Optical isolator for wavelength band of 780-820 nm

The use of a composite oxide with a high Verdet constant and a hollow NdFeB magnet in the optical isolator for the 780-820 nm wavelength band addresses the size limitations of conventional isolators, achieving compact, high-performance optical isolators with reduced losses for semiconductor laser applications.

WO2024224958A1PCT designated stage expired Publication Date: 2024-10-31SHIN ETSU CHEMICAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013700
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-03
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional optical isolators for the 780-820 nm wavelength band are too large due to the insufficient Verdet constant of terbium gallium garnet (TGG) materials, which limits miniaturization and creates layout challenges in semiconductor laser applications.

Method used

A compact optical isolator is achieved by using a Faraday rotator made from a composite oxide with a Verdet constant of 0.80 min/(Oe cm) or more, combined with a hollow neodymium-iron-boron (NdFeB) magnet, allowing for a smaller size and higher magnetic flux density, and the Faraday rotator is preferably made of ceramic materials with a terbium oxide content of 80% or more.

Benefits of technology

This configuration enables further miniaturization of optical isolators, reduces absorption and insertion loss, and enhances isolation performance, making them suitable for smaller semiconductor laser packages while maintaining high isolation and low loss characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013700_31102024_PF_FP_ABST
    Figure JP2024013700_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention pertains to an optical isolator for a wavelength band of 780-820 nm comprising a Faraday rotator (2) which is composed of a composite oxide containing, as a main component, an oxide represented by formula (A) and which has a Verdet constant of at least 0.80 min / (Oe∙cm) at a wavelength of 800 nm, and hollow magnets (7) arranged on the outer periphery of the Faraday rotator (2), the optical isolator being characterized in that: the sample length L (cm) of the Faraday rotator (2) is within the range of [expression 1]; and the magnetic flux density B (Oe) applied to the Faraday rotator (2) is within the range of [expression 2]. Formula (A): (TbxR1-x)2O3 In formula (A), x satisfies 0.8≤x≤1.0, and R includes at least one element selected from the set consisting of lanthanoid element groups other than scandium, yttrium, and terbium (Tb). [Expression 1]: 0.8≤L≤1.1 [Expression 2]: B≤0.4×104
Need to check novelty before this filing date? Find Prior Art

Description

Optical isolator for the 780-820 nm wavelength band

[0001] The present invention relates to an optical isolator for use in the 780-820 nm wavelength band.

[0002] Semiconductor lasers are the main industrial lasers used in optical recording, medical, and optical measurement applications. Traditionally, compact semiconductor lasers with a wavelength of 780 nm have been used for optical recording on CDs, pulsed semiconductor lasers in the 800 nm band have been used for bioimaging using two-photon fluorescence microscopy or second-harmonic generation microscopy to visualize biomolecules, and semiconductor lasers in the infrared wavelength range of 780-800 nm have been used for laser length measuring instruments with positioning accuracy of a few nanometers to a few picometers.

[0003] A typical example of this type of semiconductor laser is the Fabry-Perot laser diode. The principle of laser oscillation is to utilize a resonator with two opposing reflective surfaces formed by cleaving a crystal at both ends of the path through which light passes, and to emit a laser when stimulated emission becomes stronger than light absorption. While these resonator structures are very simple and have the advantage of allowing for the miniaturization of laser packages, there is a risk that when the emitted laser light is incident on the coupling end face of an optical fiber or the like, a portion of it may be reflected and become return light. If this return light is guided into the resonator, it interferes with the laser light that is originally output, causing the problem of unstable laser output.

[0004] Therefore, for stable operation of the semiconductor laser, it is essential to place an optical isolator between the light source and the workpiece, which has the function of transmitting forward light and blocking backward light, in order to prevent reflected light from returning to the light emitting element, which is the light source, and to block light that is reflected from the optical fiber and returns to the light emitting element.

[0005] To function as an optical isolator, a Faraday rotation angle of approximately 45° is required. Specifically, light incident on an optical isolator has its polarization plane rotated by 45° by a Faraday rotator and is transmitted through the angle-adjusted input and output polarizers. On the other hand, the nonreciprocity of the Faraday rotator is used to rotate the polarization plane of the returning light by 45° in the opposite direction, resulting in a polarization plane orthogonal to the input polarizer at 90°, making it impossible to transmit the returning light. Optical isolators utilize this phenomenon to transmit light in only one direction and block reflected returning light.

