Drug co-delivery degradable porous microsphere, preparation method therefor, and use thereof
By using degradable polymers to prepare porous microspheres in traditional drug delivery systems, the problem of insufficient drug release at the lesion site is solved, efficient and controllable release of drug molecules and inorganic nanoparticles is achieved, and the therapeutic effect and safety are improved. sex.
Patent Information
- Application Number
- PCT/CN2023/141688
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2023-12-25
- Publication Date
- 2024-10-24
AI Technical Summary
Traditional drug delivery systems are difficult to achieve efficient concentration and long-term stable release of drugs at the lesion site, resulting in limited therapeutic effects and serious side effects.
Porous microspheres are prepared using degradable polymers, by uniformly dispersing drug molecules and inorganic nanoparticles in volatile organic solvents, using the double emulsion-solvent evaporation method to prepare microspheres, and removing the surface continuous film layer and etching by alkali solution treatment. It erodes the internal pores to form a porous structure loaded with drug molecules and embedded with inorganic nanoparticles.
It achieves controlled release of drug molecules and inorganic nanoparticles, improves the bioavailability and targeting of drugs, enhances drug delivery efficiency and safety, and is suitable for the treatment of a variety of chronic diseases.
Smart Images

Figure CN2023141688_24102024_PF_FP_ABST
Abstract
Description
A drug co-delivery degradable porous microsphere and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of biomedical materials, and in particular to a drug co-delivery degradable porous microsphere and a preparation method and application thereof. Background Art
[0002] The main challenges facing drug formulations are enhancing the therapeutic effects of drugs on diseases while minimizing their side effects. Specifically, they aim to deliver drugs to the lesion site to enhance their efficacy while avoiding systemic distribution to minimize damage to normal tissues. Therefore, developing high-load, safe, and controllable drug delivery systems has significant research significance and clinical application value.
[0003] In recent years, research on drug-loaded microsphere dispersions prepared using biodegradable polymer materials as substrates for sustained and controlled drug release has been increasing. Biodegradable polymer materials gradually degrade in the body through reactions such as hydrolysis, oxidation, and enzymatic hydrolysis. While releasing the loaded drug, they also generate small, non-toxic degradation products that are metabolized out of the body. Therefore, compared with non-biodegradable materials, they exhibit improved biocompatibility and biosafety. Microsphere drug delivery systems prepared using biodegradable polymer materials typically have particle sizes ranging from 1 to 500 μm. Their size is highly controllable and amenable to large-scale synthesis and modification. Encapsulating drugs within the microspheres protects them from the effects of the in vivo biological environment, such as enzymatic hydrolysis and gastric acid, prior to release, significantly improving their bioavailability. Furthermore, by varying parameters such as the viscosity and molecular weight of the biodegradable polymer material, the degradation rate of the drug-loaded microspheres can be flexibly controlled, thereby regulating the release rate of the encapsulated drug. This allows for the maintenance of effective drug concentrations at the lesion site over a long period of time, thereby improving drug targeting, delaying or controlling drug release, reducing dosing frequency, and reducing drug toxicity. Drug-loaded microspheres can be administered by injection, oral administration, intranasal drip, subcutaneous implantation, or intra-articular administration. Specific surface modification of the drug-loaded microspheres can also enable active targeting, allowing precise localization to the lesion or altering release behavior. Due to their excellent sustained-release and active targeting properties, microsphere drug delivery systems are currently primarily used for indications requiring frequent and prolonged dosing, such as cancer, Parkinson's disease, analgesia, diabetes, endometriosis, osteoarthritis-related knee pain, and periodontitis. Technical issues
[0004] Due to the good sustained-release ability and active targeting of the microsphere drug delivery system, it is currently mainly used for indications that require long-term and frequent administration, such as tumors, Parkinson's disease, analgesia, diabetes, endometriosis, osteoarthritis-related knee pain, periodontitis, etc. Technical Solutions
[0005] In order to solve the above technical problems, the present invention provides a drug co-delivery degradable porous microsphere and its preparation method and application.
