Cutting tool
The cutting tool employs a multilayer coating structure with alternating TiAlBN and TiAlN layers, addressing the challenge of short tool life by enhancing wear resistance and thermal stability, resulting in improved durability and extended tool life.
Patent Information
- Application Number
- PCT/JP2023/016837
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional cutting tools face challenges in achieving long tool life, particularly in stainless steel turning, due to high wear rates and limited durability, necessitating advancements in coating technologies to enhance wear resistance and thermal stability.
A cutting tool with a multilayer coating structure comprising alternating layers of TiAlBN and TiAlN, where the first layer has a high titanium content and the second layer has a higher aluminum content, providing improved hardness and thermal stability, and further enhanced by alternating third and fourth unit layers, which suppress crack propagation and improve chipping resistance.
The multilayer coating structure significantly extends the tool life by balancing crater wear resistance and chipping resistance, maintaining stable hardness under high temperatures and reducing large-scale damage, thus improving the overall performance of the cutting tool.
Smart Images

Figure JP2023016837_31102024_PF_FP_ABST
Abstract
Description
cutting tools
[0001] The present disclosure relates to cutting tools.
[0002] BACKGROUND ART Conventionally, in order to improve the performance of cutting tools, development has been underway for coatings that coat the surfaces of substrates made of cemented carbide, cubic boron nitride sintered bodies, etc. (for example, Patent Document 1).
[0003] International Publication No. 2022 / 176057
[0004] A cutting tool according to the present disclosure is a cutting tool including a substrate and a coating provided on the substrate, wherein the coating includes a first layer and a second layer, the second layer is provided closer to the substrate than the first layer, the first layer has a multilayer structure in which first unit layers and second unit layers are alternately stacked, the average thickness of the first unit layers is 2 nm or more and 50 nm or less, the average thickness of the second unit layers is 2 nm or more and 50 nm or less, and the first unit layers are made of Ti. a Al 1-a-b B b N, wherein 0.30≦a≦0.50 and 0<b≦0.10 are satisfied, and the second unit layer is composed of Ti c Al 1-c N, wherein 0.70≦c≦1.00 is satisfied, in the first layer, a percentage (T2 / T1)×100 of the number of titanium atoms T2 to the total number T1 of titanium and aluminum atoms is 60% or more, the second layer has a multilayer structure in which third unit layers and fourth unit layers are alternately stacked, the average thickness of the third unit layers is 2 nm or more and 100 nm or less, the average thickness of the fourth unit layers is 2 nm or more and 100 nm or less, and the third unit layers are composed of Ti, d Al 1-d-e B e N, and the fourth unit layer is made of Ti f Al 1-f-g B gN, wherein the following conditions are satisfied: 0.25≦d<0.45, 0<e≦0.10, 0.35≦f<0.55, 0<g≦0.10, 0.05≦f−d≦0.20; and in the X-ray diffraction spectrum of the second layer, a ratio I(200) / I(002) of a peak intensity I(200) derived from the (200) plane to a peak intensity I(002) derived from the (002) plane is 2 or more, and a half-width of the peak derived from the (002) plane is 2 degrees or more.
[0005] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a cutting tool according to embodiment 1. FIG. 2 is a schematic cross-sectional view showing an example of the configuration of a film-forming apparatus. FIG. 3 is a schematic cross-sectional view showing an example of the configuration of a film-forming apparatus. FIG. 4 is a diagram for explaining a measurement area when measuring the diameter of the maximum inscribed circle of a crystal grain in a first layer. FIG. 5 is a diagram for explaining a method for measuring the diameter of the maximum inscribed circle of a crystal grain in a first layer, and is a diagram schematically showing a bright-field image of the measurement field. FIG. 6 is a diagram for explaining the positional relationship between the crystal grain and the first and second unit layers.
[0006] [Problem to be Solved by the Present Disclosure] In recent years, there has been an increasing demand for cost reduction, and there is a demand for longer tool life. For example, there is a demand for cutting tools with long tool life in the turning of stainless steel.
[0007] Therefore, an object of the present disclosure is to provide a cutting tool having a long tool life.
[0008] Effect of the Present Disclosure The cutting tool of the present disclosure can have a long tool life.
[0009] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described. (1) A cutting tool of the present disclosure is a cutting tool including a substrate and a coating provided on the substrate, wherein the coating includes a first layer and a second layer, the second layer is provided closer to the substrate than the first layer, the first layer has a multilayer structure in which first unit layers and second unit layers are alternately stacked, the average thickness of the first unit layers is 2 nm or more and 50 nm or less, the average thickness of the second unit layers is 2 nm or more and 50 nm or less, and the first unit layers are made of Ti. a Al 1-a-b B b N, wherein 0.30≦a≦0.50 and 0<b≦0.10 are satisfied, and the second unit layer is composed of Ti c Al 1-c N, wherein 0.70≦c≦1.00 is satisfied, in the first layer, a percentage (T2 / T1)×100 of the number of titanium atoms T2 to the total number T1 of titanium and aluminum atoms is 60% or more, the second layer has a multilayer structure in which third unit layers and fourth unit layers are alternately stacked, the average thickness of the third unit layers is 2 nm or more and 100 nm or less, the average thickness of the fourth unit layers is 2 nm or more and 100 nm or less, and the third unit layers are composed of Ti, d Al 1-d-e B e N, and the fourth unit layer is made of Ti f Al 1-f-g B g N, wherein the following conditions are satisfied: 0.25≦d<0.45, 0<e≦0.10, 0.35≦f<0.55, 0<g≦0.10, 0.05≦f−d≦0.20; and in the X-ray diffraction spectrum of the second layer, a ratio I(200) / I(002) of a peak intensity I(200) derived from the (200) plane to a peak intensity I(002) derived from the (002) plane is 2 or more, and a half-width of the peak derived from the (002) plane is 2 degrees or more.
[0010] The cutting tools of the present disclosure can have a long tool life.
[0011] (2) In the above (1), the first layer may have a nanoindentation hardness of 30 GPa or more at 25° C. This improves the wear resistance of the cutting tool.
[0012] (3) In the above (1) or (2), the first layer may have an average thickness of 1.0 μm or more and 20 μm or less. This increases the number of first unit layers and second unit layers in the first layer, further improving the effect of suppressing crack propagation. This can prevent large-scale damage to the coating and extend the tool life of the cutting tool.
[0013] (4) In any of (1) to (3) above, the second layer may have an average thickness of 0.5 μm or more and 10 μm or less. This increases the number of third unit layers and fourth unit layers in the second layer, further improving the effect of suppressing crack propagation. This can prevent large-scale damage to the coating and extend the tool life of the cutting tool.
[0014] [Details of the Embodiments of the Present Disclosure] Specific examples of cutting tools according to the present disclosure will be described below with reference to the drawings. In the drawings of the present disclosure, the same reference numerals represent the same or corresponding parts. Furthermore, dimensional relationships such as length, width, thickness, and depth have been appropriately changed for clarity and simplification of the drawings, and do not necessarily represent actual dimensional relationships.
[0015] In the present disclosure, the notation in the form of "A to B" means the upper and lower limits of a range (i.e., A or more and B or less), and when no unit is specified for A and a unit is specified only for B, the units of A and B are the same.
[0016] In the present disclosure, when a compound or the like is represented by a chemical formula, unless the atomic ratio is particularly limited, it is intended to include any conventionally known atomic ratio, and should not necessarily be limited to only those within the stoichiometric range.
