Degradable PVC film and preparation method for adhesive tape
By combining low molecular weight liquid hyperbranched polylactic acid, thermoplastic starch and vegetable oil, degradable PVC films and tapes are prepared, which solves the problem of difficult degradation of PVC materials and achieves high performance and environmentally friendly degradation effects.
Patent Information
- Application Number
- PCT/CN2023/116288
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2023-08-31
- Publication Date
- 2024-10-17
AI Technical Summary
Existing PVC materials are difficult to degrade, leading to environmental pollution, and there is a lack of degradable high-performance PVC film and tape preparation methods.
Low molecular weight liquid hyperbranched polylactic acid, thermoplastic starch and vegetable oil are combined with PVC resin, and degradable PVC films and tapes are prepared through suspension method and melt polycondensation method. High-speed mixers, internal mixers and extruders are used for molding, and through Coater prepares tape.
It achieves the good mechanical properties of PVC films and tapes and the migration resistance of plasticizers, and can be completely degraded under natural conditions. The disintegration degree, tensile strength and elongation at break are significantly improved, and the degradation performance is excellent.
Smart Images

Figure CN2023116288_17102024_PF_FP_ABST
Abstract
Description
A method for preparing degradable PVC film and tape Technical Field
[0001] The invention relates to the technical field of PVC films and tapes, in particular to a preparation method of a degradable PVC film and tape. Background Art
[0002] The widespread use of products made from synthetic polymers has brought significant convenience to modern life and production. However, discarded plastics are difficult to degrade in nature. Long-term environmental residues can cause severe "white pollution," severely harming soil, rivers, lakes, oceans, and other ecological environments, and even threatening human health. As awareness of environmental protection continues to grow, the production of biodegradable plastic products is becoming increasingly urgent.
[0003] Polyvinyl chloride (PVC) is a thermoplastic polymer material synthesized by free radical polymerization of vinyl chloride monomer. It is also one of the most widely used general polymer materials. PVC is an amorphous white powder with a low degree of branching and a relative density of 1.4g / cm 3 The glass transition temperature is 77-90℃, and it begins to decompose at around 170℃.
[0004] Starch is a natural high-molecular carbohydrate that can be considered a polymer of glucose. It comes from a wide range of sources, including wheat starch, potato starch, corn starch, mung bean starch, and sweet potato starch. With the increasing depletion of petroleum resources and the increasing white pollution caused by plastic products, starch, as a renewable and biodegradable natural polymer material, has attracted widespread attention and research from researchers both domestically and internationally. The modification of starch for use in synthetic polymer materials has also yielded considerable results.
[0005] Polylactic acid (PLA) is a new biodegradable material made from starch derived from renewable plant resources such as corn. This starch is fermented into lactic acid, which is then converted into PLA through chemical synthesis. It exhibits excellent biodegradability and is completely degraded by natural microorganisms, ultimately producing carbon dioxide and water without polluting the environment. This is highly beneficial for environmental protection and is recognized as an environmentally friendly material. Low-molecular-weight liquid hyperbranched PLA, synthesized by melt polycondensation, exhibits higher plasticizing efficiency than linear PLA, making it more suitable for use in PVC film products.
[0006] The invention provides a biodegradable PVC plastic film, which has good mechanical properties, good plasticizer migration resistance and can be degraded under natural conditions.
[0007] Summary of the Invention
[0008] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a method for preparing a degradable PVC film and tape to solve the problems raised in the above technical background.
[0009] To achieve the above object, the present invention is implemented through the following technical solutions:
[0010] In a first aspect, the present invention provides a degradable PVC film comprising the following raw materials in parts by weight: 100 parts of PVC resin, 80-90 parts of starch, 45-65 parts of polylactic acid, 10-15 parts of vegetable oil, 50-60 parts of filler, and 5-8 parts of stabilizer.
[0011] Furthermore, the PVC resin adopts suspension method general-purpose PVC resin powder with a polymerization degree of 800-1800.
[0012] Furthermore, the starch is thermoplastic starch.
[0013] Furthermore, the polylactic acid is a low molecular weight liquid hyperbranched polylactic acid with a viscosity of 2000-5000 mPa·S.
[0014] Furthermore, the vegetable oil is one or more of epoxidized soybean oil, castor oil, and sunflower oil.
[0015] Furthermore, the filler is one or more of talc, kaolin, and montmorillonite.
[0016] Furthermore, the stabilizer is one or more of a barium zinc stabilizer, a calcium zinc stabilizer, and a rare earth stabilizer.