[0006] An optical isolator with this function consists of three main components: a Faraday rotator, a pair of polarizers arranged on the light input and output sides of the Faraday rotator, and a magnet that applies a magnetic field in the light transmission direction (optical axis direction) of the Faraday rotator. In this optical isolator, when light enters the Faraday rotator, a phenomenon occurs in which the polarization plane rotates within the Faraday rotator. This phenomenon is generally known as the Faraday effect, and the angle by which the polarization plane rotates is called the Faraday rotation angle, and its magnitude θ is expressed by the following equation: θ = V × H × L, where V is the Verdet constant, a constant determined by the material of the Faraday rotator and the measurement wavelength. Furthermore, H is the magnetic flux density, and L is the length of the Faraday rotator (= sample length).

[0007] The factor that determines the size of an optical isolator is the size of the magnet that generates the magnetic flux density H. A larger magnet will have a larger magnetic flux density H, and using a smaller magnet to achieve miniaturization will reduce the magnetic flux density H. Therefore, for a Faraday rotator of the same length, it is necessary to develop a material with a larger Verdet constant.

[0008] Conventionally, the material of the Faraday rotator used in the wavelength range of 780 nm to 820 nm has been TGG (terbium gallium garnet) (chemical formula: Tb 3 Ga 5 O 12) are known. The Verdet constant of this TGG in the wavelength band of 780 nm to 820 nm is a small value of 0.25-0.29 min / (Oe cm), and even the Verdet constant of TGG single crystals actually used is approximately 0.27 min / (Oe cm) at a wavelength of 800 nm. With a Verdet constant of approximately 0.27 min / (Oe cm), an even larger magnet with an outer diameter of φ3.5 cm and a length of 2.0 cm would be required to function as an optical isolator, which would result in a larger optical isolator size, making it unsuitable as a material for a Faraday rotator. Note that 1 min represents 1 / 60 degrees.

[0009] Therefore, Patent Document 1 describes an oxide containing terbium oxide at a molar ratio of 50% or more as a material that can be used to miniaturize optical isolators. According to this description, when this oxide is used, the Verdet constant V at a wavelength of 800 nm is 0.62 min / (Oe cm) or more, and the magnetic flux density B (Oe) applied to the Faraday rotator is 0.5×10 4 Specifically, it has been shown that for an oxide with a molar ratio of 60%, a Faraday rotation angle of 45 degrees was obtained with a magnet having an inner diameter of 0.4 cm, an outer diameter of 3.5 cm, and a length of 2.0 cm, which gave a magnetic flux density of 3950 Oe (=0.395 T) for a sample length of 1.1 cm.

[0010] JP 2015-018145 A

[0011] However, in recent years, in the fields of optical recording, medical, and measurement applications using semiconductor lasers, the package size of semiconductor lasers used in the infrared wavelength band of 780-820 nm has been steadily decreasing, and optical isolators installed outside of these packages are also required to be even more compact in the same wavelength band. The Faraday rotator described in Patent Document 1 has a Verdet constant of 0.62 min / (Oe·cm) at a wavelength of 800 nm, so the magnet size requires dimensions of an outer diameter of φ3.5 cm and a length of 2.0 cm for a sample length of 1.1 cm. With these dimensions, the optical isolator would be larger than the laser package size, resulting in layout limitations for both. Therefore, a realistic outer diameter of a mountable optical isolator is φ1.7 cm or less, less than half of φ3.5 cm, and a length of 2.0 cm or less would be more suitable.

[0012] Therefore, conventional terbium oxide materials, which have a Verdet constant of 0.62 min / (Oe·cm) at a wavelength of 800 nm, are not sufficient to meet this demand.

[0013] The present invention has been made in consideration of the above circumstances, and aims to provide an even smaller optical isolator by combining a Faraday rotator with a large Faraday effect and a magnet with a small outer diameter in the wavelength band of 780-820 nm.

[0014] In order to solve the above problems, the optical isolator for the 780-820 nm wavelength band of the present invention is an optical isolator that is composed of a composite oxide containing an oxide represented by the following formula (A) as a main component, and that is composed of a Faraday rotator having a Verdet constant of 0.80 min / (Oe cm) or more at a wavelength of 800 nm, and a hollow magnet arranged on the outer periphery of the Faraday rotator, wherein the sample length L (cm) of the Faraday rotator is within the range of the following formula (1), and the magnetic flux density B (Oe) applied to the Faraday rotator is within the range of the following formula (2). (Tb x R 1-x ) 2 O 3(A) In the above formula (A), x is 0.8≦x≦1.0, and R includes at least one element selected from the group consisting of lanthanoid elements other than scandium, yttrium, and Tb (terbium). 0.8≦L≦1.1 (1) B≦0.4×10 4 (2)

[0015] In such an optical isolator, the Verdet constant is large, resulting in a high Faraday effect, which requires a small magnetic field to obtain a specified Faraday rotation angle, allowing the hollow magnet to be made smaller, thereby achieving even greater miniaturization of the optical isolator.

[0016] The oxide is preferably a ceramic.

