Zinc-plated steel sheet, member, and methods for producing same

The optimization of the base steel composition and structure, combined with a controlled manufacturing process, effectively addresses hydrogen embrittlement in high-strength galvanized steel sheets, enhancing workability and tensile strength while preventing weld cracking.

WO2024224583A1PCT designated stage expired Publication Date: 2024-10-31JFE STEEL CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/016786
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

High-strength hot-dip galvanized steel sheets face challenges with hydrogen embrittlement and reduced workability due to hydrogen penetration during manufacturing, leading to issues with bendability, stretch flangeability, and cracking in spot welds, which existing methods fail to adequately address.

Method used

A galvanized steel sheet with a base steel composition and structure optimized to reduce diffusible hydrogen, featuring a steel structure with tempered martensite and controlled carbide precipitation, along with a galvanized layer, to enhance hydrogen trapping and embrittlement resistance, and a manufacturing process that includes specific heating and cooling steps to minimize hydrogen retention.

Benefits of technology

The solution achieves a high yield ratio, excellent bendability, and hydrogen embrittlement resistance, ensuring a tensile strength of 780 MPa to 1180 MPa, while preventing cracking in spot welds and maintaining ductility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention provides a technology for a zinc-plated steel sheet that has a high yield ratio, excellent bendability and stretch flangeability, and excellent hydrogen embrittlement resistance, and has a TS of not less than 780 MPa but less than 1180 MPa. This zinc-plated steel sheet comprises: a steel structure in which the area percentage of ferrite is less than 65%, the total area percentage of martensite and bainite is at least 25%, the area percentage of residual austenite is 3-10%, and at least 70% of all martensite in the steel structure at 1 / 8 to 3 / 8 of the thickness of a base steel sheet is tempered martensite containing a carbide having an average particle size of 50-200 nm; and a zinc plating layer formed on the base steel sheet. The zinc-plated steel sheet has a TS of not less than 780 MPa but less than 1180 MPa, a yield ratio of at least 0.60, and a diffusible hydrogen amount of at most 0.45 ppm by mass.
Need to check novelty before this filing date? Find Prior Art

Description

Galvanized steel sheets, components, and their manufacturing methods

[0001] The present invention relates to a high-strength galvanized steel sheet having excellent formability, a member made from the high-strength galvanized steel sheet, and a method for manufacturing the same. The galvanized steel sheet of the present invention is suitable for use mainly as an automotive steel sheet.

[0002] In recent years, from the perspective of global environmental conservation, 2 There is a strong demand for improved fuel efficiency to reduce emissions. Accordingly, there has been a growing trend to reduce the weight of vehicle bodies by thinning the thickness of body parts, which has led to a growing need for higher strength steel sheets for these components. In particular, to ensure automobile crashworthiness, steel sheets used around the cabin must have not only high tensile strength but also high yield strength. Furthermore, to ensure that high strength does not impair the freedom of part shape, they must also possess press formability. Furthermore, if corrosion progresses during use as an automotive part, the material may not be able to demonstrate its original strength in the event of a collision. Therefore, the use of hot-dip galvanized steel sheets, which have excellent corrosion resistance, is expanding.

[0003] However, increasing the strength of steel sheets raises concerns about hydrogen embrittlement. Hydrogen embrittlement in high-strength steel sheets can be caused not only by hydrogen infiltrating from the outside due to corrosion during use, but also by hydrogen infiltrating during the manufacturing process. In particular, hot-dip galvanized steel sheets are typically manufactured by performing a series of processes, from annealing to hot-dip galvanizing, continuously in a hydrogen-containing atmosphere to prevent reduction and oxidation of the steel sheet. As a result, the galvanized layer is formed while retaining hydrogen that infiltrated from the atmosphere. Hydrogen diffusion during galvanization is very slow, acting as a barrier to the external release of diffusible hydrogen in the steel. This residual diffusible hydrogen can promote cracking during processing, leading to hydrogen embrittlement and a risk of deteriorating local ductility, particularly in bendability and stretch flangeability. Therefore, it is important to establish hot-dip galvanized steel sheets with excellent hydrogen embrittlement resistance and a manufacturing method for such steel sheets, in which hydrogen in the steel is sufficiently reduced.

[0004] Regarding the problems related to the workability and hydrogen embrittlement resistance of high-strength hot-dip galvanized steel sheets, for example, Patent Document 1 discloses a high-strength hot-dip galvanized steel sheet excellent in bendability and a method for manufacturing the same. Also, Patent Document 2 discloses a high-strength steel sheet of TS900 MPa or more excellent in ductility and delayed fracture resistance, a method for manufacturing a high-strength cold-rolled steel sheet, and a method for manufacturing a high-strength galvanized steel sheet.

[0005] International Publication No. 2016 / 113788 Japanese Patent Application Laid-Open No. 2011-111671

[0006] However, while Patent Document 1 describes improving bendability by refining martensite grains, it does not disclose a method for improving hydrogen embrittlement resistance. Furthermore, Patent Document 2 describes achieving both ductility and hydrogen embrittlement resistance, but only deals with hydrogen embrittlement resistance after processing, and does not describe improving hydrogen embrittlement resistance due to hydrogen intrusion into the steel during manufacturing. It is believed that the manufacturing methods disclosed in these patent documents leave a large amount of hydrogen in the steel, which poses a risk of hydrogen embrittlement occurring during the processing process, such as deterioration of bendability and stretch flangeability, and cracking in nuggets at spot welds.

[0007] The present invention has been made in view of the above circumstances, and provides a galvanized steel sheet and member suitable for automotive applications, which have a high yield ratio (YR), excellent bendability and stretch flangeability, and excellent hydrogen embrittlement resistance, and which have a tensile strength (TS) of 780 MPa or more but less than 1180 MPa, and a method for manufacturing the same.

[0008] Here, a high yield ratio means that a JIS No. 5 tensile test piece (JIS Z2201) is taken in the direction perpendicular to the rolling direction, and the strain rate is increased to 10 -3 A tensile test is conducted in accordance with the provisions of JIS Z2241 (2011) where YR is 0.60 or more.

[0009] The tensile strength (TS) was measured by taking JIS No. 5 tensile test pieces (JIS Z2201) perpendicular to the rolling direction and -3 This refers to the tensile strength obtained by conducting a tensile test in accordance with the provisions of JIS Z2241 (2011) where tensile strength is 1 / s.

[0010] "Excellent bendability" means that 35 mm x 100 mm strip test pieces are taken from a galvanized steel sheet so that the bending test axis is parallel to the rolling direction, and a 90-degree V-bend test is performed at various bending radii at a stroke speed of 50 mm / s, an indentation load of 10 ton, and a holding time of 5 seconds. The ridge line at the bend apex of the test piece is observed with a 10x magnifying glass, and R / t, which is the value obtained by dividing the minimum bending radius R (mm) at which no cracks of 0.5 mm or more in length were observed by the sheet thickness (mm), is determined, and either (A) or (B) below is satisfied: (A) TS: 780 MPa or more but less than 980 MPa, and R / t: 4.5 or less; or (B) TS: 980 MPa or more but less than 1180 MPa, and R / t: 5.0 or less.

[0011] "Excellent stretch flangeability" refers to a test piece of 100 mm x 100 mm taken from a galvanized steel sheet, a hole of 10 mm diameter formed at the center of the test piece by punching with a clearance of 12.5%, and then using a die with an inner diameter of 75 mm, a blank holding force of 9 tons (88.26 kN) is applied around the hole, and a conical punch with an apex angle of 60° is pressed into the hole to expand it, and the diameter of the hole when a crack occurs is measured, and the critical hole expanding ratio λ (%) calculated from the following formula (1) is 35% or more. λ (%) = {(D f -D 0 ) / D 0}×100...Formula (1) D f D: diameter of hole at crack occurrence (mm) 0 : Hole diameter before hole expansion (mm)

[0012] "Excellent hydrogen embrittlement resistance" refers to a nugget having cracks of 100 μm or less when spot welding is performed using the following method. (1) A 30 mm x 100 mm test piece taken from a galvanized steel sheet is prepared by sandwiching a 2 mm thick spacer between both ends and spot welding the center between the spacers to prepare a welded test piece. (2) An inverter DC resistance spot welding machine is used for spot welding, and a dome-shaped electrode made of chromium copper with a tip diameter of 6 mm is used. The pressure is 380 kgf, the current flow time is 16 cycles / 50 Hz, and the hold time is 5 cycles / 50 Hz. (3) The welding current value is adjusted to form a nugget diameter corresponding to the sheet thickness. The nugget diameter satisfies the following formula (2): 3.0 x t 1/2 < Nugget diameter < 3.5 x t 1/2 ...Equation (2) In equation (2), t is the plate thickness (mm). (4) After leaving the nugget for 24 hours after spot welding, the spacer portion is cut off and the cross section of the nugget is observed.

[0013] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result, have found that diffusible hydrogen in steel can be reduced by optimizing the steel sheet structure and appropriately controlling the precipitation morphology of carbides in the steel and utilizing them as hydrogen trapping sites, thereby making it possible to obtain a high-strength galvanized steel sheet that has a high yield ratio, excellent bendability, and a low risk of cracking in nuggets at spot welds.

[0014] The present invention was made based on this finding, and its gist is as follows: [1] A galvanized steel sheet having a base steel sheet and a galvanized layer formed on the base steel sheet, wherein the base steel sheet has a steel structure having, in area ratios, ferrite: less than 65%, a total of martensite and bainite: 25% or more, and retained austenite: 3% to 10%, wherein, in area ratios, 70% or more of all martensite in the steel structure within 1 / 8 to 3 / 8 of the sheet thickness of the base steel sheet is tempered martensite having carbides with an average grain size of 50 nm to 200 nm, wherein the galvanized steel sheet has a tensile strength of 780 MPa or more and less than 1180 MPa, a yield ratio of 0.60 or more, and wherein the integrated value of the amount of hydrogen released when the base steel sheet is heated from room temperature to 200°C is 0.45 ppm by mass or less. [2] The galvanized steel sheet according to [1], wherein the steel components of the base steel sheet contain, in mass%, C: 0.080% or more and 0.300% or less, Si: 0.20% or more and 2.00% or less, Mn: 1.00% or more and 4.00% or less, P: 0.10% or less, S: 0.0200% or less, Al: 0.003% or more and 0.100% or less, N: 0.0100% or less, with the balance being Fe and unavoidable impurities. [3] The steel components further include, in mass%, B: 0.0100% or less, Ti: 0.200% or less, Nb: 0.200% or less, Sb: 0.200% or less, Sn: 0.200% or less, V: 0.100% or less, Cu: 2.00% or less, Cr: 2.00% or less, Ni: 2.00% or less, Mo: 1.00% or less, Ta: 0.100% or less, W: 0.500% or less, Zr: 0.020% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, Zn: 0.020% or less, Co: 0.020% or less, Ce: 0.0200% or less, Se: 0.0200% or less, The galvanized steel sheet according to [2], containing at least one selected from Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0200% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM (excluding Ce): 0.0200% or less.[4] The galvanized steel sheet according to any one of [1] to [3], wherein the base steel sheet has a soft surface layer in the surface layer, the Vickers hardness of which is 85% or less of the Vickers hardness at a position 1 / 4 of the sheet thickness, when the surface layer is an area of ​​200 μm or less from the surface of the base steel sheet in the sheet thickness direction. [5] The galvanized steel sheet according to [4], wherein, when the nanohardness is measured at 300 or more points in a 50 μm × 50 μm region of the sheet surface at a position 1 / 4 of the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet and a position 1 / 2 of the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet, the ratio of the number of measurements where the nanohardness of the sheet surface at a position 1 / 4 of the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet is 7.0 GPa or more to the total number of measurements is 0.10 or less, further, the standard deviation σ of the nanohardness of the sheet surface at a position 1 / 4 of the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet is 1.8 GPa or less, and further, the standard deviation σ of the nanohardness of the sheet surface at a position 1 / 2 of the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet is 2.2 GPa or less. [6] The galvanized steel sheet according to any one of [1] to [5], which has a metal plating layer formed between the base steel sheet and the galvanized layer on one or both sides of the galvanized steel sheet. [7] The galvanized steel sheet according to any one of [1] to [6], wherein the galvanized layer is a galvannealed plating layer. [8] The galvanized steel sheet according to any one of [1] to [7], wherein when the base steel sheet is heated from room temperature to 600°C, the integrated value of the amount of hydrogen released in a temperature range of 350 to 600°C is 0.05 ppm by mass or more. [9] A member made using the galvanized steel sheet according to any one of [1] to [8].

[10] A hot rolling process in which a slab having the steel composition according to [2] or [3] is heated to a temperature range of 1100 to 1350°C, hot rolled at a finish rolling end temperature of 800 to 950°C, and coiled at a coiling temperature of 650°C or less; a reducing process in which the steel sheet after the hot rolling process is held at 700°C or higher in a reducing atmosphere having a hydrogen concentration of 8 to 30% by volume for 20 seconds or more; a soaking process in which the steel sheet after the reducing process is held at 750°C or higher in a soaking atmosphere having a hydrogen concentration of 0.2 to 8% by volume for 20 seconds or more and 300 seconds or less; a first cooling process in which the steel sheet after the soaking process is cooled; and a galvanizing process in which a galvanized layer is formed on the surface of the steel sheet after the first cooling process. A method for producing a galvanized steel sheet, comprising: a second cooling step in which the steel sheet after the galvanizing step is cooled from a temperature range of 350 to 450°C to (Ms point - 100°C) at an average cooling rate of 20°C / s or less, and is allowed to remain in a temperature range of 100 to 350°C for 5 seconds or more, to a cooling stop temperature of 100 to 300°C; and a reheating step in which the steel sheet after the second cooling step is held in a temperature range of not less than the cooling stop temperature and not more than 450°C for 5 to 600 seconds.

[11] The method for producing a galvanized steel sheet according to

[10] above, wherein, after the galvanizing step, the galvanized layer is formed on the surface of the steel sheet, and then the steel sheet is further subjected to an alloying treatment.

