Preparation method for aluminum nitride film and device based on aluminum nitride film

By setting a protective layer on the surface of the aluminum nitride layer facing away from the substrate and performing thermal annealing treatment in an ammonia atmosphere, the problem of decomposition of the aluminum nitride film at high temperatures is solved and high crystal quality, low defect density and high surface area are achieved. Preparation of uniform aluminum nitride thin films.

WO2024212928A1PCT designated stage expired Publication Date: 2024-10-17ZHUHAI PICNOVA SEMICON TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/086614
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-04-08
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

It is difficult to prepare aluminum nitride films with high crystal quality, low defect density and high surface uniformity using existing technology. In particular, the film is prone to decomposition during high-temperature thermal annealing, resulting in increased surface roughness and limited improvement in crystal quality.

Method used

A protective layer is provided on the surface of the aluminum nitride layer facing away from the substrate, including a recessed area and a flat area surrounding the periphery of the recessed area. The crystal quality of the aluminum nitride film is improved and the defect density is reduced through thermal annealing in an ammonia atmosphere.

Benefits of technology

An aluminum nitride film with high crystal quality, low defect density and high surface uniformity is achieved. The thermal annealing treatment effectively reduces the defect density of the film and improves the surface smoothness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024086614_17102024_PF_FP_ABST
    Figure CN2024086614_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation method for an aluminum nitride film and an aluminum nitride film-based device. The preparation method comprises: providing an aluminum nitride substrate, wherein the aluminum nitride substrate comprises a substrate and an aluminum nitride layer having a first temperature that are arranged in a stacked manner; providing a protective layer on the surface of the aluminum nitride layer facing away from the substrate, wherein the protective layer comprises a recessed area and a flat sheet area arranged around the periphery of the recessed area, and the root mean square roughness (RMS) of the surface of the flat sheet area facing the aluminum nitride layer is within the following range: 0 nm < RMS ≤ 50 nm; and carrying out thermal annealing treatment on the aluminum nitride substrate and the protective layer to obtain the aluminum nitride film having a second temperature, wherein the second temperature is greater than the first temperature. The preparation method for an aluminum nitride film allows for preparation of an aluminum nitride film having high crystal quality, low defect density and high surface uniformity.
Need to check novelty before this filing date? Find Prior Art

Description

A method for preparing aluminum nitride film and a device based on aluminum nitride film This application claims priority to the prior application with application number 202310405617.0 filed on April 14, 2023, entitled “A method for preparing aluminum nitride thin film and devices based on aluminum nitride thin film”, and the contents of the above-mentioned prior application are incorporated into this text by introduction. Technical Field The present application relates to a process for preparing semiconductor materials, and in particular to a method for preparing an aluminum nitride film and a device based on the aluminum nitride film. Background Art Aluminum nitride films with high crystal quality and low defect density are important underlying structures of electronic and optoelectronic devices based on group III nitrides (such as aluminum gallium nitride, etc.). Due to the high melting point of aluminum nitride materials and the large covalent bond energy of aluminum-nitrogen, it is difficult to prepare high-quality and low-cost aluminum nitride films by pulling single crystals. Aluminum nitride films are mostly obtained on heterogeneous substrates such as silicon carbide, gallium nitride, and sapphire, usually by physical deposition or chemical deposition methods. However, due to the certain lattice mismatch and thermal mismatch between aluminum nitride films and heterogeneous substrates, heteroepitaxial aluminum nitride films have more grains and grain boundaries, and there are a large number of dislocations inside the aluminum nitride films. The aluminum nitride film can be subjected to thermal annealing treatment to partially recrystallize the grains and grain boundaries in the aluminum nitride film into a more stable crystal state, so as to reduce the dislocation density inside the aluminum nitride film and improve the crystal quality of the aluminum nitride film. Usually, in a nitrogen atmosphere, the aluminum nitride film is subjected to high-temperature thermal annealing at any high temperature of 1773.15K to 1973.15K (for example, 1823.15K, 1923.15K, etc.). At high temperatures, the surface of the aluminum nitride film will decompose, so the face-to-face placement of the samples is used to inhibit the decomposition of the surface of the aluminum nitride film during the high-temperature thermal annealing process. However, during the annealing process, the samples are adhered to each other, and the peeling of the adhered samples results in an increase in the surface roughness and a decrease in the uniformity of the aluminum nitride film. At the same time, heat treatment in this temperature range has a very limited effect on the improvement of the crystal quality of the aluminum nitride film. Summary of the invention In view of this, the present application provides a method for preparing an aluminum nitride film and a device based on the aluminum nitride film. The method for preparing an aluminum nitride film can prepare an aluminum nitride film with high crystal quality, low defect density and high surface uniformity. The present application provides a method for preparing an aluminum nitride film, the preparation method comprising: providing an aluminum nitride substrate, the aluminum nitride substrate comprising a stacked substrate and an aluminum nitride layer having a first temperature; arranging a protective layer on the surface of the aluminum nitride layer away from the substrate, the protective layer comprising a recessed area and a flat sheet area arranged around the periphery of the recessed area, the root mean square roughness RMS of the surface of the flat sheet area facing the aluminum nitride layer being in the range of: 0nm<RMS≤50nm; and performing a thermal annealing treatment on the aluminum nitride substrate and the protective layer to obtain the aluminum nitride film having a second temperature; wherein the second temperature is greater than the first temperature. Furthermore, providing an aluminum nitride substrate includes: providing a substrate; depositing an aluminum nitride layer at a first temperature on the surface of the substrate by a physical or chemical method, wherein the deposition method includes but is not limited to sputtering, atomic layer deposition, molecular beam epitaxy, chemical vapor deposition, pulsed laser deposition, etc. Furthermore, the provision of an aluminum nitride substrate includes: providing a substrate; depositing an aluminum nitride layer having a first temperature on the surface of the substrate using a chemical vapor deposition method, wherein the temperature T1 ranges from 723.15K≤T1≤1873.15K; and the reaction pressure P1 ranges from 0Torr<P1≤800Torr, and the thickness d1 of the deposited aluminum nitride layer ranges from 0nm<d1≤1000nm; wherein the chemical vapor deposition method is a metal organic chemical vapor deposition method. Furthermore, the protective layer also includes one or more protruding structures, one of the protruding structures is arranged on the surface of the recessed area facing the aluminum nitride layer, and a plurality of the protruding structures are arranged at intervals on the surface of the recessed area facing the aluminum nitride layer, the protruding structure has an end face facing the aluminum nitride layer, the flat sheet area has a preset surface facing the aluminum nitride layer, and the end face portion is not higher than the preset surface. Furthermore, the distance d2 between the two farthest points of the protruding structure on the area enclosed by the orthographic projection of the surface of the aluminum nitride facing the protective layer is in the range of 0.1 μm≤d2≤50000 μm; the minimum spacing d3 between any two adjacent protruding structures is in the range of 0 μm≤d3≤50000 μm. Furthermore, along the stacking direction of the substrate and the aluminum nitride layer, the maximum height d4 of the protruding structure is in the range of 0 μm<d4≤200 μm. Furthermore, the thermal annealing of the aluminum nitride substrate and the protective layer includes: performing the thermal annealing in an ammonia atmosphere. Furthermore, the thermal annealing of the aluminum nitride substrate and the protective layer includes: performing thermal annealing in an ammonia atmosphere; wherein the range of the thermal annealing temperature T2 is: 773.15K≤T2≤2273.15K; and the range of the thermal annealing time t1 is: 0min<t1≤180min. Furthermore, the aluminum nitride film after thermal annealing satisfies at least one of the following conditions: the root mean square roughness of the surface of the aluminum nitride film away from the substrate is less than 3.3 nm, and the dislocation density of the aluminum nitride film is less than 5×10 10 cm -2 , the aluminum nitride film along

