Cast aluminum alloy and preparation method therefor, motor rotor and automobile
By adding elements such as Fe and Ni to aluminum alloys, combined with Mg or Cu, to form a specific phase combination, the problem of the contradiction between the conductivity and mechanical properties of aluminum alloys is solved, and the preparation of aluminum alloys with low cost and high performance is achieved, which is suitable for high-voltage applications. Speeding motor rotors and energy efficient cars.
Patent Information
- Application Number
- PCT/CN2024/089642
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-31
AI Technical Summary
There is a contradiction between improving electrical conductivity and mechanical properties of existing aluminum alloys. Highly conductive and high-strength aluminum alloys are more expensive and prone to produce coarse dendrites, which affects the density of the structure.
By adding Fe, Ni and other alloying elements to the aluminum alloy, combined with Mg or Cu, the (Fe, Ni)4Al13 phase and α-Al eutectic phase are formed to improve the electrical conductivity and mechanical properties of the aluminum alloy while reducing the nickel content to reduce cost, and adopts a simple preparation method suitable for industrial promotion.
It achieves a significant increase in the electrical conductivity of aluminum alloys while ensuring yield strength and tensile strength, reduces production costs, and improves the density and performance stability of aluminum alloys. It is suitable for high-speed motor rotors and high-energy-efficiency automobiles.
Smart Images

Figure CN2024089642_31102024_PF_FP_ABST
Abstract
Description
A cast aluminum alloy, a preparation method thereof, a motor rotor and a vehicle
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application is based on the Chinese patent application with application number 202310449856.6 and application date on April 24, 2023, and the Chinese patent application with application number 202310451120.2 and application date on April 24, 2023, and claims the priority of the Chinese patent application. The entire contents of the Chinese patent application are hereby introduced into this application as a reference. Technical Field
[0003] The present disclosure belongs to the technical field of cast aluminum alloys, and particularly relates to a cast aluminum alloy and a preparation method thereof, a motor rotor, and an automobile. Background Art
[0004] Automotive motor rotors require cast aluminum alloys with high electrical conductivity, excellent mechanical properties, and machinability. However, in practice, a conflicting relationship exists between the electrical conductivity and strength of aluminum alloys: as strength increases, electrical conductivity decreases, and vice versa. Strategies for improving the electrical conductivity of aluminum alloys while simultaneously maintaining excellent mechanical properties are limited. Therefore, developing an aluminum alloy with both high electrical conductivity and excellent mechanical properties is highly desirable.
[0005] Since aluminum-silicon alloys have excellent casting properties, good mechanical properties, and good electrical conductivity, most of the high-conductivity and high-strength aluminum alloys are aluminum-silicon alloys. According to relevant technology [1], when the Si content in aluminum alloy reaches 13%, the electrical conductivity of aluminum alloy at room temperature is less than 40% IACS.
[0006] In order to solve the above problem, aluminum alloys without Si can be selected and alloying elements such as Fe and Ni can be added to them to improve the electrical conductivity of the aluminum alloy while ensuring that the yield strength and tensile strength are not reduced too much. For example, the related art [2] discloses a high-strength, high-conductivity, silicon-free aluminum-iron-nickel alloy, which contains from 4.3wt.% to 6wt.% Ni, from 0.2wt.% to 0.8wt.% Fe, and from 0.01wt.% to 1wt.% Ti, with the remainder being Al. The electrical conductivity of the aluminum-iron-nickel alloy is 40-50% IACS, the yield strength is not less than 90MPa, and the ultimate tensile strength is 150MPa. However, the aluminum-iron-nickel alloy still has the following problems: (1) Since nickel is expensive, the cost of alloy products with high nickel content is also expensive. At present, for every 1wt.% of Ni added in aluminum alloy smelting, the price of aluminum ingots increases by 2,000-3,000 yuan / ton, which is not conducive to industrial production; (2) The solidification temperature range of the aluminum-iron-nickel alloy is large, which easily produces coarse dendrites, making it difficult to feed the alloy liquid for shrinkage, and easily reducing the density of the structure.
[0007] [1]KNPrahbu and BNRavishankar.2003.Mater.Sci.Eng.A.[J].Effect of Modification Melt Treatment on Casting / Chill Interfacial Heat Transfer and Electrical Conductivity of Al-13%Si Alloy.360:293-298.
[0008] [2] Patent application HK40042796A, Aluminum alloy for die casting.
[0009] Summary of the Invention
[0010] The present disclosure aims to at least partially address one of the technical problems in the related art. To this end, embodiments of the present disclosure provide a cast aluminum alloy for a motor rotor, a method for preparing the same, a motor rotor, and an automobile, wherein the cast aluminum alloy has low cost and improves both electrical conductivity and strength.
[0011] In a first aspect, an embodiment of the present disclosure provides a cast aluminum alloy for a motor rotor, comprising the following components, based on 100 wt.% of the total mass of the cast aluminum alloy:
[0012] Fe 0.5-2wt.%,
[0013] Ni 0.1-1wt.%
[0014] Mg 0.1-0.5wt.%,
[0015] The balance is Al and inevitable impurities.
[0016] The advantages and technical effects of the cast aluminum alloy for the motor rotor of the embodiment of the present disclosure are as follows:
[0017] (1) The present invention adds Fe and Ni elements that can improve the strength of the aluminum alloy to the cast aluminum alloy. Therefore, the cast aluminum alloy can greatly improve the electrical conductivity while ensuring that the yield strength and tensile strength are not greatly reduced;
[0018] (2) The cast aluminum alloy of the embodiment of the present disclosure contains Mg, which is dissolved in the matrix α-Al phase and plays a role in solid solution strengthening. 13 The combined effect of the two phases makes the cast aluminum alloy have good yield strength and tensile strength;
[0019] (3) Compared with the cast aluminum alloys disclosed in the related art, the Ni content in the cast aluminum alloys of the embodiments disclosed herein is relatively low and no heat treatment is required, so the cost of the resulting cast aluminum alloy is also relatively low.
[0020] In some embodiments, the cast aluminum alloy comprises the following components based on the total mass of the cast aluminum alloy as 100 wt. %:
[0021] Fe 0.5-1.5wt.%,
[0022] Ni 0.5-1wt.%
[0023] Mg 0.1-0.35wt.%,
[0024] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0025] In some embodiments, the total content of Fe and Ni is 2-2.5 wt. %.