[12] The method for producing a galvanized steel sheet according to

[10] or

[11] above, comprising a cold rolling step in which the steel sheet is cold rolled at a reduction of 20% or more after the hot rolling step and before the reducing step.

[13] The method for producing a galvanized steel sheet according to any one of

[10] to

[12] above, wherein in the first cooling step, the steel sheet after the soaking step is cooled from 600 to 900°C to 150 to 500°C at an average cooling rate of 20°C / s or less in an atmosphere having a hydrogen concentration of 0.5 vol% or more and 30 vol% or less and a dew point of 0°C or less.

[14] The method for producing a galvanized steel sheet according to any one of

[10] to

[13] above, wherein in the second cooling step, the steel sheet is cooled from a temperature range of 350 to 450°C to (Ms point - 100°C) at an average cooling rate of 10°C / s or less, and is allowed to remain in a temperature range of 100 to 350°C for 10 seconds or more, to a cooling stop temperature of 100 to 300°C.

[15] The method for producing a galvanized steel sheet according to any one of

[10] to

[14] above, wherein the soaking atmosphere in the soaking step is an atmosphere with a dew point of −30° C. or higher.

[16] The method for producing a galvanized steel sheet according to any one of

[10] to

[15] above, including a pre-plating step of applying a metal plating to one or both sides of the steel sheet after the hot rolling step and before the reducing step to form a metal plating layer.

[17] The method for producing a galvanized steel sheet according to any one of

[10] to

[16] above, including an oxidation step of heating the steel sheet after the hot rolling step and before the reducing step to 600° C. or higher in an oxidizing atmosphere containing an oxygen concentration of 1,000 ppm by volume or more and 30,000 ppm by volume or less.

[18] A method for producing a member, including a step of subjecting the galvanized steel sheet according to any one of [1] to [8] above to at least one of forming and joining to produce a member.

[0015] The galvanized steel sheet provided by the present invention has a tensile strength of 780 MPa or more and less than 1180 MPa, a yield ratio of 0.60 or more, and excellent bendability, stretch-flangeability, and hydrogen embrittlement resistance. Also, the member provided by the present invention has a tensile strength of 780 MPa or more and less than 1180 MPa, a yield ratio of 0.60 or more, and excellent bendability, stretch-flangeability, and hydrogen embrittlement resistance.

[0016] Fig. 1 is a diagram for explaining (a) the primary bending process and (b) the secondary bending process in the U-bend + contact bending test and the V-bend + orthogonal VDA bending test of the examples. Fig. 2 is a (a) front view and (b) perspective view of a test member manufactured for the axial crush test of the examples, in which a hat-shaped member and a steel plate are spot-welded, and (c) a schematic diagram for explaining the axial crush test.

[0017] The present invention will be described in detail below.

[0018] <Galvanized Steel Sheet> The galvanized steel sheet of the present invention is a galvanized steel sheet having a base steel sheet and a galvanized layer formed on the base steel sheet, wherein the base steel sheet has a steel structure which, in area ratio, is less than 65% ferrite, a total of 25% or more of martensite and bainite, and 3% to 10% or less retained austenite, and 70% or more of all martensite in the steel structure at ⅛ to ⅜ of the sheet thickness of the base steel sheet, in area ratio, is tempered martensite having carbides having an average particle size of 50 nm to 200 nm, and the galvanized steel sheet has a tensile strength of 780 MPa or more and less than 1180 MPa, a yield ratio of 0.60 or more, and an integrated value of the amount of hydrogen released when the base steel sheet from which the galvanized layer has been peeled is heated from room temperature to 200°C is 0.45 ppm by mass or less.

[0019] First, we will explain the area ratio of each structure in the base steel sheet of the present invention. The area ratio of each structure refers to the area ratio of each constituent phase to the total observed area. The area ratio of each structure can be determined from image data obtained by polishing a steel sheet cross section parallel to the rolling direction, corroding it with nital solution, and photographing it with a scanning electron microscope (SEM) at 1500x magnification. The measurement areas are a region extending from the surface to 1 / 8 of the sheet thickness and a region extending from 1 / 8 to 3 / 8 of the sheet thickness. In the image data, ferrite is black, bainite is black containing island-shaped retained austenite or gray containing uniformly oriented carbides, tempered martensite is light gray containing fine, randomly oriented carbides, and retained austenite is white. Here, as-quenched martensite and retained austenite both appear white, making them difficult to distinguish from SEM images. Therefore, the area fraction of retained austenite is determined individually by measuring its X-ray diffraction intensity, and the area fraction of as-quenched martensite is determined by subtracting this from the area fraction of the white area described above. The area fraction of retained austenite is determined from the ratio of the integrated X-ray diffraction intensity of the (200), (220), and (311) planes of fcc iron to the integrated X-ray diffraction intensity of the (200), (211), and (220) planes of bcc iron in the quarter-thickness plane. Although retained austenite is calculated as a volume fraction by the above measurement, the volume fraction of retained austenite is taken as the area fraction of retained austenite, assuming that the retained austenite is three-dimensionally homogeneous. Note that the martensite defined in the present invention includes both as-quenched martensite and tempered martensite, and may consist of as-quenched martensite and tempered martensite.

[0020] Ferrite area ratio: less than 65% If the ferrite area ratio is 65% or more, a TS of 780 MPa or more may not be obtained. Therefore, the ferrite area ratio is less than 65%, preferably less than 60%. The lower limit is not particularly limited and may be 0%, but from the viewpoint of the balance between tensile strength and ductility, the ferrite area ratio is preferably 5% or more, more preferably 10% or more.

[0021] Total area ratio of martensite (including tempered martensite) and bainite: 25% or more. Martensite is a hard structure formed from austenite at a low temperature below the martensitic transformation start point (Ms point). In the present invention, martensite includes not only as-quenched martensite (as-quenched martensite) but also tempered martensite obtained by tempering formed martensite at a predetermined temperature. Bainite is formed from austenite at a relatively low temperature above the Ms point and is a hard structure in which fine carbides are dispersed in acicular or plate-like ferrite. Martensite and bainite are responsible for the strength of the steel sheet of the present invention. If the total area ratio is less than 25%, a TS of 780 MPa or more may not be achieved. Therefore, the total area ratio of martensite and bainite is 25% or more, preferably 30% or more. Note that only one of martensite and bainite may be within the above range. Although there is no particular upper limit, the total area ratio of martensite (including tempered martensite) and bainite is preferably 85% or less, and more preferably 80% or less, from the viewpoint of more suitably controlling the balance between TS and ductility.

[0022] Area fraction of retained austenite: 3% or more and 10% or less If an excessive amount of retained austenite is contained, during bending or punching, work-induced transformation to hard martensite may promote crack generation and deteriorate bendability and hole expandability. This effect becomes significant when the retained austenite content exceeds 10%. Therefore, the area fraction of retained austenite is 10% or less. The area fraction of retained austenite is preferably 9% or less, and more preferably 8% or less. On the other hand, if the retained austenite content is less than 3%, sufficient ductility cannot be obtained. Therefore, the retained austenite content is 3% or more. The area fraction of retained austenite is preferably 4% or more, and more preferably 5% or more.

[0023] As long as the contents of ferrite, martensite, bainite, and retained austenite satisfy the above ranges, the remaining structure may contain other structures at an area ratio of 5% or less. Examples of other structures include pearlite.

[0024] Tempered martensite having carbides with an average grain size of 50 nm to 200 nm, accounting for 70% or more of the total martensite in the steel structure at ⅛ to ⅜ of the thickness of the base steel sheet, in terms of area fraction. In the present invention, by controlling the area fraction of the total martensite in the structure at ⅛ to ⅜ of the thickness of the base steel sheet so that 70% or more is tempered martensite having carbides of a predetermined size, a high yield ratio can be achieved through precipitation strengthening. At the same time, by utilizing fine carbides as hydrogen trapping sites in the steel to reduce diffusible hydrogen, excellent hydrogen embrittlement resistance can also be achieved. To fully achieve these effects, the area fraction of tempered martensite having carbides of a predetermined size is 70% or more, preferably 80% or more, and even 100%, of the total martensite in the structure at ⅛ to ⅜ of the thickness of the base steel sheet. This effect can be achieved by controlling the carbide size to be in the range of an average grain size of 50 nm to 200 nm. Generally, when the volume fraction of precipitates is constant, smaller precipitate grain sizes are advantageous for precipitation strengthening. Furthermore, from the perspective of hydrogen trapping, a larger surface area of ​​carbides is advantageous, so a smaller carbide grain size is preferable when the volume fraction is constant. Furthermore, coarse carbides can cause deterioration of bendability. Therefore, the average grain size of the carbides is 200 nm or less. On the other hand, when the average grain size of carbides is less than 50 nm, the carbide volume fraction decreases, and the precipitation strengthening and hydrogen trapping effects required for the present invention may not be fully achieved. For these reasons, in the present invention, tempered martensite having carbides with an average grain size of 50 nm to 200 nm inclusive is set to 70% or more of the total martensite in the 1 / 8 to 3 / 8 thickness of the base steel sheet. Here, the average grain size is the average of the major and minor axis lengths when approximated as an ellipse. The average grain size can be measured as an example using the method shown in the Examples.

[0025] The cumulative amount of hydrogen released when a base steel sheet from which the coating layer has been stripped is heated from room temperature to 200°C: 0.45 mass ppm or less. The galvanized steel sheet of the present invention effectively traps hydrogen that has entered the steel during the manufacturing process by controlling the amount of carbides in martensite to fall within the aforementioned range, thereby reducing diffusible hydrogen and providing excellent bendability, stretch-flangeability, and hydrogen embrittlement resistance. In the present invention, the cumulative amount of hydrogen released when a base steel sheet from which the coating layer (a zinc coating layer, including a metal coating layer, if present) has been stripped is heated from room temperature (15 to 35°C) to 200°C at a rate of 200°C / h is defined as the amount of diffusible hydrogen in the steel. If the amount of diffusible hydrogen exceeds 0.45 mass ppm, excellent bendability, stretch-flangeability, and hydrogen embrittlement resistance may not be achieved. Therefore, the amount of diffusible hydrogen is 0.45 mass ppm or less, preferably 0.40 mass ppm or less. The lower limit is not particularly limited, but since the smaller the amount of diffusible hydrogen, the better, it may be set to 0 ppm by mass.

[0026] When a base steel sheet from which the coating layer has been stripped is heated from room temperature to 600°C, the cumulative amount of hydrogen released in the temperature range of 350 to 600°C is 0.05 ppm by mass or more (preferred conditions). The galvanized steel sheet of the present invention effectively traps hydrogen that has entered the steel during the manufacturing process by controlling the amount of carbides in the martensite to fall within the aforementioned range, thereby reducing diffusible hydrogen. Hydrogen trapped in carbides is less likely to be desorbed from the steel than diffusible hydrogen, and is not released by heating up to 200°C, but is released at 350°C or higher. To fully achieve the effects of the present invention, when a steel sheet from which the coating layer (a zinc coating layer, including a metal coating layer, if present) has been stripped, is heated from room temperature (15 to 35°C) to 600°C at a rate of 200°C / h, the cumulative amount of hydrogen released in the temperature range of 350 to 600°C is preferably 0.05 ppm by mass or more. The upper limit is not particularly limited, but the integrated value of the amount of hydrogen released at 350 to 600°C may be 1.00 mass ppm or less.

[0027] The method for quantifying hydrogen in steel described above involves taking a test piece for hydrogen analysis measuring approximately 5 × 30 mm from a galvanized steel sheet, removing the surface galvanized layer (including the metal plating layer, if present) using a precision grinder, and quickly placing the test piece in a quartz tube whose atmosphere is replaced with Ar gas. The tube is heated to 600°C at a heating rate of 200°C / h, and the amount of released hydrogen during the heating period is measured using a gas chromatograph. The integrated value of the amount of hydrogen released in the temperature range from room temperature to 200°C is determined as the "diffusible hydrogen amount," and the integrated value of the amount of hydrogen released in the temperature range from 350°C to 600°C is determined as the "trapped hydrogen amount." Here, the measurement of the hydrogen amount is preferably performed after the completion of the steel sheet production. That is, the measurement of the diffusible hydrogen amount is preferably performed after the completion of the steel sheet production. Furthermore, the measurement of the trapped hydrogen amount is preferably performed after the completion of the steel sheet production. Furthermore, it is more preferable that the measurement of the amount of diffusible hydrogen and the amount of trapped hydrogen be carried out within 72 hours after the steel sheet first reaches room temperature (40°C or lower) after the reheating step specified in the present invention.

[0028] Zinc Plated Layer The galvanized steel sheet of the present invention has a zinc plated layer on a base steel sheet, and the zinc plated layer may be a galvannealed layer, a hot-dip galvannealed layer, or a galvannealed layer.

[0029] The galvanized steel sheet of the present invention has a zinc plating layer (a second plating layer when a metal plating layer (first plating layer) is formed) formed on a base steel sheet as the outermost layer (on the surface of the base steel sheet or on the surface of the metal plating layer when a metal plating layer is formed), and this zinc plating layer may be formed on only one surface of the base steel sheet, or on both surfaces. That is, the galvanized steel sheet of the present invention may have a base steel sheet on which a second plating layer (a zinc plating layer, an aluminum plating layer, etc.) is formed, or may have a base steel sheet on which a metal plating layer (a first plating layer (excluding a second plating layer of a zinc plating layer)) and a second plating layer (a zinc plating layer, an aluminum plating layer, etc.) are formed in that order on the base steel sheet.

[0030] The galvanized layer referred to here refers to a plating layer containing Zn as a main component (Zn content of 50.0% or more), and examples thereof include a galvanized layer such as a hot-dip galvanized layer and a galvannealed layer such as an alloyed hot-dip galvanized layer.

[0031] Here, the hot-dip galvanized layer (galvanized layer) is preferably composed of, for example, Zn, 20.0 mass% or less of Fe, and 0.001 mass% to 1.0 mass% of Al. The hot-dip galvanized layer may optionally contain one or more elements selected from the group consisting of Pb, Sb, Si, Sn, Mg, Mn, Ni, Cr, Co, Ca, Cu, Li, Ti, Be, Bi, and REM in a total amount of 0.0 mass% to 3.5 mass%. The Fe content of the hot-dip galvanized layer is more preferably less than 7.0 mass%. The remainder other than the above elements is unavoidable impurities.

