Formed ultra-microporous metal-organic framework material, and preparation method therefor and use thereof in selective adsorption of sulfur hexafluoride

The ultra-microporous metal-organic framework material prepared by the wet granulation method solves the problem of difficult to balance the separation selectivity and adsorption capacity of SF6/N2 or SF6/CF4 in the existing technology, and achieves efficient gas separation and purification. It overcomes the application defects of powder materials and has high selectivity and stability.

WO2024222076A1PCT designated stage expired Publication Date: 2024-10-31ZHEJIANG UNIV

Patent Information

Application Number
PCT/CN2024/073233
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-01-19
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

It is difficult to effectively separate and purify greenhouse gases such as sulfur hexafluoride (SF6) and carbon tetrafluoride (CF4) with existing technologies, especially at low concentrations, and the selection of conventional solid porous adsorbents for SF6/N2 or SF6/CF4 It is difficult to balance performance and adsorption capacity. In practical applications of powder materials, there are problems such as dust pollution, excessive pressure drop in the adsorption tower bed, and pipeline blockage.

Method used

The wet granulation method is used to prepare ultra-microporous metal-organic framework materials. Through the coordination reaction of specific metal ions and fumaric acid derivatives, a material with infinitely extending one-dimensional square pores is formed. Combined with a polyhydroxy binder, the material is improved The stability and mechanical properties enable SF6/N2 or SF6/CF4 separation with high selectivity and high adsorption capacity.

Benefits of technology

It achieves efficient and selective adsorption of sulfur hexafluoride, can separate high-purity nitrogen or carbon tetrafluoride from mixed gases, overcomes the application problems of powder materials, has excellent stability and mechanical properties, and reduces energy consumption. Consumption and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024073233_31102024_PF_FP_ABST
    Figure CN2024073233_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of chemical engineering. A formed ultra-microporous metal-organic framework material, a preparation method therefor and the use thereof in the selective adsorption of sulfur hexafluoride. An ultra-microporous metal-organic framework material, a binder and water are mixed and are subjected to wet granulation to obtain a formed ultra-microporous metal-organic framework material, wherein the binder is one or more of hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyvinyl butyral and kaolin. The ultra-microporous metal-organic framework material is prepared from a soluble metal salt, an organic ligand, an alkali and water by means of mixing and a coordination reaction, wherein metal ions of the soluble metal salt are one or more of Cr3+, Al3+, V3+ and Fe3+, and the organic ligand is fumaric acid or a fumaric acid derivative. The prepared formed ultra-microporous metal-organic framework material has a high SF6 adsorption capacity and good selectivity, and can achieve effective separation of SF6 / N2 or SF6 / CF4.
Need to check novelty before this filing date? Find Prior Art

Description

A molded ultra-microporous metal-organic framework material, a preparation method thereof, and application thereof in selectively adsorbing sulfur hexafluoride

[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on April 26, 2023, with application number CN202310462676.1 and invention name “A shaped ultra-microporous metal-organic framework material, its preparation method and application for selective adsorption of sulfur hexafluoride”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of chemical engineering technology, and in particular to a molded ultra-microporous metal-organic framework material, a preparation method thereof, and an application thereof in selectively adsorbing sulfur hexafluoride. Background Art

[0003] Sulfur hexafluoride (SF6) is the most potent greenhouse gas, with a global warming potential approximately 23,900 times that of carbon dioxide (CO2), and it can remain in the atmosphere for up to 3,200 years. Because SF6 is non-toxic and has excellent dielectric and arc-extinguishing properties, it is also widely used in the electronics industry. Pure SF6 gas is relatively expensive, so industry typically mixes SF6 with a certain proportion of nitrogen (N2) to reduce the impact of the greenhouse effect and lower costs while maintaining dielectric properties comparable to pure SF6. Accordingly, efficient separation and recovery of SF6 from scrapped devices or industrial exhaust gases is crucial to improving overall economic efficiency and environmental sustainability.

[0004] In addition to SF6, another greenhouse gas, carbon tetrafluoride (CF4), is also one of the most widely used plasma etching gases in the electronics industry. It is mainly used for etching thin film materials such as silicon, silicon dioxide, and silicon nitride. It is also used for electronic device surface cleaning, low-temperature refrigeration, gas insulation, etc. The direct fluorocarbon synthesis method is the main method for preparing CF4 in industry. However, the crude CF4 product obtained by this method also contains impurity components such as hydrofluoric acid (HF), fluorine gas (F2), and sulfur hexafluoride (SF6), which cannot meet the use standards of electronic grade CF4. Therefore, CF4 needs to be further purified to reach a purity of more than 99.999%. Among them, acidic impurities such as HF and F2 can be removed by water washing and alkali washing, while SF6 and CF4 have similar properties (both are relatively inert), and their molecular shapes and sizes are similar (the molecular dynamic diameters are respectively and ), whose separation is extremely challenging.

[0005] In industry, the difference in boiling points between SF6 and other gases is used to achieve effective separation of SF6 / N2 or SF6 / CF4 through low-temperature distillation, liquefaction, etc. However, the temperature change process involved in these technologies requires a lot of energy consumption, which is very uneconomical, especially when the SF6 concentration is low. In contrast, adsorption separation technology that does not involve phase change processes is more energy-efficient and clean, and has more significant advantages in separating low-concentration SF6. Conventional solid porous adsorbents show a certain SF6 adsorption capacity, such as molecular sieve materials MFI-1 and MFI-2 (pore size The adsorption capacity of 13X molecular sieve (pore size) at 25 ° C and 10 kPa is 0.86 mmol / g and 0.70 mmol / g respectively (Journal of Industrial and Engineering Chemistry, 2018, 62: 64-71). ) can also achieve an SF6 adsorption capacity of 0.97mmol / g (Chemical Engineering Journal, 2015, 262: 683-690). However, due to the lack of diversity in their pore structures, it is difficult for these materials to significantly improve their affinity for SF6, and the adsorption capacity is still not high enough. At the same time, since the molecular sizes of these gases are similar, for example, the molecular kinetic diameters of SF6 and CF4 differ by only Conventional adsorption materials are difficult to achieve highly selective separation. Therefore, there is an urgent need to develop new and efficient adsorption materials and adsorption separation methods.

