Iron-based powder for supplying iron ions
By controlling the half-width of the diffraction intensity curve and particle size of the iron-based powder, the challenges of iron ion elution and plant growth are addressed, resulting in enhanced plant growth and crop yields through efficient and continuous iron ion supply.
Patent Information
- Application Number
- PCT/JP2024/015657
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-24
AI Technical Summary
Existing iron-based powders for supplying divalent iron ions to plants face challenges such as rapid oxidation and leaching in moist environments, leading to reduced elution of divalent iron ions and delayed plant growth benefits, due to the passive role of iron oxyhydroxide and oxide, and the slow action of iron-reducing bacteria.
An iron-based powder with a controlled half-width of the diffraction intensity curve corresponding to the (110) diffraction plane of the α-Fe crystal, within the range of 0.03° to 3.00°, is developed to enhance chemical activation and oxygen reactivity, allowing for efficient elution of divalent iron ions, with a median particle size of 50 μm or more and a maximum particle size of 80 μm or less, ensuring stable and continuous iron ion supply.
The solution enables a high iron ion supply ability, promoting plant growth and increasing crop yields by ensuring efficient and continuous elution of divalent iron ions, thereby improving plant growth conditions and crop yields.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Iron-based powder for supplying iron ions
[0001] The present invention relates to an iron-based powder for supplying iron ions, which supplies iron ions that contribute to plant growth.
[0002] Iron is an essential nutrient for plant growth, and plays a role in chlorophyll synthesis, energy production in mitochondria, and conversion of nitrogen fertilizer to amino acids.
[0003] Plants absorb this iron as divalent iron ions, but a lack of iron in the soil can cause poor growth of new shoots, as seen in the yellowing of rice plants, resulting in reduced rice yields. Taking paddy fields as an example, when fertilizers containing sulfate ions are used in cases where the soil is iron deficient as described above, hydrogen sulfide is generated from the soil, causing poor root growth in rice plants, leading to lodging due to reduced root penetration into the soil, and reduced rice yields due to reduced absorption of nutrients from the soil. In any case, improving plant growth requires a stable and sustained supply of divalent iron ions, and iron ion supply materials have traditionally been attracting attention as a means to achieve this.
[0004] As such an iron ion supplying material, for example, Patent Document 1 discloses an iron powder that contains 80 mass % or more of iron and 0.4 mass % to 1.5 mass % of oxygen as a material for stably supplying divalent iron ions to plants, with 50 mass % or more of the total having a particle size of 100 μm to 10 mm.
[0005] Furthermore, Patent Document 2 discloses a plant growth promoter that comprises ferrous oxide and a chelating substance to allow plants to efficiently absorb iron.
[0006] JP 2015-119685 A JP 2004-123677 A
[0007] In paddy fields and fields, where moisture is present, divalent iron ions are eluted from the spread iron powder, and at the same time, the surface of the iron powder is oxidized by oxygen dissolved in the water and oxygen in the air, producing mainly iron oxyhydroxide and iron oxide.
[0008] Because such iron oxyhydroxides and iron oxides act as passive particles, the amount of divalent iron ions leaching from the iron powder decreases once the iron powder has oxidized to a certain extent. Iron-reducing bacteria of the genus Geobacter and Anaeromyxobacter exist in soil (Monthly Modern Agriculture, October 2020 issue). Therefore, the trivalent iron in the iron oxyhydroxides and iron oxides is reduced to divalent iron by these iron-reducing bacteria, which then leaches out as divalent iron ions, but this leaching takes time.
[0009] That is, as described in Patent Document 1, when iron powder containing a large amount of metallic iron with a low oxygen concentration is spread, the surface of the iron powder is oxidized after spreading, and then iron-reducing bacteria reduce the oxidized portion. Although this contributes significantly to plant growth, it takes a relatively long time for the effect to be realized.
[0010] Furthermore, as described in Patent Document 2, when ferrous oxide is sprayed, the surface of the ferrous oxide (FeO) is first oxidized to iron oxyhydroxide or iron oxide and then reduced by iron-reducing bacteria, so the amount of eluted divalent iron ions is reduced, and even if elution occurs, it takes a long time to obtain the required amount.
