Sintered body of molybdenum oxide, sputtering target, and oxide thin film
By adding specific metal dopants to molybdenum oxide, the sinterability and grain size control of molybdenum oxide-based ceramic materials are enhanced, addressing the challenges of low-density targets and poor thin film quality, resulting in high-density, low-reflection, and low-resistance oxide thin films for LCD and OLED applications.
Patent Information
- Application Number
- PCT/KR2023/019512
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2023-11-30
- Publication Date
- 2024-10-17
AI Technical Summary
Molybdenum oxide-based ceramic materials are difficult to sinter, leading to low-density targets and poor thin film quality due to nodules and foreign matter generation during sputtering, which affects the reliability and performance of LCD and OLED devices.
Incorporating specific metal dopants such as niobium oxide, alkaline earth metal oxides, and metals like Mo, Ti, Cr, or Cu into molybdenum oxide to improve sinterability and control grain size, allowing for high-density sintered bodies and low-reflection, low-resistance oxide thin films without pressure sintering.
The approach results in a high-density sputtering target and oxide thin films with improved reliability, reduced reflection, and low resistance, suitable for applications in LCD and OLED TFT structures, expanding material application ranges.
Smart Images

Figure KR2023019512_17102024_PF_FP_ABST
Abstract
Description
Molybdenum oxide sintered body, sputtering target and oxide thin film
[0001] The present invention relates to an oxide sintered body used in a TFT structure of an LCD and / or OLED, a sputtering target including the sintered body, and a thin film production method using the same, and more specifically, to an oxide sintered body having improved density characteristics and improved grain size refinement control by some added elements, a sputtering target, and an oxide thin film having low resistance and low reflection characteristics using the same.
[0002]
[0003] Low-reflectivity conductive thin films are commonly used in flat panel displays (FPDs), touch screen panels, solar cells, light emitting diodes (LEDs), and organic light emitting diodes (OLEDs).
[0004] Indium oxide-tin oxide (In2O3-SnO2) ("ITO") is a representative material for this purpose, and ITO compositions are used to form conductive thin films with high visible light transmittance and electrical conductivity. While these ITO compositions exhibit excellent low-reflectivity performance, they are not cost-effective, and research into materials that can completely or partially replace indium oxide is ongoing.
[0005] However, the area of interest in these studies is the low reflectivity of the thin film formed through the target material, and it is necessary to consider the chemical resistance and heat resistance characteristics that can increase the reliability of the thin film for long-term use.
[0006] Meanwhile, molybdenum oxide is a difficult-to-sinter material. Using molybdenum oxide ceramic materials with such low sintering densities makes it difficult to fabricate high-density (e.g., greater than 90%) targets. Furthermore, sputtering using these targets inevitably leads to the generation of foreign matter, such as back deposits and nodules, which deteriorate the properties of the thin film.
[0007] [Prior Art Literature]
[0008] [Patent Document]
[0009] (Patent Document 1) Republic of Korea Publication No. 10-2020-0069314
[0010]
[0011] The present invention has been made to solve the above-mentioned problems, and the technical task of the present invention is to provide a novel molybdenum oxide-based sintered body, which improves sinterability, enables grain size control, and ensures high density even when sintered under no pressure by adding a specific metal dopant in a predetermined content range to the main raw material, difficult-to-sinter molybdenum oxide, a sputtering target including the sintered body, and an oxide thin film formed therefrom with improved low-reflection and low-resistance characteristics.
[0012] Other objects and advantages of the present invention can be more clearly explained by the detailed description of the invention and the claims below.
[0013]
[0014] In order to achieve the above-mentioned technical task, the present invention provides an oxide sintered body comprising: molybdenum (M1) oxide; niobium (M2) oxide; at least one alkaline earth metal (M3) oxide; and at least one metal (M4) selected from the group consisting of Mo, Ti, Cr, W, and Cu; wherein the metal (M4) is included in an amount of 3 to 60 wt% based on the total weight of the sintered body.
[0015] In one embodiment of the present invention, the metal (M4) may be included in an amount of 5 to 55 wt% relative to the total weight of the sintered body.
[0016] In one embodiment of the present invention, the average grain size (D50) in the oxide sintered body may be 80% or less compared to the average grain size (D50) in the oxide sintered body that does not include the metal (M4).
[0017] In one embodiment of the present invention, the surface resistance of the oxide sintered body may be 60% or less compared to the surface resistance of an oxide sintered body that does not include metal (M4).
[0018] In one embodiment of the present invention, the oxide sintered body is Mo (1-x) Nb x It may include an O2 (x is 0 to 0.25) crystal phase and a metal (M4) crystal phase.
[0019] In one embodiment of the present invention, the oxide sintered body may be a molded body manufactured by mixing molybdenum (M1) oxide; niobium (M2) oxide; at least one alkaline earth metal (M3) oxide; and metal (M4), and then pressurelessly sintering the molded body under atmospheric pressure.
[0020] In one embodiment of the present invention, the molybdenum oxide (M1) includes at least one of MoO2 and MoO3, and may be included in an amount of 20 to 70 wt% based on the total weight of the oxide sintered body.
[0021] In one embodiment of the present invention, the molybdenum oxide (M1) and the niobium oxide (M2) are included in an amount of 45.0 wt% or more and less than 95 wt% based on 100 wt% of the oxide sintered body, and the content ratio of the molybdenum oxide (M1) and the niobium oxide (M2) may be a weight ratio of 80:20 to 45:55.
[0022] In one embodiment of the present invention, the alkaline earth metal (M3) metal oxide may include at least one selected from the group consisting of CaCO3 and MgO.
[0023] In one embodiment of the present invention, the alkaline earth metal (M3) metal oxide (M3) may be included in an amount of more than 0 wt% and less than 10 wt% based on 100 wt% of the oxide sintered body.
[0024] In one embodiment of the present invention, the at least one alkaline earth metal (M3) metal oxide and the metal (M4) may be included in a weight ratio of 1:1 to 20.
[0025] In one embodiment of the present invention, the average grain size (D50) of the non-pressurized sintered oxide sintered body is 5 to 30 ㎛, and the resistivity is 3×10 -3 Ωcm or less, and the relative density may be 80% or more.