[0006] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0007] The first aspect of the present invention provides a method for preparing drug co-delivery degradable porous microspheres, which includes the following steps: resuspending and uniformly dispersing drug molecules and inorganic nanoparticles in a volatile organic solvent containing a degradable polymer, adding a porogen and using a double emulsion-solvent volatilization method to obtain polymer microspheres; treating the polymer microspheres with an alkaline solution to remove the continuous film layer formed on the outer layer during the microsphere curing process and simultaneously etching the porous structure inside the microspheres, thereby obtaining drug co-delivery degradable porous microspheres that are loaded with drug molecules and embedded with inorganic nanoparticles and partially exposed in a porous skeleton.
[0008] Furthermore, the drug molecules include one or more of anti-inflammatory drugs, anti-osteoporosis drugs, and hypoglycemic drugs; wherein the anti-inflammatory drugs include dexamethasone and aspirin; the anti-osteoporosis drugs include alendronate sodium; and the hypoglycemic drugs include metformin.
[0009] Furthermore, the inorganic nanoparticles include one or more of metal or alloy nanoparticles, oxide nanoparticles, and inorganic salt nanoparticles; wherein the metal or alloy nanoparticles include gold nanoparticles; the oxide nanoparticles include SiO2, TiO2, ZnO, and Fe2O3 nanoparticles; and the inorganic salt nanoparticles include CaCO3 nanoparticles.
[0010] Furthermore, the degradable polymer includes one or more of polycaprolactone (PCL), polyglycolic acid (PGA), polylactic acid (PLA), polylactic acid-glycolic acid copolymer (PLGA), polytrimethylene carbonate (PTMC), and poly 3-hydroxybutyrate (PHB).
[0011] Furthermore, the volatile organic solvent includes one or more of dichloromethane, chloroform, dimethylformamide, xylene, tetrahydrofuran, and ethyl acetate.
[0012] Furthermore, the method specifically includes the following steps: dissolving polylactic acid-glycolic acid copolymer in dichloromethane (DCM) to obtain a dichloromethane solution; adding drug molecules and inorganic nanoparticles to the dichloromethane solution, and ultrasonically treating them in a water bath until they are uniformly dispersed to obtain an oil-phase dichloromethane mixed solution; adding a 0.05wt% ammonium bicarbonate aqueous solution with a volume ratio of 20% to 50% to emulsify the dichloromethane mixed solution to form colostrum; adding the colostrum dropwise to a 1wt% aqueous solution of polyvinyl alcohol under stirring, and stirring at room temperature until the dichloromethane is completely volatilized to obtain polymer microspheres; and adding the polymer microspheres to an alkaline solution for treatment to obtain the drug co-delivery degradable porous microspheres.
[0013] Furthermore, the step of treating the polymer microspheres in an alkaline solution includes treating the polymer microspheres in an aqueous solution containing 0.1 M to 0.5 M NaOH for 3 to 10 minutes. It should be noted that the higher the NaOH concentration and the longer the treatment time, the stronger the etching effect. Therefore, the goal of etching is to eliminate the continuous film layer formed on the microsphere surface and partially etch the microsphere skeleton, while not damaging the overall microsphere structure.
[0014] The second aspect of the present invention provides degradable porous microspheres for drug co-delivery prepared according to the above-mentioned method for preparing degradable porous microspheres for drug co-delivery.
[0015] The third aspect of the present invention provides the use of the above-mentioned drug co-delivery degradable porous microspheres in the field of pharmaceutical preparations.
