Cellulose molded body production method and cellulose molded body

The method of dissolving cellulose in tetraalkylammonium acetate and aprotic polar solvent solvents addresses inefficiencies and safety concerns in the viscose method by enabling controlled crystallinity and improved properties in cellulose molded products, ensuring compliance and versatility in applications.

WO2024224842A1PCT designated stage expired Publication Date: 2024-10-31FUTAMURA CHEM CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009417
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-17
Filing Date
2024-03-11
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The viscose method for producing cellulose molded products is inefficient and environmentally harmful, requiring multiple steps and safety precautions due to sulfide gas presence, and struggles to control crystallinity for specific applications like cosmetics and textiles, which can lead to non-compliance with safety standards.

Method used

A method involving dissolving cellulose in a mixed solvent containing tetraalkylammonium acetate and an aprotic polar solvent, allowing for direct formation of cellulose solutions that can be coagulated into various shapes, with adjustable crystallinity by controlling temperature and solvent concentration, eliminating the need for alkaline and acid treatments.

Benefits of technology

This approach reduces the number of processing steps, improves safety, and allows for the production of cellulose molded products with controlled crystallinity, enhancing transparency, flexibility, and dyeability, while meeting safety standards for diverse applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009417_31102024_PF_FP_ABST
    Figure JP2024009417_31102024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide: a cellulose molded body production method by which a low-crystalline cellulose molded body can be obtained by adjusting the molding conditions regardless of the xylose concentration in the constituent sugar of the cellulose material; and the cellulose molded body. [Solution] A cellulose molded body production method comprising: a cellulose dissolution step for dissolving a cellulose material in a cellulose solvent to obtain a cellulose solution; a molding step for fabricating a wet-molded body by dispensing the cellulose solution into an aqueous solution for molding having a temperature of 10-70°C and containing 20-50% of the cellulose solvent; and a drying step for drying the wet-molded body after washing, thereby obtaining a cellulose molded body.
Need to check novelty before this filing date? Find Prior Art

Description

Cellulose molding and method for producing the same

[0001] The present invention relates to a method for producing a cellulose moulded body and to a cellulose moulded body.

[0002] Cellulose is generally produced by the viscose process, in which a cellulosic material such as pulp is soaked in an alkaline solution such as sodium hydroxide to form alkali cellulose, which is then sulfurized with carbon disulfide and further dissolved in an alkaline solution to form viscose, which is then coagulated with an acid solution such as sulfuric acid. The cellulose produced in this manner is molded into an appropriate shape such as fiber, film, or sphere, depending on the shape after coagulation, and processed into various products such as paper products, clothing, and sanitary goods.

[0003] The viscose method involves many steps to prepare viscose from cellulose materials, which requires a huge amount of equipment and work time. In addition, there are challenges in improving work efficiency and reducing the environmental burden, such as exhaust gas treatment and waste liquid treatment due to the use of alkaline solutions, acid solutions, hydrogen sulfide, etc. Furthermore, because the work environment is subject to the presence of sulfur gas due to processes such as sulfurization, cleaning, and desulfurization, it is essential that workers take safety measures such as wearing protective clothing.

[0004] Therefore, a method for producing a cellulose film by directly dissolving a cellulose material without going through a process of producing viscose from the cellulose material has been proposed (see, for example, Patent Document 1). In this production method, the cellulose material is dissolved in a mixed solvent containing an ionic liquid such as an imidazolium salt and an aprotic polar solvent to form a cellulose solution, and the cellulose solution is then solidified to obtain a cellulose film. This reduces the number of steps, thereby reducing the burden on equipment and improving work efficiency, and also improves safety measures and reduces the environmental impact by eliminating work environments where sulfur gas is present.

[0005] Furthermore, a production method has been proposed in which a mixed solvent of tetrabutylammonium acetate and an aprotic polar solvent such as dimethyl sulfoxide is used instead of an ionic liquid when directly dissolving a cellulose material (see, for example, Patent Documents 2, 3, and 4). The mixed solvent used in this production method contains tetrabutylammonium acetate, which has a higher dissolution efficiency than ionic liquids and is inexpensive, and therefore can improve productivity.

[0006] However, all of the above methods for producing cellulose molded bodies by directly dissolving cellulose materials are methods for producing cellulose films. However, cellulose molded bodies can be obtained in various forms, such as fibers and spheres, in addition to films. Of the resulting molded bodies, films are mainly used for packaging, fibers are mainly used for cosmetics and textiles, and spheres (beads) are mainly used for cosmetics, etc.

[0007] Generally, cellulose molded bodies for cosmetics are required to have properties appropriate for their intended use, such as transparency and flexibility, cellulose molded bodies for textiles are required to have dyeability, and cellulose molded bodies for packaging materials are required to have transparency. In these cellulose molded bodies, the refractive index of light differs between the crystalline and amorphous parts of cellulose, so the higher the degree of crystallinity, the more diffusely reflected light there is, resulting in a decrease in transparency. On the other hand, the lower the degree of crystallinity, the better the transparency and flexibility. Furthermore, the amorphous parts are more susceptible to impregnation with dyes and chemicals, resulting in better dyeability and chemical reactivity during post-processing.

[0008] As a method for obtaining cellulose fibers with low crystallinity and good dyeability, a production method using pulp containing a high concentration of hemicellulose, whose constituent sugars are xylose and the like, as the cellulose raw material has been proposed (see, for example, Patent Document 5). However, in this production method, in order to obtain cellulose fibers with low crystallinity, it is necessary to adjust the xylose concentration in the constituent sugars of the raw material itself, making it difficult to arbitrarily adjust the degree of crystallinity.

[0009] Furthermore, since the cellulose fibers obtained by the above manufacturing method contain a high concentration of xylose as a constituent sugar, when used in sanitary products such as nonwoven gauze, they may not meet the safety standards for sanitary materials. The medical nonwoven gauze standard, which complies with JIS L 1912 (1997) for testing medical nonwoven fabrics, stipulates that the weight of the substance remaining undistilled when the nonwoven fabric is boiled in water and the resulting solution is evaporated must be 20.0 mg or less per 2 g of nonwoven fabric, a chemical requirement for distillation residue. Fibers containing a high concentration of xylose as a constituent sugar, such as the cellulose fibers obtained by the above manufacturing method, are susceptible to xylose elution in hot water, which may result in the distillation residue exceeding the standard.

[0010] Therefore, the inventors have intensively investigated a method for producing a cellulose molded body that can control the crystallinity of cellulose regardless of the xylose concentration in the constituent sugars of the raw material. As a result, they have invented a method that can obtain a low-crystalline cellulose molded body regardless of the xylose concentration in the constituent sugars of the raw material by adjusting the type, concentration, and temperature conditions of the solution used when solidifying the dissolved cellulose material.

[0011] JP 2011-184541 A JP 2015-074704 A JP 2015-093876 A JP 2016-196526 A JP 2021-517214 A

[0012] The present invention has been made in consideration of the above points, and provides a method for producing a cellulose molded body and a cellulose molded body that can obtain a low-crystalline cellulose molded body by adjusting the molding conditions regardless of the xylose concentration in the constituent sugars of the cellulose material.