[0026] The present invention also provides a sputtering target including the above-described oxide sintered body.
[0027] In addition, the present invention provides an oxide thin film formed from the sputtering target of claim 13.
[0028] In one embodiment of the present invention, the oxide thin film has a light reflectance of 25% or less for a wavelength of 550 nm and a sheet resistance of 2.6×10 at a thickness of 100 to 500 Å. 4 It may be less than Ω / sq.
[0029]
[0030] According to one embodiment of the present invention, by adding a metal dopant that suppresses the growth of crystal grains constituting a sintered body to a difficult-to-sinter molybdenum oxide in a predetermined content range, the sinterability of the molybdenum oxide sintered body can be improved even under no pressure, and particle size optimization, low resistance, low reflection, and high density can be secured.
[0031] Accordingly, the molybdenum oxide-based sintered body and sputtering target according to the present invention can be usefully applied to forming electrodes or wiring used in TFT structures of LCDs and OLEDs.
[0032] The effects according to the present invention are not limited to those exemplified above, and more diverse effects are included in this specification.
[0033]
[0034] Figure 1 is a photograph showing the microstructure and average grain size of oxide sintered bodies manufactured in Examples 1 to 5 in which molybdenum metal (M4) was added.
[0035] Figure 2 is a photograph showing the microstructure and average grain size of the oxide sintered bodies manufactured in Comparative Examples 1 and 2 without adding molybdenum metal (M4).
[0036] Figure 3 is a graph showing the average particle diameter of the oxide sintered bodies sintered without pressure in Examples 1 to 5 and Comparative Examples 1 to 2.
[0037] Figure 4 is a graph showing the change in relative density according to the sintering temperature of the oxide sintered bodies manufactured in Examples 1 to 5 and Comparative Examples 1 to 2.
[0038] Figure 5 is a graph showing the change in shrinkage ratio according to the sintering temperature of the oxide sintered bodies manufactured in Examples 1 to 5 and Comparative Examples 1 to 2.
[0039] Figure 6 is a graph showing the change in surface resistance of a unit film according to the thickness of the thin film formed from an oxide sputtering target according to Examples 1 to 5 and Comparative Example 2.
[0040] Figure 7 is a graph of the average reflectance and sheet resistance per unit film of thin films formed from oxide sputtering targets according to Examples 3 to 5.
[0041] Figure 8 is a graph showing the change in average reflectance of a unit film according to the thickness of the thin film formed from an oxide sputtering target according to Examples 1 to 5 and Comparative Example 2.
[0042] Figure 9 is an XRD graph of the oxide sintered bodies manufactured in Example 1, Example 4, Comparative Example 1, and Comparative Example 2.
[0043]
[0044] All terms (including technical and scientific terms) used in this specification may be used with meanings commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Furthermore, terms defined in commonly used dictionaries should not be interpreted ideally or excessively unless explicitly and specifically defined otherwise.
[0045] Furthermore, throughout the specification, when a part is said to "include" a component, unless otherwise specifically stated, this does not exclude other components but rather means that other components may be included. Furthermore, throughout the specification, the terms "above" or "on" include not only cases where the target part is located above or below it, but also cases where there is another part in between, and do not necessarily mean that the target part is located above it in the direction of gravity. In addition, terms such as "first" and "second" in the specification do not indicate any arbitrary order or importance, but are used to distinguish between components.
[0046] MoO2-Nb2O5 materials, conventionally used as n-type semiconductor thin films, are typically manufactured via pressure sintering. However, pressure sintering is not suitable for mass production due to the increased manufacturing process costs associated with equipment costs. Furthermore, the high-pressure manufacturing process limits the ability to increase the size of the sintered body.
[0047] In order to solve the above-mentioned problems, when MoO2-Nb2O5 materials are sintered without pressure, there is a limit to the increase in sintered density, so it is difficult to apply, and also, when the sintering temperature is increased, the amount of melting and volatilization increases, which actually causes the density to decrease. In other words, heat is required as a driving force during sintering, and while higher heat is generally advantageous in securing sinterability (densification), in the case of some raw materials, problems such as volatilization occur, which actually lowers the density.
[0048] Meanwhile, the inventors of the present invention, in Korean Patent Application No. 10-2022-0132119, have shown that by using a small amount of an alkaline earth metal oxide dopant (M3) that assists sinterability in a difficult-to-sinter material having a basic composition of molybdenum oxide and niobium oxide, they can simultaneously secure the effects of improving sinterability and securing high density even when sintering without pressure under atmospheric conditions. At this time, the addition of the alkaline earth metal oxide (M3) dopant, such as CaCO3 or MgO, can secure bonding between particles within the oxide sintered body, but this causes the particle size within the sintered body to increase. When the crystal grain size of the sintered body increases in this way, the particles are formed unevenly and foreign substances are generated during the sputtering process, which leads to a deterioration in the quality and reliability of the final oxide thin film.
[0049] Accordingly, in the present invention, a difficult-to-sinter material having a basic composition of molybdenum oxide (M1) and niobium oxide (M2) is mixed with an alkaline earth metal oxide dopant (M3) that assists sinterability and a specific metal (M4) that optimizes the particle size by suppressing the grain growth of the sintered body and thereby improves the homogeneity of the thin film, and the metal element ratio (composition) thereof is controlled. Accordingly, in the present invention, not only can a high-density target be obtained due to the improvement in sinterability, but also a high-quality thin film can be obtained by improving the compositional non-uniformity and the generation of foreign substances such as back deposits and nodules that may occur during sputtering through the control of grain growth. In addition, by applying a high-content metal (M4) dopant, low-resistance and low-reflection characteristics of the oxide thin film formed from the sintered body are simultaneously secured, thereby expanding the range of application of materials for TFTs equipped in conventional LCDs and OLEDs.
[0050]
[0051] High-density targets for oxide sintering and sputtering
[0052] An example of the present invention is a molybdenum-based oxide sintered body used in a thin film transistor (TFT) structure of an LCD and / or OLED, and a high-density target for sputtering comprising the same.
