Low-temperature-sintering bonding material and bonded structure

A low-temperature sinterable bonding material with silver and silicon particles forming an atomic interface addresses the reliability and manufacturing complexity issues in bonding semiconductor elements, achieving strong and thermally stable bonds.

WO2024219382A1PCT designated stage expired Publication Date: 2024-10-24DAICEL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015092
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-04-16
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Current low-temperature sinterable bonding materials face challenges in achieving high reliability and ease of preparation for bonding semiconductor elements like SiC chips to substrates, with issues such as thermal fatigue and cracking due to the large thermal expansion coefficient difference between SiC and metals like silver, and the complexity of manufacturing processes for coated silver particles.

Method used

A low-temperature sinterable bonding material comprising silver particles and silicon particles, where more than 50% of the silicon particles' surface is composed of silicon atoms, with a preferred ratio of silver to silicon forming an interface at the atomic level during sintering, enhancing bonding strength and thermal conductivity while simplifying the manufacturing process.

Benefits of technology

The proposed bonding material allows for reliable bonding at low temperatures, reducing the likelihood of cracking and improving thermal fatigue resistance, with enhanced mechanical and thermal properties, and a simplified preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015092_24102024_PF_FP_ABST
    Figure JP2024015092_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a low-temperature-sintering bonding material that is easy to prepare and that, when used for sintering bonding, enables sintering at low temperatures and can provide highly reliable bonded structures. A low-temperature-sintering bonding material according to an embodiment contains silver particles and silicon particles, and more than 50% of the surface of the silicon particles is composed of silicon atoms. A low-temperature-sintering bonding material according to another embodiment contains silver particles and silicon particles, wherein sintering brings about the formation of an interface at the atomic level between the silver constituting the silver particles and the silicon constituting the silicon particles.
Need to check novelty before this filing date? Find Prior Art

Description

Low-temperature sinterable joining material and joined structure

[0001] The present invention relates to a low-temperature sinterable bonding material and a bonded structure (bonded body) used for bonding semiconductor elements and heat dissipation substrates. This application claims priority from Japanese Patent Application No. 2023-068160, filed on April 18, 2023, the contents of which are incorporated herein by reference.

[0002] In semiconductor devices that mount electronic components such as semiconductor elements on metal substrates such as copper substrates, the electronic components are fixed with solder. In recent years, in consideration of the burden on the human body and the environment, a shift from conventional lead-containing solder to lead-free solder has been underway. Recently, the use of SiC chips, which have lower loss and superior characteristics than the widely used Si chips, as semiconductor chips has been considered. However, semiconductor devices with SiC chips mounted on substrates can operate at temperatures exceeding 200°C. Therefore, solder with a high melting point must be used to fix the SiC chips to the substrate, but solder with a high melting point is difficult to make lead-free.

[0003] In recent years, when die-bonding (die-attaching) semiconductor elements that operate at high temperatures, such as SiC chips, sinter bonding has been considered, in which a metal paste containing nano-sized or micro-sized particles of silver or copper is used as a bonding material, and the bonding material is interposed between objects to be bonded and heated for a predetermined time to sinter the metal, such as silver, in the bonding material, thereby bonding the objects to be bonded together with a metal bonding layer (see, for example, Patent Document 1). This metal bonding technology is expected to be applied to various electronic elements, such as power semiconductor elements and LED elements.

[0004] However, metals such as silver are too hard as die-attach materials, and the difference in thermal expansion coefficient between a semiconductor element such as Si or SiC and a metal layer such as silver is very large, so in thermal fatigue tests above 200°C, cracks develop in the sintered portion, and insulating substrates such as the semiconductor element and DBC (Direct Bonded Copper) break, resulting in insufficient reliability. Furthermore, when metal is used as the bonding material, the only way to improve bonding strength and heat resistance is to control the density of the sintering, which does not essentially change the mechanical properties of the bonded body.

[0005] Also known is a low-temperature sinterable joining paste containing silver powder (A) and silver-coated particles of an element other than silver (B) (see Patent Document 2). When used for sinter joining, the low-temperature sinterable joining paste allows sintering at low temperatures, and a highly reliable joined structure can be obtained.

[0006] JP 2011-80147 A International Publication No. 2021 / 039874

[0007] However, the low-temperature sinterable bonding paste of Patent Document 2 requires the preparation of elementary particles other than silver coated with silver, and there is room for improvement in the manufacturing process of the low-temperature sinterable bonding paste.

[0008] Therefore, an object of the present disclosure is to provide a low-temperature sinterable joining material that can be sintered at a low temperature when used in sinter joining, can produce a highly reliable joined structure, and is easy to prepare. Another object of the present disclosure is to provide a highly reliable joined structure that is easy to fabricate.

[0009] As a result of intensive research to solve the above problems, the inventors of the present disclosure have found that when a specific low-temperature sinterable bonding material containing silver particles and silicon particles is used for sinter bonding, it is possible to easily prepare the material, sinter it at a low temperature, and obtain a highly reliable bonded structure. The present invention has been completed based on these findings.

[0010] That is, the present disclosure provides a low-temperature sinterable joining material comprising silver particles and silicon particles, with more than 50% of the surfaces of the silicon particles being composed of silicon atoms.

[0011] Preferably, 60% or more of the silicon particles are composed of silicon atoms.

[0012] The average particle size of the silicon particles is preferably 0.05 to 40 μm.

[0013] It is preferable that an interface be formed at the atomic level between the silver constituting the silver particles and the silicon constituting the silicon particles by sintering.

[0014] The average particle size of the silver particles is preferably 0.5 to 40 μm.

[0015] The silver particles are preferably in the form of flakes.

[0016] The present disclosure also provides a low-temperature sinterable bonding material that includes silver particles and silicon particles, and in which, upon sintering, the silver that constitutes the silver particles and the silicon that constitutes the silicon particles form an interface at the atomic level.

[0017] It is preferable that, as a result of the sintering, 10% or more of the surface of the silicon particles forms the interface with the silver particles.

[0018] It is preferable that, as a result of the sintering, 40% or more of the surface of the silicon particles forms the interface with the silver particles.

[0019] The present disclosure also provides a low-temperature sinterable bonding material comprising silver particles and silicon particles, wherein the average particle size of the silicon particles is at least 1 / 20 of the average particle size of the silver particles, and the content of the silicon particles relative to the total of the silver particles and the silicon particles is 10 to 70 volume %.

[0020] The average particle size of the silicon particles is preferably 0.05 to 40 μm.

