Stainless steel clad plate for bridge structure, and preparation method for stainless steel clad plate

By adopting billet assembly and rolling technology in the preparation of stainless steel composite plates, the problems of poor plate shape and poor interface bonding quality are solved, the production efficiency and yield rate are improved, and high-quality stainless steel composite plates are achieved.

WO2024221603A1PCT designated stage expired Publication Date: 2024-10-31INST OF RES OF IRON & STEEL JIANGSU PROVINCE +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/105901
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2023-07-05
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The existing stainless steel composite plate preparation technology has problems such as poor plate shape, poor surface quality, poor interface bonding quality, difficult and weak welding, and the production process is highly polluted, difficult, low-efficiency, and has a low yield rate.

Method used

It adopts the process of billet preparation, coating with isolating agent, billet assembly, sealing and welding, vacuuming, sealing, heating, rolling, cooling, plate splitting and flattening to wrap the stainless steel composite layer through billet assembly, combined with rolling technology Ensure interface bonding quality and temperature uniformity, avoid air leakage and cracking, and improve production efficiency.

Benefits of technology

It achieves high-quality preparation of stainless steel composite plates, ensures plate shape, interface bonding quality and surface quality, solves defects in the existing technology, improves production efficiency and yield, and avoids dissimilar welding problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023105901_31102024_PF_FP_ABST
    Figure CN2023105901_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a stainless steel clad plate for a bridge structure, and a preparation method for the stainless steel clad plate. In the method, billet assembling is performed by means of using a carbon steel substrate A on an upper layer, a carbon steel substrate B on a lower layer, and at least two stainless steel composite materials on an intermediate layer, and four seals surrounding four side edges of the intermediate layer, wherein the seals are provided with circular through holes, steel tubes are welded in the through holes, and holes are reserved around the steel tubes during surfacing; after vacuumizing, the steel tubes are bent into the reserved holes; full welding is then carried out to seal-weld the steel tubes in the holes; during whole rolling, transverse rolling is used for the first N passes, and longitudinal rolling is subsequently used; and after the nth pass and the (n+2)th pass, a billet is subjected to one instance of back-and-forth water cooling in six sets of headers.
Need to check novelty before this filing date? Find Prior Art

Description

Stainless steel composite plate for bridge structure and preparation method thereof Technical Field

[0001] The invention relates to a stainless steel composite plate for a bridge structure and a preparation method of the stainless steel composite plate for a bridge structure, belonging to the technical field of steel material preparation. Background Art

[0002] With the continuous advancement of science and industry, ordinary alloy plates have become less able to meet the comprehensive performance requirements of industrial development, leading to the emergence of composite plates. Stainless steel composite plates are composite materials composed of a carbon steel or low-alloy steel base layer and a stainless steel cladding layer, with the base and cladding layers metallurgically bonded together. Stainless steel composite plates offer the corrosion resistance of the stainless steel cladding layer, combined with the outstanding mechanical properties and price advantages of the carbon steel or low-alloy steel base layer, making them a key development direction for steel materials.

[0003] In recent years, with the increasing demands for safety and longevity of steel bridges, the rust and corrosion protection of steel bridge structures has become increasingly prominent. Applying a corrosion-resistant protective material to the surface of bridge steel, replacing a single bridge steel plate, can achieve long-term corrosion protection that cannot be achieved with spray coating. Therefore, stainless steel composite plates have become an ideal choice. However, due to technical limitations, existing stainless steel composite plates suffer from defects such as poor plate shape, poor surface quality, poor interface bonding quality, and difficult and unstable welding during application. The preparation process also poses significant pollution, difficulty, low production efficiency, and low yield rates.

[0004] Specifically, the current preparation technologies of stainless steel composite plates are divided into two types: explosive composite and rolling composite.

[0005] Among them, regarding the preparation technology of explosive composite, for example, the Chinese patent application with publication number CN110064835A uses explosive composite to achieve the combination between the substrate and the composite material. On the one hand, the explosion will cause vibration, noise and smoke pollution to the environment. On the other hand, the composite board produced by the explosive composite method has relatively poor plate shape and surface quality.

[0006] Regarding the preparation technology of rolled composites, some have problems such as high processing difficulty, low production efficiency, and low yield rate, such as the grooving blanking technology used in the Chinese patent application with publication number CN107009090A; some have problems such as poor interface bonding and poor surface quality, such as the Chinese patent application with publication number CN109694986A, in which the stainless steel composite layer is exposed, and the surface quality of the side surface of the stainless steel composite layer is difficult to guarantee. In addition, the aluminum strips are easily detached during the handling of the composite blank, resulting in air leakage, which in turn affects the interface bonding quality. Furthermore, no existing technology discloses the impact of the rolling process on the interface bonding quality, especially the solution of ensuring the inherent performance of the substrate layer and the composite layer while taking into account the interface bonding quality.

[0007] Summary of the Invention

[0008] The object of the present invention is to provide a stainless steel composite plate for a bridge structure and a method for preparing the same, so as to solve at least one of the technical problems mentioned in the background technology.

[0009] To achieve the above-mentioned object, an embodiment of the present invention provides a method for preparing a stainless steel composite plate for a bridge structure, the method comprising a process flow of blank preparation, coating with a release agent, blank assembly, sealing, vacuuming, sealing, heating, rolling, cooling, separating the plates, and flattening; wherein,

[0010] During the assembly process, the blank is assembled in a manner such that an upper carbon steel substrate A, a lower carbon steel substrate B, an intermediate layer of at least two stainless steel composite materials, and four sealing strips surround the four sides of the intermediate layer. Gas shielded welding is performed between the seals and substrate A, and between the seals and substrate B, to form a blank. The four sides of the blank have grooves of depth D enclosed by substrate A, the seals, and substrate B. In addition, the seal on one side of the blank has a circular through hole, into which a steel pipe with an outer diameter of r is welded.

[0011] In the sealing welding process: the groove is surfacing welded, and a hole with a radius R>r and concentric with the steel pipe is reserved around the steel pipe during surfacing welding; when the groove on the side where the steel pipe is located is surfacing welded to a penetration depth of 2 / 3 of the groove depth, and the grooves on other sides are surfacing welded to a penetration depth of more than 2 / 3 of the groove depth, surfacing welding is stopped;

[0012] In the sealing process: after the base blank is vacuumed, the steel pipe is heated with a flame gun, flattened, and folded into the reserved hole; the hole is then fully welded with gas shielded welding to seal the steel pipe in the hole; then, surfacing welding is continued until the groove is filled, and finally, cap welding is performed to obtain a composite blank;

[0013] In the rolling process: the composite billet coming out of the heating furnace is rolled to obtain a large composite plate; in the entire rolling process, the first n passes are transverse rolling, and the longitudinal rolling is adopted after the n+1 pass, and the rolling reduction of the first pass is ≥25mm and the rolling temperature is ≥1060℃. The width of the billet obtained by rolling the nth pass is Wt+0~40mm, Wt is the target width of the large composite plate, and the rolling temperature of the nth pass is ≥1030℃; between the nth pass and the n+1 pass and between the n+2 pass and the n+3 pass, the billet is water-cooled once in 6 groups of headers, and the cooling water volume of the upper header of each group of headers is 120~180m 3 / h, cooling water volume of lower header: 160~220m 3 / h, and the roller speed is 0.8~1.2m / s; the rolling reduction from the n+1th to the n+3th pass is ≥40mm, and the rolling temperature of the n+1th pass is ≥950℃; when it comes to the mth pass, the rolling temperature is ≥900℃, and the billet is rolled to a thickness of 2.5~3.5 times the target thickness of the composite plate; then water cooling is carried out until the surface temperature of the billet drops below 840℃; then the second stage rolling is carried out until the billet thickness reaches the target thickness of the composite plate, completing the entire rolling process, the rolling temperature of the first pass of the second stage rolling is 810℃~840℃, and the rolling temperature of the last pass is 780~810℃.

[0014] To achieve the above-mentioned purpose, an embodiment of the present invention provides a stainless steel composite plate for bridge structure, wherein the preparation method thereof includes a process flow of blank preparation, coating of a release agent, blank assembly, sealing welding, vacuuming, sealing, heating, rolling, cooling, plate separation, and flattening; wherein,

[0015] During the assembly process, the blank is assembled in a manner such that an upper carbon steel substrate A, a lower carbon steel substrate B, an intermediate layer of at least two stainless steel composite materials, and four sealing strips surround the four sides of the intermediate layer. Gas shielded welding is performed between the seals and substrate A, and between the seals and substrate B, to form a blank. The four sides of the blank have grooves of depth D enclosed by substrate A, the seals, and substrate B. In addition, the seal on one side of the blank has a circular through hole, into which a steel pipe with an outer diameter of r is welded.

[0016] In the sealing welding process: the groove is surfacing welded, and a hole with a radius R>r and concentric with the steel pipe is reserved around the steel pipe during surfacing welding; when the groove on the side where the steel pipe is located is surfacing welded to a penetration depth of 2 / 3 of the groove depth, and the grooves on other sides are surfacing welded to a penetration depth of more than 2 / 3 of the groove depth, surfacing welding is stopped;

[0017] In the sealing process: after the base blank is vacuumed, the steel pipe is heated with a flame gun, flattened, and folded into the reserved hole; the hole is then fully welded with gas shielded welding to seal the steel pipe in the hole; then, surfacing welding is continued until the groove is filled, and finally, cap welding is performed to obtain a composite blank;

[0018] In the rolling process: the composite billet coming out of the heating furnace is rolled to obtain a large composite plate; in the entire rolling process, the first n passes are transverse rolling, and the longitudinal rolling is adopted after the n+1 pass, and the rolling reduction of the first pass is ≥25mm and the rolling temperature is ≥1060℃. The width of the billet obtained by rolling the nth pass is Wt+0~40mm, Wt is the target width of the large composite plate, and the rolling temperature of the nth pass is ≥1030℃; between the nth pass and the n+1 pass and between the n+2 pass and the n+3 pass, the billet is water-cooled once in 6 groups of headers, and the cooling water volume of the upper header of each group of headers is 120~180m 3 / h, cooling water volume of lower header: 160~220m 3 / h, and the roller speed is 0.8~1.2m / s; the rolling reduction from the n+1th to the n+3th pass is ≥40mm, and the rolling temperature of the n+1th pass is ≥950℃; when it comes to the mth pass, the rolling temperature is ≥900℃, and the billet is rolled to a thickness of 2.5~3.5 times the target thickness of the composite plate; then water cooling is carried out until the surface temperature of the billet drops below 840℃; then the second stage rolling is carried out until the billet thickness reaches the target thickness of the composite plate, completing the entire rolling process, the rolling temperature of the first pass of the second stage rolling is 810℃~840℃, and the rolling temperature of the last pass is 780~810℃;

[0019] The chemical composition of the substrate layer of the composite plate is as follows, by mass percentage: C: 0.03-0.16%, Si: 0.11-0.29%, Mn: 1.31-1.54%, P≤0.018%, S≤0.0030%, Cr: 0.06-0.29%, Ni≤0.24%, Cu≤0.24%, Mo≤0.24%, Nb: 0.011-0.034%, Ti: 0.011-0.019%, Al: 0.030-0.040%, and the balance is Fe and unavoidable impurities;

[0020] The chemical composition of the composite material layer of the composite plate is as follows in percentage by mass: C≤0.15%, Si≤1.00%, Mn≤2.00%, P≤0.045%, S≤0.030%, Ni: 6.0-22.0%, Cr: 16.0-26.0%, Mo≤3.0%, and the balance is Fe and unavoidable impurities;

[0021] The composite interface bonding rate of the composite plate is 100%, and the shear strength is ≥300 MPa.

[0022] Thus, compared with the prior art, one embodiment of the present invention, on the one hand, can wrap the stainless steel composite material within the substrate and the seal through the assembly method, sealing and sealing method, which is beneficial to ensuring the surface quality of the stainless steel composite material, and there is no need to dig grooves and make blanks as in the prior art, and the yield rate is high. In addition, it can achieve vacuuming and avoid air leakage and cracks in the composite blank, thereby ensuring the interface bonding quality. On the other hand, the assembly, sealing and sealing methods are combined with rolling technology, especially the use of a new rolling technology in this field, which can ensure the temperature uniformity of the composite blank and ensure that the core of the composite blank is effectively penetrated. Furthermore, it can not only ensure that the advantages of the substrate and the composite material themselves can be brought into play, but more importantly, it can also ensure the interface bonding quality between the substrate and the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] For the sake of clarity in presentation and description, in the various drawings of the present invention, certain dimensions of structures or parts are exaggerated relative to other structures or parts. Therefore, these drawings are only used to illustrate the basic structure of the subject matter of the present invention.

[0024] FIG1 is a flow chart of the preparation method provided by the present invention;

[0025] FIG2 is a schematic diagram of a composite blank in the preparation stage according to the first embodiment of the present invention;

[0026] 3 is a schematic cross-sectional view of a base blank obtained in the sealing welding step in the composite blank preparation stage of the first embodiment of the present invention, wherein the cross-section passes through the central axis of the steel pipe and is perpendicular to the width direction of the base blank;

[0027] FIG4 is an enlarged view of the circled area in FIG3 ;

[0028] 5 is another schematic cross-sectional view of the base blank obtained in the sealing welding step in the composite blank preparation stage of the first embodiment of the present invention, the cross section passing through the central axis of the steel pipe and perpendicular to the thickness direction of the base blank;

[0029] FIG6 is a schematic diagram of a finished single-sided stainless steel composite plate obtained according to the first embodiment of the present invention;

[0030] 7 is a schematic diagram of a composite blank in the preparation stage according to the second embodiment of the present invention;

[0031] 8 is a schematic cross-sectional view of a base blank obtained in the sealing welding step in the composite blank preparation stage according to the second embodiment of the present invention, wherein the cross-section passes through the central axis of the steel pipe and is perpendicular to the width direction of the base blank;

[0032] FIG9 is an enlarged view of the circled area in FIG8 ;

[0033] 10 is another schematic cross-sectional view of the base blank obtained in the sealing welding step in the composite blank preparation stage of the second embodiment of the present invention, the cross section passing through the central axis of the steel pipe and perpendicular to the thickness direction of the base blank;

[0034] FIG11 is a schematic diagram of a finished single-sided stainless steel composite plate obtained according to the second embodiment of the present invention;

[0035] 12 is a schematic diagram of a composite blank in the preparation stage according to the third embodiment of the present invention;

[0036] 13 is a schematic cross-sectional view of a base blank obtained during the sealing and welding step in the composite blank preparation stage according to the third embodiment of the present invention, wherein the cross-section passes through the central axis of the steel pipe and is perpendicular to the width direction of the base blank;

[0037] FIG14 is an enlarged view of the circled area in FIG13 ;

[0038] 15 is another schematic cross-sectional view of the base blank obtained in the sealing welding step in the composite blank preparation stage of the third embodiment of the present invention, the cross section passing through the central axis of the steel pipe and perpendicular to the thickness direction of the base blank;

[0039] FIG16 is a schematic diagram of a finished single-sided stainless steel composite plate obtained according to the third embodiment of the present invention;

[0040] 17 is a schematic diagram of a composite blank in the preparation stage according to the fourth embodiment of the present invention;

[0041] FIG18 is a schematic cross-sectional view of a base blank obtained during the sealing welding step in the composite blank preparation stage according to the fourth embodiment of the present invention, wherein the cross-section passes through the central axis of the steel pipe and is perpendicular to the width direction of the base blank;

[0042] FIG19 is an enlarged view of the circled area in FIG18 ;

[0043] FIG20 is another schematic cross-sectional view of the base blank obtained in the sealing welding step in the composite blank preparation stage of the fourth embodiment of the present invention, the cross section passing through the central axis of the steel pipe and perpendicular to the thickness direction of the base blank;

[0044] FIG21 is a schematic diagram of a finished single-sided stainless steel composite plate obtained according to the fourth embodiment of the present invention;

[0045] 22 is a schematic diagram of a composite blank in the preparation stage according to the fifth embodiment of the present invention;

[0046] FIG23 is a schematic cross-sectional view of a base blank obtained during the sealing welding step in the composite blank preparation stage according to the fifth embodiment of the present invention, wherein the cross-section passes through the central axis of the steel pipe and is perpendicular to the width direction of the base blank;

[0047] FIG24 is an enlarged view of the circled area in FIG23;

[0048] FIG25 is another schematic cross-sectional view of the base blank obtained in the sealing welding step in the composite blank preparation stage of the fifth embodiment of the present invention, the cross section passing through the central axis of the steel pipe and perpendicular to the thickness direction of the base blank;

[0049] FIG26 is a schematic diagram of a finished single-sided stainless steel composite plate obtained according to the fifth embodiment of the present invention. DETAILED DESCRIPTION

[0050] One embodiment of the present invention provides a method for preparing a single-sided stainless steel composite plate for a bridge structure, and provides a single-sided stainless steel composite plate for a bridge structure, wherein the composite plate is prepared using the preparation method of one embodiment of the present invention.