[0053] In general, when sintering an oxide sintered body, heat or pressure is required as a driving force. At this time, the higher the heat and pressure, the more secure the sinterability of the sintered body and the more advantageous it is for densification, but in the case of some materials, problems such as melting and volatilization occur, which actually lowers the density. In the present invention, molybdenum oxide and niobium oxide are used as the basic composition, but through intermediate phase synthesis of the main raw materials (e.g., solid solution between molybdenum oxide and niobium oxide) and addition of additional elements (e.g., M3, M4 dopants), it is possible to secure a density (densification) of the sintered body that can be used as a sputtering target even when sintered without pressure, and in addition, it is intended to secure homogeneity, low resistance, and low reflection characteristics of the thin film formed by sputtering by optimizing the particle size.
[0054] For example, the oxide sintered body includes molybdenum (M1) oxide; niobium (M2) oxide; at least one alkaline earth metal (M3) oxide; and at least one metal (M4) selected from the group consisting of Mo, Ti, Cr, W, and Cu, wherein the metal (M4) is included in a predetermined amount (e.g., 3-60 wt%).
[0055] Below, each component is described in detail.
[0056] The molybdenum oxide included in the oxide sintered body according to the present invention is a main component constituting the sintered body.
[0057] Molybdenum (M1) oxide is a component that has oxygen bonded to molybdenum, such as MoO2, MoO3, and MoO4. In the present invention, MoO is used as molybdenum (M1) oxide. 2, MoO3, or MoO2 and A mixture of MoO3 can be used. In this case, when using a mixture of MoO2 and MoO3 as molybdenum oxide, the mixing ratio between them is not particularly limited and can be appropriately adjusted within the typical content range known in the art. Meanwhile, since MoO3 has a melting point of approximately 800°C, it volatilizes at high temperatures of 1,000°C or higher. Accordingly, in the present invention, which performs pressureless sintering at high temperatures of 1,000°C or higher, it is preferable to use MoO2 as the molybdenum (M1) oxide.
[0058] Additionally, one of the additive components included in the oxide sintered body according to the present invention is niobium (M2) oxide.
[0059] This niobium (M2) oxide is an oxide dopant that improves chemical resistance and heat resistance properties, and the chemical resistance and heat resistance properties of molybdenum oxide can be improved by adding the metal oxide. The niobium oxide is not particularly limited as long as it is a component in which oxygen is bonded to niobium, and may be Nb2O5, for example. In the following description, the niobium oxide component is symbolized as M2.
[0060] Another of the additive components included in the oxide sintered body according to the present invention is a metal oxide containing at least one alkaline earth metal (M3).
[0061] For example, the metal oxide (M3) may include at least one of Ba, Ca, Mg, and Sr, and specifically, may include a metal oxide (M3) including at least one of Ca and Mg.
[0062] The metal oxide containing an alkaline earth metal (M3) acts as a dopant that assists the sintering of difficult-to-sinter molybdenum oxide and exhibits a density-increasing effect. By adding such a metal oxide (M3), the chemical resistance and heat resistance properties of the molybdenum oxide can be improved. The metal oxide containing an alkaline earth metal (M3) is not particularly limited as long as it is a component in which oxygen is bonded to at least one element (A) among Ca and Mg, and may include, for example, one or more selected from the group consisting of CaCO3 and MgO.
[0063] One of the additive components included in the oxide sintered body according to the present invention is at least one metal (M4) selected from the group consisting of Mo, Ti, Cr, W, and Cu.
[0064] When the density of the conventional oxide sintered body is low (relative density ≥ 90%), foreign substances such as back deposits and nodules are generated in the thin film during sputtering, and the higher the density, the more advantageous it is for the sputtering process. Meanwhile, during sputtering, pull-out of each particle on the target surface occurs. At this time, the space where the particles fall out becomes empty, and the smaller the particle, the smaller the space where the particles fall out, so the curvature of the sputtered target surface is reduced. Accordingly, under the same density, the smaller the particle size constituting the oxide sintered body, the more uniform the particle deposition is possible during the sputtering process, and the effect of improving the compositional unevenness and foreign substance generation that may occur during the sputtering process can be secured.
[0065] The metal (M4) used in the present invention controls the growth of particles constituting the oxide sintered body, thereby improving the compositional inhomogeneity and foreign matter generation that may occur during the sputtering process. That is, the metal (M4) suppresses the particle growth caused by the addition of metal oxides (M3) such as CaCO3 and MgO, and promotes uniformity and refinement of the grain size of the sintered body, thereby improving the quality of the oxide thin film formed by sputtering. In addition, due to the electrical conductivity of the metal, the sheet resistance of the unit film can be reduced, thereby ensuring low-resistance characteristics. In addition, as a metal dopant that assists the sinterability of molybdenum oxide and exhibits a density-increasing effect, the addition of the metal can increase the high-density, chemical resistance, and heat-resistant characteristics of the molybdenum oxide. In the following description, at least one component among Mo, Ti, Cr, W, and Cu is symbolized and represented as M4, and preferably Mo.
[0066] The metal oxide sintered body including the above-mentioned molybdenum (M1) oxide, niobium (M2) oxide, at least one alkaline earth metal (M3)-containing metal oxide, and metal (M4) may contain 45.0 wt% or more and less than 95 wt% of molybdenum (M1) oxide and niobium (M2) oxide, more than 0 wt% and less than 10 wt% of alkaline earth metal (M3)-based metal oxide, and 3.0 to 60 wt% of metal (M4), based on 100 wt% of the sintered body. More specifically, the sintered body may have a composition consisting of 45.0 to 90.0 wt% of molybdenum (M1) oxide and niobium (M2) oxide; 0.5 to 5.0 wt% of alkaline earth metal (M3)-based metal oxide; and 5.0 to 55 wt% of metal (M4).
[0067] Here, the content ratio of molybdenum oxide (M1) and niobium oxide (M2) is 80:20 to 45:55 by weight, specifically 72:28 to 47:53 by weight, and more specifically 63:37 to 56:44 by weight. In the present invention, when the content ratio of molybdenum oxide, for example, MoO2, is 20 to 70 wt%, specifically 20 to 68 wt%, of the entire metal oxide sintered body, it can have low-reflection characteristics when deposited as a thin film.