[0011] The present invention aims to solve the above problems and provide an iron-based powder for supplying iron ions, which improves the growth conditions of plants (crops) by dissolving divalent iron ions, and thereby increases the yield of the crops.
[0012] When a solid substance is subjected to mechanical energy such as crushing, impact, or friction, its crystalline properties change. When distortion occurs in the crystalline structure of the solid, it becomes chemically activated and more susceptible to chemical reactions.
[0013] Therefore, in order to solve the above-mentioned problems, the inventors have focused on the chemical activity of iron-based powders and conducted studies with the aim of promoting the elution of divalent iron ions from the iron-based powders. As a result, they have found that divalent iron ions can be effectively eluted by controlling the half-width of the diffraction intensity curve corresponding to the (110) diffraction plane of the α-Fe crystal. In addition, they have also found that the particle size of chemically activated iron-based powders is not necessarily affected by the particle size, and therefore it is not necessary to specify the particle size of the iron-based powders.
[0014] The present invention is based on the above findings and is summarized as follows: 1. An iron-based powder for supplying iron ions, which supplies iron ions that contribute to plant growth, wherein, among the diffraction peaks of X-ray diffraction using Cu-Kα rays of the iron-based powder constituting the iron-ion supplying iron powder, the half-width of a diffraction intensity curve corresponding to the (110) diffraction plane of an α-Fe crystal is in the range of 0.03° to 3.00°.
[0015] 2. Median diameter D 50 is 50 μm or more, 10 × 10 3 μm or less and maximum particle size is 80 μm or more 30 × 10 3 2. The iron-based powder for supplying iron ions according to 1 above, having a particle size of 1 μm or less.
[0016] According to the present invention, by limiting the range of the half-width of the diffraction intensity curve corresponding to the (110) diffraction plane of the α-Fe crystal of the iron-based powder, it is possible to provide an iron-ion supplying iron-based powder that has a high iron ion supplying ability that contributes to the growth of plants (crops).
[0017] Hereinafter, an embodiment of the present invention will be described. [Among the diffraction peaks of X-ray diffraction using Cu-Kα radiation of the iron-based powder constituting the iron-ion supplying iron-based powder, the half-width of the diffraction intensity curve corresponding to the (110) diffraction plane of the α-Fe crystal is in the range of 0.03° to 3.00°] The reason why the iron-based powder for supplying iron ions of the present invention has a high iron ion supplying ability is presumed to be as follows. When mechanical energy is applied to the iron-based powder by pulverization using a pulverizer or mixing using a mixer, distortion occurs in the crystal structure of the iron-based powder particles, improving oxygen reactivity. Here, the distortion of the crystal structure occurring within the iron-based powder particles can be evaluated from the value of the half-width of the X-ray diffraction intensity curve corresponding to the (110) plane of the α-Fe crystal derived from iron. When the non-uniform distortion occurring between the crystal lattice in which the atoms constituting the α-Fe crystal are three-dimensionally arranged and the adjacent crystal lattice increases, the half-width increases. As the distortion increases, the effect of improving oxygen reactivity becomes greater. However, if the distortion is excessive, the iron ion elution effect due to oxygen reaction caused by the moisture in the cultivated land becomes significantly greater, and although a large amount of iron ions is eluted within a short period of time after application, the elution period becomes shorter. Because a continuous supply of iron ions is necessary for plant growth, it is more important to continuously supply a stable amount of iron ions throughout the entire growth period, from the early to late stages, rather than supplying a large amount of iron ions in the early stages. Therefore, the half-width is set to a range of 0.03° to 3.00°. Preferably, it is set to a range of 0.05° to 3.00°, more preferably 0.07° to 3.00°.
[0018] In the present invention, the half-value width is measured as follows. First, X-ray diffraction measurement is performed on the iron-based powder for supplying iron ions using Cu-Kα radiation to obtain a diffraction intensity curve corresponding to the (110) diffraction plane of the α-Fe crystal. Next, the width of the diffraction intensity curve is determined at an intensity that is half the maximum intensity of the diffraction intensity. This width is defined as the half-value width in the present invention.