[0017] With such oxides, a Faraday rotator with a large Verdet constant can be easily realized.

[0018] It is also preferable that the Faraday rotator has an insertion loss of 1 dB or less and an extinction ratio of 30 dB or more within the sample length L (cm).

[0019] Such a Faraday rotator can provide a high performance optical isolator with low loss and high isolation.

[0020] The hollow magnet is preferably made of a neodymium-iron-boron (NdFeB) magnet.

[0021] With such a hollow magnet, it is possible to reliably apply the magnetic flux density B to the Faraday rotator even if the magnet is small in size.

[0022] As described above, the optical isolator for the 780-820 nm wavelength band of the present invention has a large Verdet constant, resulting in a high Faraday effect. This means that a small magnetic field is required to obtain a predetermined Faraday rotation angle, allowing for a smaller magnet, thereby enabling further miniaturization of the optical isolator. It also allows for greater freedom in the spatial dimensions of the laser device incorporating the optical isolator. Furthermore, since the length can be made shorter than that of a conventional TGG Faraday rotator, this shortening reduces absorption loss and insertion loss, which is an important characteristic of an optical isolator.

[0023] FIG. 1 is a cross-sectional view showing a configuration example of an optical isolator according to the present invention; FIG. 2 is a cross-sectional view showing a configuration example of an optical isolator of Comparative Example 1; FIG. 3 is a wavelength characteristic diagram of the transmittance of the Faraday rotator (without AR coating) used in Example 1 and Comparative Example 1; and FIG. 4 is a graph showing the relationship between the sample length L (0.8 to 1.1 cm) of the Faraday rotator and the magnetic flux density T (10 4 1 is a graph showing the relationship between the magnitude of the magnetic flux density (Oe) and the magnetic flux density (Oe). FIG. 2 is a graph showing a simulation of magnetic flux density for calculating the magnet shape used in Example 1. FIG. 3 is a graph showing a simulation of magnetic flux density for calculating the magnet shape used in Comparative Example 1.

[0024] As described above, there has been a demand for further miniaturization of optical isolators for the 780-820 nm wavelength band.

[0025] The inventors have conducted extensive research and found that in the wavelength band of 780 nm to 820 nm, in order to set the magnet outer diameter to φ1.2 cm or less and the length to 2.0 cm or less, the Verdet constant must be 0.80 min / (Oe cm) or more, and if the value is less than this, the magnitude of the specified magnetic field used will be 0.4 × 10 4 (Oe) or more, and it has been found that it is difficult to further miniaturize the optical isolator.

[0026] To this end, the inventors conducted further research and developed an oxide material containing 80% or more terbium oxide in terms of molar ratio, which has a Verdet constant of 0.85 min / (Oe cm) or more at a wavelength of 800 nm. They discovered that when this material is used in a Faraday rotator, its length can be shortened to 1.1 cm or less, and that it can be mounted within the above-mentioned magnet dimensions.

[0027] Furthermore, the inventors have found that further miniaturization can be achieved by combining the oxide material having such a large Faraday effect with a hollow magnet having a large magnetic flux density, which has led to the present invention.

[0028] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited to this.

[0029] The optical isolator according to the present invention is used for laser light in the wavelength band of 780 to 820 nm. This laser includes semiconductor lasers. However, the design of the optical isolator according to the present invention can be modified to use laser light in wavelength bands other than the above.

[0030] Fig. 1 is a cross-sectional schematic diagram showing an example of the configuration of an optical isolator. In Fig. 1, an input polarizer 1, a Faraday rotator 2, and an output polarizer 3 are sequentially arranged on an optical axis 6 extending from the input side on the left to the output side on the right. On the input side, the input polarizer 1 is fixed to a polarizer holder 4, and on the output side, the output polarizer 3 is also fixed to a polarizer holder 4. The polarization directions of the input and output light are adjusted and fixed to metal holders 5, respectively.

[0031] The shape of the Faraday rotator 2 is not particularly limited, and may be a triangular prism or a quadrangular prism, but a cylindrical shape is preferable, so the following description will be given taking a cylindrical Faraday rotator 2 as an example.

[0032] A hollow magnet 7 is disposed on the outer periphery of this Faraday rotator 2. When the Faraday rotator 2 is cylindrical, the hollow magnet 7 is preferably hollow cylindrical, and the central axis of the Faraday rotator 2 and the central axis of the hollow part of the hollow magnet 7 are preferably coaxial. Furthermore, the outer diameter of the Faraday rotator 2 and the inner diameter of the hollow part of the hollow magnet 7 are preferably approximately the same, and alignment is preferably performed after the optical isolator is assembled. With this arrangement, the Faraday rotator 2 is located at the center of the hollow magnet 7.