[0016] The fourth aspect of the present invention provides the use of the above-mentioned degradable porous microspheres for drug co-delivery in the fields of injection, oral administration, nasal drops, subcutaneous implantation or intra-articular administration. Beneficial effects
[0017] The present invention provides a method for preparing degradable porous microspheres that simultaneously load drug molecules and inorganic nanoparticles. First, the drug molecules and inorganic nanoparticles are dispersed in a volatile organic solvent containing a degradable polymer, and a porogen is added before emulsification. The microspheres are then prepared by a double emulsion-dissolution volatilization method. After the volatile organic solvent is evaporated, solidified microspheres are obtained. Subsequently, an alkaline solution is used to remove the continuous film layer formed on the surface of the microspheres during the curing process and to partially etch the internal pore structure of the microspheres, thereby obtaining degradable porous microspheres that simultaneously load drug molecules and inorganic nanoparticles. By controlling the amount of drug molecules and inorganic nanoparticles added during the microsphere preparation process, their release trends can be regulated respectively; by controlling the stirring speed during the double emulsion process, the particle size of the microspheres can be regulated; by controlling the concentration of the alkaline solution and the treatment time parameters, the surface and internal pore structure of the microspheres and the exposure degree of the inorganic nanoparticles can be regulated, thereby regulating the degradation trend and release trend of the microspheres.
[0018] The present invention provides a method for preparing degradable porous microspheres that simultaneously load drug molecules and inorganic nanoparticles, which has the following advantages:
[0019] 1) The porous microspheres prepared by the present invention simultaneously load drug molecules and inorganic nanoparticles;
[0020] 2) The porous microspheres prepared by the present invention have uniformly distributed internal pores and a porous surface, thereby increasing the efficiency of material exchange between the interior of the microspheres and the outside world;
[0021] 3) In the porous microspheres prepared by the present invention, the inorganic nanoparticles are embedded in the porous structure skeleton and partially exposed, which is conducive to the presentation of the physical properties of the nanoparticles;
[0022] 4) The microsphere preparation method of the present invention is based on the double emulsion-solvent evaporation method, which has a simple process and low cost, and is easy to achieve large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] FIG1 is a scanning electron microscope photograph of SiO2 nanoparticles used in Example 1;
[0024] FIG2 a is a scanning electron micrograph of the PLGA microspheres prepared in Example 3 (magnification 100);
[0025] FIG2 b is a scanning electron micrograph of the PLGA microspheres prepared in Example 3 (magnification 500);
[0026] FIG2 c is a scanning electron micrograph of the PLGA microspheres prepared in Example 3 (magnification 2000);
[0027] FIG2 d is a scanning electron micrograph of the PLGA microspheres prepared in Example 3 (magnification 5000);
[0028] FIG3 a is a scanning electron micrograph of the PLGA microspheres prepared in Example 4 (magnification 100);
[0029] FIG3 b is a scanning electron micrograph of the PLGA microspheres prepared in Example 4 (magnification 500);
[0030] FIG3 c is a scanning electron micrograph of the PLGA microspheres prepared in Example 4 (magnification 2000);
[0031] FIG3 d is a scanning electron micrograph of the PLGA microspheres prepared in Example 4 (magnification 5000);
[0032] FIG3 e is a scanning electron micrograph of the interior of the PLGA microspheres prepared in Example 4 (magnification 500);
[0033] FIG3 f is a scanning electron micrograph of the interior of the PLGA microspheres prepared in Example 4 (magnification 2000);
[0034] FIG3 g is a scanning electron micrograph of the interior of the PLGA microspheres prepared in Example 4 (magnification 5000);
[0035] FIG3h is a scanning electron micrograph of the interior of the PLGA microspheres prepared in Example 4 (magnification 10000);
[0036] FIG4 shows the release trend of the loaded drug molecule dexamethasone during incubation of the microspheres with different treatments in phosphate buffer in Example 5. Modes for Carrying Out the Invention
[0037] The inventors have discovered that drug molecules, after intravenous injection or oral administration, are distributed systemically, have a short half-life, making it difficult to achieve sustained therapeutic concentrations. Clinical applications have shown limited therapeutic efficacy and severe side effects. To overcome these obstacles, numerous drug carriers have been developed, such as liposomes, hydrogels, and microspheres. Compared to other carriers, microsphere drug delivery systems based on degradable polymer materials offer numerous advantages, including biodegradability, good biocompatibility, high drug loading capacity, and high encapsulation efficiency. More importantly, the encapsulated drug is released through degradation or erosion of the polymer matrix, allowing controlled and sustained release of drug molecules by manipulating the degradation behavior of the polymer matrix. The shape, size, and surface topology of polymer microspheres profoundly influence their biological effects. Currently used drug delivery systems are mostly solid microspheres. In contrast, porous microspheres offer a larger specific surface area and interconnected internal and external pore structures, which facilitate drug delivery and transport. Modulating the particle size and pore size of the porous microspheres allows for effective regulation of drug release rate.