[0019] By growing plants using an iron-based powder that satisfies the above-mentioned characteristics, effective iron ion elution can be achieved, leading to improved growth. The iron-based powder can be produced by any of the following methods: atomization (e.g., water atomization, gas atomization, etc.), pulverization, and oxide reduction. The atomization method involves spraying water or gas onto a molten metal, pulverizing it, and then cooling and solidifying it. Either water atomization or gas atomization can be used. The oxide reduction method is a method of reducing iron oxide (mill scale) or iron ore powder that is generated on the surface of a steel sheet during hot rolling of the steel. The pulverization method is a method of pulverizing small metal pieces using a pulverizer.
[0020] The term "iron-based powder" refers to a metal powder containing 50% by mass or more of Fe. The iron-based powder in the present invention preferably contains 50% by mass or more of metallic iron. The iron-based powder is preferably an iron powder. Here, the iron powder refers to a powder consisting of Fe and inevitable impurities. The inevitable impurities may include C, S, O, N, Si, Mn, P, S, Cr, Cu, etc.
[0021] The method for measuring the metallic iron content of the iron-based powder is in accordance with JIS A 5011-2 "Method for determining metallic iron."
[0022] The crystallinity of the iron-based powder is preferably 90% by volume or more. The crystallinity is calculated by the following method. First, the X-ray diffraction spectrum of the iron-based powder is measured by powder X-ray diffraction using characteristic X-rays of Cu-Kα. In the obtained X-ray diffraction spectrum, the crystallinity (Vcry) of the iron-based powder is calculated by the following formula (1) based on the area of a broad diffraction pattern derived from the amorphous phase (Amo.P) and the sum of the areas of multiple peaks derived from the crystalline phase (Cry.P). Vcry (volume %) = Cry.P / (Amo.P + Cry.P) × 100 (1)
[0023] In the present invention, the median diameter D of the iron-based powder 50 The maximum particle size is not particularly limited as long as it does not cause any problems in handling, but the median diameter D 50 It is preferable that the median diameter D 50 is 10 x 10 3It is preferable that the maximum particle size is 80 μm or more. It is also preferable that the maximum particle size is 30×10 3 It is preferable that the thickness is 1 μm or less.
[0024] The particle size specification in Patent Document 1 only limits the particle size to 50% or more by mass of the total iron powder, and is not an index of the particle size of the entire iron powder. In other words, Patent Document 1 allows for the mixing of extremely fine iron powder. However, if there is a large amount of extremely fine iron powder, it may be blown away by the wind during application and cultivation, reducing the amount actually applied to the soil, or the amount of iron powder in the soil available for plant roots may be reduced, resulting in insufficient effectiveness.
[0025] Furthermore, Patent Document 1 allows for extremely coarse iron powder to be mixed in. If there is a large amount of extremely coarse iron powder, the specific surface area, which is the area per unit mass of the iron powder, becomes small.
[0026] In other words, the leaching of divalent iron ions from iron powder in soil and the oxidation of iron powder begin from the surface of the iron powder. Therefore, the larger the specific surface area of the iron powder, the greater the amount of divalent iron ions leached, and the greater the iron ion leaching effect. On the other hand, if the specific surface area is small, there is a risk that sufficient iron ion leaching effect will not be achieved.
[0027] From the above considerations, it is preferable that the iron-based powder for supplying iron ions of the present invention has the following particle size: That is, the median diameter (median value of particle size) D of the iron-based powder for supplying iron ions 50 50 μm or more 10 × 10 3 It is preferable that the maximum particle size is in the range of 80 μm or less, and that the maximum particle size is 80 μm or more. 3 The iron-based powder for supplying iron ions is preferably too fine (D 50 This is because if the particle size is less than 50 μm or the maximum particle size is less than 80 μm, the iron-based powder may be blown away by the wind during application or cultivation, which may lead to a decrease in the amount actually applied to the soil or a decrease in the amount of iron-based powder in the soil that can be used by plant roots.
