Preparation method for NANO nickel oxide / graphene composite electrode material

By modifying nano-nickel oxide on graphene oxide and using the sol-gel method to prepare nano-nickel oxide/graphene composite electrode materials, the problem of insufficient electrode capacity and reversibility is solved, and more efficient electrochemical performance and faster speed are achieved. charging speed.

WO2024222012A1PCT designated stage expired Publication Date: 2024-10-31TIANNENG BATTERY GROUP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/142234
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-12-27
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing nano-nickel oxide/graphene composite electrode materials have low electrode capacity, poor reversibility and insufficient charging speed, which limits their application in the field of energy storage.

Method used

The sol-gel method is used to modify nano-nickel oxide on graphene oxide. By controlling the particle size and compounding low-rate graphene, a nano-nickel oxide/graphene composite electrode material is prepared. Gelatin is used to control the particle size and remove it at 300°C. , improving the conductivity and reversibility of the material.

Benefits of technology

Significantly improved electrode capacity (up to more than 50%), reversibility (average reversible potential increased by 20mV) and charging speed (charging time shortened by more than 20%).

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023142234_31102024_PF_FP_ABST
    Figure CN2023142234_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A preparation method for a nano nickel oxide / graphene composite electrode material, comprising the following steps: (1) respectively dissolving a water-soluble nickel salt, graphene oxide and gelatin into water to form a water-soluble nickel salt solution, a graphene oxide solution and a gelatin solution; (2) adding the water-soluble nickel salt solution to the graphene oxide solution to form a mixed solution, adding the mixed solution to the gelatin solution, and heating and stirring same to obtain a gel; and (3) drying the gel to obtain a nano nickel oxide / graphene composite electrode material. Also provided are the nano nickel oxide / graphene composite electrode material prepared by means of the method and the use of the electrode material in the preparation of a composite electrode.
Need to check novelty before this filing date? Find Prior Art

Description

A method for preparing nano nickel oxide / graphene composite electrode material Technical Field

[0001] The present application relates to the technical field of graphene composite batteries, and in particular to a method for preparing a nano nickel oxide / graphene composite electrode material. Background Art

[0002] Energy is a crucial component of the world's ongoing technological development. In recent decades, the energy crisis has become increasingly severe due to the high cost and limited supply of fossil fuels and growing concerns about environmental pollution. Growing energy demand, coupled with increasing concerns about global warming and air pollution, has prompted intensive research into renewable energy and energy storage devices. Due to their intermittent nature, renewable energy sources face challenges that need to be overcome. Therefore, efficient energy storage methods are a technological challenge to ensure energy availability in the 21st century. Recently, green energy technologies have been adopted in hybrid and electric vehicles, mobile phones, entertainment devices, and space equipment. Fast charging and discharging, high volumetric energy density, low cost, legal resources, safety, environmental friendliness (recyclability), long life, and high efficiency are key factors in future new energy storage devices. Among alternative energy storage methods, electrical energy storage is one of the most promising technologies due to its long-distance transmission capabilities and its perceived clean energy source. The positive electrode plays a crucial role in energy storage systems, with porosity, structure, specific surface area, and electrical conductivity, particularly influencing energy storage capacity, during electrochemical reactions.

[0003] As an ideal matrix, graphene has many attractive properties, such as high electrical conductivity, large specific surface area, high mechanical flexibility, and remarkable thermal and chemical stability. Extensive research has been conducted on the manufacture of graphene-transition metal oxide composites for energy storage applications. These composites can combine the advantages of the two components and produce special properties through mutual reinforcement or modification. Recently, Meryl D. Stoller's group reported the use of chemically modified graphene as an electrode material for supercapacitors (Nano Lett 2008; 8(10): 3498-502). The graphene has high conductivity and good performance at a wide voltage scan rate, but the specific capacitance is low.