[0006] In recent years, metal-organic frameworks (MOFs) have shown great potential in gas separation due to their diverse pore structures and finely tuned properties. However, for SF6 / N2 or SF6 / CF4 separations, the MOFs reported so far still struggle to balance selectivity and adsorption capacity. Furthermore, these MOFs are all powder materials, which present numerous challenges in actual use, including dust contamination, excessive pressure drop in the adsorption tower bed, pipeline blockage, and transportation difficulties. Furthermore, once these powder materials are formed, their selectivity and adsorption capacity often decrease further due to pore blockage and partial collapse of the skeleton structure.

[0007] Summary of the Invention

[0008] In view of this, the present application aims to provide a molded ultra-microporous metal-organic framework material, a preparation method thereof, and an application thereof for selectively adsorbing sulfur hexafluoride. The molded ultra-microporous metal-organic framework material prepared in this application has a high adsorption capacity for SF6 and good selectivity, enabling effective separation of SF6 / N2 or SF6 / CF4.

[0009] In order to achieve the above application objectives, this application provides the following technical solutions:

[0010] The present application provides a method for preparing a molded ultra-microporous metal-organic framework material, comprising the following steps:

[0011] The ultra-microporous metal-organic framework material, a binder and water are mixed and wet granulated to obtain the shaped ultra-microporous metal-organic framework material; the binder is one or more of hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyvinyl butyral and kaolin;

[0012] The ultra-microporous metal-organic framework material is prepared by mixing a soluble metal salt, an organic ligand, an alkali and water and performing a coordination reaction; the metal ion in the soluble metal salt is Cr 3+ 、Al 3+ 、V 3+ and Fe 3+ One or more of the following; the organic ligand is fumaric acid or a fumaric acid derivative.

[0013] Preferably, the mass of the binder is 0.1 to 15% of the sum of the mass of the binder and the ultra-microporous metal-organic framework material.

[0014] Preferably, the particle size of the molded ultramicroporous metal-organic framework material is 1 to 2 mm.

[0015] Preferably, the fumaric acid derivative has the structure shown in Formula I:

[0016] In formula I, R1 and R2 are independently selected from H, F, Cl, Br, I or CH3, and R1 and R2 are not H at the same time.

[0017] Preferably, the base is sodium hydroxide; and the molar ratio of the metal ions in the organic ligand and the soluble metal salt to the base is 1-2:2:4-8.

[0018] Preferably, the ultra-microporous metal-organic framework material has infinitely extended periodic one-dimensional square channels with a pore size of

[0019] The present application provides a shaped ultra-microporous metal-organic framework material prepared by the preparation method described in the above technical solution.

[0020] The present application provides the use of the molded ultra-microporous metal-organic framework material described in the above technical solution to selectively adsorb sulfur hexafluoride from a mixed gas; the mixed gas includes sulfur hexafluoride and nitrogen or sulfur hexafluoride and carbon tetrafluoride.

[0021] Preferably, the volume ratio of sulfur hexafluoride to nitrogen or sulfur hexafluoride to carbon tetrafluoride in the mixed gas is 99:1 to 1:99.

[0022] Preferably, the adsorption is one or more of fixed bed adsorption, fluidized bed adsorption and moving bed adsorption; the adsorption temperature is -20 to 60° C., and the pressure is 0.5 to 10 bar.

[0023] The present application provides a preparation method of a molded ultra-microporous metal-organic framework material, comprising the following steps: mixing an ultra-microporous metal-organic framework material, a binder and water and performing wet granulation to obtain the molded ultra-microporous metal-organic framework material; the binder is one or more of hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyvinyl butyral and kaolin; the ultra-microporous metal-organic framework material is prepared by mixing a soluble metal salt, an organic ligand, an alkali and water and performing a coordination reaction; the metal ion in the soluble metal salt is Cr 3+ 、Al 3+ 、V 3+ and Fe 3+ One or more of; the organic ligand is fumaric acid or a fumaric acid derivative. The present application synthesizes ultra-microporous metal-organic framework materials with specific metal ions and carboxylic acid organic ligands of specific sizes. Compared with conventional adsorbents and other MOFs materials, the ultra-microporous metal-organic framework materials have stronger SF6 affinity (the adsorption capacity for SF6 under equilibrium conditions is significantly higher than that of N2 or CF4) and significantly improved SF6 selectivity, and can achieve effective separation of sulfur hexafluoride and nitrogen mixed gas (SF6 / N2) or sulfur hexafluoride and carbon tetrafluoride mixed gas (SF6 / CF4); the present application prepares a molded ultra-microporous metal-organic framework material by granulation with a specific binder. The molded material still maintains almost the same specific surface area and SF6 adsorption and separation performance as the original metal-organic framework material, and has a complete surface morphology and excellent mechanical properties, overcoming many problems of the currently used powder materials, such as dust pollution, excessive pressure drop in the adsorption tower bed, pipeline blockage, and transportation difficulties. Furthermore, this application significantly improves the stability of the formed ultraporous metal-organic framework material through hydrogen bonding interactions between the polyhydroxy binder and the ultraporous metal-organic framework material. Furthermore, the preparation method provided in this application offers outstanding advantages such as mild operating conditions, energy conservation and environmental protection, and low equipment investment. Furthermore, the raw material cost is low, potentially bringing economic benefits to small and medium-sized enterprises.

