Phenolic resin sponge having asymmetric structure and preparation method therefor

Through a new preparation method, an asymmetric structure phenolic resin sponge was constructed, which solved the problems of large heat loss and low interface photothermal conversion efficiency caused by the traditional symmetric structure, achieved rapid water transmission and efficient heat insulation, and improved solar energy Evaporator performance.

WO2024221795A1PCT designated stage expired Publication Date: 2024-10-31JIANGNAN UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/127591
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2023-10-30
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Traditional phenolic resin sponges have a symmetrical structure, which results in large heat loss and reduces the interface photothermal conversion efficiency, limiting its application in the field of photothermal conversion, especially in the field of solar evaporation.

Method used

A new preparation method is adopted, by mixing phenol and formaldehyde solutions with sodium hydroxide and heating, adjusting the pH value, then adding the pore-forming agent to the ethanol solution, stirring, pouring into an open container to evaporate the ethanol, and vacuuming the bubbles. and heat treatment, followed by acid treatment, ethanol aqueous solution dialysis and freeze-drying to obtain a phenolic resin sponge with an asymmetric structure.

Benefits of technology

The fast water transmission performance and efficient heat insulation of the phenolic resin sponge are achieved, and the interface light-to-heat conversion efficiency is improved. Specifically, the evaporation efficiency of the sponge evaporator is improved, and the material has better strength and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023127591_31102024_PF_FP_ABST
    Figure CN2023127591_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a phenolic resin sponge having an asymmetric structure and a preparation method therefor. The method comprises: firstly, mixing phenol, a formaldehyde solution and a sodium hydroxide solution, heating, drying, and then adding the mixture into an ethanol solution containing a pore-forming agent; after stirring, pouring the mixture into an open container, and volatilizing the solvent; and then performing processes such as high-temperature acid treatment, ethanol aqueous solution dialysis, and freeze-drying, so as to obtain a phenolic resin sponge having an asymmetric structure. The method involves a simple operation, and the prepared phenolic resin sponge having an asymmetric structure has high porosity, a controllable microstructure, good hydrophilicity and chemical corrosion resistance, can realize rapid water transmission and reduce heat loss, and has potential application value in the fields of seawater desalination, wastewater purification and the like.
Need to check novelty before this filing date? Find Prior Art

Description

A phenolic resin sponge with an asymmetric structure and a preparation method thereof Technical Field

[0001] The invention relates to a phenolic resin sponge with an asymmetric structure and a preparation method thereof, belonging to the technical field of material science. Background Art

[0002] Phenolic resin sponge has been used in fields such as adsorption / filtration materials, seawater desalination or wastewater purification due to its advantages such as low density, large specific surface area, controllable porosity, low raw material price, simple preparation method, and strong chemical corrosion resistance and heat resistance.

[0003] The currently synthesized phenolic resin sponge is a solid material with a network skeleton structure formed by cross-linking polymer molecules. The traditional synthesis method is to dissolve two monomers in deionized water, add an acid or base catalyst to cause a sol-gel reaction, and then obtain the phenolic resin sponge through aging, solvent replacement, and drying. However, the obtained phenolic resin sponge usually has a symmetrical structure and has a high water storage capacity. It is very easy to cause heat loss through conduction, convection, radiation, etc., thereby reducing the interfacial photothermal conversion efficiency, limiting its application in photothermal conversion fields such as interfacial solar evaporation. Therefore, in order to further improve the water transport characteristics and thermal insulation performance of phenolic resin sponge, it is urgent to develop a convenient and efficient method to prepare phenolic resin sponge to achieve rapid water transport, efficient thermal insulation and interfacial photothermal conversion efficiency.

[0004] Summary of the Invention

[0005] In response to the above-mentioned problems, the present invention aims to provide a phenolic resin sponge with an asymmetric structure to improve the water transmission performance of the phenolic resin sponge. The method is simple to operate, and the pore size decreases from top to bottom, thereby achieving rapid water transmission performance.

[0006] The invention discloses a preparation method of a phenolic resin sponge with an asymmetric structure. The method comprises the following steps: mixing phenol, formaldehyde solution and sodium hydroxide solution, adjusting the pH value of the solution to 5-9 after heating reaction, adding the solution to an ethanol solution containing a pore-forming agent after drying, stirring and pouring the mixture into an open container to volatilize the ethanol, vacuum-degassing the bubbles and then performing heat treatment, and finally performing acid treatment, dialysis with an ethanol-water solution and freeze-drying to obtain the phenolic resin sponge with an asymmetric structure.