[0068] In addition, at least one alkaline earth metal (M3) metal oxide and metal (M4) constituting the above oxide sintered body may be included in a weight ratio of 1:1 to 20, and specifically, may be configured in a weight ratio of 1:10 to 15.
[0069] The oxide sintered body according to the present invention may be a compact manufactured by mixing oxides containing each metal component (M1, M2, M3, M4), for example, molybdenum (M1) oxide; niobium (M2) oxide; alkaline earth metal (M3) containing metal oxide; and metal (M4) according to a target composition, and then pressurelessly sintering the compact under atmospheric pressure.
[0070] The oxide sintered body according to the present invention, which is configured as described above, may have a relative density of 80% or more, and specifically 90% or more, even when sintered without pressure under atmospheric pressure. In this case, the upper limit thereof is not particularly limited. In addition, the resistivity of the oxide sintered body may be 1×10 -2 Ωcm or less, and its lower limit is not specifically limited.
[0071] In addition, the oxide sintered body composed of the aforementioned composition not only has a finer average grain size (D50) compared to a conventional sintered body that does not include metal (M4), but also has a smaller difference in surface roughness before and after sputtering of the sintered body target, so that it can have uniform surface characteristics and excellent thin film characteristics.
[0072] For example, the average grain size (D50) in the oxide sintered body may be 80% or less, specifically 60% or less, and more specifically 40 to 50%, of the average grain size (D50) in the oxide sintered body that does not include the metal (M4). For example, the grain size (D50) of the oxide sintered body that includes the metal (M4) may be 5 to 30 μm, specifically 10 to 20 μm. In comparison, the grain size of the oxide sintered body that does not include the metal (M4) may be 20 to 50 μm.
[0073] In addition, since the oxide sintered body of the present invention having the aforementioned composition includes an electrically conductive metal (M4) component, the oxide thin film formed therefrom can have low resistance characteristics.
[0074] For example, the sheet resistance of the oxide sintered body may be 60% or less, specifically 50% or less, and more specifically 1 to 10%, of the sheet resistance of the oxide sintered body that does not contain metal (M4). For example, the sheet resistance of the oxide sintered body that contains metal (M4) or the thin film formed therefrom may be 2.60×10 4 0.01×10 4 Ω / sq, specifically 1.30×10 4 0.03×10 4 Ω / sq. In comparison, the sheet resistance of an oxide sintered body or thin film without metal (M4) is 3.00×10 4 1.60×10 4 It could be Ω / sq.
[0075] The oxide sintered body according to the present invention comprises at least one crystal phase, and in particular, is distinguished from a sintered body formed using only a metal oxide as a conventional reactant in that at least one crystal phase component essentially comprises at least one metal (M4) among Mo, Ti, Cr, W, and Cu. For example, the oxide sintered body may include at least a portion of a crystal phase formed as shown in the following reaction formula.
[0076] 2(1-x)MoO2+ xNb2O5→ 2Mo(1-x)NbxO2+ 2.5xO2
[0077] MgO+Nb2O5→ MgNb2O6
[0078] CaCO3→ CaO + CO2
[0079] CaO + Nb2O5→ CaNb2O6
[0080] 2MgO + MoO2→ Mg2Mo3O8
[0081] For example, the oxide sintered body is a MoO2 phase in which Nb2O5 is partially dissolved, for example, Mo 1-x Nb x It includes O2 (wherein, x is 0 to 0.25, specifically 0.15 to 0.25) as a main crystal phase, and may include MgNb2O6, CaNb2O6, Mg2Mo3O8 and / or Mo as a sub-crystal phase. More specifically, it may include a form in which metal Mo is dispersed in at least a portion of the above-mentioned main crystal phase and sub-crystal phase. The area ratio (area ratio) of such crystal phase is not particularly limited, and for example, the main crystal phase may be included in an amount of 25% or more, more specifically in a range of 27 to 83%, relative to the entire crystal phase of the sintered body.
[0082] Meanwhile, the oxide sintered body according to the present invention may include stoichiometric molybdenum oxides such as MoO2 and MoO3 based on the final product, but may also include substoichiometric molybdenum oxides, such as Mo4O 11 , Mo 17 O 47 , Mo5O 14 , Mo8O 23 , Mo9O 26 , and Mo 18 O 52At least one or more of the above are substantially absent. Here, "substantially absent" means that an unavoidable content of 2.0 wt% or less, specifically 1.0 wt% or less, and more specifically 0.5 wt% or less may be present relative to 100 wt% of the oxide sintered body.
[0083]
[0084] <Method for manufacturing oxide sintered body and sputtering target>
[0085] Hereinafter, a method for manufacturing an oxide sintered body and a sputtering target according to one embodiment of the present invention will be described. However, the present invention is not limited to the manufacturing method described below, and each process step may be modified or selectively combined as needed.
[0086] The present invention relates to the manufacture of a sputtering target, wherein raw metal or ceramic powder is heat-treated to form a single mass. For example, when manufacturing the oxide sintered body and sputtering target, the raw metal or ceramic powder is made of MoO2 and / or MoO3, Nb2O5 as a base material, and additional elements are added and mixed to form the final sputtering target.
[0087] One example of the above manufacturing method may comprise the steps of: (i) preparing and mixing raw material powders containing molybdenum (M1) oxide; niobium (M2) oxide; metal oxide containing at least one alkaline earth metal (M3); and metal (M4) according to a target composition ('step S10'); (ii) manufacturing a molded body using the mixed raw material powders ('step S20'); and (iii) performing a pressureless heat treatment on the molded body under atmospheric pressure in an inert atmosphere at 1,200 to 1,600°C for 1 to 20 hours to manufacture a sintered body ('step S30').
[0088] Hereinafter, the above manufacturing method is explained in detail by each process step.