[0024] The present application provides a shaped ultra-microporous metal-organic framework material prepared by the preparation method described in the above technical solution. The shaped ultra-microporous metal-organic framework material provided in the present application has the advantages of large adsorption capacity for sulfur hexafluoride, high selectivity, and recyclability, and has excellent stability and a thermal decomposition temperature of nearly 400°C. The shaped ultra-microporous metal-organic framework material is used to selectively adsorb sulfur hexafluoride from a mixture of sulfur hexafluoride and nitrogen or a mixture of sulfur hexafluoride and carbon tetrafluoride, and nitrogen or carbon tetrafluoride gas with a purity of up to 99.999% and sulfur hexafluoride gas with a purity of up to 99.99% can be obtained at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] FIG1 is an adsorption isotherm diagram of the ultra-microporous metal-organic framework material Al(fum) obtained in Example 1 for SF6, CF4 and N2 at 298K;

[0026] FIG2 is an adsorption isotherm diagram of the ultra-microporous metal-organic framework material Al(fum) obtained in Example 1 for SF6, CF4 and N2 at 273K;

[0027] FIG3 is a fixed-bed penetration curve of the ultra-microporous metal-organic framework material Al(fum) in Example 2 for a mixed gas of SF6 / N2 (volume ratio of 10:90) and a mixed gas of SF6 / CF4 (volume ratio of 4:96) at 273K and 298K; FIG3A is a fixed-bed penetration curve for a mixed gas of SF6 / N2 (volume ratio of 10:90), and FIG3B is a fixed-bed penetration curve for a mixed gas of SF6 / CF4 (volume ratio of 4:96);

[0028] Figure 4 is a fixed-bed desorption curve of the ultra-microporous metal-organic framework material Al(fum) in Example 2 at 298K after saturation adsorption of SF6 / N2 (volume ratio 10:90) mixed gas and SF6 / CF4 (volume ratio 4:96) mixed gas; In Figure 4, A is a fixed-bed desorption curve after saturation adsorption of SF6 / N2 (volume ratio 10:90) mixed gas, and B is a fixed-bed desorption curve after saturation adsorption of SF6 / CF4 (volume ratio 4:96) mixed gas;

[0029] FIG5 shows the SF6 dynamic adsorption capacity of the ultra-microporous metal-organic framework material Al(fum) in Example 2 after five adsorption-desorption cycles of SF6 / N2 (volume ratio 10:90) mixed gas at 298K;

[0030] Figure 6 is a comparison of the morphologies of the molded materials obtained by molding the ultramicroporous metal-organic framework material with different binders in Example 3; in Figure 6, A is Al(fum)@5%HPC, B is Al(fum)@2%HPC, C is Al(fum)@5%PVA, D is Al(fum)@2%PVA, E is Al(fum)@10% sucrose, and F is Al(fum)@5% sucrose;

[0031] FIG7 is a thermogravimetric graph of the ultra-microporous materials Al(fum)@2%HPC and Al(fum)@5%HPC obtained in Example 4 and Example 5;

[0032] FIG8 is a thermogravimetric graph of the ultra-microporous materials Al(fum)@2%PVA and Al(fum)@5%PVA obtained in Examples 6 and 7;

[0033] FIG9 is an X-ray diffraction pattern of the ultra-microporous materials obtained in Examples 4, 5, 6 and 7;

[0034] Figure 10 is an adsorption isotherm diagram of N2 at 77K for the molded ultraporous materials Al(fum)@2%HPC and Al(fum)@2%PVA obtained in Examples 4 and 6; Figure 10A is an adsorption isotherm diagram of N2 at 77K for the molded ultraporous material Al(fum)@2%HPC, and Figure 10B is an adsorption isotherm diagram of N2 at 77K for the molded ultraporous material Al(fum)@2%PVA;

[0035] FIG11 is a diagram showing the wear test results of the ultra-microporous materials obtained in Examples 4, 5, 6, and 7;

[0036] FIG12 is an adsorption isotherm diagram of SF6, CF4 and N2 of the formed ultra-microporous material Al(fum)@2%HPC obtained in Example 4 at 298K;

[0037] FIG13 is a fixed-bed penetration curve of the ultra-microporous material Al(fum)@2%HPC formed in Example 8 for a mixed gas of SF6 / N2 (volume ratio of 10:90) and a mixed gas of SF6 / CF4 (volume ratio of 4:96) at 273K and 298K; FIG13A is a fixed-bed penetration curve for a mixed gas of SF6 / N2 (volume ratio of 10:90), and FIG13B is a fixed-bed penetration curve for a mixed gas of SF6 / CF4 (volume ratio of 4:96);

[0038] FIG14 is a fixed-bed desorption curve of the ultra-microporous material Al(fum)@2%HPC formed in Example 8 after saturation adsorption of SF6 / N2 (volume ratio 10:90) mixed gas and SF6 / CF4 (volume ratio 4:96) mixed gas at 298K; FIG14A is a fixed-bed desorption curve after saturation adsorption of SF6 / N2 (volume ratio 10:90) mixed gas, and FIG14B is a fixed-bed desorption curve after saturation adsorption of SF6 / CF4 (volume ratio 4:96) mixed gas;

[0039] Figure 15 is a graph showing the dynamic adsorption capacity of SF6 for the ultra-microporous material Al(fum)@2%HPC formed in Example 8 after four adsorption-desorption cycles of SF6 / N2 (volume ratio 10:90) mixed gas at 298K. DETAILED DESCRIPTION

[0040] The present application provides a method for preparing a molded ultra-microporous metal-organic framework material, comprising the following steps:

[0041] The ultra-microporous metal-organic framework material, a binder and water are mixed and wet granulated to obtain the shaped ultra-microporous metal-organic framework material; the binder is one or more of hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyvinyl butyral and kaolin;

[0042] The ultra-microporous metal-organic framework material is prepared by mixing a soluble metal salt, an organic ligand, an alkali and water and performing a coordination reaction; the metal ion in the soluble metal salt is Cr 3+ 、Al 3+ 、V 3+ and Fe 3+ One or more of the following; the organic ligand is fumaric acid or a fumaric acid derivative.

[0043] This application first describes the ultra-microporous metal-organic framework material.