[0051] Specifically, as shown in Figure 1, the preparation method includes a process flow of blank preparation, release agent coating, blank assembly, sealing, vacuuming, sealing, heating, rolling, cooling, plate separation, and flattening. In other words, the present invention produces a single-sided stainless steel composite plate through a process of blank preparation - release agent coating - blank assembly - sealing - vacuuming - sealing - heating - rolling - cooling - plate separation - and flattening.

[0052] Among them, a composite blank is prepared through the blank preparation process, the isolation agent coating process, the blank assembly process, the sealing process, the vacuum process and the sealing process, so the stage from the blank preparation process to the sealing process is referred to as the composite blank preparation stage in this application; thereafter, the composite blank is made into a large composite plate through the heating process, the rolling process and the cooling process, so the stage from the heating process to the cooling process is referred to as the composite blank rolling stage in this application; finally, the large composite plate is made into at least two small single-sided stainless steel composite plates through the plate separation process and the flattening process, that is, the finished single-sided stainless steel composite plate, so this stage is referred to as the finished plate stage in this application.

[0053] Furthermore, the present invention provides multiple implementations of the composite blank preparation stage, which are described in detail below.

[0054] <First embodiment of composite blank preparation stage>

[0055] 2 to 6 , a first embodiment of the composite blank preparation stage is shown.

[0056] In this embodiment, referring to FIG2 , the blank preparation process specifically includes:

[0057] Prepare two carbon steel billets with a thickness of T1, a length of L1, and a width of W1 as two substrates, which are distinguished as substrate 11A and substrate 11B in FIG2 ;

[0058] The surface to be composited of each substrate is ground and polished, for example, the surface 11As of substrate 11A and the surface 11Bs of substrate 11B, to remove surface oxide scale and expose the metallic luster. After the surface grinding treatment, the roughness Ra of the surface to be composited is less than 5 μm.

[0059] Two stainless steel billets with a thickness of T2, a length of L2, and a width of W2 are prepared as two composite materials, which are distinguished as composite materials 12A and 12B in FIG2 ;

[0060] The surface to be composited of each composite material is ground and polished, for example, surface A1s of composite material 12A and surface B1s of composite material 12B, to remove surface oxide scale and reveal metallic luster. After the surface grinding treatment, the roughness Ra of the surface to be composited is less than 5 μm.

[0061] Wherein, L2<L1, W2<W1, and the length and width of the composite material are both smaller than those of the base material. More preferably, L1≥2500mm, W2≥1600mm, and T1≥60mm; the range of L1-L2 is 90-150mm, and the range of W1-W2 is also 90-150mm.

[0062] It can be understood that in this embodiment, each substrate is a uniformly thick blank with a constant thickness of T1. Accordingly, the substrate layer of the stainless steel composite plate obtained in this embodiment (obtained from the substrate by the preparation method) has a constant thickness.

[0063] Here, the term "surface to be bonded" refers to the surface of the substrate and composite material that requires interfacial bonding when forming a composite panel. For example, for a pair of substrates and composite materials, one of the two surfaces along their thickness direction can be selected as the surface to be bonded, and these surfaces will be interfacially bonded in a subsequent step. For example, surface 11As of substrate 11A and surface A1s of composite material 12A will be interfacially bonded in a subsequent step, and surface 11Bs of substrate 11B and surface B1s of composite material 12B will be interfacially bonded in a subsequent step.

[0064] Preferably, surface 11As of substrate 11A and surface 11Bs of substrate 11B are ground and polished using a grinding wheel, belt sander, or milling machine to remove surface oxide scale and reveal a metallic luster. Surface A1s of composite material 12A and surface B1s of composite material 12B are ground and polished using a wire wheel to remove surface oxide scale and reveal a metallic luster.

[0065] Here, only the surface grinding treatment of the to-be-combined surface of each substrate and each composite is described. However, it should be noted that the surface grinding treatment of other surfaces of each substrate and composite can be further performed. Although such additional grinding treatment of other surfaces is not necessary to achieve the technical effect of the present invention, it may be more preferable.

[0066] Furthermore, in this embodiment, the release agent application step specifically includes applying the release agent to the non-composite surface of at least one composite material. Specifically, the release agent can be applied to the non-composite surface of each composite material, such as surface A2s of composite material 12A or surface B2s of composite material 12B. Alternatively, the release agent can be applied to only one of the two composite materials. In this manner, the release agent prevents the two composite materials from bonding during the subsequent composite billet rolling step, which could result in difficulty in separating the composite materials.

[0067] It can be understood that the surface not to be composited is opposite to the surface to be composited of the composite material, and the two constitute two surfaces of the composite material in the thickness direction.

[0068] Regarding the composition of the release agent, the first option is: a coating solution containing silicon oxide and magnesium oxide, wherein the mass ratio of silicon oxide to magnesium oxide is 3:1. The release agent of this embodiment can achieve a good isolation effect and ensure the subsequent separation of the two composite board plates. Using the release agent, the total amount of the release agent 13 (see Figure 3) between the two composite materials is 20 μmg / m 2 , y is the ratio of the thickness of the composite blank prepared in the composite blank preparation step to the thickness of the composite plate formed by subsequent rolling. This ratio is also called the composite blank rolling reduction ratio. Here, a method for configuring the release agent is provided, which is: polyvinyl alcohol and thermosetting phenolic resin are mixed in a mass ratio of 1:1 to obtain binder powder; silicon oxide and magnesium oxide are mixed in a mass ratio of 3:1 to obtain release agent powder; and the release agent powder, binder powder and water are mixed in a mass ratio of 27:3:70 to obtain a fluid release agent coating liquid. After the release agent is applied and before the subsequent assembly process, the composite material coated with the release agent is placed in a trolley furnace for heating and drying. The drying temperature is 340-360°C and the drying time is 35-45 minutes.

[0069] Regarding the composition of the release agent, a second optional solution is: a weight ratio of 25-35% silicon nitride, 5-10% thermosetting amino resin, and 55-70% water. Compared to existing release agents, and even compared to the first embodiment of the release agent, this release agent not only achieves excellent isolation, ensuring the subsequent separation of the two composite board panels, but also boasts strong chemical stability and high-temperature and thermal shock resistance from the active ingredient, silicon nitride. The thermosetting amino resin, serving as the binder, cures at low temperatures, is non-toxic, and achieves strong adhesion with minimal usage. Consequently, it offers low cost, simple operation, and excellent isolation and adhesion properties.

[0070] Here, a preferred configuration method of the release agent of the second optional scheme is provided, comprising: first placing 5-10% silicon nitride (by weight percentage) in a container such as a beaker, and then pouring in 15-25% water and stirring; after the silicon nitride has no granularity and no bubbles, pouring in 2-3% thermosetting amino resin and continuing to stir; when it becomes viscous, continue to pour in the remaining silicon nitride and water, stir for 3-5 minutes, and then pour in the remaining thermosetting amino resin; when it is stirred until it becomes viscous, the release agent is prepared.

[0071] For the release agent of the second optional solution, the total amount of release agent 13 (see Figure 3) between the two composite materials is applied to a thickness of 0.2 to 0.5 mm. After the release agent is applied and before the subsequent assembly process, the composite materials coated with the release agent are heated and dried at a temperature of 100 to 250°C for 20 to 40 minutes. It should be noted that in the drawings of this application, the thickness of the release agent 13 between the two composite materials is exaggerated for ease of understanding and explanation. That is, the thickness of the release agent 13 illustrated in the drawings is exaggerated relative to the thickness of the substrate, the composite material, and the width of the seal described later.

[0072] For the first and second optional options of the release agent, if the release agent is applied to both surface A2s of the composite material 12A and surface B2s of the composite material 12B, the amount of release agent applied to each of surface A2s and surface B2s can be half of the total amount. If the release agent is applied to only one of surface A2s and surface B2s, the release agent is applied according to the total amount.

[0073] Furthermore, referring to FIG. 3 , the blank assembly process specifically includes: assembling the blank in a manner in which the composite materials 12A and 12B are the middle layers, the base material 11A is stacked on top, the base material 11B is stacked on the bottom, and four seals 14 are surrounded on the four sides of the middle layer; and performing gas shielded welding between the upper edge of the seal 14 and the base material 11A, and between the lower edge of the seal 14 and the base material 11B, to form a blank.

[0074] Specifically, in an alternative embodiment, the substrate 11A, composite material 12A, composite material 12B, and substrate 11B can be stacked first, and then the seal 14 can be wrapped around the four sides of the composite materials 12A and 12B. Finally, the upper edge of the seal 14 and the surface 11As of the substrate 11A, and the lower edge of the seal 14 and the surface 11Bs of the substrate 11B can be welded together. Of course, in an alternative embodiment, the lower edge of the seal 14 and the surface 11Bs of the substrate 11B can also be welded together first, with the seal 14 forming a quadrilateral frame on the surface 11Bs of the substrate 11B. The composite materials 12B and 12A can then be placed in this frame, and the composite material 12A and the frame can then be covered with the substrate 11A. Finally, the upper edge of the seal 14 and the surface 11As of the substrate 11A can be welded together. In yet another alternative embodiment, gas shielded welding can be performed on the upper edge of the seal 14 and the surface 11As of the substrate 11A. The substrate 11B, composite material 12B, and composite material 12A are then stacked in sequence from bottom to top. The combined seal 14 and substrate 11A are then placed over and around the composite materials 12A and 12B. Finally, gas shielded welding can be performed on the lower edge of the seal 14 and the surface 11Bs of the substrate 11B. These embodiments do not deviate from the spirit of the present invention.

[0075] Further preferably, during the billet assembly process, after the base material 11A, composite material 12A, composite material 12B, and base material 11B have been stacked, and before the upper or lower edge of the seal 14 is welded to the base material, the stacked steel materials are placed under a four-column hydraulic press. The opposing surfaces of the two base materials (i.e., the upper surface of base material 11A and the lower surface of base material 11B) are pressurized to a pressure of 500 tons or more. This ensures closer contact between adjacent steel billets.

[0076] Preferably, during the assembly process, when performing gas shielded welding between the edge of seal 14 and the substrate, the welding current is 220-240A, the welding voltage is 28-32V, the welding speed is 300-360mm / min, and the interpass temperature is controlled at 140-160°C. Furthermore, prior to gas shielded welding, substrates 11A and 11B are preferably preheated and baked using a flame gun at a temperature of 150-250°C.

[0077] In this embodiment, referring to FIG. 3 , in the middle layer, the composite material 12A and the composite material 12B are stacked up and down, and the sealing strip 14 is wrapped around the four sides of the composite materials 21 and 22 .

[0078] It can be understood that in the base blank obtained in the assembly process, the surface 11As of the substrate 11A and the surface A1s of the composite material 12A are facing each other and in contact as the surfaces to be composited, the surface 11Bs of the substrate 11B and the surface B1s of the composite material 12B are facing each other and in contact as the surfaces to be composited, and the surface A2s of the composite material 12A and the surface B2s of the composite material 12B are facing each other and in contact as the surfaces not to be composited.

[0079] Furthermore, all four sides of the resulting base blank have grooves formed by the base material 11A, the sealing strip 14, and the base material 11B. Preferably, the depth of the grooves on all four sides of the base blank is set to be the same, as indicated by depth D in Figure 4, with a value ranging from 40 to 60 mm. By controlling this depth D, not only can weld cracking during rolling of the composite blank be effectively avoided, but also the formation of weld thermal cracks due to deep penetration during subsequent sealing, which can affect the sealing quality of the composite blank.

[0080] It is understood that the depth of the groove depends on the length and width difference between the composite material and the substrate, as well as the thickness of the seal 14. For example, during the blank assembly process, the composite material is centered relative to the substrate, and the distance between the two sides (i.e., long sides) of the composite material in the transverse direction (i.e., width direction) and the corresponding two sides (i.e., long sides) of the substrate are equal, and the distance is 45-75 mm. The distance between the two sides (i.e., short sides) of the composite material in the longitudinal direction (i.e., length direction) and the corresponding two sides (i.e., short sides) of the substrate are also equal, and the distance is 45-75 mm. The thickness T3 of the seal is 10-15 mm. The groove depth D of the long side of the blank is (W1-W2-2T3) / 2, and the groove depth D of the short side is (L1-L2-2T3) / 2.

[0081] Regarding the overall dimensions of the four seals 14, at the long sides of the baseboard, the length L31 of the seal 14 is L2 to L2-2 mm, while at the short sides, the length L32 of the seal 14 is W2 to W2-2 mm. The width W3 of the seal 14 is 2T2 to 2T2-2 mm, and the thickness T3 is 10-15 mm, as previously mentioned. Preferably, the width W3 and thickness T3 of the seals 14 on all four sides of the baseboard are the same. However, this is not a limitation. It should be noted that, as previously mentioned, the thickness of the release agent 13 is exaggerated in FIG3 for ease of understanding and illustration. Accordingly, the width of the seal 14 shown in FIG3 and FIG4 appears to be greater than the sum of the thicknesses of the two composite materials. This is simply due to the exaggerated thickness of the release agent 13. In reality, the width W3 of the seal 14 is equal to or slightly less than the sum of the thicknesses of composite materials 12A and 12B by approximately 2 mm.