[0038] Inorganic nanoparticles are another type of pharmaceutical agent that has been widely used clinically. Inorganic nanoparticles have the advantages of large specific surface area, easy surface modification, and adjustable size. They not only provide a large number of adsorption sites for drug molecules and exogenous genes to achieve the purpose of drug and gene therapy, but can also be modified with molecules with different targeting functions, thereby improving the specific recognition and treatment of tumor cells. In addition, inorganic nanoparticles possess a range of excellent physical properties, such as optical and magnetic properties, and have been widely used in cancer chemotherapy, gene therapy, phototherapy, and magnetic hyperthermia. For example, gold nanoparticles have a high photothermal conversion efficiency and can be used for photothermal ablation of tumors under near-infrared laser irradiation. Superparamagnetic nanoiron oxide has excellent magnetic properties and good biocompatibility, and can be used as a contrast agent for drug delivery and cancer magnetic resonance imaging diagnosis.
[0039] Based on the above background and current situation, the present invention provides a method for preparing a biodegradable porous microsphere delivery system capable of simultaneously loading drug molecules and inorganic nanoparticles. The resulting drug molecule and inorganic nanoparticle co-delivery system can overcome the limitations and obstacles of traditional drug delivery methods, providing the possibility of multi-factor, multi-drug synergistic treatment.
[0040] The present invention provides a method for preparing biodegradable porous microspheres that simultaneously load drug molecules and inorganic nanoparticles. The porous microspheres have a uniform, interconnected pore structure. The porous microsphere matrix is loaded with drug molecules, and the pore framework is embedded with inorganic nanoparticles, enabling controlled delivery and release of both drug molecules and inorganic nanoparticles. This porous microsphere delivery system boasts high drug loading, a simple and economical preparation process, and is suitable for mass production.
[0041] The present invention is described in detail below with reference to specific embodiments. In the following examples, the steroidal anti-inflammatory drug dexamethasone (DEX) was selected as the drug molecule and SiO2 nanoparticles were selected as the inorganic nanoparticles. Both substances were simultaneously loaded into porous microspheres made of a biodegradable polymer, PLGA, to demonstrate the feasibility of the method described herein.
[0042] Example 1
[0043] First, PLGA was dissolved in the volatile organic solvent DCM to obtain a 5 wt% DCM solution. DEX and SiO2 nanoparticles were then added to the DCM solution, achieving a DEX and SiO2 mass fraction relative to PLGA of 5% and 0.5%, respectively. The solution was then ultrasonicated in a water bath for 5 minutes to uniformly disperse the drug molecules and SiO2 nanoparticles in the DCM solution, resulting in a DCM mixed solution. Figure 1 shows a scanning electron micrograph of the SiO2 nanoparticles used, demonstrating a uniform particle size distribution of approximately 100 nm.
[0044] Example 2
[0045] Prepare a 0.05 wt% aqueous solution of ammonium bicarbonate as a porogen. Add 1.5 mL of this 0.05 wt% aqueous solution to 5 mL of the DCM mixed solution from Example 1, then emulsify using ultrasonic probes. Under ultrasonic waves, the ammonium bicarbonate rapidly decomposes into large amounts of NH3 and CO2. A small portion of the NH3 and CO2 dissolves in water, while the remaining gas is sequestered by the oil phase under ultrasonic waves, resulting in a large amount of milky white water-in-oil (W / O) primary emulsion.