[0044] In the present application, the ultra-microporous metal-organic framework material is prepared by mixing a soluble metal salt, an organic ligand, a base and water through a coordination reaction. In the present application, the metal ion in the soluble metal salt is Cr 3+ 、Al 3+ 、V 3+ and Fe 3+ One or more of the following, preferably Al 3+, the soluble metal salt is preferably a sulfate, carbonate or nitrate of the metal ion. In the present application, the organic ligand is fumaric acid or a fumaric acid derivative, and the fumaric acid derivative preferably has a structure shown in Formula I, wherein R1 and R2 are independently selected from H, F, Cl, Br, I or CH3, and R1 and R2 are not H at the same time; in the embodiments of the present application, the R1 and R2 are preferably independently selected from H or CH3. The present application has no special requirements for the source of the fumaric acid derivative, and it can be prepared using commercial products well known to those skilled in the art or using preparation methods well known to those skilled in the art. In the present application, the base is preferably sodium hydroxide; the molar ratio of the metal ion to the base in the organic ligand and the soluble metal salt is preferably 1-2:2:4-8, more preferably 2:2:6. The present application has no special requirements for the amount of water used, as long as it can achieve sufficient dissolution of each component.

[0045] In the present application, the coordination reaction can adopt the interfacial slow diffusion method or the solvent stirring method. In the present application, the specific operation of the interfacial slow diffusion method is preferably: mixing the organic ligand, alkali and part of the water to obtain a first mixed solution; mixing the soluble metal salt with the remaining water to obtain a second mixed solution; adding the first mixed solution dropwise to the second mixed solution, and then standing at 0 to 25°C for coordination reaction; the dropping speed is preferably 2 to 3 mL / min; the time of the coordination reaction (i.e., the standing time) is preferably 7 to 21 days. In the present application, the specific operation of the solvent stirring method is preferably: mixing the organic ligand, alkali and part of the water to obtain a third mixed solution; mixing the soluble metal salt with the remaining water to obtain a fourth mixed solution; stirring the third mixed solution and the fourth mixed solution to carry out coordination reaction; the temperature of the coordination reaction is preferably 25 to 85°C, more preferably 60°C, the time is preferably 0.1 to 24h, more preferably 2h, and the stirring rate is preferably 200 to 800r / min, more preferably 600r / min. In the present application, after the coordination reaction is completed, the obtained coordination reaction solution is preferably filtered, the solid phase is washed with water and dried in sequence, and the drying temperature is preferably 60°C.

[0046] During the coordination reaction, the metal ions (denoted as M) in the soluble metal salt aqueous solution, the organic ligands of fumaric acid and its derivatives (denoted as L) and the μ-OH provided by the base are coordinated through coordination bonds. Specifically, the metal ion M acts as a six-coordinate central node and coordinates with the four carboxyl oxygen atoms of the organic ligand L and the oxygen atoms on the two μ-OH of the base to form a MO6 spatial octahedral structure, which is connected through the dicarboxylic acid organic ligand L to form a periodic one-dimensional square channel with infinite extension and a pore size of There is a high density of -OH polar sites distributed on the pore surface, and the product formed by the coordination reaction (i.e., ultra-microporous metal-organic framework material) has a general structural formula expressed as M(OH)L.

[0047] The present invention synthesizes ultra-microporous metal-organic framework materials with specific metal ions and specific size carboxylic acid organic ligands. The ultra-microporous metal-organic framework materials have a kinetic diameter close to that of SF6. The pore size can enhance the confinement effect of molecules in the confined pores, and the high-density -OH polar sites distributed on the pore surface can effectively identify the polarizability differences among SF6, N2, and CF4 molecules (the polarizability is 65.4×10 -25 cm 3 、38.4×10 -25 cm 3 and 17.4×10 -25 cm 3 ), thus being able to selectively and efficiently identify SF6 molecules and obtain a strong affinity for them, significantly improving the material's adsorption and separation selectivity for SF6 and N2, as well as SF6 and CF4, and achieving highly selective and high-capacity SF6 / N2 and SF6 / CF4 separation effects. For example, in an embodiment of the present application, an ultra-microporous MOF material with the structural formula of Al(OH)(C4H2O4) (abbreviated as Al(fum)) hardly adsorbs N2 (0.24mmol / g, 298K and 100kPa conditions), while the adsorption capacity for SF6 under the corresponding conditions is as high as 3.50mmol / g, and the adsorption capacity for SF6 at low pressure reaches a record 2.77mmol / g (10kPa), and the IAST (Ideal Adsorbed Solution Theory) selectivity for a SF6 / N2 mixed gas with a volume ratio of 10:90 is as high as 1610, which is much higher than other adsorbents.

[0048] The following is a detailed description of the method for preparing the ultra-microporous metal-organic framework material of the present application.

[0049] In the present application, the ultraporous metal-organic framework material, a binder, and water are mixed and wet granulated to obtain the shaped ultraporous metal-organic framework material. In the present application, the binder is one or more of hydroxyethyl cellulose (HEC), hydroxypropyl cellulose (HPC), polyvinyl alcohol (PVA), polyvinyl butyral (PVB), and kaolin, preferably hydroxypropyl cellulose or polyvinyl alcohol. The present application has no particular requirements for the source of the binder; commercially available products familiar to those skilled in the art can be used. In the present application, the mass of the binder is preferably 0.1-15% of the combined mass of the binder and the ultraporous metal-organic framework material, more preferably 2-10%, and even more preferably 2-5%; the water is preferably deionized water. In the present application, the specific mixing operation is preferably: the ultraporous metal-organic framework material and the binder are placed in a mortar and ground and mixed uniformly, and water is added in small amounts and multiple times during the grinding and stirring until the mixture becomes a paste. The present application has no particular requirements for the amount of water used; it only needs to be able to form a paste. In the present application, the wet granulation method specifically involves extruding the semi-dried paste into spherical particles. The particle size of the formed ultraporous metal-organic framework material is preferably 1-2 mm. In the examples of the present application, the formed ultraporous metal-organic framework material is expressed as M(OH)L@x%B, where B represents the binder and x% represents the percentage of the binder mass to the total mass of the binder and the ultraporous metal-organic framework material.