[0017] In a second aspect, the present invention provides an adhesive tape comprising the degradable PVC film described in the first aspect.
[0018] In a third aspect, the present invention provides a method for preparing an adhesive tape, comprising the following steps:
[0019] Step 1: Add PVC resin powder, polylactic acid, vegetable oil and stabilizer into a high-speed mixer according to the formula and stir at high speed for 10-15 minutes. Then add starch and filler into the high-speed mixer and continue stirring for 3-5 minutes to mix evenly.
[0020] Step 2: Add the mixture obtained in step 1 into an internal mixer for internal mixing and plasticization, then plasticize it in an open mixer and an extruder, form it in a calender at 180-200°C, and finally cool and coil it to make a degradable PVC film.
[0021] Step 3: The degradable PVC film obtained in step 2 is coated by a high-speed coating machine to prepare a degradable PVC tape semi-finished product with a thickness of 20 microns.
[0022] Step 4: Cut the semi-finished product obtained in step 3 into pieces according to the specified width requirements to obtain the required electrical tape.
[0023] Furthermore, the polylactic acid adopts a low molecular weight liquid hyperbranched polylactic acid with a viscosity of 2000-5000 mPa·S, and its preparation method is as follows: using citric acid as a core molecule, citric acid and L-lactic acid in a ratio of 1:20-1:50, and using 0.7wt%-1.2wt% of stannous chloride and p-toluenesulfonic acid as catalysts, and synthesizing the low molecular weight liquid branched polylactic acid by melt polycondensation method, with a viscosity of 2000-5000 mPa·S.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The PVC film obtained by the present invention has good mechanical properties, good plasticizer migration resistance, and can be degraded under natural conditions.
[0026] 2. The plasticizer polylactic acid of the present invention adopts low molecular weight liquid hyperbranched polylactic acid with a viscosity of 2000-5000 mPa·s. The hyperbranched polylactic acid uses citric acid as the core molecule and is polymerized to generate hyperbranched polylactic acid. Due to its multi-arm structure, it can effectively increase the distance between PVC molecular chains when plasticizing PVC. Compared with traditional straight-chain plasticizers, its plasticizing efficiency is higher. Since its molecular weight is higher than that of traditional phthalic plasticizers, it has excellent migration resistance and volatility resistance.
[0027] 3. The present invention uses hyperbranched polylactic acid, thermoplastic starch, vegetable oil (castor oil) and PVC resin to work synergistically, so that the disintegration, tensile strength and elongation at break of the obtained PVC film are significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] FIG1 is a bar graph showing the disintegration degree of the PVC film and the tensile strength of the PVC film and the adhesive tape of the present invention. DETAILED DESCRIPTION
[0029] The following describes the embodiments of the present invention through specific examples. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments. The details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other unless they conflict.
[0030] Some of the raw materials used in this application are as follows:
[0031] Suspension method general-purpose PVC resin powder with a degree of polymerization of 800-1800, specifications are 800-1000 degree of polymerization, 1000-1200 degree of polymerization, 1200-1400 degree of polymerization, 1400-1600 degree of polymerization, and 1600-1800 degree of polymerization. The manufacturer is Qilu Petrochemical;
[0032] Thermoplastic starch, manufactured by Suzhou Hesumei Technology Co., Ltd.
[0033] Liquid hyperbranched polylactic acid
[0034] In the present invention, the polylactic acid adopts low molecular weight liquid hyperbranched polylactic acid with a viscosity of 2000-5000 mPa·s, which contains lactic acid, citric acid and a catalyst; wherein the citric acid and L-lactic acid are mixed in a ratio of 1:20-1:50, the content of the catalyst is 0.7wt%-1.2wt%, and the catalyst contains stannous octoate and p-toluenesulfonic acid.
[0035] The preparation method comprises the following steps: using citric acid as a core molecule, mixing citric acid and L-lactic acid in a ratio of 1:20-1:50, using 0.7wt%-1.2wt% of stannous octoate and p-toluenesulfonic acid as catalysts, and adopting a melt polycondensation method to synthesize low-molecular-weight liquid hyperbranched polylactic acid with a viscosity of 2000-5000 mPa·s.
[0036] Example 1
[0037] A low-molecular-weight liquid hyperbranched polylactic acid is prepared from the following raw materials in the following weight ratio: 100 parts of L-lactic acid, 5 parts of citric acid, 0.4 parts of stannous octoate as a catalyst, and 0.4 parts of p-toluenesulfonic acid.
