35 carbon atoms.
2. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 1 wherein at least one of R1^R6is ^PO3R7R8with at least one of R7or R8being ^H.
3. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 2 wherein R7and R8are both ^H.
4. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 2 wherein at least two of R1^R6is ^PO3R7R8.
5. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 4 wherein at least three of R1^R6is ^PO3R7R8.
6. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 5 wherein at least four of R1^R6is ^PO3R7R8.
7. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 6 wherein at least five of R1^R6is ^PO3R7R8.
8. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 7 wherein each of R1^R6is ^PO3R7R8.
9. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 8 with each R7and R8is ^H.
10. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 1 wherein at least one R7or R8is a cation.
11. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 10 wherein said cation is selected from the group consisting of quaternary amines and saturated or unsaturated carbon chain of up 35 carbon atoms.
12. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 1 wherein each R9is independently an alkyl of 1 to 3 carbon atoms.
13. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 12 wherein each R9is ^CH3.
14. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 1 wherein each R10is independently an alkyl of 1 to 3 carbon atoms.
15. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 14 wherein each R10is ^CH3.
16. The formation electrolyte suitable for formation of an oxide on a tantalum anode of claim 1 wherein said derivative of inositol is selected from the group consisting of myo-inoViWol and iW¶V iVomeUV and WheiU UeVpecWiYe deUiYaWiYeV namely myo-inositol hexakis phosphate (phytic acid); pentakis-, tri-, di- phosphates and their isomers; and myo-inositol mono phosphate, myo-inositol trispyrophosphate, 1-phosphatidyl-myo-inositol , 1-phosphatidyl-myo-inositol 3-phosphate, derivatives of ononitol, sequoytol,dombonitol, viscumitol, pinitol, quebrachitol, pinpollitol and brahol, myo-inositol 1,3,4,5,6-pentakis-O- (trimethylsilyl)-, bis(trimethylsilyl) phosphate, phosphatidylinositol 5-phosphate PI(5) diC8 ammonium salt, phosphatidylinositol 5-phosphate diC16 (PI(5)P diC16) sodium salt, 1,2 -ciacyl-sn-glycero-3-phospho-(1-D-myo-inositol 4,5-biphosphate), phosphatidylinositol, phosphatidylinositol 3-phosphate, phosphatidylinositol 4-phosphate, phosphatidylinositol 4,5-phosphate, di-myo- inositol-phosphate, ciceritol phosphate, fagopyritol phosphate, glycosylinositol phosphryl ceramide, C25,25-Archeditylinositol, ceramide phosphoinositol, D- myo-inositol-4-hydrogen phosphate monoammonium salt and phosphatidylinositol phosphate, and D-myo-inositol-4-hydrogen phosphate, monoammonium salt.
17. The formation electrolyte suitable for formation of an oxide on a valve metal anode of claim 1 further comprising additives selected from metal salts, salts of organic acids, salts of inorganic acids, organic acids, inorganic acids, organometallic compounds, inorganic solvents, organic solvents, crosslinking agents, surface active agents and buffers.
18. The formation electrolyte suitable for formation of an oxide on a valve metal anode of claim 17 wherein said metal salts, salts of inorganic acids and salts of organic acids comprise halides, nitrides, sulfides, amides, nitrates, sulfates, phosphates, carbonates, chromates, chlorates, perchlorates, oxides, oxychlorides, peroxides, carboxylates, amides and esters.
19. The formation electrolyte suitable for formation of an oxide on a valve metal anode of claim 17 wherein said organic and inorganic acids comprise carboxylic acids, phosphonic acids, phosphinic acids, phosphoric acid, phthalic acid, maleic acid, malonic acid and trimesic acid.
20. The formation electrolyte suitable for formation of an oxide on a valve metal anode of claim 17 wherein said organometallic compounds comprise organosilanes, organoboranes, carbonyls, phosphines, crosslinking agents, surface active agents and buffers.
21. The formation electrolyte suitable for formation of an oxide on a valve metal anode of claim 17 further comprising at least one solvent selected from the group consisting of water, alcohol, ethylene glycol, polyethylene glycol, tetraglyme, propylene glycol, glycol ether and alkanolamines.