[0050] The present application prepares a molded ultra-microporous metal-organic framework material by granulating with a specific binder, which can still retain the porous structure, rich action sites and excellent stability of the original ultra-microporous metal-organic framework material that matches the size of SF6, that is, it still maintains excellent SF6 adsorption and separation performance after molding. For example, in the embodiment of the present application, the ultra-microporous MOF material with the structural formula of Al(OH)(C4H2O4) (abbreviated as Al(fum)) is molded by adding 2wt% hydroxypropyl cellulose (HPC) as a binder. The specific surface area of ​​the particles after molding (Al(fum)@2%HPC) is basically the same as that before molding (the specific surface area of ​​Al(fum)@2%HPC after molding is 999m 2 / g, the specific surface area of ​​Al(fum) before molding is 1040m 2 / g), and at 298K and 10kPa, the SF6 adsorption capacity of Al(fum)@2% HPC was 2.67mmol / g, a decrease of only 3.5% compared to Al(fum) powder (2.77mmol / g), indicating that the molded particles still have excellent SF6 adsorption performance. Furthermore, the binder molding method can produce molded particles with complete surface morphology, suitable particle size, and improved mechanical properties, providing strong support for the long-term and stable industrial application of the material.

[0051] This application provides a molded ultra-microporous metal-organic framework material prepared by the preparation method described in the above technical solution. The molded ultra-microporous metal-organic framework material provided in this application has the advantages of large sulfur hexafluoride adsorption capacity, high selectivity, recyclability, and excellent stability, with a thermal decomposition temperature of nearly 400°C.

[0052] The present application provides the use of the shaped ultra-microporous metal-organic framework material described in the above technical solution for selectively adsorbing sulfur hexafluoride from a mixed gas; the mixed gas includes sulfur hexafluoride and nitrogen or sulfur hexafluoride and carbon tetrafluoride. In the present application, the volume ratio of sulfur hexafluoride to nitrogen or sulfur hexafluoride to carbon tetrafluoride in the mixed gas is preferably 99:1 to 1:99, and more preferably 4:96 to 10:90. In the present application, when the shaped ultra-microporous metal-organic framework material is used as an adsorbent and comes into contact with a mixed gas containing sulfur hexafluoride and nitrogen or a mixed gas containing sulfur hexafluoride and carbon tetrafluoride, the adsorbent selectively adsorbs sulfur hexafluoride molecules due to the difference in molecular size and polarizability between sulfur hexafluoride and nitrogen or carbon tetrafluoride, thereby achieving separation of sulfur hexafluoride and nitrogen or sulfur hexafluoride and carbon tetrafluoride; the mixed gas may also contain impurities such as oxygen, carbon dioxide, and moisture, which do not affect the adsorption and separation performance of the shaped ultra-microporous metal-organic framework material for sulfur hexafluoride.

[0053] In the present application, the adsorption is preferably one or more of fixed bed adsorption, fluidized bed adsorption, and moving bed adsorption, preferably fixed bed adsorption; the specific operation of the fixed bed adsorption is preferably: at a set adsorption temperature and adsorption pressure, the mixed gas is passed into a fixed bed adsorption column filled with the molded ultra-microporous metal-organic framework material, the nitrogen or carbon tetrafluoride component in the mixed gas has a weak interaction with the molded ultra-microporous metal-organic framework material, the adsorption amount is relatively small, and it preferentially penetrates the bed layer, and nitrogen or carbon tetrafluoride gas with a sulfur hexafluoride content of less than 0.01 vol% is directly obtained from the outlet of the adsorption column. The sulfur hexafluoride component has a strong interaction with the molded ultra-microporous metal-organic framework material and is enriched in the bed layer. In the present application, after the sulfur hexafluoride is adsorbed to saturation, it can be desorbed to obtain sulfur hexafluoride-rich gas (high-purity sulfur hexafluoride gas with a purity greater than 99.99%). In the present application, the adsorption temperature is preferably -20 to 60°C, and the pressure is preferably 0.5 to 10 bar; lowering the adsorption temperature is beneficial to increasing the adsorption capacity of sulfur hexafluoride, and increasing the adsorption temperature is beneficial to narrowing the temperature difference between the adsorption process and the desorption process, reducing the energy consumption required for the separation process, and increasing the diffusion rate of sulfur hexafluoride in the pores. Therefore, taking the above two factors into consideration, the adsorption temperature is further preferably 0 to 35°C, and the pressure is further preferably 1 to 5 bar.

[0054] In the present application, the desorption method can be desorption by reducing pressure and heating, desorption by heating and purging with inert gas at normal pressure, or a combination of multiple desorption methods; the desorption temperature of the desorption by reducing pressure and heating is preferably 25 to 120°C, more preferably 25 to 40°C, and the desorption pressure is preferably 0.000001 to 0.1 bar. The desorption temperature of the desorption by heating and purging with inert gas at normal pressure is preferably 25 to 120°C, more preferably 25 to 40°C.

[0055] The following describes in detail the shaped ultra-microporous metal-organic framework material provided by the present application, its preparation method, and its application in selective adsorption of sulfur hexafluoride with reference to the examples. However, these examples should not be construed as limiting the scope of protection of the present application.

[0056] Example 1

[0057] 1.05 mmol of aluminum sulfate 18hydrate (0.7 g) was weighed and dissolved in 6 mL of deionized water, preheated to 60°C, designated as Solution A. Separately, 2.1 mmol of fumaric acid (0.243 g) and 6.3 mmol of sodium hydroxide (0.252 g) were weighed and dissolved in 7.2 mL of deionized water, preheated to 60°C, designated as Solution B. The preheated Solution B was mixed with the preheated Solution A, stirred at 60°C for 2 hours, and then filtered. The filtered solid product was washed with deionized water and then dried at 60°C to obtain a white powder, the ultramicroporous metal-organic framework material, designated as Al(fum). The yield based on aluminum was 89% (292 mg).

[0058] The synthesized powder material was vacuum degassed at 120°C for 24 hours, with a degassing pressure below 5 μmHg. Single-component static adsorption isotherms for SF6, CF4, and N2 were then measured on a Micrometrics ASAP 2460 adsorption instrument at 273K and 298K, respectively.