[0021] The average particle size of the silver particles is preferably 0.1 to 50 μm.

[0022] The low-temperature sinterable joining material is preferably in the form of a paste or a sheet.

[0023] The present disclosure also provides a bonded structure in which an object to be bonded is bonded to a substrate via a silver bonding layer containing a sintered body of the above-mentioned low-temperature sinterable bonding material.

[0024] The low-temperature sinterable bonding material of the present disclosure is easy to prepare, yet can be sintered at low temperatures, and can provide a highly reliable bonded structure. As a result, the resulting bonded structure is less susceptible to problems such as cracks developing in the sintered portion and cracks in the bonded objects, such as semiconductor elements (e.g., Si or SiC) or substrates (e.g., DBCs).

[0025] 1 is a cross-sectional view showing one embodiment of a bonded structure according to the present disclosure. 2 is a TEM image of a cross section of the bonded structure obtained in Example 1.

[0026] [Low-Temperature Sinterable Bonding Material] The low-temperature sinterable bonding material according to one embodiment of the present disclosure contains at least silver particles and silicon particles. The silver particles and the silicon particles may each contain only one type, or two or more types.

[0027] (Silver Particles) The average particle size (median diameter; D50) of the silver particles is preferably 0.1 to 50 μm, more preferably 0.5 to 40 μm, even more preferably 0.5 to 20 μm, and particularly preferably 1 to 5 μm. When the average particle size is 0.1 μm or more, the conductivity of the sintered portion formed by sintering is superior. When the average particle size is 50 μm or less, problems such as cracks developing in the sintered portion and cracking of the substrates to be bonded, such as semiconductor elements such as Si or SiC, or DBC, are less likely to occur. The average particle size of the silver particles can be measured by laser diffraction / scattering.

[0028] The specific surface area of ​​the silver particles is 0.5 to 4.0 m 2 / g, and more preferably 0.6 to 3.0 m 2 / g, more preferably 0.7 to 2.5 m 2 / g, particularly preferably 0.8 to 2.0 m 2 The specific surface area of ​​the silver particles can be measured by the BET method.

[0029] Examples of the shape of the silver particles include spherical, flake (flat), and polyhedral shapes. Silver particles of different shapes may be used in combination, or only silver particles of the same shape may be used. The shape of the silver particles is preferably flake. When flake-shaped silver particles are used, many crystal grain boundaries formed during flake formation are contained within the particles, which promotes crystal coarsening during heating and promotes sintering.

[0030] When flake-shaped silver particles are used, their average diameter is preferably 0.5 to 10 μm, more preferably 2 to 8 μm, and even more preferably 3 to 7 μm. When flake-shaped particles are used, their average thickness is preferably 30 nm to 2 μm, more preferably 80 nm to 1 μm, and even more preferably 100 nm to 700 nm. When flake-shaped particles are used, their aspect ratio is preferably 3 to 70, more preferably 5 to 50, and even more preferably 7 to 20.

[0031] As the silver particles, commercially available products may be used, such as those under the trade name "AgC-239" (manufactured by Fukuda Metal Foil and Powder Co., Ltd.).

[0032] (Silicon Particles) Silicon particles are particles containing silicon atoms as a constituent component. The proportion of silicon atoms in the silicon particles is preferably 50% or more (for example, 50 to 100%), more preferably 60% or more, even more preferably 70% or more, even more preferably 80% or more, even more preferably 90% or more, and particularly preferably 95% or more.

[0033] Preferably, more than 50% of the surface of the silicon particles is composed of silicon atoms. That is, the proportion of silicon atoms on the silicon particle surface is preferably 50% or more (e.g., 50 to 100%), more preferably 60% or more, even more preferably 70% or more, even more preferably 90% or more, and particularly preferably 95% or more. The proportion R (%) of silicon atoms on the silicon particle surface can be determined as the proportion of the Si layer on the powder surface from a cross-sectional image of the powder particle taken at 1000 to 10,000 magnifications by SEM observation.

[0034] Before sintering, when silicon particles whose surfaces are coated with Ag are used, an interface between Ag and Si (a state in which Ag and Si are bonded without mixing) is not formed at the atomic level. Furthermore, the Ag coating on the silicon particle surface covers the silicon particles, reducing the opportunity for activated silver particles to directly contact the silicon particle surface during the sintering process and inhibiting the formation of an interface between Ag and silicon particles at the atomic level. Furthermore, the Ag coating on the surface of the silicon particles undergoes intense atomic diffusion between the Ag coating portions during sintering, causing the Ag coating to coarsen and become granular before forming an interface with the silicon particles. Although the silicon particles were coated with Ag before sintering, the Ag coating on the silicon particles eventually peeled off from the silicon particles during sintering. In contrast, by using silicon particles whose surface is composed of more than 50% silicon atoms, an interface is formed at the atomic level between the silver constituting the silver particles and the silicon constituting the silicon particles after sintering, and peeling of Ag from the silicon particles can be prevented.

[0035] While it is difficult to form an interface between Ag and Si at the atomic level using the Ag coating technology on silicon particles in a ball mill, an interface between Ag and silicon particles at the atomic level can be formed by directly reacting silver particles activated at a low temperature of around 300°C during the sintering process without coating the silicon particles with silver in advance.

[0036] The average particle size (median diameter; D50) of the silicon particles is preferably 0.05 to 40 μm, more preferably 0.01 to 30 μm, even more preferably 1 to 20 μm, and particularly preferably 5 to 15 μm. When the average particle size is within the above range, problems such as cracks developing in the sintered part and cracking of the substrates to be joined, such as semiconductor elements such as Si or SiC, or DBC, are less likely to occur. The average particle size of the silicon particles can be measured by laser diffraction / scattering.

[0037] Examples of the shape of the silicon particles include spherical, flake (flat), polyhedral, etc., and different shapes may be used in combination, or only particles of the same shape may be used. The shape of the silicon particles is preferably spherical or polyhedral, in order to maintain uniform dispersion of the particles during the paste application process when forming the bonded portion. In particular, the thermal conductivity of the bonding material is very important at the bonded portions of semiconductors and heat sinks of power devices. Silicon particles, which have lower thermal conductivity than silver particles, should have a shape that reduces the surface area per volume in order to suppress the decrease in thermal conductivity, and ideally, a spherical shape is preferable.

[0038] As the silicon particles, commercially available products such as commercially available silicon particles that have not been surface-treated or commercially available silicon particles that have been surface-treated over an area ratio of 50% or less of the particle surface may be used. Alternatively, for example, powder obtained by pulverizing commercially available Si ingots of about several mm in size using a ball mill may also be used.