22. A method of forming a solid electrolytic capacitor comprising: forming a dielectric oxide on a tantalum anode by: applying a formation electrolyte on said anode wherein said formation electrolyte comprises a derivative of inositol is defined by Formula 1:wherein: each of R1-R6is independently selected from H, substituted or unsubstituted carbon chain of up to 20 carbon atoms, -PO3R7R8; -SiR93,-C(O)R10; and ;or adjacent groups may be taken together to represent ^P(O)OH^O^P(O)OH^; each R7and R8are independently selected from H, a cation; saturated or unsaturated carbon chain of up 35 carbon atoms; or ^CH2CHR12CH2R13; each R9is independently an alkyl of 1 to 10 carbon atoms; each R10is independently an alkyl of 1 to 10 carbon atoms; each R11represents a bond to an oxygen of the derivative of inositol of Formula 1; and R12and R13are esters terminated with H, saturated or unsaturated carbon chain of 1 to 35 carbon atoms; and forming a conductive polymer cathode on said dielectric oxide.
23. The method of forming a solid electrolytic capacitor of claim 22 wherein at least one of R1^R6is ^PO3R7R8with at least one of R7or R8being ^H.
24. The method of forming a solid electrolytic capacitor of claim 23 wherein R7and R8are both ^H.
25. The method of forming a solid electrolytic capacitor of claim 23 wherein at least two of R1^R6is ^PO3R7R8.
26. The method of forming a solid electrolytic capacitor of claim 25 wherein at least three of R1^R6is ^PO3R7R8.
27. The method of forming a solid electrolytic capacitor of claim 25 wherein at least four of R1^R6is ^PO3R7R8.
28. The method of forming a solid electrolytic capacitor of claim 27 wherein at least five of R1^R6is ^PO3R7R8.
29. The method of forming a solid electrolytic capacitor of claim 27 wherein each of R1^R6is ^PO3R7R8.
30. The method of forming a solid electrolytic capacitor of claim 29 with each R7and R8is ^H.
31. The method of forming a solid electrolytic capacitor of claim 22 wherein at least one R7or R8is a cation.
32. The method of forming a solid electrolytic capacitor of claim 22 wherein said cation is selected from the group consisting of quaternary amines and saturated or unsaturated carbon chain of up 35 carbon atoms.
33. The method of forming a solid electrolytic capacitor of claim 22 wherein each R9is independently an alkyl of 1 to 3 carbon atoms.
34. The method of forming a solid electrolytic capacitor of claim 33 wherein each R9is ^CH3.
35. The method of forming a solid electrolytic capacitor of claim 22 wherein each R10is independently an alkyl of 1 to 3 carbon atoms.
36. The method of forming a solid electrolytic capacitor of claim 35 wherein each R10is ^CH3.
37. The method of forming a solid electrolytic capacitor of claim 22 wherein said derivative of inositol is selected from the group consisting of myo-inositol and iW¶V iVomeUV and WheiU UeVpecWiYe deUiYaWiYeV namel\ m\o-inositol hexakis phosphate (phytic acid); pentakis-, tri-, di-phosphates and their isomers; and myo-inositol mono phosphate, myo-inositol trispyrophosphate, 1- phosphatidyl-myo-inositol , 1-phosphatidyl-myo-inositol 3-phosphate, derivatives of ononitol, sequoytol,dombonitol, viscumitol, pinitol, quebrachitol, pinpollitol and brahol, myo-inositol 1,3,4,5,6-pentakis-O-(trimethylsilyl)-,bis(trimethylsilyl) phosphate, phosphatidylinositol 5-phosphate PI(5) diC8 ammonium salt, phosphatidylinositol 5-phosphate diC16 (PI(5)P diC16) sodium salt, 1,2 -ciacyl-sn-glycero-3-phospho-(1-D-myo-inositol 4,5- biphosphate), phosphatidylinositol, phosphatidylinositol 3-phosphate, phosphatidylinositol 4-phosphate, phosphatidylinositol 4,5-phosphate, di-myo- inositol-phosphate, ciceritol phosphate, fagopyritol phosphate, glycosylinositol phosphryl ceramide, C25,25-Archeditylinositol, ceramide phosphoinositol, D- myo-inositol-4-hydrogen phosphate monoammonium salt and phosphatidylinositol phosphate.