[0007] In one embodiment of the present invention, the molar ratio of phenol:formaldehyde:sodium hydroxide is 20:40:(0.1-2).

[0008] In one embodiment of the present invention, the temperature during the heating reaction is 65-80° C., and the reaction time is 0.5-2 h.

[0009] In one embodiment of the present invention, the drying is preferably vacuum drying, and the vacuum drying time is 12 to 72 hours.

[0010] In one embodiment of the present invention, the pore-forming agent is a mixture of polyether and zinc chloride, the polyether is polyether P123 or polyether F127, and the mass ratio of the polyether to zinc chloride is 0.16 to 0.48.

[0011] In one embodiment of the present invention, the mass ratio of the pore-forming agent to phenol is 0.03 to 0.26.

[0012] In one embodiment of the present invention, the temperature during the heat treatment is 100-145° C., and the heat treatment time is 12-72 hours.

[0013] In one embodiment of the present invention, the temperature during the acid treatment is 90-100° C., and the time is 6-24 hours.

[0014] In one embodiment of the present invention, the acid used in the acid treatment includes at least one of sulfuric acid, hydrochloric acid, phosphoric acid, and nitric acid, the concentration of the sulfuric acid is 20 to 98 wt %, the concentration of the hydrochloric acid is 20 to 37%, the concentration of the phosphoric acid is 20 to 47%, and the concentration of the nitric acid is 20 to 67%.

[0015] In one embodiment of the present invention, the concentration of the ethanol aqueous solution used in dialysis is 5 to 30 wt %, and the dialysis time is 1 to 7 days.

[0016] In one embodiment of the present invention, the freeze-drying temperature is -150 to -50°C, the freezing time is 2 to 10 hours, and the drying time is 48 to 96 hours.

[0017] The invention discloses a phenolic resin sponge with an asymmetric structure prepared by the above-mentioned preparation method.

[0018] The present invention also discloses an application of the phenolic resin sponge in the field of photothermal conversion. [Beneficial Effects]

[0019] (1) The present invention is simple to operate, green and environmentally friendly, and is a new method for preparing phenolic resin sponge conveniently and efficiently.

[0020] (2) The present invention prepares a phenolic resin sponge with an asymmetric structure by regulating the microstructure of the material. A resol phenolic resin is first prepared, and then mechanically stirred with a pore-forming agent and anhydrous ethanol to form a homogeneous solution. After heat treatment, acid treatment, and freeze-drying, a phenolic resin sponge with an asymmetric structure is obtained. On the one hand, a three-dimensional porous structure is constructed, the pore-forming agent is easily removed, and the material has good strength; on the other hand, the asymmetric pore structure has faster water transmission performance than the symmetric pore structure.

[0021] (3) The phenolic resin sponge prepared by the present invention has an asymmetric porous structure and has the advantages of high porosity, fast water transmission, and low heat loss. The phenolic resin sponge prepared by the method of the present invention can quickly absorb water within 62ms and has good water transmission performance. After it is prepared into a sponge evaporator, the sponge evaporator can absorb sunlight at a rate of up to 96.8%.

[0022] (4) The evaporation efficiency of the solar evaporator prepared from the phenolic resin sponge with an asymmetric structure of the present invention is higher than that of the solar evaporator prepared from the phenolic resin sponge with a symmetric structure in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] FIG1 is a physical picture of a phenolic resin sponge with an asymmetric structure prepared in Example 1 of the present invention;

[0024] FIG2 is a bottom structural diagram of a phenolic resin sponge with an asymmetric structure prepared in Example 1 of the present invention, wherein (a) and (b) are a scanning electron microscope image and a statistical diagram of sponge pore size, respectively;

[0025] FIG3 is a top structural diagram of a phenolic resin sponge with an asymmetric structure prepared in Example 1 of the present invention, wherein (a) and (b) are a scanning electron microscope image and a statistical diagram of the sponge pore size, respectively;

[0026] FIG4 is a water contact angle test graph of the small-pore surface of the phenolic resin sponge with an asymmetric structure prepared in Example 1 of the present invention.

[0027] FIG5 is a water contact angle test graph of the macroporous surface of the phenolic resin sponge with an asymmetric structure prepared in Example 1 of the present invention.

[0028] FIG6 is the absorbance of sunlight by the phenolic resin sponge evaporator prepared in Example 1.

[0029] FIG7 is a physical picture of the phenolic resin sponge with an asymmetric structure prepared in Example 4.

[0030] FIG8 is a Fourier transform infrared spectrum of the sponge prepared in Comparative Example 2.