[0002] The full width at half maximum of the X-ray rocking curve along the [10-12] direction is less than 0.3°, and the full width at half maximum of the X-ray rocking curve of the aluminum nitride film along the [10-12] direction is less than 0.6°. The present application also provides a device, which includes an aluminum nitride film prepared by the preparation method provided in the present application and a functional layer, wherein the functional layer is arranged on a surface of the aluminum nitride film facing away from the substrate. In the preparation method of the aluminum nitride film provided in the present application, a protective layer is provided on the surface of the aluminum nitride layer with the first temperature away from the substrate, which is beneficial to prevent the aluminum nitride layer from decomposing during the thermal annealing process, and is beneficial to improving the crystal quality of the aluminum nitride film with the second temperature and reducing the defect density of the aluminum nitride film. In addition, the flat plate area is arranged around the recessed area, that is, when the protective layer is provided on the surface of the aluminum nitride layer away from the substrate, the flat plate area is in contact with the periphery of the aluminum nitride layer. The root mean square roughness of the surface of the flat plate area facing the aluminum nitride layer satisfies the range of 0nm<RMS≤50nm, and the surface of the flat plate area facing the aluminum nitride layer is smoother, so that the contact between the flat plate area and the aluminum nitride layer is closer, so that the recessed area is separated from the external environment, which is beneficial to inhibiting the decomposition of the aluminum nitride layer during the thermal annealing process, and is beneficial to improving the crystal quality of the aluminum nitride film, and effectively reducing the defect density of the aluminum nitride film through thermal annealing. BRIEF DESCRIPTION OF THE DRAWINGS In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the implementation will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work. FIG1 is a schematic diagram of a process for preparing an aluminum nitride thin film according to an embodiment of the present application; FIG2 is a schematic diagram of a stacked structure of a substrate, an aluminum nitride layer, and a protective layer according to an embodiment of the present application; FIG3 is a side view of a protective layer according to an embodiment of the present application; FIG4 is a schematic diagram of a stacked structure of a substrate, an aluminum nitride layer, and a protective layer according to another embodiment of the present application; FIG5 is a side view of a protective layer according to another embodiment of the present application; FIG6 is a top view of a protective layer according to an embodiment of the present application; FIG7 is a side view of a protective layer according to another embodiment of the present application; FIG8 is a schematic diagram of a stacked structure of a substrate, an aluminum nitride layer, and a protective layer according to another embodiment of the present application; FIG9 is a schematic diagram of a process for preparing a low-temperature aluminum nitride film according to an embodiment of the present application; FIG10 is a schematic diagram of the structure of an aluminum nitride film according to an embodiment of the present application; FIG11 is a schematic structural diagram of a device according to an embodiment of the present application; FIG. 12 is a schematic diagram of the structure of an ultraviolet light emitting diode according to an embodiment of the present application. Description of reference numerals: 100-aluminum nitride film, 110-aluminum nitride substrate, 111-substrate, 112-aluminum nitride layer, 130-protective layer, 131-depression area, 1311 - raised structure, 1312 - end face, 132 - main body, 133 - flat plate area, 134 - preset surface, 135 - groove, 200 - ultraviolet light emitting diode, 210 - light emitting layer, 211 - light emitting unit, 220 - driving substrate, 300 - device, 310 - functional layer. DETAILED DESCRIPTION The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application. The terms "first", "second", etc. in the specification and claims of this application and the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally includes steps or units that are not listed, or optionally includes other steps or units inherent to these processes, methods, products or devices. Reference to "embodiment" or "implementation" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiment or implementation may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments. Aluminum nitride thin film is an important underlying structure of high-performance III-nitride-based (such as aluminum gallium nitride, etc.) electronic and optoelectronic devices. Aluminum nitride layers are usually deposited on heterogeneous substrates such as silicon carbide, gallium nitride, sapphire, etc. by physical or chemical methods using heteroepitaxial methods. However, there is a certain lattice mismatch and thermal mismatch between the aluminum nitride layer and the heterogeneous substrate, and the nitrogen-aluminum covalent bond of aluminum nitride itself has a large bond energy, which makes the defect density of the aluminum nitride layer large. Therefore, it is usually necessary to thermally anneal the aluminum nitride layer. When the annealed sample is a single piece, the surface of the annealed sample with the aluminum nitride layer deposited is stacked face to face with the smooth surface of a new substrate; when the annealed sample is two pieces, the surfaces of the two annealed samples with the aluminum nitride layer deposited are stacked face to face. The above-mentioned samples are placed in a high-temperature annealing furnace, and thermally annealed in a nitrogen atmosphere at an annealing temperature ranging from 1373.15K to 2073.15K (for example, 1373.15K, 1573.15K, 1973.15K or 2073.15K, etc.), to finally obtain an aluminum nitride film. In the preparation process of the above aluminum nitride film, nitrogen is used as the protective gas for thermal annealing. Due to the stable nature of nitrogen, it cannot decompose and provide -N groups at the thermal annealing temperature of 1373.15K to 2073.15K, making it impossible to suppress the decomposition of the aluminum nitride layer into -Al and -N at the thermal annealing temperature of 1373.15K to 2073.15K, so that the crystal quality of the aluminum nitride film obtained is still poor and there is still a large defect density. In addition, during the thermal annealing process, when the annealing sample is a single piece, the aluminum nitride layer will partially adhere to the new smooth substrate after the annealing is completed; when the annealing sample is two pieces, the aluminum nitride layers of the two samples will adhere together after the annealing is completed, making the surface morphology of the final aluminum nitride film uneven, which is not conducive to the further preparation of high-performance devices. Referring to FIG. 1 to FIG. 3 , an embodiment of the present application provides a method for preparing an aluminum nitride film 100 , the method comprising: S101, providing an aluminum nitride substrate 110, wherein the aluminum nitride substrate 110 includes a stacked substrate 111 and an aluminum nitride layer 112 having a first temperature. Optionally, the material of the substrate 111 includes at least one of silicon, silicon carbide, gallium nitride and aluminum oxide. Preferably, in some embodiments, the material of the substrate 111 is aluminum oxide. It can be understood that the value of the first temperature Ta satisfies the range of 723.15K≤Ta≤1873.15K. Specifically, the value of the first temperature Ta can be, but is not limited to, 723.15K, 773.15K, 793.15K, 813.15K, 853.15K, 873.15K, 933.15K, 953.15K, 973.15K, 993.15K, 1073.15K, 1133.15K, 1193.15K, 1273.15K, 1333.15K, 1393.15K, 1473.15K, 1533.15K, 1593.15K, 1673.15K, 1733.15K, 1793.15K, 1873.15K, etc. S102, a protective layer 130 is disposed on the surface of the aluminum nitride layer 112 facing away from the substrate 111, the protective layer 130 includes a recessed area 131 and a flat area 133 disposed around the recessed area 131, and the root mean square roughness RMS of the surface of the flat area 133 facing the aluminum nitride layer 112 is in the range of 0nm<RMS≤50nm. It can be understood that the protective layer includes a main body 132 having a preset surface 134 facing the aluminum nitride layer 112 and a groove 135 recessed in the preset surface 134 , the recessed area 131 covers the groove 135 , and the flat sheet area 133 is arranged around the periphery of the groove 135 . It can be understood that in the embodiment of the present application, the substrate 111, the aluminum nitride layer 112 and the protective layer 130 are stacked in sequence. In other words, the surface of the substrate 111 on which the aluminum nitride layer 112 is deposited is placed opposite to the side of the protective layer 130 on which the flat plate area 133 and the recessed area 131 are provided, so as to prevent the nitrogen and aluminum elements in the aluminum nitride layer 112 from evaporating from the surface of the aluminum nitride layer 112 during the thermal annealing process, thereby inhibiting the decomposition of the aluminum nitride layer 112. Specifically, the root mean square roughness RMS value of the surface of the flat area 133 facing the aluminum nitride layer 112 can be but is not limited to 0.1nm, 1nm, 1.6nm, 3nm, 5nm, 8nm, 10nm, 12nm, 15nm, 18nm, 20nm, 22nm, 25nm, 28nm, 33nm, 37nm, 39nm, 42nm, 43nm, 46nm and 50nm, etc. When the root mean square roughness RMS value of the surface of the flat area 133 facing the aluminum nitride layer 112 satisfies the range of 0nm<RMS≤50nm, the contact between the flat area 133 and the aluminum nitride layer 112 is closer, which is beneficial to separate the recessed area 131 from the outside, and is beneficial to inhibiting the evaporation of nitrogen and aluminum elements in the aluminum nitride layer 112 from the surface of the aluminum nitride layer 112 during the thermal annealing process, thereby inhibiting the decomposition of the aluminum nitride layer 112, which is beneficial to improving the crystal quality of the aluminum nitride film 100, and is also beneficial to the peeling of the aluminum nitride film 100 and the protective layer 130 after thermal annealing. When the root mean square roughness RMS value of the surface of the flat area 133 facing the aluminum nitride layer 112 is greater than 50nm, the surface of the flat area 133 facing the aluminum nitride layer 112 is relatively rough, the protective layer 130 is difficult to be in close contact with the aluminum nitride layer 112, and it is difficult to separate the recessed area 131 from the external environment, which is not conducive to inhibiting the evaporation of nitrogen and aluminum elements in the aluminum nitride layer 112 from the surface of the aluminum nitride layer 112 during the thermal annealing process, thereby reducing the crystal quality of the aluminum nitride film 100 and making it difficult to effectively reduce the defect density of the aluminum nitride film 100 through thermal annealing treatment. S103, performing thermal annealing on the aluminum nitride substrate 110 and the protective layer 130 to obtain the aluminum nitride film 100 having a second temperature; wherein the second temperature is greater than the first temperature. It can be understood that the value of the second temperature Tb satisfies the range of 773.15K≤Tb≤2273.15K. Specifically, the value of the second temperature Tb may be, but is not limited to, 773.15K, 823.15K, 873.15K, 1000.15K, 1078.15K, 1098.15K, 1123.15K, 1173.15K, 1223.15K, 1273.15K, 1300.15K, 1323.15K, 1350.15K, 1373.15K, 1393.15K, 1473.15K, 1533.15K, 1593.15K, 1673.15K, 1733.15K, 1793.15K, 1873.15K, 1973.15K, 2073.15K, 2173.15K, and 2273.15K. In the embodiment of the present application, a protective layer 130 is provided on the surface of the aluminum nitride layer 112 with the first temperature away from the substrate 111, which is beneficial to prevent the aluminum nitride layer 112 from decomposing during the thermal annealing process. The crystal quality of the aluminum nitride film 100 having the second temperature is improved and the defect density of the aluminum nitride film 100 is reduced. In addition, the flat plate area 133 is arranged around the recessed area 131, that is, when the protective layer 130 is arranged on the surface of the aluminum nitride layer 112 away from the substrate 111, the flat plate area 133 is in contact with the periphery of the aluminum nitride layer 112, and the recessed area 131 is in contact with the area of ​​the aluminum nitride layer 112 away from the periphery. In other words, the recessed area 131 is in contact with the middle area of ​​the aluminum nitride layer 112. The root mean square roughness of the surface of the flat area 133 facing the aluminum nitride layer 112 satisfies the range of 0nm<RMS≤50nm, and the surface of the flat area 133 facing the aluminum nitride layer 112 is smoother, so that the contact between the flat area 133 and the aluminum nitride layer 112 is closer, and the recessed area 131 is separated from the external environment, which is beneficial to inhibiting the evaporation of nitrogen and aluminum elements in the aluminum nitride layer 112 from the surface of the aluminum nitride layer 112 during the thermal annealing process, thereby inhibiting the decomposition of the aluminum nitride layer 112, which is beneficial to improving the crystal quality of the aluminum nitride film 100, and effectively reducing the defect density of the aluminum nitride film 100 through thermal annealing treatment. Optionally, in some embodiments, the substrate 111 is a patterned substrate 111. The patterned substrate 111 can change the aluminum nitride layer 112 from longitudinal epitaxy to lateral epitaxy, which can effectively reduce the dislocation density of the aluminum nitride layer 112. When the aluminum nitride film 100 is applied to optoelectronic devices, the aluminum nitride layer 112 with a smaller dislocation density can reduce the non-radiative recombination of the active region and reduce the reverse leakage current, thereby extending the service life of the optoelectronic device; in addition, the light emitted from the active region is scattered multiple times at the interface between the aluminum nitride layer 112 and the patterned substrate 111, and the emission angle of the total reflected light changes, which increases the probability of the light of the flip-chip optoelectronic device being emitted from the substrate 111, thereby improving the light extraction efficiency. Optionally, in some other embodiments, the substrate 111 is a flat substrate 111. Compared with the patterned substrate 111, the flat substrate 111 has a simple preparation process and a low cost, but the performance of the prepared device 300 is relatively poor. When the flat substrate 111 and the aluminum nitride layer 112 are stacked, the aluminum nitride layer 112 is longitudinally epitaxially grown on the substrate 111, so that the dislocation density of the aluminum nitride layer 112 is large, which is not conducive to the preparation of a high-performance aluminum nitride film 100. Optionally, in some embodiments, the thickness h1 of the substrate 111 is in the range of 200 μm ≤ h1 ≤ 1500 μm. Specifically, the thickness h1 of the substrate 111 may be, but is not limited to, 200 μm, 220 μm, 250 μm, 280 μm, 300 μm, 320 μm, 350 μm, 380 μm, 400 μm, 450 μm, 480 μm, 500 μm, 530 μm, 560 μm, 600 μm, 650 μm, 800 μm, 900 μm, 1150 μm, 1200 μm, 1300 μm, 1500 μm, etc. In the embodiment of the present application, when the thickness h1 of the