[0017] In the present disclosure, when one or more numerical values are recited as the lower limit and the upper limit of a numerical range, a combination of any one numerical value recited as the lower limit and any one numerical value recited as the upper limit is also considered to be disclosed. For example, when a1 or more, b1 or more, and c1 or more are recited as the lower limit and a2 or less, b2 or less, and c2 or less are recited as the upper limit, a1 or more and a2 or less, a1 or more and b2 or less, a1 or more and c2 or less, b1 or more and a2 or less, b1 or more and b2 or less, b1 or more and c2 or less, c1 or more and a2 or less, c1 or more and b2 or less, and c1 or more and c2 or less are considered to be disclosed.
[0018] [Embodiment 1: Cutting Tool] A cutting tool according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 1") is a cutting tool including a substrate and a coating provided on the substrate, wherein the coating includes a first layer and a second layer, the second layer is provided closer to the substrate than the first layer, the first layer has a multilayer structure in which first unit layers and second unit layers are alternately stacked, the average thickness of the first unit layers is 2 nm or more and 50 nm or less, the average thickness of the second unit layers is 2 nm or more and 50 nm or less, and the first unit layers are made of Ti. a Al 1-a-b B b N, wherein 0.30≦a≦0.50 and 0<b≦0.10 are satisfied, and the second unit layer is composed of Ti c Al 1-c N, wherein 0.70≦c≦1.00 is satisfied, in the first layer, the percentage (T2 / T1)×100 of the number of titanium atoms T2 to the total number of titanium and aluminum atoms T1 is 60% or more, the second layer has a multilayer structure in which third unit layers and fourth unit layers are alternately stacked, the average thickness of the third unit layers is 2 nm or more and 100 nm or less, the average thickness of the fourth unit layers is 2 nm or more and 100 nm or less, and the third unit layers are composed of Ti, d Al 1-d-e B e N, and the fourth unit layer is made of Ti f Al 1-f-g B gN, wherein the following conditions are satisfied: 0.25≦d<0.45, 0<e≦0.10, 0.35≦f<0.55, 0<g≦0.10, 0.05≦f−d≦0.20; and in the X-ray diffraction spectrum of the second layer, a ratio I(200) / I(002) of a peak intensity I(200) derived from the (200) plane to a peak intensity I(002) derived from the (002) plane is 2 or more, and the half width of the peak derived from the (002) plane is 2 degrees or more.
[0019] The cutting tool of the present disclosure can have a long tool life, and the reason for this is presumably as follows.
[0020] (i) The coating of the cutting tool of the present disclosure includes a first layer having a multilayer structure in which first unit layers and second unit layers are alternately stacked. The first unit layers and second unit layers have different compositions. This makes it possible to suppress the propagation of cracks from the surface of the coating that occur during use of the cutting tool near the interface between the first unit layer and the second unit layer.
[0021] (ii) The first unit layer is Ti a Al 1-a-b B b The first unit layer is made of TiAlN (where 0.30≦a≦0.50, 0<b≦0.10). The hardness of the first unit layer is improved by adding a small amount of boron (B) to TiAlN. The second unit layer is made of Ti c Al 1-c N (where 0.70≦c≦1.00 is satisfied). The second unit layer has a high titanium (Ti) content and has excellent high-temperature stability. In the present disclosure, the first layer has a multilayer structure in which high-hardness first unit layers and second unit layers with excellent high-temperature stability are alternately stacked, thereby providing stable hardness even at high temperatures and improving crater wear resistance. Crater wear is wear that occurs mainly on the rake face of a cutting tool due to frictional heat between the cutting tool and the chips. Furthermore, the first layer has a multilayer structure in which high-hardness first unit layers and second unit layers with a lower hardness than the first unit layers are alternately stacked, thereby improving chipping resistance. Therefore, the crater wear resistance and chipping resistance of the coating are improved in a balanced manner, and the tool life of the cutting tool is extended.
[0022] (iii) The first unit layer and the second unit layer have different Ti and Al contents. Therefore, the first unit layer and the second unit layer have different crystal lattices, which causes distortion of the crystal lattice in the first layer, allowing the first layer to have high hardness. Therefore, a coating including the first layer can have excellent wear resistance.
[0023] (iv) In the first layer, the percentage (T2 / T1)×100 of the number of titanium atoms T2 to the total number of titanium and aluminum atoms T1 is 60% or more, which allows the first layer to have excellent crater wear resistance and extends the tool life of the cutting tool.
[0024] (v) The coating of the cutting tool of the present disclosure includes a second layer having a multilayer structure in which third unit layers and fourth unit layers are alternately stacked. The third unit layers and fourth unit layers have different compositions. This makes it possible to suppress the propagation of cracks from the surface of the coating near the interface between the third unit layer and the fourth unit layer during use of the cutting tool.
[0025] (vi) The second layer has a higher aluminum (Al) content and higher toughness than the first layer, so that the coating having the second layer can have excellent chipping resistance.
[0026] (vii) The third unit layer and the fourth unit layer have different Ti contents. Therefore, the third unit layer and the fourth unit layer have different crystal lattices, which causes distortion of the crystal lattice in the second layer, allowing the second layer to have high hardness. Therefore, a coating including the second layer can have excellent wear resistance.
[0027] <Cutting Tool> The cutting tool of embodiment 1 is not particularly limited in shape, use, etc., as long as it is a cutting tool. The cutting tool of embodiment 1 may be, for example, a drill, an end mill, an indexable insert for milling, an indexable insert for turning, a metal saw, a gear cutting tool, a reamer, a tap, or an insert for pin milling of a crankshaft.
[0028] 1 is a schematic partial cross-sectional view showing an example of the configuration of a cutting tool according to a first embodiment. The cutting tool 100 includes a substrate 10 and a coating 20 provided on the substrate 10. The coating 20 includes a first layer 21 and a second layer 22. The second layer 22 is provided closer to the substrate 10 than the first layer 21. The first layer 21 has a multilayer structure in which first unit layers 1 and second unit layers 2 are alternately stacked. The second layer 22 has a multilayer structure in which third unit layers 3 and fourth unit layers 4 are alternately stacked.
[0029] <<Substrate>> The substrate 10 is not particularly limited. The substrate 10 may be made of, for example, cemented carbide, cermet, high-speed steel, ceramics, cubic boron nitride sintered body, diamond sintered body, or the like. The substrate 10 is preferably made of cemented carbide. This is because cemented carbide has excellent wear resistance.
[0030] A cemented carbide is a sintered body whose main component is tungsten carbide (WC) particles. The cemented carbide includes a hard phase and a binder phase. The hard phase contains WC particles. The binder phase bonds the WC particles together. The binder phase contains, for example, cobalt (Co). The binder phase may further contain titanium carbide (TiC), tantalum carbide (TaC), niobium carbide (NbC), or the like.
[0031] The cemented carbide may contain impurities that are inevitably mixed in during the manufacturing process. The cemented carbide may also contain free carbon or an abnormal layer called an "η layer" in its structure. Furthermore, the cemented carbide may be subjected to a surface modification treatment. For example, the cemented carbide may include a de-β layer on its surface.
[0032] The cemented carbide may contain 85% by mass or more and 98% by mass or less of WC grains and 2% by mass or more and 15% by mass or less of Co. The WC grains may have an average grain size of 0.2 μm or more and 4 μm or less.