[0004] As is well known, amorphous hydrated ruthenium oxide is the most promising electrode material for high-power and high-energy-density supercapacitors, but its high price, scarcity of resources, and environmental pollution caused by the electrolyte used have greatly limited its commercial development. While oxide electrode materials such as NiO have similar functions to RuO2·xH2O and are inexpensive, NiO has two very fatal disadvantages as a supercapacitor material: one is its relatively poor conductivity, and the other is that NiO nanomaterials are prone to agglomeration. In recent years, Cheng et al. (J Power Sources 2008; 185(2): 1563-68.) used a template method to synthesize gradient porous NiO as an electrode material for supercapacitors. Compared with commercially available NiO, its capacitance, power density, and energy density are much better, but its stability is poor at higher voltages.

[0005] One of the current research hotspots is the study of nickel oxide and graphene composites. Composite materials can leverage the advantages of each material, overcome the shortcomings of a single material, and expand the application range of the materials. Patent CN101733985A discloses a graphene / nickel oxide layered composite film and its preparation method. Graphene and nickel oxide are mixed using an ultrasonic method and then subjected to high-temperature heat treatment to obtain the graphene / nickel oxide layered composite film. The composite film produced by this method has good electrical conductivity and mechanical strength, but requires high-temperature sintering and has a long reaction time. Patent CN102522218A reports a nano-nickel oxide / graphene composite electrode material, its preparation method, and its application. This material primarily utilizes the high electrical conductivity of reduced graphene oxide to reduce the internal resistance of the composite electrode. Its high specific surface area and its ability to function as an electric double-layer capacitor enhance the high-power discharge capability of the composite capacitor. The nano-nickel oxide / graphene composite electrode material has a pore size ranging from 2 to 65 nm and a nano-nickel oxide particle size of 750 nm. Although this method improves the specific capacitance of the composite material to a certain extent, the nano nickel oxide with an average particle size of 750 nm will limit its electrochemical performance.

[0006] The electrodes prepared by existing technologies have low capacity, poor reversibility, and the charging speed of the prepared batteries needs to be further improved, which limits the use of batteries in more fields.

[0007] Summary of the Invention

[0008] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0009] In response to the shortcomings of the existing technology, the present application provides a method for preparing a nano nickel oxide / graphene (NiO-GO) composite electrode material, which can improve the electrode capacity and reversibility. The battery prepared by the electrode material prepared by the present application has the technical effects of faster charging speed and low battery loss, thereby solving at least one technical problem raised in the above background technology and belonging to the field of graphene composite battery technology.

[0010] In order to achieve the above objectives, this application is implemented through the following technical solutions:

[0011] In the first aspect of the present application, a method for modifying NiO NPs on graphene oxide (GO) is provided, wherein NiO NPs are modified on graphene oxide (GO) by a sol-gel method, i.e., a method for preparing a nano nickel oxide / graphene composite electrode material, comprising the following steps:

[0012] (1) dissolving a water-soluble nickel salt, graphene oxide, and gelatin in water to form a water-soluble nickel salt solution, a graphene oxide solution, and a gelatin solution;

[0013] (2) adding a water-soluble nickel salt solution to a graphene oxide solution to form a mixed solution, adding the mixed solution to a gelatin solution, heating and stirring, and obtaining a gel;

[0014] (3) drying the gel to obtain the nano nickel oxide / graphene composite electrode material;

[0015] The mass ratio of the water-soluble nickel salt, graphene oxide and gelatin is 80-200:1:40-125.

[0016] The particle size in the prior art is about 500 nm, while the particle size prepared by the method of the present application is about 10 nm. In the sol-gel method, a reagent must be used to control the particle size. The applicant uses gelatin, and the synthesized nanoparticles have high quality and uniform size, and the gelatin can be removed at 300°C.

[0017] In an exemplary embodiment of the method for modifying NiO NPs on graphene oxide (GO) of the present application, the water-soluble nickel salt is at least one of nickel nitrate, nickel sulfate, nickel acetate, nickel chloride, and nickel sulfite.

[0018] In an exemplary embodiment of the method for modifying NiO NPs on graphene oxide (GO) of the present application, in step (1), when gelatin is dissolved in water, it is dissolved by heating in a water bath and maintaining the temperature at 60-80°C.