[0039] The average particle size of the silicon particles is preferably 1 / 20 or more of the average particle size of the silver particles, more preferably 1 / 10 or more, and even more preferably 1 / 3 or more. When the average particle size of the silicon atoms is 1 / 20 or more, it not only does not inhibit the sintering of the silver particles with the silver particles, but also serves as a heat-dissipating conductive path without inhibiting the sintering of the silver particles themselves, and it also promotes the sintering of the silver particles that form the tangles between the joints, thereby achieving a good bonding state. Note that when the particles are not spherical but, for example, flake-shaped, the flake particles are considered to be disk-like, and the volume is calculated from their average diameter and thickness, and the value converted to the volume in a spherical shape is used as the average diameter.

[0040] Preferably, the silver particles and silicon particles are sintered so that an interface is formed at the atomic level between the silver constituting the silver particles and the silicon constituting the silicon particles. By forming such an interface, the Ag-Si interface is stable and interfacial delamination can be suppressed when stress occurs at the joint due to environmental changes. The interface is preferably formed over 10% or more of the surface of the silicon particles, more preferably 20% or more, and even more preferably 40% or more. The formation of the interface can be determined by observing the interface at a magnification of, for example, 50,000x using a field emission scanning electron microscope (FE-SEM), and observing a representative interface at a magnification of, for example, 100,000x using a TEM. If there is no gap of 1 nm or more between the Si and Ag at the interface, or if there is no gap of 1 nm or more between the Si and Ag through a metal layer or oxide phase mainly composed of Ag or Si, the interface can be determined to be formed at the atomic level. Furthermore, the proportion of the silicon particle surface that forms the interface can be measured by observing the cross section of the joint using an FE-SEM, and then observing a representative interface using a TEM to confirm the formation of an Ag / Si interface at the atomic level, and then confirming the overall image of the silicon particle using an FE-SEM, and manually measuring the area of ​​the Ag-Si interface that does not have gaps of 10 nm or more at a magnification of, for example, 20,000 times or more, at which gaps of 10 nm can be confirmed.

[0041] The content of silicon particles relative to the total of silver particles and silicon particles is preferably 10 to 70% by volume, more preferably 20 to 50% by volume, and even more preferably 30 to 40% by volume. When the content is 10% or more, problems such as cracks developing in the sintered part and cracking of the bonded object, such as a semiconductor element (e.g., Si or SiC) or a substrate (e.g., DBC), are less likely to occur. When the content is 70% or less, the conductivity of the sintered part formed by sintering is superior. Specifically, when the content is 70% or less by volume, a relatively sufficient amount of Ag network structure can be secured in the sintered bonded part, resulting in extremely excellent bond strength, a sufficient heat dissipation path through the Ag layer, and excellent thermal conductivity.

[0042] The low-temperature sinterable bonding material may contain conductive particles other than silver particles and silicon particles (hereinafter, sometimes referred to as "other conductive particles"). The total content of silver particles and silicon particles is, for example, 75% by mass or more, preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, based on the total amount of conductive particles contained in the low-temperature sinterable bonding material. When the silver particles and silicon particles are contained in the above ranges, a bonded structure with particularly excellent electrical properties can be formed.

[0043] The form of the low-temperature sinterable bonding material is not particularly limited, but examples thereof include a composition containing organic components such as a solvent (medium) and a binder component (low-temperature sinterable bonding ink composition), and a sheet-like material (low-temperature sinterable bonding sheet).

[0044] The low-temperature sinterable bonding ink composition can take various forms without any particular limitation. For example, an ink composition called a metal ink can be prepared by dispersing silver particles and silicon particles in a suspension state in an appropriate solvent (dispersion medium, particularly an organic solvent). Alternatively, an ink composition called a paste (low-temperature sinterable bonding paste) can be prepared by dispersing silver particles and silicon particles in a kneaded state in a solvent.

[0045] In the above-mentioned low-temperature sinterable bonding paste, the total content of silver particles and silicon particles relative to the total amount of the low-temperature sinterable bonding paste is preferably 75 to 95% by mass, more preferably 80 to 93% by mass, and even more preferably 85 to 90% by mass.

[0046] (Solvent) The low-temperature sinterable bonding ink composition generally contains a solvent. As the solvent, a solvent generally used in conductive pastes can be used. Examples of such solvents include dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoisopropyl ether, dipropylene glycol monobutyl ether, dipropylene glycol monoisobutyl ether, dipropylene glycol monopentyl ether, and dipropylene glycol monoisopentyl ether. 1-6 Alkyl ethers: dipropylene glycol dimethyl ether, dipropylene glycol methyl ethyl ether, dipropylene glycol methyl propyl ether, dipropylene glycol methyl butyl ether, dipropylene glycol methyl isobutyl ether, dipropylene glycol methyl pentyl ether, dipropylene glycol methyl isopentyl ether, dipropylene glycol diethyl ether, dipropylene glycol ethyl propyl ether, dipropylene glycol ethyl butyl ether, dipropylene glycol ethyl isobutyl ether, dipropylene glycol ethyl pentyl ether, dipropylene glycol ethyl isopentyl ether, dipropylene glycol dipropyl ether Dipropylene glycol di-C such as dipropylene glycol propyl butyl ether, dipropylene glycol propyl isobutyl ether, dipropylene glycol propyl pentyl ether, dipropylene glycol propyl isopentyl ether, dipropylene glycol dibutyl ether, dipropylene glycol diisobutyl ether, dipropylene glycol butyl isobutyl ether, dipropylene glycol butyl pentyl ether, dipropylene glycol butyl isopentyl ether, dipropylene glycol isobutyl pentyl ether, dipropylene glycol isobutyl isopentyl ether, dipropylene glycol dipentyl ether, and dipropylene glycol pentyl isopentyl ether 1-6 Alkyl ethers and the like (including isomers).