substrate 111 satisfies the range of 200 μm ≤ h1 ≤ 1500 μm, the thickness of the substrate 111 is within a reasonable range, so that after the thermal annealing treatment is completed, the substrate 111 is easy to be peeled off from the aluminum nitride layer 112. When the thickness h1 of the substrate 111 is less than 200 μm, the thickness of the substrate 111 is too small, and after the thermal annealing treatment is completed, the substrate 111 is difficult to be peeled off from the aluminum nitride layer 112, resulting in poor surface uniformity of the prepared aluminum nitride film 100. When the thickness h1 of the substrate 111 is greater than 1500 μm, the thickness of the substrate 111 is too large, which will increase the production cost of the substrate 111. Optionally, in some embodiments, the range of the thickness h2 of the protective layer 130 is: 100μm≤h2≤800μm. Specifically, the value of the thickness h2 of the protective layer 130 can be, but is not limited to, 100μm, 150μm, 200μm, 220μm, 250μm, 280μm, 300μm, 320μm, 350μm, 380μm, 400μm, 430μm, 450μm, 480μm, 500μm, 560μm, 600μm, 650μm, 750μm, 800μm, etc. It can be understood that the thickness h2 of the protective layer 130 refers to the maximum distance between two opposite surfaces of the protective layer 130 along the stacking direction of the protective layer 130 and the substrate 111 . In the embodiment of the present application, when the thickness h2 of the protective layer 130 satisfies the range of 100μm≤h2≤800μm, the thickness of the protective layer 130 is within a reasonable range, so that after the thermal annealing treatment is completed, the protective layer 130 is easy to peel off from the aluminum nitride layer 112. When the thickness h2 of the protective layer 130 is less than 100μm, the thickness of the protective layer 130 is too small. After the thermal annealing treatment is completed, the protective layer 130 is difficult to peel off from the aluminum nitride layer 112, resulting in poor surface uniformity of the prepared aluminum nitride film 100. When the thickness h2 of the protective layer 130 is greater than 800μm, the thickness of the protective layer 130 is too small. The production cost of the protective layer 130 will be increased. In some embodiments, providing the aluminum nitride substrate 110 includes: providing a substrate 111; depositing an aluminum nitride layer 112 having a first temperature on the surface of the substrate 111 using a physical or chemical method, and the deposition method may be but is not limited to sputtering, atomic layer deposition, molecular beam epitaxy, chemical vapor deposition, pulsed laser deposition, etc. In an embodiment of the present application, the aluminum nitride substrate 110 includes a substrate 111 and an aluminum nitride layer 112 having a first temperature which are stacked in sequence. One of the surfaces of the substrate 111 is a surface to be deposited. The aluminum nitride layer 112 having a first temperature is deposited on the surface to be deposited of the substrate 111 by one of the methods such as sputtering, atomic layer deposition, molecular beam epitaxy, chemical vapor deposition, and pulsed laser deposition. This is beneficial for providing a good substrate for the protective layer 130, so that the protective layer 130 is further deposited on the surface of the aluminum nitride layer 112 away from the substrate 111. Preferably, in some embodiments, the method for depositing the aluminum nitride layer 112 on the surface of the substrate 111 is metal organic chemical vapor deposition, which can deposit the aluminum nitride layer 112 at a faster speed, and the deposited aluminum nitride layer 112 has good uniformity and repeatability. Please refer to Figures 4 to 6. In some embodiments, the protective layer 130 also includes one or more protruding structures 1311, one of the protruding structures 1311 is arranged on the surface of the recessed area 131 facing the aluminum nitride layer 112, and multiple protruding structures 1311 are arranged at intervals on the surface of the recessed area 131 facing the aluminum nitride layer 112, the protruding structure 1311 has an end face 1312 facing the aluminum nitride layer, the flat area 133 has a preset surface 134 facing the aluminum nitride layer 112, and the end face 1312 is not higher than the preset surface 134. In other words, the protective layer 130 includes a main body 132 and at least one protruding structure 1311, the main body 132 has a preset surface 134 facing the aluminum nitride layer 112 and a groove 135 recessed in the preset surface 134, the protruding structure 1311 is arranged at intervals in the groove 135, and the protruding structure 1311 has an end face 1312 facing the aluminum nitride layer 112, and the end face 1312 is not higher than the preset surface 134. Optionally, in some embodiments, the preset surface 134 is coplanar with the end surface 1312. In other words, the preset surface 134 is flush with the end surface 1312. In other embodiments, the end surface 1312 is lower than the preset surface 134. Optionally, the recessed area 131 and the raised structure 1311 are obtained by etching a flat sheet, and the end surface 1312 may be made not higher than the preset surface 134 by grinding, polishing, etc. In an embodiment of the present application, the protruding structure 1311 is arranged in the recessed area 131, and the end face 1312 of the protruding structure 1311 is not higher than the preset surface 134, so that when the protective layer 130 is arranged on the surface of the aluminum nitride layer 112 away from the substrate 111, the protective layer 130 can be smoothly stacked with the aluminum nitride layer 112, avoiding the unevenness of the aluminum nitride substrate 110 caused by the uneven surface of the protective layer 130 facing the aluminum nitride, thereby improving the surface uniformity of the aluminum nitride film 100, which is conducive to further preparing a high-performance device 300; in addition, the recessed area 131 can be separated from the external environment, which is conducive to inhibiting the decomposition of the aluminum nitride layer 112 during the thermal annealing process, and is conducive to improving the crystal quality of the aluminum nitride film 100, and effectively reducing the defect density of the aluminum nitride film 100 through thermal annealing treatment. When the preset surface 134 is lower than the end face 1312, the aluminum nitride layer 112 cannot be in close contact with the flat plate area 133, so that the recessed area 131 cannot be effectively separated from the external environment, which is not conducive to inhibiting the decomposition of the aluminum nitride layer 112 during the thermal annealing process, reducing the crystal quality of the aluminum nitride film 100, and it is difficult to effectively reduce the defect density of the aluminum nitride film 100 through thermal annealing. Furthermore, when the protective layer 130 includes one protruding structure 1311, it is beneficial to save raw materials and simplify the assembly process. When the protective layer 130 includes a plurality of protruding structures 1311, compared with the solution of only providing one protruding structure 1311, the plurality of protruding structures 1311 can provide support for the aluminum nitride 112, which is beneficial to improving the surface uniformity of the aluminum nitride film 100. It can be understood that the recessed area 131 faces the surface of the aluminum nitride layer 112 and the multiple protruding structures 1311 are arranged at intervals, and the roughness of the recessed area 131 is greater than that of the flat area 133; in other words, the flat area 133 is smoother than the recessed area 131. Optionally, the protruding structure 1311 may be, but is not limited to, a cone, a pyramid, a frustum, or the like. Preferably, the protruding structure 1311 is a cone. Compared with other protruding structures 1311, the cone can minimize the contact area between the recessed area 131 and the aluminum nitride layer 112, increase the roughness of the recessed area 131, and the manufacturing process of the cone is simple, which is conducive to reducing the manufacturing cost of the recessed area 131. Optionally, in some embodiments, the value of the height difference h3 between the preset surface 134 and the end surface 1312 satisfies 0nm≤h3≤50nm. Specifically, the value of the height difference h3 between the preset surface 134 and the end surface 1312 may be, but is not limited to, 0nm, 5nm, 8nm, 15nm, 18nm, 20nm, 25nm, 28nm, 30nm, 35nm, 38nm, 40nm, 43nm, 45nm, 50nm, etc. In an embodiment of the present application, the value of the height difference h3 between the preset surface 134 and the end face 1312 satisfies the range of 0nm≤h3≤50nm, so that the end face 1312 of the protruding structure 1311 can provide support for the aluminum nitride layer 112, so that the aluminum nitride layer 112 will not be deformed due to its own gravity during the thermal annealing process, so that the prepared aluminum nitride film 100 has good surface uniformity. In addition, the end face 1312 of the protruding structure 1311 is lower than the preset surface 134, so that the contact area between the protruding structure 1311 of the recessed area 131 and the aluminum nitride layer 112 is small or almost zero, thereby reducing the contact area between the protective layer 130 and the aluminum nitride layer 112, so that the bonding force between the aluminum nitride layer 112 and the protective layer 130 is small. After the thermal annealing process is completed, the probability of adhesion between the aluminum nitride layer 112 and the protective layer 130 is reduced, so that the surface of the aluminum nitride film 100 has a higher surface uniformity, which is conducive to the further preparation of high-performance devices 300. In some embodiments, when the aluminum nitride substrate 110 and the protective layer 130 are tightly stacked together, the recessed area 131 of the protective layer 130 in the orthographic projection area of ​​the surface away from the aluminum nitride layer 112 and the orthographic projection of the surface of the protective layer 130 away from the aluminum nitride layer 112 are concentric circle structures, the diameter of the recessed area 131 in the orthographic projection area of ​​the surface of the protective layer 130 away from the aluminum nitride layer 112 is D1, and the diameter of the surface of the protective layer 130 away from the aluminum nitride layer 112 is D2, then 0.6D2≤D1≤0.95D2. Specifically, the diameter D1 of the recessed area 131 may be, but is not limited to, 0.6D2, 0.63D2, 0.68D2, 0.71D2, 0.74D2, 0.78D2, 0.81D2, 0.83D2, 0.84D2, 0.86D2, 0.89D2, 0.93D2, and 0.95D2. When the diameter D1 of the orthographic projection area of ​​the recessed area 131 on the surface of the protective layer 130 away from the aluminum nitride layer 112 and the diameter D2 of the surface of the protective layer 130 away from the aluminum nitride layer 112 satisfy the condition 0.6D2≤D1≤0.95D2, the area of ​​the recessed area 131 and the area of ​​the flat area 133 are within a reasonable range, so that the flat area 133 can be in close contact with the protective layer 130 to inhibit the decomposition of the aluminum nitride layer 112 during thermal annealing, and the recessed area 131 can improve the adhesion between the aluminum nitride layer 112 and the protective layer 130, so that the prepared aluminum nitride film 100 has high crystal quality, low defect density, lower cost and high surface uniformity. When the diameter D1 of the recessed area 131 is less than 0.6D2, the diameter of the recessed area 131 is too small, so that the area of ​​the recessed area 131 is small. In the process of thermal annealing, the effect of the recessed area 131 in improving the adhesion between the aluminum nitride layer 112 and the protective layer 130 is not good and a smaller device 300 area is formed, so that the surface uniformity of the aluminum nitride film 100 is poor and the cost is high. When the diameter D1 of the recessed area 131 is greater than 0.95D2, the diameter of the recessed area 131 is too large, so that the area of ​​the recessed area 131 is large, and the area of ​​the flat plate area 133 is small, which is not conducive to the close contact between the protective layer 130 and the aluminum nitride layer 112. The recessed area 131 is difficult to be separated from the external environment, which is not conducive to suppressing the decomposition of the aluminum nitride layer 112 during the thermal annealing process, so that the crystal quality of the aluminum nitride film 100 is poor and the defect density is large. Preferably, in some embodiments, the diameter D1 of the recessed area 131 is 0.85D2. The area of ​​the recessed area 131 and the area of ​​the flat plate area 133 are within a reasonable range, so that the flat plate area 133 can be in close contact with the protective layer 130 to inhibit the decomposition of the aluminum nitride layer 112 during the thermal annealing process, and the recessed area 131 can improve the adhesion between the aluminum nitride layer 112 and the protective layer 130, and the prepared aluminum nitride film 100 has high crystal quality, low defect density and high surface uniformity. Optionally, in some embodiments, the plane perpendicular to the stacking direction of the substrate 111 and the aluminum nitride layer 112 is On the surface, the contact area per unit area of ​​the recessed area 131 and the aluminum nitride layer 112 is smaller than the contact area per unit area of ​​the flat area 133 and the aluminum nitride layer 112. It can be understood that the stacking direction perpendicular to the substrate 111 and the aluminum nitride layer 112 can be the thickness direction of the aluminum nitride film 100 to be processed. In the embodiment of the present application, the recessed area 131 includes one or a plurality of convex structures 1311 arranged at intervals, and the end surface 1312 of the convex structure 1311 is coplanar with the preset surface 134 of the protective layer 130, so that along the stacking direction perpendicular to the substrate 111 and the aluminum nitride layer 112, the contact area per unit area of ​​the recessed area 131 and the aluminum nitride layer 112 is smaller than the contact area per unit area of ​​the flat plate area 133 and the aluminum nitride layer 112. The contact area between the recessed area 131 and the aluminum nitride layer 112 is small, so that the bonding force between the aluminum nitride layer 112 and the protective layer 130 is small. After the thermal annealing process is completed, the probability of adhesion between the aluminum nitride layer 112 and the protective layer 130 is reduced, and the surface of the aluminum nitride film 100 has a high surface uniformity, which is conducive to the further preparation of a high-performance device 300. In some embodiments, along a plane perpendicular to the stacking direction of the substrate 111 and the aluminum nitride layer 112, the contact area per unit area of ​​the recessed area 131 and the aluminum nitride layer 112 is 9.75% to 64% of the contact area per unit area of ​​the flat plate area 133 and the aluminum nitride layer 112. Specifically, the contact area per unit area of ​​the recessed area 131 and the aluminum nitride layer 112 may be, but is not limited to, 9.75%, 10%, 15%, 17%, 19%, 21%, 25%, 29%, 33%, 38%, 45%, 48%, 50%, 56%, 60%, 64%, etc., of the contact area per unit area of ​​the flat plate area 133 and the aluminum nitride layer 112. In an embodiment of the present application, when the contact area per unit area of ​​the recessed area 131 and the aluminum nitride layer 112 is 9.75% to 64% of the contact area per unit area of ​​the flat area 133 and the aluminum nitride layer 112, the contact area per unit area of ​​the recessed area 131 and the aluminum nitride layer 