[0032] The galvannealed layer (galvannealed layer) is preferably composed of, for example, 20% by mass or less of Fe and 0.001% by mass to 1.0% by mass of Al. The galvannealed layer may optionally contain one or more elements selected from the group consisting of Pb, Sb, Si, Sn, Mg, Mn, Ni, Cr, Co, Ca, Cu, Li, Ti, Be, Bi, and REM in a total amount of 0.0% by mass to 3.5% by mass. The Fe content of the galvannealed layer is more preferably 7.0% by mass or more, and even more preferably 8.0% by mass or more. The Fe content of the galvannealed layer is more preferably 15.0% by mass or less, and even more preferably 13.0% by mass or less. The remainder other than the above elements is unavoidable impurities.

[0033] In addition, the plating weight of the zinc plating layer per side is not particularly limited, but is preferably 20 g / m 2 The coating weight of the zinc plating layer on one side is preferably 80 g / m or more. 2 It is preferable to do the following:

[0034] The coating weight of the zinc plating layer is measured as follows. That is, a treatment solution is prepared by adding 0.6 g of a corrosion inhibitor for Fe (Ivit 700BK (registered trademark) manufactured by Asahi Chemical Industry Co., Ltd.) to 1 L of a 10 mass % aqueous hydrochloric acid solution. Next, a steel sheet to be used as a test material is immersed in the treatment solution to dissolve the zinc plating layer. The mass loss of the test material before and after dissolution is measured, and this value is divided by the surface area of ​​the base steel sheet (the surface area of ​​the part that was covered with the plating) to determine the coating weight (g / m 2 ) is calculated.

[0035] Next, a preferred composition of the steel sheet (base steel sheet (hereinafter sometimes simply referred to as steel sheet)) constituting the galvanized steel sheet will be described. Note that "%" representing the content of component elements means "mass %" unless otherwise specified.

[0036] C: 0.080% or more and 0.300% or less. C improves hardenability and makes it easier to obtain martensite and bainite. Furthermore, by precipitating fine carbides in the structure, C can trap hydrogen in the steel, reducing the amount of diffusible hydrogen and improving hydrogen embrittlement resistance. If the C content is less than 0.080%, it is impossible to achieve both the required strength and bendability. Therefore, the C content is preferably 0.080% or more, and more preferably 0.100% or more. On the other hand, if the C content exceeds 0.300%, the hydrogen trapping effect of the fine carbides saturates, and the strength of martensite becomes excessively high, which may impair ductility. Therefore, the C content is preferably 0.300% or less, and more preferably 0.250% or less.

[0037] Si: 0.20% or more and 2.00% or less. Si is an element effective in strengthening ferrite, which has excellent ductility. It also inhibits the formation of coarse carbides when annealed steel sheets are held at relatively low temperatures, thereby promoting the formation of retained austenite and contributing to an improved balance between strength and ductility. This effect is not fully achieved when the Si content is less than 0.20%. Therefore, the Si content is 0.20% or more, preferably 0.30% or more. On the other hand, when the Si content exceeds 2.00%, the carbide formation action becomes excessive, making it impossible to obtain the fine carbides in martensite required for the present invention. As a result, diffusible hydrogen in the steel increases, and the desired yield ratio and hydrogen embrittlement resistance of the present invention may not be achieved. Therefore, the Si content is preferably 2.00% or less, more preferably 1.50% or less.

[0038] Mn: 1.00% or more and 4.00% or less Mn improves the hardenability of steel, making it easier to obtain martensite and bainite. If the Mn content is less than 1.00%, the area ratio of ferrite becomes excessive, and the required strength and yield ratio may not be obtained. Therefore, the Mn content is preferably 1.00% or more, and more preferably 1.50% or more. On the other hand, if the Mn content exceeds 4.00%, the strength of martensite becomes excessively high, and the formation of coarse MnS is promoted, which may make it difficult to obtain excellent bendability. Therefore, the Mn content is preferably 4.00% or less, and more preferably 3.50% or less.

[0039] P: 0.10% or less Excessive P segregates at prior austenite grain boundaries, embrittling the grain boundaries and causing deterioration of bendability. Therefore, the P content is preferably 0.10% or less, more preferably 0.05% or less. The P content is preferably 0.03% or less, and more preferably 0.02% or less. Although there is no particular lower limit, since P is also an element effective in increasing the strength of steel sheet through solid solution strengthening, in order to obtain such an effect, the P content is preferably 0.001% or more. The P content may be 0.002% or more, or may be 0.005% or more.

[0040] S: 0.0200% or less S forms inclusions such as MnS, which causes deterioration of bendability. Therefore, the S content is preferably 0.0200% or less, and more preferably 0.0100% or less. Although there is no particular lower limit, due to constraints on production technology, the S content may be 0.0001% or more. The S content may be 0.0002% or more, or 0.0004% or more.

[0041] Al: 0.003% or more and 0.100% or less In addition to being used as a deoxidizer, Al also contributes to solid solution strengthening of steel. If the Al content is less than 0.003%, these effects may not be obtained. Therefore, the Al content is preferably 0.003% or more. The Al content is preferably 0.005% or more, and more preferably 0.007% or more. On the other hand, if the Al content exceeds 0.100%, it will cause deterioration of slab quality during steelmaking. Therefore, the Al content is preferably 0.100% or less, and more preferably 0.050% or less.

[0042] N: 0.0100% or less N forms coarse nitrides, which may become the starting point for void formation and reduce bendability. By setting the N content to 0.0100% or less, it is possible to prevent N from forming coarse nitrides. Therefore, the N content is preferably 0.0100% or less, and more preferably 0.0060% or less. There is no particular lower limit, but due to constraints on production technology, the N content may be 0.0005% or more.

[0043] The balance other than the above consists of Fe and unavoidable impurities. The steel sheet of the present invention preferably has a composition containing the above components, with the balance consisting of Fe and unavoidable impurities. The composition may further optionally contain a predetermined amount of at least one element selected from the following group of elements. When the following optional elements are contained in an amount less than the preferred lower limit, the optional elements can be considered to be contained as unavoidable impurities.

[0044] B: 0.0100% or less B is an element effective in improving the hardenability of steel. To improve hardenability, the B content is preferably 0.0001% or more, more preferably 0.0002% or more, and even more preferably 0.0003% or more. The B content is preferably 0.0005% or more, and preferably 0.0007% or more. In order to obtain better formability, when B is contained, the B content is preferably 0.0100% or less, more preferably 0.0050% or less, and even more preferably 0.0030% or less.

[0045] Ti: 0.200% or less Ti precipitates fine carbides, contributing to increased strength and hydrogen trapping effect. There is no particular lower limit for Ti, but to obtain these effects, it is preferably 0.001% or more, more preferably 0.005% or more, and even more preferably 0.010% or more. On the other hand, excessive Ti content may cause the carbides to coarsen, resulting in deterioration of bendability. Therefore, when Ti is contained, the Ti content is preferably 0.200% or less, more preferably 0.100% or less, and even more preferably 0.060% or less.

[0046] Nb: 0.200% or less Nb precipitates fine carbides, contributing to increased strength and hydrogen trapping effect. There is no particular limit on the lower limit of Nb, but to obtain these effects, it is preferably 0.001% or more, more preferably 0.005% or more, and even more preferably 0.010% or more. On the other hand, if Nb is contained in excess, the carbides may become coarse, which may cause deterioration in bendability. Therefore, when Nb is contained, the Nb content is preferably 0.200% or less, more preferably 0.100% or less, and even more preferably 0.060% or less.

[0047] Sb: 0.200% or less Sb is an element that is effective in suppressing excessive decarburization of the steel sheet surface and preventing a decrease in the amount of martensite formed. To achieve this effect, the Sb content is preferably 0.001% or more, more preferably 0.002% or more, and even more preferably 0.005% or more. On the other hand, when Sb is contained, to obtain better toughness, the Sb content is preferably 0.200% or less. The Sb content is more preferably 0.060% or less, and even more preferably 0.020% or less.

[0048] Sn: 0.200% or less Sn is an element that is effective in suppressing decarburization, denitrification, etc., and suppressing a decrease in the strength of steel. To achieve this effect, the Sn content is preferably 0.001% or more, more preferably 0.002% or more, and even more preferably 0.005% or more. On the other hand, in order to obtain better impact resistance, when Sn is contained, the Sn content is preferably 0.200% or less. The Sn content is more preferably 0.060% or less, and even more preferably 0.020% or less.

[0049] V: 0.100% or less V precipitates fine carbides, contributing to increased strength and hydrogen trapping effect. There is no particular lower limit for V, but to achieve these effects, it is preferably 0.001% or more, more preferably 0.002% or more, and even more preferably 0.005% or more. The V content is preferably 0.007% or more, and more preferably 0.009% or more. On the other hand, excessive V content may cause coarsening of carbides, which may lead to deterioration of bendability. Therefore, when V is contained, the V content is preferably 0.100% or less, more preferably 0.080% or less, and even more preferably 0.060% or less.

[0050] Cu: 2.00% or less Cu is an element that improves hardenability and is effective for keeping the area ratio of the hard phase within a more preferable range. To achieve this effect, the Cu content is preferably 0.005% or more, more preferably 0.010% or more, and even more preferably 0.020% or more. The Cu content is preferably 0.040% or more, and preferably 0.060% or more. Furthermore, when Cu is contained, from the viewpoint of preventing an increase in cost, the Cu content is preferably 2.00% or less, more preferably 1.00% or less, and even more preferably 0.50% or less.

[0051] Cr: 2.00% or less The addition of Cr can improve hardenability and the balance between strength and ductility. To achieve this effect, the Cr content is preferably 0.001% or more, more preferably 0.002% or more, and even more preferably 0.005% or more. The Cr content is preferably 0.007% or more, and preferably 0.009% or more. Furthermore, when Cr is contained, from the viewpoint of preventing an increase in costs, the Cr content is preferably 2.00% or less, more preferably 1.00% or less, and even more preferably 0.80% or less.

[0052] Ni: 2.00% or less The addition of Ni can improve hardenability and the balance between strength and ductility. To achieve this effect, the Ni content is preferably 0.005% or more, more preferably 0.010% or more, and even more preferably 0.020% or more. The Ni content is preferably 0.030% or more, and preferably 0.040% or more. Furthermore, when Ni is contained, from the viewpoint of preventing an increase in cost, the Ni content is preferably 2.00% or less, more preferably 1.00% or less, and even more preferably 0.80% or less. The Ni content is preferably 0.60% or less, and preferably 0.40% or less.

[0053] Mo: 1.00% or less The addition of Mo can provide a strength adjustment effect. To achieve this effect, the Mo content is preferably 0.005% or more, more preferably 0.01% or more, and even more preferably 0.02% or more. The Mo content is preferably 0.03% or more, and preferably 0.04% or more. Furthermore, when Mo is contained, from the viewpoint of preventing an increase in cost, the Mo content is preferably 1.00% or less, more preferably 0.80% or less, and even more preferably 0.60% or less. The Mo content is preferably 0.50% or less, and preferably 0.40% or less.

[0054] Ta: 0.100% or less The addition of Ta can provide the effect of improving strength. To achieve this effect, the Ta content is preferably 0.001% or more, more preferably 0.002% or more, and even more preferably 0.003% or more. Furthermore, when Ta is contained, from the viewpoint of preventing an increase in costs, the Ta content is preferably 0.100% or less. The Ta content is more preferably 0.050% or less, and even more preferably 0.020% or less. The Ta content is preferably 0.010% or less, and preferably 0.008% or less.

[0055] W: 0.500% or less The addition of W can provide the effect of improving strength. To achieve this effect, the W content is preferably 0.001% or more, more preferably 0.002% or more, and even more preferably 0.003% or more. The W content is preferably 0.005% or more, and preferably 0.007% or more. Furthermore, when W is contained, from the viewpoint of preventing an increase in cost, the W content is preferably 0.500% or less, more preferably 0.450% or less, and even more preferably 0.400% or less. The W content is preferably 0.350% or less, and preferably 0.300% or less.

[0056] Zr: 0.020% or less The addition of Zr can improve the ultimate deformability of the steel sheet and improve the stretch flangeability. To achieve this effect, the Zr content is preferably 0.0005% or more, more preferably 0.0010% or more, and even more preferably 0.0015% or more. Furthermore, when Zr is contained, from the viewpoint of preventing an increase in costs, the Zr content is preferably 0.020% or less. The Zr content is more preferably 0.010% or less, and even more preferably 0.0050% or less.

[0057] Ca: 0.0200% or less By containing Ca, the morphology of sulfides can be controlled and ductility and toughness can be further improved. In order to obtain better ductility, when Ca is contained, the Ca content is preferably 0.0200% or less. The Ca content is more preferably 0.0100% or less, and even more preferably 0.0050% or less. The Ca content is preferably 0.0040% or less, and preferably 0.0030% or less. In addition, the lower limit of the Ca content is not particularly limited and may be 0.0000%. However, due to constraints on production technology, the Ca content is preferably 0.0001% or more. In addition, from the viewpoint of controlling the morphology of the sulfides and further improving ductility and toughness, the Ca content is more preferably 0.0005% or more.

[0058] Mg: 0.0200% or less By including 0.0001% or more of Mg, the morphology of sulfides can be controlled and ductility and toughness can be improved. The content is more preferably 0.0005% or more, and even more preferably 0.001% or more. Furthermore, in order to obtain better ductility, when Mg is included, the Mg content is preferably 0.0200% or less. The Mg content is more preferably 0.0100% or less, and even more preferably 0.0050% or less.

[0059] Zn: 0.020% or less The addition of Zn can improve the ultimate deformability of the steel sheet and improve stretch flangeability. To achieve this effect, the Zn content is preferably 0.001% or more, more preferably 0.002% or more, and even more preferably 0.003% or more. Furthermore, when Zn is contained, from the viewpoint of preventing an increase in cost, the Zn content is preferably 0.020% or less. The Zn content is more preferably 0.010% or less, and even more preferably 0.008% or less.

