Method for forming conductive interconnection structure

By using doped and undoped mask patterns in semiconductor manufacturing, conductive lines of different heights are formed, which solves the problem of alignment deviation between conductive paths and conductive lines, and achieves self-alignment of conductive paths and process simplification. Manufacturing costs are reduced.

WO2024222723A1PCT designated stage expired Publication Date: 2024-10-31BEIJING NAURA MICROELECTRONICS EQUIP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/089491
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-24
Publication Date
2024-10-31

Smart Images

  • Figure CN2024089491_31102024_PF_FP_ABST
    Figure CN2024089491_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Embodiments of the present disclosure provide a method for forming a conductive interconnection structure. The method comprises: forming a predetermined mask pattern on a conductive layer; doping a first mask pattern to form a doped region having a predetermined depth in the first mask pattern, wherein the first mask pattern is a doped predetermined mask pattern, a second mask pattern is an undoped predetermined mask pattern, and the etch rate of the doped region is greater than the etch rate of an undoped region; and etching the conductive layer by using the first mask pattern and the second mask pattern to form the conductive interconnection structure, wherein the height of a conductive line corresponding to a region of the second mask pattern is greater than the height of a conductive line corresponding to a region of the first mask pattern, and the conductive line corresponding to the region of the second mask pattern is formed as a conductive path.
Need to check novelty before this filing date? Find Prior Art

Description

Method for forming conductive interconnect structure Technical Field

[0001] The present disclosure belongs to the field of semiconductor manufacturing technology, and particularly relates to a method for forming a conductive interconnect structure. Background Art

[0002] In the semiconductor manufacturing process, metal interconnect structures are fabricated through back-end of line (BEOL) processes to wire integrated circuits. Typically, metal interconnect structures consist of several metal interconnect layers, with conductive vias used to electrically connect different metal interconnect layers.

[0003] As the spacing and line width of wires in integrated circuits gradually decrease, there is an urgent need to provide a method for forming a conductive path with good conductive contact between metal interconnect layers.

[0004] Summary of the Invention

[0005] The embodiments of the present disclosure disclose a method for forming a conductive interconnect structure to solve the problem in the related art that it is difficult to form a conductive path with good conductive contact.

[0006] In order to solve the above technical problems, the present disclosure discloses a method for forming a conductive interconnect structure, including:

[0007] forming a predetermined mask pattern on the conductive layer;

[0008] doping the first mask pattern to form a doped region of a predetermined depth in the first mask pattern, wherein the first mask pattern is the predetermined mask pattern that has been doped, and the second mask pattern is the predetermined mask pattern that has not been doped; wherein an etching rate of the doped region is greater than an etching rate of the undoped region;

[0009] The conductive layer is etched using the first mask pattern and the second mask pattern to form a conductive interconnect structure; wherein the height of the conductive lines in the area corresponding to the second mask pattern is higher than the height of the conductive lines in the area corresponding to the first mask pattern, and the conductive lines in the area corresponding to the second mask pattern form a conductive path.

[0010] In some embodiments, etching the conductive layer using the first mask pattern and the second mask pattern includes:

[0011] while etching the conductive layer using the first mask pattern and the second mask pattern, etching the first mask pattern and the second mask pattern;

[0012] Wherein, an etching selectivity ratio between the conductive layer and the undoped region in the predetermined mask pattern is less than a predetermined value.

[0013] In some embodiments, while etching the conductive layer using the first mask pattern and the second mask pattern, the step of etching the first mask pattern and the second mask pattern includes the following stages:

[0014] When the doped region in the first mask pattern is etched away, the second mask pattern is partially etched, and the conductive layer not covered by the predetermined mask pattern is also partially etched at the same time;

[0015] When the first mask pattern is completely removed, the second mask pattern is also etched accordingly, and the conductive layer not covered by the predetermined mask pattern is also continuously etched at the same time;

[0016] When the second mask pattern is completely removed, the conductive layer not covered by the predetermined mask pattern is completely removed to form a number of conductive lines, the conductive layer in the area corresponding to the first mask pattern is partially etched, the height of the conductive layer in the area corresponding to the second mask pattern is higher than the height of the conductive lines in the area corresponding to the first mask pattern, and the conductive lines in the area corresponding to the second mask pattern serve as the conductive paths.

[0017] In some embodiments, etching the conductive layer using the first mask pattern and the second mask pattern includes:

[0018] removing the doped region in the first mask pattern;

[0019] etching the remaining first mask pattern and the second mask pattern to completely remove the first mask pattern;

[0020] While removing the remaining second mask pattern, a portion of the conductive layer in the area where the first mask pattern is located is removed to form a conductive path in the conductive line in the area corresponding to the second mask pattern.

[0021] In some embodiments, while the first mask pattern and the second mask pattern are being removed by etching, the conductive layer not covered by the predetermined mask pattern is etched.