112 is within a reasonable range, the processing difficulty of the protruding structure 1311 is relatively small, and the contact area between the recessed area 131 and the aluminum nitride layer 112 is relatively small. After the thermal annealing process is completed, the area where the aluminum nitride layer 112 and the protective layer 130 are adhered is relatively small, so that the obtained aluminum nitride film 100 has a higher surface uniformity. When the contact area per unit area of ​​the recessed area 131 and the aluminum nitride layer 112 is less than 9.75% of the contact area per unit area of ​​the flat plate area 133 and the aluminum nitride layer 112, the contact area per unit area of ​​the recessed area 131 and the aluminum nitride layer 112 is too small, which increases the difficulty of processing the convex structure 1311 of the recessed area 131. When the contact area per unit area of ​​the recessed area 131 and the aluminum nitride layer 112 is greater than 64% of the contact area per unit area of ​​the flat plate area 133 and the aluminum nitride layer 112, the contact area per unit area of ​​the recessed area 131 and the aluminum nitride layer 112 is too large, so that the contact area between the recessed area 131 and the aluminum nitride layer 112 is too large, and after the thermal annealing process is completed, the area where the aluminum nitride layer 112 and the protective layer 130 are adhered is relatively large, so that the surface uniformity of the obtained aluminum nitride film 100 is poor. Please refer to Figures 7 and 8. Optionally, in some embodiments, the two opposite surfaces of the protective layer 130 have a recessed area 131. In this embodiment, when thermal annealing is performed, an aluminum nitride substrate 110 can be provided on the two opposite surfaces of the protective layer 130, and the aluminum nitride layer 112 is provided facing the protective layer 130. In other words, when thermal annealing is performed, the substrate 111, the aluminum nitride layer 112, the protective layer 130, the aluminum nitride layer 112 and the substrate 111 are stacked in sequence. Compared with the solution of providing one protective layer 130 for one aluminum nitride substrate 110, in the embodiment of the present application, only one protective layer 130 is required for two aluminum nitride substrates 110, and only two protective layers 130 are required for four aluminum nitride substrates 110, and so on. This is conducive to reducing the use of half of the protective layer 130, while simplifying the assembly process of the protective layer 130 and increasing the number of samples treated by a single thermal annealing. In other words, the two opposite surfaces of the protection layer 130 both have the recessed areas 131 , which improves the utilization rate of the protection layer 130 and increases the number of aluminum nitride layers 112 that are processed by a single thermal annealing process. In some embodiments, the distance d2 between the two farthest points of the protruding structure 1311 on the area surrounded by the orthographic projection of the surface of the aluminum nitride facing the protective layer 130 is in the range of: 0.1 μm ≤ d2 ≤ 50000 μm. Specifically, the distance d2 between the two farthest points of the protruding structure 1311 on the area surrounded by the orthographic projection of the surface of the aluminum nitride facing the protective layer 130 is in the range of: 0.1 μm ≤ d2 ≤ 50000 μm. The value of the distance d2 between the two electrodes may be, but is not limited to, 0.1 μm, 0.5 μm, 1 μm, 5 μm, 10 μm, 15 μm, 17 μm, 18 μm, 20 μm, 22 μm, 24 μm, 27 μm, 28 μm, 31 μm, 33 μm, 35 μm, 37 μm, 42 μm, 45 μm, 48 μm, 50 μm, 65 μm, 80 μm, μm, 140μm, 170μm, 230μm, 450μm, 500μm, 780μm, 1000μm, 1200μm, 1500μm, 2500 μm, 3800μm, 5800μm, 8000μm, 10000μm, 15000μm, 30000μm, 40000μm and 50000μm, etc. In an embodiment of the present application, when the distance d2 between the two farthest points on the area enclosed by the orthographic projection of the protruding structure 1311 on the surface of the aluminum nitride facing the protective layer 130 satisfies the range of 0.1μm≤d2≤50000μm, the distance between the two farthest points on the area enclosed by the orthographic projection of the protruding structure 1311 is within a reasonable range, and the protruding structure 1311 in the recessed area 131 has a reasonable density, which is beneficial to the contact between the protective layer 130 and the aluminum nitride layer 112, thereby improving the surface uniformity of the aluminum nitride film 100; at the same time, the processing difficulty of the protruding structure 1311 is reduced. When the value of the distance d2 between the two farthest points on the area surrounded by the orthographic projection of the aluminum nitride surface facing the protective layer 130 of the protruding structure 1311 is less than 0.1 μm, the distance between the two farthest points on the area surrounded by the orthographic projection of the protruding structure 1311 is too small, which increases the difficulty of processing the protruding structure 1311 and makes it difficult to meet the height requirement of the protruding structure 1311, thereby affecting the surface uniformity of the aluminum nitride film 100. When the value of the distance d2 between the two farthest points on the area surrounded by the orthographic projection of the aluminum nitride surface facing the protective layer 130 of the protruding structure 1311 is greater than 50,000 μm, the protruding structure 1311 can hardly provide support for the recessed area 131 of the protective layer 130. Preferably, a distance d2 between two points of the protruding structure 1311 that are farthest apart in an area surrounded by an orthographic projection of the surface of the aluminum nitride facing the protective layer 130 is in the range of 0.1 μm≤d2≤500 μm. Specifically, the distance d2 between the two farthest points on the area surrounded by the orthographic projection of the surface of the aluminum nitride facing the protective layer 130 of the protruding structure 1311 can be, but is not limited to, 0.1 μm, 0.5 μm, 1 μm, 5 μm, 10 μm, 15 μm, 17 μm, 18 μm, 20 μm, 22 μm, 24 μm, 27 μm, 28 μm, 31 μm, 33 μm, 35 μm, 37 μm, 42 μm, 45 μm, 48 μm, 50 μm, 65 μm, 80 μm, 140 μm, 170 μm, 230 μm, 450 μm and 500 μm. When the distance d2 between the two farthest points on the area enclosed by the orthographic projection of the surface of the aluminum nitride facing the protective layer 130 of the protruding structure 1311 satisfies the range of 0.1μm≤d2≤500μm, the distance between the two farthest points on the area enclosed by the orthographic projection of the protruding structure 1311 is within a more reasonable range, and the protruding structure 1311 in the recessed area 131 has a more reasonable density, which is beneficial for the contact between the protective layer 130 and the aluminum nitride layer 112, further improving the surface uniformity of the aluminum nitride film 100; at the same time, the processing difficulty of the protruding structure 1311 is further reduced. More preferably, the distance d2 between the two farthest points of the protruding structure 1311 on the area surrounded by the orthographic projection of the surface of the aluminum nitride facing the protective layer 130 is in the range of 0.1 μm ≤ d2 ≤ 65 μm. Specifically, the value of the distance d2 between the two farthest points of the protruding structure 1311 on the area surrounded by the orthographic projection of the surface of the aluminum nitride facing the protective layer 130 can be, but is not limited to, 0.1 μm, 0.5 μm, 1 μm, 5 μm, 10 μm, 15 μm, 17 μm, 18 μm, 20 μm, 22 μm, 24 μm, 27 μm, 28 μm, 31 μm, 33 μm, 35 μm, 37 μm, 42 μm, 45 μm, 48 μm, 50 μm, 55 μm, 60 μm, 65 μm, etc. When the distance d2 between the two farthest points on the area enclosed by the orthographic projection of the surface of the aluminum nitride facing the protective layer 130 of the protruding structure 1311 satisfies the range of 0.1μm≤d2≤65μm, the distance between the two farthest points on the area enclosed by the orthographic projection of the protruding structure 1311 is within a more reasonable range, and the protruding structure 1311 in the recessed area 131 has a more reasonable density, which is beneficial to the contact between the protective layer 130 and the aluminum nitride layer 112, greatly improving the surface uniformity of the aluminum nitride film 100; at the same time, the processing difficulty of the protruding structure 1311 is greatly reduced. In some preferred embodiments, the distance d2 between the two farthest points on the area surrounded by the orthographic projection of the aluminum nitride surface facing the protective layer 130 is 27 μm. The distance between the two farthest points on the area surrounded by the orthographic projection of the convex structure 1311 is within a reasonable range, and the convex structure 1311 in the concave area 131 has a reasonable density, which is conducive to the contact between the protective layer 130 and the aluminum nitride layer 112, and improves the surface of the aluminum nitride film 100. uniformity; at the same time, the processing difficulty of the protruding structure 1311 is reduced. Optionally, in some embodiments, the protruding structure 1311 is a cone, and the distance d2 between the two farthest points on the area enclosed by the orthographic projection of the surface of the aluminum nitride facing the protective layer 130 of the protruding structure 1311 is the diameter of the bottom surface of the cone, and the diameter d2 of the bottom surface of the protruding structure satisfies the range of 0.1μm≤d2≤50000μm. Optionally, the range of the minimum distance d3 between any two adjacent protrusion structures 1311 is: 0 μm≤d3≤50000 μm. Specifically, the value of the minimum spacing d3 between any two adjacent protrusion structures 1311 can be, but is not limited to, 0μm, 1μm, 1.3μm, 2.5μm, 3.8μm, 4μm, 5.8μm, 6μm, 6.3μm, 6.8μm, 7.2μm, 7.8μm, 8.5μm, 9.5μm, 12.5μm, 13μm, 13.8μm, 15μm, 25μm, 38μm, 40μm, 58μm, 60μm, 63μm, 68μm, 72μm, 78μm, 85μm, 95μm, 100μm, 1000μm, 10000μm, 20000μm, 30000μm, 40000μm and 50000μm, etc. In the embodiment of the present application, when the value of the minimum spacing d3 between any two adjacent protrusion structures 1311 satisfies the range of 0μm≤d3≤50000μm, the minimum spacing between any two adjacent protrusion structures 1311 is within a reasonable range, and the arrangement density of the protrusion structures 1311 in the recessed area 131 is moderate, which is conducive to the contact between the recessed area 131 and the aluminum nitride layer 112 and plays a supporting role. In addition, the minimum spacing between any two adjacent protrusion structures 1311 is within a reasonable range, so that the aluminum nitride layer 112 and the protective layer 130 can contact and have a small bonding force. After the thermal annealing process is completed, the probability of adhesion between the aluminum nitride layer 112 and the protective layer 130 is reduced, and the surface of the aluminum nitride film 100 has a high surface uniformity, which is conducive to the further preparation of high-performance devices 300. When the value of the minimum spacing d3 between any two adjacent protrusion structures 1311 is 0, the protrusion structures 1311 in the recessed area 131 are arranged too closely, increasing the probability of adhesion between the aluminum nitride layer 112 and the protective layer 130; when the value of the minimum spacing d3 between any two adjacent protrusion structures 1311 is greater than 50,000 μm, the protrusion structures 1311 in the recessed area 131 are arranged too loosely, and the supporting effect between the recessed area 131 of the protective layer 130 and the aluminum nitride layer 112 is limited. Preferably, the range of the minimum spacing d3 between any two adjacent protrusion structures 1311 is: 0μm≤d3≤100μm. Specifically, the value of the minimum spacing d3 between any two adjacent protrusion structures 1311 can be, but is not limited to, 0μm, 1μm, 1.3μm, 2.5μm, 3.8μm, 4μm, 5.8μm, 6μm, 6.3μm, 6.8μm, 7.2μm, 7.8μm, 8.5μm, 9.5μm, 12.5μm, 13μm, 13.8μm, 15μm, 25μm, 38μm, 40μm, 58μm, 60μm, 63μm, 68μm, 72μm, 78μm, 85μm, 95μm and 100μm, etc. When the minimum distance d3 between any two adjacent protrusion structures 1311 satisfies the range of 0 μm≤d3≤100 μm, it is beneficial to further improve the surface uniformity of the aluminum nitride film 100 and further prepare a high-performance device 300 . More preferably, the minimum spacing d3 between any two adjacent protrusion structures 1311 is in the range of 0μm≤d3≤15μm. Specifically, the value of the minimum spacing d3 between any two adjacent protrusion structures 1311 may be, but is not limited to, 0μm, 1μm, 1.3μm, 2.5μm, 3.8μm, 4μm, 5.8μm, 6μm, 6.3μm, 6.8μm, 7.2μm, 7.8μm, 8.5μm, 9.5μm, 12.5μm, 13μm, 13.8μm and 15μm, etc. When the minimum spacing d3 between any two adjacent protrusion structures 1311 satisfies the range of 0μm≤d3≤15μm, it is beneficial to further improve the surface uniformity of the aluminum nitride film 100 and further prepare a high-performance device 300. In some preferred embodiments, the minimum spacing between any two adjacent protrusion structures 1311 is 4 μm. The minimum spacing between any two adjacent protrusion structures 1311 is within a reasonable range, the arrangement density of the protrusion structures 1311 in the recessed area 131 is moderate, the aluminum nitride layer 112 and the protective layer 130 can be effectively in contact and the bonding force between the two is small, which is conducive to improving the surface uniformity of the aluminum nitride surface. After the thermal annealing process is completed, the probability of adhesion between the aluminum nitride layer 112 and the protective layer 130 is reduced, and the surface of the aluminum nitride film 100 has a high surface uniformity, which is conducive to further preparing a high-performance device 300. In some embodiments, along the stacking direction of the substrate 111 and the aluminum nitride layer 112, the protruding structure 1311 The range of the maximum height d4 is: 0μm<d4≤200μm. Specifically, the value of the maximum height d4 of the protruding structure 1311 can be, but is not limited to, 0.2μm, 3μm, 5μm, 8μm, 10μm, 12μm, 14μm, 15μm, 17μm, 21μm, 22μm, 24μm, 26μm, 27μm, 28μm, 30μm, 35μm, 38μm, 40μm, 42μm, 45μm, 48μm, 50μm, 58μm, 75μm, 89μm, 100μm, 110μm, 135μm, 155μm, 165μm, 178μm, 186μm, 190μm, 195μm and 200μm, etc. It can be understood that the stacking direction along the substrate 111 and the aluminum nitride layer 112 may be the thickness direction of the aluminum nitride film 100 to be processed. It can be understood that the maximum height of the protruding structure 1311 can be the distance from the end of the protruding structure 1311 farthest from the recessed area 131 to the surface of the recessed area 131 facing the aluminum nitride layer 112 along the stacking direction of the substrate 111 and the aluminum nitride layer 112. In an embodiment of the present application, when the value of the maximum height d4 of the protruding structure 1311 satisfies the range of 0μm<d4≤200μm, the maximum height of the protruding structure 1311 is within a reasonable range, and the aluminum nitride layer 112 can be tightly combined with the recessed area 131 and the flat area 133, so that the recessed area 131 is effectively separated from the external environment, which is beneficial to inhibiting the decomposition of the aluminum nitride layer 112 during the thermal annealing process, thereby improving the crystal quality of the aluminum nitride film 100, and the defect density of the aluminum nitride film 100 can be effectively reduced and the surface uniformity of the aluminum nitride film 100 can be improved through thermal annealing treatment. When the maximum height