[0046] Example 3
[0047] Polyvinyl alcohol (PVA) was used as an emulsifier. Its molecular chains contain both hydrophilic and hydrophobic moieties, allowing it to form a thin film at the oil-water interface. This protects the oil phase droplets during magnetic stirring, further stabilizing them and improving the sphericity and dispersibility of the prepared microspheres. 5 g of PVA was dissolved in 500 mL of deionized water. The water-in-oil primary emulsion obtained in Example 2 was added dropwise while maintaining magnetic stirring to form a water-in-oil-in-water (W / O / W) double emulsion. Stirring was continued at room temperature for at least 4 hours until the DCM in the solution completely evaporated, resulting in solidified PLGA microspheres. The microspheres were then washed with deionized water at least three times.
[0048] The surface morphology of the microspheres was observed using a scanning electron microscope. As shown in Figures 2a to 2d, although the obtained PLGA microspheres had a porous structure inside, a continuous thin film was formed on the surface of the microspheres.
[0049] Example 4
[0050] The microspheres prepared in Example 3 were subjected to alkaline etching. The microspheres were resuspended in an aqueous solution containing 0.1 M sodium hydroxide (NaOH) and stirred at room temperature for 5 minutes. The microspheres were then washed three or more times with deionized water. NaOH promotes hydrolysis of the PLGA microsphere surface, removing the continuous film formed on the microsphere surface during the curing process. It also exposes a portion of the SiO2 nanoparticles loaded in the polymer matrix, allowing them to be embedded in the porous framework structure.
[0051] The surface morphology of the microspheres was observed using a scanning electron microscope. As shown in Figures 3a to 3d, after NaOH alkaline etching, the continuous film layer on the surface of the microspheres disappeared, increasing the pore structure on the surface of the microspheres, thereby enhancing the material exchange capacity between the microspheres and the outside world, that is, the drug delivery efficiency. In addition, the SiO2 nanoparticles loaded inside the PLGA substrate were partially exposed. Further observation of the interior of the microspheres, as shown in Figures 3e to 3h, shows that the pores inside the microspheres are intertwined and evenly distributed, and some SiO2 nanoparticles are exposed and embedded in the porous skeleton.
[0052] Example 5
[0053] The microspheres in Example 3 (Before treatment) and the microspheres in Example 4 (After treatment) were respectively added to dialysis bags and placed in 30 mL of phosphate buffered saline (PBS). The mixture was shaken and incubated at 37°C. 5 mL of dialysate was periodically collected and supplemented with an equal amount of fresh PBS. The concentration of dexamethasone released from the microspheres in the dialysate was detected, and a release curve was plotted.
[0054] Figure 4 shows the release curves of dexamethasone loaded into the two microspheres. It can be seen that after alkaline etching, the release rate of dexamethasone is faster than before treatment due to the higher mass transfer efficiency between the porous microspheres and the external solution.
[0055] In summary, the present invention provides a method for preparing degradable porous microspheres that simultaneously load drug molecules and inorganic nanoparticles. The drug molecules and inorganic nanoparticles are uniformly dispersed in a volatile organic solvent containing a degradable polymer, and after preparing polymer microspheres by a double emulsion-solvent evaporation method, the polymer microspheres are treated with an alkaline solution. Without affecting the basic configuration of the microspheres, the continuous film layer formed on the outer surface of the microspheres during the curing process is removed, and the inorganic nanoparticles loaded in the polymer are partially exposed, thereby obtaining porous microspheres with a highly interconnected porous structure that are loaded with drug molecules and embedded with inorganic nanoparticles on the porous skeleton.
[0056] Those skilled in the art will appreciate that the above-described embodiments are specific examples for implementing the present application, and that in actual applications, various changes in form and detail may be made thereto without departing from the spirit and scope of the present application. Any person skilled in the art may make changes and modifications without departing from the spirit and scope of the present application. Therefore, the scope of protection of the present application shall be subject to the scope defined in the claims.