[0013] That is, the first invention relates to a method for producing a cellulose molded body, characterized by comprising a cellulose dissolving step of dissolving a cellulose material in a cellulose solvent to obtain a cellulose solution, a molding step of producing a wet molded body by ejecting the cellulose solution into a molding aqueous solution at 10 to 70°C containing 20 to 50% of the cellulose solvent, and a drying step of washing the wet molded body and drying it to obtain a cellulose molded body.

[0014] A second invention relates to a method for producing a cellulose molded body according to the first invention, wherein the cellulose material is pulp containing cellulose as a main component and contains 0.1 to 20% by weight of xylose as a constituent sugar.

[0015] The third invention relates to a method for producing a cellulose molded body according to the first or second invention, wherein the cellulose solvent contains a tetraalkylammonium acetate represented by the following formula (Fi) and an aprotic polar solvent, and the content of the aprotic polar solvent is 55% by weight or more.

[0016] In the formula, R 1 , R 2 , R 3 and R 4 each independently represents an alkyl group having 3 to 6 carbon atoms.

[0017] A fourth invention relates to the method for producing a cellulose molded article according to the third invention, wherein the cellulose solvent has a Kamlet-Taft parameter hydrogen bond accepting capacity (β value) of 0.8 to 1.3.

[0018] A fifth invention relates to the method for producing a cellulose molded article according to the third invention, wherein the tetraalkylammonium acetate is tetrabutylammonium acetate.

[0019] A sixth aspect of the present invention relates to the method for producing a cellulose molded article according to the third aspect of the present invention, wherein the aprotic polar solvent has a donor number of 20 to 50.

[0020] A seventh invention relates to the method for producing a cellulose molded body according to the third invention, wherein the aprotic polar solvent is at least one selected from the group consisting of amide-based solvents, sulfoxide-based solvents, and pyridine-based solvents.

[0021] An eighth invention relates to the method for producing a cellulose molded body according to the third invention, wherein the aprotic polar solvent is at least one selected from the group consisting of N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N,N'-dimethylpropyleneurea, 1,3-dimethyl-2-imidazolidinone, tetramethylurea, tetraethylurea, pyridine, 4-methylpyridine, and derivatives thereof.

[0022] A ninth aspect of the present invention relates to the method for producing a cellulose shaped article according to the first aspect of the present invention, wherein the cellulose shaped article is in the form of any one of fibers, films, and spheres.

[0023] A tenth aspect of the present invention relates to the method for producing a cellulose shaped article according to the third aspect of the present invention, wherein the cellulose shaped article is in the form of any one of fibers, films, and spheres.

[0024] An eleventh aspect of the present invention relates to the method for producing a cellulose shaped article according to the eighth aspect of the present invention, wherein the cellulose shaped article is in the form of any one of fibers, films, and spheres.

[0025] The twelfth invention relates to a cellulose molded body obtained through a cellulose dissolving process in which a cellulose material is dissolved in a cellulose solvent to obtain a cellulose solution, a molding process in which the cellulose solution is ejected into a molding aqueous solution at 10 to 70°C containing 20 to 50% of the cellulose solvent to produce a wet molded body, and a drying process in which the wet molded body is washed and then dried, wherein the cellulose molded body has a crystallinity of 60% or less, as represented by the following formula (i):

[0026] Ic: Diffraction intensity of the crystal lattice plane of cellulose type II ((1-10) plane, peak value around 2θ = 13°) Ia1: Diffraction intensity at the point where the line connecting the diffraction intensities at 2θ = 8° and 15° intersects with the line drawn vertically from 13° Ia2: Diffraction intensity of the amorphous part (2θ = 15°)

[0027] A thirteenth aspect of the present invention relates to the twelfth aspect of the present invention, wherein the cellulose shaped article contains 0.1 to 20% by weight of xylose as a constituent sugar.

[0028] The fourteenth invention relates to a cellulose molded body according to the twelfth or thirteenth invention, wherein the cellulose solvent contains a tetraalkylammonium acetate represented by the above formula (Fi) and an aprotic polar solvent, and the content of the aprotic polar solvent is 55% by weight or more.

[0029] A fifteenth aspect of the present invention relates to the cellulose molded article of the fourteenth aspect, wherein the cellulose solvent has a hydrogen bond accepting capacity (β value) of the Kamlet-Taft parameter of 0.8 to 1.3.

[0030] A sixteenth invention relates to the cellulose molded article of the fourteenth invention, wherein the aprotic polar solvent is at least one selected from the group consisting of N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N,N'-dimethylpropyleneurea, 1,3-dimethyl-2-imidazolidinone, tetramethylurea, tetraethylurea, pyridine, 4-methylpyridine, and derivatives thereof.

[0031] The method for producing a cellulose molded body according to the first invention includes a cellulose dissolving step in which a cellulose material is dissolved in a cellulose solvent to obtain a cellulose solution, a molding step in which the cellulose solution is ejected into a molding aqueous solution at 10 to 70°C containing 20 to 50% of the cellulose solvent to produce a wet molded body, and a drying step in which the wet molded body is washed and then dried to obtain a cellulose molded body. Therefore, it is possible to provide a low-crystalline cellulose molded body by adjusting the molding conditions regardless of the xylose concentration in the constituent sugars of the cellulose material.

[0032] According to the method for manufacturing cellulose molded bodies of the second invention, in the first invention, the cellulose material is pulp whose main component is cellulose and contains 0.1 to 20% by weight of xylose as a constituent sugar, making it possible to use raw materials with high cellulose purity that have not previously been used as raw materials for low-crystalline cellulose molded bodies, and by expanding the range of raw materials to be used, it is possible to expand the uses of the resulting molded bodies.

[0033] According to the method for producing a cellulose molded body of the third invention, in the first or second invention, the cellulose solvent contains tetraalkylammonium acetate and an aprotic polar solvent, and the content of the aprotic polar solvent is 55% by weight or more.Therefore, the cellulose material can be dissolved uniformly in a short time without relying on the crystalline form of the cellulose material and without performing a pretreatment process, and the fluidity of the cellulose solution obtained by dissolving the cellulose material can be increased.

[0034] According to the method for producing a cellulose molded body of the fourth invention, in the third invention, the hydrogen bond accepting capacity (β value) of the Kamlet-Taft parameter of the cellulose solvent is 0.8 to 1.3, so that the cellulose material can be dissolved uniformly in a short time without relying on the crystalline form of the cellulose material and without performing a pretreatment process, and the fluidity of the cellulose solution obtained by dissolving the cellulose material can be increased.

[0035] According to the method for producing a cellulose molded body of the fifth invention, in the third invention, the tetraalkylammonium acetate is tetrabutylammonium acetate, so that the dissolution efficiency of the cellulose material is excellent.

[0036] According to the sixth invention, the method for producing a cellulose molded body is the same as in the third invention, in which the aprotic polar solvent has a donor number of 20 to 50, so that it has good compatibility with tetraalkylammonium acetate and the solubility of the cellulose material is good.