[0033] Next, the optical isolator of the present invention has a Faraday rotator whose Verdet constant at a wavelength of 800 nm is 0.80 min / (Oe·cm) or more, and this Faraday rotator will be described.

[0034] The Faraday rotator is made of an oxide material containing 80% or more terbium oxide in terms of molar ratio, which has a Verdet constant of 0.85 min / (Oe cm) or more at a wavelength of 800 nm. Specific materials are those whose main component is an oxide represented by the following formula (A), and may also contain a sintering aid. (Tb x R 1-x ) 2 O 3 (A) In formula (A), x is 0.8≦x≦1.0, and R contains at least one element selected from the group consisting of lanthanoid elements other than scandium, yttrium, and Tb (terbium).

[0035] When such oxide crystals are used as Faraday rotators for isolators, it is preferable to mirror-finish the surface after cutting using an abrasive or the like. The abrasive is not particularly limited, but colloidal silica is an example.

[0036] The Faraday rotator may be made of any material, as long as it is made of the above-mentioned material, but ceramics can be used because ceramics can easily realize a Faraday rotator with a large Verdet constant. Hereinafter, this will be referred to as "transparent ceramics."

[0037] [Method of Manufacturing Transparent Ceramics] Transparent ceramics are manufactured using oxide powders with a desired blending ratio. A conventionally known manufacturing method can be appropriately selected and used as the method for manufacturing transparent ceramics, and is not particularly limited. Examples of methods for manufacturing transparent ceramics include a hot isostatic pressing method, a method combining a solid-state method with a press molding method, and a vacuum sintering method using mold molding, and are described in, for example, Akio Ikesue, "From Optical Single Crystals to Optical Polycrystals," Applied Physics, Vol. 75, No. 5, pp. 579-583 (2006), Takahiro Yanagiya and Hideyoshi Yagi, "Current Status and Future of Ceramic Laser Materials," Laser Research, Vol. 36, No. 9, pp. 544-548 (2008), etc.

[0038] Hereinafter, an example of a method for producing transparent ceramics using hot isostatic pressing (HIP) will be described.

[0039] (Preparation of Raw Powder) It is preferable to use a powder material of the oxide represented by the formula (A) used as a starting material that is of high purity, preferably 99.9% by weight or more, more preferably 99.99% by weight or more, and even more preferably 99.999% by weight or more. Terbium oxide is preferably Tb 2 O 3 is not limited to, but includes, but is not limited to, Tb 4 O 7 can also be used.

[0040] Transparent ceramics are produced using oxide powders with the desired blending ratio, but the shape and size of the powder particles used are not particularly limited. The method for preparing these raw material powders is also not particularly limited. Raw material powders produced by dry milling, wet milling, coprecipitation, alkoxide hydrolysis, sol-gel, hydrothermal synthesis, spray pyrolysis, or any other synthesis method can be suitably used. It is sufficient for the raw material to contain the oxide powder material as the main component, and other components may be intentionally contained as secondary components.

[0041] Here, "containing as a main component" means that the composite oxide represented by formula (A) is contained in an amount of 50% by mass or more. The content of the composite oxide represented by formula (A) is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 97% by mass or more, and particularly preferably 98% by mass or more.

[0042] Common examples of other minor components (components other than the main component) include dopants and fluxes that are doped during single crystal growth, and sintering aids that are added during ceramic production.

[0043] Examples of sintering aids include oxides of Group 4 elements such as titanium, zirconium, and hafnium, and oxides of Group 2 elements such as magnesium and calcium. Furthermore, oxides of Group 4 elements and oxides of Group 2 elements may be used simultaneously. These oxides have no absorption at wavelengths around 800 nm and are suitable for the transparent ceramics of the present invention. A predetermined amount of sintering aid may be added, preferably in an amount of more than 0.01 parts by mass and not more than 5.0 parts by mass, more preferably more than 0.03 parts by mass and not more than 3.0 parts by mass, and even more preferably more than 0.05 parts by mass and not more than 2.0 parts by mass, per 100 parts by mass of the composite oxide.

[0044] On the other hand, elements other than those mentioned above have problems such as absorption at a wavelength of around 800 nm, they do not easily dissolve in rare earth oxides and therefore do not react as sintering aids but precipitate alone, their activity is too high and the crystal grain size does not fall within the optimum range, and they gradually react with moisture over a long period of time, causing the ceramic to become hygroscopic and devitrifying, and therefore they are unsuitable as sintering aids for producing the transparent ceramics of the present invention.

[0045] Next, the obtained raw powder material is weighed out at the desired molar ratio, and then at least one of a dispersant such as ammonium polyacrylate or ammonium polycarboxylate is added as needed to make the particle size uniform, and a binder such as methyl cellulose, polyvinyl alcohol, or polyethylene glycol is added to obtain the desired molded body. Furthermore, a solvent such as water, methyl alcohol, or ethyl alcohol is used to make a slurry, which is then subjected to a general mixing and grinding process using a ball mill or the like for several to 10-odd hours. The obtained slurry is then spray-dried to obtain dry spherical bodies.