[0047] Further, examples of the solvent include tripropylene glycol mono C ethers such as tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, tripropylene glycol monopropyl ether, tripropylene glycol monoisopropyl ether, tripropylene glycol monobutyl ether, tripropylene glycol monoisobutyl ether, tripropylene glycol monopentyl ether, and tripropylene glycol monoisopentyl ether. 1-6 Alkyl ethers: tripropylene glycol dimethyl ether, tripropylene glycol methyl ethyl ether, tripropylene glycol methyl propyl ether, tripropylene glycol methyl butyl ether, tripropylene glycol methyl isobutyl ether, tripropylene glycol methyl pentyl ether, tripropylene glycol methyl isopentyl ether, tripropylene glycol diethyl ether, tripropylene glycol ethyl propyl ether, tripropylene glycol ethyl butyl ether, tripropylene glycol ethyl isobutyl ether, tripropylene glycol ethyl pentyl ether, tripropylene glycol ethyl isopentyl ether, tripropylene glycol dipropyl ether tripropylene glycol di-C such as tripropylene glycol propyl butyl ether, tripropylene glycol propyl isobutyl ether, tripropylene glycol propyl pentyl ether, tripropylene glycol propyl isopentyl ether, tripropylene glycol dibutyl ether, tripropylene glycol diisobutyl ether, tripropylene glycol butyl isobutyl ether, tripropylene glycol butyl pentyl ether, tripropylene glycol butyl isopentyl ether, tripropylene glycol isobutyl pentyl ether, tripropylene glycol isobutyl isopentyl ether, tripropylene glycol dipentyl ether, and tripropylene glycol pentyl isopentyl ether 1-6 Alkyl ethers and the like (including isomers).

[0048] Further, examples of the solvent include ethylene glycol mono-C ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, and ethylene glycol monohexyl ether. 1-6 Alkyl ethers: ethylene glycol di-C such as ethylene glycol methyl n-propyl ether, ethylene glycol methyl n-butyl ether, and ethylene glycol methyl isoamyl ether 1-6 Alkyl ethers: diethylene glycol mono C such as diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monoisopropyl ether, and diethylene glycol monobutyl ether 1-6 Alkyl ethers: diethylene glycol di-C such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol isopropyl methyl ether, and diethylene glycol methyl-n-butyl ether 1-6 Alkyl ethers: triethylene glycol monomethyl ether, triethylene glycol monobutyl ether, and other triethylene glycol mono-C 1-6 Alkyl ethers; triethylene glycol di-C such as triethylene glycol methyl-n-butyl ether 1-10 Alkyl ethers and the like (including isomers).

[0049] Further, as the solvent, for example, C esters such as ethylene glycol monomethyl ether acetate, ethylene glycol monobutyl ether acetate, and propylene glycol monomethyl ether acetate are usable. 2-3 Alkylene glycol C 1-6 Alkyl Ether C 1-10 Alkyl esters: di-C alkyl esters such as diethylene glycol-n-butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, and dipropylene glycol methyl ether acetate2-3 Alkylene glycol C 1-6 Alkyl Ether C 1-10 Alkyl esters: triethylene glycol n-butyl ether acetate, triethylene glycol ethyl ether acetate, triethylene glycol butyl ether acetate, tripropylene glycol methyl ether acetate, and other tri-C 2-3 Alkylene glycol C 1-6 Alkyl Ether C 1-10 Alkyl esters; C such as propylene glycol diacetate 2-3 Alkylene glycol di C 1-10 Alkyl esters and the like (including isomers).

[0050] Other examples of the solvent that can be used include ethyl acetate lactate, tetrahydrofurfuryl acetate, tetrahydrofurfuryl alcohol, and ethylene glycol.

[0051] The above solvents may be used alone or in combination of two or more.

[0052] In the low-temperature sinterable bonding paste, the content of the solvent is preferably 1 to 50 parts by mass, more preferably 2 to 40 parts by mass, and even more preferably 3 to 35 parts by mass, per 100 parts by mass of the total amount of silver particles and silicon particles.

[0053] The low-temperature sinterable bonding ink composition may contain organic additives such as adhesives, thickeners, and binders.

[0054] The low-temperature sinterable joining sheet may be a sheet having a network structure formed of metal components including silver and silicon, and capable of maintaining a sheet state with only the metal components and silicon components, or a sheet in which metal particles are dispersed in a resin and the sheet state is maintained by the resin components.

[0055] The low-temperature sinterable joining sheet has a sinterable region on at least one surface. The low-temperature sinterable joining sheet may have voids near the surface. In this case, the porosity near the surface of the low-temperature sinterable joining sheet (particularly the porosity near the surface in the sinterable region) is preferably 20% or less, more preferably 10% or less, and even more preferably 5% or less. When the porosity is 20% or less, better joining properties can be exhibited.

[0056] The porosity near the surface can be determined by exposing a cross section of the low-temperature sinterable bonding sheet, observing the cross section of the low-temperature sinterable bonding sheet near the end in the thickness direction (for example, from the surface of the low-temperature sinterable bonding sheet to within 5% of the thickness of the low-temperature sinterable bonding sheet (for example, within 2 μm)) using a scanning electron microscope, and analyzing the obtained cross-sectional image to calculate the occupancy of metal and silicon, and then calculating it using the following formula. Note that when the boundary between the surface vicinity and the interior of the low-temperature sinterable bonding sheet can be recognized by the difference in porosity, the porosity near the surface can be measured in a region that can be distinguished from the interior, regardless of the distance from the surface. Porosity [%] = 100 - occupancy [%]

[0057] The low-temperature sinterable joining sheet may have voids inside. In this case, the void ratio inside the low-temperature sinterable joining sheet is preferably 50% or less, more preferably 30% or less, even more preferably 20% or less, and particularly preferably 10% or less. When the void ratio is 50% or less, the mechanical strength is such that chipping or cracking is less likely to occur during handling.

[0058] The internal porosity can be calculated by exposing a cross section of the low-temperature sinterable bonding sheet, observing the cross section of the low-temperature sinterable bonding sheet near the center in the thickness direction using a scanning electron microscope, and analyzing the obtained cross-sectional image to calculate the occupancy rates of metal and silicon, and then using the following formula: Porosity [%] = 100 - Occupancy [%]

[0059] The low-temperature sinterable bonding sheet can be produced, for example, by heating and / or pressurizing a composition containing silver particles and silicon particles to melt the surfaces of metal particles, including silver particles, and silicon atoms, fusing the particles together to form a network. The porosity within the low-temperature sinterable bonding sheet can be adjusted by adjusting the particle size, heating temperature, pressing pressure, and heating and pressing time. The heating and pressing may be performed either singly or both. When both heating and pressing are performed, they may be performed simultaneously or sequentially. The heating temperature is, for example, 180 to 400°C. The pressing pressure is, for example, 0.3 to 40 MPa.