[0038] Specific steps:
[0039] The raw materials in the aforementioned mass ratios were added to a reaction vessel. Nitrogen was continuously introduced during the addition process to ensure that oxygen within the vessel was completely expelled, thereby preventing oxidation of the hydroxyl groups due to the high temperature during the reaction. After the addition of the raw materials, the reaction was continued at a temperature of 110°C and a vacuum of 8 kPa for 2 hours to allow the L-lactic acid to react and form a lactic acid prepolymer with a certain degree of polymerization. As the degree of polymerization increases, the viscosity of the material within the vessel increases. The temperature was then raised to 140°C, the vacuum reduced to 3 kPa, and the reaction continued for another 2 hours. Upon completion of the reaction, hyperbranched polylactic acid was obtained. The resulting polylactic acid had a viscosity of approximately 2000 mPa·s.
[0040] Example 2
[0041] A hyperbranched biodegradable polyester plasticizer is prepared from the following raw materials in the following weight ratio: 100 parts of L-lactic acid, 3 parts of citric acid, 0.5 parts of stannous octoate as a catalyst, and 0.5 parts of p-toluenesulfonic acid.
[0042] Specific steps:
[0043] The raw materials in the aforementioned mass ratios were added to a reaction vessel. Nitrogen was continuously introduced during the addition process to ensure that oxygen within the vessel was completely expelled, thereby preventing oxidation of the hydroxyl groups due to the high temperature during the reaction. After the addition of the raw materials, the reaction was continued at a temperature of 120°C and a vacuum of 8 kPa for 2 hours to allow the L-lactic acid to react and form a lactic acid prepolymer with a certain degree of polymerization. As the degree of polymerization increases, the viscosity of the material within the vessel increases. At this point, the temperature was raised to 140°C, the vacuum was reduced to 3 kPa, and the reaction was continued for another 3 hours. Upon completion of the reaction, a hyperbranched polylactic acid (PLA) was obtained. The resulting polylactic acid had a viscosity of approximately 3000 mPa·s.
[0044] Example 3
[0045] A hyperbranched biodegradable polyester plasticizer is prepared from the following raw materials in the following weight ratio: 100 parts of L-lactic acid, 5 parts of citric acid, 0.6 parts of stannous octoate as a catalyst, and 0.6 parts of p-toluenesulfonic acid.
[0046] Specific steps:
[0047] The raw materials in the aforementioned mass ratios were added to a reaction vessel. Nitrogen was continuously introduced during the addition process to ensure that all oxygen in the vessel was completely expelled, thereby preventing oxidation of the hydroxyl groups due to the high temperature during the reaction. After the addition of the raw materials, the reaction was continued at a temperature of 120°C and a vacuum of 5 kPa for 2 hours to allow the L-lactic acid to react and form a lactic acid prepolymer with a certain degree of polymerization. As the degree of polymerization increases, the viscosity of the material in the vessel increases. At this point, the temperature was raised to 150°C, the vacuum was reduced to 1 kPa, and the reaction was continued for another 4 hours. After completion of the reaction, a hyperbranched polylactic acid was obtained. The resulting polylactic acid had a viscosity of approximately 4000 mPa·s.
[0048] Example 4
[0049] A hyperbranched biodegradable polyester plasticizer is prepared from the following raw materials in the following weight ratio: 100 parts of L-lactic acid, 5 parts of citric acid, 0.6 parts of stannous octoate as a catalyst, and 0.6 parts of p-toluenesulfonic acid.
[0050] Specific steps:
[0051] The raw materials in the aforementioned mass ratios were added to a reaction vessel. Nitrogen was continuously introduced during the addition process to ensure that oxygen within the vessel was completely expelled, thereby preventing oxidation of the hydroxyl groups due to the high temperature during the reaction. After the addition of the raw materials, the reaction was continued at a temperature of 120°C and a vacuum of 5 kPa for 2 hours to allow the L-lactic acid to react and form a lactic acid prepolymer with a certain degree of polymerization. As the degree of polymerization increases, the viscosity of the material in the vessel increases. At this point, the temperature was raised to 150°C, the vacuum was reduced to 1 kPa, and the reaction was continued for another 6 hours. Upon completion of the reaction, a hyperbranched polylactic acid was obtained. The resulting polylactic acid had a viscosity of approximately 5000 mPa·s.