[0028] On the other hand, D 50 is 10 x 103 μm or the maximum particle size is 30 × 10 3 If the particle size is larger than 1 μm, the particles will be too coarse overall, resulting in a small specific surface area. Since the elution of divalent iron ions from the iron-based powder in soil and the oxidation of the iron-based powder both proceed from the surface of the iron-based powder, if the specific surface area is too small, the amount of eluted divalent iron ions may decrease. Therefore, it is preferable to satisfy the above-mentioned particle size specification.
[0029] In the present invention, the powder D 50 The method for measuring the maximum particle size conforms to JIS Z 8815 "General rules for sieving test methods."
[0030] Median diameter D of iron-based powder for supplying iron ions 50 In order to adjust the median diameter D of the iron-based powder for supplying iron ions to 50 μm or more, specifically, classification with a sieve may be performed. 50 10 x 10 3 To adjust the particle size to 1 μm or less, specifically, the crushing conditions for the iron-based powder as the raw material may be adjusted.
[0031] In order to adjust the maximum particle size of the iron-based powder for supplying iron ions to 80 μm or more, classification with a sieve may be performed. 3 To adjust the particle size to 1 μm or less, specifically, the crushing conditions for the iron-based powder as the raw material may be adjusted.
[0032] [Production of Iron-Based Powder] The iron-based powder according to the present invention can be produced by subjecting iron-based powder produced by, for example, an atomization method, an oxide reduction method, or a pulverization method to a treatment for increasing the distortion of the α-Fe crystal. First, the iron-based powder used in the present invention is preferably produced by a water atomization method, a gas atomization method, an oxide reduction method, or a pulverization method. Furthermore, the produced powder may be classified or mixed by various methods to prepare the iron-based powder according to the present invention.
[0033] Next, in the present invention, the iron-based powder obtained by the above-mentioned method must be subjected to a treatment to increase the distortion of the α-Fe crystals in the iron-based powder for supplying iron ions. This treatment is preferably a treatment in which mechanical energy is applied using a mixer or a pulverizer. Mixers such as a V-type mixer, double cone mixer, conical blender, and agitator granulator, or pulverizers such as a ball mill, vibration mill, roller mill, jet mill, hammer mill, and disk mill can all be suitably used.
[0034] When the above mixer or pulverizer is used, appropriate mixing or pulverization conditions can be set to impart strain to the α-Fe crystals and adjust the half-value width to fall within the range of the present invention.
[0035] The iron-based powders used in this example were prepared by the following procedure. In order to evaluate the ability of iron-ion supplying iron-based powders to supply iron ions to plants, iron-based powders having the particle sizes and the like shown in Table 1 were prepared. First, mill scale generated during hot rolling of steel was reduced to prepare iron powder. Next, a high-speed mixer (manufactured by Earth Technica Co., Ltd.) was used as an agitation granulator to agitate 1 kg of each iron powder, thereby obtaining iron-based powders for supplying iron ions having the particle sizes and the like shown in Table 1. All of the iron-based powders for supplying iron ions were iron powders. The agitation was performed by using an agitator blade in a sample-charging container at a constant rotation speed of 500 rpm, while varying the agitation time.
[0036] The iron-based powder in this example was evaluated for its properties as follows: The iron-based powder according to the example was measured in accordance with JIS Z 8815 "General rules for sieving test methods," and the maximum particle size and the median diameter D, which is a representative value of the particle size, were determined from the particle size distribution based on mass. 50 He asked for this.
[0037] Furthermore, the half-width of the X-ray diffraction intensity curve of the (110) plane of the α-Fe crystal of the powder was measured as follows. That is, using an X-ray diffractometer (SmartLab manufactured by Rigaku Corporation), the iron-based powder to be measured was measured using Cu-Kα characteristic X-rays (wavelength 1.54178 Å) at a scanning speed of 4° / min and a measurement angle of 35° to 55°, thereby obtaining a diffraction intensity curve of the (110) plane of the α-Fe crystal in the iron-based powder. The half-width was then calculated from this diffraction intensity curve. More specifically, the measurement was performed in accordance with JIS K 0131 "General Rules for X-ray Diffraction Analysis." Furthermore, using the above-mentioned method, it was confirmed that the iron-based powder according to the example had a metallic iron content of 50% or more and a crystallinity of 90% or more by volume.