[0022] In some embodiments, before removing the doped region in the first mask pattern, the method further includes:

[0023] etching the conductive layer using the first mask pattern and the second mask pattern to form the conductive line; or

[0024] After removing the doped region in the first mask pattern, the method further includes:

[0025] The conductive layer is etched using the remaining first mask pattern and the second mask pattern to form the conductive line.

[0026] In some embodiments, forming a predetermined mask pattern on the conductive layer includes:

[0027] forming a core layer on the conductive layer;

[0028] A partition wall is formed on the side wall of the core layer, and the partition wall serves as the predetermined mask pattern.

[0029] In some embodiments, doping the first mask pattern includes:

[0030] The first partition wall is doped to form a doped region with a predetermined depth in the first partition wall, wherein the first partition wall is the doped partition wall and the second partition wall is the undoped partition wall.

[0031] In some embodiments, doping the first spacer comprises:

[0032] forming a planarization layer on the conductive layer to fill the area between the partition walls;

[0033] performing a planarization process on the planarization layer to expose the core layer and the partition wall;

[0034] forming a mask layer on the surface of the planarization layer to cover the second partition wall;

[0035] Ions are implanted into the first partition walls that are not blocked.

[0036] In some embodiments, the planarization layer is a SOC material; or

[0037] The element implanted by the ion implantation is Ge.

[0038] In some embodiments, the method further comprises:

[0039] The core layer and the planarization layer are removed.

[0040] In some embodiments, the doped region of the first spacer is removed simultaneously with the removal of the core layer and / or the planarization layer.

[0041] In some embodiments, a hard mask layer is further included between the conductive layer, the core layer, and the planarization layer, and removing the core layer and the planarization layer includes:

[0042] The core layer and the planarization layer are removed using the hard mask layer as an etch stop layer.

[0043] In some embodiments, etching the conductive layer using the first mask pattern and the second mask pattern includes:

[0044] The hard mask layer and the conductive layer not covered by the first and second partition walls are removed using the first and second partition walls as masks.

[0045] In some embodiments, a liner layer is further included below the conductive layer, and removing the hard mask layer and the conductive layer not covered by the first spacer walls and the second spacer walls using the first spacer walls and the second spacer walls as masks further includes:

[0046] The liner layer that is not covered by the first and second partition walls is removed.

[0047] In some embodiments, the liner layer includes at least one of TiN, TaN, Al, Cu, Ni, Co, Ru, Ti, and Ta.

[0048] In some embodiments, the conductive layer is a metal conductive layer; or

[0049] The conductive layer includes at least one of Ru, Co, Mo, W, Al, and Rh.

[0050] In some embodiments, forming a predetermined mask pattern on the conductive layer includes:

[0051] The predetermined mask pattern is formed by adopting a self-aligned multiple patterning method.

[0052] In the method for forming a conductive interconnect structure provided by an embodiment of the present disclosure, a predetermined mask pattern is doped so that the etching rate of the doped regions in the predetermined mask pattern is greater than the etching rate of the undoped regions. This allows for the formation of conductive lines of varying heights through subsequent etching steps, with the height of the conductive lines in the region corresponding to the second mask pattern being higher than the height of the conductive lines in the region corresponding to the third mask pattern, thereby forming a conductive path. The conductive path is formed using a self-aligned process, eliminating the misalignment problem between the conductive path and the conductive line that can occur with a damascene process in related techniques. Furthermore, compared to the subtractive etching process in related techniques, the process requires fewer steps and does not require a precise mask pattern. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] FIG1 is a schematic diagram showing a method for forming a metal interconnect structure in the related art;

[0054] FIG2 is a schematic diagram showing another method for forming a metal interconnect structure in the related art;

[0055] 3 to 11 are schematic diagrams of semiconductor structures corresponding to respective steps in the method for forming a conductive interconnect structure provided according to an embodiment of the present disclosure;

[0056] 12 to 20 are schematic diagrams of semiconductor structures corresponding to respective steps in a method for forming a conductive interconnect structure provided according to another embodiment of the present disclosure. DETAILED DESCRIPTION

[0057] To make the objectives, technical solutions, and advantages of the present disclosure more clear, the technical solutions in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present disclosure, not all of them. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present disclosure without creative work are within the scope of protection of the present disclosure.

[0058] It should be understood by those skilled in the art that the embodiments of the present disclosure are merely illustrations of the structures and methods claimed in the present disclosure that can be implemented in various forms. In addition, each example given in conjunction with the various embodiments is intended to be illustrative rather than restrictive. In addition, the drawings are not necessarily drawn to scale, and some features may be exaggerated to show the details of specific components. Therefore, the specific structural and functional details in the embodiments of the present disclosure should not be interpreted as restrictive, but merely as a representative basis for teaching those skilled in the art to adopt the methods and structures of the embodiments of the present disclosure in different ways. It should also be noted that identical and corresponding elements are represented by the same reference numerals.