[0052] The degradation performance and plasticizing efficiency of the liquid hyperbranched polylactic acid obtained in this application were compared and tested. The specific method is: refer to ISO20200:2015 "Determination of the degree of decomposition of plastic materials under laboratory simulated composting conditions" standard for degradation test; use the liquid hyperbranched polylactic acid of Examples 1-4 and commercially available straight-chain ordinary polyester plasticizer (manufacturer Taiwan Changchun Group D1200, as a control group). PVC is plasticized, and the same sample is made. The DOP-plasticized PVC sample is used as a standard part. The tensile stress of each sample is tested, and the plasticizing efficiency ratio of each embodiment and the control group is calculated, wherein the plasticizing efficiency ratio = sample tensile stress / standard part tensile stress; the volatilization rate of each embodiment is tested by constant temperature treatment at 155°C for 240 hours. The disintegration degree (%), plasticizing efficiency ratio and volatilization rate (%) of the liquid hyperbranched polylactic acid obtained according to the above method are shown in Table 1.
[0053] Table 1
[0054] As shown in Table 1, the disintegration of the liquid hyperbranched polylactic acid prepared in Examples 1-4 under composting conditions reached 99%, indicating almost complete degradation. Compared with the control group, the polylactic acid of the present application has better degradation performance. At the same viscosity, the hyperbranched polylactic acid plasticizer has higher plasticizing efficiency and better volatility resistance than the linear polyester plasticizer.
[0055] PVC film and tape
[0056] Example 5
[0057] A degradable PVC film is prepared from the following raw materials in the following proportions by weight: 100 parts of PVC with a degree of polymerization of 800-1000, 80 parts of thermoplastic starch, 45 parts of low-molecular-weight liquid hyperbranched polylactic acid with a viscosity of 2000 mPa·s provided in Example 1, 10 parts of epoxidized soybean oil, 50 parts of talc, and 5 parts of a barium-zinc composite stabilizer.
[0058] The above formula is pressed and formed on a 180°C calendering device according to the above production process steps to obtain a degradable PVC film product, which is then coated on a high-speed coater to obtain a PVC tape semi-finished product, and then cut into finished tapes of specified widths.
[0059] Example 6
[0060] A degradable PVC film is made from the following raw materials in the following proportions by weight: 100 parts of PVC with a degree of polymerization of 1000-1200, 85 parts of thermoplastic starch, 50 parts of low-molecular-weight liquid hyperbranched polylactic acid with a viscosity of 3000 mPa·s provided in Example 2, 12 parts of epoxidized soybean oil, 55 parts of kaolin, and 6 parts of a rare earth stabilizer.
[0061] The above formula is pressed and formed on a 185°C calendering device according to the above production process steps to obtain a degradable PVC film product, which is then coated on a high-speed coater to obtain a PVC tape semi-finished product, and then cut into finished tapes of specified widths.
[0062] Example 7
[0063] A degradable PVC film is made from the following raw materials in the following proportions by weight: 100 parts of PVC with a degree of polymerization of 1200-1400, 90 parts of thermoplastic starch, 55 parts of low-molecular-weight liquid hyperbranched polylactic acid with a viscosity of 4000 mPa·s provided in Example 3, 15 parts of sunflower oil, 60 parts of montmorillonite, and 7 parts of a calcium-zinc composite stabilizer.
[0064] The above formula is pressed and formed on a 190°C calendering device according to the above production process steps to obtain a degradable PVC film product, which is then coated on a high-speed coater to obtain a PVC tape semi-finished product, and then cut into finished tapes of specified widths.
[0065] Example 8
[0066] A degradable PVC film is made from the following raw materials in the following proportions by weight: 100 parts of PVC with a degree of polymerization of 1400-1600, 90 parts of thermoplastic starch, 60 parts of low-molecular-weight liquid hyperbranched polylactic acid with a viscosity of 4000 mPa·s provided in Example 3, 15 parts of castor oil, 30 parts of kaolin, 30 parts of talc, and 7 parts of a calcium-zinc composite stabilizer.
[0067] The above formula is pressed and formed on a 195°C calendering device according to the above production process steps to obtain a degradable PVC film product, which is then coated on a high-speed coater to obtain a PVC tape semi-finished product, and then cut into finished tapes of specified widths.
[0068] Example 9
[0069] A degradable PVC film is made from the following raw materials in the following proportions by weight: 100 parts of PVC with a degree of polymerization of 1600-1800, 90 parts of thermoplastic starch, 65 parts of the low molecular weight liquid hyperbranched polylactic acid with a viscosity of 5000 mPa·s provided in Example 4, 15 parts of castor oil, 30 parts of kaolin, and 8 parts of a calcium-zinc composite stabilizer.