[0019] Specifically, the graphene oxide is prepared according to the Hummers method, which includes the following steps: 0.1-2M sulfuric acid solution, 0.1-2M phosphoric acid solution, graphite flakes and potassium permanganate are mixed uniformly by magnetic stirring to obtain a mixed solution, wherein the mass ratio of the sulfuric acid solution, phosphoric acid solution, graphite flakes and potassium permanganate is 50-170:10-50:1:2.67-12; after the color of the mixed solution changes from dark purple-green to dark brown, H2O2 solution is gradually added to cause a racemization reaction; after the reaction lasts for 10-15 minutes, that is, when the color of the mixed solution changes to bright yellow, a reaction solution is obtained; and the supernatant of the reaction solution is centrifuged and washed to obtain the graphene oxide.

[0020] The present application obtains a composite low-rate GO, which is more suitable for industrial production compared to the use of reduced graphene oxide (RGO) to achieve large-capacity work at high rates, and RGO is more expensive than GO.

[0021] In an exemplary embodiment of the method for modifying NiO NPs on graphene oxide (GO) of the present application, the volume concentration of the H2O2 solution is 30%, and the amount of the added H2O2 solution is 30 mL.

[0022] In an exemplary embodiment of the method for modifying NiO NPs on graphene oxide (GO) of the present application, in step (2), the mixed solution is added to the gelatin solution, and the temperature is maintained at 60-80° C. during heating and stirring.

[0023] In an exemplary embodiment of the method for modifying NiO NPs on graphene oxide (GO) of the present application, in step (3), the drying conditions are: heating to 300-350°C at a rate of 20-30°C / min, and maintaining at 300-350°C for 1-3h.

[0024] The present application also provides a nano nickel oxide / graphene composite electrode material prepared by the preparation method.

[0025] The present application also provides the use of the nano nickel oxide / graphene composite electrode material in the preparation of a composite electrode.

[0026] The composite electrode was prepared by mixing 60-80 wt.% NiO / GO powder with 12-18 wt.% acetylene black to prepare a NiO / GO electrode. 8-12 wt.% polyvinylidene fluoride (PVDF) and 1-methyl-2-pyrrolidone (NMP) were used as solvents to prepare a slurry. A clean nickel foil (0.125 mm thick, 1 cm thick) was then placed on the slurry. 2 The slurry was applied to one side of the electrode (area) and dried in air at 80-90°C in a horizontal furnace tube for 12-16 hours. The mass of the NiO / GO composite material coated on each electrode was approximately between 1-2 mg.

[0027] In an exemplary embodiment of the method for preparing the NiO / GO composite electrode of the present application, the amount of 1-methyl-2-pyrrolidone (NMP) is 20 to 35 parts of NMP for every 10 parts of active material. Beneficial effects:

[0028] In summary, the beneficial effects of the preparation method of a NiO-GO composite electrode material provided in this application are:

[0029] 1) By controlling the size and compounding low-rate GO to achieve high capacity, the capacity of the NiO-graphene oxide composite electrode is effectively increased by more than 50%;

[0030] 2) The NiO-graphene oxide composite electrode has better reversibility, and its average reversible potential can be increased by 20mV;

[0031] 3) The NiO / GO composite electrode has a faster charging speed, and the charging time can be effectively shortened by more than 20%.

[0032] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.

[0034] Figure 1 is a diagram of a prefabricated electrode; wherein, a is the various materials used to prepare the electrode, and b is a diagram of the electrode material and the electrode coated with Marcopit.

[0035] Figure 2 shows the electrochemical measurement process of the NiO / GO coating using a three-electrode system; (a) is a potentiostat (Versa STAT 3, AMETEK), and (b) is a three-electrode electrochemical cell.

[0036] FIG3 is an XRD pattern of NiO NPs prepared in Example 1 and the NiO / GO (1%) composite material prepared in Example 3 after calcination at 300° C.

[0037] FIG4 shows the Raman spectra of NiO prepared in Example 1 and NiO / GO prepared in Example 3.