d4 of the protruding structure 1311 is greater than 200 μm, the maximum height of the protruding structure 1311 is too large, making it difficult for the aluminum nitride layer 112 to be in close contact with the flat area 133, and making it impossible to effectively separate the recessed area 131 from the external environment, which is not conducive to inhibiting the decomposition of the aluminum nitride layer 112 during the thermal annealing process, reduces the crystal quality of the aluminum nitride film 100, and makes it difficult to effectively reduce the defect density of the aluminum nitride film 100 through thermal annealing treatment. Preferably, the maximum height d4 of the protruding structure 1311 is in the range of 0 μm < d4 ≤ 50 μm. Specifically, the maximum height d4 of the protruding structure 1311 may be, but is not limited to, 0.2 μm, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 14 μm, 15 μm, 17 μm, 21 μm, 22 μm, 24 μm, 26 μm, 27 μm, 28 μm, 30 μm, 35 μm, 38 μm, 40 μm, 42 μm, 45 μm, 48 μm, 50 μm, etc. In some preferred embodiments, the maximum height d4 of the protruding structure 1311 is 17 μm. The maximum height of the protruding structure 1311 is within a reasonable range, and the aluminum nitride layer 112 can be closely combined with the recessed area 131 and the flat plate area 133, so that the recessed area 131 is effectively separated from the external environment, which is beneficial to inhibiting the decomposition of the aluminum nitride layer 112 during the thermal annealing process, improving the crystal quality and surface uniformity of the aluminum nitride film 100, and effectively reducing the defect density of the aluminum nitride film 100. Optionally, in some embodiments, the protruding structure 1311 is a cone, and the maximum height of the protruding structure 1311 is the height of the cone. In some embodiments, the thermal annealing of the aluminum nitride substrate 110 and the protective layer 130 includes: performing the thermal annealing in an ammonia atmosphere. The substrate 111, the aluminum nitride layer 112 and the protective layer 130 stacked in sequence are subjected to thermal annealing at high temperature, and the aluminum nitride layer 112 is thermally decomposed into -Al groups and -N groups at high temperature. In an embodiment of the present application, the thermal annealing process is carried out in an ammonia atmosphere, and the aluminum nitride layer 112 can be decomposed into groups such as -N and -NH2 at high temperature, so that there are saturated -N groups in the ambient atmosphere of the thermal annealing treatment. The saturated -N group can effectively inhibit the decomposition of the aluminum nitride layer 112 at high temperature, which is beneficial to improving the crystal quality of the aluminum nitride film 100, and the defect density of the aluminum nitride film 100 is effectively reduced by thermal annealing to obtain an aluminum nitride film 100 with a low defect density. In some embodiments, the thermal annealing of the aluminum nitride substrate and the protective layer includes: performing the thermal annealing in an ammonia atmosphere at a temperature T2 in the range of 773.15K≤T2≤2273.15K. Specifically, the temperature of the thermal annealing can be, but is not limited to, 773.15K, 823.15K, 873.15K, 923.15K, 973.15K, 1023.15K, 1073.15K, 1123.15K, 1273.15K, 1323.15K, 1473.15K, 1573.15K, 1623.15K, 1673.15K, 1723.15K, 1773.15K, 1823.15K, 1873.15K, 1923.15K, 1973.15K, 2023.15K, 2073.15K, 2123.15K, 2173.15K, 2223.15K and 2273.15K, etc. In the embodiment of the present application, when the value of the thermal annealing temperature T2 satisfies the range of 773.15K≤T2≤2273.15K, the temperature of the thermal annealing is within a reasonable range, so that the aluminum nitride film 100 can be fully recrystallized during the thermal annealing process, and the defect density of the aluminum nitride film 100 is effectively reduced during the thermal annealing process, so that the defect density of the aluminum nitride film 100 is relatively small. When the value of the thermal annealing temperature T2 is less than 773.15K, the temperature of the thermal annealing is too low, and it is difficult for the aluminum nitride film 100 to fully recrystallize during the thermal annealing process, and it is difficult to achieve the purpose of reducing the defect density of the aluminum nitride film 100, so that the defect density of the aluminum nitride film 100 is relatively large. When the value of the thermal annealing temperature T2 is greater than 2273.15K, the temperature of the thermal annealing is too high, and cracks are likely to appear on the surface of the aluminum nitride film 100, which in turn affects the normal use of the aluminum nitride film 100, and is not conducive to further preparing a high-performance device 300. Preferably, in some embodiments, the thermal annealing treatment is performed in an ammonia atmosphere at a temperature T2 of 2073.15 K. The thermal annealing temperature is relatively high, so that the aluminum nitride film 100 can be fully recrystallized during the thermal annealing process, and the defect density of the aluminum nitride film 100 is effectively reduced during the thermal annealing process, and the crystal quality of the aluminum nitride film 100 is improved. In addition, the surface of the aluminum nitride film 100 is not prone to cracks, so that the generated aluminum nitride film 100 has high crystal quality, low defect density and high surface uniformity. In some embodiments, the thermal annealing treatment includes: performing the thermal annealing treatment in an ammonia atmosphere at a thermal annealing time t1 in the range of 0min<t1≤180min. Specifically, the value of the thermal annealing time t1 can be, but is not limited to, 3min, 5min, 8min, 10min, 15min, 20min, 25min, 30min, 38min, 40min, 45min, 50min, 66min, 78min, 90min, 100min, 110min, 120min, 130min, 140min, 150min, 160min, 170min, and 180min. In the embodiment of the present application, when the value of the thermal annealing time t1 satisfies the range of 0min<t1≤180min, the thermal annealing time is within a reasonable range, the aluminum nitride film 100 can achieve sufficient recrystallization, and the surface uniformity of the aluminum nitride film 100 can be maintained, and the purpose of reducing the defect density of the aluminum nitride film 100 is achieved through thermal annealing. When the value of the thermal annealing time t1 is greater than 180min, the thermal annealing time is too long, making the surface of the aluminum nitride film 100 too rough, which is not conducive to further preparing a high-performance device 300. Preferably, in some embodiments, the thermal annealing treatment is performed in an ammonia atmosphere at a thermal annealing time t1 of 90 minutes. When the thermal annealing time is within a reasonable range, the aluminum nitride film 100 can be fully recrystallized and the surface uniformity of the aluminum nitride film 100 can be maintained, thereby obtaining an aluminum nitride film 100 with a lower defect density. Referring to FIG. 9 , in some embodiments, providing an aluminum nitride substrate 110 includes: S1011, provide a substrate 111. Optionally, the material of the substrate 111 includes at least one of silicon, silicon carbide, aluminum oxide, etc. Preferably, the material of the substrate 111 is aluminum nitride. Optionally, the thickness of the substrate 111 is in the range of 200 μm ≤ h1 ≤ 1500 μm. The thickness of the substrate 111 being within a reasonable range is conducive to producing an aluminum nitride layer 112 of good quality and saving production costs. S1012, a chemical vapor deposition method is used to deposit an aluminum nitride layer 112 with a first temperature on the surface of the substrate 111, and the temperature T1 ranges from 723.15K≤T1≤1873.15K; the reaction pressure P1 ranges from 0Torr<P1≤800Torr, and the thickness d1 of the deposited aluminum nitride layer 112 ranges from 0nm<d1≤1000nm; wherein the chemical vapor deposition method is a metal organic chemical vapor deposition method. In the embodiment of the present application, the aluminum nitride layer 112 having a first temperature is deposited on the surface of the substrate 111 by using a metal organic compound vapor deposition method, and the temperature T1 is in the range of: 723.15K≤T1≤1873.15K; at the reaction pressure P1 The range is: 0Torr<P1≤800Torr, and the aluminum nitride layer 112 is deposited on the surface of the substrate 111, so that the deposited aluminum nitride layer 112 has good quality and surface uniformity, which is conducive to further preparing a high-performance aluminum nitride substrate 110. In addition, the deposition speed of the aluminum nitride layer 112 is fast and the deposition efficiency is high, which is conducive to improving the deposition efficiency of the aluminum nitride substrate 110. In an embodiment of the present application, the method for depositing the aluminum nitride layer 112 on the surface of the substrate 111 is a metal organic chemical vapor deposition method. The speed of depositing the aluminum nitride layer 112 by the method is fast, and the deposited aluminum nitride layer 112 has good uniformity and repeatability. It can be understood that when the value of the temperature T1 satisfies the range of 723.15K≤T1≤1873.15K, the temperature of depositing the aluminum nitride layer 112 on the surface of the substrate 111 is within a reasonable range, so that the deposited aluminum nitride layer 112 has good quality and surface uniformity. When the value of the temperature T1 is less than 723.15K, the temperature of depositing the aluminum nitride layer 112 on the surface of the substrate 111 is too low, so that the quality of the deposited aluminum nitride layer 112 is poor; when the value of the temperature T1 is greater than 1873.15K, the temperature of depositing the aluminum nitride layer 112 on the surface of the substrate 111 is too high, so that the surface of the deposited aluminum nitride layer 112 is prone to cracks, and it is not easy to further prepare a high-performance aluminum nitride substrate 110. Specifically, the value of the temperature T1 may be, but is not limited to, 723.15K, 823.15K, 873.15K, 923.15K, 973.15K, 1023.15K, 1073.15K, 1123.15K, 1173.15K, 1223.15K, 1273.15K, 1323.15K, 1373.15K, 1423.15K, 1473.15K, 1523.15K, 1573.15K, 1623.15K, 1673.15K, 1723.15K, 1773.15K, 1823.15K, 1873.15K, etc. Preferably, the value of the temperature T1 is 1373.15K. The aluminum nitride layer 112 deposited at this temperature has good quality and surface uniformity. It can be understood that when the value of the reaction pressure P1 satisfies the range of 0Torr<P1≤800Torr, the reaction pressure of depositing the aluminum nitride layer 112 on the surface of the substrate 111 is within a reasonable range, so that the aluminum nitride layer 112 has good quality and a high deposition rate. When the value of the reaction pressure P1 is greater than 800Torr, the reaction pressure of depositing the aluminum nitride layer 112 on the surface of the substrate 111 is too high, so that the deposition rate of the aluminum nitride layer 112 on the surface of the substrate 111 is slowed down, and the efficiency of depositing the aluminum nitride layer 112 on the surface of the substrate 111 is reduced. Specifically, the value of the reaction pressure P1 can be, but is not limited to, 0.001 Torr, 0.004 Torr, 0.01 Torr, 0.1 Torr, 1 Torr, 10 Torr, 20 Torr, 30 Torr, 40 Torr, 45 Torr, 50 Torr, 60 Torr, 70 Torr, 80 Torr, 90 Torr, 100 Torr, 150 Torr, 200 Torr, 230 Torr, 300 Torr, 350 Torr, 390 Torr, 420 Torr, 470 Torr, 550 Torr, 610 Torr, 650 Torr, 720 Torr, 750 Torr, and 800 Torr, etc. Preferably, the value of the reaction pressure P1 is 50 Torr. The aluminum nitride layer 112 deposited under this reaction pressure has good quality and a faster deposition rate. Optionally, in some embodiments, the thickness d1 of the aluminum nitride layer 112 deposited on the surface of the substrate 111 is in the range of 0nm<d1≤1000nm. When the thickness d1 of the aluminum nitride layer 112 deposited on the surface of the substrate 111 satisfies the range of 0nm<d1≤1000nm, the aluminum nitride layer 112 has good quality and surface uniformity. When the thickness of the aluminum nitride layer 112 is greater than 1000nm, the aluminum nitride layer 112 is too thick, and the probability of cracks on the surface of the aluminum nitride layer 112 due to stress increases, which is not conducive to further preparing a high-performance aluminum nitride substrate 110. Specifically, the value of the thickness d1 of the aluminum nitride layer 112 deposited on the surface of the substrate 111 may be, but is not limited to, 10 nm, 50 nm, 60 nm, 100 nm, 150 nm, 200 nm, 320 nm, 400 nm, 450 nm, 500 nm, 650 nm, 700 nm, 750 nm, 800 nm, 860 nm, 890 nm, 900 nm, 950 nm, 980 nm, and 1000 nm. Preferably, the value of the thickness d1 of the aluminum nitride layer 112 deposited on the surface of the substrate 111 is 600 nm. The thickness of the aluminum nitride layer 112 is moderate, and the aluminum nitride layer 112 has good quality and surface uniformity. Optionally, in some embodiments, before the thermal annealing treatment is performed, the root mean square roughness of the surface of the aluminum nitride layer 112 away from the substrate 111 is greater than or equal to 3.3 nm. Specifically, the root mean square roughness of the surface of the aluminum nitride layer 112 away from the substrate 111 may be, but is not limited to, 3.3 nm, 3.4 nm, 3.5 nm, 3.6 nm, 3.7 nm, 3.9 nm, 4.0 nm, 4.1 nm, 4.2 nm, 4.4 nm, 4.5 nm, 4.6 nm, 4.8 nm, 4.9 nm, 5.0 nm, 5.1 nm, etc. It can be understood that the root mean square roughness of the surface of the aluminum nitride layer 112 away from the substrate 111 reflects the roughness of the surface of the aluminum nitride layer 112 away from the substrate 111. The greater the root mean square roughness of the surface of the aluminum nitride layer 112 away from the substrate 111, the rougher the surface of the aluminum nitride layer 112 away from the substrate 111, and the worse the surface uniformity of the aluminum nitride layer 112 away from the substrate 111; the smaller the root mean square roughness of the surface of the aluminum nitride layer 112, the smoother the surface of the aluminum nitride layer 112 away from the substrate 111, and the better the surface uniformity of the aluminum nitride layer 112 away from the substrate 111. In the embodiment of the present application, the surface roughness of the aluminum nitride layer 112 is relatively large, and the surface uniformity of the aluminum nitride layer 112 is not good enough. In some embodiments, before the thermal annealing treatment is performed, the dislocation density of the aluminum nitride layer 112 deposited on the surface of the substrate 111 is greater than or equal to 5×10 10 cm -2 Specifically, the dislocation density of the aluminum nitride layer 112 deposited on the substrate 111 may be, but is not limited to, 5×10 10 cm -2 , 5.02×10 10 cm -2 , 5.3×10 10 cm -2 , 6.5×10 10 cm -2 , 7.3×10 10 cm -2 , 7.8×10 10 cm -2 8.0×10 10 cm -2 , 9.1×10 10 cm -2 and 9.3×10 10 cm -2 wait. It can be understood that the dislocation density refers to the number of distortions per unit area, and the greater the dislocation density, the worse the crystal quality of the aluminum nitride layer 112; the smaller the dislocation density, the better the crystal quality of the aluminum nitride layer 112. In the embodiment of the present application, the aluminum nitride layer 112 deposited on the surface of the substrate 111 still has a large dislocation density, the defect density of the aluminum nitride layer 112 is large, and the crystal quality is poor. In some embodiments, before the thermal annealing treatment is performed, the half-maximum full width of the X-ray rocking curve of the aluminum nitride layer 112 along the