[0060] [Bonded Structure] The low-temperature sinterable bonding material can be used to form a conductive layer such as metal wiring on the workpieces to be joined or to bond the workpieces to each other. For example, the low-temperature sinterable bonding ink composition can be applied to the surfaces of the workpieces to be joined, and the solvent can be evaporated by heating or other means if necessary. Then, the metal particles, including silver particles, can be sintered (fired) by heating, pressure, or active energy ray irradiation, etc., to obtain a bonded structure having a conductive layer (bonding layer) on the workpieces to be joined. Alternatively, for example, the low-temperature sinterable bonding sheet can be placed on the workpieces to be joined so that the sinterable region of the low-temperature sinterable bonding sheet contacts the surfaces of the workpieces to be joined. The metal in the sinterable region can be sintered (fired) by heating, pressure, or active energy ray irradiation, etc., to bond the low-temperature sinterable bonding sheet to the workpieces to obtain a bonded structure (joined body) having a conductive layer (bonding layer) on the workpieces to be joined.

[0061] Furthermore, by laminating a first bonded member and a second bonded member with a low-temperature sinterable bonding material interposed therebetween and sintering (firing) metal particles including silver particles, a bonded structure can be obtained in which the first and second bonded members are bonded via a bonding layer. Furthermore, it is preferable that a metallized layer is formed on the surface of the bonded members bonded to the low-temperature sinterable bonding sheet. The metal constituting the metallized layer is preferably silver.

[0062] Examples of the bonded members include a substrate, a semiconductor chip, etc. For example, a substrate can be used as the first bonded member, and a semiconductor chip can be used as the second bonded member.

[0063] Fig. 1 shows one embodiment of a bonded structure according to the present disclosure. In the bonded structure 1 shown in Fig. 1, a workpiece 30 is bonded to a substrate 10 via a silver bonding layer 20 including a sintered body of the low-temperature sinterable bonding material.

[0064] The substrate (substrate) may be any known or commonly used material for providing the bonding layer. The substrate may be a conductive substrate, a non-conductive substrate, or a dielectric material. The substrate may be a single layer or a multilayer structure in which multiple layers are laminated.

[0065] Examples of materials for forming the non-conductive substrate include resins, glass, ceramics, wood, paper, etc. Examples of the resins include heat-resistant plastics such as polyimide resins, polycarbonate resins, isocyanate resins, melamine resins, and glass epoxy resins, as well as resins with low heat resistance such as polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin resins such as polyethylene and polypropylene, acrylic resins, epoxy resins, phenolic resins, and polyamide resins, as well as polychlorinated biphenyl (PCB), liquid crystal polymers (LCP), vinyl chloride, molded resins, and epoxy resins.

[0066] Examples of the conductive substrate include metal substrates such as metal foils and metal plates formed from metals (copper, iron, alloys thereof, etc.); carbon substrates such as carbon cloth, carbon paper, graphite, etc.; composite substrates such as conductive particle-containing films, metal mesh films, metal-plated films, and optical laminates having a transparent conductive layer; resin substrates such as conductive polymer films; metal wire-containing films; and metal film laminates (printed circuit boards, etc.) having a metal (silver, copper, etc.) film on a part or all of a non-conductive substrate.

[0067] Examples of the substrate include metal substrates such as copper substrates, ceramic substrates, SiC substrates, gallium nitride substrates, glass epoxy substrates, BT resin substrates, glass substrates, resin substrates, semiconductor elements such as IGBTs, diodes, Schottky barrier diodes, MOS-FETs, thyristors, logic circuits, sensors, analog integrated circuits, LEDs, semiconductor lasers, and oscillators; substrates for mounting semiconductor elements such as lead frames, metal plate-attached ceramic substrates (for example, DBC), piezoelectric ceramics, semiconductor packages, and LED packages; power supply members such as copper ribbons, metal blocks, and terminals; heat sinks; water-cooled plates; lenses for eyeglasses and sunglasses; glass (automotive glass such as windshields, side windows, and rear windows of automobiles); sensor covers; thermal transfer rollers; printed circuit boards; vias in printed circuit boards; displays of personal computers, televisions, and the like; convex mirrors; traffic lights; smartphones; wearable devices such as watches and earphones; writing implements; glass slides; and office automation equipment such as mice.

[0068] When the above-mentioned low-temperature sinterable bonding paste is used, it can be manufactured by applying it to a substrate by a printing method (specifically, a dispenser printing method, a mask printing method, a screen printing method, an inkjet printing method, or the like) to form a coating layer, mounting the member to be joined 30 on the coating layer, and then sintering it.

[0069] The sintering temperature of the coating layer is, for example, 150° C. or higher and lower than 300° C., preferably 160 to 280° C., more preferably 200 to 270° C., and even more preferably 230 to 260° C. The sintering time is, for example, 0.1 to 2 hours, and preferably 0.5 to 1.5 hours.

[0070] When using the low-temperature sinterable bonding sheet, the sintering temperature (sintering temperature) can be, for example, 500°C or less, preferably 300°C or less, more preferably 250°C or less, and even more preferably room temperature (e.g., 25°C) to 150°C. Sintering temperatures of 300°C or less (particularly 250°C or less) can suppress thermal deformation even when the substrate is a material that is prone to thermal deformation. In particular, when it is desired to complete sintering of the metal in a short period of time, sintering is preferably performed at, for example, 60 to 200°C, preferably 70 to 180°C, more preferably 80 to 150°C, and even more preferably 90 to 120°C. The sintering time can be determined appropriately taking into account the type of metal particles, the amount applied, the sintering temperature, etc., and is, for example, within several hours (e.g., within 40 seconds to 33 hours), preferably within 1 hour, more preferably within 50 minutes, even more preferably 10 to 40 minutes, and particularly preferably 15 to 30 minutes.

[0071] The thickness of the low-temperature sinterable bonding material is in the range such that the thickness of the bonded structure formed by the above method is, for example, 15 to 400 μm, preferably 20 to 250 μm, and more preferably 40 to 180 μm.

[0072] The sintering may be carried out in an air atmosphere, or in an inert gas atmosphere such as a nitrogen atmosphere or an argon atmosphere.

[0073] Examples of the second bonded member (bonded member 30) include electronic components and heat dissipation substrates. Examples of electronic components include electronic elements (chips, dies) such as power semiconductor elements and LED elements. The bonding surface of the bonded member 30 with the silver bonding layer 20 is preferably silver-plated. The material of the bonded member 30 may be any of Si (silicon), SiC (silicon carbide), etc., but particularly excellent effects are obtained when the bonded member 30 is SiC (silicon carbide).