[0060] Co: 0.020% or less The addition of Co can improve the ultimate deformability of the steel sheet and improve stretch flangeability. To achieve this effect, the Co content is preferably 0.001% or more, more preferably 0.002% or more, and even more preferably 0.003% or more. Furthermore, when Co is contained, the Co content is preferably 0.020% or less from the viewpoint of preventing an increase in cost. The Co content is more preferably 0.010% or less, and even more preferably 0.008% or less.

[0061] Content of each of Ce, Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM (excluding Ce): 0.0200% or less. Addition of these elements improves the ultimate deformability of the steel sheet and improves stretch flangeability. To achieve this effect, it is preferable to contain at least one of these elements in an amount of 0.0001% or more. On the other hand, from the viewpoint of preventing an increase in cost, when at least one of these elements is contained, it is preferable that the content of each be 0.0200% or less. Ce is more preferably 0.0002% or more, and even more preferably 0.0005% or more. Furthermore, Ce is more preferably 0.0150% or less, and even more preferably 0.0100% or less. Ce is preferably 0.0080% or less, and even more preferably 0.0060% or less. The Se content is preferably 0.0002% or more, and even more preferably 0.0005% or more. The Se content is preferably 0.0007% or more, and even more preferably 0.0009% or more. The Se content is more preferably 0.0150% or less, and even more preferably 0.0100% or less. The Se content is preferably 0.0080% or less, and even more preferably 0.0060% or less. The Te content is more preferably 0.0002% or more, and even more preferably 0.0005% or more. The Te content is preferably 0.0007% or more, and even more preferably 0.0009% or more. The Te content is more preferably 0.0150% or less, and even more preferably 0.0100% or less. The Ge content is more preferably 0.0002% or more, and even more preferably 0.0005% or more. Ge is preferably 0.0007% or more, and more preferably 0.0009% or more. Ge is more preferably 0.0150% or less, and even more preferably 0.0100% or less. As is more preferably 0.0002% or more, and even more preferably 0.0005% or more. As is preferably 0.0007% or more, and even more preferably 0.0009% or more.As is more preferably 0.0150% or less, and even more preferably 0.0100% or less. Sr is more preferably 0.0002% or more, and even more preferably 0.0005% or more. Sr is preferably 0.0007% or more, and even more preferably 0.0009% or more. Sr is more preferably 0.0150% or less, and even more preferably 0.0100% or less. Cs is more preferably 0.0002% or more, and even more preferably 0.0005% or more. Cs is preferably 0.0007% or more, and even more preferably 0.0009% or more. Cs is more preferably 0.0150% or less, and even more preferably 0.0100% or less. Hf is more preferably 0.0002% or more, and even more preferably 0.0005% or more. Hf is preferably 0.0007% or more, and more preferably 0.0009% or more. Hf is more preferably 0.0150% or less, and even more preferably 0.0100% or less. Pb is more preferably 0.0002% or more, and even more preferably 0.0005% or more. Pb is preferably 0.0007% or more, and even more preferably 0.0009% or more. Pb is more preferably 0.0150% or less, and even more preferably 0.0100% or less. Pb is preferably 0.0080% or less, and even more preferably 0.0060% or less. Bi is more preferably 0.0002% or more, and even more preferably 0.0005% or more. Bi is preferably 0.0007% or more, and even more preferably 0.0009% or more. Bi is more preferably 0.0150% or less, and even more preferably 0.0100% or less. Bi is preferably 0.0080% or less, and even more preferably 0.0060% or less. REM is more preferably 0.0002% or more, and even more preferably 0.0005% or more. REM is preferably 0.0007% or more, and even more preferably 0.0009% or more.The REM content is more preferably 0.0150% or less, and even more preferably 0.0100% or less. The REM content defined in the present invention excludes the aforementioned Ce. The REM content in the present invention refers to scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanides ranging from lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. The REM concentration in the present invention refers to the total content of one or more elements selected from the above-mentioned REMs. While the REM content is not particularly limited, Sc, Y, and La are preferred.

[0062] Soft Surface Layer The base steel sheet of the galvanized steel sheet according to one embodiment of the present invention preferably has a soft surface layer on the surface. The soft surface layer contributes to suppressing bending crack propagation during press forming and vehicle collisions, thereby further improving bending fracture resistance. The soft surface layer refers to a decarburized layer, a surface region having a Vickers hardness of 85% or less of the Vickers hardness of a cross section (a plane parallel to the steel sheet surface) at 1 / 4 of the sheet thickness. The soft surface layer is formed to a thickness of 200 μm or less from the surface of the base steel sheet in the sheet thickness direction. The region where the soft surface layer is formed is preferably 150 μm or less, more preferably 120 μm or less, from the surface of the base steel sheet in the sheet thickness direction. While there is no particular lower limit for the thickness of the soft surface layer, it is preferably 7 μm or more, more preferably 14 μm or more, and even more preferably 17 μm or more. The soft surface layer is preferably 30 μm or more, more preferably 40 μm or more. The position at 1 / 4 of the sheet thickness of the base steel sheet where the Vickers hardness is measured is a non-soft surface layer (a layer that does not satisfy the hardness conditions of the soft surface layer specified in the present invention). The Vickers hardness is measured based on JIS Z 2244-1 (2020) at a load of 10 gf.

[0063] Nano-hardness of soft surface layer In the galvanized steel sheet of the present invention, when the nano-hardness is measured at 300 or more points in a 50 μm × 50 μm region of the sheet surface at a position 1 / 4 of the way to the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet and at a position 1 / 2 of the way to the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet, it is preferable that the ratio of the number of measurements where the nano-hardness of the sheet surface at a position 1 / 4 of the way to the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet is 7.0 GPa or more is 0.10 or less relative to the total number of measurements, and further, the standard deviation σ of the nano-hardness of the sheet surface at a position 1 / 4 of the way to the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet is 1.8 GPa or less, and further, the standard deviation σ of the nano-hardness of the sheet surface at a position 1 / 2 of the way to the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet is 2.2 GPa or less.

[0064] When the proportion of the number of pieces having a nano-hardness of 7.0 GPa or more is 0.10 or less relative to the total number of measurements, this means that the proportion of hard structures (such as martensite), inclusions, etc. is small, and it becomes possible to further suppress the generation and connection of voids and the growth of cracks in the hard structures (such as martensite), inclusions, etc. during press forming and collision, thereby obtaining excellent R / t and SFmax.

[0065] Furthermore, in order to obtain excellent bendability during press forming and excellent bending fracture properties during collision, it is preferable that the standard deviation σ of the nanohardness of the sheet surface at a position ¼ of the thickness direction depth of the soft surface layer from the surface of the base steel sheet be 1.8 GPa or less, and further, the standard deviation σ of the nanohardness of the sheet surface at a position ½ of the thickness direction depth of the soft surface layer from the surface of the base steel sheet be 2.2 GPa or less. When the standard deviation σ of the nanohardness of the sheet surface at a position ¼ of the thickness direction depth of the soft surface layer from the surface of the base steel sheet is 1.8 GPa or less, and further, the standard deviation σ of the nanohardness of the sheet surface at a position ½ of the thickness direction depth of the soft surface layer from the surface of the base steel sheet is 2.2 GPa or less, this means that the difference in microstructural hardness in the microregion is small, and because the difference in microstructural hardness in the microregion is small, it is possible to further suppress the generation and connection of voids and the propagation of cracks during press forming and collision, and excellent R / t and SFmax are obtained. Furthermore, the standard deviation σ of the nanohardness of the sheet surface at a position ¼ of the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet is preferably 1.7 GPa or less. The standard deviation σ of the nanohardness of the sheet surface at a position ¼ of the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet is more preferably 1.3 GPa or less. Although there is no particular lower limit, the standard deviation σ of the nanohardness of the sheet surface at a position ¼ of the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet may be 0.5 GPa or more. The standard deviation σ of the nanohardness of the sheet surface at a position ½ of the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet is preferably 2.1 GPa or less. The standard deviation σ of the nanohardness of the sheet surface at a position ½ of the depth in the sheet thickness direction of the soft surface layer from the surface of the base steel sheet is more preferably 1.7 GPa or less. Although there is no particular lower limit, the standard deviation σ of the nano-hardness of the sheet surface at a position halfway from the surface of the base steel sheet to the depth of the soft surface layer in the sheet thickness direction may be 0.6 GPa or more.

[0066] Here, the nanohardness of the sheet surface at the 1 / 4 and 1 / 2 positions in the sheet thickness direction refers to the hardness measured by the following method. First, after peeling off the zinc plating layer, for steel sheets on which a metal plating layer such as a metal electroplating layer is formed, after peeling off the metal plating layer, mechanical polishing is performed from the surface of the base steel sheet to the 1 / 4 position in the sheet thickness direction of the soft surface layer, buffing with diamond and alumina, and further colloidal silica polishing is performed. Using a Tribo-950 from Hysitron, the nanohardness is measured using a Berkovich-shaped diamond indenter under the conditions of a load of 500 μN, a measurement area of ​​50 μm × 50 μm, and a dot spacing of 2 μm. Furthermore, mechanical polishing is performed to the 1 / 2 position in the sheet thickness direction of the soft surface layer, buffing with diamond and alumina, and further colloidal silica polishing. Then, using a Tribo-950 manufactured by Hysitron, a Berkovich-shaped diamond indenter is used to measure the nanohardness under the following conditions: load: 500 μN, measurement area: 50 μm × 50 μm, and impact spacing: 2 μm. At a 1 / 4 position in the thickness direction, the nanohardness is measured at 300 or more points, and also at a 1 / 2 position in the thickness direction. For example, when the thickness of the surface soft layer is 100 μm, the 1 / 4 position is 25 μm from the surface of the surface soft layer, and the 1 / 2 position is 50 μm from the surface of the surface soft layer. At this 25 μm position, the nanohardness is measured at 300 or more points, and also at a 50 μm position, the nanohardness is measured at 300 or more points.

[0067] Metal Plating Layer Furthermore, a galvanized steel sheet according to one embodiment of the present invention preferably has a metal plating layer (first plating layer, pre-plating layer) formed between the base steel sheet and the galvanized layer on one or both sides of the base steel sheet (note that the metal plating layer excludes the galvanized layer of a hot-dip galvanized layer and a galvannealed hot-dip galvanized layer). The metal plating layer is preferably a metal electroplating layer, and the following description will be given taking a metal electroplating layer as an example. By forming a metal electroplating layer on the base steel sheet, the outermost metal electroplating layer contributes to suppressing the occurrence of bending cracks during press forming and vehicle collisions, thereby further improving bending fracture resistance. In the present invention, by setting the dew point in the soaking step to −5°C or higher, the thickness of the soft layer can be increased, thereby achieving extremely excellent axial crushing properties. In this regard, in the present invention, by having a metal plating layer, even if the dew point is below −5°C and the soft layer thickness is small, axial crushing properties equivalent to those obtained when the soft layer is thick are obtained.

[0068] The metal species of the metal electroplating layer may be any of Cr, Mn, Fe, Co, Ni, Cu, Ga, Ge, As, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Os, Ir, Rt, Au, Hg, Ti, Pb, and Bi, but Fe is more preferred. The following description will be given using an Fe-based electroplating layer as an example, but the following conditions for Fe can also be used for other metal species.

[0069] The deposition amount of the Fe-based electroplating layer is 0 g / m 2 More than 2.0 g / m 2 Although there is no particular upper limit to the amount of the Fe-based electroplated layer deposited on one side of the base steel sheet, from the viewpoint of cost, the amount of the Fe-based electroplated layer deposited on one side is set to 60 g / m or more. 2 The coating weight of the Fe-based electroplating layer is preferably 50 g / m or less. 2 More preferably, it is 40 g / m or less. 2 More preferably, it is 30 g / m or less. 2 The following is the result.

[0070] The deposition weight of the Fe-based electroplated layer is measured as follows: A 10 × 15 mm sample is taken from the Fe-based electroplated steel sheet and embedded in resin to form a cross-section embedded sample. Three randomly selected locations on the cross-section are observed using a scanning electron microscope (SEM) at an accelerating voltage of 15 kV and a magnification of 2,000 to 10,000 times depending on the thickness of the Fe-based electroplated layer. The average thickness of the three fields of view is multiplied by the iron density to convert it into the deposition weight of the Fe-based electroplated layer per side.

[0071] The Fe-based electroplating layer may be made of pure Fe or an alloy such as an Fe—B alloy, an Fe—C alloy, an Fe—P alloy, an Fe—N alloy, an Fe—O alloy, an Fe—Ni alloy, an Fe—Mn alloy, an Fe—Mo alloy, or an Fe—W alloy. The composition of the Fe-based electroplating layer is not particularly limited, but it preferably contains one or more elements selected from the group consisting of B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co in a total amount of 10% by mass or less, with the remainder consisting of Fe and unavoidable impurities. By limiting the total amount of elements other than Fe to 10% by mass or less, a decrease in electrolysis efficiency can be prevented and the Fe-based electroplating layer can be formed at low cost. In the case of an Fe—C alloy, the C content is preferably 0.08% by mass or less.

[0072] <Method for manufacturing galvanized steel sheet> Next, a method for manufacturing a galvanized steel sheet according to an embodiment of the present disclosure will be described. Note that, unless otherwise specified, the temperatures when heating or cooling a steel slab (steel material), steel sheet, etc., referred to below refer to the surface temperatures of the steel slab (steel material), steel sheet, etc.