[0038] Figure 5 is a FESEM image of the NiO / GO morphology prepared in Example 3.

[0039] Figure 6 shows the HRTEM images of the NiO / GO nanoparticle structure prepared in Example 3; (a) is a TEM image of NiO NPs modified GO sheet, and (b) is a TEM image of a single NiO nanoparticle attached to a GO sheet.

[0040] Figure 7 shows the electrochemical test of the NiO / GO composite material prepared in Example 5, and the cyclic voltammograms observed for NiO NPs calcined at 300°C at scan rates of 1, 5, 15, 20, and 30 mV / s in 1 M KOH.

[0041] FIG8 is a CV curve of the NiO prepared in Comparative Example 1 and the NiO / GO composite material prepared in Example 5.

[0042] FIG9 is a charge and discharge test diagram of the NiO / GO electrode prepared in Example 5 at different current densities.

[0043] FIG10 is a charge-discharge test diagram of the NiO NPs prepared in Comparative Example 1 and the NiO / GO electrode prepared in Example 5. DETAILED DESCRIPTION

[0044] Example 1

[0045] Preparation of NiO particles

[0046] Dissolve 4g of Ni(NO3)2·6H2O in 20mL of deionized water and stir for 30 minutes. Meanwhile, dissolve 2g of gelatin in 40mL of deionized water and stir at 40°C for 45 minutes to obtain a clear gelatin solution. Then, add the nickel nitrate solution to the gelatin solution and heat it in a 60°C water bath while stirring. Continue stirring for 15 hours to obtain a honey-like and bright green gel. The green gel is then placed in a furnace. The furnace is heated from room temperature to 300°C at a rate of 25°C / min. After maintaining the final temperature for 2 hours, the furnace is naturally cooled to room temperature to obtain nickel oxide nanoparticles (NiO NPs).

[0047] Example 2

[0048] 8g of NiSO4·6H2O was dissolved in 40mL of deionized water and stirred for 45 minutes. Meanwhile, 4g of gelatin was separately dissolved in 80mL of deionized water and stirred at 60°C for 30 minutes to obtain a clear gelatin solution. The nickel sulfate solution was then added to the gelatin solution and heated in an 80°C water bath while stirring. Stirring was continued for 10 hours to obtain a honey-like and bright green gel. The green gel was then placed in a furnace. The furnace was heated from room temperature to 300°C at a rate of 25°C / min. After maintaining the final temperature for 2 hours, the furnace was naturally cooled to room temperature to obtain nickel oxide nanoparticles (NiO NPs).

[0049] Example 3

[0050] The specific steps of the preparation process of nano nickel oxide / graphene composite materials are as follows:

[0051] S1: 320 ml of H2SO4 (0.1 M), 80 ml of H3PO4 (0.1 M), 3 g of graphite flakes and 18 g of KMnO4 were slowly added to the reactor and mixed using a magnetic stirrer to oxidize the graphite. The color of the mixture changed from dark purple-green to dark brown. Then 30 ml of a 30% volume concentration of H2O2 solution was added to stop the oxidation process, and the color of the mixture changed to bright yellow. The formed graphite oxide was washed three times with a 1 M HCl aqueous solution to pH 4-5 and repeatedly washed with deionized water. The washing process was carried out by simply decanting the supernatant using a centrifugal technique. During the washing process with deionized water, the graphite oxide underwent exfoliation, resulting in the thickening of the graphene solution and the formation of GO gel.

[0052] S2: 4 g of Ni(NO3)2·6H2O and 0.04 g of GO were dissolved in 20 mL of deionized water, respectively, and then stirred for 30 minutes. The nickel nitrate solution was then added very slowly to the GO solution. Meanwhile, 2 g of gelatin was dissolved in 40 mL of deionized water, and then stirred at 60°C for 45 minutes to obtain a clear gelatin solution. Afterwards, the nickel nitrate / GO solution was added to the gelatin solution and heated in a 60°C water bath while stirring. Stirring was continued for 15 hours to obtain a honey-like and black gel. The black gel was placed in a furnace, and the furnace was heated from room temperature to 300°C at a rate of 25°C / min. After maintaining the final temperature for 2 hours, the furnace was naturally cooled to room temperature to obtain a nano-nickel oxide / graphene (NiO / GO) composite material.