[0059] In the following description, numerous specific details are set forth, such as specific structures, components, materials, dimensions, processing steps and techniques, in order to provide an understanding of the various embodiments of the present disclosure. However, it will be understood by those skilled in the art that the various embodiments of the present disclosure may be practiced without these specific details. In other cases, well-known structures or processing steps have not been described in detail to avoid obscuring the present disclosure.

[0060] For the purposes of the following description, the terms "upper," "right," "left," "vertical," "horizontal," "top," "bottom," and their derivatives shall relate to the orientation of the structures and methods disclosed in the drawings of the specification. It will be understood that when an element as a layer, region, or substrate is referred to as being "on" another element, the element can be directly on the other element or intervening elements may be present. In contrast, when an element is referred to as being "directly on" another element, there are no intervening elements between the two. It will also be understood that when an element is referred to as being "under" another element, the element can be directly under the other element or intervening elements may be present. Conversely, when an element is referred to as being "directly under" another element, there are no intervening elements between the two.

[0061] A related art method for forming a metal interconnect structure is provided. As shown in FIG1 , this method uses a damascene process to form an insulating layer on a metal interconnect line 11, forms a via hole in the insulating layer, and then fills the via hole with metal to form a conductive path 12. The conductive path 12 is used to electrically connect the current metal interconnect line 11 to the metal interconnect line on the upper layer. However, this method makes it difficult to align the via hole with the underlying metal interconnect line 11 when forming the via hole, especially when the wire width is very narrow. On the other hand, the metal interconnect line may experience line wiggling, which may cause a deviation in the alignment between the conductive path 12 and the metal interconnect line 11, thereby increasing the impedance of the metal interconnect structure.

[0062] Related art also provides a method for forming a metal interconnect structure, as shown in FIG2 . This method uses a subtractive etching process to form a mask pattern 13 at the location where a conductive path is desired. The metal interconnect is then etched, with the unetched portion being higher than the etched portion, and the unetched portion serving as the conductive path. However, this method requires forming a precise mask pattern 13 when the pitch of the conductors is very tight. If the mask pattern 13 has deviations, it may result in the formation of an undesirable conductive path at a location where a conductive path is not desired.

[0063] The technical solutions disclosed in the embodiments of the present disclosure will be described in detail below with reference to the accompanying drawings.

[0064] In order to solve the above technical problems, an embodiment of the present disclosure provides a method for forming a conductive interconnect structure, which may include the following steps.

[0065] S11 , forming a predetermined mask pattern on the conductive layer.

[0066] The semiconductor structure shown in FIG. 3 includes a substrate 100 , a liner layer 110 formed on the substrate 100 , a conductive layer 120 formed on the liner layer 110 , a hard mask layer 130 formed on the conductive layer 120 , and a predetermined mask pattern 140 formed on the hard mask layer 130 .

[0067] The substrate 100 may be composed of a silicon-containing material. Silicon-containing materials include, but are not limited to, silicon, single-crystal silicon, polycrystalline silicon, SiGe, single-crystal SiGe, polycrystalline SiGe, carbon-doped silicon (Si:C), amorphous silicon, or a combination thereof. The substrate 100 may be a single layer or multiple layers. The substrate 100 may also be composed of other semiconductor materials such as germanium (Ge) and a compound semiconductor substrate. The compound semiconductor substrate may be, for example, a III-V semiconductor substrate such as gallium arsenide (GaAs).

[0068] The liner layer 110 can be formed by methods such as sputtering, chemical vapor deposition (CVD), or atomic layer deposition (ALD). The liner layer 110 may include a conductive material such as titanium nitride (TiN) or tantalum nitride (TaN). In some embodiments, the liner layer 110 may also be composed of other conductive materials, such as aluminum (Al), copper (Cu), nickel (Ni), cobalt (Co), ruthenium (Ru), titanium (Ti), tantalum (Ta), or a combination thereof.

[0069] The conductive layer 120 may be a metal conductive layer or a non-metallic conductive layer. In some embodiments of the present disclosure, the conductive layer 120 is a metal conductive layer and may include ruthenium (Ru), cobalt (Co), molybdenum (Mo), tungsten (W), aluminum (Al), or rhodium (Rh), or alloys thereof. The conductive layer 120 may be formed using, for example, CVD, plasma enhanced chemical vapor deposition (PECVD), physical vapor deposition (PVD), or other deposition processes.

[0070] The hard mask layer 130 is a material used as an etch mask in semiconductor processing. For example, it can be used to protect the conductive layer 120 from being etched during the subsequent etching process of the predetermined mask pattern 140. The hard mask layer 130 can be composed of a metal or a dielectric material, such as silicon nitride, silicon oxide, or a combination of silicon nitride and silicon oxide. It can be formed using a process such as low-pressure chemical vapor deposition (LPCVD).