[0073] The method for producing a galvanized steel sheet of the present invention comprises a hot rolling step of heating a slab having the above-described chemical composition to a temperature range of 1100 to 1350°C, hot rolling the slab at a finish rolling end temperature of 800 to 950°C, and coiling the slab at a coiling temperature of 650°C or lower; a reducing step of holding the steel sheet after the hot rolling step in a reducing atmosphere at 700°C or higher and a hydrogen concentration of 8 to 30% by volume for 20 seconds or longer; and a soaking step of holding the steel sheet after the reducing step in a soaking atmosphere at 750°C or higher and a hydrogen concentration of 0.2 to 8% by volume for 20 seconds or longer and 300 seconds or shorter. a first cooling step of cooling the steel sheet after the soaking step; a galvanizing step of forming a galvanized layer on the surface of the steel sheet after the first cooling step; a second cooling step of cooling the steel sheet after the galvanizing step to a cooling stop temperature of 100 to 300°C at an average cooling rate of 20°C / s or less from a temperature range of 350 to 450°C to (Ms point - 100°C) and by allowing the steel sheet to remain in a temperature range of 100 to 350°C for 5 seconds or more; and a reheating step of holding the steel sheet after the second cooling step in a temperature range of not less than the cooling stop temperature and not more than 450°C for 5 to 600 seconds.

[0074] [Hot Rolling Step] The slab is hot rolled under the following conditions.

[0075] Slab heating temperature: 1100 to 1350°C In order to dissolve carbides and reduce the rolling load, the slab heating temperature is set to 1100°C or higher. The slab heating temperature is preferably 1150°C or higher. In addition, in order to prevent an increase in scale loss, the slab heating temperature is set to 1350°C or lower, and preferably 1300°C or lower.

[0076] Finish rolling end temperature: 800 to 950°C If the finish rolling end temperature is less than 800°C, ferrite transformation occurs during rolling, and extended ferrite is generated in the surface layer of the hot-rolled sheet, which may remain in the next process and deteriorate the final bendability. Therefore, the finish rolling end temperature is 800°C or higher, preferably 850°C or higher. On the other hand, if the finish rolling end temperature exceeds 950°C, the crystal grains may become coarse, which may cause insufficient strength and deterioration of bendability. Therefore, the finish rolling end temperature is 950°C or lower, preferably 930°C or lower.

[0077] Coiling temperature: 650°C or less If the coiling temperature exceeds 650°C, carbides in the hot-rolled steel sheet will coarsen and will not be completely melted by the time of the soaking step, which may cause deterioration in bendability. Therefore, the coiling temperature is 650°C or less, and preferably 600°C or less. There are no particular restrictions on the lower limit of the coiling temperature, but from the viewpoint of suppressing the occurrence of defective shape of the steel sheet and preventing the steel sheet from becoming excessively hard, it is preferably 400°C or more.

[0078] [Cold Rolling Step (Preferred Conditions)] Before subjecting the base steel sheet after the hot rolling step (hot rolling step) to the reducing step, cold rolling may be performed as necessary. The cold rolling in the cold rolling step is performed before the oxidation step if an oxidation treatment is to be performed in the oxidation step described below, and is performed before the pre-plating step if metal plating is to be performed in the pre-plating step. When cold rolling is performed, it is preferable that the hot-rolled steel sheet obtained after the hot rolling step (hot rolling step) is subjected to pre-treatment such as pickling and degreasing by a known method before cold rolling.

[0079] When cold rolling is performed, the rolling reduction (cumulative rolling reduction) is not particularly limited, but in order to promote ferrite recrystallization, it is preferably 20% or more, and more preferably 30% or more. There is no particular upper limit to the rolling reduction, but it is preferably 80% or less.

[0080] [Pre-plating (Metal Plating, Metal Electroplating, First Plating) Process (Preferred Conditions)] In one embodiment of the present invention, the base steel sheet may be subjected to a pre-plating (metal plating) process after the hot rolling process (or after the cold rolling process if cold rolling is performed) and before the reducing process, thereby forming a metal plating layer, such as a metal electroplating layer, on one or both sides of the base steel sheet to produce a pre-annealed metal-plated steel sheet (pre-annealed metal electroplated steel sheet). Note that the metal plating referred to here excludes zinc plating (second plating). While the metal plating process method is not particularly limited, as described above, a metal electroplating layer is preferably formed on the base steel sheet, and therefore, metal electroplating is preferred. For example, when an Fe-based electroplating bath is used, a sulfuric acid bath, a hydrochloric acid bath, or a mixture of both can be used. Furthermore, the coating weight of the pre-annealed metal electroplating layer can be adjusted by, for example, the current application time. The term "pre-annealed metal electroplated steel sheet" means that the metal electroplated layer has not undergone an oxidation step, a reduction step, or a soaking step, and does not exclude a hot-rolled steel sheet or a cold-rolled steel sheet that has been annealed in advance before the metal electroplating treatment.

[0081] The metal species of the electroplating layer may be any of Cr, Mn, Fe, Co, Ni, Cu, Ga, Ge, As, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Os, Ir, Rt, Au, Hg, Ti, Pb, and Bi, but is preferably Fe. The following description will be given using Fe-based electroplating as an example, but the following conditions for Fe-based electroplating can also be used for other metal-based electroplating.

[0082] The Fe ion content in the Fe-based electroplating bath before the start of current application is Fe 2+ The Fe ion content in the Fe-based electroplating bath is preferably 0.5 mol / L or more. 2+ In order to obtain a sufficient amount of Fe deposited, the Fe ion content in the Fe-based electroplating bath before the start of current application is preferably 2.0 mol / L or less.

[0083] The Fe-based electroplating bath may contain Fe ions and at least one element selected from the group consisting of B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co. The total content of these elements in the Fe-based electroplating bath is preferably 10 mass% or less in the Fe-based electroplated layer before annealing. Metal elements may be contained as metal ions, and nonmetal elements may be contained as part of boric acid, phosphoric acid, nitric acid, organic acids, etc. The iron sulfate plating solution may also contain conductivity aids such as sodium sulfate and potassium sulfate, chelating agents, and pH buffers.

[0084] Other conditions for the Fe-based electroplating bath are not particularly limited. The temperature of the Fe-based electroplating solution is preferably 30°C or higher in consideration of the ability to maintain a constant temperature. The temperature of the Fe-based electroplating solution is preferably 85°C or lower. The pH of the Fe-based electroplating bath is not particularly specified, but is preferably 1.0 or higher in consideration of preventing a decrease in current efficiency due to hydrogen generation, and is preferably 3.0 or lower in consideration of the electrical conductivity of the Fe-based electroplating bath. The current density is preferably 10 A / dm from the viewpoint of productivity. 2 It is preferable that the current is 150 A / dm or more, and from the viewpoint of facilitating control of the deposition amount of the Fe-based electroplating layer, 2 The sheet threading speed is preferably 5 mpm or more from the viewpoint of productivity, and is preferably 150 mpm or less from the viewpoint of stable control of the amount of adhesion.

[0085] Prior to the Fe-based electroplating treatment, the steel sheet may be subjected to a degreasing treatment and water rinsing to clean the surface, and further to a pickling treatment and water rinsing to activate the surface. These pretreatments are followed by the Fe-based electroplating treatment. The degreasing and water rinsing methods are not particularly limited, and conventional methods can be used. Various acids can be used in the pickling treatment, such as sulfuric acid, hydrochloric acid, nitric acid, and mixtures thereof. Among these, sulfuric acid, hydrochloric acid, or mixtures thereof are preferred. The acid concentration is not particularly specified, but a concentration of 1 to 20 mass% is preferred, taking into consideration the ability to remove oxide films and the prevention of surface roughness (surface defects) due to excessive pickling. The pickling treatment solution may also contain an antifoaming agent, a pickling accelerator, a pickling inhibitor, etc.

[0086] [Oxidation step (preferred conditions)] The steel sheet after the hot rolling step, or the steel sheet after the cold rolling step if cold rolling is performed, may be subjected to oxidation treatment in an oxidation step before the reduction step described below. By performing the oxidation treatment in the oxidation step, an iron oxide layer is formed on the surface of the steel sheet, and a reduced iron layer is formed during the subsequent annealing in a reducing atmosphere, thereby improving the wettability of the steel sheet.

[0087] Oxygen concentration: 1000 ppm by volume or more and 30,000 ppm by volume or less When performing oxidation treatment in the oxidation step, if the oxygen concentration of the atmosphere is less than 1000 ppm by volume, the formation of an iron oxide layer is not promoted, and the effect of improving wettability may be small. Therefore, the oxygen concentration is 1000 ppm by volume or more, preferably 1500 ppm by volume or more. On the other hand, if the oxygen concentration exceeds 30,000 ppm by volume, excessive iron oxide is formed, and reduction is not completed before the galvanizing step, such as hot-dip galvanizing, and the remaining iron oxide may actually deteriorate the plating wettability. Therefore, the oxygen concentration is 30,000 ppm by volume or less, preferably 25,000 ppm by volume or less. The oxygen concentration is preferably 22,000 ppm by volume or less, more preferably 20,000 ppm by volume or less.

[0088] Steel sheet temperature (maximum temperature reached during oxidation treatment): 600°C or higher When oxidation treatment is performed in the oxidation step, even in the above atmosphere, if the steel sheet temperature (maximum temperature reached during oxidation treatment) is less than 600°C, the amount of iron oxide formed on the surface may be small, and the effect of improving plating wettability may be reduced. Therefore, the steel sheet temperature (maximum temperature reached during oxidation treatment) in the oxidation step is 600°C or higher, preferably 620°C or higher. There is no particular upper limit for the steel sheet temperature, but in order to more appropriately prevent excessive oxidation of the steel sheet, which would result in unreduced iron oxide remaining in the subsequent reduction step, and to more stably obtain excellent plating properties, the steel sheet temperature is preferably 900°C or lower, more preferably 880°C or lower. The steel sheet temperature in the oxidation step (maximum temperature reached during oxidation treatment) is preferably 860°C or lower, more preferably 840°C or lower.

[0089] [Reduction step] A reduced iron layer is formed by heating the natural oxide film on the steel sheet surface or the iron oxide layer on the surface that is formed when oxidation is performed in the oxidation step in an iron-reducing atmosphere. In the subsequent soaking step, the atmosphere has a relatively low hydrogen concentration, which slows down the iron reduction reaction rate. Therefore, it is necessary to complete the reduction of the iron oxide in the reduction step.

[0090] Steel sheet temperature (maximum temperature reached during reduction treatment): 700°C or higher If the steel sheet temperature (maximum temperature reached during reduction treatment) is less than 700°C, the reduction rate is slow and unreduced iron oxide may remain. Therefore, the steel sheet temperature in the reduction step is 700°C or higher, preferably 750°C or higher. There is no particular upper limit to the steel sheet temperature, but from the viewpoint of reducing the load on the furnace body, it is preferably 950°C or lower. The steel sheet temperature in the reduction step is preferably 920°C or lower, more preferably 900°C or lower.

[0091] Holding time (holding time during reduction treatment): 20 seconds or more If the holding time in the reduction step (holding time during reduction treatment) is less than 20 seconds, the reduction of iron oxide may not be completed. Therefore, the holding time in the reduction step is 20 seconds or more, preferably 25 seconds or more. There is no particular upper limit to the holding time, but from the viewpoint of productivity, it is preferably 150 seconds or less. The holding time is preferably 120 seconds or less, more preferably 100 seconds or less.

[0092] Hydrogen concentration (hydrogen concentration during reduction treatment): 8 vol% or more and 30 vol% or less If the hydrogen concentration in the atmosphere during the reduction process (hydrogen concentration during reduction treatment) is less than 8 vol%, unreduced iron oxide may remain. Therefore, the hydrogen concentration during the reduction process is 8 vol% or more, preferably 10 vol% or more. On the other hand, if the hydrogen concentration exceeds 30 vol%, the reduction rate may saturate and the penetration of hydrogen into the steel may increase excessively, making it difficult to sufficiently reduce the amount of hydrogen in the steel in the subsequent soaking process. Therefore, the hydrogen concentration during the reduction process is 30 vol% or less, preferably 28 vol% or less. The hydrogen concentration is preferably 26 vol% or less, more preferably 24 vol% or less.

[0093] The dew point of the atmosphere in the reduction step (reduction dew point) is not particularly limited, but is preferably 30°C or lower, more preferably 25°C or lower, in order to effectively prevent oxidation of the surface of the base steel sheet or the surface of the Fe-based electroplated layer and to improve plating adhesion when a hot-dip galvanized layer is formed. The reduction dew point is preferably 22°C or lower, more preferably 20°C or lower. The lower limit of the dew point is also not particularly limited, but is preferably −50°C or higher, more preferably −45°C or higher, in terms of ease of industrial control. The reduction dew point is preferably −40°C or higher, more preferably −35°C or higher.

[0094] [Soaking Step] In the soaking step, annealing is carried out to obtain the structure of the galvanized steel sheet of the present invention, and the hydrogen that has entered the steel in the reduction step is reduced.

[0095] Steel sheet temperature (annealing temperature): 750°C or higher If the steel sheet temperature (annealing temperature) in the soaking step is lower than 750°C, the steel sheet surface may be reoxidized. Furthermore, the structure required for the steel sheet of the present invention may not be obtained due to the presence of unrecrystallized ferrite or insufficient austenite formation during annealing. Therefore, the steel sheet temperature is 750°C or higher, preferably 760°C or higher. On the other hand, the upper limit of the steel sheet temperature in the soaking step is not particularly limited, but is preferably 950°C or lower from the viewpoints of reducing the furnace load and preventing excessive coarsening of austenite grains. The annealing temperature is preferably 930°C or lower, more preferably 910°C or lower.

[0096] Holding time (holding time during soaking): 20 seconds or more and 300 seconds or less If the holding time in the soaking step is less than 20 seconds, hydrogen in the steel may not be sufficiently reduced. Furthermore, austenite may not be generated sufficiently, and the steel sheet structure of the present invention may not be obtained. Therefore, the holding time is 20 seconds or more, preferably 50 seconds or more. On the other hand, if the holding time exceeds 300 seconds, coarsening of austenite grains and decarburization of the surface layer may progress, and the steel sheet structure of the present invention may not be obtained. Therefore, the holding time is 300 seconds or less, preferably 200 seconds or less. The holding time is preferably 180 seconds or less, more preferably 160 seconds or less.