[0053] Example 4

[0054] NiO NPs modified on graphene oxide (GO).

[0055] S1: 320 ml of H2SO4 (2M), 80 ml of H3PO4 (2M), 3 g of graphite flakes and 18 g of KMnO4 were slowly added to the reactor and mixed using a magnetic stirrer to oxidize the graphite. The color of the mixture changed from dark purple-green to dark brown. Then 30 ml of 30% volume concentration H2O2 solution was added to stop the oxidation process, and the color of the mixture changed to bright yellow, indicating that the oxidation level of the graphite was very high. The formed graphite oxide was washed three times with 1 M HCl aqueous solution to pH 4-5 and repeatedly washed with deionized water. The washing process was carried out by simply decanting the supernatant using a centrifugal technique. During the washing process with deionized water, the graphite oxide underwent exfoliation, resulting in the thickening of the graphene solution and the formation of GO gel.

[0056] S2: 8 g of NiSO4·6H2O and 0.08 g of GO were dissolved in 40 mL of deionized water, respectively, and then stirred for 45 minutes. The nickel sulfate solution was then very slowly added to the GO solution. Meanwhile, 5 g of gelatin was dissolved in 40 mL of deionized water, and then stirred at 80°C for 30 minutes to obtain a clear gelatin solution. The nickel nitrate / GO solution was then added to the gelatin solution and heated in an 80°C water bath while stirring. Stirring was continued for 12 hours to obtain a honey-like and black gel. The black gel was placed in a furnace, and the furnace was heated from room temperature to 350°C at a rate of 25°C / min. After maintaining the final temperature for 2 hours, the furnace was naturally cooled to room temperature to obtain a nano-nickel oxide / graphene (NiO / GO) composite material.

[0057] Example 5

[0058] Figure 1 shows a diagram of the prefabricated electrodes; (a) shows the various materials used to prepare the electrodes, and (b) shows the electrode materials and the electrodes coated with MarcoPit. Figure 2 shows the electrochemical measurement process of the coated NiO / GO using a three-electrode system; (a) shows the potentiostat (Versa STAT 3, AMETEK), and (b) shows the three-electrode electrochemical cell. The specific preparation process is as follows:

[0059] Preparation of NiO / GO composite electrodes.

[0060] NiO / GO electrodes were prepared by mixing 80 wt.% NiO / GO powder (prepared in Example 3) with 18 wt.% acetylene black. A slurry was prepared using 12 wt.% polyvinylidene fluoride (PVDF) and 1-methyl-2-pyrrolidone (NMP) as solvents. A clean nickel foil (0.125 mm thick, 1 cm 2 The slurry was coated on one side of the electrode (area) and dried in air at 90°C in a horizontal furnace for 16 hours to obtain a NiO / GO composite electrode. The mass of the NiO / GO composite coated on each electrode was approximately 2 mg.

[0061] The amount of 1-methyl-2-pyrrolidone (NMP) used was 35 ml of NMP for every 10 g of active material (NiO+acetylene black+PVDF).

[0062] Example 6

[0063] Preparation of NiO / GO composite electrodes.

[0064] NiO / GO electrodes were prepared by mixing 60 wt.% NiO / GO powder (prepared in Example 4) with 18 wt.% acetylene black. A slurry was prepared using 12 wt.% polyvinylidene fluoride (PVDF) and 1-methyl-2-pyrrolidone (NMP) as solvents. A clean nickel foil (0.125 mm thick, 1 cm 2 The slurry was coated on one side of the electrode (area) and dried in air at 90°C in a horizontal furnace for 16 hours to obtain a NiO / GO composite electrode. The mass of the NiO / GO composite coated on each electrode was approximately 2 mg.