[0074] Examples of the bonded structure include electric and electronic devices such as electromagnetic wave control materials, circuit boards, antennas, heat sinks, liquid crystal displays, organic EL displays, field emission displays (FEDs), IC cards, IC tags, solar cells, LED elements, organic transistors, capacitors, electronic paper, flexible batteries, flexible sensors, membrane switches, touch panels, and EMI shields.

[0075] The low-temperature sinterable bonding material disclosed herein forms a sintered bond made of an Ag—Si alloy by sintering, which allows for changes in the mechanical properties (strength and thermal expansion coefficient) of the bond. This essentially improves the properties of the bond, such as thermal fatigue resistance. Furthermore, the bond contains a large number of silicon particles, which are difficult to diffuse into silver, and these particles block the solid-phase diffusion of silver. Furthermore, the addition of silicon particles reduces stress at the bond, preventing the metal layer from becoming coarse-grained.

[0076] Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. Each configuration and combination thereof in each embodiment is an example, and addition, omission, substitution, and other modifications of configurations are possible as appropriate within the scope of the present disclosure. Furthermore, each invention according to this disclosure is not limited by the embodiments or the following examples, but is limited only by the scope of the claims.

[0077] Hereinafter, one embodiment of the present disclosure will be described in more detail based on examples. In the following, the average particle size (median size) of particles is a value measured by a laser diffraction / scattering method.

[0078] The raw materials used are as follows: [Silver flake powder (flake silver powder)] Product name "AgC-239": average diameter 5.0 μm, average thickness 260 nm, specific surface area 1.2 m 2 / g, manufactured by Fukuda Metal Foil & Powder Co., Ltd. [Silicon (Si) particles] Product name "Metallic Silicon Powder": Si purity > 98.9%, particle size D50 = 32.8 μm [Solvent] Product name "DPNP": dipropylene glycol n-propyl ether: boiling point 212°C, manufactured by Daicel Corporation

[0079] Comparative Example 1 53 parts by mass of silver flake powder (trade name "AgC-239") and 47 parts by mass of silicon (Si) particles (trade name "metal silicon powder") were mixed and pulverized using the high-speed three-dimensional motion (strong frictional force motion) of a three-dimensional ball mill (trade name "3D Ball Mill") manufactured by Nagao System Co., Ltd. to obtain silicon (Si) particles coated with silver. The proportion of the silver coating layer on the particle surface of these silver-coated silicon (Si) particles was calculated from an image taken at 3000x magnification using an SEM, and was found to be 72%. Hereinafter, these silver-coated silicon (Si) particles may be referred to as "Si-20% by volume Ag particles." 21 parts by mass of a solvent (trade name "DPNP") was added to 100 parts by mass of the above-mentioned "Si-20% by volume Ag particles" and mixed to obtain "Si-Ag paste-1." This paste had a viscosity suitable for use as a bonding paste. "Si-Ag Paste-1" was printed onto a silver-plated copper substrate (10 mm x 100 mm x 2 mm thick) using a metal mask to form a coating film approximately 100 μm thick. A Si die (3 mm x 3 mm x 0.45 mm thick) with a silver-coated backside was mounted on top of this paste coating. The resulting test sample (bonded structure) having a layered structure of Si die / Si-Ag paste / copper substrate was heated in an air atmosphere at 2.0 MPa (gauge pressure) and 250°C for 60 minutes using a reflow furnace to sinter the Si-Ag paste (die bonding). To examine the bond strength between the Si die and copper substrate in the sintered test sample, the shear strength (shear head speed: 50 μm / s) between the Si die and copper substrate was measured using a die shear tester (manufactured by DAGE, product name "XD-7500"). The resulting shear strength was 2.9 N.

[0080] Comparative Example 2 75 parts by mass of silver flake powder (trade name "AgC-239") and 25 parts by mass of silicon (Si) particles (trade name "metal silicon powder") were mixed and pulverized using the high-speed three-dimensional motion (strong frictional force motion) of a three-dimensional ball mill (trade name "3D Ball Mill") manufactured by Nagao System Co., Ltd. to obtain silicon (Si) particles coated with silver. The proportion of the silver coating layer on the particle surface of these silver-coated silicon (Si) particles was determined in the same manner as in Comparative Example 1, and was found to be 92%. Hereinafter, these silver-coated silicon (Si) particles may be referred to as "Si-40% by volume Ag particles." 25 parts by mass of a solvent (trade name "DPNP") was added to 100 parts by mass of the above-mentioned "Si-40% by volume Ag particles" and mixed to obtain "Si-Ag paste-2." This paste had a viscosity suitable for use as a bonding paste. Using the above "Si-Ag paste-2," a test sample (bonded structure) having a layer structure of Si die / Si-Ag paste / copper substrate was produced in the same manner as in Comparative Example 1. This test sample was heated in a reflow furnace under an air atmosphere at a pressure (gauge pressure) of 2.0 MPa and a temperature of 250°C for 60 minutes to sinter the Si-Ag paste (die bonding). To examine the bond strength between the Si die and copper substrate in the sintered test sample, the shear strength (shear head speed: 50 μm / s) between the Si die and copper substrate was measured in the same manner as in Comparative Example 1, and was found to be 13 N.

[0081] Comparative Example 3 87.2 parts by mass of silver flake powder (trade name "AgC-239") and 12.8 parts by mass of silicon (Si) particles (trade name "metal silicon powder") were mixed and pulverized using the high-speed three-dimensional motion (strong frictional force motion) of a three-dimensional ball mill (trade name "3D Ball Mill") manufactured by Nagao System Co., Ltd. to obtain silicon (Si) particles coated with silver. The proportion of the silver coating layer on the particle surface of these silver-coated silicon (Si) particles was determined in the same manner as in Comparative Example 1, and was found to be 98%. Hereinafter, these silver-coated silicon (Si) particles may be referred to as "Si-60% by volume Ag particles." 100 parts by mass of the above-mentioned "Si-60% by volume Ag particles" were mixed with 30 parts by mass of a solvent (trade name "DPNP") to obtain "Si-Ag paste-3." This paste had a viscosity suitable for use as a bonding paste. Using the above "Si-Ag Paste-3," a test sample (bonded structure) having a layer structure of Si die / Si-Ag paste / copper substrate was produced in the same manner as in Comparative Example 1. This test sample was heated in a reflow furnace under an air atmosphere at a pressure (gauge pressure) of 2.0 MPa and a temperature of 250°C for 60 minutes to sinter the Si-Ag paste (die bonding). To examine the bond strength between the Si die and copper substrate in the sintered test sample, the shear strength (shear head speed: 50 μm / s) between the Si die and copper substrate was measured in the same manner as in Comparative Example 1, and was found to be 23 N.