[0071] The predetermined mask pattern 140 can be formed from any dielectric material, such as a dielectric oxide, a dielectric nitride, and / or a dielectric oxynitride. In some embodiments, the mask pattern 140 can be formed from a non-conductive, low-capacitance dielectric material, such as silicon dioxide. To obtain a finer mask pattern 140, a self-aligned multiple patterning method, such as self-aligned double patterning or self-aligned quadruple patterning, can be employed.

[0072] Those skilled in the art should understand that, in the above description, the substrate 100, the liner layer 110 and the hard mask layer 130 are optional, and in some implementations of the embodiments of the present disclosure, one or more of the substrate 100, the liner layer 110 and the hard mask layer 130 may not be formed.

[0073] It should be noted that in the example of FIG. 3 , other layers may exist between substrate 100 and conductive layer 120. The present disclosure does not limit the metal interconnect layer where conductive layer 120 is located to the bottommost metal interconnect layer; it may be any interconnect layer. In other words, other metal interconnect layers may be in direct contact with conductive layer 120.

[0074] S12 . Doping the first mask pattern to form a doped region with a predetermined depth in the first mask pattern, wherein the first mask pattern is a doped predetermined mask pattern, and the second mask pattern is an undoped predetermined mask pattern.

[0075] As shown in FIG4 , among the multiple predetermined mask patterns, some predetermined mask patterns form doping regions with predetermined depths (indicated by the shaded portions in FIG4 ), and these predetermined mask patterns are all first mask patterns; the remaining predetermined mask patterns do not form doping regions (i.e., there are no shaded portions) and are second mask patterns.

[0076] In some embodiments, the first mask pattern 141 can be doped using methods such as ion implantation. For example, Ge can be implanted into the first mask pattern 141. By controlling the implantation energy and implantation dose of the ion implantation, the implantation depth of the ion implantation can be precisely controlled. As will be seen below, the ion implantation depth is related to the height of the conductive path (via) to be formed subsequently. In the subsequent etching process, the etching rate of the area after ion implantation is higher than the etching rate of the area without ion implantation, that is, the etching rate of the doped area is greater than the etching rate of the undoped area.

[0077] During the doping process, a photoresist (not shown) may be used to shield regions not requiring doping, thereby obtaining the first mask pattern 141 and the second mask pattern 142 .

[0078] S13. Etching the conductive layer using the first mask pattern and the second mask pattern to form a conductive interconnect structure; wherein the height of the conductive lines in the area corresponding to the second mask pattern is higher than the height of the conductive lines in the area corresponding to the first mask pattern, and the conductive lines in the area corresponding to the second mask pattern form a conductive path.

[0079] That is, the height of the conductive line in the region corresponding to the second mask pattern is higher than that of the conductive line in the region corresponding to the first mask pattern, forming a conductive path.

[0080] It is easy to understand that, during the process of etching the conductive layer, the portion of the hard mask layer 130 not covered by the first mask pattern and the second mask pattern is completely etched.

[0081] The above step S13 can be performed by a one-step etching method or a step-by-step etching method. For the sake of clarity, the step-by-step etching method is first described in detail herein.

[0082] In some implementations of the present disclosure, step S13 may include:

[0083] S131 , removing the doped region in the first mask pattern.

[0084] As shown in FIG5 , an etching process can be used to remove the doped regions in the first mask pattern 141. Because portions of the first mask pattern 141 are doped, the etching rate of the doped regions is greater than that of the undoped regions during the etching process, thereby removing the doped regions. In some embodiments, while etching away the doped regions of the first mask pattern 141, the conductive layer not covered by the predetermined mask pattern 140 is also etched, saving process steps.

[0085] S132 , etching the conductive layer using the remaining first mask pattern and the second mask pattern to form a conductive line.

[0086] As shown in FIG6 , after this etching step, a plurality of conductive lines 121 are formed in the semiconductor structure. It should be noted that the disclosed embodiment is not limited thereto. Prior to step S131, the conductive layer 120 may be etched using the first mask pattern 141 and the second mask pattern 142 to form the conductive lines 121. The first mask pattern 141 and the second mask pattern 142 do not remove the doped regions.

[0087] Those skilled in the art should understand that step S132 is optional. In some embodiments, the conductive layer 120 not covered by the predetermined mask pattern can be etched while the first mask pattern 141 and the second mask pattern 142 are being etched away, thereby eliminating the need for a separate etching step to form the conductive line 121, thereby saving process steps.

[0088] S133 , etching the remaining first mask pattern and the second mask pattern to completely remove the first mask pattern.

[0089] As shown in FIG. 7 , since the height of the second mask pattern 142 is greater than the remaining first mask pattern 141 , a portion of the second mask pattern 142 still remains after the first mask pattern 141 is completely removed.