Claims
1. A method for preparing degradable porous microspheres for drug co-delivery, characterized in that: The method comprises the following steps: The drug molecules and inorganic nanoparticles are resuspended and uniformly dispersed in a volatile organic solvent containing a degradable polymer, and a porogen is added and then a double emulsion-solvent evaporation method is used to obtain polymer microspheres; The polymer microspheres are treated with an alkaline solution to remove the continuous film layer formed on the outer surface during the microsphere solidification process and to simultaneously etch the porous structure inside the microspheres, thereby obtaining drug co-delivery degradable porous microspheres loaded with drug molecules and inlaid with inorganic nanoparticles and partially exposed in the porous skeleton.
2. The method for preparing drug co-delivery degradable porous microspheres according to claim 1, characterized in that: The drug molecules include one or more of anti-inflammatory drugs, anti-osteoporosis drugs, and hypoglycemic drugs; wherein the anti-inflammatory drugs include dexamethasone and aspirin; the anti-osteoporosis drugs include sodium alendronate; and the hypoglycemic drugs include metformin.
3. The method for preparing drug co-delivery degradable porous microspheres according to claim 1, characterized in that: The inorganic nanoparticles include one or more of metal or alloy nanoparticles, oxide nanoparticles, and inorganic salt nanoparticles; wherein the metal or alloy nanoparticles include gold nanoparticles; the oxide nanoparticles include SiO2, TiO2, ZnO, and Fe2O3 nanoparticles; and the inorganic salt nanoparticles include CaCO3 nanoparticles.
4. The method for preparing drug co-delivery degradable porous microspheres according to claim 1, characterized in that: The degradable polymer includes one or more of polycaprolactone, polyglycolic acid, polylactic acid, polylactic acid-co-glycolic acid, polytrimethylene carbonate, and poly-3-hydroxybutyrate.
5. The method for preparing drug co-delivery degradable porous microspheres according to claim 1, characterized in that: The volatile organic solvent includes one or more of dichloromethane, chloroform, dimethylformamide, xylene, tetrahydrofuran, and ethyl acetate.
6. The method for preparing drug co-delivery degradable porous microspheres according to claim 1, characterized in that: The method specifically comprises the following steps: dissolving poly(lactic acid-co-glycolic acid) in dichloromethane to obtain a dichloromethane solution; Adding drug molecules and inorganic nanoparticles to the dichloromethane solution, and subjecting the solution to ultrasonic treatment in a water bath until the solution is uniformly dispersed, thereby obtaining an oil phase dichloromethane mixed solution; Adding 20% to 50% by volume of an aqueous solution of ammonium bicarbonate with a concentration of 0.05 wt % to the dichloromethane mixed solution for emulsification to form colostrum; The colostrum is added dropwise into a 1 wt % aqueous solution of polyvinyl alcohol under stirring, and stirred at room temperature until the dichloromethane is completely evaporated, thereby obtaining polymer microspheres; The polymer microspheres are added into an alkaline solution for treatment to obtain the drug co-delivery degradable porous microspheres.
7. The method for preparing drug co-delivery degradable porous microspheres according to claim 6, characterized in that: The step of adding the polymer microspheres to an alkaline solution for treatment includes: adding the polymer microspheres to an aqueous solution containing 0.1 M to 0.5 M NaOH for treatment for 3 to 10 minutes. 8 . Degradable porous microspheres for drug co-delivery obtained by the method for preparing degradable porous microspheres for drug co-delivery according to any one of claims 1 to 7.
9. Use of the drug co-delivery degradable porous microspheres as claimed in claim 8 in the field of pharmaceutical preparations.
10. Use of the drug co-delivery degradable porous microspheres as claimed in claim 8 in the fields of injection, oral administration, nasal drops, subcutaneous implantation or intra-articular administration.
Citation Information
Patent Citations
Preparation of degradable pollutant polyalcohol stephanoporate microballoons and uses thereof
CN101249077A
Preparation method of organic / inorganic hybrid nano fiber drug carrying microsphere
CN103800292A
Hierarchical porous polylactic acid drug carrier and preparation method thereof
CN104784698A
Method for preparing PLGA microspheres with porous surfaces
CN105664242A
Drug co-delivery degradable porous microsphere as well as preparation method and application thereof
CN116747318A