[0082] More preferably, referring to FIG4 , the upper and lower edges of the outer surface of seal 14 are beveled, with a bevel angle of 10-20° and a vertical bevel depth P of 10-15 mm. Here, the "outer surface of seal 14" refers to the surface of seal 14 facing away from composite materials 12A and 12B. To put it another way, bevels are formed on both the upper and lower edges of one surface of seal 14. During the assembly process, seal 14 is assembled with substrate 11A, substrate 11B, composite material 12B, and composite material 12A with this "one surface" of seal 14 facing outward. Beveling not only avoids spot welding the inner side of the seal and the thermal effects on the substrate caused by multiple welding passes, but also facilitates subsequent bevel welding and ensures robustness.

[0083] 4 , the groove angle K1 at the upper edge and the groove angle K2 at the lower edge of the outer surface of the seal 14 are respectively 10-20°, and the two can be the same or different.

[0084] Furthermore, a circular through-hole is formed in the seal on one side of the base blank. During the assembly process, a steel tube 16 with an outer diameter r is welded into the through-hole. The through-hole can be machined before the gas shielded welding of the seal 14 and the base materials 11A and 11B, or it can be machined after the gas shielded welding is completed and the base blank is formed. All of these remain within the technical scope of this application.

[0085] Preferably, the aperture of the through hole is consistent with the outer diameter of the steel pipe 16, both being r.

[0086] More preferably, as shown in FIG5 , the through hole is formed on the seal 14 at one short side of the base blank, and the through hole is centered at a position 1 / 3 of the length (i.e., 1 / 3 of L32) and 1 / 2 of the width (i.e., 1 / 2 of W3) of the seal 14. Referring to FIG4 , the end surface of the steel tube 16 is flush with the inner surface of the seal 14. This ensures a vacuum effect.

[0087] Preferably, the length of the steel pipe 16 ranges from T3+2D to T3+2D+R.

[0088] Furthermore, in this embodiment, the sealing process specifically includes:

[0089] The grooves on the four sides of the base blank are subjected to surfacing welding, specifically, for example, submerged arc surfacing welding; and, during the surfacing welding process, referring to FIG. 4 and FIG. 5 , a hole 15H concentric with the steel pipe 16 and having a radius R>r is reserved around the steel pipe 16;

[0090] When the groove on the side where the steel pipe 16 is located is built-up welded to a depth of 2 / 3 of the groove depth, and the grooves on other sides are built-up welded to a depth of more than 2 / 3 of the groove depth, for example, in an embodiment where the groove depths of all four sides are D, that is, when the groove on the side where the steel pipe 16 is located is built-up welded to a depth of 2 / 3D, and the grooves on other sides are built-up welded to a depth of more than 2 / 3D, the build-up welding is terminated.

[0091] It can be understood that a filling layer in the shape of a square frame is formed outside the surrounding frame formed by the seal 14 by surfacing welding, referring to FIG. 3 to FIG. 5 , in which the filling layer formed by surfacing welding is marked as 15 .

[0092] More preferably, the sealing process is terminated when the groove on the side where the steel pipe 16 is located is built-up welded to a penetration depth of 2 / 3 of the groove depth, and the grooves on the other sides are built-up welded to a penetration depth of the groove depth. For example, in an embodiment where the groove depths on all four sides are D, that is, when the groove on the side where the steel pipe 16 is located is built-up welded to a penetration depth of 2 / 3D, and the grooves on the other sides are built-up welded to a penetration depth of D. In this way, the grooves on the other three sides are completely filled with built-up welding, which not only ensures that the base blank will not leak during vacuuming, but also facilitates the subsequent complete sealing welding of the vacuum tube in the groove, thereby further ensuring the sealing of the composite blank.

[0093] Furthermore, during the surfacing process, multi-layer and multi-pass welding is performed in the order of the upper and lower edges first and the middle area later, which not only allows the heat generated during the welding process to be fully diffused, but also avoids welding through the seal; each layer is welded for more than 4 passes, the interpass temperature is 140-160°C, the total number of welding layers is 6-8 layers, and the interlayer temperature is 150-250°C, which not only effectively improves the strength of the welded joint, but also reduces the impact of welding on the microstructure and properties of the base material and composite material.

[0094] In addition, before surfacing, the flux used is pre-baked and kept warm for use. The baking temperature is 300-350°C, the baking time is 90-120 minutes, and the insulation temperature is 100-150°C.

[0095] Preferably, during the surfacing process, the welding current is 550-650 A, the welding voltage is 28-32 V, and the welding speed is 400-500 mm / min.

[0096] Furthermore, after the surfacing welding is stopped as described above, the base blank is vacuumed and then sealed. The vacuuming process can be implemented using existing known technologies, and this embodiment provides a preferred solution. Specifically, the preferred vacuuming process includes: vacuuming the inner space of the base blank three times and breaking the vacuum twice through the steel pipe, and finally maintaining the vacuum degree of the inner space of the base blank at ≤10 -2 Pa.

[0097] More preferably, the vacuuming process includes:

[0098] First, connect the steel pipe to the vacuum pump to evacuate the interior space of the base blank to a vacuum degree of ≤10 -2 Pa, and then maintain the pressure for more than 4 hours; then connect the steel pipe to the nitrogen supply device, break the base blank, and fill it with nitrogen;

[0099] Afterwards, the steel pipe is connected to the vacuum pump again to evacuate the base blank to a vacuum degree of ≤10 -1 Pa, no pressure maintenance; then the steel pipe is connected to the nitrogen supply device again, the base blank is broken and filled with nitrogen;

[0100] Finally, the steel pipe is connected to the vacuum pump for the third time to evacuate the base blank to a vacuum degree of ≤10 -2 Pa, then there is no need to maintain pressure, and the sealing process can be carried out directly.

[0101] Furthermore, the sealing process specifically includes: heating the steel pipe 16 with a flame gun, flattening it, and then folding it into the reserved hole 15H; then fully welding the hole with gas shielded welding to seal the steel pipe in the hole 15H; next, continuing the surfacing welding until the groove on the side where the steel pipe 16 is located is filled, and finally performing cover welding to obtain a composite billet.

[0102] In this way, through the assembly, welding and sealing steps of the present invention, a hole 15H is reserved at the weld, which increases the handling space of the steel pipe 16, reduces the difficulty of welding, improves the welding efficiency, avoids sealing leakage, prevents the steel pipe 16 from falling off due to collision, and thus ensures the sealing of the composite blank as a whole, thereby preventing cracking and leakage during rolling; furthermore, the interface bonding of the prepared composite plate is excellent and the production cost is reduced.

[0103] It is understandable that the shape and size of the blanks prepared in the composite blank preparation stage and the method of assembly affect the structural shape of the final stainless steel composite plate.

[0104] As shown in FIG6 , in this embodiment, based on the equal-thickness substrates prepared in the blank preparation process and the intermediate layers in the blank assembly process being the stacked arrangement of composite material 12A and composite material 12B, the composite blanks based on this embodiment, after the subsequent composite blank rolling stage and the plate finished product stage, produce two stainless steel composite plates, both of which have a constant thickness of the substrate layer and consistent length and width of the composite layer and the substrate layer.

[0105] For example, the obtained stainless steel clad plate 10A has a base layer 11A and a composite layer 12A, each of which is obtained by rolling the base layer 11A and the composite material 12A described above. Therefore, the designations of the original base layer 11A and the composite material 12A are retained. The base layer 11A is a carbon steel material of uniform thickness, and the composite layer 12A is a stainless steel material. The length and width of the composite layer 12A are consistent with those of the base layer 11A.

[0106] For another example, the obtained stainless steel composite plate 10B has a base layer 11B and a composite layer 12B, each of which is obtained by rolling the base layer 11B and the composite material 12B described above. Therefore, the numbers of the original base layer 11B and the composite material 12B are retained. The base layer 11B is a carbon steel material of uniform thickness, and the composite layer 12B is a stainless steel material. The length and width of the composite layer 12B are consistent with those of the base layer 11B.

[0107] In summary, a single-sided stainless steel clad plate is provided, which is manufactured from the clad blank prepared in this embodiment through a clad blank rolling stage and a plate finishing stage. The clad plate is a fully covered uniform thickness plate having a total thickness of 5 to 55 mm, a base material layer thickness of 4 to 45 mm, and a clad material layer thickness of 1 to 10 mm.

[0108] The above describes in detail the various steps involved in preparing the composite blanks according to this embodiment. In the various experimental examples provided below, Experimental Examples 1 through 3 employ this embodiment to prepare composite blanks, which are then used to produce stainless steel composite plates. Table 1 shows some parameters of the composite blanks used in these examples. The parameters denoted by the symbols are described above.

[0109] Table 1

[0110] <Second embodiment of composite billet preparation stage>

[0111] Figures 7 to 11 illustrate a second embodiment of the composite blank preparation stage. This embodiment differs from the first embodiment of the composite blank preparation stage described above only in the shape of the substrate prepared during the blank preparation process. The release agent coating, blank assembly, welding, vacuuming, and sealing processes remain the same as those of the first embodiment. Only the differing blank preparation steps will be described in detail below; the remaining steps will be understood in conjunction with the accompanying drawings and the first embodiment of the composite blank preparation stage described above and will not be further elaborated.

[0112] In this embodiment, referring to FIG7 , the blank preparation process specifically includes:

[0113] Prepare two carbon steel billets with a length L1, a width W1, and a thickness varying along the X direction as two substrates, which are distinguished as substrate 21A and substrate 21B in FIG7 ;

[0114] The surface to be composited of each substrate is ground and polished, for example, the surface 21As of substrate 21A and the surface 21Bs of substrate 21B, to remove surface oxide scale and expose the metallic luster. After the surface grinding treatment, the roughness Ra of the surface to be composited is less than 5 μm.

[0115] Two stainless steel billets having a thickness of T2, a length of L2, and a width of W2 are prepared as two composite materials, which are distinguished as composite materials 22A and 22B in FIG. 7 ;

[0116] The surface to be composited of each composite material is ground and polished, for example, surface A1s of composite material 22A and surface B1s of composite material 22B, to remove surface oxide scale and reveal metallic luster. After the surface grinding treatment, the roughness Ra of the surface to be composited is less than 5 μm.

[0117] Wherein, L2<L1, W2<W1, and the length and width of the composite material are both smaller than those of the base material. More preferably, L1≥2500mm, W2≥1600mm; the range of L1-L2 is 90-150mm, and the range of W1-W2 is also 90-150mm.

[0118] Furthermore, substrates 21A and 21B are carbon steel billets with varying thickness along the X-direction. That is, they are not billets of constant thickness, but rather have thicknesses that vary along the X-direction. Here, the X-direction is the width or length of the substrate. In the embodiment shown in FIG10 , the X-direction is illustrated as the length of the substrate.

[0119] Further preferably, the surface to be laminated 21As of substrate 21A and the surface to be laminated 21Bs of substrate 21B are relatively complementary, that is, the two surfaces complement each other when facing each other. This complementarity makes the surface of substrate 21A not to be laminated (i.e., the upper surface of substrate 21A in FIG. 7 ) and the surface of substrate 21B not to be laminated (i.e., the lower surface of substrate 21B in FIG. 7 ) parallel. Accordingly, as shown in FIG. 8 , in the base blank produced in the subsequent assembly process, the upper surface of substrate 21A and the lower surface of substrate 21B are parallel. To put it another way, the surface to be composited 21As of the substrate 21A and the surface to be composited 21Bs of the substrate 21B are relatively complementary, that is, when the surface to be composited 21As of the substrate 21A and the surface to be composited 21Bs of the substrate 21B are relatively buckled up and down, the two can just fit together surface to surface, that is, when the surface to be composited 21As of the substrate 21A and the surface to be composited 21Bs of the substrate 21B are relatively buckled up and down, the sum of the thicknesses of the substrate 21A and the substrate 21B is constant.

[0120] In the embodiment shown in the accompanying drawings, substrates 21A and 21B are both plates of varying thickness, with thicknesses varying monotonically along the X-direction. Both the surface to be bonded 21As of substrate 21A and the surface to be bonded 21Bs of substrate 21B are inclined planes. The inclination angle of surface to be bonded 21As (e.g., the angle with the non-bonded surface of substrate 21A) is equal to the inclination angle of surface to be bonded 21Bs (e.g., the angle with the non-bonded surface of substrate 21B).

[0121] It is understandable that the shape and size of the blanks prepared in the composite blank preparation stage and the method of assembling the blanks affect the structural shape of the final stainless steel composite plate.

[0122] In this embodiment, as shown in FIG11 , based on the substrate with monotonically varying thickness along the X direction prepared in the blank preparation process, and the intermediate layer in the blank assembly process being the stacked arrangement of composite material 22A and composite material 22B, the composite blank based on this embodiment, after the subsequent composite blank rolling stage and the plate finished product stage, produces two stainless steel composite plates, both of which have a substrate layer with monotonically varying thickness along the X direction, and the four sides of the composite layer and the substrate layer are flush.

[0123] For example, as shown in Figure 11, the resulting stainless steel clad plate 20A comprises a lower carbon steel substrate layer 21A and an upper stainless steel clad layer 22A, each of which is obtained by rolling the previously described substrate 21A and clad material 22A. Therefore, the original reference numbers of the original substrate 21A and clad material 22A are retained. The thickness of the substrate layer 21A varies along the X-direction. Specifically, the thickness varies monotonically along the X-direction. More specifically, the upper surface of the substrate layer 21A is an inclined plane relative to the lower surface of the substrate layer 21A. The four sides of the clad material 22A and the substrate layer 21A are flush, and the clad material 22A completely covers the upper surface of the substrate layer 21A.

[0124] For another example, as shown in Figure 11 , the resulting stainless steel composite plate 20B has a lower carbon steel substrate layer 21B and an upper stainless steel composite layer 22B, each of which is obtained by rolling the previously described substrate 21B and composite 22B. Therefore, the original substrate 21B and composite 22B reference numbers are retained. The thickness of substrate layer 21B varies along the X-direction. Specifically, the thickness varies monotonically along the X-direction. More specifically, the upper surface of substrate layer 21B is an inclined plane relative to the lower surface of substrate layer 21B. The four sides of composite layer 22B and substrate layer 21B are flush, and composite layer 22B completely covers the upper surface of substrate layer 21B.

[0125] In summary, a single-sided stainless steel clad plate is provided, which is manufactured from the clad blank prepared in this embodiment through a clad blank rolling stage and a plate finishing stage. The clad plate is a non-uniform plate with a total thickness of (5-47) to (7-55) mm, a base material layer thickness of (4-37) to (6-45) mm, and a clad material layer thickness of 1 to 10 mm, with the thickness of the clad material layer varying monotonically in the X direction.

[0126] The above describes in detail the various steps involved in preparing the composite blanks according to this embodiment. Among the various experimental examples provided below, Experimental Examples 4 through 6 employ this embodiment to prepare composite blanks, which are then used to produce stainless steel composite plates. Table 2 shows some parameters of the composite blanks used in these examples. The parameters denoted by the symbols are described above.