[0059] The adsorption isotherms of the ultra-microporous metal-organic framework material Al(fum) obtained in this example for SF6, CF4, and N2 at 298K are shown in Figure 1. The material has a high SF6 adsorption capacity (3.50 mmol / g) at room temperature and pressure, while almost no N2 adsorption. The adsorption capacity of SF6 at a low pressure (10 kPa) reaches a record high of 2.77 mmol / g. After calculation, the IAST (Ideal Adsorbed Solution Theory) selectivity of the material for a SF6 / N2 gas mixture with a volume ratio of 10:90 is 1610. The adsorption isotherms of the ultra-microporous metal-organic framework material Al(fum) obtained in this example for SF6, CF4, and N2 at 273K are shown in Figure 2. The material has a high SF6 adsorption capacity (3.77 mmol / g) at 273K and 1 bar, while almost no N2 adsorption.

[0060] Example 2

[0061] The ultra-microporous metal-organic framework material Al(fum) powder (0.57 g) obtained in Example 1 was loaded into a 5 cm long fixed bed adsorption column, and SF6 / N2 (volume ratio 10:90) mixed gas or SF6 / CF4 (volume ratio 4:96) mixed gas was introduced into the adsorption column at a flow rate of 2.7 mL / min at 273 K or 298 K, and high-purity N2 or CF4 (purity greater than 99.999%) was obtained in the outflowing gas, respectively; when SF6 penetrated (adsorption saturation), the adsorption was stopped, and He gas was purged at 40°C for 10 h for desorption to obtain high-purity SF6 (purity greater than 99.99%), and the adsorption column could be recycled.

[0062] The penetration curves of the ultra-microporous metal-organic framework material Al(fum) powder of this example are shown in Figure 3, where the mixed gas flow rate is 2.7 mL / min, C represents the component concentration of the raw material at the outlet of the adsorption column, and C0 represents the initial concentration of the raw material. For the SF6 / N2 (10:90) gas mixture, the N2 component rapidly penetrates at different temperatures, and the SF6 component retention time reaches 171 min / g (298 K) and 190 min / g (273 K), indicating that the ultra-microporous metal-organic framework material has a high dynamic SF6 adsorption capacity and almost no N2 adsorption. For the SF6 / CF4 (4:96) gas mixture, the CF4 component rapidly penetrates at different temperatures, and the SF6 component retention time reaches 310 min / g (298 K) and 363 min / g (273 K), also indicating that the material has a high dynamic SF6 adsorption capacity. High-purity SF6 (purity greater than 99.99%) can be obtained by desorption under the conditions of 40°C and 6.0 mL He gas purge. The desorption curve is shown in Figure 4, and the dynamic SF6 adsorption capacity of the material does not decrease significantly after 5 cycles (as shown in Figure 5).

[0063] Example 3

[0064] Three polyhydroxyl materials, hydroxypropyl cellulose (HPC), polyvinyl alcohol (PVA), and sucrose, were selected as binders (sucrose was used as a control) and mixed uniformly with the ultra-microporous metal-organic framework material Al(fum) powder prepared in Example 1 in a mortar. The total mass of the binder and powder material was 1g, and the binder mass percentages were 2% / 5% (HPC), 2% / 5% (PVA), and 5% / 10% (sucrose), respectively. 2mL of deionized water was added in small amounts and stirred until it became a paste. After it was semi-dry, it was extruded into spherical particles with a particle size of 1-2mm. The molding material was recorded as Al(fum)@x%B, where B represents the binder and x% represents the percentage of the binder mass to the total mass of the binder and metal-organic framework material.

[0065] The surface morphologies of the six prepared molding materials are shown in Figure 6. In Figure 6, A is Al(fum)@5% HPC, B is Al(fum)@2% HPC, C is Al(fum)@5% PVA, D is Al(fum)@2% PVA, E is Al(fum)@10% sucrose, and F is Al(fum)@5% sucrose. The molding results differed among the three materials. HPC and PVA both achieved good molding results, while sucrose produced poorer results. For example, using HPC as a binder at a binder dosage of 5% facilitated the molding process, resulting in well-formed, smooth, and resistant particles. When the binder dosage was reduced to 2%, intact particles were still formed. Using PVA as a binder, since PVA is insoluble in water at room temperature, it must be dissolved in hot water to form a solution before further use. This process is slightly more complex than with HPC. However, both 5% and 2% binder dosages still produced particles with good morphology and smooth surfaces. When sucrose is used as a binder, due to its weak viscosity, it is difficult to form stable particles when the binder dosage is 5%, and it is very easy to break. When the binder dosage is increased to 10%, the viscosity increases and particles can be formed, but the surface is not smooth enough and there are obvious cracks.

[0066] Example 4

[0067] 980 mg of the ultraporous metal-organic framework material Al(fum) powder (undegassed) prepared in Example 1 and 20 mg of hydroxypropyl cellulose (HPC) were weighed and mixed in a mortar. 2 mL of deionized water was added in small portions and stirred until it became a paste. After it was semi-dry, it was extruded into spherical particles with a particle size of 1 to 2 mm. After drying, the resulting ultraporous metal-organic framework material, namely Al(fum)@HPC particles with a binder mass fraction of 2%, was obtained, denoted as Al(fum)@2%HPC.

[0068] The thermogravimetric curve of the molded ultra-microporous metal-organic framework material Al(fum)@2%HPC obtained in this embodiment is shown in FIG7 , and it can be seen that the material still maintains excellent thermal stability after molding.

[0069] X-ray diffraction analysis of the molded ultraporous metal-organic framework material, Al(fum)@2%HPC, is shown in Figure 9. As can be seen from Figure 9, the peak shape of the material molded with 2% HPC as a binder is consistent with that of the ultraporous metal-organic framework powder material, demonstrating that the Al(fum)@2%HPC framework structure remains intact after molding.

[0070] The Al(fum)@2%HPC shaped granular material was placed in a vacuum degassing at 120°C for 24 hours with a degassing pressure below 5μmHg. Then, the single-component static adsorption isotherm of N2 was tested on a Micrometrics ASAP 2460 adsorption instrument at a test temperature of 77K. Test results: The adsorption isotherm of N2 for the shaped ultra-microporous material Al(fum)@2%HPC obtained in this example at 77K is shown in Figure 10A. After molding, the N2 adsorption curve of the material is consistent with the adsorption curve of the ultra-microporous metal-organic framework material powder, and the specific surface area remains basically unchanged (Al(fum)@2%HPC: 999m 2 / g, Al(fum):1040m 2 / g).