[0089] (i) Preparation of raw powder ('Step S10')
[0090] In the above step S10, a raw material powder containing molybdenum (M1) oxide, niobium (M2) oxide, at least one alkaline earth metal (M3)-containing metal oxide, and a metal (M4) is prepared. Specifically, molybdenum (M1) oxide; niobium (M2) oxide; at least one alkaline earth metal (M3)-based metal oxide selected from the group consisting of CaCO3 and MgO; and a metal (M4) powder selected from Mo, Ti, Cr, W, and Cu are weighed according to the target composition, and each powder is placed into a mixer and ground and mixed to prepare a mixture.
[0091] When mixing the above-mentioned raw material powders, conventional additives known in the art, such as binders, dispersants, and antifoaming agents, may be additionally included as needed. At this time, the amount of additives used may be appropriately adjusted within a conventional range known in the art, and for example, 0.01 to 10 wt% may be used relative to the total weight of powders in the slurry (e.g., 100 wt%).
[0092] The mixing and grinding of raw material powders is not particularly limited and can be performed using a conventional ball mill, attraction mill, bead mill, etc. known in the art. For example, the mixed raw material powders can be mixed and ground using a wet bead mill using zirconia balls, and then the powder can be spheroidized (spray dryer) and then sieved to obtain the final powder.
[0093] Add pure water, antifoaming agent, plasticizer, binder, etc. in an amount approximately twice that of the raw material powder, and mix thoroughly using a mixer for approximately 2 hours.
[0094] Afterwards, 0.8 pi zirconia beads (about 2 kg) are placed in a 1 L sized vessel made of zirconia, and the raw materials mixed with pure water are added and crushed sufficiently. At this time, the bead mill speed is not particularly limited, and may be, for example, about 2000 to 4000 rpm, specifically 2500 to 3500 rpm, and more specifically about 3000±200 rpm, and the raw materials are added at a speed of 4 to 6 liters per minute, specifically 4.5 to 6.5 liters, and more specifically about 5 liters.
[0095] After sufficient crushing, a spherical powder is produced using a spray dryer. Afterwards, the good powder and scrap powder are separated using a 90 to 110 mesh screen, specifically a 100 mesh screen, as needed.
[0096] (ii) Manufacturing of molded body ('Step S20')
[0097] The above S0 step is a step of manufacturing a molded body using prepared raw material powder. More specifically, a molded body of a predetermined specification is manufactured through a process of putting raw material powder into a molding machine and molding it.
[0098] To increase the density of the molded body, the molding process may be performed at least once, or more specifically, twice. For example, the first molding process may involve feeding raw material powder into a single-screw molding machine to produce the primary molded body, while the second molding process may utilize a hydrostatic press (CIP) machine.
[0099] The conditions in the above first molding process are not particularly limited and can be appropriately adjusted within the general conditions known in the art. For example, a first molded body is manufactured using a 50Φ ultra-hard mold according to the weight of a given powder. At this time, the pressure during the first molding can be carried out at the minimum pressure required to form a shape, and specifically, it can be carried out at a level where it is maintained at about 10 Mpa for about 1 minute. Thereafter, the second molding process can be carried out using isostatic pressing (CIP) under conditions of about 200 Mpa with a holding time of several hours. At this time, since the second isostatic pressing is carried out together with an organic solvent including water, it can be carried out while being placed in an acrylic sealant (e.g., an envelope).
[0100] (iii) Manufacturing of sintered body ('S30 stage')
[0101] In the above step S30, the manufactured molded body is sintered under predetermined conditions to manufacture a sintered body.
[0102] At this time, the sintering conditions are not particularly limited and can be appropriately adjusted within the conventional conditions known in the art. For example, pressureless sintering can be performed at 1,200 to 1,600°C for 1 to 20 hours, and specifically, sintering can be performed at 1,350 to 1,550°C for 3 to 7 hours. The sintering can be performed under an oxygen atmosphere, or under an inert gas condition such as nitrogen or argon for the purpose of improving electrical conductivity due to partial oxygen deficiency.
[0103] As a specific example of the above S30 step, the prepared molded body is placed in an alumina crucible of a certain specification and sintered. In this experiment, in order to confirm the difference in properties between the molded body before heat treatment and the pressureless sintered body after heat treatment, the weight, diameter, height, etc. of the molded body and the sintered body were measured and each physical property was compared (see Table 2 and Figures 4 and 5 below).
[0104] The pressureless sintered body manufactured through this process may have a relative density of 80% or more, specifically 85% or more, and more specifically 90% or more. In this case, the upper limit is not particularly limited.
[0105] (iv) Sputtering target manufacturing
[0106] Next, the sintered body after sintering is completed is removed and processed. For example, after removing the sintered body obtained after heat treatment, the surface of the target can be polished by processing the upper and lower parts of the target by at least 1 mm.
[0107] Afterwards, a commercial sputtering target is manufactured through diffusion bonding and final processing commonly known in the industry.
[0108] Specifically, the oxide sintered body obtained and processed in step S30 is bonded to a backing plate. Indium may be used as an adhesive, and a bonding rate of 95% or higher is preferably achieved. Subsequently, processing is performed using processing equipment to reach the final target thickness, and the backing plate surface is treated with beads and / or arc spray to obtain the final sputtering target.
[0109] A metal oxide target can be manufactured through the aforementioned process. The target density of the manufactured target is preferably at least 90%, and more specifically, at least 95%.
[0110]
[0111] <Oxide thin film>
[0112] Another example of the present invention is a metal oxide thin film deposited using the aforementioned molybdenum-based oxide target. This metal oxide thin film can be formed by performing sputtering using the aforementioned sintered body as a target material.
[0113] The oxide film described above may have slight differences in composition depending on the deposition atmosphere, but since it is manufactured by sputtering the oxide target described above, its composition is substantially the same as that of the target. Accordingly, it has a density characteristic of 80% or more relative density and a density of 1×10 -2 An oxide thin film having excellent resistivity characteristics of Ωcm or less can be formed.
[0114] In addition, the oxide thin film according to the present invention can secure low resistance and low reflection characteristics of the oxide thin film by controlling the crystal grain growth of the sintered body and increasing the conductivity by adding a high content of metal (M4) dopant such as Mo. In addition, by adding specific metal oxides and metals to the main raw material, molybdenum oxide, in a predetermined range, the chemical resistance and heat resistance characteristics can be improved by optimizing the molybdenum oxide ratio and composition. In addition, since the sintering characteristics and density are improved by adding a small amount of specific dopants (M3, M4), it is possible to manufacture a difficult-to-sinter Mo-Nb-O sputtering target with high density and excellent resistivity through pressureless sintering instead of the conventional pressure sintering.