[0127] Table 2

[0128] <Third Implementation Method of Composite Billet Preparation Stage>

[0129] Figures 12 to 16 illustrate a third embodiment of the composite blank preparation stage. This embodiment differs from the first embodiment of the composite blank preparation stage described above only in the shape of the substrate prepared during the blank preparation process. The release agent coating, blank assembly, welding, vacuuming, and sealing processes remain the same as those of the first embodiment. Only the differing blank preparation steps will be described in detail below; the remaining steps will be understood in conjunction with the accompanying drawings and the first embodiment of the composite blank preparation stage described above and will not be further elaborated.

[0130] In this embodiment, referring to FIG12 , the blank preparation process specifically includes:

[0131] Prepare two carbon steel billets with a length L1, a width W1, and a thickness varying along the X direction as two substrates, which are distinguished as substrate 31A and substrate 31B in FIG12 ;

[0132] The surface to be composited of each substrate is ground and polished, for example, surface 31As of substrate 31A and surface 31Bs of substrate 31B, to remove surface oxide scale and expose metallic luster. After the surface grinding treatment, the roughness Ra of the surface to be composited is less than 5 μm.

[0133] Two stainless steel billets having a thickness of T2, a length of L2, and a width of W2 are prepared as two composite materials, which are distinguished as composite materials 32A and 32B in FIG. 7 ;

[0134] The surface to be composited of each composite material is ground and polished, for example, surface A1s of composite material 32A and surface B1s of composite material 32B, to remove surface oxide scale and reveal metallic luster. After the surface grinding treatment, the roughness Ra of the surface to be composited is less than 5 μm.

[0135] Wherein, L2<L1, W2<W1, and the length and width of the composite material are both smaller than those of the base material. More preferably, L1≥2500mm, W2≥1600mm; the range of L1-L2 is 90-150mm, and the range of W1-W2 is also 90-150mm.

[0136] Furthermore, substrates 31A and 31B are carbon steel billets with varying thickness along the X-direction. That is, they are not billets of constant thickness, but rather have thickness that varies along the X-direction. Here, the X-direction is the width or length of the substrate. In the embodiment shown in FIG15 , the X-direction is illustrated as the length of the substrate.

[0137] Further preferably, the surface to be laminated 31As of substrate 31A and the surface to be laminated 31Bs of substrate 31B are relatively complementary, that is, the two surfaces complement each other when facing each other. This complementarity makes the surface of substrate 31A not to be laminated (i.e., the upper surface of substrate 31A in FIG13 ) and the surface of substrate 31B not to be laminated (i.e., the lower surface of substrate 31B in FIG13 ) parallel. Accordingly, as shown in FIG13 , in the base blank produced in the subsequent assembly process, the upper surface of substrate 31A and the lower surface of substrate 31B are parallel. To put it another way, the surface to be composited 31As of the substrate 31A and the surface to be composited 31Bs of the substrate 31B are relatively complementary, that is, when the surface to be composited 31As of the substrate 31A and the surface to be composited 31Bs of the substrate 31B are relatively buckled up and down, the two can just fit together surface to surface, that is, when the surface to be composited 31As of the substrate 31A and the surface to be composited 31Bs of the substrate 31B are relatively buckled up and down, the sum of the thicknesses of the substrate 31A and the substrate 31B is constant.

[0138] In the embodiment shown in the drawings, both substrate 31A and substrate 31B are non-uniform thickness plates whose thickness varies non-monotonically along the X direction, and the surface to be composited 31As of substrate 31A and the surface to be composited 31Bs of substrate 31B both include two or more planes arranged along the X direction.

[0139] For example, shown in FIG12 , the surface 31As to be laminated of substrate 31A and the surface 31Bs to be laminated of substrate 31B both have seven planes. Taking surface 31Bs to be laminated of substrate 31B as an example, from left to right in FIG12 , the following are: a horizontal plane, an upwardly inclined plane, a downwardly inclined plane, a horizontal plane, a downwardly inclined plane, an upwardly inclined plane, and a horizontal plane. Of course, the specific shapes of surface 31As to be laminated of substrate 31A and surface 31Bs to be laminated of substrate 31B shown in the figure are merely examples, and the number of inclined planes each contains is not limited to that shown in the figure.

[0140] Furthermore, in this embodiment, the shape of each composite material prepared in the blank preparation step corresponds to the surface of the substrate to be bonded. For example, the shape of composite material 32A matches the surface 31As of substrate 31A to be bonded, and the shape of composite material 32B matches the surface 31Bs of substrate 31B to be bonded. Specifically, stainless steel billets of equal thickness can be bent to obtain composite materials having shapes matching the surfaces of the corresponding substrates to be bonded.

[0141] It is also understandable that the shape and size of the blanks prepared in the composite blank preparation stage and the method of assembling the blanks affect the structural shape of the final stainless steel composite plate.

[0142] In this embodiment, as shown in FIG16 , based on the substrate with non-monotonic thickness variation along the X direction prepared in the blank preparation process, and the intermediate layer in the blank assembly process being the stacked arrangement of composite material 32A and composite material 32B, the composite blank based on this embodiment, after the subsequent composite blank rolling stage and the plate finished product stage, produces two stainless steel composite plates, both of which have a substrate layer with non-monotonic thickness variation along the X direction, and the four sides of the composite material layer and the substrate layer are flush.

[0143] For example, as shown in Figure 16 , the resulting stainless steel clad plate 30A comprises a lower carbon steel substrate layer 31A and an upper stainless steel clad layer 32A, each of which is obtained by rolling the previously described substrate 31A and clad material 32A. Therefore, the original reference numbers of the original substrate 31A and clad material 32A are retained. The thickness of the substrate layer 31A varies along the X-direction. Specifically, the thickness varies non-monotonically along the X-direction. More specifically, the upper surface of the substrate layer 31A includes at least two planes arranged along the X-direction, with five planes being illustrated in the figure. The four sides of the clad layer 32A and the substrate layer 31A are flush, and the clad layer 32A completely covers the upper surface of the substrate layer 31A.

[0144] For another example, as shown in FIG16 , the resulting stainless steel composite plate 30B comprises a lower carbon steel substrate layer 31B and an upper stainless steel composite layer 32B, each of which is obtained by rolling the previously described substrate 31B and composite material 32B. Therefore, the original substrate 31B and composite material 32B are referenced. The thickness of substrate layer 31B varies along the X-direction. Specifically, the thickness varies non-monotonically along the X-direction. More specifically, the upper surface of substrate layer 31B includes at least two planes arranged along the X-direction, with five planes being illustrated in the figure. The four sides of composite layer 32B and substrate layer 31B are flush, and composite layer 32B completely covers the upper surface of substrate layer 31B.

[0145] In summary, a single-sided stainless steel clad plate is provided, which is manufactured from the clad blank prepared in this embodiment through a clad blank rolling stage and a plate finished product stage. The clad plate has a total thickness of (5-47) to (7-55) mm, a base material layer thickness of (4-37) to (6-45) mm, and a clad material layer thickness of 1 to 10 mm, with a non-uniform thickness plate having a non-monotonically varying thickness in the X direction.

[0146] The above describes in detail the various steps involved in preparing the composite blanks according to this embodiment. Among the various experimental examples provided below, Experimental Examples 7 through 9 employ this embodiment to prepare composite blanks, which are then used to produce stainless steel composite plates. Table 3 shows some parameters of the composite blanks used in these examples. The parameters denoted by the symbols are described above.

[0147] Table 3

[0148] <Fourth Implementation Method of Composite Billet Preparation Stage>

[0149] Figures 17 to 21 illustrate a fourth embodiment of the composite blank preparation stage. This embodiment differs from the first embodiment of the composite blank preparation stage described above only in the blank preparation process, the release agent coating process, and the blank assembly process. The welding, vacuuming, and sealing processes remain the same as those of the first embodiment. Only the differing processes will be described in detail below; the remaining processes will be understood in conjunction with the accompanying drawings and the first embodiment of the composite blank preparation stage described above and will not be further elaborated upon.

[0150] In this embodiment, referring to FIG17 , the blank preparation process specifically includes:

[0151] Two carbon steel billets having an X-axis dimension L1 and a Y-axis dimension W1 are prepared as two substrates, which are distinguished as substrate 41A and substrate 41B in FIG. 17 . Furthermore, the thicknesses of substrates 41A and 41B can be set to be the same or different. If different thicknesses are set, stainless steel composite plates of different thickness specifications can be produced accordingly.

[0152] The surface to be composited of each substrate is ground and polished, for example, surface 41As of substrate 41A and surface 41Bs of substrate 41B, to remove surface oxide scale and expose metallic luster. After the surface grinding treatment, the roughness Ra of the surface to be composited is less than 5 μm.

[0153] A stainless steel billet having an X-axis dimension L22, a Y-axis dimension W2, and a thickness T2 is prepared as a composite material, such as composite material 42A in FIG17 ; a side A3s of composite material 42A in the X-axis direction is a hypotenuse having a width V;

[0154] A stainless steel billet having an X-direction dimension of L21, a Y-direction dimension of W2, and a thickness of T2 is prepared as another composite material, such as composite material 42B in FIG. 17 ; one side B3s of composite material 42B in the X-direction is a hypotenuse having a width V;

[0155] A smaller surface of each composite material in the thickness direction constitutes a non-composite surface, such as surface A2s of composite material 42A and surface B2s of composite material 42B, while another larger surface constitutes a surface to be composited, such as surface A1s of composite material 42A and surface B1s of composite material 42B. The surface to be composited of each composite material is ground and polished to remove surface oxide scale and reveal a metallic luster. After this surface grinding process, the roughness Ra of the surface to be composited is less than 5 μm.

[0156] Based on the above dimensions, composite material 42A and composite material 42B have the same dimensions and thickness in the Y direction; while composite material 42A and composite material 42B can have the same dimensions in the X direction (i.e., L21 = L22) or different dimensions (i.e., L21 ≠ L22). If L21 = L22, a stainless steel composite plate can be produced with composite layers of the same dimensions and specifications in the X direction; if L21 ≠ L22, a stainless steel composite plate can be produced with composite layers of different dimensions and specifications in the X direction.

[0157] The width V refers to the span of the hypotenuse in the X direction. Due to the existence of the hypotenuse, one of the two surfaces in the thickness direction of each composite material is the larger surface and the other is the smaller surface.

[0158] Furthermore, L1 ≥ 2500 mm, W2 ≥ 1600 mm, and T1 ≥ 60 mm. Regarding the dimensional relationship between composite materials 42A, 42B and substrates 41A, 41B, L21 + L22 - V < L1, W2 < W1. More preferably, W1 = W2 + 90 to 150 mm, and L1 = L21 + L22 - V + 90 to 150 mm.

[0159] Preferably, surface 41As of substrate 41A and surface 41Bs of substrate 41B are ground and polished using a grinding wheel, belt sander, or milling machine to remove surface oxide scale and reveal a metallic luster. Surface A1s of composite material 42A and surface B1s of composite material 42B are ground and polished using a wire wheel to remove surface oxide scale and reveal a metallic luster.

[0160] Here, only the surface grinding treatment of the to-be-combined surface of each substrate and each composite is described. However, it should be noted that the surface grinding treatment of other surfaces of each substrate and composite can be further performed. Although such additional grinding treatment of other surfaces is not necessary to achieve the technical effect of the present invention, it may be more preferable.

[0161] Furthermore, in this embodiment, the release agent coating step specifically includes applying a release agent to the non-composite surface and bevel edges of each composite material. For example, the release agent is applied to the surface A2s and bevel edge A3s of composite material 42A, and the surface B2s and bevel edge B3s of composite material 42B.

[0162] Regarding the composition of the release agent, the first option is: a coating solution containing silicon oxide and magnesium oxide, wherein the mass ratio of silicon oxide to magnesium oxide is 3:1. The release agent of this embodiment can achieve a good isolation effect and ensure the subsequent separation of the two composite board plates. Using the release agent, the amount of release agent 43 applied on the surface to be composited and on the bevel of each composite material is 20 μmg / m 2 y is the ratio of the thickness of the composite billet produced in the composite billet preparation step to the thickness of the composite plate subsequently rolled. This ratio is also known as the composite billet rolling reduction ratio. The method for preparing the release agent and subsequent drying are the same as those described in the first embodiment of the composite billet preparation stage described above and will not be repeated here.

[0163] Regarding the composition of the release agent, a second optional solution is: a composition by weight of 25-35% silicon nitride + 5-10% thermosetting amino resin + 55-70% water. Compared to existing release agents, and even compared to the first embodiment of the release agent, the release agent of this embodiment not only achieves excellent isolation, ensuring the subsequent separation of the two composite board panels, but also has the chemical stability of the active ingredient, silicon nitride, and is resistant to high temperatures and thermal shocks. The thermosetting amino resin, used as a binder, cures at low temperatures, is non-toxic, and can achieve a strong bond with a small amount. Therefore, the release agent is generally inexpensive, easy to operate, and provides excellent isolation and adhesion. Using this release agent, the release agent 43 is applied to a thickness of 0.2-0.5 mm on the surface to be laminated and on the bevel edge of each composite material. The preparation method and subsequent drying of this release agent are the same as those described in the first embodiment of the composite blank preparation stage, and will not be repeated here.

[0164] Furthermore, in this embodiment, referring to FIG. 18 , the blank assembly process specifically includes: assembling the blank in a manner such that composite materials 42A and 42B form an intermediate layer, substrate 41A is stacked on top, substrate 41B is stacked on the bottom, and four seals 44 surround the four sides of the intermediate layer. Gas shielded welding is performed between the upper edge of seal 44 and substrate 41A, and between the lower edge of seal 44 and substrate 41B, to form a blank. In the intermediate layer, composite materials 42A and 42B are laid side by side in the X direction, with the hypotenuse A3s of composite material 42A and the hypotenuse B3s of composite material 42B parallel and in contact.

[0165] It can be understood that in the base blank obtained in the assembly process, the surface 41As of the substrate 41A and the surface A1s of the composite material 42A are facing each other and in contact as the surfaces to be composited, the surface 41Bs of the substrate 41B and the surface B1s of the composite material 42B are facing each other and in contact as the surfaces to be composited, and the surface A2s of the composite material 42A and the substrate 41B, the surface B2s of the composite material 42B and the substrate 41A, and the oblique edge A3s of the composite material 42A and the oblique edge B3s of the composite material 42B are coated with a release agent, and they are in contact with each other but will not be composited.

[0166] Further preferably, during the billet assembly process, after the base material 41A, composite material 42A, composite material 42B, and base material 41B have been stacked, and before the upper or lower edge of the seal 44 is welded to the base material, the stacked steel materials are placed under a four-column hydraulic press. The opposing surfaces of the two base materials (i.e., the upper surface of base material 41A and the lower surface of base material 41B) are pressurized to a pressure of 500 tons or more. This ensures closer contact between adjacent steel billets.