[0026] In some embodiments, the (Fe,Ni)4Al 13 The mole fraction of the phase is 4-6 mol%.
[0027] In some embodiments, the room temperature electrical conductivity of the cast aluminum alloy is greater than 50% IACS.
[0028] In some embodiments, the cast aluminum alloy has a yield strength of 65 MPa or greater.
[0029] In some embodiments, the cast aluminum alloy has a tensile strength of 150 MPa or greater.
[0030] In some embodiments, the cast aluminum alloy has a porosity of 0.3% or less.
[0031] In some embodiments, the cast aluminum alloy has an elongation of greater than 14%.
[0032] In a second aspect, an embodiment of the present disclosure further provides a cast aluminum alloy for a motor rotor, comprising the following components, based on 100 wt% of the total mass of the cast aluminum alloy:
[0033] Fe 0.5-2wt%,
[0034] Ni 0.3-1.5wt%,
[0035] Cu 0.1-0.8wt%,
[0036] The balance is Al and inevitable impurities.
[0037] The advantages and technical effects brought by the cast aluminum alloy of the embodiment of the present disclosure are:
[0038] (1) The cast aluminum alloy of the embodiment of the present disclosure does not contain Si, which reduces the electrical conductivity of the aluminum alloy, but contains Fe and Ni, which can improve the strength of the aluminum alloy. Therefore, the cast aluminum alloy can improve the electrical conductivity of the aluminum alloy while ensuring that the yield strength and tensile strength are not greatly reduced.
[0039] (2) The cast aluminum alloy of the embodiment of the present disclosure contains Cu, which is dissolved in the matrix α-Al phase and plays a role in solid solution strengthening. 13 The combined effect of the two phases makes the cast aluminum alloy have excellent yield strength and tensile strength;
[0040] (3) Compared with the cast aluminum alloys disclosed in the related art, the Ni content in the cast aluminum alloys of the embodiments disclosed herein is relatively low, and thus the cost of the resulting cast aluminum alloys is also relatively low.
[0041] In some embodiments, the cast aluminum alloy comprises the following components based on the total mass of the cast aluminum alloy as 100 wt %:
[0042] Fe 1-1.5wt%,
[0043] Ni 0.3-1wt%,
[0044] Cu 0.1-0.6wt%,
[0045] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0046] In some embodiments, the total content of Fe and Ni is 0.8-3 wt %.
[0047] In some embodiments, the total content of Fe and Ni is 2-2.5 wt%.
[0048] In some embodiments, the room temperature electrical conductivity of the cast aluminum alloy is greater than 47% IACS.
[0049] In some embodiments, the cast aluminum alloy has a porosity of 0.1% or less.
[0050] In some embodiments, the cast aluminum alloy has an elongation of greater than 13%.
[0051] In a third aspect, the present disclosure also provides a method for preparing a cast aluminum alloy for a motor rotor, comprising the following steps:
[0052] Aluminum alloy raw materials are added in proportion and smelted to obtain an aluminum alloy melt; the aluminum alloy melt is refined and degassed, and then cast into a casting mold to obtain the cast aluminum alloy.
[0053] The advantages and technical effects of the method for preparing the cast aluminum alloy for the motor rotor according to the embodiment of the present disclosure are as follows:
[0054] (1) The preparation method of the disclosed embodiment has simple steps and is suitable for industrial promotion;
[0055] (2) The cast aluminum alloy obtained by the preparation method of the embodiment of the present disclosure is not only low in cost but also has both electrical conductivity and mechanical properties.
[0056] In some embodiments, the casting mold is not preheated and maintained at room temperature.
[0057] In some embodiments, no heat treatment is performed after the cast aluminum alloy is obtained.
[0058] In some embodiments, the preparation method comprises the following steps:
[0059] Preheating the pit furnace in an empty state to remove moisture in the furnace at a preheating temperature of 400° C. or higher, preheating pure aluminum, and then placing the preheated pure aluminum into the pit furnace for smelting at a smelting temperature of 780-800° C. After the pure aluminum is completely melted, removing the surface slag and removing the oxide scale, maintaining the melt temperature, adding pure iron, pure nickel, and pure magnesium, or adding an aluminum-iron master alloy, an aluminum-nickel master alloy, and an aluminum-magnesium master alloy, and completely submerging the aluminum liquid. After the aluminum alloy raw material is completely melted, standing for 2-3 hours to obtain the aluminum alloy melt;
[0060] The refining agent is wrapped with aluminum foil and dried, and a stainless steel bell jar is preheated at the same time. The preheated refining agent is then pressed to the bottom of the aluminum alloy melt using the preheated stainless steel bell jar, and high-purity argon gas is introduced into the aluminum alloy melt to perform a refining and degassing process of the aluminum alloy melt, while maintaining the casting temperature at 700-740°C; the aluminum alloy melt is poured into the casting mold, and after the aluminum-iron-nickel alloy melt solidifies and cools, the casting is opened and removed from the mold to obtain a cast aluminum alloy.
[0061] In a fourth aspect, the embodiments of the present disclosure further provide a motor rotor, which is prepared from the cast aluminum alloy of the embodiments of the present invention.
[0062] The advantages and technical effects brought by the motor rotor of the embodiment of the present invention are as follows:
[0063] Since the motor rotor of the embodiment of the present invention is made of the cast aluminum alloy of the embodiment of the present invention, the electronic rotor will not fail even when the rotation speed is as high as 18,000 rpm.
[0064] In a fifth aspect, an embodiment of the present invention further provides a vehicle, comprising the motor rotor of an embodiment of the present invention.
[0065] The advantages and technical effects brought by the automobile of the embodiment of the present invention are as follows:
[0066] The automobile according to the embodiment of the present invention accelerates faster and can match a higher speed and a higher energy efficiency level because it uses the motor rotor according to the embodiment of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] FIG1 is a SEM image of the cast aluminum alloy of Example 1;
[0068] FIG2 is a SEM image of the cast aluminum alloy of Example 10. DETAILED DESCRIPTION
[0069] The embodiments of the present disclosure are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present disclosure, but should not be understood as limiting the present disclosure.