[0070] The above formula is pressed and formed on a 200°C calendering device according to the above production process steps to obtain a degradable PVC film product, which is then coated on a high-speed coater to obtain a PVC tape semi-finished product, and then cut into finished tapes of specified widths.
[0071] Comparative Example 1
[0072] A degradable PVC film is similar to Example 8, except that the low molecular weight liquid hyperbranched polylactic acid with a viscosity of 4000 mPa·s is replaced with a commercially available linear common polyester plasticizer with a viscosity of 4000 mPa·s. The film is specifically made of the following raw materials in the following weight ratio: 100 parts of PVC with a degree of polymerization of 1400-1600, 90 parts of thermoplastic starch, 60 parts of a commercially available linear common polyester plasticizer, 15 parts of castor oil, 30 parts of kaolin, 30 parts of talc, and 7 parts of a calcium-zinc composite stabilizer. The commercially available linear common polyester plasticizer is D1200 from Taiwan Changchun Group.
[0073] The above formula is pressed and formed on a 195°C calendering device according to the above production process steps to obtain a degradable PVC film product, which is then coated on a high-speed coater to obtain a PVC tape semi-finished product, and then cut into finished tapes of specified widths.
[0074] Comparative Example 2
[0075] A degradable PVC film is similar to Example 8, except that the low molecular weight liquid hyperbranched polylactic acid with a viscosity of 4000 mPa·s is replaced with DOP. The film is specifically made of the following raw materials in the following weight ratio: 100 parts of PVC with a degree of polymerization of 1400-1600, 90 parts of thermoplastic starch, 60 parts of DOP, 15 parts of castor oil, 30 parts of kaolin, 30 parts of talc, and 7 parts of a calcium-zinc composite stabilizer.
[0076] The above formula is pressed and formed on a 195°C calendering device according to the above production process steps to obtain a degradable PVC film product, which is then coated on a high-speed coater to obtain a PVC tape semi-finished product, and then cut into finished tapes of specified widths.
[0077] Comparative Example 3
[0078] A degradable PVC film is similar to Example 8, except that the thermoplastic starch is omitted. The film is specifically made of the following raw materials in the following weight ratio: 100 parts of PVC with a degree of polymerization of 1400-1600, 60 parts of low molecular weight liquid hyperbranched polylactic acid with a viscosity of 4000 mPa·s, 15 parts of castor oil, 30 parts of kaolin, 30 parts of talc, and 7 parts of a calcium-zinc composite stabilizer.
[0079] The above formula is pressed and formed on a 195°C calendering device according to the above production process steps to obtain a degradable PVC film product, which is then coated on a high-speed coater to obtain a PVC tape semi-finished product, and then cut into finished tapes of specified widths.
[0080] Comparative Example 4
[0081] A degradable PVC film is similar to Example 8, except that castor oil is omitted. The film is specifically made of the following raw materials in the following proportions by weight: 100 parts of PVC with a degree of polymerization of 1400-1600, 90 parts of thermoplastic starch, 60 parts of low molecular weight liquid hyperbranched polylactic acid with a viscosity of 4000 mPa·s, 30 parts of kaolin, 30 parts of talc, and 7 parts of a calcium-zinc composite stabilizer.
[0082] The above formula is pressed and formed on a 195°C calendering device according to the above production process steps to obtain a degradable PVC film product, which is then coated on a high-speed coater to obtain a PVC tape semi-finished product, and then cut into finished tapes of specified widths.
[0083] The specific formula contents and processes of the PVC films and tapes obtained in Examples 5-9 and Comparative Examples 1-4 are shown in Table 2.
[0084] Table 2
[0085] The degradation performance and physical properties of the degradable PVC films and tapes prepared in Examples 5-9 and Comparative Examples 1-4 were tested. The degradation test was carried out with reference to ISO 20200:2015 "Plastics - Determination of the degree of decomposition of plastic materials under laboratory simulated composting conditions", the physical property test was carried out with reference to GB / T3830-2008 "Soft polyvinyl chloride calendered film and sheet" standard, and the test was carried out with reference to GB / T20631.2-2006 "Pressure-sensitive adhesive tapes for electrical use - Part 2: Test methods". The disintegration degree, tensile strength, and elongation at break of the PVC film, and the tensile strength and elongation at break of the tape are shown in Table 3 and Figure 1.
[0086] Table 3
[0087] As can be seen from Table 3 and Figure 1, the relevant indicators of the degradable PVC films and tapes prepared in Examples 5-9 all meet the requirements of the enterprise standard Q / XSJ0202, and all have good degradation performance, among which Example 8 has better degradation performance and physical property indicators.