[0033] Co is softer than WC particles. As described below, the soft Co can be removed by subjecting the surface of the substrate 10 to ion bombardment treatment. When the cemented carbide has the above composition and the WC particles have the above average particle size, appropriate irregularities are formed on the surface after the Co is removed. It is believed that forming the coating 20 on such a surface produces an anchor effect, improving the adhesion between the coating 20 and the substrate 10.
[0034] Here, the grain size of a WC grain refers to the diameter of a circle circumscribing a two-dimensional projected image of the WC grain. The grain size is measured using a scanning electron microscope (SEM) or a transmission electron microscope (TEM). That is, the cemented carbide is cut and the cut surface is observed using an SEM or TEM. In the observed image, the diameter of the circle circumscribing the WC grain is regarded as the grain size of the WC grain. In the observed image, the grain sizes of 10 or more (preferably 50 or more, more preferably 100 or more) randomly selected WC grains are measured, and the arithmetic mean value is taken as the average grain size of the WC grains. Before the observation, it is desirable to process the cut surface with a cross section polisher (CP) or a focused ion beam (FIB) or the like.
[0035] <Coating> The coating 20 is provided on the substrate 10. The coating 20 may be provided on a portion of the surface of the substrate 10, or may be provided on the entire surface. However, the coating 20 is provided on at least a portion of the surface of the substrate 10 that corresponds to the cutting edge. In the present disclosure, the portion of the surface of the substrate 10 that corresponds to the cutting edge refers to an area on the surface of the substrate 10 that is within 0.5 mm or 2 mm from the cutting edge ridge. As long as the effects of the present disclosure are not impaired, it does not deviate from the scope of the present disclosure even if a coating is not formed on at least a portion of the portion that corresponds to the cutting edge.
[0036] The coating 20 includes a first layer 21 and a second layer 22. The second layer 22 may be provided directly on the substrate 10. The first layer 21 may be the outermost layer of the coating 20. The coating 20 may consist of a second layer 22 provided directly on the substrate 10 and the first layer 21 provided directly on the second layer 22. The coating 20 may include other layers in addition to the first layer 21 and the second layer 22, as long as the effects of the present disclosure are not impaired. For example, the coating 20 may include one or both of a base layer provided between the substrate 10 and the second layer 22 and a surface layer provided on the outermost surface of the coating 20. The base layer may include at least one layer selected from the group consisting of a TiCN layer, a TiN layer, and a TiCNO layer. The surface layer may include at least one layer selected from the group consisting of a TiC layer, a TiN layer, and a TiCN layer.
[0037] The layer structure of the coating 20 does not need to be uniform over the entire coating 20, and the layer structure may be partially different.
[0038] The thickness of the coating 20 may be 1.5 μm or more and 30 μm or less. When the thickness of the coating 20 is 1.5 μm or more, wear resistance is improved. When the thickness of the coating 20 is 30 μm or less, chipping resistance is improved. The thickness of the coating 20 may be 2.0 μm or more and 25 μm or less, or 3.0 μm or more and 20 μm or less. Here, the thickness of the coating means the sum of the thicknesses of the layers that make up the coating. Examples of the "layers that make up the coating" include a first layer, a second layer, a base layer, and a surface layer.
[0039] The thickness of each layer constituting the coating is measured by obtaining a thin section sample (hereinafter also referred to as a "cross-sectional sample") of a cross section parallel to the normal direction of the surface of the cutting tool and observing the cross-sectional sample with a scanning transmission electron microscope (STEM). An example of a scanning transmission electron microscope is the JEM-2100F (trade name) manufactured by JEOL Ltd. The cross-sectional sample is observed at a magnification of 5,000 to 10,000 times, and the thickness of each layer is measured at five locations, and the arithmetic average value is taken as the "thickness of each layer."
[0040] It has been confirmed that as long as measurements are made using the same cutting tool, there is no variation in the measurement results even if the measurement location is selected arbitrarily.
[0041] <First Layer> The first layer 21 has a multilayer structure in which first unit layers 1 and second unit layers 2 are alternately stacked. The number of stacked layers is not particularly limited as long as the average thickness of each of the first unit layers 1 and second unit layers 2 is 2 nm or more and 50 nm or less. The number of stacked layers refers to the number of first unit layers 1 and second unit layers 2 included in the first layer 21. The number of stacked layers may be 10 or more and 5,000 or less, 200 or more and 5,000 or less, 400 or more and 2,000 or less, or 500 or more and 1,000 or less. In the first layer 21, the layer closest to the substrate 10 may be either the first unit layer 1 or the second unit layer 2. In the first layer 21, the layer farthest from the substrate 10 may be either the first unit layer 1 or the second unit layer 2.
[0042] The average thickness of the first layer can be 1.0 μm or more and 20 μm or less. When the average thickness of the first layer is 1.0 μm or more, wear resistance is improved. When the average thickness of the first layer is 20 μm or less, chipping resistance is improved. The lower limit of the average thickness of the first layer may be 1.0 μm or more, 2.0 μm or more, or 3.0 μm or more. The upper limit of the average thickness of the first layer may be 20 μm or less, 18 μm or less, 16 μm or less, or 12 μm or less. The average thickness of the first layer may be 1.0 μm or more and 20 μm or less, 2.0 μm or more and 16 μm or less, or 3.0 μm or more and 12 μm or less.
[0043] <Average Thickness of First Unit Layer and Second Unit Layer> The average thickness of the first unit layer 1 is 2 nm or more and 50 nm or less, and the average thickness of the second unit layer 2 is 2 nm or more and 50 nm or less. By alternately stacking such thin layers in the first layer, crack propagation can be suppressed. If the average thickness of one or both of the first unit layer 1 and the second unit layer 2 is less than 2 nm, the compositions of the first unit layer 1 and the second unit layer 2 may be mixed, potentially reducing the effect of suppressing crack propagation. If the average thickness of one or both of the first unit layer 1 and the second unit layer 2 exceeds 50 nm, the effect of suppressing delamination may be reduced. The average thickness of the first unit layer and the average thickness of the second unit layer may be the same or different.
[0044] The lower limit of the average thickness of the first unit layer is 2 nm or more, or may be 4 nm or more, 6 nm or more, or 8 nm or more. The upper limit of the average thickness of the first unit layer is 50 nm or less, or may be 46 nm or less, or may be 40 nm or less, or may be 30 nm or less. The average thickness of the first unit layer is 2 nm or more and 50 nm or less, or may be 4 nm or more and 40 nm or less, or may be 6 nm or more and 30 nm or less.
[0045] The lower limit of the average thickness of the second unit layer is 2 nm or more, or may be 4 nm or more, 6 nm or more, or 8 nm or more. The upper limit of the average thickness of the second unit layer is 50 nm or less, or may be 46 nm or less, or may be 40 nm or less, or may be 30 nm or less. The average thickness of the second unit layer is 2 nm or more and 50 nm or less, or may be 4 nm or more and 40 nm or less, or may be 6 nm or more and 30 nm or less.
[0046] The method for measuring the average thickness of each of the first unit layer and the second unit layer is as follows. A thin section sample (hereinafter also referred to as a "cross-sectional sample") of the cutting tool cross section parallel to the normal direction of the surface of the cutting tool is obtained. The cross-sectional sample is observed with a scanning transmission electron microscope (STEM). An example of a scanning transmission electron microscope is the JEM-2100F (product name) manufactured by JEOL Ltd. The observation magnification of the cross-sectional sample is adjusted appropriately depending on the thickness of the first unit layer 1 and the second unit layer 2. For example, the observation magnification can be approximately 1,000,000 times. The thickness is measured at five locations for one first unit layer. The arithmetic mean value of the thicknesses of the five locations of the first unit layer is calculated, and this arithmetic mean value is defined as the average thickness of the first unit layer. The thickness is measured at five locations for one second unit layer.