[0167] Preferably, during the assembly process, when performing gas shielded welding between the edge of seal 44 and the substrate, the welding current is 220-240A, the welding voltage is 28-32V, the welding speed is 300-360mm / min, and the interpass temperature is controlled at 140-160°C. Furthermore, prior to gas shielded welding, substrates 41A and 41B are preferably preheated and baked using a flame gun at a temperature of 150-250°C.

[0168] Furthermore, all four sides of the resulting base blank have grooves formed by the base material 41A, the sealing strip 44, and the base material 41B. Preferably, the depth of the grooves on all four sides of the base blank is set to be the same, as indicated by depth D in Figure 19, with a value ranging from 40 to 60 mm. By controlling this depth D, not only can weld cracking during rolling of the composite blank be effectively avoided, but also the formation of weld thermal cracks due to deep penetration during subsequent sealing, which can affect the sealing quality of the composite blank.

[0169] It is understood that the groove depth depends on the dimensional differences between the composite material and the substrate in the X and Y directions, as well as the thickness of the seal 44. For example, during the assembly process, the intermediate layer is centered relative to the substrate, and the distance between the two sides of the intermediate layer in the Y direction and the corresponding two sides of the substrate is equal, ranging from 45 to 75 mm. The corresponding groove depth D = (W1-W2-2T3) / 2. The distance between the two sides of the intermediate layer in the X direction and the corresponding two sides of the substrate is also equal, ranging from 45 to 75 mm. The corresponding groove depth D = (L1-(L21+L22-V)-2T3) / 2. T3 is the thickness of the seal, ranging from 10 to 15 mm.

[0170] Regarding the overall dimensions of the four seals 44, at both sides of the base in the X direction, the length L31 of the seals 44 is W2 to W2-2 mm, while at both sides of the base in the Y direction, the length L32 of the seals 44 is L21 + L22-V to L21 + L22-V-2 mm. The width W3 of the seals 44 is T2 to T2-2 mm, and the thickness T3 is 10 to 15 mm, as previously mentioned. Preferably, the width W3 and thickness T3 of the seals 44 are the same on all four sides of the base.

[0171] More preferably, as shown in FIG19 , both the upper and lower edges of the outer surface of the seal 44 are grooved, with a groove angle of 10-20° and a vertical groove depth P of 10-15 mm. The grooves not only avoid spot welding the inner side of the seal and the thermal effects of multiple welding passes on the substrate, but also facilitate subsequent welding of the grooves, ensuring a secure seal.

[0172] 19 , the groove angle K1 at the upper edge and the groove angle K2 at the lower edge of the outer surface of the seal 44 are respectively 10 to 20°, and the two can be the same or different.

[0173] Furthermore, a circular through-hole is formed in the seal on one side of the base blank. During the assembly process, a steel tube 46 having an outer diameter of r and a length of T3+2D to T3+2D+R is welded into the through-hole. The through-hole can be machined before the gas shielded welding of the seal 44 and base materials 41A and 41B, or it can be machined after the gas shielded welding is completed and the base blank is formed. All of these remain within the technical scope of this application.

[0174] Preferably, the aperture of the through hole is consistent with the outer diameter of the steel pipe 46, both being r.

[0175] More preferably, as shown in FIG20 , the through hole is formed on a seal 44 at one short side of the base blank, and the through hole is centered at a position 1 / 3 of the length and 1 / 2 of the width of the seal 44. Referring to FIG20 , the end surface of the steel tube 46 is flush with the inner surface of the seal 44. This ensures a vacuum effect.

[0176] It should be noted that, according to the example in the figure, the X direction is the length direction of the substrate, and the Y direction is the width direction of the substrate, that is, the two composite materials in the figure are arranged side by side between the two substrates in the length direction of the substrate; of course, in a variation, the X direction may also be the width direction of the substrate, and the Y direction may be the length direction of the substrate, that is, the two composite materials are arranged side by side between the two substrates in the width direction of the substrate.

[0177] Furthermore, as mentioned above, the shape and size of the blanks prepared in the composite blank preparation stage and the method of assembly affect the structural shape of the final stainless steel composite plate.

[0178] As shown in Figure 21, in this embodiment, the intermediate layer in the billet assembly process is composed of composite material 42A and composite material 42B arranged side by side, so that the composite billet based on this embodiment, after the subsequent composite billet rolling stage and plate finished product stage, the two stainless steel composite plates prepared are both composed of the composite layer covering part of the upper surface of the base material layer but not the entire upper surface.

[0179] For example, the resulting stainless steel clad plate 40A has a carbon steel substrate layer 41A and a stainless steel clad layer 42A, each obtained by rolling the aforementioned substrate 41A and clad layer 42A. Therefore, the original substrate 41A and clad layer 42A retain their designations. Three sides of clad layer 42A are flush with the three sides of substrate layer 41A, while the other side of clad layer 42A lies within the top surface of substrate layer 41A. Thus, clad layer 42A covers only one end of substrate layer 41A, leaving the other end exposed.

[0180] For example, the resulting stainless steel clad plate 40B has a carbon steel base layer 41B and a stainless steel clad layer 42B, each obtained by rolling the previously described base layer 41B and clad material 42B. Therefore, the original base layer 41B and clad material 42B are referenced. Three sides of the clad layer 42B are flush with the three sides of the base layer 41B; the other side of the clad layer 42B is located within the upper surface of the base layer 41B. Thus, the clad layer 42B only covers one end of the base layer 41B, leaving the other end exposed.

[0181] The beneficial effects of the composite plate prepared from the composite blank of this embodiment also need to be understood in conjunction with the current status of the use of existing stainless steel composite plates in bridge engineering. Specifically, for stainless steel composite plates used in bridge structures, they need to be docked with steel plates used in bridge structures during processing and use in downstream structural plants. At this docking position, the base material layer of the stainless steel composite plate and the steel plate used in the bridge structure are made of the same material, and the welding strength is easy to ensure. However, the stainless steel composite layer and the steel plate used in the bridge structure are made of different materials, which makes welding difficult and has poor strength, which has a certain impact on the safety of the overall structural parts. The composite plate prepared by the composite blank of this embodiment has a composite structure composed of carbon steel and stainless steel at one end (for example, the left end of the composite plates 40A and 40B in Figure 21). This end can be like the existing composite plate, with both the corrosion resistance of the composite layer and the good mechanical properties of the base material layer; and the other end is purely a carbon steel plate (for example, the right end of the composite plates 40A and 40B in Figure 21). In this way, the stainless steel composite plate avoids the existing dissimilar welding problems during use, has strong firmness during use, low production difficulty and cost in later use, and high construction efficiency.

[0182] Further preferably, the side edge of the composite layer 42A "located inside the upper surface of the base layer 41A" is configured as a beveled edge, which forms an obtuse angle with the upper surface of the composite layer 42A; similarly, the side edge of the composite layer 42B "located inside the upper surface of the base layer 41B" is configured as a beveled edge, which forms an obtuse angle with the upper surface of the composite layer 42B. In this regard, when existing composite panels are used in bridge engineering, in order to avoid a step (height difference) between the edge of the stainless steel composite layer and the steel plate used for the bridge structure, an additional stainless steel plate is required for transition. This not only increases the material cost, but also requires that the additional stainless steel plate be welded to both the composite layer of the stainless steel composite panel and the steel plate used for the bridge structure, greatly increasing the welding workload and affecting construction efficiency. In contrast, in this embodiment, there is no step between the edge of the stainless steel composite layer and the steel plate used for the bridge structure, but rather a beveled transition, eliminating the need for an additional transition plate. This results in high construction efficiency, low workload, and high structural strength.

[0183] In summary, a single-sided stainless steel clad plate is provided, which is manufactured from the clad blank prepared in this embodiment through a clad blank rolling stage and a plate finishing stage. The clad plate has a total thickness of 5 to 55 mm, a base material layer thickness of 4 to 45 mm, and a clad material layer thickness of 1 to 10 mm, and has one end in the X direction covered and the other end uncovered.

[0184] The above describes in detail the various steps involved in preparing the composite blanks according to this embodiment. Among the various experimental examples provided below, Experimental Examples 10-12 employ this embodiment to prepare composite blanks, which are then used to produce stainless steel composite plates. Table 4 shows some parameters of the composite blanks used in these examples. The parameters indicated by the symbols are described above.

[0185] Table 4

[0186] <Fifth Implementation Method of Composite Billet Preparation Stage>

[0187] Figures 22 to 26 illustrate a fifth embodiment of the composite blank preparation stage. This embodiment differs from the first embodiment of the composite blank preparation stage described above in the blank preparation process, the release agent coating process, and the blank assembly process. The welding, vacuuming, and sealing processes remain the same as those of the first embodiment. Only the differing processes are described in detail below; the remaining processes can be understood in conjunction with the accompanying drawings and the first embodiment of the composite blank preparation stage described above and will not be further elaborated.

[0188] In this embodiment, referring to FIG22 , the blank preparation process specifically includes:

[0189] Two carbon steel billets having an X-axis dimension L1 and a Y-axis dimension W1 are prepared as two substrates, which are distinguished as substrate 51A and substrate 51B in FIG. 22 . Furthermore, the thicknesses of substrates 51A and 51B can be the same or different.

[0190] The surface to be composited of each substrate is ground and polished, for example, surface 51As of substrate 51A and surface 51Bs of substrate 51B, to remove surface oxide scale and expose metallic luster. After the surface grinding treatment, the roughness Ra of the surface to be composited is less than 5 μm.

[0191] A stainless steel billet having an X-direction dimension L22, a Y-direction dimension W2, and a thickness T2 is prepared as a composite material, such as composite material 52A in FIG. 22 . One side A3s of composite material 52A in the X-direction is a hypotenuse of width V1, and the other side A4s in the X-direction is a hypotenuse of width V2.

[0192] A stainless steel billet having an X-direction dimension of L21, a Y-direction dimension of W2, and a thickness of T2 is prepared as another composite material, such as composite material 52B in FIG. 22 ; one side B3s of composite material 52B in the X-direction is a hypotenuse having a width of V1;

[0193] A stainless steel billet having an X-direction dimension of L23, a Y-direction dimension of W2, and a thickness of T2 is prepared as another composite material, such as composite material 52C in FIG. 22 ; a side C3s of composite material 52C in the X-direction is a hypotenuse having a width of V2;

[0194] A smaller surface of each composite material in the thickness direction constitutes a non-composite surface, such as surface A2s of composite material 52A, surface B2s of composite material 52B, and surface C2s of composite material 52C, while another larger surface constitutes a surface to be composited, such as surface A1s of composite material 52A, surface B1s of composite material 52B, and surface C1s of composite material 52C. The surface to be composited of each composite material is ground and polished to remove surface oxide scale and reveal a metallic luster. After this surface grinding process, the roughness Ra of the surface to be composited is less than 5 μm.

[0195] Based on the above dimensions, that is, the dimensions of composite materials 52A, 52B, and 52C in the Y direction are the same and the thickness is also the same; and the dimensions of composite materials 52A, 52B, and 52C in the X direction can be all the same (i.e., L21=L23=L22), or they can be the same (i.e., L21=L23≠L22, or L21≠L23=L22, or L21=L22≠L23), or they can be completely different (i.e., L21≠L22≠L23).

[0196] The widths V1 and V2 refer to the span of the hypotenuse in the X-direction. Precisely because of the hypotenuse, one of the two surfaces in the thickness direction of each composite material is the larger surface, while the other is the smaller surface. Side A3s of composite material 52A and side B3s of composite material 52B both have hypotenuses of width V1. Thus, as described in the subsequent assembly process, side A3s and side B3s are parallel and connected. Similarly, side A4s of composite material 52A and side C3s of composite material 52C both have hypotenuses of width V2. Thus, as described in the subsequent assembly process, side A3s and side B3s are parallel and connected.

[0197] Preferably, both the side edge A3s and the side edge A4s of the composite material 52A form an obtuse angle with the surface A2s of the composite material 52A not to be composited.

[0198] Furthermore, L1 ≥ 2500 mm, W2 ≥ 1600 mm, and T1 ≥ 60 mm. Regarding the dimensional relationship between composite materials 52A, 52B, and 52C and substrates 51A and 51B, L21 + L22 + L23 - V1 - V2 < L1, and W2 < W1. More preferably, W1 = W2 + 90 to 150 mm, and L1 = L21 + L22 + L23 - V1 - V2 + 90 to 150 mm.

[0199] Preferably, surface 51As of substrate 51A and surface 51Bs of substrate 51B are ground and polished using a grinding wheel, belt sander, or milling machine to remove surface oxide scale and reveal a metallic luster. Surface A1s of composite material 52A, surface B1s of composite material 52B, and surface C1s of composite material 52C are ground and polished using a wire wheel to remove surface oxide scale and reveal a metallic luster.

[0200] Here, only the surface grinding treatment of the to-be-combined surface of each substrate and each composite is described. However, it should be noted that the surface grinding treatment of other surfaces of each substrate and composite can be further performed. Although such additional grinding treatment of other surfaces is not necessary to achieve the technical effect of the present invention, it may be more preferable.

[0201] Furthermore, in this embodiment, the release agent coating step specifically includes applying a release agent to the non-composite surface and bevel edges of each composite material. Specifically, for example, a release agent is applied to surface A2s, bevel edges A3s, and bevel edges A4s of composite material 52A, surface B2s and bevel edges B3s of composite material 52B, and surface C2s and bevel edges C3s of composite material 52C.

[0202] Regarding the composition of the release agent, the first option is: a coating solution containing silicon oxide and magnesium oxide, wherein the mass ratio of silicon oxide to magnesium oxide is 3:1. The release agent of this embodiment can achieve a good isolation effect and ensure the subsequent separation of the two composite board plates. Using the release agent, the amount of release agent 53 applied on the surface to be composited and on the bevel of each composite material is 20 μmg / m 2 y is the ratio of the thickness of the composite billet produced in the composite billet preparation step to the thickness of the composite plate subsequently rolled. This ratio is also known as the composite billet rolling reduction ratio. The method for preparing the release agent and subsequent drying are the same as those described in the first embodiment of the composite billet preparation stage described above and will not be repeated here.

[0203] Regarding the composition of the release agent, a second optional solution is: a composition by weight of 25-35% silicon nitride + 5-10% thermosetting amino resin + 55-70% water. Compared to existing release agents, and even compared to the first embodiment of the release agent, the release agent of this embodiment not only achieves excellent isolation, ensuring the subsequent separation of the two composite board panels, but also has the strong chemical stability of the active ingredient, silicon nitride, and resistance to high temperatures and thermal shocks. The thermosetting amino resin, used as a binder, cures at low temperatures, is non-toxic, and can achieve a strong bonding effect with a small amount. Therefore, the overall price is low, the operation is simple, and the isolation and adhesion effects are excellent. Using this release agent, the release agent 53 is applied to a thickness of 0.2-0.5 mm on the surface to be composited and on the bevel edge of each composite material. The preparation method and subsequent drying of this release agent are the same as those described in the first embodiment of the composite blank preparation stage described above and will not be repeated here.