[0037] According to the seventh invention, the method for producing a cellulose molded body is the same as in the third invention, in which the aprotic polar solvent is at least one selected from amide-based solvents, sulfoxide-based solvents, and pyridine-based solvents, thereby providing good solubility of the cellulose material.

[0038] According to the eighth invention, in the method for producing a cellulose molded body of the third invention, the aprotic polar solvent is at least one selected from the group consisting of N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N,N'-dimethylpropyleneurea, 1,3-dimethyl-2-imidazolidinone, tetramethylurea, tetraethylurea, pyridine, 4-methylpyridine, and derivatives thereof, and therefore can be procured cheaply and easily, which is advantageous in terms of economy and mass production, etc.

[0039] According to the method for manufacturing a cellulose molded body of the ninth invention, in the first invention, the cellulose molded body is in the form of a fiber, a film, or a sphere, making it easy to manufacture the molded body and process it into a product.

[0040] According to the method for manufacturing a cellulose molded body of the tenth invention, in the third invention, the cellulose molded body is in the form of a fiber, a film, or a sphere, making it easy to manufacture the molded body and process it into a product.

[0041] According to the method for producing a cellulose molded body of the eleventh invention, in the seventh invention, the cellulose molded body is in the form of a fiber, a film, or a sphere, making it easy to produce the molded body and process it into a product.

[0042] The cellulose molded body of the twelfth invention is a cellulose molded body obtained through a cellulose dissolution process in which a cellulose material is dissolved in a cellulose solvent to obtain a cellulose solution, a molding process in which the cellulose solution is ejected into a molding aqueous solution at 10 to 70°C containing 20 to 50% of the cellulose solvent to produce a wet molded body, and a drying process in which the wet molded body is washed and then dried.Since the crystallinity of the cellulose molded body is 60% or less, it has good properties such as transparency when wet, flexibility, dyeability, and chemical reactivity in post-processing, and can be suitably used as a molding material for a wide variety of cellulose products according to their shape.

[0043] According to the cellulose molded body of the thirteenth invention, in the twelfth invention, the cellulose molded body contains 0.1 to 20% by weight of xylose as a constituent sugar, so that in addition to cellulose molded bodies with low cellulose purity, cellulose molded bodies with high cellulose purity that comply with various safety standards can also be provided.

[0044] According to the cellulose molded body of the 14th invention, in the 12th or 13th invention, the cellulose solvent contains tetraalkylammonium acetate and an aprotic polar solvent, and the content of the aprotic polar solvent is 55% by weight or more.Therefore, the cellulose material can be dissolved uniformly in a short time without relying on the crystalline form of the cellulose material and without performing a pretreatment process, and the fluidity of the cellulose solution obtained by dissolving the cellulose material is increased, improving the processability of the molded body.

[0045] According to the method for producing a cellulose molded body of the 15th invention, in the 14th invention, the hydrogen bond accepting capacity (β value) of the Kamlet-Taft parameter of the cellulose solvent is 0.8 to 1.3, so that the cellulose material can be dissolved uniformly in a short time without relying on the crystalline form of the cellulose material and without performing a pretreatment process, and the fluidity of the cellulose solution obtained by dissolving the cellulose material can be increased, resulting in good processability of the molded body.

[0046] According to the cellulose molded body of the sixteenth invention, in the fourteenth invention, the aprotic polar solvent is at least one selected from the group consisting of N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N,N'-dimethylpropyleneurea, 1,3-dimethyl-2-imidazolidinone, tetramethylurea, tetraethylurea, pyridine, 4-methylpyridine, and derivatives thereof, and therefore can be procured cheaply and easily, which is advantageous in terms of economy, mass production, etc.

[0047] 1 is a schematic process diagram of a method for producing a cellulose molded body according to one embodiment of the present invention.

[0048] The method for producing a cellulose molded body according to one embodiment of the present invention shown in Figure 1 is a method for obtaining a low-crystalline cellulose molded body regardless of the xylose concentration in the constituent sugars of the cellulose material, and includes a cellulose dissolving process, a molding process, and a drying process.

[0049] The cellulose shaped body obtained by the manufacturing method of the present invention can be molded into any suitable shape, but from the viewpoint of ease of manufacturing and product processing, it is preferable to mold it into any of the following shapes: fibrous, film-like, and spherical. In particular, fibrous cellulose shaped bodies are so-called cellulose fibers and can be widely used as materials for processed products such as nonwoven fabrics. In the following description, the cellulose shaped body will be referred to as cellulose fiber (fibrous cellulose) unless otherwise specified.

[0050] The cellulose dissolution process is a process in which a cellulose material is dissolved in a cellulose solvent to obtain a cellulose solution. Cellulose materials are materials containing cellulose components, and include natural materials such as pulp and cotton, and processed materials such as paper products. Among natural materials, pulp is easily available and is preferably used as a cellulose material. In the case of processed materials, it is preferable to reuse discarded paper products and other processed materials from the perspective of reducing environmental impact.

[0051] Pulp is a fibrous material obtained primarily by crushing wood and removing impurities. Generally, pulp used as a raw material for low-crystalline cellulose molded bodies is often pulp containing a high concentration of cellulose and xylose as a constituent sugar, obtained by removing impurities such as lignin. In the method for producing cellulose molded bodies of the present invention, pulp containing 0.1 to 20% by weight of xylose as a constituent sugar can be used as a raw material for low-crystalline cellulose molded bodies. That is, in addition to the commonly used pulp with a low cellulose purity, pulp with a high cellulose purity can also be used when producing low-crystalline cellulose molded bodies. This not only broadens the range of raw materials available, but also expands the range of uses for the resulting molded bodies.

[0052] Furthermore, when xylose is included as a constituent sugar in the cellulose solution described below, it inhibits the crystallization of cellulose when the cellulose solution solidifies, so it can also be added to arbitrarily control the crystallinity of cellulose. A cellulose molded body with a high degree of crystallinity increases rigidity and decreases transparency, while a low degree of crystallinity increases flexibility and improves transparency. Therefore, the content can be adjusted appropriately depending on the physical properties required for the desired cellulose molded body. In the following explanation, the cellulose material will be described as pulp.

[0053] The cellulose solvent is a solvent for dissolving cellulose materials such as pulp, and in particular, a solvent that can dissolve the pulp uniformly in a short time without a pretreatment step, regardless of the crystalline form of the pulp. From the viewpoint of reducing environmental impact, it is preferable that this cellulose solvent does not contain halogen as an anion. As the cellulose solvent, a solvent containing a tetraalkylammonium acetate represented by the following formula (Fi) and an aprotic polar solvent is preferably used.

[0054]

[0055] In formula (Fi), R 1 , R 2 , R 3 and R 4 is an alkyl group having 3 to 6 carbon atoms. 1 ~R 4If the number of carbon atoms in the alkyl group is 2 or less or 7 or more, the solubility of the solvent in the pulp may decrease.