[0070] In a first aspect, an embodiment of the present disclosure provides a cast aluminum alloy for a motor rotor, comprising the following components, based on 100 wt.% of the total mass of the cast aluminum alloy:
[0071] Fe 0.5-2wt.%,
[0072] Ni 0.1-1wt.%
[0073] Mg 0.1-0.5wt.%,
[0074] The balance is Al and inevitable impurities.
[0075] The cast aluminum alloy of the embodiment of the present disclosure does not contain Si element, so compared with the cast aluminum alloy containing high Si content in the related art, the cast aluminum alloy has excellent electrical conductivity; although the absence of Si element will reduce the strength of the cast aluminum alloy, since the cast aluminum alloy contains Fe, Ni and Mg elements at the same time, the main phase of the cast aluminum alloy includes primary (Fe, Ni)4Al 13 phase, α-Al phase and (Fe,Ni)4Al 13 and α-Al eutectic phase, (Fe,Ni)4Al 13 The Mg phase improves the yield strength and tensile strength of the aluminum alloy. Furthermore, the Mg element does not react with Fe and Ni to form compounds, but instead dissolves in the matrix α-Al phase, providing solid solution strengthening and increasing the yield strength and tensile strength of the aluminum alloy. Therefore, the cast aluminum alloy can maintain excellent electrical conductivity while also exhibiting good yield strength and tensile strength. Furthermore, compared to high-Ni-content cast aluminum alloys in related art, the Ni content in the cast aluminum alloys of the disclosed embodiments is relatively low, resulting in a relatively low cost cast aluminum alloy, which helps companies reduce production costs.
[0076] Based on the total mass of the cast aluminum alloy as 100 wt.%, in the cast aluminum alloy of the embodiment of the present disclosure, the mass fraction of Fe is 0.5-2 wt.%, such as 0.5 wt.%, 0.8 wt.%, 1 wt.%, 1.2 wt.%, 1.4 wt.%, 1.6 wt.%, 1.8 wt.%, 2 wt.%, etc., and the mass fraction of Ni is 0.1-1 wt.%, such as 0.1 wt.%, 0.3 wt.%, 0.5 wt.%, 0.7 wt.%, 1.0 wt.%, etc. When the mass fraction of Fe is lower than 0.5 wt.%, and the mass fraction of Ni is lower than 0.1 wt.%, it is difficult to form sufficient (Fe, Ni)4Al 13Phase, the yield strength and tensile strength of cast aluminum alloy are both low. When the mass fraction of Fe is higher than 2wt.%, (Fe,Ni)4Al 13 If the amount of Fe is too high, the conductivity of the cast aluminum alloy decreases. When the mass fraction of Ni is higher than 1 wt.%, the cost of the cast aluminum alloy increases accordingly due to the high cost of Ni. Preferably, the mass fraction of Fe is 0.5-1.5 wt.%, and the mass fraction of Ni is 0.5-1 wt.%.
[0077] Based on the total mass of the cast aluminum alloy as 100 wt.%, the mass fraction of Mg in the cast aluminum alloy of the embodiments of the present disclosure is 0.1-0.5 wt.%, for example, 0.1 wt.%, 0.2 wt.%, 0.3 wt.%, 0.4 wt.%, 0.5 wt.%, etc. When the mass fraction of Mg is less than 0.1 wt.%, it does not have a solid solution strengthening effect, thereby significantly reducing the yield strength and tensile strength of the cast aluminum alloy. When the mass fraction of Mg is greater than 0.5 wt.%, the electrical conductivity of the cast aluminum alloy is reduced. Preferably, the mass fraction of Mg is 0.1-0.35 wt.%.
[0078] In some embodiments, the content of a single impurity is ≤0.05 wt.%, and the total impurity content is ≤0.15 wt.%. The impurity content meets the requirements of standard GB / T 8733-2016.
[0079] In some embodiments, the total content of Fe and Ni is 0.6-3wt.%, for example, 0.6wt.%, 0.8wt.%, 1wt.%, 1.2wt.%, 1.4wt.%, 1.6wt.%, 1.8wt.%, 2wt.%, 2.2wt.%, 2.4wt.%, 2.6wt.%, 2.8wt.%, 3wt.%, etc. Compared with the high-Ni content casting aluminum alloy in the related art, the Ni content of the casting aluminum alloy in the embodiment of the present disclosure is lower, so the total content of Fe and Ni is also relatively low. On the one hand, it can reduce the solidification temperature range of the casting aluminum alloy, reduce shrinkage and thermal cracking tendencies, reduce porosity, increase the density of the casting aluminum alloy, and thus improve its casting performance; on the other hand, it can reduce the coarse (Fe, Ni)4Al 13 The content of phase can improve the elongation of cast aluminum alloy, so that cast aluminum alloy can absorb more energy without breaking after being impacted, and reduce the coarse (Fe, Ni)4Al 13 The content of the phase can also improve the electrical conductivity of the cast aluminum alloy. Preferably, the total content of Fe and Ni is 2-2.5 wt.%.
[0080] In some embodiments, the (Fe,Ni)4Al 13 The molar fraction of the phase is 4-6 mol%. (Fe,Ni)4Al13 It is the primary phase and the eutectic part is formed at the end of solidification. The eutectic part is formed at the end of solidification through the melt →α-Al+(Fe,Ni)4Al 13 Formation, eutectic part (Fe,Ni)4Al 13 The fine and uniform particles are beneficial to reduce the impact on elongation. 13 When the content of the phase is lower than 4 mol%, it is not conducive to improving the yield strength and tensile strength of the cast aluminum alloy; when the (Fe, Ni)4Al 13 When the content of the phase is higher than 6 mol%, it is not conducive to improving the elongation of the cast aluminum alloy.
[0081] In some embodiments, the room temperature electrical conductivity of the cast aluminum alloy is above 50% IACS, preferably 50-53% IACS, such as 50% IACS, 50.5% IACS, 51% IACS, 51.5% IACS, 52% IACS, 52.5% IACS, 53% IACS, etc.
[0082] In some embodiments, the yield strength of the cast aluminum alloy is above 65 MPa, preferably 65-80 MPa, for example, 65 MPa, 68 MPa, 70 MPa, 73 MPa, 75 MPa, 78 MPa, 80 MPa, etc.