[0046] Alternatively, the materials may be mixed and pulverized in a ball mill or the like and then calcined, or may be calcined and then further pulverized. Specifically, a method in which the materials are mixed and pulverized in a ball mill or the like and then spray-dried, and the resulting mixed powder is calcined, can be exemplified.

[0047] The firing temperature and firing time are not particularly limited, but the firing temperature is preferably 600 to 1,600°C, more preferably 800 to 1,400°C, and even more preferably 800 to 1,100°C. The firing atmosphere is not particularly limited, and can be suitably selected from among air, oxygen and oxygen-containing atmospheres, argon atmospheres, nitrogen gas atmospheres, and other inert atmospheres. The firing time is also not particularly limited and may be selected appropriately depending on the moisture content of the mixed powder and the firing temperature, but is preferably 1 to 20 hours, more preferably 5 to 15 hours. When firing is performed, it is preferable to further pulverize and mix the mixture in a ball mill or the like for several to 10-odd hours after firing.

[0048] In order to sharpen the average particle size distribution of the mixed powder and further increase the purity, the powder material may be melted, recrystallized, and pulverized before being used as a raw material powder. Specifically, a raw material powder of high purity (for example, 99.9% by mass or more) is prepared, and Tb 2 O 3 :R 2 O 3These raw material powders are dissolved in a 1 mol / L aqueous nitric acid solution, mixed with a 1 mol / L aqueous ammonium sulfate solution, and then ultrapure water is added to adjust the concentration. While stirring the resulting aqueous solution, a 0.5 mol / L aqueous ammonium hydrogen carbonate solution is added dropwise at a constant rate until the pH reaches 8, and the solution is left to stand at room temperature for several days while stirring. Thereafter, the solution is filtered, washed with ultrapure water, and dried at 150° C. for several days.

[0049] The resulting mixed powder is placed in an alumina crucible and calcined in an inert atmosphere such as a nitrogen atmosphere or an argon atmosphere at preferably 800 to 1,500°C, more preferably 1,000 to 1,400°C, and even more preferably 1,100 to 1,200°C for preferably 0.5 to 10 hours, more preferably 1 to 7 hours, and even more preferably 2 to 4 hours. The inert atmosphere is used here to prevent the valence of terbium oxide from changing.

[0050] [Manufacturing Process] The raw material powder is molded into a predetermined shape, degreased, sintered, and further processed by hot isostatic pressing (HIP) to produce a transparent complex oxide sintered body.

[0051] (Molding) In molding, a normal press molding process can be suitably used. That is, a very common press process in which the material is filled into a mold and pressurized from a certain direction, or a CIP (Cold Isostatic Press) process in which the material is sealed in a deformable waterproof container and pressurized with hydrostatic pressure can be used. The applied pressure can be adjusted appropriately while checking the relative density of the resulting molded body, and is not particularly limited. In addition, other molding methods such as slip casting can also be suitably used in the molding process. In addition, the shape to be molded is not particularly limited and can be selected appropriately depending on the equipment used, etc., and an example is molding into a cylindrical shape.

[0052] (Degreasing) A normal degreasing process can be suitably used for degreasing. That is, a temperature-raising degreasing process using a heating furnace can be performed. The temperature at this time is preferably 200 to 600°C, more preferably 250 to 400°C. The atmosphere in which degreasing is performed is not particularly limited, and air, oxygen, argon gas atmosphere, etc. can be suitably used.

[0053] (Sintering) In sintering, a general sintering process can be suitably used. That is, a heat sintering process such as a resistance heating method or an induction heating method can be suitably used. The atmosphere used in this process is not particularly limited, and various atmospheres such as air, inert gas, oxygen gas, hydrogen gas, and helium gas can be suitably used, but sintering under reduced pressure (vacuum) can be more suitably used.

[0054] The degree of vacuum during sintering was 1 x 10 -1 Pa or less, and -2 Pa or less is more preferable. Sintering conditions are preferably 1,300 to 1,800°C, more preferably 1,400 to 1,700°C, and even more preferably 1,400 to 1,600°C. The sintering time is preferably 1 to 50 hours, more preferably 2 to 25 hours, and even more preferably 5 to 20 hours. In this case, the temperature rise rate is preferably 100 to 500°C / hr, more preferably 200 to 400°C / hr, and even more preferably 250 to 350°C / hr up to about 1,200°C, and at temperatures above that, the temperature rise rate is preferably slowed down, more preferably 20 to 100°C / hr.