[0097] Hydrogen concentration (hydrogen concentration during soaking): 0.2 vol% or more and 8 vol% or less. Since the reduction of iron oxide is completed in the reduction step, the hydrogen concentration in the soaking step atmosphere is set to a low level within a range that does not cause reoxidation of the reduced iron, thereby reducing the hydrogen that has entered the steel during the reduction step. If the hydrogen concentration exceeds 8 vol%, the hydrogen in the steel cannot be sufficiently reduced, and the steel sheet of the present invention cannot be obtained. Therefore, the hydrogen concentration is 8 vol% or less, preferably 5 vol% or less. On the other hand, if the hydrogen concentration is less than 0.2 vol%, reoxidation of the reduced iron may occur. Therefore, the hydrogen concentration in the soaking atmosphere is 0.2 vol% or more, preferably 0.5 vol% or more. The hydrogen concentration is preferably 0.8 vol% or more, more preferably 1.0 vol% or more.

[0098] Dew point of the soaking atmosphere (annealing atmosphere) in the soaking step (dew point during soaking): −30°C or higher (preferred conditions) In one embodiment of the present invention, the dew point of the soaking atmosphere in the soaking step is preferably −30°C. By performing soaking with a dew point of the atmosphere in the soaking step of −30°C or higher, the decarburization reaction is promoted and a deeper soft surface layer can be formed. The dew point of the atmosphere in the soaking step is more preferably −15°C or higher, and even more preferably −5°C or higher. There is no particular upper limit for the dew point of the atmosphere in the soaking step, but in order to suitably prevent oxidation of the surface of the base steel sheet or the surface of the Fe-based electroplated layer and to improve plating adhesion when a hot-dip galvanized layer is formed, it is preferably 30°C or lower, more preferably 25°C or lower. Even more preferably 20°C or lower.

[0099] [First Cooling Step] The steel sheet after the soaking step is cooled, for example, to a temperature at which it can be immersed in hot dip galvanizing. The cooling conditions are not necessarily limited, but it is preferable to perform the cooling under the following conditions.

[0100] Hydrogen concentration (hydrogen concentration during first cooling treatment): 0.5 vol% or more and 30 vol% or less, dew point (dew point during first cooling treatment): 0°C or less (preferred conditions) By setting the hydrogen concentration of the cooling atmosphere in the first cooling step to 0.5 vol% or more and 30 vol% or less and the dew point to 0°C or less, reoxidation during cooling can be suppressed. More preferably, the hydrogen concentration is 1.0 vol% or more and the dew point is -20°C or less. The hydrogen concentration is preferably 1.5 vol% or more, more preferably 2.0 vol% or more. The dew point is preferably -25°C or less, and even more preferably -30°C or less. In addition, the lower limit of the dew point is not particularly limited, but the dew point is preferably -55°C or more, and even more preferably -50°C or more. On the other hand, by setting the hydrogen concentration to 30 vol% or less, an increase in hydrogen in the steel due to hydrogen penetration during the cooling process can be suppressed. The hydrogen concentration is more preferably 20 vol% or less, and even more preferably 10 vol% or less.

[0101] Cooling from a steel sheet temperature of 600 to 900°C (steel sheet temperature during the first cooling treatment) to 150 to 500°C at an average cooling rate (average cooling rate during the first cooling treatment) of 20°C / s or less (preferred conditions). Furthermore, to more effectively prevent an increase in the amount of hydrogen in the steel during cooling, cooling is preferably performed from a steel sheet temperature of 600 to 900°C at an average cooling rate of 20°C / s or less. The average cooling rate is preferably 10°C / s or more. Furthermore, since the steel sheet temperature in the subsequent galvanizing process must be cooled to the same temperature as the galvanizing bath temperature, the cooling stop temperature (cooling stop temperature during the first cooling treatment) is 500°C or less. Furthermore, if the cooling stop temperature is less than 150°C, excessive martensitic transformation occurs before the galvanizing process, which is then tempered after the galvanizing process, resulting in insufficient strength of the final structure. Therefore, the cooling stop temperature is 150°C or higher. Here, the average cooling rate (°C / s) is obtained from (steel plate temperature (600 to 900°C) - cooling stop temperature (150 to 500°C)) / cooling time (s) from the start of cooling to the end of cooling.

[0102] [Zinc plating step] A zinc plating layer is formed on the surface of the steel sheet after the first cooling step. A typical method is to immerse the steel sheet in a hot-dip galvanizing bath. The following describes immersion in a hot-dip galvanizing bath as an example.

[0103] The conditions for immersion in the hot-dip galvanizing bath are not particularly limited, and a general method may be used. The hot-dip galvanizing bath contains Al, Zn, and unavoidable impurities. The composition is not particularly specified, but in one example, the Al concentration in the bath may be 0.05 mass% or more and 0.190 mass% or less. If the Al concentration in the bath is 0.05 mass% or more, the occurrence of bottom-dross can be more effectively prevented. Furthermore, if the Al concentration in the bath is 0.190 mass% or less, the occurrence of top-dross can be more effectively prevented. From a cost perspective, it is preferable that the Al concentration in the bath be 0.190 mass% or less. The plating bath temperature is also not particularly specified, but may be 440°C or more and 500°C or less. Note that the galvanizing applied in the present invention is not limited to the hot-dip galvanizing described above, and other methods such as electrogalvanizing or electrogalvanizing may be used as long as the desired steel sheet temperature is met in the preceding and following processes.

[0104] The plating amount per side is not particularly limited, but in one example, it is 25 g / m 2 or more, and 120 g / m 2 The plating weight per side is 25 g / m or less. 2 If the coating weight per side is 120 g / m or more, the corrosion resistance is particularly good and the coating weight is particularly easy to control. 2 The method for adjusting the coating weight is not particularly limited, but in the case of hot-dip galvanizing, for example, gas wiping can be used and the coating weight can be adjusted by adjusting the gas pressure and the distance between the wiping nozzle and the steel sheet.

[0105] In the galvanizing process, after forming a galvanized layer, an alloying treatment may be performed to obtain a galvannealed steel sheet. By forming the galvanized layer into an alloyed galvanized layer, it is possible to further promote the desorption of hydrogen from the steel in the subsequent reheating process. The conditions for the alloying treatment are not particularly limited as long as a desired degree of alloying is obtained. For example, in the alloying treatment in hot-dip galvanizing, it is preferable to hold the steel sheet at a predetermined temperature for a predetermined time. For example, the steel sheet temperature can be 440°C or higher. The steel sheet temperature can be 600°C or lower. Furthermore, the holding time can be 5 seconds or longer. The holding time can be 60 seconds or shorter.

[0106] When alloying treatment is performed, the Fe content (degree of alloying) in the coating layer is preferably 7% by mass or more. Furthermore, this Fe content (degree of alloying) is preferably 15% by mass or less. By setting the degree of alloying to 7% by mass or more, no η-Zn phase remains in the alloyed galvanized layer, and hydrogen in the steel can be more suitably reduced in the reheating step. Furthermore, if the degree of alloying exceeds 15% by mass, the formation of the Γ phase at the interface between the alloyed galvanized layer and the base steel sheet may be promoted, resulting in a decrease in coating adhesion, so the degree of alloying is preferably 15% by mass or less.

[0107] [Second Cooling Step] The steel sheet after the galvanizing step is cooled to a cooling stop temperature of 100 to 300° C. The cooling method is not particularly limited as long as it satisfies the following cooling conditions.2 It may be gas-cooled, water-cooled, or a combination thereof.

[0108] Cooling stop temperature (cooling stop temperature during second cooling treatment): 100°C or higher and 300°C or lower. In the second cooling step, untransformed austenite is cooled to a temperature lower than the Ms point to generate martensite. Because the hydrogen diffusion rate is faster in martensite with a BCT crystal structure than in austenite with an FCC crystal structure, this can facilitate hydrogen reduction in the subsequent reheating step. As mentioned above, the steel sheet of the present invention must be controlled so that 70% or more of the area fraction of the total martensite contained in the structure becomes tempered martensite with carbides of a predetermined size. This cannot be achieved with a cooling stop temperature exceeding 300°C. Therefore, the cooling stop temperature is 300°C or lower, preferably 280°C or lower. Furthermore, if the cooling stop temperature is lower than 100°C, almost all austenite is transformed into martensite at this point, leaving little untransformed austenite in the final structure, which may impair ductility. Furthermore, the desired strength may not be achieved. Therefore, the cooling stop temperature is set to 100°C or higher, and preferably 120°C or higher.

[0109] Average cooling rate from the temperature range of 350 to 450 °C to reach (Ms point - 100 °C) (average cooling rate during the second cooling treatment): 20 °C / s or less. In the second cooling step, it is preferable to cool so that the temperature remains in the temperature range below Ms and above the cooling stop temperature for a predetermined period of time. This allows the martensite formed just below the Ms point to self-temper during cooling, further promoting the formation of carbides in the martensite required for the present invention. If the average cooling rate exceeds 20 °C / s, self-tempering may be insufficient and the carbides may not be sufficiently obtained. Therefore, the average cooling rate is 20 °C / s or less, preferably 10 °C / s or less, and more preferably 5 °C / s or less. Furthermore, there is no particular lower limit to the average cooling rate, but a rate of 1 °C / s or more is preferred in order to more stably prevent the carbide size (average particle size of carbides contained in tempered martensite) from exceeding 200 nm due to excessively slow cooling. Here, the average cooling rate (°C / s) is obtained from "(cooling start temperature (350 to 450°C)) - (Ms point - 100°C)) / cooling time (s) from the start of cooling to (Ms point - 100°C)".

[0110] Residence time in the temperature range of 100 to 350°C for 5 seconds or more. Furthermore, if the residence time in the temperature range of 100 to 350°C is less than 5 seconds in the second cooling step, self-tempering may be insufficient and the carbides may not be sufficiently produced. Therefore, the residence time is 5 seconds or more, preferably 10 seconds or more, and more preferably 15 seconds or more. The upper limit of the residence time is not particularly limited, but 60 seconds or less is preferred in order to more stably prevent the carbide size from exceeding 200 nm.

[0111] The Ms point is the martensitic transformation start temperature and can be calculated using the following formula: Ms (°C) = 539 - 423 x {[C mass %] x 100 / (100 - [α area %])} - 30 x [Mn mass %] - 12 x [Cr mass %] - 18 x [Ni mass %] - 8 x [Mo mass %] In the above formula, [M mass %] (M: element) is the amount of each element contained in the steel sheet. Also, [α area %] is the ferrite area ratio (%) in the steel sheet structure after annealing.

[0112] [Reheating Step] In this step, the steel sheet obtained in the second cooling step is reheated to temper the martensite necessary to obtain the steel sheet of the present invention, and at the same time, to reduce diffusible hydrogen.

[0113] Since the reheating step already has a zinc-plated layer on the surface of the steel sheet, there is no need to consider iron reoxidation as in the soaking step, and the reheating step can be performed in an atmosphere with a low hydrogen concentration, for example, in the air. On the other hand, if the hydrogen concentration is excessively high, the diffusible hydrogen remaining in the steel will not be reduced, and an excessively high hydrogen concentration may actually increase it again. Therefore, although not particularly limited, it is preferable that the hydrogen concentration in the reheating step be 0.2 vol% or less.

[0114] Reheating temperature: Cooling stop temperature (cooling stop temperature during second cooling treatment) or higher and 450°C or lower. If the reheating temperature is lower than the cooling stop temperature (cooling stop temperature during second cooling treatment), tempering of the martensite is insufficient, and the carbides and tempered martensite required for the present invention cannot be obtained. Furthermore, if the reheating temperature is lower than the cooling stop temperature (cooling stop temperature during second cooling treatment), the effect of reducing diffusible hydrogen in the steel is also insufficient. Therefore, the reheating temperature is higher than the cooling stop temperature (cooling stop temperature during second cooling treatment), preferably 120°C or higher. On the other hand, if the reheating temperature exceeds 450°C, excessive tempering can lead to a decrease in tensile strength and coarsening of carbides, making it impossible to obtain the steel sheet of the present invention. Furthermore, if the reheating temperature exceeds 450°C, the appearance of the galvanized coating may be impaired. Therefore, the reheating temperature is 450°C or lower, preferably 430°C or lower.

[0115] Holding time (holding time during reheat treatment): 5 to 600 seconds. If the holding time is less than 5 seconds, the martensite is not sufficiently tempered, the carbides and tempered martensite required for the present invention are not obtained, and diffusible hydrogen in the steel is not sufficiently reduced. Therefore, the holding time is 5 seconds or more, preferably 10 seconds or more. The holding time is more preferably 15 seconds or more, more preferably 20 seconds or more. On the other hand, if the holding time exceeds 600 seconds, not only does it reduce production efficiency, but excessive tempering can also cause a decrease in tensile strength and coarsening of carbides, making it impossible to obtain the steel sheet of the present invention. Therefore, the holding time is 600 seconds or less, preferably 500 seconds or less. The holding time is more preferably 400 seconds or less, more preferably 300 seconds or less.

[0116] The manufacturing conditions other than those mentioned above can be the same as those in the ordinary method.

[0117] The thickness of the galvanized steel sheet of the present invention is not particularly limited, but is preferably 0.4 mm or more, and more preferably 0.6 mm or more. The thickness is preferably more than 0.8 mm. The thickness is more preferably 0.9 mm or more. The thickness is even more preferably 1.0 mm or more. The thickness is still more preferably 1.2 mm or more. The thickness is preferably 3.2 mm or less, and more preferably 3.0 mm or less.

[0118] <Member> Next, a member according to one embodiment of the present invention will be described. The member according to one embodiment of the present invention is a member made using (using as a raw material) the above-mentioned galvanized steel sheet. For example, the raw material galvanized steel sheet is subjected to at least one of forming and joining to form a member. Here, the above-mentioned galvanized steel sheet has a high yield ratio (YR), excellent bendability and stretch flangeability, excellent hydrogen embrittlement resistance, and a tensile strength (TS) of 780 MPa or more and less than 1180 MPa. Therefore, the member according to one embodiment of the present invention has a high yield ratio (YR), excellent bendability and stretch flangeability, excellent hydrogen embrittlement resistance, and a tensile strength (TS) of 780 MPa or more and less than 1180 MPa. Therefore, the member according to one embodiment of the present invention is particularly suitable as a member used in the automotive field.