[0047] For each of five different first unit layers, the average thickness of the first unit layer is measured using the above procedure. The arithmetic mean value of the average thicknesses of the five first unit layers is determined. In the present disclosure, this arithmetic mean value is referred to as the average thickness of the first unit layer. For each of five different second unit layers, the average thickness of the second unit layer is measured using the above procedure. The arithmetic mean value of the average thicknesses of the five second unit layers is determined. In the present disclosure, this arithmetic mean value is referred to as the average thickness of the second unit layer. The average thicknesses of the third and fourth unit layers described below are also measured in the same manner as above.
[0048] It has been confirmed that as long as measurements are made using the same cutting tool, there is no variation in the measurement results even if the measurement location is selected arbitrarily.
[0049] <Composition of First Unit Layer and Second Unit Layer> In the cutting tool of the present disclosure, the first unit layer comprises Ti a Al 1-a-b B b N, where 0.30≦a≦0.50, 0<b≦0.10 are satisfied, and the second unit layer is Ti c Al 1-c N, where 0.70≦c≦1.00 is satisfied. The first unit layer may be made of Ti as long as it does not impair the effect of the present disclosure. a Al 1-a-b B b The first unit layer may contain impurities together with N. a Al 1-a-b B b The second unit layer may be composed of N and impurities. c Al 1-c The second unit layer may contain impurities together with N. c Al 1-c It can be composed of N and impurities, such as carbon (C) and oxygen (O).
[0050] In the first unit layer, the lower limit of a is 0.30 or more, or may be 0.36 or more, or 0.37 or more, or 0.39 or more. The upper limit of a is 0.50 or less, or may be 0.48 or less, or may be 0.45 or less. a may be 0.36≦a≦0.48 or 0.37≦a≦0.45.
[0051] In the first unit layer, the lower limit of b is greater than 0, and may be 0.01 or greater, 0.02 or greater, or 0.05 or greater. The upper limit of b is 0.10 or less, 0.08 or less, or 0.07 or less. b may satisfy 0.01≦b≦0.08 or 0.02≦b≦0.07.
[0052] In the second unit layer, the lower limit of c is 0.70 or more, or may be 0.75 or more, or 0.80 or more, or 0.87 or more. The upper limit of c is 1.00 or less, or may be 0.95 or less, or may be 0.92 or less. c may be in the range of 0.75≦d≦0.95, or 0.80≦d≦0.92.
[0053] Ti of the first unit layer a Al 1-a-b B b a, b and second unit layer Ti in N c Al 1-c The c in N is determined by measuring the composition of each layer using energy dispersive X-ray spectrometry (EDX). An EDX (TEM-DEX) attached to a transmission electron microscope (TEM) is used for the composition analysis. An example of an EDX device is the JED-2300 (trademark) manufactured by JEOL Ltd.
[0054] The composition analysis is performed as follows: A thin section sample (hereinafter also referred to as a "cross-sectional sample") of a cross section parallel to the normal direction of the cutting tool surface is obtained. While observing the cross-sectional sample with a TEM, EDX analysis is performed at five arbitrarily selected points within one first unit layer or one second unit layer. The first unit layer and the second unit layer can be distinguished by the difference in contrast. Here, the "five arbitrarily selected points" are selected from different crystal grains. The composition ratios of each element obtained from the measurements at the five points are arithmetically averaged to identify the respective compositions of the first unit layer and the second unit layer.
[0055] For each of five different first unit layers, the composition of the first unit layer is determined using the above procedure. In the present disclosure, the average of the compositions of the five first unit layers is taken as the composition of the first unit layer, and a and b are determined based on this. For each of five different second unit layers, the composition of the second unit layer is determined using the above procedure. In the present disclosure, the average of the compositions of the five second unit layers is taken as the composition of the second unit layer, and c is determined based on this. The compositions of the third and fourth unit layers described below, as well as the Ti of the third unit layer, are determined. d Al 1-d-e B e d and e in N, Ti in the fourth unit layer f Al 1-f-g B g f and g in N are also measured in the same manner as above.
[0056] It has been confirmed that as long as measurements are taken using the same cutting tool, there is no variation in the measurement results even if the measurement points are selected arbitrarily.
[0057] <Composition of First Layer> In the first layer, the percentage (T2 / T1) × 100 (hereinafter also referred to as "percentage (T2 / T1) × 100") of the number of titanium atoms T2 relative to the total number of titanium and aluminum atoms T1 is 60% or more. This allows the first layer to have excellent crater wear resistance. From the viewpoint of improving crater wear resistance, the lower limit of percentage (T2 / T1) × 100 is 60% or more, or may be 60.0% or more, 62.2% or more, 62.5% or more, 63% or more, 63.5% or more, or 66% or more. From the viewpoint of improving oxidation resistance, the upper limit of percentage (T2 / T1) × 100 may be 80% or less, 77% or less, 76.9% or less, or 75% or less. The percentage (T2 / T1) x 100 may be 60% or more and 80% or less, 63% or more and 77% or less, or 66% or more and 75% or less.
[0058] The percentage (T2 / T1) x 100 in the first layer is measured by TEM-EDX. An example of an EDX device is the JED-2300 (product name) manufactured by JEOL Ltd. The percentage (T2 / T1) x 100 is measured by the following procedure.
[0059] A thin section sample (hereinafter also referred to as a "cross-sectional sample") of a cross section parallel to the normal direction of the cutting tool surface is obtained. While observing the cross-sectional sample with a TEM, EDX analysis is performed on five arbitrarily selected fields within the first layer to measure the percentage (T2 / T1) x 100 of the number of titanium atoms T2 relative to the total number of titanium and aluminum atoms T1. Here, the "five arbitrarily selected fields" are set so that they do not overlap with each other. The range of one field is 200 x 200 nm. In the present disclosure, the arithmetic mean of the percentages (T2 / T1) x 100 obtained by measuring the five fields is defined as the percentage (T2 / T1) x 100 in the first layer.
[0060] It has been confirmed that as long as measurements are taken using the same cutting tool, there is no variation in the measurement results even if the measurement points are selected arbitrarily.
[0061] <Nanoindentation hardness of first layer> The nanoindentation hardness of the first layer at 25°C may be 30 GPa or more. This improves the wear resistance of the cutting tool. The lower limit of the nanoindentation hardness may be 32 GPa or more, or 34 GPa or more. The upper limit of the nanoindentation hardness H is not particularly limited, but from a manufacturing standpoint, it may be 60 GPa or less, 40 GPa or less, or 36 GPa or less. The nanoindentation hardness H may be 30 GPa or more and 60 GPa or less, 32 GPa or more and 60 GPa or less, or 34 GPa or more and 60 GPa or less.
[0062] The nanoindentation hardness of the first layer at 25°C is measured by the nanoindentation method in accordance with the standard procedure defined in "ISO 14577-1: 2015 Metallic materials - Instrumented indentation test for hardness and materials parameters -." The measuring instrument used is an "ENT-1100a" manufactured by Elionix. The indenter load is 1 g. In a cross section parallel to the normal direction of the cutting tool surface, the indenter is pressed against the first layer in the direction perpendicular to the cross section (i.e., parallel to the surface of the cutting tool).