[0082] Comparative Example 4 (Ag:Si = 66:34 vol% = 90:10 vol%): 80 parts by mass of the "Si-60 vol% Ag particles" obtained in Comparative Example 3, 20 parts by mass of silver flake powder (product name "AgC-239"), and 20 parts by mass of a solvent (product name "DPNP") were mixed together to obtain "Si-Ag Paste-4." This paste had a viscosity suitable for use as a bonding paste. Using the above-mentioned "Si-Ag paste-4," a test sample (bonded structure) having a layer structure of Si die / Si-Ag paste / copper substrate was produced in the same manner as in Comparative Example 1. This test sample was heated in a reflow furnace in an air atmosphere at a pressure (gauge pressure) of 2.0 MPa and a temperature of 250°C for 60 minutes to sinter the Si-Ag paste (die bonding). In order to examine the bonding strength between the Si die and copper substrate in the sintered test sample, the shear strength (shear head speed: 50 μm / s) between the Si die and copper substrate was measured in the same manner as in Comparative Example 1, and was found to be 43 N.

[0083] Comparative Example 5 (Ag:Si = 73:27 vol% = 92:8 t% by mass) 60 parts by mass of the "Si-60 vol% Ag particles" obtained in Comparative Example 3, 40 parts by mass of silver flake powder (product name "AgC-239"), and 20 parts by mass of a solvent (product name "DPNP") were mixed together to obtain "Si-Ag Paste-5." This paste had a viscosity suitable for use as a bonding paste. Using the above-mentioned "Si-Ag paste-5," a test sample (bonded structure) having a layer structure of Si die / Si-Ag paste / copper substrate was produced in the same manner as in Comparative Example 1. This test sample was heated in a reflow furnace in an air atmosphere at a pressure (gauge pressure) of 2.0 MPa and a temperature of 250°C for 60 minutes to sinter the Si-Ag paste (die bonding). In order to examine the bonding strength between the Si die and copper substrate in the sintered test sample, the shear strength (shear head speed: 50 μm / s) between the Si die and copper substrate was measured in the same manner as in Comparative Example 1, and was found to be 84 N.

[0084] Comparative Example 6 (Ag:Si = 80:20 vol% = 95:5 vol%): 40 parts by mass of the "Si-60 vol% Ag particles" obtained in Comparative Example 3, 60 parts by mass of silver flake powder (product name "AgC-239"), and 20 parts by mass of a solvent (product name "DPNP") were mixed together to obtain "Si-Ag Paste-6." This paste had a viscosity suitable for use as a bonding paste. Using the above-mentioned "Si-Ag paste-6," a test sample (bonded structure) having a layer structure of Si die / Si-Ag paste / copper substrate was produced in the same manner as in Comparative Example 1. This test sample was heated in a reflow furnace in an air atmosphere at a pressure (gauge pressure) of 2.0 MPa and a temperature of 250°C for 60 minutes to sinter the Si-Ag paste (die bonding). In order to examine the bonding strength between the Si die and copper substrate in the sintered test sample, the shear strength (shear head speed: 50 μm / s) between the Si die and copper substrate was measured in the same manner as in Comparative Example 1, and was found to be 146 N.

[0085] Example 1: 94.6 parts by mass of silver flake powder (trade name "AgC-239") and 5.4 parts by mass of silicon (Si) particles (trade name "Metallic Silicon Powder") were mixed, and 25 parts by mass of a solvent (trade name "DPNP") was added to 100 parts by mass of the mixed powder to obtain "Si-Ag Paste-1A." This paste had a viscosity suitable for use as a bonding paste. Using the above "Si-Ag Paste-1A," a test sample (bonded structure) having a layer structure of Si die / Si-Ag paste / copper substrate was produced in the same manner as in Comparative Example 1. This test sample was heated in a reflow furnace under an air atmosphere at a pressure of 2.0 MPa (gauge pressure) and a temperature of 250°C for 60 minutes to sinter the Si-Ag paste (die bonding). To examine the bond strength between the Si die and copper substrate in the sintered test sample, the shear strength (shear head speed: 50 μm / s) between the Si die and copper substrate was measured in the same manner as in Comparative Example 1, and was found to be 250 N. Thus, Example 1 exhibited higher shear strength than Comparative Example 6, which had the same Ag and Si mixing ratio (volume ratio). The silicon particle content relative to the total silver flake powder and silicon particles in the paste was 20% by volume. Furthermore, a cross section of the sintered test sample was exposed and observed at 50,000x magnification using an FE-SEM. Representative interfaces were observed at 100,000x magnification using a TEM, confirming that Si and Ag formed an interface at the atomic level. Furthermore, 15% of the surface of the silicon particles formed an interface with the silver particles. A cross-sectional TEM image of the test sample obtained in Example 1 is shown in FIG. 2.

[0086] Example 2: 92 parts by weight of silver flake powder (trade name "AgC-239") and 8 parts by weight of silicon (Si) particles (trade name "Metallic Silicon Powder") were mixed, and 25 parts by weight of a solvent (trade name "DPNP") was added to 100 parts by weight of the mixed powder to obtain "Si-Ag Paste-2A." This paste had a viscosity suitable for use as a bonding paste. Using the above-mentioned "Si-Ag Paste-2A," a test sample (bonded structure) having a layer structure of Si die / Si-Ag paste / copper substrate was produced in the same manner as in Comparative Example 1. This test sample was heated in a reflow furnace in an air atmosphere at a pressure of 2.0 MPa (gauge pressure) and a temperature of 250°C for 60 minutes to sinter the Si-Ag paste (die bonding). To examine the bond strength between the Si die and copper substrate in the sintered test sample, the shear strength (shear head speed: 50 μm / s) between the Si die and copper substrate was measured in the same manner as in Comparative Example 1, and was found to be 180 N. Thus, Example 2 exhibited higher shear strength than Comparative Example 5, which had the same Ag and Si mixing ratio (volume ratio). The silicon particle content relative to the total silver flake powder and silicon particles in the paste was 27% by volume. Furthermore, a cross section of the sintered test sample was exposed and observed at a magnification of 50,000 times using an FE-SEM. A representative interface was observed at a magnification of 100,000 times using a TEM. It was confirmed that Si and Ag formed an interface at the atomic level. Furthermore, 20% of the surface of the silicon particles formed an interface with the silver particles.