[0119] <Method for manufacturing a member> Next, a method for manufacturing a member according to one embodiment of the present invention will be described. The method for manufacturing a member according to one embodiment of the present invention includes a step of subjecting the above-mentioned galvanized steel sheet (for example, a galvanized steel sheet manufactured by the above-mentioned method for manufacturing a galvanized steel sheet) to at least one of forming and joining to form a member. Here, the forming method is not particularly limited, and for example, a general processing method such as press working can be used. In addition, the joining method is also not particularly limited, and for example, general welding such as spot welding, laser welding, and arc welding, rivet joining, caulking joining, etc. can be used. Note that the forming conditions and joining conditions are not particularly limited, and may be in accordance with conventional methods.

[0120] The present invention will be specifically described with reference to examples, but the scope of the present invention is not limited to the following examples.

[0121] Example 1 Using steel having the chemical composition shown in Table 1, cold-rolled steel sheets with a thickness of 1.4 mm or hot-rolled steel sheets with a thickness of 1.8 mm were produced under the conditions shown in Table 2. Galvanized steel sheets (hot-dip galvanized steel sheets) were then produced and evaluated as follows. For all steel sheets, the slab heating temperature in the hot rolling process was 1250°C, the finish rolling end temperature was 900°C, and the coiling temperature was 520°C. Reheating in the reheating process was performed in the air. The evaluation results are shown in Table 3. The galvanizing and alloying processes in the galvanizing process were performed under the following conditions. All of the following evaluations were performed within 72 hours after the steel sheets first reached room temperature (40°C or less) after the reheating process specified in the present invention. Galvanizing bath composition: Zn bath containing 0.13 mass% Al; Galvanizing bath temperature: 460°C; Galvanizing coating weight range: 30 to 60 g / m -2 Alloying temperature: 450 to 560°C Alloying degree range: 8.0 to 14.0 mass%

[0122]

[0123]

[0124] <Tensile Test> A JIS No. 5 tensile test piece (JIS Z2201) was taken from the obtained zinc-plated steel sheet in the direction perpendicular to the rolling direction, and the strain rate was increased to 10 -3 Tensile tests were conducted in accordance with the provisions of JIS Z2241 (2011), where the yield strength (YS), tensile strength (TS), elongation (EL), and yield ratio (YR = YS / TS) were determined. Those with a TS of 780 MPa or more but less than 1180 MPa and a YR of 0.60 or more were considered to be examples of the present invention. EL was evaluated as having an excellent TS-EL balance when the product of EL and TS was 10,000 or more.

[0125] <Hole Expanding Test> To evaluate stretch flangeability, a hole expanding test was performed according to JIS Z 2256. A 100 mm x 100 mm test piece was taken from the obtained galvanized steel sheet, and a 10 mm diameter hole was formed in the center of the test piece by punching. The clearance during punching was 12.5%. Next, using a die with an inner diameter of 75 mm, a blank holding force of 9 ton (88.26 kN) was applied around the hole, and a conical punch with an apex angle of 60° was pressed into the hole to expand the hole, and the hole diameter at the time of crack initiation was measured. The critical hole expanding ratio λ (%) was calculated according to the following formula. Those with a λ of 35% or more were considered to be examples of the present invention. λ (%) = {(D f -D 0 ) / D 0} x 100 D f D: diameter of hole at crack occurrence (mm) 0 : Hole diameter before hole expansion (mm)

[0126] <Structural Observation> Test specimens for structural observation were taken from the resulting galvanized steel sheets. The cross-sections of the steel sheets parallel to the rolling direction were polished and then etched with nital solution. Using an SEM, the microstructures of three fields of view were photographed at 1500x magnification in the region from the surface to 1 / 8 of the sheet thickness and the region from 1 / 8 to 3 / 8 of the sheet thickness. The area fraction of retained austenite was determined individually by measuring X-ray diffraction intensity, and the area fraction of as-quenched martensite was determined by subtracting this from the area fraction of the white area (as-quenched martensite and retained austenite). The area fraction of retained austenite was determined from the ratio of the X-ray diffraction integrated intensities of the (200), (220), and (311) planes of fcc iron to the X-ray diffraction integrated intensities of the (200), (211), and (220) planes of bcc iron in the 1 / 4 sheet thickness plane. The retained austenite was calculated as a volume fraction by the above measurement. However, the volume fraction of the retained austenite was considered to be three-dimensionally homogeneous, and the volume fraction of the retained austenite was taken as the area fraction of the retained austenite. The area fraction of each constituent phase was determined from the obtained images using the above method. The area fraction of each constituent phase in each region was calculated using the average value of all the images taken. Furthermore, a single field of view of the structure was photographed at a magnification of 5000x for a region of ⅛ to ⅜ of the plate thickness of the base steel sheet using an SEM. The number and total area of ​​carbides present inside the prior austenite grains containing martensite were determined from the image, and the area per carbide was calculated to obtain the average grain size of the carbides. Here, the average grain size is the average of the major and minor axis lengths when the carbides are approximated as an ellipse. Note that, for one carbide, a region that is formed integrally and without interruption in the SEM image is counted as one carbide.

[0127] <Quantification of Hydrogen in Steel> A test piece for hydrogen analysis measuring approximately 5 × 30 mm was taken from the obtained galvanized steel sheet, the surface plating layer was removed using a precision grinder, and the test piece was placed in a quartz tube whose atmosphere was replaced with Ar gas. The test piece was heated to 600°C at a heating rate of 200°C / h, and the amount of released hydrogen during the heating period was measured using a gas chromatograph. The integrated value of the amount of hydrogen released in the temperature range from room temperature to 200°C was determined as the "amount of diffusible hydrogen," and the integrated value of the amount of hydrogen released in the temperature range of 350°C to 600°C was determined as the "amount of trapped hydrogen." Note that samples with a diffusible hydrogen amount of 0.45 mass ppm or less were considered to be examples of the present invention. The measurements of the amount of diffusible hydrogen and the amount of trapped hydrogen were performed after the production of the steel sheet was completed.

[0128] <Bending Test> 35 mm x 100 mm strip-shaped test specimens were taken from the obtained galvanized steel sheets, with the bending test axis parallel to the rolling direction. A 90° V-bend test was performed at various bending radii with a stroke speed of 50 mm / s, a 10 ton indentation load, and a 5 second hold time. For steel sheets with a thickness of more than 1.4 mm, one side of the steel sheet was ground to 1.4 mm before the test. To prevent the grinding process from affecting the bending test results, the ground surface was placed on the inner side of the bend (the valley side). After the test, the ridgeline of the bent apex of the test specimen was observed with a 10x magnifying glass. The minimum bending radius R (mm) at which no cracks of 0.5 mm or more were observed was divided by the sheet thickness t (mm) (t = 1.4, 1.8 mm) to determine R / t. Examples of the present invention were those that satisfied either (A) or (B) below. (A) TS: 780 MPa or more and less than 980 MPa, and R / t: 4.5 or less. (B) TS: 980 MPa or more and less than 1180 MPa, and R / t: 5.0 or less.

[0129] <Evaluation of Hydrogen Embrittlement Resistance> Test pieces measuring 30 mm x 100 mm were taken from the obtained galvanized steel sheets, and 2 mm thick spacers were sandwiched at both ends. The center between the spacers was spot-welded to prepare welded test pieces. Spot welding was performed using an inverter DC resistance spot welder, and a chromium-copper dome-shaped electrode with a tip diameter of 6 mm was used. The welding pressure was 380 kgf, the current flow time was 16 cycles / 50 Hz, and the hold time was 5 cycles / 50 Hz. The welding current value was adjusted to form a nugget diameter according to the sheet thickness. The nugget diameter was 3.8 mm for a sheet thickness of 1.4 mm and 4.4 mm for a sheet thickness of 1.8 mm, satisfying the following formula (2): 3.0 x t 1/2 < Nugget diameter < 3.5 x t 1/2 ...Equation (2) In equation (2), t is the plate thickness (mm). After leaving the specimen for 24 hours after spot welding, the spacer portion was cut off, and the cross section of the nugget was observed and evaluated according to the following criteria. Those ranked 1 or 2 were considered to be within the preferred range of the present invention. Crack observation results Rank No cracks: 1 (particularly excellent hydrogen embrittlement resistance) Only microcracks of 100 μm or less: 2 (excellent hydrogen embrittlement resistance) Cracks of more than 100 μm: 3 (poor hydrogen embrittlement resistance)

[0130]

[0131] Example 2 Cold-rolled steel sheets having a thickness of 1.4 mm were manufactured using steels having the chemical compositions shown in Table 1 under the conditions shown in Table 4. Hot-dip galvanized steel sheets or galvannealed hot-dip galvanized steel sheets were manufactured, and the same evaluations as in Example 1 were performed. For all steel sheets, the slab heating temperature in the hot rolling process was 1250°C, the finish rolling end temperature was 900°C, and the coiling temperature was 520°C. Reheating in the reheating process was performed in the air. In Example 2, some steel sheets (those marked "with pre-plating process" in Table 4) were subjected to a metal plating treatment in a pre-plating process after the cold rolling process and before the reduction process (or before the oxidation process, if treatment was performed in the oxidation process). The evaluation results are shown in Table 5. The galvanizing and alloying processes in the galvanizing process were performed in the same manner as in Example 1.

[0132]

[0133] The tensile test, hole expansion test, structure observation, quantitative determination of hydrogen in steel, bending test, and evaluation of hydrogen embrittlement resistance were carried out in the same manner as in Example 1.

[0134] <U-bending + Adhesion Bending Test> The U-bending + Adhesion Bending test was performed as follows. A 60 mm x 30 mm test piece was obtained from the obtained galvanized steel sheet by shearing and edge grinding. Here, the 60 mm side was parallel to the width (C) direction. A U-bending (primary bending) was performed in the width (C) direction with a curvature radius / sheet thickness of 4.2, with the rolling (L) direction as the axis, to prepare the test piece. In the U-bending (primary bending), as shown in Figure 1(a), a punch B1 was pressed into a steel sheet placed on a roll A1 to obtain a test piece T1. Next, as shown in Figure 1(b), an adhesion bending (secondary bending) was performed on the test piece T1 placed on a lower die A2 by crushing it with an upper die B2. In Figures 1(a) and 1(b), D1 indicates the width (C) direction, and D2 indicates the rolling (L) direction.

[0135] The U-bending conditions in the U-bending + close bending test are as follows: Test method: roll support, punch pressing Punch tip R: 5.0 mm Distance between rolls: sheet thickness x 2 mm Stroke speed: 10 mm / min Bending direction: direction perpendicular to rolling (C) The U-bending conditions in the close bending test are as follows: Spacer thickness: changed in 0.5 mm increments Test method: die support, punch pressing Forming load: 10 ton Test speed: 10 mm / min Holding time: 5 s Bending direction: direction perpendicular to rolling (C)

[0136] The U-bend + close bending test was performed three times, and the critical spacer thickness (ST) was evaluated when no cracks occurred in any of the three tests. Using a Leica stereo microscope, cracks of 200 μm or more in length at 25x magnification were judged to be cracks. Note that ST is an index for evaluating fracture resistance during a collision (the fracture resistance of the vertical wall portion in an axial crushing test). The results are also shown in Table 5.

[0137] The following cases (A) and (B) were evaluated as excellent in fracture resistance during a collision (fracture resistance of the vertical wall portion in an axial crushing test): (A) 780 MPa≦TS<980 MPa, 2.0 mm≧ST; (B) 980 MPa≦TS<1180 MPa, 3.0 mm≧ST.

[0138] <V-bend + Orthogonal VDA Bending Test> The V-bend + orthogonal VDA bending test was performed as follows. A 60 mm x 65 mm test piece was obtained from the obtained galvanized steel sheet by shearing and edge grinding. Here, the 60 mm side was parallel to the rolling (L) direction. The test piece was prepared by bending the steel sheet 90° (primary bending) in the rolling (L) direction with the width (C) direction as the axis at a curvature radius / sheet thickness of 4.2. In the 90° bending (primary bending), as shown in FIG. 1(a), a punch B1 was pressed into a steel sheet placed on a die A1 with a V groove to obtain a test piece T1. Next, as shown in FIG. 1(b), an orthogonal bending (secondary bending) was performed by pressing a punch B2 into the test piece T1 placed on a support roll A2 so that the bending direction was perpendicular to the rolling direction. In FIGS. 1(a) and 1(b), D1 indicates the width (C) direction, and D2 indicates the rolling (L) direction.

[0139] The V-bending conditions in the V-bending + orthogonal VDA bending test are as follows: Test method: die support, punch pressing Forming load: 10 ton Test speed: 30 mm / min Holding time: 5 s Bending direction: rolling (L) direction

[0140] The VDA bending conditions for the V-bending + orthogonal VDA bending test are as follows: Test method: roll support, punch pressing Roll diameter: φ30 mm Punch tip R: 0.4 mm Distance between rolls: (sheet thickness × 2) + 0.5 mm Stroke speed: 20 mm / min Test piece size: 60 mm × 60 mm Bending direction: perpendicular (C) direction to rolling

[0141] The stroke at maximum load is determined from the stroke-load curve obtained when the VDA bending is performed. The average value of the stroke at maximum load when the V bending + orthogonal VDA bending test is performed three times is taken as SFmax (mm). SFmax is an index for evaluating fracture resistance characteristics during collision (fracture resistance characteristics of the bend ridge line in the axial crush test). The results are also shown in Table 5. The following cases (A) and (B) were evaluated as excellent in fracture resistance characteristics during collision (fracture resistance characteristics of the bend ridge line in the axial crush test). (A) When 780 MPa≦TS<980 MPa, 29.5 mm≦SFmax. (B) When 980 MPa≦TS<1180 MPa, 28.5 mm≦SFmax.