[0065] The amount of 1-methyl-2-pyrrolidone (NMP) used was 35 ml of NMP for every 10 g of active material (NiO+acetylene black+PVDF).

[0066] Comparative Example 1

[0067] Preparation of NiO composite electrodes.

[0068] A NiO electrode was prepared by mixing 80 wt.% NiO powder (prepared in Example 1) with 12 wt.% acetylene black, and 8 wt.% polyvinylidene fluoride (PVDF) and 1-methyl-2-pyrrolidone (NMP) were used as solvents to prepare a slurry. A clean nickel foil (0.125 mm thick, 1 cm 2 The slurry was coated on one side of the electrode (area) and dried in air at 80°C in a horizontal furnace for 12 hours to obtain a NiO / GO composite electrode. The mass of the NiO composite material coated on each electrode was approximately 1 mg.

[0069] The amount of 1-methyl-2-pyrrolidone (NMP) used was 20 ml of NMP for every 10 g of active material (NiO+acetylene black+PVDF).

[0070] Test Example 1

[0071] The nano nickel oxide prepared in Example 1 and the NiO / GO prepared in Example 3 were characterized. The XRD patterns of the calcined NiO NPs and the NiO / GO (1%) composite material are shown in FIG3 .

[0072] The Raman spectra of NiO and NiO / GO are shown in Figure 4. The Raman spectra of NiO / GO sample are at 1380 and 1600 cm -1 There are two peaks near the graphene, corresponding to the D and G bands. Usually, the D / G intensity ratio is related to the sp 2 / sp 3 It is related to the carbon ratio and is in an amorphous state.

[0073] The morphology of the NiO / GO composite was studied by recording FESEM, and the results, as shown in Figure 5, showed that the NiO NPs underwent aggregation through vander-Wals interactions. Most of the graphene nanosheets curled up and entangled together to form a layered structure. The TEM image (a) in Figure 6 shows that the NiO NPs were modified on the GO sheets. In addition, the TEM image showed that the average particle size of the nanoparticles was approximately 8.7 nm. Figure 6 (b) shows the HRTEM image of a single NiO NP. It can be seen that the nanoparticles are single crystals with high crystal quality and there are no defects caused by stacking failures. In addition, the HRTEM image shows that the lattice distance is approximately 0.21 nm.

[0074] Test Example 2

[0075] The capacity-enhancing cyclic voltammetry (CV) technique was used to investigate the electrochemical performance of NiO NPs produced by the sol-gel method as electrode materials. Figure 7 shows the cyclic voltammograms observed for NiO NPs calcined at 300 °C at scan rates of 1, 5, 15, 20, and 30 mV / s.

[0076] CV spectra of the NiO / GO electrode at different scan rates show an increase in current density and potential at the oxidation and reduction peaks. The shift in the redox peaks is attributed to the rapid ion / electron diffusion rates and, at higher scan rates, to enhanced polarization and irreversible reactions. This is because the reaction is limited by the ion diffusion rate.

[0077] The cyclic voltammetry obtained for the NiO / GO composite is compared with that for NiO NPs, as shown in Figure 8. The redox peak potentials in the CV patterns are denoted as Ea and Ec, respectively. The NiO / GO electrode was found to exhibit superior reversibility in the Faradaic reaction. Therefore, during the reaction, electrolyte ions can diffuse more easily within the porous structure of the NiO / GO composite compared to NiO NPs.

[0078] Figure 9 shows charge / discharge measurements of the NiO / GO electrode at various current densities and 1 M KOH. The figure shows that increasing the current density reduces the charge / discharge time and increases the potential window. The nonlinear charge / discharge curves confirm the pseudocapacitive behavior of the NiO / GO electrode, which is consistent with the CV results.

[0079] To investigate the effects of graphene oxide and NiO NPs, NiO NPs and NiO / GO electrodes were charged and discharged under identical conditions. As shown in Figure 10, the charge time for NiO / GO was shorter than that for the NiO NPs electrode, and the discharge time for NiO / GO was longer than that for the NiO NPs electrode. The shorter charge time for the NiO / GO electrode is attributed to the presence of graphene, which enhances the conductivity of the electrode material, allowing ions to diffuse faster across the inner and outer pore surfaces of the NiO / GO compared to the NiO NPs electrode.