[0063] The above measurement is performed at five locations on one measurement sample. The average value of the nanoindentation hardness at the five locations is taken as the nanoindentation hardness of the first layer. Note that data that appear to be abnormal at first glance are to be excluded.
[0064] It has been confirmed that as long as measurements are taken using the same cutting tool, there is no variation in the measurement results even if the measurement points are selected arbitrarily.
[0065] <Diameter of the largest inscribed circle of the crystal grains in the first layer> The first layer may be composed of a plurality of crystal grains, and the diameter of the largest inscribed circle of the crystal grains may be 5 nm or more and 500 nm or less. This improves the crater wear resistance of the cutting tool. The first layer of the present disclosure may include, in addition to the plurality of crystal grains, regions that do not constitute crystal grains (regions with random atomic arrangement), as long as the effects of the present disclosure are not impaired.
[0066] The upper limit of the diameter of the maximum inscribed circle of the crystal grain may be 500 nm or less, 450 nm or less, or 400 nm or less from the viewpoint of improving wear resistance and chipping resistance. The lower limit of the diameter of the maximum inscribed circle of the crystal grain may be 5 nm or more, 7 nm or more, or 10 nm or more from the viewpoint of suppressing a decrease in film hardness due to excessive crystal grain refinement. The diameter of the maximum inscribed circle of the crystal grain may be 5 nm or more and 500 nm or less, 7 nm or more and 450 nm or less, or 10 nm or more and 400 nm or less.
[0067] The diameter of the maximum inscribed circle of the crystal grain is measured as follows. A thin section sample (thickness: approximately 10 to 100 nm, hereinafter also referred to as "cross-sectional sample") of the cutting tool cross section parallel to the normal direction of the cutting tool surface is obtained. The cross-sectional sample is observed with a transmission electron microscope (TEM) to obtain a bright-field image. The observation magnification is 1,000,000 to 5,000,000 times. As shown in Figure 4, the bright-field image is obtained so as to include an area A sandwiched between a line L2 that is 0.2 μm away from a line L1 indicating the center of the average thickness direction of the first layer toward the substrate side, and a line L3 that is 0.2 μm away from the line L1 toward the surface side of the coating. A rectangular measurement field of 150 nm x 150 nm is arbitrarily set within the area A.
[0068] In the above measurement field of view, a region where the atomic arrangement is ±0.5° or less is identified and this region is defined as a crystal grain. The method for identifying the region where the atomic arrangement is ±0.5° or less and the crystal grain will be described with reference to FIG. 5 .
[0069] FIG. 5 is a schematic diagram showing an example of a bright-field image of the above-mentioned measurement field. In FIG. 5, atoms are indicated by black dots with the reference numeral 50. Note that FIG. 5 shows only a portion of the atoms. In the bright-field image, regularly arranged atoms 50 are connected by line segments that provide the shortest interatomic distances. In FIG. 5, the line segments are indicated by L10 to L14, L20 to L22, and L30 to L34. Regions where the angle between the line segments is ±0.5° or less (i.e., −0.5° or more and 0.5° or less) are defined as crystal grains.
[0070] 5, the angle between line segments L10 to L14 is ±0.5° or less, and the region containing these line segments corresponds to crystal grain 24a. The angle between line segments L20 to L22 is ±0.5° or less, and the region containing these line segments corresponds to crystal grain 24b. The angle between line segments L30 to L34 is ±0.5° or less, and the region containing these line segments corresponds to crystal grain 24c.
[0071] The diameter of the largest inscribed circle of each crystal grain in the measurement field is determined. The diameter of the largest inscribed circle means the diameter of the largest inscribed circle that can be drawn inside the crystal grain and that contacts at least a part of the outer edge of the crystal grain.
[0072] In Fig. 5, the diameter of the maximum inscribed circle 25a of crystal grain 24a is D1. The diameter of the maximum inscribed circle 25b of crystal grain 24b is D2. The diameter of the maximum inscribed circle 25c of crystal grain 24c is D3. When D1, D2, and D3 are all 50 nm or less, it is confirmed that the first layer shown in Fig. 5 is made up of a plurality of crystal grains, and the diameters of the maximum inscribed circles of the crystal grains are 50 nm or less.
[0073] It has been confirmed that, as long as the measurement is performed using the same cutting tool, there is no variation in the measurement results of the diameter of the maximum inscribed circle of the crystal grain, even if the measurement field is set arbitrarily.
[0074] In Figure 5, there are spaces between crystal grains 24a, 24b, and 24c, but in reality, crystal grains exist in the spaces. Because the thickness of a cross-sectional sample for TEM is approximately 10 to 100 nm, the bright-field image also reflects information in the depth direction. In areas where multiple crystal grains overlap in the thickness direction of the sample, a regular atomic arrangement cannot be confirmed in the bright-field image. Therefore, the areas where multiple crystal grains overlap are not identified as crystal grains using the above identification method.
[0075] <Positional Relationship Between Crystal Grains and First and Second Unit Layers> The positional relationship between crystal grains and first and second unit layers will be described with reference to FIG. 6 . FIG. 6 is a schematic diagram illustrating a cross section of the first layer of embodiment 1 taken along the film thickness direction. As shown in FIG. 6 , the first layer 21 has a multilayer structure in which first unit layers 1 and second unit layers 2 are alternately stacked. FIG. 6 illustrates a plurality of crystal grains 24, and the boundaries between the crystal grains 24 are indicated as crystal grain boundaries 25. Each crystal grain 24 can be composed of only the first unit layer or only the second unit layer. Furthermore, each crystal grain 24 can exist across one or more first unit layers and one or more second unit layers. That is, each crystal grain 24 can have a lamellar structure in which first unit layers and second unit layers are alternately stacked.
[0076] <Second Layer> The second layer 22 has a multilayer structure in which third unit layers 3 and fourth unit layers 4 are alternately stacked. The number of stacked layers is not particularly limited as long as the average thickness of each of the third unit layers 3 and the fourth unit layers 4 is 2 nm or more and 50 nm or less. The number of stacked layers refers to the number of third unit layers 3 and the number of fourth unit layers 4 included in the second layer 22. The number of stacked layers may be 10 to 5,000, 200 to 5,000, 400 to 2,000, or 500 to 1,000. In the second layer 22, the layer closest to the substrate 10 may be either the third unit layer 3 or the fourth unit layer 4. In the second layer 22, the layer farthest from the substrate 10 may be either the third unit layer 3 or the fourth unit layer 4.
[0077] The average thickness of the second layer can be 0.5 μm or more and 10 μm or less. When the average thickness of the second layer is 0.5 μm or more, wear resistance is improved. When the average thickness of the second layer is 10 μm or less, chipping resistance is improved. The lower limit of the average thickness of the second layer may be 1.0 μm or more, 2.0 μm or more, or 3.0 μm or more. The upper limit of the average thickness of the second layer may be 10 μm or less, 9 μm or less, 8 μm or less, or 7 μm or less. The average thickness of the second layer may be 1.0 μm or more and 9 μm or less, 2.0 μm or more and 8 μm or less, or 3.0 μm or more and 7 μm or less.