[0071] Single-component static adsorption isotherms for SF6, CF4, and N2 were measured on a Micrometrics ASAP 2460 adsorption instrument at 298K. The results are shown in Figure 12. The SF6 adsorption curve for Al(fum)@2% HPC particles remains very steep at low pressure, with the SF6 adsorption capacity remaining at 2.67 mmol / g at 298K and 10 kPa. The SF6 adsorption capacity at 273K is slightly higher than that at 298K, reaching 3.04 mmol / g at 10 kPa, a decrease of approximately 5% compared to the powder (3.20 mmol / g). The CF4 adsorption capacity of Al(fum)@2% HPC particles also decreased. For example, at 100 kPa, the CF4 adsorption capacity at 298K was 1.73 mmol / g, a 6.5% decrease compared to the powder. However, the Al(fum)@2% HPC particles still exhibited very low N2 adsorption, for example, at 100 kPa and 298 K, the N2 adsorption was 0.23 mmol / g, essentially unchanged from the original powder. This indicates that the formed Al(fum)@2% HPC particles still possess excellent SF6 / N2 and SF6 / CF4 separation potential.

[0072] 200 mg of the molded Al(fum)@2% HPC particles were weighed and placed in a conical flask. The flask was then placed in an oscillating incubator at 25°C and 300 rpm, and the mass change of the particles was recorded, as shown in Figure 11. This shows that the molded Al(fum)@2% HPC particles have good mechanical properties, with a mass loss of less than 0.4% after 24 hours.

[0073] Example 5

[0074] 950 mg of the ultraporous metal-organic framework material Al(fum) powder (undegassed) prepared in Example 1 and 50 mg of hydroxypropyl cellulose (HPC) were weighed and mixed in a mortar. 2 mL of deionized water was added in small amounts and stirred until it became a paste. After it was semi-dry, it was extruded into spherical particles with a particle size of 1 to 2 mm. After drying, the resulting ultraporous metal-organic framework material, namely Al(fum)@HPC particles with a binder mass fraction of 5%, was obtained, which were recorded as Al(fum)@5%HPC.

[0075] The thermogravimetric curve of the molded ultra-microporous material Al(fum)@5%HPC obtained in this embodiment is shown in FIG7 . It can be seen that the material still maintains excellent thermal stability after molding.

[0076] X-ray diffraction analysis of the Al(fum)@5%HPC ultraporous material was performed, and the results are shown in Figure 9. As can be seen from Figure 9, the peak shape of the material formed with 5% HPC as a binder remains consistent with that of the powder material, demonstrating that the Al(fum)@5%HPC framework structure remains intact after forming.

[0077] 200 mg of the molded Al(fum)@5% HPC was weighed and placed in a conical flask. The flask was then placed in a shaking incubator at 25°C and 300 rpm, and the mass change of the particles was recorded, as shown in Figure 11. As can be seen, the molded Al(fum)@5% HPC particles have good mechanical properties, with a mass loss of less than 0.4% after 24 hours.

[0078] Example 6

[0079] 980 mg of the ultraporous metal-organic framework (MOF) Al(fum) powder (undegassed) prepared in Example 1 and 20 mg of polyvinyl alcohol (PVA) were weighed and mixed in a mortar. 2 mL of deionized water was added in small portions and stirred until the mixture became a paste. After the paste was semi-dry, it was extruded into spherical particles with a particle size of 1 to 2 mm. After drying, the resulting ultraporous MOF material, namely Al(fum)@PVA particles with a binder mass fraction of 2%, was obtained, denoted as Al(fum)@2%PVA.

[0080] The thermogravimetric curve of the molded ultra-microporous material Al(fum)@2%PVA obtained in this embodiment is shown in FIG8 . It can be seen that the material still maintains excellent thermal stability after molding.

[0081] X-ray diffraction analysis of the molded ultra-microporous material Al(fum)@2%PVA is shown in Figure 9. As can be seen from Figure 9, the peak shape of the material molded with 2%PVA as the binder remains consistent with that of the powder material, demonstrating that the Al(fum)@2%PVA framework structure remains intact after molding.

[0082] The Al(fum)@2%PVA shaped particles were placed in a vacuum degassing chamber at 120°C for 24 hours with a degassing pressure below 5 μmHg. The single-component static adsorption isotherm of N2 was then measured on a Micrometrics ASAP 2460 adsorption instrument at a test temperature of 77 K. The adsorption isotherm of N2 for the shaped ultra-microporous material Al(fum)@2%PVA obtained in this example at 77 K is shown in FIG10B . The N2 adsorption curve of the material after molding is consistent with that of the powder, and the specific surface area remains essentially unchanged (Al(fum)@2%PVA: 958 m 2 / g, Al(fum):1040m 2 / g).

[0083] 200 mg of the molded Al(fum)@2% PVA was weighed and placed in a conical flask. The flask was then placed in a shaking incubator at 25°C and 300 rpm, and the mass change of the particles was recorded, as shown in Figure 11. As can be seen, the molded Al(fum)@2% PVA particles have good mechanical properties, with a mass loss of less than 0.4% after 24 hours.

[0084] Example 7

[0085] 950 mg of the ultraporous metal-organic framework material Al(fum) powder (undegassed) prepared in Example 1 and 50 mg of polyvinyl alcohol (PVA) were weighed and mixed in a mortar. 2 mL of deionized water was added in small amounts and stirred until it became a paste. After it was semi-dry, it was extruded into spherical particles with a particle size of 1 to 2 mm. After drying, the ultraporous metal-organic framework material, i.e., Al(fum)@PVA particles with a binder mass fraction of 5%, were obtained, which were recorded as Al(fum)@5%PVA.

[0086] The thermogravimetric curve of the molded ultra-microporous material Al(fum)@5%PVA obtained in this embodiment is shown in FIG8 . It can be seen that the material still maintains excellent thermal stability after molding.