Claims

1. A method for preparing a nano nickel oxide / graphene composite electrode material, comprising the following steps: (1) dissolving a water-soluble nickel salt, graphene oxide and gelatin in water respectively to form a water-soluble nickel salt solution, a graphene oxide solution and a gelatin solution; (2) adding a water-soluble nickel salt solution to a graphene oxide solution to form a mixed solution, adding the mixed solution to a gelatin solution, heating and stirring, and obtaining a gel; (3) drying the gel to obtain the nano nickel oxide / graphene composite electrode material; Wherein, the mass ratio of the water-soluble nickel salt, graphene oxide and gelatin is 80-200:1:40-125.

2. The method for preparing the nano nickel oxide / graphene composite electrode material according to claim 1, wherein: The water-soluble nickel salt is at least one of nickel nitrate, nickel sulfate, nickel acetate, nickel chloride and nickel sulfite.

3. The method for preparing the nano nickel oxide / graphene composite electrode material according to claim 1 or 2, wherein: In step (1), when gelatin is dissolved in water, it is heated in a water bath and dissolved, and the temperature is maintained at 60-80°C.

4. The method for preparing the nano nickel oxide / graphene composite electrode material according to any one of claims 1 to 3, wherein: The graphene oxide is prepared according to the Hummers method, which includes the following steps: 0.1-2M sulfuric acid solution, 0.1-2M phosphoric acid solution, graphite flakes and potassium permanganate are mixed uniformly by magnetic stirring to obtain a mixed solution, wherein the mass ratio of the sulfuric acid solution, the phosphoric acid solution, the graphite flakes and the potassium permanganate is 50-170:10-50:1:2.67-12, H2O2 solution is gradually added to cause a racemization reaction, and after reacting for 10-15 minutes, a reaction solution is obtained, and the supernatant of the reaction solution is centrifuged and washed to obtain the graphene oxide.

5. The method for preparing the nano nickel oxide / graphene composite electrode material according to claim 4, wherein: The volume concentration of the H2O2 solution is 30%, and the amount of the H2O2 solution added is 30 mL.

6. The method for preparing the nano nickel oxide / graphene composite electrode material according to any one of claims 1 to 5, wherein: In step (2), the mixed solution is added to the gelatin solution, and the temperature is maintained at 60-80° C. during heating and stirring.

7. The method for preparing the nano nickel oxide / graphene composite electrode material according to any one of claims 1 to 6, wherein: In step (3), the drying conditions are: heating to 300-350°C at a rate of 20-30°C / min, and maintaining at 300-350°C for 1-3h.

8. The nano nickel oxide / graphene composite electrode material prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the nano nickel oxide / graphene composite electrode material as claimed in claim 8 in the preparation of a composite electrode.

10. The use according to claim 9, wherein: The preparation method of the composite electrode is as follows: 60-80wt.% of the nano nickel oxide / graphene composite electrode material is uniformly mixed with 12-18wt.% of acetylene black to obtain a mixture, the mixture is mixed with a solvent to prepare a slurry, the slurry is coated on one side of a nickel foil, and the slurry is dried in air at 80-90°C in a horizontal furnace tube for 12-16 hours to prepare a composite electrode, wherein the solvent is polyvinylidene fluoride and 1-methyl-2-pyrrolidone.

Citation Information

Patent Citations

  • Nano nickel oxide / graphene composite electrode material as well as preparation method and application thereof

    CN102522218A

  • Preparation and application of non-enzymatic nickel oxide and reduced graphene oxide composite electrode

    CN109142475A

  • Preparation method and application of gelation-coated electrode material

    CN109920974A

  • Graphene-based negative electrode material and preparation method thereof

    CN112103499A

  • Preparation method of nano nickel oxide / graphene composite electrode material

    CN116443956A