[0142] <Axial Crush Test> A 160 mm x 200 mm test piece was obtained from the obtained hot-dip galvanized steel sheet by shearing. Here, the 160 mm side was parallel to the rolling (L) direction. Using a mold with a punch shoulder radius of 5.0 mm and a die shoulder radius of 5.0 mm, the hat-shaped member 10 shown in Figures 2(a) and 2(b) was produced by forming (bending) the hat-shaped member to a depth of 40 mm. The steel plate used as the material for the hat-shaped member was also cut into a size of 80 mm x 200 mm. Next, the cut-out steel plate 20 and the hat-shaped member 10 were spot-welded to produce a test member 30 as shown in Figures 2(a) and 2(b). Figure 2(a) is a front view of the test member 30 produced by spot-welding the hat-shaped member 10 and the steel plate 20. Figure 2(b) is a perspective view of the test member 30. As shown in FIG. 2(b), the spot welds 40 were positioned so that the distance between the edge of the steel plate and the weld was 10 mm, and the distance between the welds was 20 mm. Next, as shown in FIG. 2(c), the test member 30 was joined to the base plate 50 by TIG welding to prepare a sample for an axial crush test. Next, an impactor 60 was made to collide with the prepared sample for the axial crush test at a constant velocity of 10 mm / min, crushing the sample for the axial crush test by 70 mm. As shown in FIG. 2(c), the crush direction D3 was parallel to the longitudinal direction of the test member 30. The results are also shown in Table 5. Evaluation of axial crush fracture (visual cracking) More preferable (◎): No visual cracking was observed in the sample after the axial crush test. Preferred (○): One or less visual cracking was observed in the sample after the axial crush test.

[0143] In the U-bend + contact bending test, V-bend + orthogonal VDA bending test, and axial crush test of galvanized steel sheets with a thickness of more than 1.2 mm, the influence of the sheet thickness was taken into consideration, and all tests were performed on steel sheets with a thickness of 1.2 mm. Steel sheets with a thickness of more than 1.2 mm were ground on one side to reduce the sheet thickness to 1.2 mm. Because grinding may affect the bendability of the steel sheet surface, the ground surface was placed on the inside of the bend (valley side) in the U-bend + contact bending test, and the ground surface was placed on the outside of the bend (crown side) in the V-bend + orthogonal VDA bending test during the V-bend test, and then on the inside of the bend (valley side) in the subsequent VDA bending test. On the other hand, the U-bend + contact bending test, V-bend + orthogonal VDA bending test, and axial crush test of galvanized steel sheets with a thickness of 1.2 mm or less were performed without grinding because the influence of the sheet thickness was small.

[0144] When the nanohardness was measured at 300 or more points in a 50 μm × 50 μm region on the sheet surface at a position 1 / 4 of the way down in the thickness direction of the soft surface layer from the surface of the base steel sheet, if the proportion of nanohardnesses of 7.0 GPa or more was 0.10 or less, it became possible to further suppress the generation and connection of voids, as well as the propagation of cracks, during press forming and collision of hard structures (such as martensite) and inclusions, and excellent R / t and SFmax were obtained.

[0145] After the plating was removed, the steel sheet was mechanically polished from the surface to a position 5 μm below the depth of the soft surface layer, which was then buffed with diamond and alumina from the surface to a position 1 / 4 below the depth of the soft surface layer, and then polished with colloidal silica. Using a Tribo-950 manufactured by Hysitron, a Berkovich-shaped diamond indenter was used to measure the nanohardness at a total of 512 points under the following conditions: load: 500 μN, measurement area: 50 μm × 50 μm, and impact spacing: 2 μm.

[0146] When the standard deviation σ of the nanohardness of the sheet surface at a position 1 / 4 of the depth in the thickness direction of the soft surface layer from the surface of the base steel sheet is 1.8 GPa or less, and further when the standard deviation σ of the nanohardness of the sheet surface at a position 1 / 2 of the depth in the thickness direction of the soft surface layer from the surface of the base steel sheet is 2.2 GPa or less, it becomes possible to further suppress the generation and connection of voids during press forming and collision, as well as the propagation of cracks, and excellent R / t and SFmax are obtained.

[0147] For steel sheets on which a metal plating layer had been formed after peeling of the zinc plating layer, mechanical polishing, buffing with diamond and alumina, and colloidal silica polishing were performed from the surface of the base steel sheet to a position one-quarter of the depth in the sheet thickness direction of the soft surface layer after peeling of the metal plating layer. Using a Tribo-950 manufactured by Hysitron, a Berkovich-shaped diamond indenter, the nanohardness was measured at a total of 512 points under the following conditions: load: 500 μN, measurement area: 50 μm × 50 μm, and impact spacing: 2 μm.

[0148] Next, the soft surface layer was mechanically polished to a position halfway down the thickness direction, buffed with diamond and alumina, and polished with colloidal silica. Using a Tribo-950 manufactured by Hysitron, a Berkovich-shaped diamond indenter was used to measure the nano-hardness at a total of 512 points under the following conditions: load: 500 μN, measurement area: 50 μm × 50 μm, and impact spacing: 2 μm.

[0149]

[0150] From Examples 1 and 2, the galvanized steel sheets of the invention examples had a TS of 780 MPa or more and 1180 MPa or less, a YR of 0.60 or more, and diffusible hydrogen in the steel of 0.45 mass ppm or less, and were excellent in stretch flangeability, bendability, and hydrogen embrittlement resistance. The steel sheets of the comparative examples were inferior in at least one of TS, YR, stretch flangeability, bendability, and hydrogen embrittlement resistance.

[0151] In Example 2, when the dew point was −15° C., the thickness of the soft surface layer was less than 17 μm, and the fracture (appearance cracking) in the axial crushing test was evaluated as “◯”. However, even when the thickness of the soft surface layer was less than 17 μm, if a metal plating layer was included, the fracture resistance characteristics were excellent, and the fracture (appearance cracking) in the axial crushing test was evaluated as “◎”.

[0152] Furthermore, members obtained by forming or joining the galvanized steel sheets of the invention examples had a TS of 780 MPa or more and 1180 MPa or less, a YR of 0.60 or more, and diffusible hydrogen in the steel of 0.45 mass ppm or less, and were excellent in stretch flangeability, bendability, and hydrogen embrittlement resistance.

[0153] REFERENCE SIGNS LIST 10 Hat-shaped member 20 Galvanized steel sheet 30 Test member 40 Spot welded portion 50 Base plate 60 Impactor A1 Die A2 Support roll B1 Punch B2 Punch D1 Width (C) direction D2 Rolling (L) direction D3 Crushing direction T1 Test piece

[0154] According to the present invention, it is possible to obtain a galvanized steel sheet which is suitable mainly for use in automobile parts, and which has a tensile strength TS of 780 MPa or more and less than 1180 MPa, a yield ratio of 0.60 or more, and excellent bendability, stretch flangeability, and hydrogen embrittlement resistance.

Claims

1. A galvanized steel sheet having a base steel sheet and a galvanized layer formed on the base steel sheet, wherein the base steel sheet has a steel structure with, in area ratio, ferrite: less than 65%, a total of martensite and bainite: 25% or more, and retained austenite: 3% to 10% or less, wherein, in area ratio, 70% or more of all martensite in the steel structure at 1 / 8 to 3 / 8 of the sheet thickness of the base steel sheet is tempered martensite having carbides with an average grain size of 50 nm to 200 nm, wherein the galvanized steel sheet has a tensile strength of 780 MPa or more and less than 1180 MPa, a yield ratio of 0.60 or more, and wherein the integrated value of the amount of hydrogen released when the base steel sheet is heated from room temperature to 200°C is 0.45 mass ppm or less.

2. The galvanized steel sheet according to claim 1, wherein the steel components of the base steel sheet contain, in mass%, C: 0.080% or more and 0.300% or less, Si: 0.20% or more and 2.00% or less, Mn: 1.00% or more and 4.00% or less, P: 0.10% or less, S: 0.0200% or less, Al: 0.003% or more and 0.100% or less, N: 0.0100% or less, with the balance being Fe and unavoidable impurities.

3. The steel components further include, in mass%, B: 0.0100% or less, Ti: 0.200% or less, Nb: 0.200% or less, Sb: 0.200% or less, Sn: 0.200% or less, V: 0.100% or less, Cu: 2.00% or less, Cr: 2.00% or less, Ni: 2.00% or less, Mo: 1.00% or less, Ta: 0.100% or less, W: 0.500% or less, Zr: 0.020% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, Zn: 0.020% or less, Co: 0.020% or less, Ce: 0.0200% or less, Se: 0.0200% or less, 3. The galvanized steel sheet according to claim 2, comprising at least one selected from the group consisting of Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0200% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM (excluding Ce): 0.0200% or less.

4. The galvanized steel sheet according to any one of claims 1 to 3, wherein the base steel sheet has a soft surface layer in which the Vickers hardness is 85% or less of the Vickers hardness at 1 / 4 of the sheet thickness when the surface layer is an area of ​​200 μm or less from the surface of the base steel sheet in the sheet thickness direction.

5. The galvanized steel sheet according to claim 4, wherein, when the nano-hardness is measured at 300 or more points in a 50 μm × 50 μm region of the sheet surface at a position 1 / 4 of the thickness direction depth of the soft surface layer from the surface of the base steel sheet and a position 1 / 2 of the thickness direction depth of the soft surface layer from the surface of the base steel sheet, the proportion of measurements where the nano-hardness of the sheet surface at a position 1 / 4 of the thickness direction depth of the soft surface layer from the surface of the base steel sheet is 7.0 GPa or more relative to the total number of measurements is 0.10 or less, further, the standard deviation σ of the nano-hardness of the sheet surface at a position 1 / 4 of the thickness direction depth of the soft surface layer from the surface of the base steel sheet is 1.8 GPa or less, and further, the standard deviation σ of the nano-hardness of the sheet surface at a position 1 / 2 of the thickness direction depth of the soft surface layer from the surface of the base steel sheet is 2.2 GPa or less.

6. A galvanized steel sheet according to any one of claims 1 to 5, having a metal plating layer formed between the base steel sheet and the galvanized layer on one or both sides of the galvanized steel sheet.

7. The galvanized steel sheet according to any one of claims 1 to 6, wherein the zinc plating layer is a zinc alloy plating layer.

8. A galvanized steel sheet according to any one of claims 1 to 7, wherein when the base steel sheet is heated from room temperature to 600°C, the integrated amount of hydrogen released in a temperature range of 350 to 600°C is 0.05 mass ppm or more.

9. A member made using the galvanized steel sheet according to any one of claims 1 to 8.

10. A hot rolling process in which a slab having the steel composition according to claim 2 or 3 is heated to a temperature range of 1100 to 1350°C, hot rolled at a finish rolling end temperature of 800 to 950°C, and coiled at a coiling temperature of 650°C or less; a reducing process in which the steel sheet after the hot rolling process is held in a reducing atmosphere at 700°C or higher and with a hydrogen concentration of 8 volume % to 30 volume % for 20 s or more; a soaking process in which the steel sheet after the reducing process is held in a soaking atmosphere at 750°C or higher and with a hydrogen concentration of 0.2 volume % to 8 volume % for 20 s to 300 s; a first cooling process in which the steel sheet after the soaking process is cooled; and a galvanizing process in which a galvanized layer is formed on the surface of the steel sheet after the first cooling process. a second cooling step of cooling the steel sheet after the galvanizing step to a cooling stop temperature of 100 to 300°C at an average cooling rate of 20°C / s or less from a temperature range of 350 to 450°C to (Ms point - 100°C) and by retaining the steel sheet in a temperature range of 100 to 350°C for 5 seconds or more; and a reheating step of holding the steel sheet after the second cooling step in a temperature range of not less than the cooling stop temperature and not more than 450°C for 5 to 600 seconds.

11. The method for producing a galvanized steel sheet according to claim 10, further comprising the steps of: forming the galvanized layer on the surface of the steel sheet after the galvanizing step; and then carrying out an alloying treatment.

12. A method for producing a galvanized steel sheet according to claim 10 or 11, comprising a cold rolling step of cold rolling at a reduction rate of 20% or more after the hot rolling step and before the reducing step.

13. A method for producing a galvanized steel sheet according to any one of claims 10 to 12, wherein in the first cooling step, the steel sheet after the soaking step is cooled from 600 to 900°C to 150 to 500°C at an average cooling rate of 20°C / s or less in an atmosphere having a hydrogen concentration of 0.5 vol.% or more and 30 vol.% or less and a dew point of 0°C or less.

14. A method for producing a zinc-plated steel sheet as described in any one of claims 10 to 13, wherein in the second cooling step, the average cooling rate from the temperature range of 350 to 450°C to (Ms point - 100°C) is 10°C / s or less, and the sheet is allowed to dwell in the temperature range of 100 to 350°C for 10 seconds or more before being cooled to a cooling stop temperature of 100 to 300°C.

15. A method for producing a zinc-plated steel sheet according to any one of claims 10 to 14, wherein the soaking atmosphere in the soaking step has a dew point of -30°C or higher.

16. A method for producing a galvanized steel sheet according to any one of claims 10 to 15, comprising a pre-plating step of applying metal plating to one or both sides of the steel sheet after the hot rolling step and before the reducing step to form a metal plating layer.

17. A method for producing a galvanized steel sheet according to any one of claims 10 to 16, further comprising an oxidation step of heating the steel sheet after the hot rolling step and before the reducing step to 600°C or higher in an oxidizing atmosphere containing an oxygen concentration of 1,000 ppm by volume or more and 30,000 ppm by volume or less.

18. A method for manufacturing a component, comprising the step of subjecting the galvanized steel sheet according to any one of claims 1 to 8 to at least one of forming and joining to form the component.

Citation Information

Patent Citations

  • HIGH STRENGTH STEEL SHEET HAVING MAXIMUM TENSILE STRENGTH OF &gt;=900 MPa AND HAVING SATISFACTORY DUCTILITY AND DELAYED FRACTURE RESISTANCE, METHOD FOR PRODUCING HIGH STRENGTH COLD ROLLED STEEL SHEET, AND METHOD FOR PRODUCING HIGH STRENGTH GALVANIZED STEEL SHEET

    JP2011111671A

  • High-strength hot-dip galvanized steel sheet and production method thereof

    WO2016113788A1

  • High strength steel sheet excellent in collision characteristic and manufacturing method therefor

    JP2015175050A

  • High-strength cold-rolled steel sheet, and process for production thereof

    WO2011093319A1

  • Thin steel sheet, and production method therefor

    WO2018030501A1