[0055] (Processing by hot isostatic pressing (HIP)) After the sintering, a post-process such as hot isostatic pressing (HIP) is carried out to further increase transparency. In particular, in the case of a transparent complex oxide sintered body that does not exhibit translucency even after the sintering process is completed, it is preferable to carry out the HIP process to remove bubbles in the sintered body and make it easier to obtain translucency.

[0056] The treatment temperature is preferably higher than the sintering temperature, and is preferably 1,300°C or higher. Furthermore, the treatment temperature in the HIP treatment is preferably 1,800°C or lower, more preferably 1,700°C or lower, since the occurrence of grain growth during the HIP treatment makes it difficult to remove bubbles. The treatment pressure is preferably 196 MPa or lower, which is convenient and allows treatment with a commercially available HIP apparatus. The treatment time is not particularly limited, but is preferably 50 hours or lower, more preferably 25 hours or lower, and even more preferably 10 hours or lower. Furthermore, it is preferably 15 minutes or longer, more preferably 30 minutes or longer, and even more preferably 1 hour or longer. The type of pressurized gas medium in this case is an inert gas such as argon, or Ar—O 2 can be suitably used.

[0057] (Processing) When the obtained transparent body is used for optical purposes, both end faces on the optically used axis are optically polished to a length L (cm). At this time, the flatness is preferably λ / 2 or less, and particularly preferably λ / 8 or less, when λ = 633 nm. It is also possible to further reduce optical loss by appropriately forming an anti-reflection film on the optically polished surface.

[0058] In the present invention, the Verdet constant is not particularly limited as long as it is 0.80 min / (Oe cm) or more, but the upper limit is the Verdet constant at a terbium oxide content of 100%. If the Verdet constant is less than 0.80 min / (Oe cm), the magnet size required to set the Faraday rotation angle to 45° becomes large, making it difficult to miniaturize the optical isolator.

[0059] The Verdet constant may be measured according to a standard method, and is not particularly limited. Specifically, an oxide having a predetermined thickness is cut out, mirror-polished, and attached to a permanent magnet having a known magnetic flux density as a Faraday rotator, and the Verdet constant is measured at a wavelength of 800 nm in air at a temperature of 25±10°C.

[0060] Table 1 shows the (Tb x R 1-x ) 2 O 3 Specific examples of the composition and the value of the Verdet constant at a wavelength of 800 nm are shown below.

[0061]

[0062] As can be seen from Table 1, in the three composition examples, when x = 0.8 and 1.0, the Verdet constant is 0.85 to 1.05 min / (Oe cm), and all of them satisfy the condition of 0.80 min / (Oe cm) or more. The upper limit of the Verdet constant is not particularly limited, but can be, for example, 1.20 min / (Oe cm) or less.

[0063] Furthermore, the length (sample length) L (cm) of the Faraday rotator of the present invention and the magnetic flux density B (Oe) of the mounted magnet satisfy the following formulas (1) and (2): 0.8≦L≦1.1 (1) B≦0.4×10 4 (2) If the length of the Faraday rotator is less than 0.8 cm, the magnetic flux density required to obtain a Faraday rotation angle of 45 degrees is 0.4 × 10 4 Oe, the external size of the magnet becomes larger, making miniaturization difficult. Furthermore, if the sample length of the Faraday rotator exceeds 1.1 cm, the applied magnetic flux density becomes extremely small, but conversely, the magnet becomes longer and the isolator length also becomes longer, again making it difficult to further miniaturize the isolator.

[0064] The Faraday rotator of the present invention preferably has an insertion loss of 1 dB or less and an extinction ratio of 30 dB or more at a sample length L (cm) that satisfies the above formula. Furthermore, it is preferable that the sample length L is within the range that satisfies the above formula, since this makes it possible to fabricate an optical isolator with low loss and high isolation optical characteristics. Optical characteristics such as insertion loss and extinction ratio are measured in accordance with a standard method under measurement conditions of 25±10°C in air at a wavelength of 800 nm. The lower limit of the insertion loss is not particularly limited, but can be, for example, 0.01 dB or more. The upper limit of the extinction ratio is not particularly limited, but can be, for example, 50 dB or less.

[0065] Furthermore, the Faraday rotator of the present invention preferably has a total light transmittance (total light transmittance) of 78% or more, more preferably 80% or more, at a wavelength of 800 nm and a sample length L cm in the range of 0.8≦L≦1.1. The higher the total transmittance, the more preferable it is, but the upper limit is not particularly limited, and is 100% or less.