[0088] Embodiment 8 is compared with comparative example 1 as can be known, and hyperbranched polylactic acid is compared straight chain polylactic acid and the tensile strength and the elongation at break of PVC film have an improving effect, and this is because the branched structure of plasticizer (hyperbranched polylactic acid) improves its plasticizing efficiency. Embodiment 8 is compared with comparative example 2 as can be known, and liquid hyperbranched polylactic acid plasticizer improves its degradation efficiency under the prerequisite that does not reduce PVC film performance. Embodiment 8 is compared with comparative example 3 as can be known, and the adding of plastic starch can significantly improve the degradation properties of PVC film. Embodiment 8 is compared with comparative example 4 as can be known, and the adding of castor oil can improve the plasticity of PVC film and improve its degradation properties.
[0089] In summary, the present invention adopts hyperbranched polylactic acid, plastic starch, vegetable oil (castor oil) and PVC resin to work synergistically, and the obtained PVC film has good mechanical properties, the plasticizer has good migration resistance, and can achieve degradation under natural conditions.
[0090] The above-described embodiments merely represent specific implementations of the present invention. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that a person skilled in the art would be able to make numerous variations and improvements without departing from the spirit of the present invention, and all such variations and improvements fall within the scope of protection of the present invention.
Claims
1. A degradable PVC film, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of PVC resin, 80-90 parts of starch, 45-65 parts of polylactic acid, 10-15 parts of vegetable oil, 50-60 parts of filler and 5-8 parts of stabilizer.
2. A degradable PVC film according to claim 1, characterized in that: The PVC resin is a suspension method general-purpose PVC resin powder with a polymerization degree of 800-1800.
3. A degradable PVC film according to claim 1, characterized in that: The starch is thermoplastic starch.
4. The degradable PVC film according to claim 1, characterized in that: The polylactic acid is low molecular weight liquid hyperbranched polylactic acid with a viscosity of 2000-5000 mPa·S.
5. The degradable PVC film according to claim 1, characterized in that: The vegetable oil is one or more of epoxidized soybean oil, castor oil and sunflower seed oil.
6. The degradable PVC film according to claim 1, characterized in that: The filler is one or more of talc, kaolin and montmorillonite.
7. The degradable PVC film according to claim 1, characterized in that: The stabilizer is one or more of a barium zinc stabilizer, a calcium zinc stabilizer, and a rare earth stabilizer.
8. An adhesive tape, characterized in that: A degradable PVC film comprising any one of claims 1 to 7.
9. The method for preparing an adhesive tape according to claim 8, characterized in that: The following steps are involved: Step 1. Add PVC resin powder, polylactic acid, vegetable oil and stabilizer into a high-speed mixer according to the formula and stir at high speed for 10-15 minutes. Then add starch and filler into the high-speed mixer and continue stirring for 3-5 minutes to mix evenly. Step 2: Add the mixture obtained in step 1 into an internal mixer for internal mixing and plasticization, then plasticize it in an open mixer and an extruder, and form it in a calender at 180-200° C., and finally cool and coil it to form a degradable PVC film. Step 3: The degradable PVC film obtained in step 2 is coated by a high-speed coating machine to prepare a degradable PVC tape semi-finished product with a thickness of 20 microns. Step 4: Cut the semi-finished product obtained in step 3 into pieces according to the specified width requirements to obtain the required electrical tape.
10. The method for preparing an adhesive tape according to claim 9, characterized in that: The polylactic acid adopts low molecular weight liquid hyperbranched polylactic acid with a viscosity of 2000-5000 mPa·S. The preparation method thereof comprises the following steps: using citric acid as a core molecule, mixing citric acid and L-lactic acid in a ratio of 1:20-1:50, using 0.7wt%-1.2wt% of stannous octoate and p-toluenesulfonic acid as catalysts, and adopting a melt polycondensation method to synthesize the low molecular weight liquid hyperbranched polylactic acid with a viscosity of 2000-5000 mPa·S.
Citation Information
Patent Citations
Preparation method for plastic packing box
CN109135223A
Formula of degradable environment-friendly plastic film and production process for degradable environment-friendly plastic film
CN110511442A
Starch-based degradable environment-friendly plastic and preparation method thereof
CN112391041A
Preparation method of degradable PVC film and adhesive tape
CN116355327A
Cited By
Medical PVC pump pipe material and production process thereof
CN118956085A