[0056] The Kamlet-Taft parameter can be used as an evaluation index for the solvent properties of a cellulose solvent. The Kamlet-Taft parameters include three parameters: hydrogen bond acidity (α), hydrogen bond basicity (β), and dipolarity / polarizability (π), with the hydrogen bond basicity (β) being related to cellulose dissolving ability. The cellulose dissolving ability required in the present invention is preferably such that the Kamlet-Taft parameter hydrogen bond accepting capacity (β value) is 0.8 to 1.3. By setting the Kamlet-Taft parameter hydrogen bond accepting capacity (β value) of the cellulose solvent to 0.8 to 1.3, the cellulose material can be dissolved uniformly in a short time without a pretreatment step, regardless of the crystalline form of the cellulose material, and the fluidity of the cellulose solution obtained by dissolving the cellulose material can be increased.

[0057] Tetraalkylammonium acetate is a material for efficiently dissolving cellulosic materials such as pulp. The tetraalkylammonium acetate is one or a combination of tetrabutylammonium acetate, tetrapropylammonium acetate, tetrapentylammonium acetate, and tetrahexylammonium acetate.

[0058] Among the above tetraalkylammonium acetates, tetrabutylammonium acetate is preferably selected due to its excellent dissolution efficiency for polysaccharides. Tetrabutylammonium acetate is an ionic ammonium acetate salt having an alkyl group with four carbon atoms, and it has a well-balanced affinity for hydrogen bonds and hydrophobicity as an organic substance. This property is thought to allow it to penetrate between crystalline cellulose molecules in pulp, severing intermolecular and intramolecular hydrogen bonds, while suppressing re-aggregation due to the action of hydrophobic groups in the molecules. This allows for efficient dissolution of cellulose crystals, the main component of pulp.

[0059] The aprotic polar solvent is a solvent for dissolving a tetraalkylammonium acetate such as tetrabutylammonium acetate, which is solid at room temperature. The aprotic polar solvent not only enables uniform dissolution of the tetraalkylammonium acetate in a short time, but also reduces the viscosity of the cellulose solution obtained by dissolving the pulp, thereby appropriately adjusting the fluidity.

[0060] Furthermore, since the tetraalkylammonium acetate that constitutes the cellulose solvent has a strong electric charge, it easily bonds electrostatically with pulp, which has a large number of hydroxyl groups in its molecule, through hydrogen bonds or the like. Therefore, if a protic solvent were used, an interaction (hydrogen bond) would occur with the tetraalkylammonium acetate, preventing the tetraalkylammonium acetate from breaking the hydrogen bonds of cellulose. Therefore, an aprotic catalyst is preferred. Furthermore, since it is difficult to dissolve the tetraalkylammonium acetate when a nonpolar (non-polar) solvent is used, a polar solvent is preferred. Therefore, aprotic polar solvents are preferably used as the cellulose solvent.

[0061] The blending ratio of tetraalkylammonium acetate is 1 to 45% by weight, preferably 5 to 40% by weight, and more preferably 10 to 35% by weight, from the viewpoint of solubility in pulp, dissolution rate, etc. If the blending ratio of tetraalkylammonium acetate is too low, the pulp may not be sufficiently dissolved, whereas if the blending ratio is too high, the solubility and dissolution rate of the pulp may decrease.

[0062] The aprotic polar solvent preferably has a strong hydrogen bond acceptor property and a solubility parameter similar to that of tetraalkylammonium acetate. Therefore, the aprotic polar solvent preferably has a donor number of 20 to 50, more preferably 25 to 40, and even more preferably 25 to 35. The donor number is one index indicating the basicity of the solvent, and is used to determine the donor number when the solvent molecules react with 3 to 10 mol / L of Lewis acid (SbCl) in a 1,2-dichloroethane solution. 5The donor number is a value that represents the heat of reaction (enthalpy) when the aprotic polar solvent reacts with the tetraalkylammonium acetate, expressed as -ΔH (kcal / mol). If the donor number is too small, the hydrogen bond acceptor property of the aprotic polar solvent may decrease, resulting in a decrease in the solubility of the pulp. If the donor number is too large, the compatibility of the aprotic polar solvent with the tetraalkylammonium acetate may decrease.

[0063] Furthermore, as the aprotic polar solvent, from the viewpoint of the solubility of tetraalkylammonium acetate and pulp, at least one solvent selected from amide solvents, sulfoxide solvents, and pyridine solvents is preferably used. Specifically, at least one solvent selected from the group consisting of N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N,N'-dimethylpropyleneurea, 1,3-dimethyl-2-imidazolidinone (N,N'-dimethylethyleneurea), tetramethylurea, tetraethylurea, pyridine, 4-methylpyridine, and derivatives thereof is preferably used. These solvents are relatively inexpensive and easily procured, and are therefore preferred from the viewpoints of economy, mass production, and the like.

[0064] The donor numbers of the aprotic polar solvents listed above, as measured by the Gutmann method, are as follows: N,N-dimethylformamide: 26.6, N,N-diethylformamide: 30.9, N,N-dimethylacetamide: 27.8, N,N-diethylacetamide: 32.2, dimethylsulfoxide: 29.8, N-methyl-2-pyrrolidone: 27.3, N,N'-dimethylpropyleneurea: 29.3, 1,3-dimethyl-2-imidazolidinone: 27.8, tetramethylurea: 31.0, tetraethylurea: 28.0, pyridine: 33.1, and 4-methylpyridine: 31.5.

[0065] These aprotic polar solvents can be used alone or in combination of two or more. For example, when two or more are used in combination, at least one of them may be an aprotic polar solvent having a donor number of 20 to 50, and the other aprotic polar solvent to be combined may be an aprotic polar solvent outside this range.

[0066] The content of the aprotic polar solvent is preferably 55% by weight or more, from the viewpoint of reducing the content of tetraalkylammonium acetate in the cellulose solvent and obtaining high fluidity in the cellulose solution in which pulp is dissolved. Increasing the fluidity of the cellulose solution improves the processability of the molded body. The upper limit of the content of the aprotic polar solvent is not particularly limited as long as even a trace amount of tetraalkylammonium acetate is blended, and is not particularly limited as long as it is not 100% by weight. The upper limit of the content of the aprotic polar solvent is, for example, 90 to 99% by weight. If the content of the aprotic polar solvent is too low, the cellulose solvent may become a slurry, reducing fluidity and potentially impairing the fluidity and homogeneity of the cellulose solution in which pulp is dissolved. Furthermore, if the content is too high, the solubility of the pulp may be reduced.

[0067] In the cellulose solvent, the solubility and dissolution rate of pulp, the viscosity of the cellulose solution, etc. can be adjusted depending on the combination of the tetraalkylammonium acetate and the aprotic polar solvent used.

[0068] Here, the dissolution mechanism of pulp (cellulose) by a cellulose solvent will be explained. In the cellulose solvent, tetraalkylammonium acetate is converted into a cation (tetraalkylammonium ion: TAA) represented by the formula (Fi) by an aprotic polar solvent (dimethyl sulfoxide: DMSO in this example). + ) and anion (acetate ion: CH 3 COO - ) and the oxygen of dimethyl sulfoxide (DMSO) and tetraalkylammonium ion (TAA + ) interacts with the macrocation ([DMSO + TAA] + ) is formed.