[0087] Example 3: 90 parts by weight of silver flake powder (trade name "AgC-239") and 10 parts by weight of silicon (Si) particles (trade name "Metallic Silicon Powder") were mixed, and 25 parts by weight of a solvent (trade name "DPNP") was added to 100 parts by weight of the mixed powder to obtain "Si-Ag Paste-3A." This paste had a viscosity suitable for use as a bonding paste. Using the above "Si-Ag Paste-3A," a test sample having a layer structure of Si die / Si-Ag paste / copper substrate was produced in the same manner as in Comparative Example 1. This test sample was heated in a reflow furnace in an air atmosphere at a pressure of 2.0 MPa (gauge pressure) and a temperature of 250°C for 60 minutes to sinter the Si-Ag paste (die bonding). To examine the bond strength between the Si die and copper substrate in the sintered test sample, the shear strength (shear head speed: 50 μm / s) between the Si die and copper substrate was measured in the same manner as in Comparative Example 1, and was found to be 150 N. Thus, Example 3 exhibited higher shear strength than Comparative Example 4, which had the same Ag and Si mixing ratio (volume ratio). The silicon particle content relative to the total silver flake powder and silicon particles in the paste was 34% by volume. Furthermore, the cross section of the sintered test sample was exposed and observed at a magnification of 50,000 times using an FE-SEM, and a representative interface was observed at a magnification of 100,000 times using a TEM. It was confirmed that Si and Ag formed an interface at the atomic level. Furthermore, 12% of the surface of the silicon particles formed an interface with the silver particles.

[0088] Variations of the invention according to the present disclosure are described below. [Appendix 1] A low-temperature sinterable bonding material comprising silver particles and silicon particles, wherein more than 50% of the surfaces of the silicon particles are composed of silicon atoms. [Appendix 2] The low-temperature sinterable bonding material according to Appendices 1, wherein 60% or more of the silicon particles are composed of silicon atoms. [Appendix 3] The low-temperature sinterable bonding material according to Appendices 1 or 2, wherein the silicon particles have an average particle size of 0.05 to 40 μm. [Appendix 4] The low-temperature sinterable bonding material according to any one of Appendices 1 to 3, wherein the silver constituting the silver particles and the silicon constituting the silicon particles form an interface at the atomic level upon sintering. [Appendix 5] The low-temperature sinterable bonding material according to any one of Appendices 1 to 4, wherein the silver particles have an average particle size of 0.5 to 40 μm. [Appendix 6] The low-temperature sinterable bonding material according to any one of Appendices 1 to 5, wherein the silver particles are in the form of flakes. [Appendix 7] A low-temperature sinterable bonding material comprising silver particles and silicon particles, wherein, upon sintering, the silver constituting the silver particles and the silicon constituting the silicon particles form an interface at the atomic level. [Appendix 8] The low-temperature sinterable bonding material according to Appendix 7, wherein, upon sintering, 20% or more of the surface of the silicon particles form the interface with the silver particles. [Appendix 9] The low-temperature sinterable bonding material according to Appendix 7 or 8, wherein, upon sintering, 40% or more of the surface of the silicon particles form the interface with the silver particles. [Appendix 10] A low-temperature sinterable bonding material comprising silver particles and silicon particles, wherein the average particle size of the silicon particles is 1 / 20 or more of the average particle size of the silver particles, and the content of the silicon particles relative to the total of the silver particles and the silicon particles is 10 to 70% by volume. [Appendix 11] The low-temperature sinterable bonding material according to Appendix 10, wherein the average particle size of the silicon particles is 0.05 to 40 μm. [Appendix 12] The low-temperature sinterable bonding material according to Appendices 10 or 11, wherein the average particle size of the silver particles is 0.1 to 50 μm. [Appendix 13] The low-temperature sinterable bonding material according to any one of Appendices 1 to 12, which is a paste or a sheet. [Appendix 14] A bonded structure in which objects to be bonded are bonded to a substrate via a silver bonding layer comprising a sintered body of the low-temperature sinterable bonding material according to any one of Appendices 1 to 12.

[0089] 1 Bonded structure 10 Base material 20 Silver bonding layer 30 Joined member

Claims

1. A low-temperature sinterable joining material comprising silver particles and silicon particles, wherein more than 50% of the surface of the silicon particles is composed of silicon atoms.

2. The low-temperature sinterable bonding material according to claim 1, wherein 60% or more of said silicon particles are composed of silicon atoms.

3. A low-temperature sintering bonding material according to claim 1, wherein the average particle size of the silicon particles is 0.05 to 40 μm.

4. A low-temperature sinterable bonding material according to claim 1, in which the silver constituting said silver particles and the silicon constituting said silicon particles form an interface at the atomic level by sintering.

5. The low-temperature sintering bonding material according to claim 1, wherein the average particle size of the silver particles is 0.5 to 40 μm.

6. The low-temperature sinterable bonding material according to claim 1, wherein the silver particles are in the form of flakes.

7. A low-temperature sinterable bonding material comprising silver particles and silicon particles, in which, upon sintering, the silver constituting the silver particles and the silicon constituting the silicon particles form an interface at the atomic level.

8. The low-temperature sinterable bonding material according to claim 7, wherein, by the sintering, 10% or more of the surface of the silicon particles forms the interface with the silver particles.

9. The low-temperature sinterable bonding material according to claim 7, wherein, by said sintering, 40% or more of the surface of said silicon particles forms said interface with said silver particles.

10. A low-temperature sinterable bonding material comprising silver particles and silicon particles, the average particle size of the silicon particles being 1 / 20 or more of the average particle size of the silver particles, and the content of the silicon particles relative to the total content of the silver particles and the silicon particles being 10 to 70 volume %.

11. The low-temperature sinterable bonding material according to claim 10, wherein the average particle size of the silicon particles is 0.05 to 40 μm.

12. The low-temperature sintering bonding material according to claim 10, wherein the average particle size of the silver particles is 0.1 to 50 μm.

13. The low-temperature sinterable joining material according to any one of claims 1 to 12, which is in the form of a paste or a sheet.

14. A bonded structure in which an object to be bonded is bonded to a substrate via a silver bonding layer comprising a sintered body of the low-temperature sinterable bonding material according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Joining material and joining method using the same

    JP2011080147A

  • Communication device, communication method, and program

    JP2023068160A

  • Metal paste and manufacture thereof

    JP1991034211A

  • Sintered material, sintered joint, and method for manufacturing a sintered joint

    JP2012515266A

  • Silver paste and semiconductor device using same

    WO2015060173A1