[0090] S134 , while removing the remaining second mask pattern, remove part of the conductive layer in the area where the first mask pattern is located, so as to form a conductive path in the conductive line in the area corresponding to the second mask pattern.

[0091] After step S133, the semiconductor structure continues to be etched. During this etching process, an etching gas with a relatively low etch selectivity between the conductive lines 121 and the second mask pattern 142 is selected. This allows etching of the remaining second mask pattern 142 while also etching the conductive lines 121 exposed after the first mask pattern 141 has been completely removed. Consequently, after the remaining second mask pattern 142 is completely removed, portions of the conductive lines in the area where the first mask pattern 141 was located are also removed, forming conductive lines 121 of varying heights. The height of the conductive lines in the area corresponding to the first mask pattern 141 is lower, while the height of the conductive lines in the area corresponding to the second mask pattern 142 is higher, thereby forming conductive pathways 123, as shown in Figures 8 and 9.

[0092] As can be seen from the above description, the main concept of the embodiments of the present disclosure is that by doping a predetermined mask pattern, the etching rate of the doped region in the predetermined mask pattern is greater than the etching rate of the undoped region, so that conductive lines of different heights can be formed through subsequent etching processes. The height of the conductive lines in the region corresponding to the first mask pattern 141 is lower, and the height of the conductive lines in the region corresponding to the second mask pattern 142 is higher, thereby forming a conductive path 123. Based on this concept, in order to further reduce the manufacturing process of the conductive interconnect structure, the above-mentioned step S13 can also be implemented by a one-step etching method, thereby reducing the manufacturing cost of the conductive interconnect structure. In some implementations of the embodiments of the present disclosure, the above-mentioned step S13 may include:

[0093] While the conductive layer 120 is being etched using the first mask pattern 141 and the second mask pattern 142 , the first mask pattern 141 and the second mask pattern 142 are being etched;

[0094] The etching selectivity between the conductive layer 120 and the undoped regions in the predetermined mask pattern 140 is less than a predetermined value. In other words, the etching selectivity between the conductive layer 120 and the undoped regions in the predetermined mask pattern 140 is relatively small, and the predetermined mask pattern 140 is etched simultaneously with the removal of the conductive layer 120. By selecting a suitable etching gas, the conductive layer 120 not covered by the predetermined mask pattern 140 can be completely removed upon completion of etching the second mask pattern 142, thereby forming a plurality of conductive lines 121.

[0095] The etching step will be described in detail in stages below.

[0096] In stage 1, when etching the semiconductor structure shown in FIG4 , when the doped region in the first mask pattern 141 is etched away, since the etching rate of the doped region in the predetermined mask pattern 140 is greater than the etching rate of the undoped region, the second mask pattern 142 is partially etched, for example, the etching amount is very small, and there is also a certain etching effect on the conductive layer 120 not covered by the predetermined mask pattern 140, that is, part of the conductive layer 120 not covered by the predetermined mask pattern 140 is also partially etched at the same time, forming a number of grooves 122, as shown in FIG10 .

[0097] Phase 2: Etching of the semiconductor structure shown in FIG. 10 continues. When first mask pattern 141 is completely removed, the remaining undoped first mask pattern 141 is etched at the same rate as second mask pattern 142. Therefore, second mask pattern 142 is also etched accordingly, decreasing in height. Simultaneously, because the etching selectivity between conductive layer 120 and the undoped regions within predetermined mask pattern 140 is less than a predetermined value, portions of conductive layer 120 not covered by predetermined mask pattern 140 are also etched, increasing in depth of recess 122, as shown in FIG. 11 .

[0098] Phase 3: Continuing to etch the semiconductor structure shown in FIG. 11 , when the second mask pattern 142 is completely removed, the conductive layer 120 not covered by the predetermined mask pattern 140 is also completely removed, thereby forming a plurality of conductive lines 121 of varying heights. Simultaneously, the conductive layer 120 corresponding to the first mask pattern 141 is partially etched. The conductive lines in the region corresponding to the first mask pattern 141 are of lower height, while the conductive lines in the region corresponding to the second mask pattern 142 are taller than those in the region corresponding to the first mask pattern 141. The conductive lines in the region corresponding to the second mask pattern 142 serve as conductive paths 123, as shown in FIG. 8 and FIG. 9 .

[0099] In the method for forming a conductive interconnect structure according to an embodiment of the present disclosure, a predetermined mask pattern is doped so that the etching rate of the doped regions in the predetermined mask pattern is greater than the etching rate of the undoped regions. This allows conductive lines of varying heights to be formed through subsequent etching processes. The height of the conductive lines in the region corresponding to the second mask pattern 142 is higher than the height of the conductive lines in the region corresponding to the first mask pattern 141. Thus, the conductive lines in the region corresponding to the second mask pattern 142 form conductive pathways 123. Conductive pathways 123 are formed using a self-aligned process. That is, during the etching process, only the exposed portions of the corresponding film layer that are not covered by the upper film layer are etched, achieving automatic alignment of the etching positions. This eliminates the misalignment between the conductive pathways and the conductive lines that can occur with damascene processes in related techniques. Furthermore, compared to subtractive etching processes in related techniques, the process requires fewer steps and does not require a precise mask pattern.