[0069] The pulp (cellulose) in the cellulose solvent reacts with acetate ions (CH 3 COO - ) breaks the hydrogen bonds of cellulose, and acetate ions (CH 3 COO -) and form hydrogen bonds with the oxygen in the cellulose and the macrocation ([DMSO + TAA] + ) forms a weak interaction with the cellulose. As a result, it is believed that cellulose exists in the solvent in the form shown in formula (Fii) below. Therefore, it is believed that cellulose can be dissolved uniformly in a short time without a pretreatment step, regardless of the crystalline form of the cellulose.

[0070]

[0071] The cellulose solution is a solution obtained by dissolving a predetermined amount of pulp in the cellulose solvent. The pulp dissolved in the cellulose solvent is determined depending on the degree of polymerization, crystallinity, etc., but from the viewpoint of production efficiency, such as easy preparation of the cellulose solution with low burden and ease of coagulation, the amount added is preferably a concentration of approximately 3 to 15 wt% relative to the weight of the cellulose solvent. If the pulp concentration is too dilute, the time required for coagulation in the molding process described below may increase, making handling during processing and treatment difficult. If the concentration is too high, the viscosity of the cellulose solution increases, requiring a long time to dissolve the pulp and requiring a large amount of tetraalkylammonium acetate, which may be disadvantageous economically and efficiently.

[0072] When dissolving pulp in a cellulose solvent, it is preferable to use a relatively mild dissolution temperature. The lower limit of the dissolution temperature is set to a value equal to or higher than the solidification temperature of the aprotic polar solvent used, e.g., about 20°C, from the viewpoint of ensuring the fluidity of the cellulose solvent and the reactivity of the pulp with the tetraalkylammonium acetate. On the other hand, the upper limit of the dissolution temperature is set to, e.g., about 50°C, from the viewpoint of suppressing excessive reaction between the pulp and the tetraalkylammonium acetate, controlling the reaction, and reducing the equipment required for heating. Since the temperature at which the pulp is dissolved in the cellulose solvent is within a mild temperature range, work can be carried out at room temperature, or even if heating is required, a simple heating device is sufficient. Therefore, no special heating equipment is required, and equipment costs required for production can be reduced. Furthermore, evaporation of the cellulose solvent components can be suppressed, resulting in a safer working environment. While increasing the dissolution temperature can shorten the reaction time, it is not preferable to increase the dissolution temperature more than necessary due to reasons such as decomposition of the cellulose solvent and the generation of colored substances due to side reactions.

[0073] In addition, when dissolving pulp in a cellulose solvent, additives such as antioxidants, plasticizers, fillers, ultraviolet absorbers, pigments, antistatic agents, and other polymeric materials may be added to the cellulose solution as needed. The amount of additive added is determined appropriately depending on the type of additive, application, etc.

[0074] The cellulose solution is prepared by adding pulp, a cellulose solvent, and, if necessary, additives and other materials in a predetermined blending ratio, followed by appropriate stirring. For example, mechanical stirring or ultrasonic vibration is suitable for stirring the materials when the pulp content is relatively low and the cellulose solution is highly fluid. For example, a twin-screw extruder or kneader is suitable for stirring the materials when the pulp content is relatively high and the cellulose solution is highly viscous. The stirring time depends on the fluidity of the solution, but is preferably approximately 10 to 90 minutes. If the stirring time is too short, it becomes difficult to fully dissolve the pulp. Furthermore, since extending the stirring time beyond necessary does not result in improved physical properties, the stirring time is terminated within an appropriate time. Stirring the materials promotes pulp dissolution and improves solution uniformity. Pulp dissolution may also be performed in an inert gas atmosphere. This prevents a decrease in the degree of polymerization of cellulose in the pulp.

[0075] The molding step is a step of molding the cellulose solution obtained in the cellulose dissolving step into a wet molded body (fibrous wet molded body), and the wet molded body is produced by discharging the cellulose solution into a molding aqueous solution at 10 to 70° C. The wet molded body (fibrous wet molded body) is an intermediate product of the cellulose molded body (cellulose fiber) that is finally obtained.

[0076] The cellulose solution is discharged using a known discharge device that corresponds to the desired shape of the formed product. For example, a spunbond die or a meltblowing die is used to form cellulose fibers. A T-die or an inflation die is used to form a cellulose film. An atomizer or a spray dryer is used to form cellulose beads.

[0077] The aqueous forming solution is an aqueous solution containing 20 to 50% of the same cellulose solvent as used in the cellulose dissolving step, and solidifies upon contact with the cellulose solution. The materials constituting the aqueous forming solution include cellulose solvent and ion-exchanged water. If the cellulose solvent content is too low, the discharged cellulose solution will solidify quickly, and cellulose crystallization will likely proceed, resulting in an excessively high degree of crystallinity. On the other hand, if the cellulose solvent content is too high, the cellulose solution will not solidify sufficiently, making forming difficult.

[0078] The reaction conditions for the cellulose solution and the aqueous molding solution are a temperature condition of about 10 to 70°C, preferably 10 to 40°C. If the temperature of the aqueous molding solution is too high, rapid solidification may occur, resulting in a decrease in the density and strength of the cellulose molded body. In addition, the energy cost for maintaining the temperature of the aqueous molding solution will increase.

[0079] When the cellulose solution is discharged into the aqueous forming solution, it solidifies, resulting in a transparent wet product (fibrous wet product) consisting of the cellulose component and the remaining cellulose solvent. Meanwhile, the cellulose solvent components (tetraalkylammonium acetate, aprotic polar solvent) that separated from the cellulose and dissolved into the aqueous forming solution are recovered by fractional distillation or other methods. After recovery, they are filtered, purified, and otherwise reused as a cellulose solvent.

[0080] The drying step is a step in which the wet compact (fibrous wet compact) obtained in the molding step is washed and then dried to obtain a cellulose compact (fibrous cellulose). The wet compact is washed by bringing the wet compact into contact with a washing liquid such as water in an ambient temperature environment of about 20 to 30°C, thereby replacing and separating the cellulose solvent in the wet compact with the washing water. As the washing water, a solvent that has a high affinity for cellulose and does not dissolve it is preferred, and water, which is easily available, is particularly preferred. This washing is preferably performed multiple times (about twice) from the viewpoint of more reliably removing components other than cellulose from the wet compact.

[0081] The washed wet shaped body is dried appropriately to obtain a cellulose shaped body (fibrous cellulose). The drying method is not particularly limited as long as it can dry the washed wet shaped body, and may be, for example, natural drying at room temperature or drying using a drying means such as a heated roll or hot air. In addition, since this drying process does not generate exhaust gases, it is not necessary to treat exhaust gases such as sulfide gases, which are required in the viscose method.