[0002] direction is greater than or equal to 0.46°. Specifically, the half-maximum full width of the X-ray rocking curve of the aluminum nitride layer 112 along the

[0002] direction may be, but is not limited to, 0.46°, 0.47°, 0.48°, 0.50°, 0.52°, 0.54°, 0.56°, 0.58°, 0.6°, 0.62°, 0.70°, 0.85°, 0.95°, 1.05°, etc. It can be understood that the full width at half maximum of the aluminum nitride layer 112 in different directions can be obtained by X-ray rocking curve testing to obtain the size of the grains in the aluminum nitride layer 112. When the full width at half maximum of the aluminum nitride layer 112 is smaller, the grains in the aluminum nitride layer 112 are larger, and the crystal quality of the aluminum nitride layer 112 is better; when the full width at half maximum of the aluminum nitride layer 112 is larger, the grains in the aluminum nitride layer 112 are smaller, and the crystal quality of the aluminum nitride layer 112 is worse. In the embodiment of the present application, the full width at half maximum of the X-ray rocking curve of the aluminum nitride layer 112 along the

[0002] direction is larger, the grains of the aluminum nitride layer 112 are smaller, and the crystal quality of the aluminum nitride layer 112 is poor. In some embodiments, before thermal annealing, the full width at half maximum of the X-ray rocking curve of the aluminum nitride layer 112 along the [10-12] direction is greater than or equal to 0.6°. Specifically, the full width at half maximum of the X-ray rocking curve of the aluminum nitride layer 112 along the [10-12] direction may be, but is not limited to, 0.6°, 0.65°, 0.67°, 0.68°, 0.69°, 0.70°, 0.71°, 0.72°, 0.73°, 0.74°, 1.00°, 1.25°, and 1.50°, etc. In the embodiment of the present application, if the full width at half maximum of the X-ray rocking curve of the aluminum nitride layer 112 along the [10-12] direction is large, the grains of the aluminum nitride layer 112 are small, and the crystal quality of the aluminum nitride layer 112 is poor. Optionally, in some embodiments, the aluminum nitride film 100 after thermal annealing satisfies at least one of the following conditions: the root mean square roughness of the surface of the aluminum nitride film 100 away from the substrate 111 is less than 3.3 nm; the dislocation density of the aluminum nitride film 100 is less than 5×10 10 cm -2 ; and the half-maximum full width of the X-ray rocking curve of the aluminum nitride film 100 along the