[0100] Hereinafter, a method for forming a conductive interconnect structure provided by an embodiment of the present disclosure will be described in more detail. The method may include the following steps.

[0101] S101 , forming a core layer (mandrel) on the conductive layer.

[0102] As shown in FIG12 , the detailed description of the substrate 100 , the liner layer 110 , the conductive layer 120 , and the hard mask layer 130 may refer to the corresponding description above, which will not be repeated here.

[0103] The core layer 150 can be composed of, for example, silicon nitride (SiN), silicon carbonitride (SiCN), SiOCN, SiBCN, or other insulating materials known in the art. Specifically, it can be formed by depositing an insulating layer on the conductive layer 120 and then etching the insulating layer. The etching process can be dry etching, laser ablation, or any other process known in the art that can achieve selective removal, and is not limited here.

[0104] S102 , forming a spacer on the sidewall of the core layer, wherein the spacer serves as a predetermined mask pattern.

[0105] As shown in Figure 13, the spacer, also known as the predetermined mask pattern 140 above, can be composed of any dielectric material, such as a dielectric oxide, a dielectric nitride and / or a dielectric oxynitride. In some embodiments, the spacer (i.e., the predetermined mask pattern 140) can be composed of a non-conductive, low-capacitance dielectric material, such as silicon dioxide. The process of forming the spacer (i.e., the predetermined mask pattern 140) can include depositing an insulating material such as silicon nitride on the exposed surface of the core layer 150 and the hard mask layer 130, for example, using CVD, plasma enhanced chemical vapor deposition (PECVD), physical vapor deposition (PVD) or other deposition processes. Then, an anisotropic etching process can be used, in which the forward etching rate is greater than the lateral etching rate, thereby etching away the horizontal portion of the deposited insulating material, thereby forming the spacer (i.e., the predetermined mask pattern 140) located on the sidewall of the core layer 150. The above describes the process of forming a partition wall as a predetermined mask pattern 140 by self-aligned double patterning. Those skilled in the art should understand that it is also feasible to use self-aligned quadruple patterning or more patterning to form a finer predetermined mask pattern 140, which will not be repeated here.

[0106] S103 , forming a planarization layer on the conductive layer to fill the area between the spacers.

[0107] S104 , performing a planarization process on the planarization layer to expose the core layer and the spacer.

[0108] As shown in FIG14 , the planarization layer 160 can be made of, for example, a spin-on carbon (SOC) material and can be formed on the conductive layer 120 by deposition, such as chemical vapor deposition. After the planarization layer 160 is deposited, the surface of the core layer 150 is also covered by the planarization layer 160 . Therefore, the planarization process is performed to expose the surface of the core layer 150 , thereby fully filling the area between the spacers (i.e., the predetermined mask pattern 140 ) and obtaining a flat surface for subsequent processing steps.

[0109] S105 , forming a mask layer on the surface of the planarization layer to cover the second partition wall.

[0110] As shown in Figure 15, a mask layer 170 is formed on the surface of the planarization layer 160 to block the second spacers (serving as the second mask pattern 142). The area corresponding to the mask layer 170 is the area where the conductive path will be formed.

[0111] S106 , performing ion implantation on the unblocked first partition walls (serving as the first mask pattern 141 ).

[0112] As shown in FIG16 , after ion implantation, a doped region of a predetermined depth is formed in the first partition wall. Unlike the related art shown in FIG2 , the mask pattern 13 is an etching mask that needs to be precisely formed at the corresponding position. When the wire pitch is as low as the nanometer level, it is very difficult to achieve the corresponding precision of the etching mask pattern. In this embodiment, the mask layer 170 is an ion implantation mask, and the requirements for the mask position accuracy are relatively low. Even if the position of the mask layer 170 is slightly offset, it will not affect the ion implantation of the first partition wall. For example, the position offset of the mask layer 170 can be overcome by slightly adjusting the ion implantation angle.

[0113] The mask layer 170 may be, for example, a photoresist. After the ion implantation process is completed, the mask layer 170 may be removed by a photoresist stripping process.

[0114] S107 , removing the planarization layer and the core layer.

[0115] The semiconductor structure after the core layer 150 and the planarization layer 160 are removed is shown in Figure 17. In step S107, the core layer 150 and the planarization layer 160 may be removed using the hard mask layer 130 as an etch stop layer.

[0116] In some implementations of the present disclosure, the core layer 150 and the planarization layer 160 may be removed simultaneously or in steps.