[0082] In the method for producing cellulose molded bodies of the present invention, the cellulose solvent used to directly dissolve the cellulose material is separated from the cellulose components during the molding process as described above, and thus the cellulose solvent can be separated into water and recovered by fractional distillation of the aqueous molding solution during the treatment process, and the recovered cellulose solvent can be reused to dissolve the cellulose material. Therefore, when continuously producing cellulose molded bodies, the amount of cellulose solvent used can be reduced by only replenishing the amount that is inevitably consumed, which is economical and reduces the environmental load.

[0083] In the method for producing a cellulose molded body of the present invention, a cellulose solution containing a dissolved cellulose material is brought into contact with a molding aqueous solution in which the concentration of the cellulose solvent and the temperature of the aqueous solution have been adjusted, thereby easily forming a low-crystalline cellulose molded body. In the molding process, the cellulose solution is discharged into the molding aqueous solution by a discharge method corresponding to the desired shape, such as fiber, film, or sphere, to obtain a cellulose molded body of any shape.

[0084] The low-crystalline cellulose molded body of the present invention has excellent properties such as transparency when wet, flexibility, dyeability, and chemical reactivity in post-processing. The crystallinity of this cellulose molded body is preferably 60% or less. The crystallinity indicates the proportion of crystalline components in the cellulose molded body and affects physical properties such as transparency and strength. Since the morphology of the crystals in the molded body is not constant, the transparency of the cellulose molded body varies slightly depending on the morphology of the crystals. However, the lower the crystallinity, the more the transparency of the cellulose molded body tends to improve.

[0085] The cellulose molded article obtained by the production method of the present invention has a cellulose type II crystalline structure. Generally, natural cellulose materials such as pulp have a cellulose type I crystalline structure. On the other hand, when natural cellulose materials are mercerized or dissolved in a cellulose solvent for regeneration, the crystalline structure changes to cellulose type II. Therefore, the crystallinity can be calculated by X-ray diffraction measurement using the following formula (i). In formula (i), Ic is the diffraction intensity of the cellulose type II crystal lattice plane ((1-10) plane, peak value near 2θ = 13°), Ia1 is the diffraction intensity at the point where the line connecting the diffraction intensities at 2θ = 8° and 15° intersects with the line drawn perpendicularly from 13°, and Ia2 is the diffraction intensity of the amorphous portion (2θ = 15°).

[0086]

[0087] The cellulose molded body of the present invention has a crystallinity of 60% or less, which improves various properties such as transparency when wet, flexibility, dyeability, and chemical reactivity in post-processing. The transparency of the cellulose molded body contributes to its appearance. A highly transparent cellulose molded body has good design and aesthetic appeal, and can produce a clean-looking product through product processing. Thus, the cellulose molded body of the present invention can be molded into a high-quality material with excellent transparency in any shape. Therefore, it can be suitably used as a molding material for a wide variety of cellulose products depending on the shape of the cellulose molded body.

[0088] Furthermore, the low-crystalline cellulose molded body of the present invention contains 0.1 to 20% by weight of xylose as a constituent sugar, corresponding to the xylose concentration in the constituent sugars of the cellulose material used. This includes not only low-crystalline cellulose molded bodies obtained from ordinary raw materials with low cellulose purity, but also low-crystalline cellulose molded bodies obtained from raw materials with high cellulose purity. Cellulose molded bodies made from high-purity cellulose contain only a small amount of xylose as a constituent sugar in the molded body, so they can be made into products that comply with safety standards such as standards for distillation residues.

[0089] Thus, the cellulose molded article of the present invention has excellent appearance, such as designability and aesthetics, due to its excellent transparency resulting from low crystallinity, and is also safe because it is molded from high-purity cellulose. Therefore, products with a clean appearance can be obtained by processing, and it is useful as a molding material for a wide range of products, such as cosmetics such as face masks and medical supplies such as medical masks.

[0090] [Preparation of cellulose molded body] When preparing the cellulose molded bodies of Prototype Examples 1 to 11, 1,410 g of a cellulose solvent described below was placed in a 2 L separable flask, and 90 g of a cellulose material described below was added to the cellulose solvent. The mixture was stirred with a stirrer ("Logbone" manufactured by Kobelco Eco-Solutions Co., Ltd.) and dissolved in a water bath at 55°C to obtain a cellulose solution.

[0091] Next, aqueous solutions for molding were prepared using the same cellulose solvent as that used to dissolve the cellulose material, but with different blending ratios and aqueous solution temperatures, and the cellulose solution was discharged from a nozzle into the aqueous solution for molding using a gear pump (manufactured by Barmag; "Oerlikon") to solidify, thereby obtaining fibrous wet molded bodies. The obtained wet molded bodies were washed with running water and then air-dried to obtain fibrous cellulose molded bodies of Prototype Examples 1 to 11.

[0092] [Cellulose Solvent] A cellulose solvent was obtained by mixing 28% by weight of tetrabutylammonium acetate (manufactured by Tokyo Chemical Industry Co., Ltd.) as a tetraalkylammonium acetate and 72% by weight of dimethyl sulfoxide (manufactured by Kishida Chemical Co., Ltd.) as an aprotic polar solvent.

[0093] The Kamlet-Taft parameter hydrogen bond accepting capacity (β value) of the obtained cellulose solvent was 1.1. The Kamlet-Taft parameter hydrogen bond accepting capacity (β value) was measured with reference to "Lauri K. J. Hauru et al., Biomacromolecules 2012, 13, 2896-2905".

[0094] [Cellulose materials] Pulp 1: Dissolving pulp (manufactured by Oji Paper Co., Ltd.; "LDKP"), xylose concentration in constituent sugars: 1.9% Pulp 2: Dissolving pulp (manufactured by Nippon Paper Industries Co., Ltd.; "LBKP"), xylose concentration in constituent sugars: 17.1% Pulp 3: Cotton linter pulp (manufactured by Buckeye), xylose concentration in constituent sugars: 0.3%

[0095] [Prototype Example 1] Prototype Example 1 is a fibrous cellulose molding obtained by solidifying a cellulose solution of Pulp 1 (xylose concentration in the constituent sugars: 1.9%) with a molding aqueous solution having a concentration of 20% and an aqueous solution temperature of 10°C.

[0096] [Prototype Example 2] Prototype Example 2 is a fibrous cellulose molding obtained by solidifying a cellulose solution of Pulp 2 (xylose concentration in the constituent sugars: 17.1%) with a molding aqueous solution having a concentration of 20% and an aqueous solution temperature of 20°C.

[0097] [Prototype Example 3] Prototype Example 3 is a fibrous cellulose molding obtained by solidifying a cellulose solution of Pulp 1 (xylose concentration in constituent sugars: 1.9%) with a molding aqueous solution having a concentration of 20% and an aqueous solution temperature of 70°C.

[0098] [Prototype Example 4] Prototype Example 4 is a fibrous cellulose molding obtained by solidifying a cellulose solution of Pulp 3 (xylose concentration in constituent sugars: 0.3%) with a molding aqueous solution having a concentration of 20% and an aqueous solution temperature of 70°C.