[0078] <Average Thickness of Third Unit Layer and Fourth Unit Layer> The average thickness of the third unit layer 3 is 2 nm or more and 100 nm or less, and the average thickness of the fourth unit layer 4 is 2 nm or more and 100 nm or less. By alternately stacking such thin layers in the second layer, crack propagation can be suppressed. If the average thickness of one or both of the third unit layer 3 and the fourth unit layer 4 is less than 2 nm, the compositions of the third unit layer 3 and the fourth unit layer 4 may be mixed, potentially reducing the effect of suppressing crack propagation. If the average thickness of one or both of the third unit layer 3 and the fourth unit layer 4 exceeds 100 nm, the effect of suppressing delamination may be reduced. The average thickness of the third unit layer and the average thickness of the fourth unit layer may be the same or different.
[0079] The lower limit of the average thickness of the third unit layer is 2 nm or more, and may be 5 nm or more, 10 nm or more, 15 nm or more, or 20 nm or more. The upper limit of the average thickness of the third unit layer is 100 nm or less, 80 nm or less, 75 nm or less, 65 nm or less, or 64 nm or less. The average thickness of the third unit layer is 2 nm or more and 100 nm or less, and may be 5 nm or more and 75 nm or less, or 10 nm or more and 65 nm or less.
[0080] The lower limit of the average thickness of the fourth unit layer is 2 nm or more, and may be 5 nm or more, 10 nm or more, 15 nm or more, or 20 nm or more. The upper limit of the average thickness of the fourth unit layer is 100 nm or less, 80 nm or less, 75 nm or less, 65 nm or less, 52 nm or less, or 50 nm or less. The average thickness of the fourth unit layer is 2 nm or more and 100 nm or less, 5 nm or more and 75 nm or less, or 10 nm or more and 50 nm or less.
[0081] The average thickness of each of the third and fourth unit layers is measured in the same manner as the average thickness of each of the first and second unit layers described above. It has been confirmed that, as long as the measurements are performed using the same cutting tool, there is no variation in the measurement results even if the measurement points are arbitrarily selected.
[0082] <Composition of Third Unit Layer and Fourth Unit Layer> In the cutting tool of the present disclosure, the third unit layer comprises Ti d Al 1-d-e B e N, where 0.25≦d<0.45 and 0<e≦0.10 are satisfied, and the fourth unit layer is Ti f Al 1-f-g B g N, where 0.35≦f<0.55, 0<g≦0.10, and 0.05≦f−d≦0.2 are satisfied. The third unit layer may be made of Ti, as long as the effect of the present disclosure is not impaired. d Al 1-d-e B e The third unit layer can contain impurities together with N. d Al 1-d-e B e The fourth unit layer may be composed of N and impurities. f Al 1-f-g B g The fourth unit layer can contain impurities together with N. f Al 1-f-g B g It can be composed of N and impurities, such as carbon (C) and oxygen (O).
[0083] In the third unit layer, the lower limit of d is 0.25 or more, and may be 0.30 or more, 0.31 or more, 0.32 or more, 0.33 or more, or 0.34 or more. The upper limit of d is less than 0.45, and may be 0.40 or less, 0.37 or less, or 0.35 or less. d may be in the range of 0.30≦d≦0.40, or 0.31≦d≦0.37.
[0084] In the third unit layer, the lower limit of e is greater than 0, and may be 0.01 or greater, 0.02 or greater, 0.04 or greater, or 0.05 or greater. The upper limit of e is 0.10 or less, 0.08 or less, 0.07 or less, or 0.06 or less. e may be in the range of 0.01≦e≦0.08, or 0.02≦e≦0.07.
[0085] In the fourth unit layer, the lower limit of f is 0.35 or more, and may be 0.40 or more, 0.41 or more, 0.42 or more, 0.43 or more, or 0.45 or more. The upper limit of f is less than 0.55 and may be 0.50 or less. c may be 0.40≦f<0.55 or 0.45≦f≦0.50.
[0086] In the fourth unit layer, the lower limit of g is greater than 0, and may be 0.01 or greater, 0.02 or greater, or 0.04 or greater. The upper limit of g is 0.10 or less, 0.08 or less, or 0.06 or less. c may be 0.01≦f≦0.10 or 0.02≦f≦0.06.
[0087] In the second layer, the lower limit of f-d is 0.05 or more, and may be 0.08 or more, 0.10 or more, or 0.11 or more. The upper limit of f-d is 0.20 or less, and may be 0.18 or less. f-d may be 0.08≦f-d≦0.18, or 0.10≦f-d≦0.18.
[0088] Ti of the third unit layer d Al 1-d-e B e d and e in N, Ti in the fourth unit layer f Al 1-f-g B g f and g in N are the Ti of the first unit layer described above.a Al 1-a-b B b a, b and second unit layer Ti in N c Al 1-c It is measured in the same manner as c in N. It has been confirmed that there is no variation in the measurement results even if the measurement location is arbitrarily selected, as long as the measurement is performed using the same cutting tool.
[0089] X-ray Diffraction Analysis of the Second Layer In the X-ray diffraction spectrum of the second layer, the ratio I(200) / I(002) of the peak intensity I(200) derived from the (200) plane to the peak intensity I(002) derived from the (002) plane is 2 degrees or greater, and the half-width of the peak derived from the (002) plane is 2 degrees or greater. This improves the hardness and toughness of the second layer, resulting in excellent wear resistance and chipping resistance. The "peak intensity I(002) derived from the (002) plane" refers to the diffraction intensity (peak height) of the highest X-ray diffraction peak derived from the (002) plane of the hexagonal crystal. The "peak intensity I(200) derived from the (200) plane" refers to the diffraction intensity (peak height) of the highest X-ray diffraction peak derived from the (200) plane of the cubic crystal. The presence of a peak derived from the (002) plane of the hexagonal crystal in the X-ray diffraction spectrum of the second layer confirms that the second layer contains a hexagonal crystal structure. If the X-ray diffraction spectrum of the second layer shows a peak due to the (200) plane of the cubic crystal, it is confirmed that the second layer has a cubic crystal structure. A ratio I(200) / I(002) of 2 or more means that a mixed crystal of cubic and hexagonal crystals is formed in the second layer.
[0090] The conditions for X-ray diffraction analysis when measuring the peak intensity I(002) and peak intensity I(200) are as follows: Scan axis: 2θ-θ X-ray source: Cu-Kα ray (1.541862 Å) Detector: 0-dimensional detector (scintillation counter) Tube voltage: 45 kV Tube current: 40 mA Incident optical system: Use of a mirror Receiving optical system: Use of an analyzer crystal (PW3098 / 27) Step: 0.03° Integration time: 2 seconds Scan range (2θ): 20° to 80°
[0091] X-ray diffraction measurement (XRD measurement) is performed using the θ / 2θ method at each of three arbitrary locations in the second layer to determine the X-ray diffraction intensity of a predetermined crystal plane, and the average of the X-ray diffraction intensities determined at the three locations is defined as the X-ray diffraction intensity of the predetermined crystal plane. The X-ray diffraction intensity of the (200) plane corresponds to the X-ray diffraction intensity at approximately 2θ = 43 to 44°, and the X-ray diffraction intensity of the (002) plane corresponds to the X-ray diffraction intensity at approximately 2θ = 30 to 40°. Examples of devices used for X-ray diffraction measurement include "SmartLab" (trade name) manufactured by Rigaku Corporation and "X'pert" (trade name) manufactured by PANalytical.