[0002] direction is less than 0.3°; the half-maximum full width of the X-ray rocking curve of the aluminum nitride film 100 along the [10-12] direction is less than 0.6°. It can be understood that the aluminum nitride film 100 meets one or more of the above conditions. When the aluminum nitride film 100 meets one or more of the above conditions, the aluminum nitride film 100 has good crystal quality, which is conducive to further preparing a device 300 with higher performance. In some embodiments, the root mean square roughness of the surface of the aluminum nitride film 100 away from the substrate 111 is less than 3.3 nm. Specifically, the root mean square roughness of the surface of the aluminum nitride film 100 away from the substrate 111 may be, but is not limited to, 0.6 nm, 0.8 nm, 0.9 nm, 1.0 nm, 1.2 nm, 1.4 nm, 1.5 nm, 1.6 nm, 1.7 nm, 1.8 nm, 1.9 nm, 2nm, 2.2nm, 2.5nm, 2.6nm, 2.8nm, 3.0nm, 3.1nm and 3.2nm, etc. In an embodiment of the present application, the root mean square roughness value of the surface of the aluminum nitride film 100 away from the substrate 111 is less than 3.3 nm, while the root mean square roughness value of the surface of the aluminum nitride layer 112 before the thermal annealing treatment is greater than or equal to 3.3 nm. Compared with the root mean square roughness of the surface of the aluminum nitride layer 112 before the thermal annealing treatment, the aluminum nitride film 100 of the embodiment of the present application is arranged opposite to the protective layer 130 having a recessed area 131 and a flat area 133 during the thermal annealing treatment. The recessed area 131 reduces the contact area with the aluminum nitride layer 112, so that after the thermal annealing treatment, there will not be excessive adhesion between the protective layer 130 and the aluminum nitride layer 112 and it is easy to peel off, and finally the surface of the aluminum nitride film 100 away from the substrate 111 is smoother and has better surface uniformity. In some embodiments, the dislocation density of the aluminum nitride film 100 is less than 5×10 10 cm -2 Specifically, the dislocation density of the aluminum nitride film 100 may be, but is not limited to, 4.9×10 10 cm -2 4.75×10 10 cm -2 , 4.3×10 10 cm -2 , 3.9×10 10 cm -2 , 3.75×10 10 cm -2 , 3.5×10 10 cm -2 , 3.0×10 10 cm -2 , 2.85×10 10 cm -2 , 2.6×10 10 cm -2 , 2.3×10 10 cm -2 , 2.0×10 10 cm -2 , 1.95×1010 cm -2 , 1.6×10 10 cm -2 , 1.35×10 10 cm -2 and 1.0×10 10 cm -2 wait. In the embodiment of the present application, the dislocation density of the aluminum nitride film 100 is less than 5×10 10 cm -2 , and the dislocation density of the aluminum nitride layer 112 before the thermal annealing treatment is greater than or equal to 5×10 10 cm -2 Compared with the aluminum nitride layer 112 before the thermal annealing treatment, the temperature T1 and the thermal annealing time t1 of the aluminum nitride film 100 of the embodiment of the present application during the thermal annealing treatment are within a reasonable range, so that the aluminum nitride layer 112 can be fully recrystallized during the thermal annealing process, and the defect density of the aluminum nitride layer 112 is effectively reduced during the thermal annealing process, and finally an aluminum nitride film 100 with low defect density and high crystal quality is obtained. In some embodiments, the full width at half maximum of the X-ray rocking curve of the aluminum nitride film 100 along the