[0083] In some embodiments, the tensile strength of the cast aluminum alloy is above 150 MPa, preferably 150-170 MPa, for example, 150 MPa, 153 MPa, 155 MPa, 158 MPa, 160 MPa, 163 MPa, 165 MPa, 168 MPa, 170 MPa, etc.
[0084] In some embodiments, the porosity of the cast aluminum alloy is less than 0.3%, preferably 0.01-0.3%, for example, 0.01%, 0.05%, 0.1%, 0.15%, 0.18%, 0.2%, 0.23%, 0.25%, 0.3%, etc.
[0085] In some embodiments, the elongation of the cast aluminum alloy is greater than 14%, preferably 14-22%, for example, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, etc.
[0086] In a second aspect, an embodiment of the present disclosure provides a cast aluminum alloy for a motor rotor, comprising the following components, based on 100 wt% of the total mass of the cast aluminum alloy:
[0087] Fe 0.5-2wt%,
[0088] Ni 0.3-1.5wt%,
[0089] Cu 0.1-0.8wt%,
[0090] The balance is Al and inevitable impurities.
[0091] The cast aluminum alloy of the embodiment of the present disclosure does not contain Si element, so compared with the cast aluminum alloy containing Si in the related art, the electrical conductivity of the cast aluminum alloy is significantly improved; although the absence of Si element will reduce the strength of the cast aluminum alloy, since the cast aluminum alloy contains Fe, Ni and Cu elements at the same time, the main phase of the cast aluminum alloy includes primary (Fe, Ni)4Al 13 phase, α-Al phase and (Fe,Ni)4Al 13 and α-Al eutectic phase, (Fe,Ni)4Al 13 The phase has the effect of improving the yield strength and tensile strength of the aluminum alloy. At the same time, the Cu element does not react with the Fe and Ni elements to form compounds, but is dissolved in the matrix α-Al phase, which plays a solid solution strengthening role and also improves the yield strength and tensile strength of the aluminum alloy. Therefore, the cast aluminum alloy can have excellent yield strength and tensile strength while maintaining good electrical conductivity. In addition, compared with the high-Ni content cast aluminum alloy in the related art, the Ni content in the cast aluminum alloy of the embodiment of the present disclosure is relatively low, so the cost of the obtained cast aluminum alloy is also relatively low, which is beneficial for enterprises to reduce production costs. The cast aluminum alloy of the embodiment of the present disclosure is suitable for preparing high-strength and high-conductivity parts such as motor rotors for new energy vehicles.
[0092] Based on the total mass of the cast aluminum alloy as 100wt%, in the cast aluminum alloy of the embodiment of the present disclosure, the mass fraction of Fe is 0.5-2wt%, such as 0.5wt%, 0.8wt%, 1wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2wt%, etc., and the mass fraction of Ni is 0.3-1.5wt%, such as 0.3wt%, 0.5wt%, 0.8wt%, 1wt%, 1.2wt%, 1.5wt%, etc. When the mass fraction of Fe is lower than 0.5wt% and the mass fraction of Ni is lower than 0.3wt%, it is difficult to form sufficient (Fe,Ni)4Al 13 Phase, the yield strength and tensile strength of cast aluminum alloy are low. When the mass fraction of Fe is higher than 2wt%, (Fe,Ni)4Al 13If the amount of Fe is too high, the conductivity of the cast aluminum alloy decreases. When the mass fraction of Ni is higher than 1.5wt%, the cost of the cast aluminum alloy increases accordingly due to the high cost of Ni. Preferably, the mass fraction of Fe is 1-1.5wt%, and the mass fraction of Ni is 0.3-1wt%.
[0093] Based on the total mass of the cast aluminum alloy as 100wt%, in the cast aluminum alloy of the embodiments of the present disclosure, the mass fraction of Cu is 0.1-0.8wt%, for example, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, etc. When the mass fraction of Cu is less than 0.1wt%, it does not have a solid solution strengthening effect, thereby significantly reducing the yield strength and tensile strength of the cast aluminum alloy. When the mass fraction of Cu is greater than 0.8wt%, the electrical conductivity of the cast aluminum alloy decreases. Preferably, the mass fraction of Cu is 0.1-0.6wt%.
[0094] In some embodiments, the total content of Fe and Ni is 0.8-3wt%, such as 0.8wt%, 1wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2wt%, 2.2wt%, 2.4wt%, 2.6wt%, 2.8wt%, 3wt%, etc. Compared with the casting aluminum alloy with high Ni content in the related art, the casting aluminum alloy of the embodiment of the present disclosure has a lower Ni content, so the total content of Fe and Ni is also relatively low. On the one hand, it can reduce the solidification temperature range of the casting aluminum alloy, reduce shrinkage and thermal cracking tendencies, reduce porosity, and increase the density of the casting aluminum alloy, thereby improving its casting performance; on the other hand, it can reduce the coarse (Fe, Ni)4Al 13 The content of phase can improve the elongation of cast aluminum alloy, so that cast aluminum alloy can absorb more energy without breaking after being impacted, and reduce the coarse (Fe, Ni)4Al 13 The content of the phase can also improve the electrical conductivity of the cast aluminum alloy. Preferably, the total content of Fe and Ni is 2-2.5wt%.
[0095] In some embodiments, the content of a single impurity is ≤0.05 wt.%, and the total impurity content is ≤0.15 wt.%. The impurity content meets the requirements of standard GB / T 8733-2016.
[0096] In some embodiments, the room temperature electrical conductivity of the cast aluminum alloy is above 47% IACS, preferably 47-52% IACS, such as 47% IACS, 48% IACS, 49% IACS, 50% IACS, 51% IACS, 52% IACS, etc.
[0097] In some embodiments, the yield strength of the cast aluminum alloy is greater than 75 MPa, preferably 75-100 MPa, such as 75 MPa, 80 MPa, 85 MPa, 90 MPa, 95 MPa, 100 MPa, etc.
[0098] In some embodiments, the tensile strength of the cast aluminum alloy is above 160 MPa, preferably 160-190 MPa, for example, 160 MPa, 165 MPa, 170 MPa, 175 MPa, 180 MPa, 185 MPa, 190 MPa, etc.