[0031] Figure 9 is a bottom structure diagram and a physical diagram of the sponge prepared in Comparative Example 3; (a) is a bottom structure diagram, and (b) is a physical diagram.

[0032] FIG10 is a water contact angle test diagram of the symmetrical structure of the phenolic resin sponge in Comparative Example 4.

[0033] FIG11 is a comparison diagram of the evaporation rates of the phenolic resin sponge evaporators with asymmetric and symmetric structures. DETAILED DESCRIPTION

[0034] Below in conjunction with specific embodiment, further set forth the present invention.Should be understood that these embodiments are only used to illustrate the present invention and are not used in limiting the scope of the present invention.In addition, should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall equally within the scope limited by the appended claims of the application.

[0035] Example 1

[0036] 0.61 g of phenol, 0.13 g of a 20 wt % sodium hydroxide solution, and 1.05 g of a 37 wt % formaldehyde solution were mixed and stirred in a 75° C. water bath for 1 h. The mixed solution was adjusted to pH 7 with 0.6 mol / L hydrochloric acid and dried in vacuo at 45° C. for 12 h. Then, 3 mL of an ethanol solution containing 0.96 g of polyether F127 and 6 g of zinc chloride was added and stirred to evaporate the ethanol. The mixture was then placed in a vacuum oven for bubble removal and heat treated at 100° C. for 60 h to obtain a phenolic resin wet gel. The wet gel was placed in 55 wt % sulfuric acid and treated at 100° C. for 7 h. Subsequently, the mixture was dialyzed in a 20 wt % ethanol aqueous solution for 6 h. The mixture was then frozen at -70° C. for 6 h and further freeze-dried for 48 h to obtain a phenolic resin sponge material with an asymmetric structure.

[0037] Characterization of phenolic resin sponge materials with asymmetric structure and their preparation methods

[0038] FIG1 is a physical picture of the phenolic resin sponge with an asymmetric structure prepared in Example 1, which is in the shape of a lightweight cylinder.

[0039] Figures 2(a) and 2(b) are, respectively, a scanning electron micrograph of the bottom and a pore size distribution diagram of the asymmetric phenolic resin sponge prepared in Example 1. The resulting phenolic resin sponge has a porous structure with a framework composed of nanoparticles and an average pore size of approximately 0.47 μm.

[0040] Figures 3(a) and 3(b) are a top SEM image and a pore size distribution diagram of the asymmetric phenolic resin sponge prepared in Example 1. The top pore size of the obtained phenolic resin sponge is approximately 3.16 μm, which is approximately 6.7 times the bottom pore size.

[0041] FIG4 is a water contact angle test diagram of the phenolic resin sponge with an asymmetric structure prepared in Example 1. The small pore size side absorbs water quickly within 62 ms and has good water transmission performance.

[0042] FIG5 is a water contact angle test diagram of the phenolic resin sponge with an asymmetric structure prepared in Example 1. The water transmission performance of the side with a larger pore size is reduced, and the water is completely absorbed within 0.936 s.

[0043] A thin layer of pyrrole was sprayed on the macroporous side of the sponge, followed by a layer of ammonium persulfate solution (2 g / mL), and the photothermal layer polypyrrole was successfully prepared. A phenolic resin sponge evaporator with an asymmetric structure was obtained. The absorbance of the evaporator to sunlight in the wavelength range of 500-2500nm was tested using an ultraviolet-visible-near-infrared diffuse reflectance spectrophotometer (Shimadzu UV-3600i Plus). The test results are shown in Figure 6. The results show that macroporous polymerized polypyrrole is beneficial to increase the multiple reflections of sunlight by the evaporator, and the absorption rate of sunlight is as high as 96.8%.

[0044] Example 2: Changing the sodium hydroxide dosage

[0045] 0.61 g of phenol, 0.06 g of 20 wt% sodium hydroxide, and 1.05 g of 37 wt% formaldehyde were mixed and stirred in a water bath at 75°C for 1 h. The solution was adjusted to pH 5 with 0.6 mol / L hydrochloric acid and vacuum-dried at 45°C for 12 h. Then, 3 mL of ethanol solution containing 0.96 g of polyether F127 and 6 g of zinc chloride was added and stirred to evaporate the ethanol. The mixture was then placed in a vacuum oven to remove bubbles and then heat-treated at 145°C for 60 h to obtain a phenolic resin wet gel. The wet gel was placed in 65 wt% sulfuric acid and treated at 100°C for 24 h. Subsequently, the wet gel was dialyzed in deionized water for 6 h, then frozen at -70°C for 6 h, and further freeze-dried for 48 h to obtain a phenolic resin sponge material with an asymmetric structure.