[0002] direction is less than 0.3°. Specifically, the full width at half maximum of the X-ray rocking curve of the aluminum nitride film 100 along the

[0002] direction may be, but is not limited to, 0.05°, 0.07°, 0.09°, 0.10°, 0.11°, 0.12°, 0.13°, 0.14°, 0.15°, 0.16°, 0.17°, 0.18°, 0.20°, 0.22°, 0.23°, 0.24°, 0.25°, 0.28°, 0.29°, etc. In the embodiment of the present application, the half-maximum full width of the X-ray rocking curve of the aluminum nitride film 100 along the

[0002] direction is less than 0.3°, while the half-maximum full width of the X-ray rocking curve of the aluminum nitride layer 112 along the

[0002] direction before thermal annealing is greater than or equal to 0.3°. The half-maximum full width of the X-ray rocking curve of the aluminum nitride film 100 in the embodiment of the present application along the

[0002] direction is smaller, and the grains of the aluminum nitride film 100 are larger, and the aluminum nitride film 100 after thermal annealing has better crystal quality. In some embodiments, the full width at half maximum of the X-ray rocking curve of the aluminum nitride film 100 along the [10-12] direction is less than 0.6°. Specifically, the full width at half maximum of the X-ray rocking curve of the aluminum nitride film 100 along the [10-12] direction may be, but is not limited to, 0.05°, 0.07°, 0.09°, 0.10°, 0.11°, 0.12°, 0.13°, 0.14°, 0.15°, 0.16°, 0.17°, 0.19°, 0.2°, 0.24°, 0.29°, 0.34°, 0.38°, 0.42°, 0.46°, 0.54°, 0.57°, 0.59°, etc. The full width at half maximum of the X-ray rocking curve of the aluminum nitride film 100 in the embodiment of the present application along the [10-12] direction is less than 0.6°, while the full width at half maximum of the X-ray rocking curve of the aluminum nitride layer 112 along the [10-12] direction before thermal annealing is greater than or equal to 0.6°. The full width at half maximum of the X-ray rocking curve of the aluminum nitride film 100 in the embodiment of the present application along the [10-12] direction is smaller, and the grains of the aluminum nitride film 100 after thermal annealing are larger, and the aluminum nitride film 100 after thermal annealing has better crystal quality. Please refer to Figures 10 and 11. The present application also provides a device 300 based on an aluminum nitride film. The device 300 is prepared on an aluminum nitride film 100 after thermal annealing. The device 300 includes: an aluminum nitride film 100 prepared by the preparation method of the aluminum nitride film 100 provided in the present application and a functional layer 310. The functional layer 310 is arranged on the surface of the aluminum nitride film 100 facing away from the substrate 111. In the embodiment of the present application, the functional layer 310 is disposed on the surface of the aluminum nitride film 100 away from the substrate 111. The aluminum nitride film 100 prepared by the preparation method provided by the present application has good crystal quality, low defect density and high Good surface uniformity enables the device 300 manufactured on the surface of the aluminum nitride film 100 to have better performance. Optionally, the device 300 may be, but is not limited to, at least one of an ultraviolet light emitting diode, a power device, a radio frequency power device, an optical waveguide device, an ultraviolet laser, a photodetector, and the like. Optionally, referring to FIG. 12 , in some embodiments, the device 300 is an ultraviolet light emitting diode 200, and the functional layer 310 of the device 300 is a light emitting layer 210. The ultraviolet light emitting diode 200 includes an aluminum nitride film 100 prepared by the preparation method provided in the present application and a light emitting layer 210, wherein the light emitting layer 210 is disposed on the surface of the aluminum nitride film 100 away from the substrate 111, and is used to generate ultraviolet light. The aluminum nitride film 100 prepared by the preparation method provided in the present application has high crystal quality, low defect density and high surface uniformity. When the light emitting layer 210 is disposed on the surface of the aluminum nitride film 100, the aluminum nitride film 100 with high crystal quality can enable the light emitting layer 210 to obtain a higher output power and a higher photoelectric conversion efficiency under the same current. Specifically, if the light-emitting layer 210 is directly disposed on the surface of the aluminum nitride layer 112 having the first temperature, the ultraviolet light-emitting diode 200 emits ultraviolet light with a wavelength of 270 nm at a current of 20 mA, and its output power is only 0.1 mW and its internal quantum efficiency is only 14%. When the light-emitting layer 210 is disposed on the surface of the aluminum nitride film 100 having the second temperature, the ultraviolet light-emitting diode 200 emits ultraviolet light with a wavelength of 270 nm at a current of 20 mA, and its output power can reach 0.8 mW and its internal quantum efficiency is higher than 14%. The aluminum nitride film 100 provides a substrate with good performance for the ultraviolet light-emitting diode 200, so that the ultraviolet light-emitting diode 200 has good performance. Optionally, in some embodiments, the light-emitting layer 210 includes a plurality of light-emitting units 211, and the plurality of light-emitting units 211 are arranged in an array. The plurality of light-emitting units 211 are arranged in an array, so that the utilization rate per unit area of ​​the light-emitting layer 210 is increased, thereby improving the product yield rate. Optionally, in some embodiments, the ultraviolet light emitting diode 200 includes a driving substrate 220, on which a driving circuit is disposed, and the driving substrate 220 is electrically connected to the light emitting layer 210, and is used to drive the light emitting layer 210 to emit light. Specifically, each of the light emitting units 211 electrically connected to the driving substrate 220 is used to drive each of the light emitting units 211 to emit light. In some embodiments, the driving substrate 220 may be a thin film transistor (TFT) substrate. In an embodiment of the present application, the light emitting layer 210 is disposed on the driving substrate 220, and the aluminum nitride film is disposed on the surface of the light emitting layer 210 away from the driving substrate 220. In other words, the driving substrate 220, the light emitting layer 210 and the aluminum nitride film are stacked in sequence. The driving substrate 220 drives the light emitting layer 210 to emit light, and the aluminum nitride film 100 is conducive to improving the output power and photoelectric conversion efficiency of the light emitted by the light emitting layer 210 under the same current. Optionally, in some embodiments, the device 300 is a power device, and the power device includes an aluminum nitride film 100, a buffer layer, a channel layer, and a first barrier layer stacked in sequence, and the functional layer 310 of the device 300 includes a buffer layer, a channel layer, and a first barrier layer. The buffer layer is used to form a two-dimensional electron gas, the channel layer is used to provide a place for the two-dimensional electron gas to move, and the first barrier layer is used to provide a sufficiently high barrier height to prevent carriers from crossing. The functional layer 310 of the power device is arranged on the surface of the aluminum nitride film 100, and the aluminum nitride film 100 has a lower defect density and better performance, providing a substrate with better performance for the functional layer 310, so that the power device has better performance. Optionally, in some embodiments, the device 300 is a photodetector, and the photodetector includes an aluminum nitride film 100, a contact layer, a second barrier layer, and an absorption layer stacked in sequence, and the functional layer 310 of the device 300 includes a contact layer, a second barrier layer, and an absorption layer. The absorption layer is used to absorb photogenerated carriers generated under illumination conditions, the second barrier layer is used to prevent the movement of carriers under non-illumination conditions, and the contact layer is used to amplify the electrical signal formed by the acquired photogenerated carriers. The functional layer 310 of the photodetector is disposed on the surface of the aluminum nitride film 100, and the aluminum nitride film 100 has a lower defect density and better performance, providing a good performance basis for the functional layer 310. The bottom makes the photodetector have better performance. Optionally, in some embodiments, the device 300 is an optical waveguide device, which includes an aluminum nitride film 100, a first covering layer, a waveguide layer, and a second covering layer stacked in sequence, and the functional layer 310 of the device 300 includes a first covering layer, a waveguide layer, and a second covering layer. The waveguide layer is used to propagate optical signals, and the first covering layer and the second covering layer are used to confine the optical signals in the waveguide layer. The functional layer 310 of the optical waveguide device is disposed on the surface of the aluminum nitride film 100, and the aluminum nitride film 100 has a lower defect density and better performance, providing a substrate with better performance for the functional layer 310, so that the optical waveguide device has better performance. Optionally, in some embodiments, the device 300 is an ultraviolet laser, which includes an aluminum nitride film 100, an N-type cladding layer, an active region, and a P-type cladding layer stacked in sequence, and the functional layer 310 of the device 300 includes an N-type cladding layer, an active region, and a P-type cladding layer. The N-type cladding layer is used to generate and conduct electrons, the P-type cladding layer is used to generate holes, and the cladding layer is used to conduct the generated laser and amplify it. The functional layer 310 of the ultraviolet laser is arranged on the surface of the aluminum nitride film 100, and the aluminum nitride film 100 has a lower defect density and better performance, providing a substrate with better performance for the functional layer 310, so that the ultraviolet laser has better performance. Mentioning "embodiment" and "implementation method" in this application means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrases in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application can be combined with other embodiments. In addition, it should also be understood that the features, structures or characteristics described in the various embodiments of the present application can be arbitrarily combined to form another embodiment that does not deviate from the spirit and scope of the technical solution of the present application, provided that there is no contradiction between them. Finally, it should be noted that the above implementation modes are only used to illustrate the technical solution of the present application and are not intended to limit it. Although the present application has been described in detail with reference to the above preferred implementation modes, a person of ordinary skill in the art should understand that the technical solution of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application.

Claims

1. A method for preparing an aluminum nitride thin film, wherein: The preparation method comprises: Providing an aluminum nitride substrate, the aluminum nitride substrate comprising a stacked substrate and an aluminum nitride layer having a first temperature; A protective layer is disposed on the surface of the aluminum nitride layer facing away from the substrate, the protective layer comprises a recessed area and a flat plate area disposed around the periphery of the recessed area, and the root mean square roughness RMS of the surface of the flat plate area facing the aluminum nitride layer is in the range of: 0nm<RMS≤50nm; and The aluminum nitride substrate and the protective layer are subjected to thermal annealing to obtain the aluminum nitride film having a second temperature; wherein the second temperature is greater than the first temperature.

2. The method for preparing an aluminum nitride thin film according to claim 1, wherein: The aluminum nitride substrate is provided, comprising: providing a substrate; An aluminum nitride layer having a first temperature is deposited on the surface of the substrate by a physical or chemical method. The deposition method may be, but is not limited to, sputtering, atomic layer deposition, molecular beam epitaxy, chemical vapor deposition, pulsed laser deposition, and the like.

3. The method for preparing an aluminum nitride thin film according to claim 2, wherein: The aluminum nitride substrate is provided, comprising: providing a substrate; A chemical vapor deposition method is used to deposit an aluminum nitride layer having a first temperature on the surface of the substrate, and the temperature T1 ranges from 723.15K≤T1≤1873.15K; the reaction pressure P1 ranges from 0Torr<P1≤800Torr, and the thickness d1 of the deposited aluminum nitride layer ranges from 0nm<d1≤1000nm; wherein the chemical vapor deposition method is a metal organic chemical vapor deposition method.

4. The method for preparing an aluminum nitride thin film according to claim 1, wherein: The protective layer also includes one or more protruding structures, one of the protruding structures is arranged on the surface of the recessed area facing the aluminum nitride layer, and a plurality of the protruding structures are arranged at intervals on the surface of the recessed area facing the aluminum nitride layer, the protruding structure has an end face facing the aluminum nitride layer, the flat sheet area has a preset surface facing the aluminum nitride layer, and the end face is not higher than the preset surface.

5. The method for preparing an aluminum nitride thin film according to claim 4, wherein: The distance d2 between the two farthest points of the protruding structure on the area surrounded by the orthographic projection of the surface of the aluminum nitride facing the protective layer is in the range of: 0.1 μm≤d2≤50000 μm; The range of the minimum distance d3 between any two adjacent protrusion structures is: 0 μm≤d3≤50000 μm.

6. The method for preparing an aluminum nitride thin film according to claim 4, wherein: Along the stacking direction of the substrate and the aluminum nitride layer, the maximum height d4 of the protruding structure is in the range of 0 μm<d4≤200 μm.

7. The method for preparing an aluminum nitride thin film according to claim 1, wherein: The step of subjecting the aluminum nitride substrate and the protective layer to thermal annealing includes: conducting thermal annealing in an ammonia atmosphere.

8. The method for preparing an aluminum nitride thin film according to claim 7, wherein: The thermal annealing of the aluminum nitride substrate and the protective layer includes: performing thermal annealing in an ammonia atmosphere; wherein the thermal annealing temperature T2 is in the range of 773.15K≤T2≤2273.15K; and the thermal annealing time t1 is in the range of 0min<t1≤180min.

9. The method for preparing an aluminum nitride thin film according to claim 1, wherein: The aluminum nitride film after thermal annealing satisfies at least one of the following conditions: the root mean square roughness of the surface of the aluminum nitride film away from the substrate is less than 3.3 nm, the dislocation density of the aluminum nitride film is less than 5×10 10 cm -2 The full width at half maximum of the X-ray rocking curve of the aluminum nitride film along the [0002] direction is less than 0.3°, and the full width at half maximum of the X-ray rocking curve of the aluminum nitride film along the [10-12] direction is less than 0.6°.

10. A device based on aluminum nitride film, wherein: The device is prepared on an aluminum nitride film after thermal annealing, and the device comprises: An aluminum nitride thin film obtained by the preparation method according to any one of claims 1 to 9; and The functional layer is arranged on the surface of the aluminum nitride film facing away from the substrate.

Citation Information

Patent Citations

  • Light-emitting device, aluminum nitride product, aluminum nitride single crystal and manufacturing method and application thereof

    CN114059165A

  • Preparation method of aluminum nitride film and device based on aluminum nitride film

    CN116695239A

  • Method for annealing nitride single crystal

    JP2013079187A

  • Manufacturing method of nitride semiconductor substrate, nitride semiconductor substrate and optical semiconductor device

    JP2020139222A

  • Method for producing group iii-nitride wafers and group iii-nitride wafers

    US20090256240A1