[0099] [Prototype Example 5] Prototype Example 5 is a fibrous cellulose molding obtained by solidifying a cellulose solution of Pulp 2 (xylose concentration in constituent sugars: 17.1%) with a molding aqueous solution having a concentration of 50% and an aqueous solution temperature of 20°C.

[0100] [Prototype Example 6] Prototype Example 6 is a fibrous cellulose molding obtained by solidifying a cellulose solution of Pulp 1 (xylose concentration in constituent sugars: 1.9%) with a molding aqueous solution having a concentration of 50% and an aqueous solution temperature of 70°C.

[0101] [Prototype Example 7] Prototype Example 7 is a fibrous cellulose molding obtained by solidifying a cellulose solution of Pulp 1 (xylose concentration in the constituent sugars: 1.9%) with a molding aqueous solution having a concentration of 10% and an aqueous solution temperature of 10°C.

[0102] [Example 8] Example 8 is a fibrous cellulose molding obtained by solidifying a cellulose solution of Pulp 1 (xylose concentration in the constituent sugars: 1.9%) with a molding aqueous solution having a concentration of 20% and an aqueous solution temperature of 5°C.

[0103] [Prototype Example 9] Prototype Example 9 is a fibrous cellulose molding obtained by solidifying a cellulose solution of Pulp 1 (xylose concentration in the constituent sugars: 1.9%) with a molding aqueous solution having a concentration of 0% (no cellulose solvent) and an aqueous solution temperature of 5°C.

[0104] [Prototype Example 10] Prototype Example 10 is a fibrous cellulose molding obtained by solidifying a cellulose solution of Pulp 1 (xylose concentration in the constituent sugars: 1.9%) with a molding aqueous solution having a concentration of 0% (no cellulose solvent) and an aqueous solution temperature of 10°C.

[0105] [Prototype Example 11] Prototype Example 11 is a fibrous cellulose molding obtained by solidifying a cellulose solution of Pulp 1 (xylose concentration in the constituent sugars: 1.9%) with a molding aqueous solution having a concentration of 0% (no cellulose solvent) and an aqueous solution temperature of 20°C.

[0106] The xylose concentration in the sugar components, the degree of crystallinity, and the transparency when wet were tested and evaluated for the fibrous cellulose molded bodies of Prototype Examples 1 to 11. The test results for the xylose concentration in the sugar components of the cellulose material, the concentration of the cellulose solvent in the aqueous solution for molding, and the temperature of the aqueous solution, as well as the xylose concentration in the sugar components of the molded bodies, the degree of crystallinity, and the transparency are shown in Table 1 below.

[0107] [Measurement of xylose concentration in constituent sugars] The fibrous cellulose bodies of Examples 1 to 11 were dissolved in 72 wt% sulfuric acid in a 30°C water bath. Water was added to dilute the sulfuric acid to 4.5 wt%, and the solution was treated in a 120°C oil bath for 15 minutes to hydrolyze the sugar components in the cellulose bodies into monosaccharides. The xylose concentration (%) in the hydrolyzate was measured using a high-performance liquid chromatograph (HPLC) (Shimadzu Corporation; "Prominence"). A ligand exchange chromatography column (Shoko Science Co., Ltd.; "SUGAR SP0810") was used to separate the sugars.

[0108] The crystallinity (%) of cellulose was calculated using the formula (i) above by wide-angle X-ray diffraction (WAXD) measurement using a fully automated multipurpose X-ray diffractometer (Rigaku Corporation; "SmartLab") under the conditions of a measurement angle 2θ of 5 to 40°, a voltage of 40 kV, and a current of 30 mA.

[0109] [Test for Transparency in Wet State] For the fibrous cellulose molded bodies of Prototype Examples 1 to 11, fibers cut to a length of 50 mm were dispersed in water to form a slurry, which was then subjected to suction filtration to prepare cylindrical short fiber sheet specimens. 2 The resulting cylindrical short fiber sheet specimen was uniformly moistened by dripping ion-exchanged water over the entire surface, and the moistened specimen was placed on a sheet with black letters printed on it, and the visibility (transparency) of the letters was visually evaluated. In evaluating transparency, cases where the visibility of the letters was high (the letters were clearly visible) were evaluated as "○ (good)," and cases where the visibility was low (the letters were poorly visible) were evaluated as "× (bad)."

[0110]

[0111] [Results and Discussion] Comparing Prototypes 1, 3, and 8 (material: Pulp 1, concentration: 20%), which had the same cellulose material and cellulose solvent concentration in the aqueous molding solution, we observed a tendency for the crystallinity of the cellulose molded body to decrease as the temperature of the aqueous molding solution increased. This is thought to be because when the cellulose solution is solidified in a high-temperature aqueous solution containing a cellulose solvent, the solid precipitates from the cellulose solution quickly, and the cellulose precipitates before forming a crystal lattice, increasing the amorphous portion and decreasing the crystallinity. Furthermore, in Prototype 8, in which the temperature of the aqueous molding solution was 5°C, the visibility of the letters on the test specimen was low, and transparency was insufficient.

[0112] Comparing Prototypes 1, 7, and 10 (material: pulp 1, temperature: 10°C), 2 and 5 (material: pulp 2, temperature: 20°C), 3 and 6 (material: pulp 1, temperature: 70°C), and 8 and 9 (material: pulp 1, temperature: 5°C), which had the same cellulose material and temperature of the aqueous molding solution, it was found that the higher the cellulose solvent concentration in the aqueous molding solution, the lower the crystallinity. This is thought to be because when the cellulose solution is solidified in an aqueous solution containing a high concentration of cellulose solvent, the cellulose solvent escapes from the cellulose solution slowly, inhibiting cellulose crystallization and reducing the crystallinity. In addition, in Prototypes 9, 10, and 11, which did not contain cellulose solvent in the aqueous molding solution, the visibility of the letters on the test specimens was low and transparency was insufficient, regardless of the temperature of the aqueous molding solution. Even in Prototype 7, which had a 10% cellulose solvent concentration, transparency was also insufficient.

[0113] Comparing Prototypes 3 and 4 (concentration: 20%, temperature: 70°C), which had the same cellulose solvent concentration and temperature in the aqueous molding solution, a tendency was observed for the degree of crystallinity to decrease as the xylose concentration in the constituent sugars of the cellulose material increased. This is thought to be due to the fact that the xylose contained as a constituent sugar inhibits cellulose crystallization when the cellulose solution solidifies, resulting in a decrease in crystallinity. It was found that the manufacturing method of the present invention can be used not only with the commonly used low-purity cellulose materials, but also with high-purity cellulose materials. Furthermore, the xylose concentrations in the constituent sugars of the fibrous cellulose molded bodies of Prototypes 1 to 11 were all 0.1 to 20 wt%, which was relatively close to the xylose concentration in the constituent sugars of the raw pulp. Thus, since the xylose in the constituent sugars of the raw material was incorporated into the molded body with almost no loss during the dissolution, molding, and drying processes, it was found that the xylose concentration in the constituent sugars of the molded body depends on the xylose concentration in the constituent sugars of the raw material.