[0204] Furthermore, in this embodiment, referring to FIG. 23 , the blank assembly process specifically includes: assembling the blank in a manner such that composite materials 52A, 52B, and 52C form an intermediate layer, substrate 51A is stacked on top, substrate 51B is stacked on the bottom, and four seals 54 surround the four sides of the intermediate layer. Gas shielded welding is performed between the upper edge of seal 54 and substrate 51A, and between the lower edge of seal 54 and substrate 51B, to form a blank. In the intermediate layer, composite materials 52B, 52A, and 52C are laid out in parallel in the X direction, with the hypotenuse A3s of composite material 52A and the hypotenuse B3s of composite material 52B parallel to each other, and the hypotenuse A4s of composite material 52A and the hypotenuse C3s of composite material 52C parallel to each other.

[0205] It can be understood that in the base blank obtained in the blank assembly process, the surface 51As of the substrate 51A and the surface A1s of the composite 52A are facing each other and in contact as the surfaces to be composited, the surface 51Bs of the substrate 51B and the surface B1s of the composite 52B are facing each other and in contact as the surfaces to be composited, and the surface 51Bs of the substrate 51B and the surface C1s of the composite 52C are also facing each other and in contact as the surfaces to be composited. The surface A2s of the composite 52A and the substrate 51B, the surface B2s of the composite 52B and the substrate 51A, the surface C2s of the composite 52C and the substrate 51A, the oblique edge A3s of the composite 52A and the oblique edge B3s of the composite 52B, and the oblique edge A4s of the composite 52A and the oblique edge C3s of the composite 52C are all coated with a release agent, and are in contact with each other but will not be composited.

[0206] Further preferably, during the billet assembly process, after the base material 51A, composite material 52B, composite material 52A, composite material 52C, and base material 51B are stacked, and before the upper or lower edge of the seal 54 is welded to the base material, the stacked steel materials are placed under a four-column hydraulic press, and the opposing surfaces of the two base materials (i.e., the upper surface of base material 51A and the lower surface of base material 51B) are pressurized to a pressure of 500 tons or more. This ensures closer contact between adjacent steel billets.

[0207] Preferably, during the assembly process, when performing gas shielded welding between the edge of seal 54 and the substrate, the welding current is 220-240A, the welding voltage is 28-32V, the welding speed is 300-360mm / min, and the interpass temperature is controlled at 140-160°C. Furthermore, prior to gas shielded welding, substrates 51A and 51B are preferably preheated and baked using a flame gun at a temperature of 150-250°C.

[0208] Furthermore, all four sides of the resulting base blank have grooves formed by the base material 51A, the sealing strip 54, and the base material 51B. Preferably, the depth of the grooves on all four sides of the base blank is set to be the same, as indicated by depth D in Figure 24, with a value ranging from 40 to 60 mm. By controlling this depth D, not only can weld cracking during rolling of the composite blank be effectively avoided, but also the formation of weld thermal cracks due to deep penetration during subsequent sealing, which can affect the sealing quality of the composite blank.

[0209] It is understood that the groove depth depends on the dimensional differences between the composite material and the substrate in the X and Y directions, as well as the thickness of the seal 54. For example, during the assembly process, the intermediate layer is centered relative to the substrate, and the distance between the two sides of the intermediate layer in the Y direction and the corresponding two sides of the substrate is equal, ranging from 45 to 75 mm. The corresponding groove depth D = (W1 - W2 - 2T3) / 2. The distance between the two sides of the intermediate layer in the X direction and the corresponding two sides of the substrate is also equal, ranging from 45 to 75 mm. The corresponding groove depth D = (L1 - (L21 + L22 + L23 - V1 - V2) - 2T3) / 2. T3 is the thickness of the seal, ranging from 10 to 15 mm.

[0210] Regarding the overall dimensions of the four seals 54, at both sides of the base in the X direction, the length L31 of the seals 54 is W2 to W2-2 mm, while at both sides of the base in the Y direction, the length L32 of the seals 54 is L21+L22+L23-V1-V2 to L21+L22+L23-V1-V2-2 mm. The width W3 of the seals 54 is T2 to T2-2 mm, and the thickness T3 is 10 to 15 mm, as previously described. Preferably, the width W3 and thickness T3 of the seals 54 are the same on all four sides of the base.

[0211] More preferably, as shown in FIG24 , both the upper and lower edges of the outer surface of the seal 54 are grooved, with a groove angle of 10-20° and a vertical groove depth P of 10-15 mm. The grooves not only avoid spot welding the inner side of the seal and the thermal effects of multiple welding passes on the substrate, but also facilitate subsequent welding of the grooves, ensuring a secure seal.

[0212] 24 , the groove angle K1 at the upper edge and the groove angle K2 at the lower edge of the outer surface of the seal 54 are respectively 10 to 20°, and the two can be the same or different.

[0213] Furthermore, a circular through-hole is formed in the seal on one side of the base blank. During the assembly process, a steel tube 56 having an outer diameter of r and a length of T3+2D to T3+2D+R is welded into the through-hole. The through-hole can be machined before the gas shielded welding of the seal 54 and the base materials 51A and 51B, or it can be machined after the gas shielded welding is completed and the base blank is formed. All of these remain within the technical scope of this application.

[0214] Preferably, the aperture of the through hole is consistent with the outer diameter of the steel pipe 56, both being r.

[0215] More preferably, as shown in FIG25 , the through hole is formed on a seal 54 at one short side of the base blank, and the through hole is centered at a position 1 / 3 of the length and 1 / 2 of the width of the seal 54. Referring to FIG24 , the end surface of the steel tube 56 is flush with the inner surface of the seal 54. This ensures a vacuum effect.

[0216] It should be noted that, according to the example in the figure, the X direction is the length direction of the substrate, and the Y direction is the width direction of the substrate, that is, the three composite materials in the figure are arranged side by side between the two substrates in the length direction of the substrate; of course, in a variation, the X direction may also be the width direction of the substrate, and the Y direction may be the length direction of the substrate, that is, the three composite materials are arranged side by side between the two substrates in the width direction of the substrate.

[0217] Furthermore, as mentioned above, the shape and size of the blanks prepared in the composite blank preparation stage and the method of assembly affect the structural shape of the final stainless steel composite plate.

[0218] As shown in Figure 26, in this embodiment, the intermediate layer in the billet assembly process is composite material 52B, composite material 52A and composite material 52C arranged side by side in sequence, so that the composite billet based on this embodiment, after the subsequent composite billet rolling stage and the plate finished product stage, three stainless steel composite plates are prepared, of which at least two are composite layers covering part of the upper surface of the substrate layer but not the entire upper surface.

[0219] For example, as shown in Figure 26 , the resulting stainless steel clad plate 50A has a carbon steel substrate layer 51A and a stainless steel clad layer 52A, each of which is obtained by rolling the previously described substrate 51A and clad layer 52A. Therefore, the original numbers of the substrate 51A and clad layer 52A are retained. The two sides of the composite layer 52A in the Y direction are flush with the corresponding two sides of the substrate layer 51A; while the two sides of the composite layer 52A in the X direction are both located within the upper surface of the substrate layer 51A. Thus, the composite layer 52A only covers the central region of the substrate layer 51A, leaving the two ends of the substrate layer 51A in the X direction exposed. This type of clad plate can be referred to as a central stainless steel clad plate. In this way, the middle part of the stainless steel composite plate is a composite structure composed of a carbon steel substrate layer 51A and a stainless steel composite layer 52A. Like the existing composite plate, it can have both the corrosion resistance of the composite layer 52A and the good mechanical properties of the substrate layer 51A; while the two ends of the stainless steel composite plate are purely carbon steel substrate layers 51A, which are directly integrally formed with the composite structure. The carbon steel substrate layers 51A at these two ends can be directly used in the project without welding. In this way, the stainless steel composite plate avoids the existing dissimilar welding problems during use, has strong firmness, low production difficulty, low cost and high construction efficiency.

[0220] Furthermore, both sides of the composite layer 52A in the X direction are configured as beveled edges, forming obtuse angles with the upper surface of the composite layer 52A. In this regard, when existing composite panels are used in bridge construction, an additional stainless steel plate is required to avoid a step (height difference) between the edge of the stainless steel composite layer and the steel plate used for the bridge structure. This not only increases material costs, but also requires welding the additional stainless steel plate to both the composite layer of the stainless steel composite panel and the steel plate used for the bridge structure, significantly increasing the welding workload and affecting construction efficiency. However, in this embodiment, there is no step between the edge of the stainless steel composite layer and the steel plate used for the bridge structure, but rather an inclined transition, eliminating the need for an additional transition plate. This results in high construction efficiency, minimal workload, and high structural strength.

[0221] For example, as shown in FIG. 26 , the stainless steel composite plates 50B and 50C are obtained by rolling the aforementioned composite materials 52B and 52C, respectively, and thus retain the designations of the composite materials 52B and 52C. The original substrate 51B is rolled and cut into two parts, one of which becomes the substrate layer 51Ba of the composite plate 50B, and the other becomes the substrate layer 51Bc of the composite plate 50C.

[0222] In the figure, in the stainless steel clad plate 50B, three sides of the composite layer 52B are flush with the three sides of the substrate layer 51Ba; while the other side of the composite layer 52B is located inside the upper surface of the substrate layer 51Ba. In this way, the composite layer 52B only covers one end of the substrate layer 51Ba (e.g., the left end in FIG. 26 ), leaving the other end of the substrate layer 51Ba exposed (e.g., the right end in FIG. 26 ). Similarly, in the stainless steel clad plate 50C, three sides of the composite layer 52C are flush with the three sides of the substrate layer 51Bc; while the other side of the composite layer 52C is located inside the upper surface of the substrate layer 51Bc. In this way, the composite layer 52C only covers one end of the substrate layer 51Bc (e.g., the right end in FIG. 26 ), leaving the other end of the substrate layer 51Bc exposed (e.g., the left end in FIG. 26 ). In this way, the composite plates 50B and 50C have a composite structure composed of carbon steel and stainless steel at one end. This end can be like the existing composite plates, combining the corrosion resistance of the composite layer with the good mechanical properties of the base material layer; while the other end is purely a carbon steel plate. In this way, the stainless steel composite plate avoids the existing dissimilar welding problems during use, has strong firmness during use, and has low production difficulty, low cost and high construction efficiency in later use.

[0223] Furthermore, the side edge of composite layer 52B located "inward of the upper surface of base layer 51Ba" is configured as a bevel, forming an obtuse angle with the upper surface of composite layer 52B. Similarly, the side edge of composite layer 52C located "inward of the upper surface of base layer 51Bc" is configured as a bevel, forming an obtuse angle with the upper surface of composite layer 52C. This creates a beveled transition between the edge of the stainless steel composite layer and the bridge structural steel plate, eliminating the need for an additional transition plate. This improves construction efficiency, reduces workload, and enhances structural strength.

[0224] It is understood that when the original substrate 51B is rolled and cut into two parts, depending on the cutting position, one composite panel can be a fully covered composite panel with the composite and substrate layers of equal length and width (e.g., composite panel 10B shown in FIG6 ), while the other composite panel can be a composite panel with one end of the substrate layer covered by the composite layer and the other end uncovered. Of course, other cutting methods can also be used as needed.

[0225] It can be seen that this embodiment can simultaneously obtain at least two different types of composite panels, which has better industrial value.

[0226] In addition, the fourth and fifth embodiments described above respectively introduce an assembly method of two and three composite materials arranged side by side, but the present invention is not limited thereto, and an assembly method of many composite materials arranged side by side can also be used.

[0227] In summary, a single-sided stainless steel composite plate is provided, which is made from the composite blank prepared in this embodiment through the composite blank rolling stage and the plate finished product stage. The total thickness of the composite plate is 5 to 55 mm, the thickness of the base material layer is 4 to 45 mm, the thickness of the composite material layer is 1 to 10 mm, and the middle area in the X direction is covered and the two ends are not covered. Of course, a single-sided stainless steel composite plate can also be provided at the same time, which is made from the composite blank prepared in this embodiment through the composite blank rolling stage and the plate finished product stage. The total thickness of the composite plate is 5 to 55 mm, the thickness of the base material layer is 4 to 45 mm, the thickness of the composite material layer is 1 to 10 mm, and one end in the X direction is covered and the other end is not covered.

[0228] The above describes in detail the various steps involved in preparing the composite blanks according to this embodiment. Among the various experimental examples provided below, Experimental Examples 13 to 15 employ this embodiment to prepare composite blanks, which are then used to produce stainless steel composite plates. Table 5 shows some parameters of the composite blanks used in these examples. The parameters indicated by the symbols are described above.

[0229] Table 5

[0230] The above describes the five implementation methods of the composite billet preparation stage. The following describes the specific implementation methods of the composite billet rolling stage and the plate finishing stage in detail. It should be noted that the specific implementation methods of the composite billet rolling stage and the plate finishing stage described below are applicable to any of the five implementation methods of the composite billet preparation stage described above. In other words, composite billets prepared using any of the five implementation methods of the composite billet preparation stage described above can be produced into single-sided stainless steel composite plates using the specific implementation methods of the composite billet rolling stage and the plate finishing stage described below.

[0231] The composite billet rolling stage involves heating, rolling, and cooling the composite billet produced in the composite billet preparation stage to produce composite slabs. Each process is described in detail below.

[0232] First, regarding the heating process, the composite billet is heated in a heating furnace to prepare in advance for the subsequent rolling process, which can be specifically implemented using techniques known in the art.

[0233] The present application provides a preferred embodiment of the heating process, specifically: the composite blank is heated in a heating furnace according to a five-stage process of preheating, first heating, second heating, third heating and soaking. The preheating temperature is ≤850°C, the first heating temperature is 1080±30°C, the second heating temperature is 1160±30°C, the third heating temperature is 1220±20°C, the soaking temperature is 1190±20°C, and the residence time of the third heating is (0.25-0.35)×t min / mm, where t is the thickness of the composite blank. The residence time of the soaking is 15min-30min. In this way, the middle layer of the composite blank is a stainless steel composite material, and the upper and lower layers are carbon steel substrates. The thermal conductivity and expansion coefficient of the two materials are quite different, and large stress will be generated during the heating process. The heating process of this embodiment can better control the heating rate of the composite blank in each section, ensure uniform heating, and thus avoid the risks of cracking, air leakage, etc., so that the final composite plate has an excellent bonding interface.

[0234] Furthermore, in the rolling process, the composite billet exiting the heating furnace is rolled to produce a large composite plate.