38. The method of forming a solid electrolytic capacitor of claim 22 wherein said formation electrolyte comprises additives selected from metal salts, salts of organic acids, salts of inorganic acids, organic acids, inorganic acids, organometallic compounds, inorganic solvents, organic solvents, crosslinking agents, surface active agents and buffers.
39. The method of forming a solid electrolytic capacitor of claim 38 wherein said metal salts, salts of inorganic acids and salts of organic acids comprise halides, nitrides, sulfides, amides, nitrates, sulfates, phosphates, carbonates, chromates, chlorates, perchlorates, oxides, oxychlorides, peroxides, carboxylates, amides and esters.
40. The method of forming a solid electrolytic capacitor of claim 38 wherein said organic and inorganic acids comprise carboxylic acids, phosphonic acids, phosphinic acids, phosphoric acid, phthalic acid, maleic acid, malonic acid and trimesic acid.
41. The method of forming a solid electrolytic capacitor of claim 38 wherein said organometallic compounds comprise organosilanes, organoboranes, carbonyls, phosphines, crosslinking agents, surface active agents and buffers.
42. The method of forming a solid electrolytic capacitor of claim 22 wherein said formation electrolyte further comprises at least one solvent selected from the group consisting of water, alcohol, ethylene glycol, polyethylene glycol, tetraglyme, propylene glycol, glycol ether and alkanolamines.
43. The method of forming a solid electrolytic capacitor of claim 22 wherein said conductive polymer is selected from the group consisting of poly(3,4- ethylenedioxythiophene), poly(4-(2,3-dihydrothieno-[3,4-b][1,4]dioxin-2- yl)methoxy)-1-butane-sulphonic acid, salt), poly(4-(2,3-dihydrothieno-[3,4- b][1,4]dioxin-2-yl)methoxy)-1-propane-sulphonic acid, salt), poly(4-(2,3- dihydrothieno-[3,4-b][1,4]dioxin-2-yl)methoxy)-1-methyl-1-propane-sulphonic acid, salt), poly(4-(2,3-dihydrothieno-[3,4-b][1,4]dioxin-2-yl)methoxy alcohol, poly(N-methylpyrrole), poly(3-methylpyrrole), poly(3-octylpyrrole), poly(3- decylpyrrole), poly(3-dodecylpyrrole), poly(3,4-dimethylpyrrole), poly(3,4- dibutylpyrrole), poly(3-carboxypyrrole), poly(3-methyl-4-carboxypyrrole), poly(3-methyl-4-carboxyethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), poly(3-hydroxypyrrole), poly(3-methoxypyrrole), polythiophene, poly(3- methylthiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3- octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3- octadecylthiophene), poly(3-bromothiophene), poly(3,4-dimethylthiophene), poly(3,4-dibutylthiophene), poly(3-hydroxythiophene), poly(3- methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), poly(3-octadecyloxythiophene), poly(3,4-dihydroxythiophene), poly(3,4- dimethoxythiophene), poly(3,4-ethylenedioxythiophene), poly(3,4- propylenedioxythiophene), poly(3,4-butenedioxythiophene), poly(3- carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4- carboxyethylthiophene), poly(3-methyl-4-carboxybutylthiophene), polyaniline, poly(2-methylaniline), poly(3-isobutylaniline), poly(2-aniline sulfonate), poly(3- aniline sulfonate) 44. The method of forming a solid electrolytic capacitor of claim 22 wherein said dielectric is not washed prior to said forming of said conductive polymer cathode.
45. A capacitor comprising an anode prepared by anodizing a pressed valve metal powder in the electrolytic solution of claim 22.
46. The capacitor of claim 45 wherein said conductive polymer layer comprises an internal polymer layer and an external polymer layer and said internal and external polymer comprise pre-polymerized conductive polymer 47. A capacitor of claim 45 having an anomalous charge current less than 4 times the theoretical value.