[0115] For example, the oxide thin film may have a light reflectance of 25% or less at a wavelength of 550 nm, and more specifically, may be 5 to 18%. Here, the measurement of the reflectance may be performed according to a method known in the art. For example, the measurement may be performed on the surface of the substrate on which the metal oxide thin film is formed, and the light reflectance for an average wavelength of 360 to 740 nm and / or a wavelength of 550 nm may be measured. In this case, the lower limit of the light reflectance is not particularly limited.
[0116] As another specific example, the sheet resistance of the oxide thin film is 2.60×10 at a thickness of 100 to 500 Å. 4 Ω / sq or less, more specifically 1.30×10 4 0.03×10 4 It can be Ω / sq.
[0117] The metal oxide thin film according to the present invention can be formed (deposited) using a conventional sputtering method known in the art. One example of the above manufacturing method includes the step of mounting the aforementioned molybdenum oxide pressureless sintered body sputtering target, and then depositing the thin film at room temperature in an oxygen and / or argon atmosphere in a vacuum chamber. In this case, the sputtering can be performed using a DC sputter.
[0118] The substrate and sputtering device used can be conventional ones known in the art without limitation. For example, the film can be formed by supplying oxygen, oxygen and high-purity argon gas, or argon (Ar) gas into a vacuum chamber at a rate of 80 to 110 sccm (standard cubic centimeters per minute), specifically, by supplying at a rate of 95 to 105 sccm, and the film can be deposited at room temperature (RT) without applying temperature to the substrate on which the film is to be formed. In addition, the power density of the DC sputter is 0.5 to 3.6 W / cm. 2 , more specifically 1.0 to 2.0 W / cm 2 The thickness of the molybdenum-based metal oxide thin film may be 100 to 500 Å, but is not particularly limited thereto. In addition, the physical properties of the thin film may be evaluated by depositing a molybdenum oxide thin film with a thickness of 100 to 500 Å, then depositing a Cu thin film with a thickness of 3000 to 6000 Å, and then measuring the reflectivity and sheet resistance of the thin film on a glass surface.
[0119] The oxide thin film obtained as described above can be used in various ways in the manufacture of semiconductor devices, and for example, can be applied for forming wires or electrodes in the manufacture of semiconductors. In particular, the metal oxide thin film can expand the range of applications in the TFT structure of LCD and OLED by securing low resistance and low reflection characteristics. For example, when the low reflection characteristic is secured, it can be used as a gate layer material of TFT, and when both low resistance and low reflection characteristics are secured, it can be applied to at least one or more of the gate layer, source layer, and drain layer of the thin film transistor (TFT) of TFT. When the thin film of the present invention is used as a gate layer, source layer, and drain layer material included in a thin film transistor (TFT) and / or a barrier layer of these layers, the contact resistance can be lowered, and the physical properties of the thin film transistor can be improved by having excellent transparency and a low refractive index.
[0120] The molybdenum oxide-based sputtering target according to the present invention described above and the oxide thin film formed therefrom can be usefully used in various technical fields. For example, the present invention can be applied without limitation to various display devices such as liquid crystal displays or organic electroluminescent displays, information transmission devices such as flat panel displays such as LCDs, PDPs, OLEDs, and LEDs; touch panels for surface light source lighting devices such as OLEDs and LEDs; mobile phones, tablets, and / or information transmission devices using the same.
[0121] Hereinafter, the present invention will be described in detail through examples. However, the following examples are only illustrative of the present invention, and the present invention is not limited to the following examples.
[0122]
[0123] [Example 1-5] Preparation of MoO2-Nb2O5, a-added and Mo-added sintered bodies
[0124] A molded body was manufactured by mixing molybdenum (M1) oxide, niobium (M2) oxide, alkaline earth metal (M3) oxide, and metal (M4) in a ratio as shown in Table 1 below.
[0125] When manufacturing molded bodies, most samples were manufactured as 127Φ discs, and some compositions were also manufactured as 50Φ discs. Afterwards, using heat treatment equipment, a heat treatment was performed at approximately 1350 to 1550°C for 6 hours in a nitrogen atmosphere to manufacture oxide sintered bodies of Examples 1 to 5.
[0126] M1M2M3M4Total(wt%)MoO2Nb2O5MgOCaCO3MoExample 16525217100Example 257252115100Example 342252130100Example 432252140100Example 522252150100Comparative Example 17525000100Comparative Example 27225210100
[0127]
[0128] [Comparative Example 1-2] Manufacturing of MoO2-Nb2O5 and α-added sintered bodies
[0129] Except for changing the composition to be input as shown in Table 1 above, the same procedure as in the above example was followed to manufacture a 127Φ disc, and in the case of some compositions, a 50Φ disc was also manufactured. Afterwards, the oxide sintered bodies of Comparative Examples 1 and 2 were manufactured by heat-treating at about 1350 to 1550°C for 6 hours in a nitrogen atmosphere using heat treatment equipment.
[0130]
[0131] [Experimental Example 1] Evaluation of the properties of the molded body
[0132] The physical properties of each molded body manufactured in Examples 1 to 5 and Comparative Examples 1 to 2 were evaluated as follows.
[0133] Specifically, the diameter (D) and height (T) of each molded body were measured using a vernier caliper, and the weight (Mass) was weighed using a scale. In addition, the relative density was converted into a volume % by converting the input amount of each weight into a level compared to the theoretical density, and the results are shown in Table 2 below. At this time, the density of the measured sample was calculated as weight / volume, and when multiple identical samples were produced, it was expressed as an average value.
[0134] For reference, in Table 2 below, each sample was not sintered and had a low relative density, and after sintering (heat treatment), the relative density of each sintered body was at the level of 96%.