[0117] In some other implementations of the present disclosure, the doped region of the first spacer (serving as the first mask pattern 141 ) may be removed simultaneously with the removal of the core layer 150 and / or the planarization layer 160 .

[0118] S108 , using the first spacer (serving as the first mask pattern 141 ) and the second spacer (serving as the second mask pattern 142 ) as masks, remove the hard mask layer 130 and the conductive layer 120 not covered by the first spacer and the second spacer.

[0119] In this step, the hard mask layer 130 and the conductive layer 120 can be etched in one step. Of course, the hard mask layer 130 and the conductive layer 120 can also be etched in separate steps to form a plurality of conductive lines 121.

[0120] In some implementations of the present disclosure, while removing the hard mask layer 130 and the conductive layer 120 not covered by the first and second spacers, the liner layer 110 not covered by the first and second spacers is also removed, as shown in FIG. 18 .

[0121] It should be noted that in the example of Figure 18, other layers may exist between the substrate 100, the pad layer 110 and the conductive line 121. The embodiment of the present disclosure does not limit the metal interconnection layer where the conductive line 121 is located to be the bottom metal interconnection layer, which can be any interconnection layer.

[0122] S109 , etching the remaining first mask pattern and the second mask pattern to completely remove the second mask pattern, so as to form a conductive path in the conductive line in the area corresponding to the second mask pattern.

[0123] In this step, because the height of the second mask pattern 142 (i.e., the second spacer) is higher than the height of the remaining first mask pattern 141 (i.e., the first spacer), a portion of the second mask pattern 142 remains after the first mask pattern 141 is completely removed. During the subsequent etching process, due to the low etching selectivity between the conductive lines 121 and the second mask pattern 142, while the remaining second mask pattern 142 is etched, the conductive lines 121 exposed after the first mask pattern 141 is completely removed are also etched. As a result, after the remaining second mask pattern 142 is completely removed, a portion of the conductive lines in the area where the first mask pattern 141 was located is also removed, forming conductive lines 121 of different heights. The conductive lines in the area corresponding to the first mask pattern 141 are of lower height, while the conductive lines in the area corresponding to the second mask pattern 142 are of higher height. As a result, the conductive lines in the area corresponding to the second mask pattern 142 form conductive pathways 123, as shown in FIG.

[0124] In this step, the remaining hard mask layer 130 on the conductive line 121 is also removed.

[0125] S110 , forming an interlayer insulating layer covering the conductive interconnect structure, and performing a planarization process to expose the conductive path.

[0126] As shown in Figure 20, an interlayer insulating layer 180 is formed on the substrate 100 to cover the entire conductive interconnect structure and is planarized, so that an upper conductive interconnect structure can be formed on the interlayer insulating layer 180. The upper conductive interconnect structure can be electrically connected to the conductive interconnect structure of the current layer through the conductive path 123.

[0127] In the method for forming a conductive interconnect structure according to an embodiment of the present disclosure, by doping a predetermined mask pattern, the etching rate of the doped regions in the predetermined mask pattern is greater than the etching rate of the undoped regions. This allows conductive lines of varying heights to be formed through subsequent etching processes. The height of the conductive lines in the region corresponding to the second mask pattern 142 is higher than the height of the conductive lines in the region corresponding to the first mask pattern 141. Thus, the conductive lines in the region corresponding to the second mask pattern 142 form conductive paths 123. Conductive paths 123 are formed using a self-aligned process, eliminating the misalignment problem between the conductive paths and conductive lines that can occur with damascene processes in related techniques. Furthermore, compared to subtractive etching processes in related techniques, the process requires fewer steps and does not require a precise mask pattern.

[0128] The above embodiments of the present disclosure focus on the differences between the various embodiments. As long as the different optimization features between the various embodiments are not contradictory, they can be combined to form a better embodiment. Considering the simplicity of the text, they will not be repeated here.

[0129] The foregoing is merely an embodiment of the present disclosure and is not intended to limit the present disclosure. Various modifications and variations are possible for those skilled in the art. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure are intended to be included within the scope of the claims of the present disclosure.

Claims

1. A method for forming a conductive interconnect structure, wherein: include: forming a predetermined mask pattern on the conductive layer; Doping the first mask pattern to form a doped region of a predetermined depth in the first mask pattern, wherein the first mask pattern is the predetermined mask pattern that has been doped, and the second mask pattern is the predetermined mask pattern that has not been doped; wherein an etching rate of the doped region is greater than an etching rate of the undoped region; The conductive layer is etched using the first mask pattern and the second mask pattern to form a conductive interconnect structure; wherein the height of the conductive lines in the area corresponding to the second mask pattern is higher than the height of the conductive lines in the area corresponding to the first mask pattern, and the conductive lines in the area corresponding to the second mask pattern form a conductive path.