[0092] The lower limit of the ratio I(200) / I(002) is 2 or more, and may be 2.0 or more, 2.2 or more, or 2.3 or more. The upper limit of the ratio I(200) / I(002) may be, for example, 10 or less, less than 10, 5 or less, or 3 or less. The ratio I(200) / I(002) may be 2 or more and 10 or less, or 2 or more and 5 or less.
[0093] The half-width of the peak derived from the (002) plane being 2 degrees or more means that hexagonal crystals are finely dispersed in the second layer, improving hardness and toughness. The lower limit of the half-width of the peak derived from the (002) plane is 2 degrees or more, and may be 2.0 degrees or more, or 2.2 degrees or more. The upper limit of the half-width of the peak derived from the (002) plane may be 4 degrees or less, or may be 3 degrees or less. The lower limit of the half-width of the peak derived from the (002) plane may be 2 degrees or more, or may be 2.2 degrees or more, or may be 2.4 degrees or more. The half-width of the peak derived from the (002) plane may be 2 degrees or more and 4 degrees or less, or may be 2 degrees or more and 3 degrees or less.
[0094] [Embodiment 2: Manufacturing Method of Cutting Tool] In Embodiment 2, a method of manufacturing the cutting tool of Embodiment 1 will be described. The manufacturing method of Embodiment 2 can include a step of preparing a substrate and a step of forming a coating on the substrate. Details of each step will be described below.
[0095] <<Step of Preparing a Substrate>> In the step of preparing a substrate, a substrate 10 is prepared. The substrate 10 may be the substrate described in the first embodiment.
[0096] <<Coating Forming Step>> In the coating forming step, the coating 20 is formed on the substrate 10. In the second embodiment, the coating 20 can be formed by a physical vapor deposition (PVD) method. Specific examples of the PVD method include an arc ion plating (AIP) method, a balanced magnetron sputtering (BMS) method, and an unbalanced magnetron sputtering (UBMS) method. In the second embodiment, it is preferable to use arc ion plating.
[0097] In the AIP method, an arc discharge is generated using a target material as a cathode. This vaporizes and ionizes the target material. The ions are then deposited on the surface of the substrate 10 to which a negative bias voltage is applied. The AIP method is excellent in terms of the ionization rate of the target material.
[0098] A film formation apparatus used in the AIP method will be described with reference to Figures 2 and 3. As shown in Figure 2, the film formation apparatus 200 includes a chamber 201. The chamber 201 is provided with a gas inlet 202 for introducing a source gas into the chamber 201 and a gas outlet 203 for discharging the source gas from the chamber 201 to the outside. The gas outlet 203 is connected to a vacuum pump (not shown). The pressure inside the chamber 201 is adjusted by adjusting the amount of gas introduced and discharged.
[0099] A rotary table 204 is disposed within the chamber 201. A substrate holder 205 for holding the substrate 10 is attached to the rotary table 204. The substrate holder 205 is connected to the negative terminal of a bias power supply 206. The positive terminal of the bias power supply 206 is grounded.
[0100] As shown in Fig. 3, a plurality of targets 211, 212, 213, and 214 are attached to the side wall of the chamber 201. As shown in Fig. 2, each of the targets 211 and 212 is connected to the negative pole of a DC power supply 221 or 222, respectively. The DC power supplies 221 and 222 are variable power supplies, and their positive poles are earthed. Although not shown in Fig. 2, the same applies to the targets 213 and 214. A specific operation will be described below.
[0101] The substrate 10 is held by the substrate holder 205. The pressure in the chamber 201 is reduced to 1.0×10 using a vacuum pump. -4 While the turntable 204 is being rotated, the temperature of the substrate 10 is adjusted to 500° C. by a heater (not shown) attached to the film forming apparatus 200 .
[0102] Ar gas is introduced from the gas inlet 202, and the pressure inside the chamber 201 is adjusted to 3.0 Pa. While maintaining this pressure, the voltage of the bias power supply 206 is gradually changed and finally adjusted to −1000 V. Then, the surface of the substrate 10 is cleaned by ion bombardment treatment using Ar ions.
[0103] Next, if the coating film includes an underlayer, the underlayer is formed on the surface of the substrate 10. For example, a TiCN layer, a TiN layer, or a TiCNO layer is formed on the surface of the substrate 10.
[0104] Next, a second layer is formed on the surface of the substrate 10 or the surface of the underlayer. The composition of each target material is selected to obtain the compositions of the third and fourth unit layers. Each target material is set in a predetermined position, nitrogen gas is introduced through the gas inlet 202, and the second layer is formed while rotating the turntable 204. When forming the second layer, the substrate is maintained at a temperature of 400 to 800°C, the reaction gas pressure is maintained at 1 to 10 Pa (nitrogen gas partial pressure is 5 to 10 Pa), and an arc current of 80 to 200 A is alternately supplied to the evaporation source for forming the third unit layer and the evaporation source for forming the fourth unit layer while gradually changing the voltage of the bias power supply within a range of 30 to 200 V (DC power supply). This generates metal ions from the evaporation source for forming the third unit layer and the evaporation source for forming the fourth unit layer. When the substrate faces the evaporation source for forming the third unit layer, the third unit layer is formed, and when the substrate faces the evaporation source for forming the fourth unit layer, the fourth unit layer is formed. Furthermore, by depositing the film while changing the voltage of the bias power supply as described above, it is possible to achieve both high hardness and cutting edge quality for the second layer. The supply of arc current is stopped after a predetermined time has elapsed. When the second layer is formed, the thickness of each of the third unit layer and the fourth unit layer is adjusted by adjusting the rotation speed of the substrate. Furthermore, the thickness of the second layer is adjusted to be within a predetermined range by adjusting the deposition time. In addition to the part involved in cutting (e.g., the rake face near the cutting edge), the second layer may also be formed on the surface of the substrate other than the part involved in cutting.
[0105] In one aspect of this embodiment, the substrate may be maintained at a temperature of 500 to 600°C, the reactive gas pressure may be maintained at 5 to 10 Pa (nitrogen gas partial pressure: 5 to 8 Pa), and an arc current of 80 to 120 A may be alternately supplied to the evaporation source for forming the third unit layer and the evaporation source for forming the fourth unit layer while gradually changing the voltage of the bias power supply within a range of 30 to 200 V (DC power supply). In this manner, it is possible to form a mixed crystal structure of cubic and hexagonal crystals in the second layer. By forming such a mixed crystal structure, coarsening of the cubic and hexagonal crystal grains is suppressed, thereby improving the toughness and heat resistance of the second layer.
[0106] Next, the first layer is formed on the second layer. The composition of each target material is selected so as to obtain the compositions of the first and second unit layers. Each target material is set in a predetermined position, and nitrogen gas is introduced from the gas inlet 202 to form the first layer while rotating the turntable 204. The conditions for forming the first layer are as follows:
[0107] <Conditions for forming the first layer> Substrate temperature: 400 to 800°C Bias voltage: -400 to -20V Arc current: 80 to 200A Reactive gas pressure: 2 to 10Pa
[0108] The substrate temperature, reaction gas pressure, bias voltage and arc current are set to constant values within the above ranges, or are varied continuously within the above ranges.
[0109] A multilayer structure in which first unit layers and second unit layers are alternately stacked can be formed by appropriately combining the following methods (A) to (D): (A) In the AIP method, a plurality of target materials (sintered alloys) with different compositions are used; (B) In the AIP method, the bias voltage applied to the substrate 10 during film formation is changed within the bias voltage range described in the above-mentioned conditions for forming the first layer; (C) In the AIP method, the gas flow rate is changed; (D) In the AIP method, the substrate 10 is rotated and its rotation period is controlled.