[0135] Dopant diameter (D) height (T) weight (g) relative density (%) theoretical density (g / cm 3 )M3M4Example 1CaCO3, MgO7% Mo120.0910.14438.0462.36.122Example 2CaCO3, MgO15% Mo120.4010.32459.2362.16.299Example 3CaCO3, MgO30% Mo120.859.02438.2863.66.657Example 4CaCO3, MgO40% Mo120.339.11460.2564.26.920Example 5CaCO3, MgO50% Mo120.029.25470.2964.36.989Comparative Example 1--120.229.12420.8560.86.098Comparative example 2CaCO3, MgO-120.1311.02457.4661.35.976
[0136]
[0137] [Experimental Example 2] Evaluation of average particle size of sintered body
[0138] The structural changes and average particle size of the sintered bodies heat-treated at 1450℃ were evaluated.
[0139] Specifically, the sintered bodies of Examples 1 to 5 manufactured under non-pressurized conditions and the Comparative Examples 1 to 2 manufactured under the same conditions were used as samples. These two types of samples were cut into 10X10X10 mm sizes using a metal blade, and then polished for several minutes using a polishing machine from SiC paper #100 to #2000, and then finally prepared using a 1㎛ paste slurry and ultrafine cloth. Afterwards, the samples were immersed in hydrogen peroxide water at about 200℃ for 1 minute and heat-treated so that the surface of the tissue could be exposed.
[0140] In addition, the average particle size of the sintered body was measured using FE-SEM (Hitachi, S-4800) at the same magnification of 300 for each sample, and 5 lines were randomly drawn on the measured photograph, and the linear intercept method according to the following mathematical formula 1 was used to calculate the diameter for about 100 particles, and the results are shown in Figures 1 to 3.
[0141] [Mathematical Formula 1]
[0142] D = 1.56 × C / MN
[0143] In the above equation, D = average particle diameter, C = total length of the line, M = magnification, and N = number of particles on the line.
[0144] As a result of the experiment, in the case of Comparative Example 1 composed of molybdenum oxide and niobium oxide, the average particle diameter of the sintered body was approximately 11.4 ㎛. However, in the case of Comparative Example 1, the relative density was less than 70%, making it unsuitable for use as a sputtering target. In addition, in the case of Comparative Example 2, which included molybdenum oxide and niobium oxide as basic compositions but also included alkaline earth metal oxides, the average particle diameter was 30.2 ㎛, indicating that the average particle diameter of the sintered body was somewhat larger due to the alkaline earth metal dopant.
[0145] In comparison, it was confirmed that Examples 1 to 5, which included molybdenum oxide and niobium oxide as basic compositions but also included alkaline earth metal oxide and molybdenum metal, had a finer average particle size than Comparative Example 2 (see Figures 1 to 3 below).
[0146]
[0147] [Experimental Example 3] Evaluation of sintered body density and shrinkage rate
[0148] After heat treatment was performed on each sample manufactured in Examples 1 to 5 and Comparative Examples 1 to 2, the changes in the physical properties of each sintered body were measured.
[0149] (1) Density evaluation after heat treatment
[0150] The physical properties of the sintered body after heat treatment were measured in the same manner as in Experimental Example 1 described above. As an example, the results of the relative density calculated by measuring the diameter, height, and weight of the heat-treated sintered body are shown in Figure 4 below.
[0151] Experimental results showed that in Examples 1 to 5, the relative density significantly increased as the sintering temperature increased from 1350°C to 1550°C (see Fig. 4). In contrast, in Comparative Example 1, the relative density of the molded body was lower or similar depending on the sintering temperature, and Comparative Example 2 had a density similar to that of the Examples.
[0152] (2) Evaluation of shrinkage rate before and after heat treatment
[0153] The diameter and height of the pre-heat-treated molded body and the post-heat-treated sintered body were measured, respectively, and the shrinkage ratio was calculated. The calculated shrinkage ratio results are shown in Figure 5 below.
[0154] As a result of the experiment, in the case of Comparative Examples 1 and 2, the shrinkage change rate according to the heat treatment was not large. In contrast, in the case of Examples 1 to 5, it was found that the shrinkage change rate of the sintered body according to the heat treatment was relatively high (see Fig. 6). For example, in the case of the Examples, the shrinkage rate increased rapidly in sintering at 1400°C compared to sintering at 1350°C. This can be seen that the sintering reaction was properly performed above 1400°C due to the addition of Mo metal. The high shrinkage rate before and after the heat treatment means that a large number of pores existing in the molded body were removed by the heat treatment, and as a result, it was found that the density and density characteristics of the sintered body were significantly improved by the heat treatment.
[0155]
[0156] [Experimental Example 4] Evaluation of Sintered Body Resistivity
[0157] The resistivity characteristics of each sintered body sample manufactured in Examples 1 to 5 and Comparative Examples 1 to 2 were evaluated.
[0158] Specifically, the entire sample used for evaluation was used as a sintered body sample, and the resistivity of the sample was measured using the Loresta-GX MCP-T700 product (Mitsubishi Chemical Co., Ltd.). The results are shown in Table 3 below.
[0159] Resistivity characteristics according to sintering temperature (10 -3 Ωcm)1350℃1400℃1425℃1450℃1475℃1500℃1525℃Example 14.5252.5242.5222.6102.5442.625-Example 24.3312.110-2.6652.242--Example 32.1602.340-2.770--1.658Example 4---0.285--1.005Example 5----0.188--Comparative Example 1-Not measurable-Not measurable-2.099-Comparative Example 24.3714.252-4.334-3.778-
[0160] As shown in Table 3 above, it was confirmed that the oxide sintered bodies of Examples 1 to 5 including a predetermined metal dopant had superior resistivity characteristics compared to the sintered bodies of Comparative Examples 1 to 2.
[0161]
[0162] [Experimental Example 5] Evaluation of Thin Film Properties
[0163] After forming a thin film using the sintered bodies manufactured in Examples 1 to 5 and Comparative Example 2 as target materials, the characteristics of the thin film were evaluated as follows.
[0164] Specifically, a thin film was fabricated using each sintered body as a low-reflection layer under the gate layer. This thin film is intended to improve the adhesion of the low-reflection and gate electrodes on the substrate (glass).