2. The method according to claim 1, wherein: The etching of the conductive layer by using the first mask pattern and the second mask pattern comprises: While etching the conductive layer using the first mask pattern and the second mask pattern, etching the first mask pattern and the second mask pattern; Wherein, an etching selectivity ratio between the conductive layer and the undoped region in the predetermined mask pattern is less than a predetermined value.

3. The method according to claim 2, wherein: The step of etching the first mask pattern and the second mask pattern while etching the conductive layer using the first mask pattern and the second mask pattern comprises the following stages: When the doped region in the first mask pattern is etched away, the second mask pattern is partially etched, and the conductive layer not covered by the predetermined mask pattern is also partially etched at the same time; When the first mask pattern is completely removed, the second mask pattern is also etched accordingly. Meanwhile, the conductive layer not covered by the predetermined mask pattern is also continuously etched; When the second mask pattern is completely removed, the conductive layer not covered by the predetermined mask pattern is completely removed to form a plurality of conductive lines, the conductive layer in the area corresponding to the first mask pattern is partially etched, the height of the conductive layer in the area corresponding to the second mask pattern is higher than the height of the conductive lines in the area corresponding to the first mask pattern, and the conductive lines in the area corresponding to the second mask pattern serve as the conductive paths.

4. The method according to claim 1, wherein: The etching of the conductive layer by using the first mask pattern and the second mask pattern comprises: removing the doped region in the first mask pattern; etching the remaining first mask pattern and the second mask pattern to completely remove the first mask pattern; While removing the remaining second mask pattern, a portion of the conductive layer in the area where the first mask pattern is located is removed to form a conductive path in the conductive line in the area corresponding to the second mask pattern.

5. The method according to claim 4, wherein: While the first mask pattern and the second mask pattern are removed by etching, the conductive layer not covered by the predetermined mask pattern is etched.

6. The method according to claim 4, wherein: Before removing the doped region in the first mask pattern, the method further includes: etching the conductive layer using the first mask pattern and the second mask pattern to form the conductive line; or After removing the doped region in the first mask pattern, the method further includes: The conductive layer is etched using the remaining first mask pattern and the second mask pattern to form the conductive line.

7. The method according to claim 1, wherein: The forming of a predetermined mask pattern on the conductive layer comprises: forming a core layer on the conductive layer; A partition wall is formed on the side wall of the core layer, and the partition wall serves as the predetermined mask pattern.

8. The method according to claim 7, wherein: The step of doping the first mask pattern comprises: The first partition wall is doped to form a doped region with a predetermined depth in the first partition wall, wherein the first partition wall is the doped partition wall and the second partition wall is the undoped partition wall.

9. The method according to claim 8, wherein: The step of doping the first partition wall comprises: forming a planarization layer on the conductive layer to fill the area between the partition walls; performing a planarization process on the planarization layer to expose the core layer and the spacer; forming a mask layer on the surface of the planarization layer to cover the second partition wall; Ions are implanted into the first partition walls that are not blocked.

10. The method according to claim 9, wherein: The planarization layer is a SOC material; or The element implanted by the ion implantation is Ge.

11. The method according to claim 9, wherein: Also includes: The core layer and the planarization layer are removed.

12. The method according to claim 11, wherein: The doped region of the first partition wall is removed while the core layer and / or the planarization layer is removed.

13. The method according to claim 11, wherein: A hard mask layer is further included between the conductive layer, the core layer and the planarization layer, and removing the core layer and the planarization layer includes: The hard mask layer is used as an etch stop layer to remove the core layer and the planarization layer.

14. The method according to claim 13, wherein: The etching of the conductive layer by using the first mask pattern and the second mask pattern comprises: The hard mask layer and the conductive layer that are not covered by the first partition wall and the second partition wall are removed using the first partition wall and the second partition wall as masks.

15. The method according to claim 14, wherein: The conductive layer further includes a liner layer below the conductive layer, and the hard mask layer and the conductive layer not covered by the first spacer and the second spacer are removed by using the first spacer and the second spacer as masks, and further includes: The liner layer that is not covered by the first partition walls and the second partition walls is removed.

16. The method according to claim 15, wherein: The liner layer includes at least one of TiN, TaN, Al, Cu, Ni, Co, Ru, Ti, and Ta.

17. The method according to claim 1, wherein: The conductive layer is a metal conductive layer; or The conductive layer includes at least one of Ru, Co, Mo, W, Al, and Rh.

18. The method according to claim 1, wherein: The forming of a predetermined mask pattern on the conductive layer comprises: The predetermined mask pattern is formed by a self-aligned multiple patterning method.

Citation Information

Patent Citations

  • Integrated circuit pattern formed based on pitch doubling and forming method

    CN107863318A

  • Fin-type semiconductor device and formation method thereof

    CN109671778A

  • Semiconductor structure and forming method thereof, and semiconductor device

    CN111627977A

  • Manufacturing method of semiconductor structure

    CN115312385A

  • Method for forming conductive interconnection structure

    CN116487322A