[0066] Such total light transmittance was measured using a V-670 UV-visible spectrophotometer manufactured by JASCO Corporation. Light was made uniform by multiple reflection using an integrating sphere with a highly reflective material applied to the inner wall, and light scattered by turbidity in the sample was also measured based on the intensity of the captured light, and was calculated based on the following formula: The wavelength at this time was 800 nm. Total light transmittance = I / Io x 100 In the above formula, I represents the transmitted light intensity (the intensity of light transmitted through a sample with a thickness of L cm), and Io represents the incident light intensity. Note that if the transmittance of the obtained oxide is not uniform and varies depending on the measurement location, the average transmittance of 10 arbitrary points is used as the transmittance of this oxide.

[0067] Next, we will explain the hollow magnet 7 used in the optical isolator of the present invention. It is preferable that this hollow magnet 7 be as small a permanent magnet as possible, and in order to obtain a large magnetic field strength, it is preferable to use a neodymium-iron-boron (NdFeB) magnet.

[0068] Generally, to provide a higher magnetic flux density, a demagnetizing magnet configuration using multiple magnets is required, including a second hollow magnet 8 and a third hollow magnet 9, as shown in Figure 2. In this case, a yoke structure made of carbon steel is required around the magnet, resulting in a larger external size.

[0069] Therefore, in order to miniaturize the optical isolator, it is preferable to use a single hollow magnet, and the hollow magnet 7 according to the present invention is preferably configured so that the magnetic field polarity of the hollow magnet 7 is oriented in the direction of the optical axis 6, a polarizer material is provided on the outer periphery of the hollow magnet 7, and a stainless steel metal holder 5 is disposed which can be fixed by welding, as shown in Fig. 1. By using such a configuration, the magnet size can be made small and the magnetic flux density applied to the Faraday rotator 2 can be maximized.

[0070] In the basic design of the optical isolator of the present invention, it is important to reduce the outer diameter and length of the hollow magnet 7 in order to achieve compactness. Therefore, it is important to combine a Faraday rotator 2 with a large Faraday effect with a hollow magnet 7 material (magnet) with a large magnetic flux density in order to achieve even smaller size.

[0071] Furthermore, when a semiconductor laser is used in an optical isolator, optical damage to the Faraday rotator 2 caused by high-power light is a problem, and is determined by the transmittance of the Faraday rotator 2 and its length L. Therefore, in order to reduce this optical damage, it is advantageous for the Faraday rotator 2 to have a high transmittance and a short length L.

[0072] Furthermore, in the optical isolator of the present invention, it is preferable to provide two or more polarization-dependent glass polarizers on the optical axis, and this configuration makes it possible to provide a polarization-dependent optical isolator.

[0073] It is more preferable to provide two or more flat birefringent crystals and one or more 45-degree optical rotators on the optical axis 6, and this configuration can also be used to make a polarization-independent isolator. In this case, it is preferable that the optical axis of the flat birefringent crystal is approximately 45° to the optical axis 6 and that the thickness is 1.0 cm or more. For example, a rutile single crystal (TiO 2 ) is used, the thickness is 1 / 10 of the diameter of 1.0 mm, and the thickness is α-BBO crystal (BaB 2 O 4 ) can accommodate a beam diameter of up to 0.35 mm, which is about 1 / 30 of the thickness.

[0074] The embodiments of the present invention have been described above.

[0075] EXAMPLES The present invention will be specifically explained below using examples and comparative examples, but the present invention is not limited to these.

[0076] Example 1 In Example 1, an optical isolator for the 780-820 nm wavelength band was fabricated, with the configuration shown in Fig. 1. For the input polarizer 1 and output polarizer 3, absorptive glass polarizers with high transparency / extinction ratio in the 780-820 nm wavelength band were used, and an anti-reflection film with a center wavelength of 800 nm was applied to their light-transmitting surfaces. In order to prevent reflected light from the light-transmitting surfaces from returning to the incident light path, the polarizers were inserted into a metal holder 5, with the bottom surfaces of the four corners of each polarizer adhesively fixed onto a polarizer holder 4 tilted at an angle of 5 degrees.

[0077] The Faraday rotator 2 was positioned at the center of the hollow part of the hollow magnet 7 and fixed at a position that maximized the magnetic field distribution produced by the hollow magnet 7. The input polarizer 1 and output polarizer 3, arranged in the order of the incident light path, had their optical axes adjusted to maximize the isolation characteristics in accordance with the 45-degree polarization angle rotated after passing through the Faraday rotator 2, and the outer periphery joints of the polarizer holder 4 and metal holder 5 were fixed by laser welding. An anti-reflection film (not shown) with a center wavelength of 800 nm was applied to the light transmission surface of the Faraday rotator 2.

[0078] Terbium / scandium oxide, which has a Verdet constant of 0.85 min / (Oe cm) or more at a wavelength of 800 nm, was used as the material for the Faraday rotator 2, as shown in Table 1. The sample length L of the Faraday rotator 2 was set to 1.1 cm, and a hollow magnet 7 made of a neodymium-iron-boron (NdFeB) magnet was placed on the outer periphery of the Faraday rotator 2, with a SUS metal housing placed on the outside of that.