[0235] In one embodiment, during the entire rolling process, the first n passes are transversely rolled, and the n+1th pass and thereafter are longitudinally rolled, and the first pass has a rolling reduction of ≥25 mm and a rolling temperature ≥1060° C. The width of the billet obtained by the nth pass is Wt+0 to 40 mm, Wt is the target width of the composite plate, and the rolling temperature of the nth pass is ≥1030° C. Between the nth pass and the n+1th pass and between the n+2th pass and the n+3th pass, the billet is water-cooled once in six sets of headers, and the cooling water volume of the upper header of each set of headers is 120 to 180 m 3 / h, cooling water volume of lower header: 160~220m 3 / h, and the roller speed is 0.8~1.2m / s; the rolling reduction from the n+1th to the n+3th pass is ≥40mm, especially the rolling reduction of the n+2th pass is preferably ≥42mm, and the rolling temperature of the n+1th pass is ≥950℃; when it comes to the mth pass, the rolling temperature is ≥900℃, and the billet is rolled to a thickness of 2.5~3.5 times the target thickness of the composite plate; then water cooling is carried out until the surface temperature of the billet drops below 840℃; then the second stage rolling is carried out until the billet thickness is the target thickness of the composite plate, completing the entire rolling process, the rolling temperature of the first pass of the second stage rolling is 810℃~840℃, and the rolling temperature of the last pass is 780~810℃.

[0236] In this way, the rolling process of this embodiment can, on the one hand, ensure the deformation penetration effect of the core, facilitate the bonding of the composite material and the substrate, and improve the interface bonding rate and bonding strength of the substrate layer and the composite material layer of the final composite plate; on the other hand, ensure the relevant mechanical properties, corrosion resistance and low-temperature impact toughness of the large composite plate, and avoid performance degradation due to the composite of the substrate and the composite material.

[0237] The next cooling step involves cooling the warm composite plate obtained from the rolling process. Specifically, after the aforementioned "final rolling pass temperature of 780-810°C," the resulting composite plate leaves the rolling mill at a temperature of approximately 780°C, after which it is cooled to room temperature. This cooling can be achieved using known and feasible cooling techniques. In a preferred embodiment of the present invention, a cooling step including intermittent cooling is provided, which can provide superior benefits compared to existing cooling techniques.

[0238] Specifically, in this preferred embodiment, the cooling process includes: after the composite plate slab leaves the rolling mill, it enters an ultra-rapid cooling system for intermittent cooling. The ultra-rapid cooling system comprises 24 sets of cooling manifolds arranged at 1m intervals along the roller table. During the intermittent cooling, each set of cooling manifolds has a cooling distance of 1m. As the composite plate slab passes through the ultra-rapid cooling system, the opening and closing states of all 24 sets of cooling manifolds are controlled by opening N sets of cooling manifolds and then closing M sets of cooling manifolds. The cooling water pressure is 0.15-0.30MPa, the cooling rate is 3-15°C / s, and the final cooling temperature is 380-590°C. N is 2, 3, or 4, and M is 2, 3, or 4.

[0239] This embodiment adopts the intermittent cooling described above. When the large composite plate passes through the ultra-fast cooling system, it travels in alternating open cooling manifolds and closed cooling manifolds. In this way, each part of the large composite plate will cool, turn red, cool, turn red... and repeat this cycle until the large composite plate leaves the ultra-fast cooling system. In this way, in the cooling-turn red cycle of the large composite plate, the carbon steel substrate continuously undergoes phase change and self-tempering effects, and the phase change reaction gradually penetrates into the core until the entire carbon steel substrate completes the phase change. This intermittent cooling process is different from conventional reciprocating cooling. The turn red and self-tempering of reciprocating cooling occur after the surface or near-surface layer has completed the phase change. The temperature difference or cooling rate between the surface and the core is large, and the microstructure and mechanical properties are also different. The difference is large, while the intermittent cooling process of this embodiment is that, at the same time, some parts of the composite plate are in a cooling state, and some parts are in red-hot / self-tempering, and each part of the composite plate is alternately cooled and red-hot / self-tempering over time, so that the differences in temperature, cooling rate, organization, performance, etc. between the surface and core of the composite plate are small. For example, the Vickers hardness difference of the base material layer of the final composite plate in the thickness direction is ≤10, the strength difference between the head, middle and tail is ≤40MPa, and the strength difference of the whole plate is ≤40MPa; at the same time, the plate shape of the composite plate can be further improved through intermittent cooling, that is, the flatness is low, even if straightening is not performed after cooling and the plate is directly cooled on the cooling bed, an excellent plate shape can be obtained.

[0240] Further preferably, in the intermittent cooling:

[0241] The thickness of the composite plate is less than 54 mm, for example, when the thickness is 10 to 54 mm, the roller speed of the ultra-fast cooling system is 0.4 to 0.8 m / s, and the composite plate passes through the ultra-fast cooling system once and then leaves the ultra-fast cooling system; preferably, the preferred control scheme of the 24 groups of cooling manifolds is, for example, the 1st to 4th groups of cooling manifolds are turned on, the 5th to 6th groups of cooling manifolds are not turned on, the 7th to 8th groups of cooling manifolds are turned on, the 9th to 10th groups of cooling manifolds are not turned on, the 11th to 12th groups of cooling manifolds are turned on, the 13th to 14th groups of cooling manifolds are not turned on, the 15th to 16th groups of cooling manifolds are turned on, the 17th to 18th groups of cooling manifolds are not turned on, the 19th to 20th groups of cooling manifolds are turned on, the 21st to 22nd groups of cooling manifolds are not turned on, and the 23rd to 24th groups of cooling manifolds are turned on;

[0242] The thickness of the composite plate is greater than 54 mm and less than 70 mm, the roller speed of the ultra-fast cooling system is greater than 0.2 m / s and less than 0.6 m / s, the composite plate passes through the ultra-fast cooling system once, and then leaves the ultra-fast cooling system; the thickness of the composite plate is greater than or equal to 70 mm, the roller speed of the ultra-fast cooling system is 0.4-0.9 m / s, the composite plate first enters the ultra-fast cooling system entrance in the forward direction, and when its head reaches the 24th group of cooling manifolds, the roller reverses, and the composite plate passes through the ultra-fast cooling system in the reverse direction and leaves the ultra-fast cooling system entrance. Among them, when the thickness of the large composite plate is greater than 54 mm, preferably, the preferred control scheme for the 24 groups of cooling manifolds is, for example, the 1st to 4th groups of cooling manifolds are turned on, the 5th to 8th groups of cooling manifolds are not turned on, the 9th to 12th groups of cooling manifolds are turned on, the 13th to 16th groups of cooling manifolds are not turned on, the 17th to 20th groups of cooling manifolds are turned on, the 21st to 22nd groups of cooling manifolds are not turned on, and the 23rd to 24th groups of cooling manifolds are turned on.

[0243] In this way, through intermittent cooling, it is also possible to achieve plate shape control and uniformity control for large composite plates with large thickness (for example, thickness >54mm and <70mm) or even extremely large thickness (for example, thickness ≥70mm), overcoming the production difficulties of existing thick stainless steel composite plates.

[0244] Furthermore, in one embodiment, the cooling process specifically includes: after leaving the ultra-fast cooling system, the composite plate slab is directly placed on a cooling bed for air cooling until it reaches room temperature. As a more preferred alternative embodiment, after leaving the ultra-fast cooling system, the composite plate slab is not directly placed on a cooling bed, but can be first pile-cooled. For example, the cooling process specifically includes: after leaving the ultra-fast cooling system, the composite plate slab is placed on a cooling bed at a temperature of T f -150℃~T f The stack cooling is carried out between two steel plates at +150℃, and the stack cooling time is 0.4min / mm×t0±5min, where t0 is the thickness of the composite plate. After the stack cooling is completed, the cooling bed on the composite plate is naturally cooled to room temperature; wherein, T f =550+30Si-20Mn+15Cr-15Ni+10Mo, where the element symbols in the formula represent 100 times the mass percentage of each element in the base material. In this way, through stack cooling, especially controlling the temperature of the stack-cooled steel plate, the temperature of the composite plate can be uniformed across its thickness while maintaining the performance of the composite plate. This avoids the situation where the base material temperature is low and the composite material temperature is high, ensuring that the expansion of the base material and the composite material is similar, thereby maintaining the shape of the composite plate.

[0245] The composite billet rolling stage is described in detail above. Next, the preparation method of the present invention further includes a plate finishing stage. As mentioned above, the plate finishing stage includes a plate separation process and a flattening process.

[0246] Specifically, during the panel separation process, a large composite panel, after air cooling to room temperature, is cut along its four sides using a plasma cutter to remove any portions other than the seal, separating the large composite panel into two upper and lower composite panel panels. These two composite panel panels can then be flattened to produce two single-sided stainless steel composite panels. Of course, these upper and lower composite panel panels can also be further cut to produce more single-sided stainless steel composite panels, such as the three finished stainless steel composite panels described in the fifth embodiment of the composite blank preparation stage described above, see stainless steel composite panels 50A, 50B, and 50C in FIG. 26 .

[0247] The "portion outside the seal" refers to the edge of the composite plate, which is formed from the seal and filler layer in the composite billet after the previous rolling steps. This portion is removed to expose the stainless steel composite layer. Without this connecting portion, the composite plate automatically separates into two smaller composite plates.

[0248] Next, the flattening process specifically includes: placing the composite material layer of the single-sided composite board obtained in the panel separation process on a flattening machine with the composite material layer facing upwards for flattening, wherein: when flattening horizontally, the flattening force of the flattening machine is controlled to be F1 = ν × a × b × c 横 ×σ 横 / (d×(ν-c 横 / a)); When flattening longitudinally, control the flattening force F2 = a × b × c 纵 ×σ 纵 / (d+c 纵 ); where a is the width of the composite board, in mm, b is the thickness of the composite board, in mm, c 横 It is the unevenness per meter of the composite board in the horizontal direction, in mm, c 纵 is the unevenness per meter of the composite board in the longitudinal direction, in mm, d is the working distance of the flattening machine, σ 横 is the tensile yield strength of the composite plate in the transverse direction, σ 纵 is the tensile yield strength of the composite plate in the longitudinal direction, and ν is the Poisson's ratio. Thus, by adjusting the flattening force and flattening direction, a better plate shape can be further ensured.

[0249] After the final flattening process, the finished single-sided stainless steel composite panel is obtained.

[0250] Furthermore, an embodiment of the present invention also provides a single-sided stainless steel composite plate, which is prepared using the preparation method described above, and includes a substrate layer transformed from the substrate and a composite layer transformed from the composite material.

[0251] Preferably, the composite material / the composite material layer is preferably austenitic stainless steel, whose chemical composition, in mass percentage, is: C ≤ 0.15%, Si ≤ 1.00%, Mn ≤ 2.00%, P ≤ 0.045%, S ≤ 0.030%, Ni: 6.0-22.0%, Cr: 16.0-26.0%, Mo ≤ 3.0%, and the balance is Fe and unavoidable impurities.

[0252] As a preferred embodiment, the chemical composition of the substrate / the substrate layer is, in percentage by mass: C: 0.03-0.16%, Si: 0.11-0.29%, Mn: 1.31-1.54%, P≤0.018%, S≤0.0030%, Cr: 0.06-0.29%, Nb: 0.011-0.034%, Ti: 0.011-0.019%, Al: 0.030-0.040%, and the rest is Fe and unavoidable impurities.

[0253] Further preferably, the chemical composition of the substrate / the substrate layer is, in mass percentage, as follows: C: 0.08-0.12%, Si: 0.16-0.24%, Mn: 1.36-1.44%, P≤0.015%, S≤0.0025%, Cr: 0.11-0.19%, Ni: 0.06-0.14%, Nb: 0.016-0.024%, Ti: 0.011-0.019%, Al: 0.030-0.040%, and the rest is Fe and unavoidable impurities.

[0254] More preferably, the chemical composition of the substrate / the substrate layer is, in mass percentage, as follows: C: 0.05-0.09%, Si: 0.14-0.22%, Mn: 1.41-1.49%, P≤0.012%, S≤0.0020%, Cr: 0.16-0.24%, Ni: 0.11-0.19%, Mo: 0.11-0.19%, Nb: 0.021-0.029%, Ti: 0.011-0.019%, Al: 0.030-0.040%, and the rest is Fe and unavoidable impurities.

[0255] Another preferred embodiment is that the chemical composition of the substrate / the substrate layer is, in mass percentage, as follows: C: 0.03-0.07%, Si: 0.11-0.19%, Mn: 1.46-1.54%, P≤0.010%, S≤0.0015%, Cr: 0.21-0.29%, Ni: 0.16-0.24%, Cu: 0.16-0.24%, Mo: 0.16-0.24%, Nb: 0.026-0.034%, Ti: 0.011-0.019%, Al: 0.030-0.040%, and the rest is Fe and unavoidable impurities.

[0256] The stainless steel composite plate has both excellent mechanical properties and corrosion resistance, and has excellent plate shape, interface bonding quality, uniformity, impact toughness and surface quality compared to the prior art.

[0257] Specifically, the single-sided stainless steel composite plate according to one embodiment of the present invention was sampled in accordance with GB / T 2975-Steel and Steel Products-"Sampling Location and Preparation of Specimens for Mechanical Properties Tests", and:

[0258] In terms of plate shape, the test is carried out in accordance with GB / T 709- "Dimensions, shape, weight and allowable deviations of hot-rolled steel plates and strips". The unevenness of the composite plate is ≤3mm / m, and even ≤2mm / m.

[0259] In terms of interface bonding quality, according to GB / T 6396-Test Methods for Mechanical and Process Properties of Composite Steel Plates, a tensile test was conducted on the composite plate. The composite interface bonding rate of the composite plate was 100%, and the shear strength was ≥300MPa, and even the shear strength was ≥360MPa.

[0260] In terms of mechanical properties, according to GB / T 6396-"Test Methods for Mechanical and Process Properties of Composite Steel Plates" and GB / T 228.1-"Tensile Tests for Metallic Materials - Part 1: Room Temperature Test Methods", the tensile test results show that the yield strength of the composite plate is ≥345MPa, the tensile strength is ≥490MPa, the elongation after fracture is ≥18%, and the yield strength ratio is ≤0.85. The Vickers hardness difference in the thickness direction of the base material layer of the composite plate is ≤10, the head-middle-tail strength difference is ≤40MPa, and the strength difference across the entire plate is ≤40MPa.

[0261] According to GB / T 6396-"Test Methods for Mechanical and Process Properties of Composite Steel Plates" and GB / T 229-"Charpy Pendulum Impact Test Method for Metallic Materials", the composite plate is tested to have an impact energy of ≥120J at 0°C, ≥120J at -20°C, and ≥120J at -40°C. Furthermore, the composite plate may have an impact energy of ≥240J at 0°C, ≥200J at -20°C, and ≥150J at -40°C.

[0262] Sampling was carried out in accordance with GB / T 2975-Steel and Steel Products-"Sampling Location and Preparation of Specimens for Mechanical Properties Tests", and testing was carried out in accordance with GB / T 6396-"Test Methods for Mechanical and Process Properties of Composite Steel Plates". The composite plate had no cracks when bent outward 180° and no cracks when bent inward 180°.

[0263] Sampling was carried out in accordance with GB / T 6396- "Test Methods for Mechanical and Processing Properties of Composite Steel Plates" and testing was conducted in accordance with GB / T 4334- "Corrosion of Metals and Alloys - Test Methods for Intergranular Corrosion of Austenitic and Ferritic-Austenitic (Duplex) Stainless Steels". The composite plate was boiled in a sulfuric acid-copper sulfate solution for 20 hours and bent 180°. No intergranular corrosion cracks were observed in the composite layer.