[0087] X-ray diffraction analysis of the Al(fum)@5% PVA ultraporous material was performed, and the results are shown in Figure 9. As can be seen from Figure 9, the peak shape of the material formed with 5% PVA as the binder remains consistent with that of the powder material, demonstrating that the Al(fum)@5% PVA framework structure remains intact after molding.

[0088] 200 mg of the molded Al(fum)@5% PVA was weighed and placed in a conical flask. The flask was then placed in a shaking incubator at 25°C and 300 rpm, and the mass change of the particles was recorded, as shown in Figure 11. As can be seen, the molded Al(fum)@5% PVA particles have good mechanical properties, with a mass loss of less than 0.4% after 24 hours.

[0089] Example 8

[0090] The shaped ultra-microporous material Al(fum)@2%HPC obtained in Example 4 was loaded into a 10 mm×100 mm fixed bed adsorption column, and a SF6 / N2 (volume ratio 10:90) mixed gas or a SF6 / CF4 (volume ratio 4:96) mixed gas was passed into the adsorption column at a flow rate of 1.3 mL / min at 273 K or 298 K, and high-purity N2 (purity greater than 99.999%) was obtained in the outflowing gas; when SF6 penetrated, the adsorption was stopped, and high-purity SF6 (purity greater than 99.99%) was obtained by desorption by He gas purging at 40°C for 10 h, and the adsorption column could be recycled.

[0091] The breakthrough curve of the molded ultra-microporous material Al(fum)@2%HPC obtained in this example is shown in Figure 13, where the mixed gas flow rate is 1.3 mL / min. It can be seen that the material still maintains excellent dynamic SF6 adsorption capacity after molding. High-purity SF6 (greater than 99.99%) can be obtained by desorption for 10 hours at 40°C and a He gas purge flow rate of 6.0 mL. The desorption curve is shown in Figure 14. Furthermore, the dynamic SF6 adsorption capacity of Al(fum)@2%HPC did not decrease significantly after four adsorption-desorption cycles of a SF6 / N2 (volume ratio 10:90) mixed gas at 298K (as shown in Figure 15).

[0092] It can be seen from the above examples that the molded ultra-microporous metal-organic framework material prepared in the present application has a high adsorption capacity for SF6 and good selectivity, and can achieve effective separation of SF6 / N2 or SF6 / CF4.

[0093] The above is only a preferred embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.

Claims

1. A method for preparing a molded ultra-microporous metal-organic framework material, comprising the following steps: The ultra-microporous metal-organic framework material, a binder and water are mixed and wet granulated to obtain the molded ultra-microporous metal-organic framework material; the binder is one or more of hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyvinyl butyral and kaolin; The ultra-microporous metal-organic framework material is prepared by mixing a soluble metal salt, an organic ligand, a base and water through a coordination reaction; the metal ion in the soluble metal salt is Cr 3+ 、Al 3+ 、V 3+ and Fe 3+ One or more of the following; the organic ligand is fumaric acid or a fumaric acid derivative.

2. The preparation method according to claim 1, characterized in that: The mass of the binder is 0.1-15% of the sum of the mass of the binder and the ultra-microporous metal-organic framework material.

3. The preparation method according to claim 2, characterized in that: The mass of the binder is 2-10% of the sum of the mass of the binder and the ultra-microporous metal-organic framework material.

4. The preparation method according to claim 1, characterized in that: The particle size of the molded ultra-microporous metal-organic framework material is 1 to 2 mm.

5. The preparation method according to claim 1, characterized in that: The fumaric acid derivative has a structure shown in Formula I: In formula I, R1 and R2 are independently selected from H, F, Cl, Br, I or CH3, and R1 and R2 are not H at the same time.

6. The preparation method according to claim 1, characterized in that: The alkali is sodium hydroxide; the molar ratio of the metal ions in the organic ligand and the soluble metal salt to the alkali is 1-2:2:4-8.

7. The preparation method according to claim 6, characterized in that: The molar ratio of the organic ligand, the metal ion and the base in the soluble metal salt is 2:2:

6.

8. The preparation method according to claim 1, 5, 6 or 7, characterized in that: The ultra-microporous metal-organic framework material has infinitely extended periodic one-dimensional square channels with a pore size of 9. The shaped ultra-microporous metal-organic framework material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the molded ultra-microporous metal-organic framework material according to claim 9 for selectively adsorbing sulfur hexafluoride from a mixed gas.

11. The use according to claim 10, characterized in that: The mixed gas includes sulfur hexafluoride and nitrogen or sulfur hexafluoride and carbon tetrafluoride.

12. The use according to claim 11, characterized in that: The volume ratio of sulfur hexafluoride to nitrogen or sulfur hexafluoride to carbon tetrafluoride in the mixed gas is 99:1 to 1:

99.

13. The use according to claim 10, 11 or 12, characterized in that The adsorption is one or more of fixed bed adsorption, fluidized bed adsorption and moving bed adsorption; the adsorption temperature is -20 to 60°C, and the pressure is 0.5 to 10 bar.

14. The use according to claim 13, characterized in that The adsorption temperature is 0-35°C and the pressure is 1-5 bar.

15. The use according to claim 10, characterized in that After the sulfur hexafluoride is saturated with adsorption, sulfur hexafluoride-rich gas is obtained by desorption.

Citation Information

Patent Citations

  • Organometallic aluminum fumarate backbone material

    CN101448568A

  • Preparation method and applications of porous metal organic skeleton material

    CN104370820A

  • Honeycomb ceramic-based aluminum-fumaric acid MOF adsorbent and in-situ synthetic method thereof

    CN110523380A

  • Forming method of nitrogen-containing aluminum-based metal-organic framework material and air water absorption application of nitrogen-containing aluminum-based metal-organic framework material

    CN113332958A

  • Molded ultra-microporous metal-organic framework material, preparation method thereof and application of molded ultra-microporous metal-organic framework material in selective adsorption of sulfur hexafluoride

    CN116586037A

Cited By

  • High-purity electronic special gas storage and separation method

    CN120204871A

  • Storage and separation method for high-purity electronic specialty gases