[0046] The size of the nanoparticles at the bottom of the sponge did not change much compared to Example 1, the pore size of the prepared sponge changed very little, and the overall water transport performance changed very little.

[0047] Example 3: Changing the sodium hydroxide dosage

[0048] 0.61 g of phenol, 0.19 g of 20 wt% sodium hydroxide, and 1.05 g of 37 wt% formaldehyde were mixed and stirred in a water bath at 75°C for 1 h. The solution was adjusted to pH 7 with 0.6 mol / L hydrochloric acid and vacuum-dried at 45°C for 12 h. Then, 3 mL of ethanol solution containing 0.96 g of polyether F127 and 6 g of zinc chloride was added and stirred to evaporate the ethanol. The mixture was then placed in a vacuum oven to remove bubbles and then heat-treated at 100°C for 60 h to obtain a phenolic resin wet gel. The wet gel was placed in 75 wt% sulfuric acid and treated at 100°C for 7 h. Subsequently, it was dialyzed in a 30 wt% ethanol aqueous solution for 7 days, then frozen at -50°C for 6 h, and further freeze-dried for 48 h to obtain a phenolic resin sponge material with an asymmetric structure.

[0049] The size of the nanoparticles at the bottom of the sponge did not change much compared to Example 1, the pore size of the prepared sponge changed very little, and the overall water transport performance changed very little.

[0050] Example 4: Changing the amount of zinc oxide

[0051] 0.61 g of phenol, 0.065 g of 20 wt% sodium hydroxide, and 1.05 g of 37 wt% formaldehyde were mixed and stirred in a water bath at 75°C for 1 h. The solution was adjusted to pH 8 with 0.6 mol / L hydrochloric acid and vacuum-dried at 45°C for 12 h. Then, 3 mL of ethanol solution containing 0.96 g of polyether P123 and 3 g of zinc chloride was added and stirred to evaporate the ethanol. The mixture was then placed in a vacuum oven to remove bubbles and then heat-treated at 100°C for 60 h to obtain a phenolic resin wet gel. The wet gel was placed in 85 wt% sulfuric acid and treated at 100°C for 7 h. Subsequently, it was dialyzed in a 20 wt% ethanol aqueous solution for 7 days, then frozen at -70°C for 6 h, and further freeze-dried for 48 h to obtain a phenolic resin sponge material with an asymmetric structure.

[0052] FIG7 is a physical picture of the phenolic resin sponge with an asymmetric structure prepared in Example 4. From the experimental results, it can be seen that after reducing the amount of zinc chloride, a certain amount of bubbles will be generated on the surface of the prepared sponge.

[0053] Comparative Example 1

[0054] The difference between Comparative Example 1 and Example 1 is that sodium hydroxide is not added in Comparative Example 1. The prepared asymmetric phenolic resin sponge material has a loose structure and its three-dimensional structure easily collapses, and cannot form a complete block sponge.

[0055] Comparative Example 2

[0056] The difference between Comparative Example 2 and Example 1 is that no high-temperature acid treatment is performed, and deionized water is used directly for dialysis to remove impurities.

[0057] As shown in Figure 8, the water-treated sample has a -1 A clear peak at , indicating that polyether F127 was not completely removed. After acid treatment, the ether bonds in polyether F127 disappeared, and the corresponding peaks disappeared, indicating that polyether F127 was completely removed. Combined with the results of Example 2, it can be seen that acid treatment has a significant impact on the removal rate of the pore-forming agent. Without high-temperature acid treatment, zinc chloride can be removed, but the polyether cannot be completely removed.

[0058] Comparative Example 3

[0059] The difference between Comparative Example 3 and Example 1 is that zinc oxide is not added in Comparative Example 3.

[0060] As can be seen from FIG9 , when zinc chloride is not added, a hard resin is formed instead of a porous sponge, and the resin does not have water transmission properties.

[0061] Comparative Example 4

[0062] 0.61 g of phenol, 0.13 g of 20 wt% sodium hydroxide solution, and 1.05 g of 37 wt% formaldehyde solution were mixed and stirred in a water bath at 75°C for 1 h. The mixed solution was adjusted to pH 7 with 0.6 mol / L hydrochloric acid and vacuum-dried at 45°C for 12 h. Then, 3 mL of ethanol solution containing 0.96 g of polyether F127 and 6 g of zinc chloride was added. The resulting mixed solution was placed in a sealed container and then placed in a vacuum oven to remove bubbles. The mixture was then heat-treated at 100°C for 60 h to obtain a phenolic resin wet gel. The wet gel was placed in 55 wt% sulfuric acid and treated at 100°C for 7 h. Subsequently, the gel was dialyzed in a 20 wt% ethanol aqueous solution for 6 h, then frozen at -70°C for 6 h, and further freeze-dried for 48 h to obtain a phenolic resin sponge material with a symmetrical structure.