[0165] (1) Evaluation of surface resistance characteristics
[0166] The low-reflection thin film was formed by using a DC sputtering target containing the sintered bodies of Comparative Example 2 and Examples 1 to 5 at a power density of 0.5 to 3.6 w / cm. 2 A thin film with a thickness of 100 to 500 Å was deposited on a transparent glass substrate under an argon gas atmosphere. The sheet resistance characteristics of each sample were measured using a CMT-SR5000 product (AIT CO. LTD) for the deposited unit film, and the results are shown in Table 4 and Fig. 6 below.
[0167] Sheet resistance (Ω / sq) according to film thickness 100 Å 200 Å 300 Å 400 Å 500 Å Example 1-258201501013110-Example 3407124181617--Example 433001287836--Example 51105456315--Comparative Example 2--285902172016970
[0168] As shown in Table 4 above, it was found that Examples 3 to 5 had superior low-resistance characteristics compared to Comparative Example 2.
[0169] (2) Reflectance evaluation
[0170] Additionally, electrodes were formed on the aforementioned thin film. The electrodes were formed using a copper (Cu) target using DC sputtering at a power density of 0.5 to 3.6 w / cm. 2 It was formed under an argon gas atmosphere, and the film thickness was 6000 Å.
[0171] In this state, the reflectivity of the thin film was measured on the glass substrate surface. At this time, the reflectivity was measured at an average wavelength of 360 to 740 nm and / or 550 nm, and the results are shown in Figures 7-8.
[0172] As a result of the experiment, it was found that Examples 3 to 5 had superior low-reflection characteristics compared to Comparative Example 2.
[0173]
[0174] [Experimental Example 6] XRD Evaluation of Sintered Body
[0175] XRD analysis was performed to confirm the crystallinity of the oxide sintered bodies according to Example 1, Example 4, Comparative Example 1, and Comparative Example 2, and the results are shown in Figure 9 below.
[0176] Unlike Comparative Examples 1 and 2, which do not contain metal Mo, it can be confirmed that the oxide sintered body of Example 4 has an additional metal Mo phase formed, and it is judged that this reduces movement between particles within the sintered body, thereby reducing the average grain size of the crystal grains (see Fig. 9).
Claims
1. Molybdenum (M1) oxide; niobium (M2) oxide; At least one alkaline earth metal (M3) oxide; and Contains at least one metal (M4) selected from the group consisting of Mo, Ti, Cr, W, and Cu; An oxide sintered body, wherein the metal (M4) is included in an amount of 3 to 60 wt% relative to the total weight of the sintered body.
2. In paragraph 1, An oxide sintered body, wherein the metal (M4) is included in an amount of 5 to 55 wt% relative to the total weight of the sintered body.
3. In paragraph 1, An oxide sintered body, wherein the average grain size (D50) in the oxide sintered body is 80% or less compared to the average grain size (D50) in the oxide sintered body that does not contain metal (M4).
4. In paragraph 1, An oxide sintered body having a surface resistance of 60% or less compared to a surface resistance of an oxide sintered body not containing metal (M4).
5. In paragraph 1, The above oxide sintered body is, Mo (1-x) Nb x An oxide sintered body comprising an O2 (x is 0 to 0.25) crystal phase and a metal (M4) crystal phase.
6. In paragraph 1, The above oxide sintered body is, An oxide sintered body, which is manufactured by mixing molybdenum (M1) oxide; niobium (M2) oxide; at least one alkaline earth metal (M3) oxide; and metal (M4) to form a molded body and then sintering the molded body under atmospheric pressure without applying pressure.
7. In paragraph 1, The above molybdenum oxide (M1) includes at least one of MoO2 and MoO3, An oxide sintered body, which comprises 20 to 70 wt% of the total weight of the oxide sintered body.
8. In paragraph 1, The above molybdenum oxide (M1) and the above niobium oxide (M2) are included in an amount of 45.0 wt% or more and less than 95 wt% based on 100 wt% of the oxide sintered body, An oxide sintered body in which the content ratio of the above molybdenum oxide (M1) and the above niobium oxide (M2) is 80:20 to 45:55 by weight.
9. In paragraph 1, An oxide sintered body, wherein the alkaline earth metal (M3) oxide comprises at least one selected from the group consisting of CaCO3 and MgO.
10. In paragraph 1, An oxide sintered body, wherein the alkaline earth metal (M3) metal oxide (M3) is contained in an amount of more than 0 wt% and less than 10 wt% based on 100 wt% of the oxide sintered body.
11. In paragraph 1, An oxide sintered body comprising at least one alkaline earth metal (M3) metal oxide and the metal (M4) in a weight ratio of 1:1 to 20.
12. In paragraph 6, The average grain size (D50) of the above non-pressurized sintered oxide sintered body is 5 to 30 ㎛, The resistivity is 3×10 -3 Ωcm or less, Oxide sintered body with a relative density of 80% or more.
13. A sputtering target comprising an oxide sintered body according to any one of claims 1 to 12.
14. An oxide thin film formed from the sputtering target of Article 13.
15. In paragraph 14, The light reflectance for a wavelength of 550 nm is less than 25%, Sheet resistance is 2.6×10 at thicknesses of 100 to 500 Å. 4 Oxide thin film with a thickness of less than Ω / sq. 16.(i) A step of preparing and mixing raw material powders containing molybdenum (M1) oxide; niobium (M2) oxide; metal oxide containing at least one alkaline earth metal (M3); and metal (M4) according to a target composition; (ii) a step of manufacturing a molded body using mixed raw material powder; and (iii) a step of manufacturing a sintered body by subjecting the molded body to a non-pressurized heat treatment under atmospheric pressure in an inert atmosphere at 1,200 to 1,600°C for 1 to 20 hours; A method for manufacturing an oxide sintered body of claim 1, comprising:
Citation Information
Patent Citations
Indium tin oxide target, method of manufacturing the same and transparent electrode manufactured by using the same
KR100787635B1
Method of fabricating a sputtering target of molybdenum having ultrafine crystalline and sputtering target of molybdenum prepared thereby
KR1020090053410A
Sputtering target for oxide thin film and process for producing the sputtering target