[0099] In some embodiments, the porosity of the cast aluminum alloy is less than 0.1%, preferably 0.01-0.1%, for example 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, etc.
[0100] In some embodiments, the elongation of the cast aluminum alloy is greater than 13%, more preferably 13-20%, for example, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc. In a third aspect, the present disclosure also provides a method for preparing a cast aluminum alloy for a motor rotor, comprising the following steps:
[0101] Melting of aluminum alloy melt: adding aluminum alloy raw materials in proportion and melting to obtain aluminum alloy melt;
[0102] Preparation of cast aluminum alloy: After refining and degassing the aluminum alloy melt, cast it into a casting mold to obtain the cast aluminum alloy.
[0103] The preparation method of the embodiment of the present disclosure has simple steps and is suitable for industrial promotion. The cast aluminum alloy prepared has not only low cost but also can take into account both electrical conductivity and mechanical properties.
[0104] In some embodiments, the refined, degassed aluminum alloy melt is cast into a casting mold that is not preheated and maintained at room temperature. Compared to preheating the casting mold, not preheating the mold increases the temperature gradient between the aluminum alloy melt and the casting mold, thereby increasing the cooling rate, which is beneficial for improving the electrical conductivity, yield strength, tensile strength, and elongation of the cast aluminum alloy.
[0105] In some embodiments, the cast aluminum alloy is not subjected to a heat treatment step after it is obtained. Compared to performing a heat treatment step after the cast aluminum alloy is obtained, not performing a heat treatment step can significantly improve the yield strength and tensile strength of the cast aluminum alloy. Heat treatment releases the aluminum alloy's internal casting stress, and a reduction in this stress leads to a decrease in strength. Furthermore, not performing a heat treatment step can significantly reduce energy consumption, optimize processes, lower industrial production costs, and improve economic efficiency.
[0106] In some embodiments, the smelting of the aluminum alloy melt specifically includes the following steps: first, preheating the pit furnace in an empty furnace to remove moisture in the furnace, the preheating temperature is above 400°C, and at the same time, preheating the pure aluminum, then placing the preheated pure aluminum into the pit furnace for smelting, the smelting temperature is 780-800°C, after the pure aluminum is completely melted, removing the surface slag and removing the oxide scale, maintaining the melt temperature, adding pure iron, pure nickel and pure magnesium, or adding aluminum-iron master alloy, aluminum-nickel master alloy and aluminum-magnesium master alloy, or adding pure iron, pure nickel and pure copper, and completely submerging them into the aluminum liquid, waiting for the alloy elements to be completely melted, and standing for 2-3 hours to obtain the aluminum alloy melt;
[0107] In some embodiments, the preparation of cast aluminum alloy specifically includes the following steps: first, wrap the refining agent with aluminum foil and dry it, and preheat the stainless steel bell jar at the same time, then use the preheated stainless steel bell jar to press the preheated refining agent to the bottom of the aluminum alloy melt, and introduce high-purity argon into the aluminum alloy melt to complete the refining and degassing process of the aluminum alloy melt, and maintain a casting temperature of 700-740°C; next, pour the aluminum alloy melt into a casting mold that is not preheated and maintained at room temperature. After the aluminum alloy melt solidifies and cools, the casting is opened and taken out to obtain a cast aluminum alloy. The material of the casting mold is cast iron and the casting time is controlled within 30s.
[0108] In a fourth aspect, the embodiments of the present disclosure further provide a motor rotor, which is prepared from the cast aluminum alloy of the embodiments of the present disclosure.
[0109] Since the motor rotor of the embodiment of the present disclosure is made of the cast aluminum alloy of the embodiment of the present disclosure, the electronic rotor will not fail even when the rotation speed is as high as 18,000 rpm.
[0110] In a fifth aspect, an embodiment of the present disclosure also provides a car, comprising the motor rotor of an embodiment of the present disclosure, and capable of matching a higher rotation speed and a high energy efficiency level.
[0111] The automobile according to the embodiment of the present disclosure accelerates faster because it uses the motor rotor according to the embodiment of the present disclosure.
[0112] The present disclosure is described in detail below with reference to embodiments and drawings.
[0113] Example 1
[0114] A cast aluminum alloy for a motor rotor, comprising the following components, based on 100 wt.% of the total mass of the cast aluminum alloy:
[0115] Fe 1.5wt.%
[0116] Ni 1wt.%
[0117] Mg 0.3wt.%
[0118] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0119] The method for preparing the cast aluminum alloy comprises the following steps:
[0120] Melting of aluminum alloy melt: First, preheat the pit furnace empty to remove moisture in the furnace at a preheating temperature of 400°C. At the same time, preheat the pure aluminum. Then, place the preheated pure aluminum into the pit furnace for melting at a melting temperature of 780-800°C. After the pure aluminum is completely melted, remove the surface slag and remove the oxide scale. Maintain the melt temperature, add pure iron, pure nickel, and pure magnesium, and completely immerse them in the aluminum liquid. After the alloy elements are completely melted, let it stand for 2 hours to obtain the aluminum alloy melt.
[0121] Preparation of cast aluminum alloy: First, wrap the refining agent with aluminum foil and dry it, and preheat the stainless steel bell jar at the same time. Then, use the preheated stainless steel bell jar to press the preheated refining agent to the bottom of the melt, and introduce high-purity argon gas into the aluminum alloy melt to complete the refining and degassing process of the aluminum alloy melt, maintaining a casting temperature of 700-740°C; next, pour the aluminum alloy melt into a casting mold that is not preheated and maintained at room temperature. After the aluminum alloy melt solidifies and cools, the casting is opened and removed from the mold to obtain the cast aluminum alloy. The casting mold is made of cast iron and the casting time should be controlled within 30 seconds.
[0122] Example 2
[0123] The alloy composition and preparation method are the same as those in Example 1, with the only difference being that a T6 heat treatment is further performed after step S2: the cast aluminum alloy obtained in step S2 is solution treated at 520°C for 4 hours, taken out and water quenched, and then aged at 180°C for 3 hours, and then taken out and air-cooled. The interval between the solution treatment and the aging treatment does not exceed 0.5 hours.