[0114] Among the cellulose molded articles of Prototypes 1 to 11, Prototypes 1 to 6 have excellent transparency and can be used appropriately as materials for cellulose products. Furthermore, since the crystallinity of Prototypes 1 to 6 is 60% or less, they also have good properties such as flexibility, dyeability, and chemical reactivity in post-processing.

[0115] Judging comprehensively from a comparison of the cellulose molded bodies of Prototype Examples 1 to 11, the conditions for the method of producing a cellulose molded body of the present invention are preferably a temperature of the aqueous molding solution of 10°C or higher and a cellulose solvent concentration of 20% or higher in the aqueous molding solution, and taking into account the cost of maintaining the temperature and the ease of solidification of the cellulose solution, it is thought that a temperature of the aqueous molding solution of about 10 to 70°C and a cellulose solvent concentration of about 20 to 50% are preferable. Furthermore, as mentioned above, the cellulose material that can be used in the production method of the present invention can be selected from a wide range of low-purity to high-purity cellulose materials, and specifically, a cellulose material with a xylose concentration of about 0.1 to 20% by weight in the constituent sugars can be selected.

[0116] As described above, according to the manufacturing method of the present invention, by appropriately adjusting the cellulose solvent concentration and temperature in the aqueous molding solution within the above-mentioned ranges, it is possible to manufacture a cellulose molded body of low crystallinity with excellent transparency from raw materials of a wide range of purity. Furthermore, since the cellulose purity of the cellulose molded body depends on the cellulose purity of the raw material, it has been difficult to obtain a molded body of high purity and low crystallinity using conventional techniques. However, by using the manufacturing method of the present invention, it is possible to mold a molded body of high purity and low crystallinity and provide a cellulose molded body that combines safety and various performances.

[0117] The method for producing cellulose molded bodies of the present invention can produce low-crystalline cellulose molded bodies with high cellulose purity in addition to conventional low-crystalline cellulose molded bodies with low cellulose purity. High-purity low-crystalline cellulose molded bodies, in particular, can provide product materials that comply with various safety tests. Furthermore, the resulting low-crystalline cellulose molded bodies have high transparency, flexibility, and dyeability, making them suitable for a wide range of uses, including cosmetics, textiles, and packaging materials. Furthermore, when the molded body is in the form of a film, it exhibits improved affinity with reactants such as laminating agents and surface coating agents, improving film performance. When the molded body is in the form of beads, it exhibits improved reactivity with hydrophobic coating agents, which are necessary when blended into foundations and other products, improving bead performance. Furthermore, the resulting cellulose molded bodies can also be used as industrial raw materials with excellent chemical reactivity.

Claims

1. A method for producing a cellulose molded body, comprising the steps of: a cellulose dissolving step of dissolving a cellulose material in a cellulose solvent to obtain a cellulose solution; a molding step of discharging the cellulose solution into an aqueous molding solution at 10 to 70°C containing 20 to 50% of the cellulose solvent to produce a wet molded body; and a drying step of washing and drying the wet molded body to obtain a cellulose molded body.

2. The method for producing a cellulose molded body according to claim 1, wherein the cellulose material is a pulp whose main component is cellulose and contains 0.1 to 20% by weight of xylose as a constituent sugar.

3. A method for producing a cellulose molded body as described in claim 1 or 2, wherein the cellulose solvent contains a tetraalkylammonium acetate represented by the following formula (Fi) and an aprotic polar solvent, and the content of the aprotic polar solvent is 55% by weight or more. In the formula, R 1 , R 2 , R 3 and R 4 each independently represents an alkyl group having 3 to 6 carbon atoms.

4. The method for producing a cellulose molded product according to claim 3, wherein the hydrogen bond accepting ability (β value) of the Kamlet-Taft parameter of the cellulose solvent is 0.8 to 1.

3.

5. The method for producing a cellulose molded article according to claim 3, wherein said tetraalkylammonium acetate is tetrabutylammonium acetate.

6. The method for producing a cellulose molded article according to claim 3, wherein the aprotic polar solvent has a donor number of 20 to 50.

7. The method for producing a cellulose molded body according to claim 3, wherein the aprotic polar solvent is at least one selected from the group consisting of amide-based solvents, sulfoxide-based solvents, and pyridine-based solvents.

8. The method for producing a cellulose molded product according to claim 3, wherein the aprotic polar solvent is at least one selected from the group consisting of N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, dimethylsulfoxide, N-methyl-2-pyrrolidone, N,N'-dimethylpropyleneurea, 1,3-dimethyl-2-imidazolidinone, tetramethylurea, tetraethylurea, pyridine, 4-methylpyridine, and derivatives thereof.

9. The method for producing a cellulose molded body according to claim 1, wherein the cellulose molded body is in the form of any one of fibers, films, and spheres.

10. The method for producing a cellulose molded body according to claim 3, wherein the cellulose molded body is in the form of any one of fibers, films, and spheres.

11. The method for producing a cellulose molded body according to claim 8, wherein the cellulose molded body is in the form of any one of fibers, films, and spheres.

12. A cellulose molded body obtained through a cellulose dissolving process in which a cellulose material is dissolved in a cellulose solvent to obtain a cellulose solution, a molding process in which the cellulose solution is discharged into an aqueous molding solution at 10 to 70°C containing 20 to 50% of the cellulose solvent to produce a wet molded body, and a drying process in which the wet molded body is washed and then dried, wherein the cellulose molded body has a crystallinity of 60% or less as represented by the following formula (i): Ic: Diffraction intensity of the crystal lattice plane of cellulose type II ((1-10) plane, peak value near 2θ = 13°) Ia1: Diffraction intensity at the intersection of a line connecting the diffraction intensities at 2θ = 8° and 15° with a line vertically dropped from 13° Ia2: Diffraction intensity of the amorphous part (2θ = 15°) 13. The cellulose shaped product according to claim 12, which contains 0.1 to 20% by weight of xylose as a constituent sugar.

14. A cellulose molded body according to claim 12 or 13, wherein the cellulose solvent contains the tetraalkylammonium acetate represented by the above formula (Fi) and an aprotic polar solvent, and the content of the aprotic polar solvent is 55% by weight or more.

15. The cellulose molded product according to claim 14, wherein the hydrogen bond accepting ability (β value) of the Kamlet-Taft parameter of the cellulose solvent is 0.8 to 1.

3.

16. The cellulose molded article according to claim 14, wherein the aprotic polar solvent is at least one selected from the group consisting of N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, dimethylsulfoxide, N-methyl-2-pyrrolidone, N,N'-dimethylpropyleneurea, 1,3-dimethyl-2-imidazolidinone, tetramethylurea, tetraethylurea, pyridine, 4-methylpyridine, and derivatives thereof.

Citation Information

Patent Citations

  • Method for producing cellulose film

    JP2011184541A

  • Method for producing heterogeneous cellulose film

    JP2015074704A

  • Method for manufacturing stretched cellulose film

    JP2015093876A

  • Method for producing self-assembled cellulose film

    JP2016196526A

  • Lyocell fibers with viscose-like properties

    JP2021517214A