[0264] To summarize, compared with the existing technology, the present invention has the following advantages: on the one hand, in the entire preparation method, the corrosion resistance and mechanical strength of the stainless steel composite plate are guaranteed through specific control of the process, and the corrosion resistance and mechanical properties are avoided from being deteriorated during the rolling process of the composite billet; on the other hand, the problems of poor plate shape, poor interface bonding quality, and poor surface quality of the existing thick plates of stainless steel composite plates are solved, so that the stainless steel composite plate has excellent plate shape and interface bonding quality, and avoids obvious surface defects such as pits and scratches caused by the existing explosive composite technology; on the other hand, it can also solve the problem of dissimilar welding in the existing technology, the types of composite plates are more diverse, the usage scenarios are higher, and the yield rate and production efficiency are high during the production process.

[0265] The detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

[0266] The beneficial effects of the present invention are further illustrated below through a plurality of embodiments. Of course, these embodiments are only a part of the many variations of the present invention, but not all of them.

[0267] The implementation methods for the composite billet preparation stage used in each of these examples are as described above, see Tables 1 to 5 above, and the specific chemical compositions of the composite and base steels in Tables 1 to 5 are shown in Table 6. "-" indicates that the corresponding element was not actively added during the billet preparation process (the content was zero or close to zero).

[0268] Table 6

[0269] Furthermore, for each example, the preferred embodiments of the heating, rolling, cooling, plate separation, and flattening steps provided by the present invention were implemented to ultimately produce finished single-sided stainless steel composite plates. The total thickness, substrate layer thickness, and composite layer thickness of the composite plates of these examples are shown in Table 7. The ranges in the columns for composite plate thickness and substrate layer thickness in Table 7 represent minimum to maximum thicknesses.

[0270] Furthermore, using the sampling and testing standards disclosed above, samples of the composite panels from various examples were sampled and tested. All examples demonstrated a 100% interfacial bonding rate, a passing 180° inward bend (no cracks), and a passing 180° outward bend (no cracks). Furthermore, after being boiled in a sulfuric acid-copper sulfate solution for 20 hours and bent 180°, the composite layer showed no intergranular corrosion cracks. Other performance test results are shown in Tables 7 and 8.

[0271] Table 7

[0272] Table 8

Claims

1. A method for preparing a stainless steel composite plate for a bridge structure, characterized in that: The method includes a process flow of blank preparation, coating of a release agent, blank assembly, sealing, vacuuming, sealing, heating, rolling, cooling, plate separation, and flattening; wherein, In the billet assembly process: the billet is assembled in a manner of an upper carbon steel substrate A, a lower carbon steel substrate B, an intermediate layer of at least two stainless steel composite materials, and four seals surrounding the four sides of the intermediate layer, and gas shielded welding is performed between the seal and the substrate A, and between the seal and the substrate B to form a base billet; the four sides of the base billet are all provided with grooves surrounded by the substrate A, the seal and the substrate B, and a circular through hole is opened on the seal of one side of the base billet, and a steel pipe with an outer diameter of r is welded in the through hole; In the sealing welding process: the groove is surfacing welded, and a hole with a radius of R>r and concentric with the steel pipe is reserved around the steel pipe during surfacing welding; when the groove on the side where the steel pipe is located is surfacing welded to a depth of 2 / 3 of the groove depth, and the grooves on other sides are surfacing welded to a depth of more than 2 / 3 of the groove depth, surfacing welding is stopped; In the sealing process: after the base blank is vacuumed, the steel pipe is heated with a flame gun, flattened, and folded into the reserved hole; the hole is fully welded with gas shielded welding to seal the steel pipe in the hole; then the surfacing welding is continued until the groove is filled, and finally the cover welding is performed to obtain a composite blank; In the rolling process: the composite billet out of the heating furnace is rolled to obtain a large composite plate; in the whole rolling process, the first n passes are transverse rolling, and the longitudinal rolling is adopted after the n+1 pass, and the rolling reduction of the first pass is ≥25mm and the rolling temperature is ≥1060℃, the width of the billet obtained by the nth pass is Wt+0~40mm, Wt is the target width of the large composite plate, and the rolling temperature of the nth pass is ≥1030℃; between the nth pass and the n+1th pass and between the n+2nd pass and the n+3rd pass, the billet is water-cooled once in 6 groups of headers, and the cooling water volume of the upper header of each group of headers is 120~180m 3 / h, cooling water volume of lower header 160~220m 3 / h, and the roller speed is 0.8~1.2m / s; the rolling reduction from the n+1th to the n+3th pass is ≥40mm, and the rolling temperature of the n+1th pass is ≥950℃; when it comes to the mth pass, the rolling temperature is ≥900℃, and the billet is rolled to a thickness of 2.5~3.5 times the target thickness of the composite plate; then water cooling is carried out until the surface temperature of the billet drops below 840℃; then the second stage of rolling is carried out until the billet thickness is the target thickness of the composite plate, completing the entire rolling process, the first rolling temperature of the second stage rolling is 810℃~840℃, and the rolling temperature of the last pass is 780~810℃.

2. The method for preparing a stainless steel composite plate for a bridge structure according to claim 1, characterized in that: In the sealing welding process, when the groove on the side where the steel pipe is located is welded to a depth of 2 / 3 of the groove depth and the grooves on other sides are welded to a depth of the groove depth, the sealing welding process is terminated.

3. The method for preparing a stainless steel composite plate for a bridge structure according to claim 1, characterized in that: During surfacing welding, the groove is welded in multiple layers and multiple passes in the order of upper edge and lower edge first and middle area later. Each layer is welded for more than 4 passes, the interpass temperature is 140-160°C, the total number of welding layers is 6-8 layers, and the interpass temperature is 150-250°C.

4. The method for preparing a stainless steel composite plate for a bridge structure according to claim 1, characterized in that: In the blank assembly process, the through hole is opened on a seal at a short side of the base blank, and the through hole is centered at a position of 1 / 3 of the length and 1 / 2 of the width of the seal; The end surface of the steel pipe is flush with the inner surface of the seal.

5. The method for preparing a stainless steel composite plate for a bridge structure according to claim 1, characterized in that: In the assembly process, grooves are formed on the upper and lower edges of the outer surface of the seal strip, with a groove angle of 10 to 20 degrees and a vertical depth of 10 to 15 mm.

6. The method for preparing a stainless steel composite plate for a bridge structure according to claim 1, characterized in that: In the assembly process, the middle layer is composed of composite material A and composite material B stacked together.

7. The method for preparing a stainless steel composite plate for a bridge structure according to claim 6, characterized in that: In the base blank obtained in the blank assembly process, the base material A and the base material B are plates of equal thickness.

8. The method for preparing a stainless steel composite plate for a bridge structure according to claim 6, characterized in that: In the base blank obtained in the blank assembly process, substrate A and substrate B are respectively plates of non-uniform thickness whose thickness varies along the X direction, and the surfaces to be composited of substrate A and substrate B are relatively complementary; the X direction is the length direction or width direction of substrate A and substrate B.

9. The method for preparing a stainless steel composite plate for a bridge structure according to claim 8, characterized in that: Substrate A and substrate B are plates of non-uniform thickness with monotonically varying thickness along the X direction, and their respective surfaces to be composited are inclined planes; Alternatively, the substrate A and the substrate B are plates of non-uniform thickness whose thickness varies non-monotonically along the X direction, and their respective surfaces to be composited include more than two planes arranged along the X direction.

10. The method for preparing a stainless steel composite plate for a bridge structure according to claim 1, characterized in that: In the assembly process, the middle layer is composed of two or more composite materials arranged side by side along the X direction, and the X direction is the length direction or width direction of the substrate A and the substrate B; The connecting sides of two adjacent composite materials are arranged as parallel and complementary oblique edges, and a smaller surface of each composite material in the thickness direction constitutes a non-to-be-compounded surface, and the other larger surface constitutes a to-be-compounded surface.

11. The method for preparing a stainless steel composite plate for a bridge structure according to claim 1, characterized in that: In the heating process: the composite blank is heated in a heating furnace according to a five-stage preheating section, a first heating section, a second heating section, a third heating section and a soaking section, the preheating section temperature is ≤850°C, the first heating section temperature is 1080±30°C, the second heating section temperature is 1160±30°C, the third heating section temperature is 1220±20°C, the soaking section temperature is 1190±20°C, the residence time of the third heating section is (0.25~0.35)×t min / mm, t is the thickness of the composite blank, and the residence time of the soaking section is 15min~30min.

12. The method for preparing a stainless steel composite plate for a bridge structure according to claim 1, characterized in that: In the cooling process: the large composite plate obtained by rolling enters the ultra-fast cooling system, which has 24 groups of cooling manifolds arranged at intervals of 1m along the roller table, and the cooling distance of each group of cooling manifolds is 1m. When the large composite plate passes through the ultra-fast cooling system, the opening and closing states of all 24 groups of cooling manifolds are controlled in a manner of opening N groups of cooling manifolds and then not opening M groups of cooling manifolds. The cooling water pressure is 0.15-0.30MPa, the cooling rate is 3-15℃ / s, and the final cooling temperature is 380-590℃; wherein N is 2, 3 or 4, and M is 2, 3 or 4.

13. The method for preparing a stainless steel composite plate for a bridge structure according to claim 12, characterized in that: During the cooling process: After leaving the ultra-fast cooling system, the composite board is air-cooled on a cooling bed until it reaches room temperature.

14. The method for preparing a stainless steel composite plate for a bridge structure according to claim 12, characterized in that: During the cooling process: After leaving the ultra-fast cooling system, the composite board is placed at a temperature of T f -150℃~T f The stack cooling is carried out between two steel plates at +150℃, and the stack cooling time is 0.4min / mm×t0±5min, where t0 is the thickness of the composite plate. After the stack cooling is completed, the cooling bed on the composite plate is naturally cooled to room temperature; Among them, T f =550+30Si-20Mn+15Cr-15Ni+10Mo, the element symbols in the formula represent 100 times the mass percentage of each element in substrate A and / or substrate B, and the chemical composition of substrate A and substrate B is the same.

15. The method for preparing a stainless steel composite plate for a bridge structure according to claim 12, characterized in that: The thickness of the composite plate is less than 54 mm, the roller speed of the ultra-fast cooling system is 0.4-0.8 m / s, and the composite plate passes through the ultra-fast cooling system once and then leaves the ultra-fast cooling system; Alternatively, the thickness of the composite plate is greater than 54 mm and less than 70 mm, the roller speed of the ultra-fast cooling system is greater than 0.2 m / s and less than 0.6 m / s, and the composite plate passes through the ultra-fast cooling system once and then leaves the ultra-fast cooling system; Alternatively, the thickness of the large composite plate is ≥70 mm, the roller speed of the ultra-fast cooling system is 0.4-0.9 m / s, the large composite plate first enters the ultra-fast cooling system inlet in the forward direction, and when its head reaches the 24th group of cooling manifolds, the roller reverses, and the large composite plate passes through the ultra-fast cooling system in the reverse direction and leaves the ultra-fast cooling system inlet.

16. The method for preparing a stainless steel composite plate for a bridge structure according to claim 1, characterized in that: In the flattening process: the composite material of the small single-sided composite board obtained in the board separation process is placed on the flattening machine with the face upwards for flattening, wherein: when flattening horizontally, the flattening force of the flattening machine is controlled to be F1 = ν × a × b × c 横 ×σ 横 / (d×(ν-c 横 / a)); When flattening longitudinally, control the flattening force of the flattening machine F2 = a×b×c 纵 ×σ 纵 / (d+c 纵 ); where a is the width of the composite board, in mm, b is the thickness of the composite board, in mm, c 横 It is the unevenness per meter of the composite board in the horizontal direction, in mm, c 纵 is the unevenness per meter of the composite board in the longitudinal direction, in mm, d is the working distance of the flattening machine, σ 横 is the tensile yield strength of the composite plate in the transverse direction, σ 纵 is the tensile yield strength of the composite plate in the longitudinal direction, and ν is the Poisson's ratio.

17. The method for preparing a stainless steel composite plate for a bridge structure according to claim 1, characterized in that: Step "The inner space of the base blank is vacuumed three times and broken twice through the steel pipe, and finally the inner space of the base blank is maintained at a vacuum degree of ≤10 -2 "Pa" includes: First, connect the steel pipe to a vacuum pump to evacuate the interior space of the base blank to a vacuum degree of ≤10 -2 Pa, and then maintain the pressure for more than 4 hours; then connect the steel pipe to the nitrogen supply device, break the base blank, and fill it with nitrogen; Afterwards, the steel pipe is connected to the vacuum pump again to evacuate the base blank to a vacuum degree of ≤10 -1 Pa, without maintaining pressure; then the steel pipe is connected to the nitrogen supply device again, the base blank is vented and filled with nitrogen; Finally, the steel pipe is connected to the vacuum pump for the third time to evacuate the base blank to a vacuum degree of ≤10 -2 Pa.

18. The method for preparing a stainless steel composite plate for a bridge structure according to claim 1, characterized in that: In the process of applying the release agent: applying the release agent to the non-composite surface of the composite material; The release agent used is a coating liquid containing silicon oxide and magnesium oxide, wherein the mass ratio of silicon oxide to magnesium oxide is 3:1; or The composition is as follows by mass ratio: 25-35% of silicon nitride, 5-10% of thermosetting amino resin, and 55-70% of water.

19. A stainless steel composite plate for a bridge structure prepared by the preparation method according to claim 1, characterized in that: The chemical composition of the substrate layer is as follows by mass percentage: C: 0.03-0.16%, Si: 0.11-0.29%, Mn: 1.31-1.54%, P≤0.018%, S≤0.0030%, Cr: 0.06-0.29%, Ni≤0.24%, Cu≤0.24%, Mo≤0.24%, Nb: 0.011-0.034%, Ti: 0.011-0.019%, Al: 0.030-0.040%, and the balance is Fe and unavoidable impurities; The chemical composition of the composite layer is calculated by mass percentage as follows: C≤0.15%, Si≤1.00%, Mn≤2.00%, P≤0.045%, S≤0.030%, Ni: 6.0-22.0%, Cr: 16.0-26.0%, Mo≤3.0%, and the balance is Fe and unavoidable impurities; The composite interface bonding rate of the composite plate is 100%, and the shear strength is ≥300MPa.

20. The stainless steel composite plate according to claim 19, characterized in that: The composite material layer covers part of the upper surface of the substrate layer but not the entire upper surface.

Citation Information

Patent Citations

  • Production method of stainless steel composite plates

    CN107009090A

  • Stainless-steel clad steel sheet for bridges and production method thereof

    CN109694986A

  • Explosive welding manufacturing method for TMCP type bridge steel stainless steel composite sheet

    CN110064835A

  • Preparation method of titanium-steel composite plate with IF steel as interlayer

    CN108393653A

  • High-corrosion-resistance marine composite steel plate and manufacturing method thereof

    CN111361235A