[0124] Example 3
[0125] A cast aluminum alloy for a motor rotor, comprising the following components, based on 100 wt.% of the total mass of the cast aluminum alloy:
[0126] Fe 1wt.%
[0127] Ni 1wt.%
[0128] Mg 0.3wt.%
[0129] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0130] The preparation method of the cast aluminum alloy is the same as that of Example 1.
[0131] Example 4
[0132] The alloy composition and preparation method are the same as those in Example 2, with the only difference being that a T6 heat treatment is further performed after step S2: the cast aluminum alloy obtained in step S2 is solution treated at 520°C for 4 hours, taken out and water quenched, and then aged at 180°C for 3 hours, and then taken out and air-cooled. The interval between the solution treatment and the aging treatment does not exceed 0.5 hours.
[0133] Example 5
[0134] The alloy composition and preparation method are the same as those in Example 3, with the only difference being that the casting mold is preheated to 150° C. and the refined and degassed aluminum alloy melt is cast into the mold.
[0135] Example 6
[0136] A cast aluminum alloy for a motor rotor, comprising the following components, based on 100 wt.% of the total mass of the cast aluminum alloy:
[0137] Fe 2wt.%
[0138] Ni 1wt.%
[0139] Mg 0.3wt.%
[0140] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0141] The preparation method of the cast aluminum alloy is the same as that of Example 1, except that pure iron, pure nickel, pure magnesium or an aluminum-based master alloy (which may be Al-Fe, Al-Ni, Al-Mg) is added in step S1 and completely immersed in the aluminum liquid.
[0142] Example 7
[0143] A cast aluminum alloy for a motor rotor, comprising the following components, based on 100 wt.% of the total mass of the cast aluminum alloy:
[0144] Fe 1.6wt.%
[0145] Ni 0.8wt.%
[0146] Mg 0.15wt.%
[0147] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0148] The preparation method of the cast aluminum alloy is the same as that of Example 1.
[0149] Example 8
[0150] A cast aluminum alloy, based on 100 wt% of the total mass of the cast aluminum alloy, comprises the following components:
[0151] Fe 1wt%,
[0152] Ni 1wt%,
[0153] Cu 0.6wt%,
[0154] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0155] The method for preparing the cast aluminum alloy comprises the following steps:
[0156] Melting of aluminum alloy melt: First, preheat the pit furnace in an empty state to remove moisture in the furnace at a preheating temperature of 400°C. At the same time, preheat the pure aluminum. Then, place the preheated pure aluminum into the pit furnace for melting at a melting temperature of 780-800°C. After the pure aluminum is completely melted, remove the surface slag and remove the oxide scale. Maintain the melt temperature, add pure iron, pure nickel, and pure copper, and completely immerse them in the aluminum liquid. After the alloy elements are completely melted, let it stand for 2 hours to obtain the aluminum alloy melt.
[0157] Preparation of cast aluminum alloy: First, wrap the refining agent with aluminum foil and dry it, and preheat the stainless steel bell jar at the same time. Then, use the preheated stainless steel bell jar to press the preheated refining agent to the bottom of the aluminum alloy melt, and introduce high-purity argon gas into the aluminum alloy melt to complete the refining and degassing process of the aluminum alloy melt, maintaining a casting temperature of 700-740°C. Next, pour the aluminum alloy melt into a non-preheated casting mold maintained at room temperature. After the aluminum alloy melt solidifies and cools, the casting is opened and removed from the mold to obtain the cast aluminum alloy. The casting mold is made of cast iron and the casting time is controlled within 30 seconds.
[0158] Example 9
[0159] A cast aluminum alloy, based on 100 wt% of the total mass of the cast aluminum alloy, comprises the following components:
[0160] Fe 1.5wt%,
[0161] Ni 1wt%,
[0162] Cu 0.6wt%,
[0163] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0164] The preparation method of the cast aluminum alloy is the same as that of Example 8.
[0165] Example 10
[0166] A cast aluminum alloy, based on 100 wt% of the total mass of the cast aluminum alloy, comprises the following components:
[0167] Fe 2wt%,
[0168] Ni 1wt%,
[0169] Cu 0.6wt%,
[0170] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0171] The preparation method of the cast aluminum alloy is the same as that of Example 8.
[0172] Example 11
[0173] A cast aluminum alloy, based on 100 wt% of the total mass of the cast aluminum alloy, comprises the following components:
[0174] Fe 1.5wt%,
[0175] Ni 1wt%,
[0176] Cu 0.6wt%,
[0177] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0178] The only difference between the preparation method of the cast aluminum alloy and Example 8 is that T6 heat treatment is also performed during the preparation process of the cast aluminum alloy: the obtained cast aluminum alloy is solution treated at 520°C for 4 hours, taken out and water quenched, and then aged at 180°C for 3 hours. After the end, it is taken out and air-cooled. The interval between the solution treatment and the aging treatment does not exceed 0.5 hours.
[0179] Example 12
[0180] The alloy composition and preparation method used are the same as those in Example 9, with the only difference being that the aluminum alloy melt is poured into a casting mold preheated at 150° C., and other conditions are the same.
[0181] Example 13
[0182] A cast aluminum alloy, based on 100 wt% of the total mass of the cast aluminum alloy, comprises the following components:
[0183] Fe 2wt%,
[0184] Ni 1.5wt%,
[0185] Cu 0.6wt%,
[0186] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0187] The preparation method of the cast aluminum alloy is the same as that of Example 8.
[0188] Example 14
[0189] A cast aluminum alloy, based on 100 wt% of the total mass of the cast aluminum alloy, comprises the following components:
[0190] Fe 1.7wt%,
[0191] Ni 0.5wt%,
[0192] Cu 0.3wt%,
[0193] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0194] The preparation method of the cast aluminum alloy is the same as that of Example 8.
[0195] Comparative Example 1
[0196] A cast aluminum alloy for a motor rotor, comprising the following components, based on 100 wt.% of the total mass of the cast aluminum alloy:
[0197] Fe 1wt.%
[0198] Ni 1wt.%
[0199] Mg 0,
[0200] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0201] The preparation method of the cast aluminum alloy is the same as that of Example 1.
[0202] Comparative Example 2
[0203] A cast aluminum alloy for a motor rotor, comprising the following components, based on 100 wt.% of the total mass of the cast aluminum alloy:
[0204] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0205] The preparation method of the cast aluminum alloy is the same as that of Example 1.