[0038] To evaluate the ability to supply iron ions to plants, rice was cultivated in paddy fields as follows. The iron-based powders according to Comparative Examples 1 to 8 and Invention Examples 1 to 12 were each applied to 100 m 2 Rice was grown by spraying 10 kg of iron-based powder per unit area, and the iron ion supply capacity to rice was evaluated based on the mass of harvested rice. Conventional Example 1 was used when rice was grown without spraying iron-based powder, and the mass of harvested rice per unit area was set to 100. The mass of harvested rice when each iron-based powder was used was shown as a mass ratio to Conventional Example 1. A larger value indicates a larger mass of harvested rice and a higher supply capacity of divalent iron ions. In other words, the iron ion supply capacity in this example was evaluated based on the mass of harvested rice per unit area. Table 1 shows the mass ratio of harvested rice per unit area as results for the conventional example, comparative example, and inventive example.
[0039]
[0040] As shown in Table 1, when the iron-based powders of Examples 1 to 12 in which the half-width of the diffraction intensity curve of the (110) plane of α-Fe is 0.03° or more and 3.00° or less are sprayed, the mass ratio of the harvested rice grains is larger than when the iron-based powders of Conventional Example 1 and Comparative Examples 1 to 8 are sprayed.
[0041] In addition, the half width of the diffraction intensity curve of the (110) plane of α-Fe is 0.03° or more and 3.00° or less, and D 50 is 50 μm or more, 10 × 10 3μm or less, and the maximum particle size is 80 μm or more 30 × 10 3 When the iron-based powders of Examples 3 and 6 to 12, each having a particle size of 1 μm or less, were sprayed, the mass ratio of the harvested rice grains was even greater than that of Examples 1, 2, 4, and 5.
[0042] The half width of the diffraction intensity curve of the (110) plane of α-Fe is 0.05° or more and 3.00° or less, and D 50 is 50 μm or more, 10 × 10 3 μm or less, and the maximum particle size is 80 μm or more 30 × 10 3 When the iron-based powders of Examples 7 to 12, each having a particle size of 1 μm or less, were sprayed, the mass ratio of the harvested rice was even greater than that of Examples 3 and 6.
[0043] The half-width of the diffraction intensity curve of the (110) plane of α-Fe is 0.07° or more and 3.00° or less, and D 50 is 50 μm or more, 10 × 10 3 μm or less, and the maximum particle size is 80 μm or more 30 × 10 3 When the iron-based powders of Examples 9 to 12, each having a particle size of 1 μm or less, were sprayed, the mass ratio of the harvested rice was even greater than that of Examples 7 and 8.
[0044] From the above results, it was found that the performance of the iron-based powder for supplying iron ions is influenced by the half-width of the diffraction intensity curve corresponding to the (110) diffraction plane of the α-Fe crystal of the powder. The use of the iron-based powder for supplying iron ions of the present invention makes it possible to efficiently supply divalent iron ions to plants, which is effective in increasing plant growth and yield.
Claims
1. An iron-based powder for supplying iron ions, which supplies iron ions that contribute to plant growth, wherein the half-width of a diffraction intensity curve corresponding to the (110) diffraction plane of an α-Fe crystal, among the diffraction peaks of X-ray diffraction using Cu-Kα rays, of the iron-based powder constituting said iron-based powder for supplying iron ions, is in the range of 0.03° to 3.00°.
2. Median diameter D 50 is 50 μm or more 10 × 10 3 μm or less and maximum particle size is 80 μm or more 30 × 10 3 2. The iron-based powder for supplying iron ions according to claim 1, wherein the particle size of the powder is 0.1 μm or less.
Citation Information
Patent Citations
Iron-based powder for oxygen reactants and oxygen reactants using the same
JP7485248B1
Iron(i) oxide-containing composition and plant growth promoter comprising the same
WO2007013217A1
Iron-ion supply material
WO2015097975A1
Iron-based powder for iron ion supply use and plant growth improving material comprising same
WO2022260019A1