[0063] FIG10 is a water contact angle test diagram of the prepared phenolic resin sponge with a symmetrical structure. As can be seen from the figure, the sponge needs 1.358 s to absorb all the water, indicating that the water transmission performance of the sponge with a symmetrical structure is poor.

[0064] In Figure 11, AP-PPy-PFDS-B, AP-PPy-PFDS-U, and AP-PPy-PFDS respectively represent the evaporation rates of an asymmetric phenolic resin sponge after PPy polymerization on the small-pore side, an evaporator after PPy polymerization on a phenolic resin sponge prepared in a closed environment, and an asymmetric phenolic resin sponge after PPy polymerization on the large-pore side. The preparation method for the asymmetric phenolic resin sponge used in this experiment is the same as that in Example 1, and the method for polymerizing PPy on the phenolic resin sponge is the same as the method for preparing the phenolic resin sponge evaporator in Example 1.

[0065] From the results, it can be seen that the asymmetric structure of the phenolic resin sponge with macroporous surface polymerization PPy has the best solar evaporation rate, and the asymmetric structure of the phenolic resin sponge has a better solar evaporation rate than the symmetric structure of the phenolic resin sponge.

[0066] Although the present invention has been disclosed above with reference to preferred embodiments, this is not intended to limit the present invention. Anyone familiar with this technology may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be defined by the claims.

Claims

1. A method for preparing a phenolic resin sponge with an asymmetric structure, characterized in that: The method comprises the following steps: Phenol, formaldehyde solution and sodium hydroxide solution are mixed, and the pH value of the solution is adjusted to 5-9 after heating reaction. After drying, the solution is added to an ethanol solution containing a pore-forming agent, and after stirring, it is poured into an open container, and after vacuuming bubbles, heat treatment is performed, and then acid treatment, ethanol aqueous solution dialysis, and freeze drying are performed to obtain a phenolic resin sponge with an asymmetric structure.

2. The preparation method according to claim 1, characterized in that: The molar ratio of the phenol, formaldehyde and sodium hydroxide is 20:40:(0.1-2), the heating reaction temperature is 65-80° C., and the reaction time is 0.5-2 hours.

3. The preparation method according to claim 1, characterized in that: The drying is vacuum drying, and the vacuum drying time is 12 to 72 hours.

4. The preparation method according to claim 1, characterized in that: The pore-forming agent is a mixture of polyether and zinc chloride, the polyether is polyether P123 or polyether F127, and the mass ratio of the polyether to the zinc chloride is 0.16-0.

48.

5. The preparation method according to claim 1, characterized in that: The mass ratio of the pore-forming agent to phenol is 0.03 to 0.

26.

6. The preparation method according to claim 1, characterized in that: The temperature during the heat treatment is 100-145° C., and the heat treatment time is 12-72 hours.

7. The preparation method according to claim 1, characterized in that: The temperature during the acid treatment is 90-100° C., and the time is 6-24 hours. The acid used in the acid treatment includes at least one of sulfuric acid, hydrochloric acid, phosphoric acid, and nitric acid. The concentration of the sulfuric acid is 20-98wt%, the concentration of the hydrochloric acid is 20-37%, the concentration of the phosphoric acid is 20-47%, and the concentration of the nitric acid is 20-67%.

8. The preparation method according to claim 1, characterized in that: The concentration of the ethanol aqueous solution used in dialysis is 5 to 30 wt %, and the dialysis time is 1 to 7 days. 9 . The phenolic resin sponge with an asymmetric structure prepared by the preparation method according to claim 1 .

10. Use of the phenolic resin sponge according to claim 9 in the field of light-to-heat conversion.

Citation Information

Patent Citations

  • Phenolic resin, phenolic foam material and synthetic methods of phenolic resin and phenolic foam material

    CN108912290A

  • Method for preparing porous carbon by taking eutectic ionic liquid as pore forming agent

    CN109485041A

  • Polyurethane sponge with good hydrophilicity and drainability and preparation method of polyurethane sponge

    CN110343229A

  • Nanogold composite mesoporous carbon material with controllable particle size as well as preparation method and application of mesoporous carbon material

    CN110759329A

  • Ionic liquid-hierarchical porous phenolic resin as well as preparation method and application thereof

    CN113368836A