[0206] Comparative Example 3
[0207] A cast aluminum alloy, based on 100 wt% of the total mass of the cast aluminum alloy, comprises the following components:
[0208] Fe 1.5wt%,
[0209] Ni 1wt%,
[0210] Cu 0,
[0211] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0212] The preparation method of the cast aluminum alloy is the same as that of Example 8.
[0213] Comparative Example 4
[0214] A cast aluminum alloy, based on 100 wt% of the total mass of the cast aluminum alloy, comprises the following components:
[0215] Fe 1.5wt%,
[0216] Ni 1wt%,
[0217] Cu 0.9wt%,
[0218] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0219] The preparation method of the cast aluminum alloy is the same as that of Example 8.
[0220] Comparative Example 5
[0221] A cast aluminum alloy, based on 100 wt% of the total mass of the cast aluminum alloy, comprises the following components:
[0222] The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
[0223] The preparation method of the cast aluminum alloy is the same as that of Example 8, except that pure iron, pure nickel, pure copper, pure magnesium and aluminum-silicon master alloy are added to the smelting step of the aluminum alloy melt and are completely immersed in the aluminum liquid.
[0224] The preparation method of the cast aluminum alloy is the same as that of Example 8.
[0225] The compositions and preparation methods of the cast aluminum alloys of Examples 1-7 and Comparative Examples 1-2 are shown in Table 1, and their corresponding performance test data are shown in Table 2. IACS testing was performed using an eddy current conductivity meter (PZ-60A). Porosity was calculated by metallographically counting the void area per unit area. Yield strength, tensile strength, and elongation were determined according to the GB / T 228.1-2010 test standard.
[0226] Table 1. Composition and preparation method of cast aluminum alloys of Examples 1-7 and Comparative Examples 1-2
[0227] Table 2. Performance test results of cast aluminum alloys of Examples 1-7 and Comparative Examples 1-2
[0228] As can be seen from Tables 1 and 2, the cast aluminum alloys of Examples 1-7 exhibit excellent overall performance, maintaining excellent electrical conductivity (above 50.0% IACS) while also exhibiting good yield strength (above 65 MPa) and tensile strength (above 150 MPa). Furthermore, compared to the high-nickel cast aluminum alloy of Comparative Example 2, the cast aluminum alloys of Examples 1-7 of the present disclosure have significantly lower production costs due to their lower nickel content.
[0229] By comparing Example 1, Example 3 and Example 6, it can be found that when the Fe content is reduced, the (Fe, Ni)4Al 13 The phase content decreases, and the conductivity and elongation increase. The same rule can be found by comparing Example 2 with Example 4.
[0230] A comparison of Examples 1 and 2 shows that omitting the T6 heat treatment significantly increases the yield strength and tensile strength of the cast aluminum alloy. A comparison of Examples 3 and 4 also reveals the same pattern. However, T6 heat treatment is not conducive to improving strength, so it is preferred not to perform heat treatment in the present disclosure.
[0231] A comparison of Examples 3 and 5 reveals that maintaining the mold at room temperature during casting is more effective than preheating the mold in advance. This is because, compared to Example 5, where the mold was preheated in advance, Example 3 casts the aluminum alloy melt into an unpreheated mold. This increases the temperature gradient between the aluminum alloy melt and the mold, which increases the cooling rate and improves the yield strength, tensile strength, and elongation of the cast aluminum alloy.
[0232] By comparing Example 3 with Comparative Example 1, it can be found that when the cast aluminum alloy does not contain Mg, the yield strength and tensile strength of the cast aluminum alloy are significantly reduced.
[0233] The compositions and preparation methods of the cast aluminum alloys of Examples 8-14 and Comparative Examples 3-5 are shown in Table 3, and their corresponding performance test data are shown in Table 4. IACS testing was performed using an eddy current conductivity meter (PZ-60A). Porosity was calculated by metallographically counting the void area per unit area. Yield strength, tensile strength, and elongation were determined according to the GB / T 228.1-2010 test standard.
[0234] Table 3. Composition and preparation method of cast aluminum alloys of Examples 8-14 and Comparative Examples 3-5
[0235] Table 4. Performance test results of cast aluminum alloys of Examples 8-14 and Comparative Examples 3-5
[0236] As can be seen from Tables 3 and 4, the cast aluminum alloys of Examples 8-14 exhibit excellent overall performance, maintaining excellent yield strength (above 76 MPa) and tensile strength (above 160 MPa) while maintaining good electrical conductivity (above 47% IACS). Furthermore, compared to high-nickel cast aluminum alloys in the related art, the cast aluminum alloys of Examples 8-14 of the present disclosure have lower production costs due to their lower nickel content.
[0237] By comparing Examples 8-10, it can be found that when the Fe content is reduced, the electrical conductivity and elongation of the cast aluminum alloy are improved.
[0238] By comparing Example 9 and Example 11, it can be found that after the cast alloy of Example 11 undergoes T6 heat treatment, the electrical conductivity of the cast aluminum alloy is slightly reduced, the elongation is reduced, and the yield strength and tensile strength are also reduced. Overall, the cast aluminum alloy that has not undergone T6 heat treatment has better comprehensive performance.
[0239] A comparison of Examples 9 and 12 shows that maintaining the mold at room temperature during casting is more effective than preheating the mold in advance. This is because, compared to Example 12, where the mold was preheated in advance, Example 9 cast the aluminum alloy melt into an unpreheated mold. This increased the temperature gradient between the aluminum alloy melt and the mold, speeding up the cooling rate and improving the electrical conductivity, yield strength, tensile strength, and elongation of the cast aluminum alloy.
[0240] By comparing Example 9 with Comparative Examples 3-4, it can be seen that when the Cu content of Comparative Example 3 is lower than the content range defined in the embodiments of the present disclosure, the yield strength and tensile strength of the cast aluminum alloy are significantly reduced; when the Cu content of Comparative Example 4 is higher than the content range defined in the embodiments of the present disclosure, although the yield strength and tensile strength of the cast aluminum alloy are excellent, its electrical conductivity is greatly reduced.