[0110] Next, when the coating includes a surface layer, the surface layer is formed, for example, on the surface of the first layer.
[0111] As described above, a cutting tool 100 including a substrate 10 and a coating 20 provided on the substrate 10 can be manufactured.
[0112] The present embodiment will be described in more detail with reference to examples, although the present embodiment is not limited to these examples.
[0113] Example 1 <Preparation of Cutting Tool> A cutting tool was prepared as follows, and the tool life was evaluated.
[0114] A cutting tip made of cemented carbide (model number: CNMG120408 (manufactured by Sumitomo Electric Hardmetal Corporation)) was prepared as a substrate. The cemented carbide contained WC particles (90% by mass) and Co (10% by mass). The average particle size of the WC particles was 1 to 2 μm.
[0115] A coating was formed on the substrate using a film-forming apparatus having the configuration shown in Figures 2 and 3. First, the surface of the substrate was cleaned by ion bombardment treatment with Ar ions. The specific conditions for the ion bombardment treatment were as described in embodiment 2.
[0116] Next, the target materials were set at predetermined positions in the film forming apparatus. The compositions of the target materials were adjusted so as to obtain the compositions of the first and second unit layers shown in Table 1 and the compositions of the third and fourth unit layers shown in Table 2.
[0117] A second layer was formed on the substrate. Specifically, nitrogen gas was introduced through a gas inlet, and the second layer was formed by alternately forming third and fourth unit layers while rotating the turntable. The substrate was maintained at a temperature of 550°C, the reaction gas pressure was 8 Pa (nitrogen gas partial pressure: 8 Pa), and an arc current of 90 A was alternately supplied to the evaporation source for forming the third unit layer and the evaporation source for forming the fourth unit layer while gradually changing the voltage of the bias power supply within a range of 35 to 180 V. The thickness and number of layers of the third and fourth unit layers were adjusted by the rotation speed of the substrate.
[0118] Next, the first layer was formed on the second layer. Specifically, nitrogen gas was introduced through the gas inlet, and the first and second unit layers were alternately formed while the turntable was rotating, thereby forming the first layer on the second layer. The conditions for forming the first layer for each sample were a substrate temperature of 400 to 800°C, a bias voltage of -400 to -20 V, an arc current of 80 to 200 A, and a reactive gas pressure of 2 to 10 Pa. The substrate temperature, reactive gas pressure, bias voltage, and arc current were either constant within the above ranges or continuously varied within the above ranges. The thickness and number of layers of each of the first and second unit layers were adjusted by the rotation speed of the substrate. Cutting tools for each sample were obtained through the above process.
[0119] <Evaluation> <Coating Structure> For each sample coating, the composition, average thickness, number of stacked layers, average thickness of the first and second layers, percentage of the number of titanium atoms relative to the total number of titanium and aluminum atoms in the first layer (shown as "(T2 / T1) x 100" in Table 1), nanoindentation hardness of the first layer (shown as "Hardness" in Table 1), ratio I(200) / I(002) of the second layer, and half-width of the peak derived from the (002) plane (shown as "(002) peak half-width" in Table 2) were measured. The measurement method for each item was as described in embodiment 1. The results are shown in Tables 1 and 2. In Table 1, the notation "1" for "Number of stacked layers" indicates that only one first or second unit layer was formed. In Table 1, the notation "-" indicates that the corresponding layer was not formed.
[0120]
[0121]
[0122] <Cutting Test> Turning was performed using the cutting tool of each sample under the following conditions, and the cutting distance was measured until the width of the chipping measured from the flank was 0.5 mm or more. The longer the cutting distance, the better the crater wear resistance and chipping resistance, and the longer the tool life. The results are shown in the "Cutting Distance" column of "Cutting Test" in Table 3.
[0123] (Cutting conditions) Workpiece: SUS316 round material Cutting speed: 200 m / min Feed rate: 0.2 mm / rev Depth of cut: 1.5 mm Wet The above cutting conditions apply to turning (high-speed cutting) of stainless steel.
[0124]
[0125] <Evaluation> Samples 1 to 15 correspond to Examples. Samples 21 to 28 correspond to Comparative Examples. It was confirmed that Samples 1 to 15 had a longer tool life than Samples 21 to 28.
[0126] Although the embodiments and examples of the present disclosure have been described above, it is intended from the beginning that the configurations of the above-described embodiments and examples may be appropriately combined or modified in various ways. The embodiments and examples disclosed herein are illustrative in all respects and should not be considered limiting. The scope of the present disclosure is defined by the claims, not the above-described embodiments and examples, and is intended to include meanings equivalent to the claims and all modifications within the scope of the claims.
[0127] 1 First unit layer, 2 Second unit layer, 3 Third unit layer, 4 Fourth unit layer, 10 Substrate, 20 Coating, 21 First layer, 22 Second layer, 24, 24a, 24b, 24c Crystal grain, 25 Crystal grain boundary, 50 Atom, 100 Cutting tool, 200 Film forming apparatus, 201 Chamber, 202 Gas inlet, 203 Gas exhaust port, 204 Rotary table, 205 Substrate holder, 206 Bias power supply, 211, 212, 213, 214 Target material, 221, 222 DC power supply
Claims
1. A cutting tool comprising a substrate and a coating provided on the substrate, the coating including a first layer and a second layer, the second layer being provided closer to the substrate than the first layer, the first layer being made of a multilayer structure in which first unit layers and second unit layers are alternately laminated, the average thickness of the first unit layers being 2 nm or more and 50 nm or less, the average thickness of the second unit layers being 2 nm or more and 50 nm or less, and the first unit layers being made of Ti. a A 1-a-b B b N, wherein 0.30≦a≦0.50 and 0<b≦0.10 are satisfied, and the second unit layer is made of Ti c A 1-c N, wherein 0.70≦c≦1.00 is satisfied, in the first layer, a percentage (T2 / T1)×100 of the number of titanium atoms T2 to a total number T1 of titanium and aluminum atoms is 60% or more, the second layer has a multilayer structure in which third unit layers and fourth unit layers are alternately laminated, the average thickness of the third unit layers is 2 nm or more and 100 nm or less, the average thickness of the fourth unit layers is 2 nm or more and 100 nm or less, and the third unit layers are composed of Ti, d A 1-d-e B e N, and the fourth unit layer is made of Ti f A 1-f-g B g N, wherein 0.25≦d<0.45, 0<e≦0.10, 0.35≦f<0.55, 0<g≦0.10, and 0.05≦f-d≦0.20 are satisfied, and in an X-ray diffraction spectrum of the second layer, a ratio I(200) / I(002) of a peak intensity I(200) originating from a (200) plane to a peak intensity I(002) originating from a (002) plane is 2 or more, and a half-width of the peak originating from the (002) plane is 2 degrees or more.
2. The cutting tool according to claim 1, wherein the nanoindentation hardness of the first layer at 25°C is 30 GPa or more.
3. A cutting tool according to claim 1 or 2, wherein the average thickness of the first layer is 1.0 μm or more and 20 μm or less.
4. A cutting tool according to any one of claims 1 to 3, wherein the average thickness of the second layer is 0.5 μm or more and 10 μm or less.
Citation Information
Patent Citations
Surface-coated cutting tool
JP2011224717A
Surface-coated cutting tool
JP2018202505A
Cutting tool for surface coating
WO2014002948A1