[0241] By comparing Example 9 and Comparative Example 5, it can be seen that Comparative Example 5 adds Mg and Si while reducing the Cu content, resulting in a significant decrease in the yield strength, tensile strength and electrical conductivity of the cast aluminum alloy. Therefore, the cast aluminum alloys of the embodiments of the present disclosure do not include Mg and Si elements.
[0242] In the present disclosure, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present disclosure. In this specification, the schematic expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and features of different embodiments or examples without contradiction.
[0243] Although the embodiments of the present disclosure have been shown and described above, it is understood that the above embodiments are illustrative and are not to be construed as limitations on the present disclosure. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present disclosure.
Claims
1. A cast aluminum alloy for a motor rotor, wherein: The cast aluminum alloy comprises the following components, based on the total mass of the cast aluminum alloy being 100 wt. %: Fe 0.5-2wt.%, Ni 0.1-1wt.% Mg 0.1-0.5wt.%, The balance is Al and inevitable impurities.
2. The cast aluminum alloy for motor rotor according to claim 1, wherein: The cast aluminum alloy comprises the following components, based on the total mass of the cast aluminum alloy being 100 wt. %: Fe 0.5-1.5wt.%, Ni 0.5-1wt.% Mg 0.1-0.35wt.%, The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
3. The cast aluminum alloy for motor rotor according to claim 1, wherein: The total content of Fe and Ni is 2-2.5 wt.%.
4. The cast aluminum alloy for motor rotor according to claim 1, wherein: The (Fe, Ni)4Al in the cast aluminum alloy 13 The mole fraction of the phase is 4-6 mol%.
5. The cast aluminum alloy for a motor rotor according to any one of claims 1 to 4, wherein: The room temperature electrical conductivity of the cast aluminum alloy is greater than 50% IACS.
6. The cast aluminum alloy for a motor rotor according to any one of claims 1 to 4, wherein: The cast aluminum alloy has a yield strength of 65 MPa or more; and / or a tensile strength of 150 MPa or more.
7. The cast aluminum alloy for a motor rotor according to any one of claims 1 to 4, wherein: The cast aluminum alloy has a porosity of 0.3% or less and / or an elongation of 14% or more.
8. A cast aluminum alloy for a motor rotor, wherein: The cast aluminum alloy comprises the following components, based on the total mass of the cast aluminum alloy being 100 wt %: Fe 0.5-2wt%, Ni 0.3-1.5wt%, Cu 0.1-0.8wt%, The balance is Al and inevitable impurities.
9. The cast aluminum alloy according to claim 8, wherein The cast aluminum alloy comprises the following components, based on the total mass of the cast aluminum alloy being 100 wt %: Fe 1-1.5wt%, Ni 0.3-1wt%, Cu 0.1-0.6wt%, The balance is Al and unavoidable impurities, the content of a single impurity is ≤0.05wt.%, and the total impurity content is ≤0.15wt.%.
10. The cast aluminum alloy according to claim 8, wherein The total content of Fe and Ni is 0.8-3 wt%.
11. The cast aluminum alloy according to claim 10, wherein The total content of Fe and Ni is 2-2.5 wt%.
12. The cast aluminum alloy according to any one of claims 8 to 11, wherein The room temperature electrical conductivity of the cast aluminum alloy is greater than 47% IACS.
13. The cast aluminum alloy according to any one of claims 8 to 11, wherein The porosity of the cast aluminum alloy is 0.1% or less.
14. The cast aluminum alloy according to any one of claims 8 to 11, wherein The elongation of the cast aluminum alloy is greater than 13%.
15. The method for preparing a cast aluminum alloy for a motor rotor according to any one of claims 1 to 14, comprising the following steps: Aluminum alloy raw materials are added in proportion and smelted to obtain an aluminum alloy melt; the aluminum alloy melt is refined and degassed, and then cast into a casting mold to obtain the cast aluminum alloy.
16. The method for preparing a cast aluminum alloy for a motor rotor according to claim 15, wherein: The casting mold was not preheated and kept at room temperature.
17. The method for preparing a cast aluminum alloy for a motor rotor according to claim 15 or 16, wherein: The cast aluminum alloy is not subjected to heat treatment after being obtained.
18. The method for preparing a cast aluminum alloy for a motor rotor according to claim 15 or 16, wherein: The following steps are involved: Preheating the pit furnace in an empty state to remove moisture in the furnace at a preheating temperature of 400° C. or higher, preheating pure aluminum, and then placing the preheated pure aluminum into the pit furnace for smelting at a smelting temperature of 780-800° C. After the pure aluminum is completely melted, removing the surface slag and removing the oxide scale, maintaining the melt temperature, adding pure iron, pure nickel, and pure magnesium, or adding an aluminum-iron master alloy, an aluminum-nickel master alloy, and an aluminum-magnesium master alloy, or adding pure iron, pure nickel, and pure copper, and completely immersing the aluminum liquid, and after the aluminum alloy raw material is completely melted, standing for 2-3 hours to obtain the aluminum alloy melt; The refining agent is wrapped with aluminum foil and dried, and a stainless steel bell jar is preheated at the same time. The preheated refining agent is then pressed to the bottom of the aluminum alloy melt using the preheated stainless steel bell jar, and high-purity argon gas is introduced into the aluminum alloy melt to perform a refining and degassing process of the aluminum alloy melt, while maintaining the casting temperature at 700-740°C; the aluminum alloy melt is poured into the casting mold, and after the aluminum-iron-nickel alloy melt solidifies and cools, the casting is opened and removed from the mold to obtain a cast aluminum alloy.
19. A motor rotor, prepared from the cast aluminum alloy according to any one of claims 1 to 14.
20. An automobile comprising the motor rotor according to claim 19.
Citation Information
Patent Citations
Aluminum alloys for die casting
HK40042796A
High-conductivity and high-heat conductivity aluminum-iron-nickel-rare earth alloy
CN104658630A
Preparation method of environment-friendly electric car cable aluminum alloy rod
CN105256181A
High-thermal-conductivity and low-expansion wrought aluminum alloy and preparation method thereof
CN113502419A
Aluminum alloy fin material for vapor phase brazing
JP1991094037A
Cited By
Aluminum alloy, preparation method thereof and aluminum alloy rotor
CN121472651A