[0079] To further explain the details of the Faraday rotator 2 of Example 1, a terbium / scandium oxide ceramic containing 80% terbium oxide in terms of molar ratio was used as the specific material for the Faraday rotator 2. When the optical characteristics of this ceramic were measured at a wavelength of 800 nm, the insertion loss was 0.1 dB, the extinction ratio was 38 dB, and the Verdet constant was 0.85 min / (Oe cm). The shape of the sample measured at this time was a cylinder with an outer diameter of φ2.3 cm and a length of 1.10 cm. Figure 3 shows the wavelength transmission characteristics of this Faraday rotator 2.

[0080] FIG. 4 shows the magnetic flux density Br (T=10 4 3 and 4 show the relationship between the dielectric strength (Oe) and the sample length L (cm). Note that in FIGS. 3 and 4, the material described in Patent Document 1 is shown as a reference example.

[0081] In the case of the Faraday rotator 2 of Example 1, the sample length L is 1.10 cm, and the Verdet constant of the Faraday rotator 2 is 0.85 min / (Oe cm). Therefore, when the magnetic flux density at which the Faraday rotation angle becomes 45 degrees is calculated from the relationship in FIG. 4, it is found that the magnetic flux density is approximately 2900 [Oe] (=0.29 [T]).

[0082] In the present invention, the lower limit of the Verdet constant is 0.80 min / (Oe cm), and the material used for the Faraday rotator 2 in this case is terbium / scandium, terbium / yttrium, or terbium / lutetium oxide, which contains at least 80% terbium oxide in terms of molar ratio. Since the lower limit of the sample length L is 0.8 cm, the magnetic flux density of this oxide is calculated from the relationship in FIG. 4 to be 0.4×10 4 It can be seen that the value of [Oe] (=0.4 [T]) is the upper limit of Br. Therefore, in order to further reduce the size of the optical isolator, it is preferable that the magnetic flux density B (Oe) of the hollow magnet used in the present invention satisfies the following formula (2): B≦0.4×10 4(2) The lower limit of the magnetic flux density B (Oe) is not particularly limited, but can be set to, for example, 2000 or more.

[0083] Next, we will explain the shape of the hollow magnet that satisfies the magnetic flux density of Example 1. The shape of this hollow magnet was determined by the following magnetic field analysis. That is, the finite element method (JMAG-Designer) was selected as the magnetic field analysis method, a neodymium-iron-boron (NdFeB) magnet manufactured by Shin-Etsu Chemical Co., Ltd. was selected as the magnet material, and SUS stainless steel was selected as the material for the metal holder 5. Also, Figure 5 shows the simulation results of the magnetic flux density distribution obtained when the outer diameter of the hollow magnet is φ1.2 cm and the length (L') of the hollow magnet is used as a parameter.

[0084] 5, it was found that the hollow magnet shape showing the magnetic flux density distribution when the sample length L of Example 1 is 1.10 cm has an inner diameter of 0.3 cm, an outer diameter of 1.2 cm, and a length of 2.0 cm. Here, Z [cm] in the figure indicates the distance from the center on the optical axis 6, and the sample length L [cm] is calculated as 2 × Z. In other words, the sample length L in FIG. 5 is 1.10 cm at the position where the horizontal axis Z is 0.55 cm.

[0085] When an optical isolator was assembled at a wavelength of 800 nm, an optical isolator having optical characteristics of an insertion loss of 0.5 [dB] and an isolation of 38 [dB] was successfully fabricated.

[0086] Comparative Example 1 In Comparative Example 1, an optical isolator was fabricated using a TGG single crystal (Verdet constant 0.27 min / (Oe cm)) as the Faraday rotator. The magnetic flux density to be applied to this TGG single crystal was calculated over a sample length range of 0.80 to 1.10 cm, resulting in the results shown in FIG. 4. In particular, it can be seen that the magnetic flux density required for Comparative Example 1 at a sample length of 1.1 cm, the same as in Example 1, is approximately 9,100 [Oe] (=0.91 [T]). Therefore, in order to calculate the hollow magnet shape in the same manner as in Example 1, the outer diameter was set to φ2.5 cm, and the simulation results of the magnetic flux density distribution obtained using the length (MT) of the hollow magnet 7 shown in FIG. 2 as a parameter are shown in FIG. 6.

[0087] 6, it was found that the hollow magnet shape that satisfies the magnetic flux density in Comparative Example 1 is a demagnetizing field configuration consisting of hollow magnet 7, second hollow magnet 8, and third hollow magnet 9, with an inner diameter of 0.3 cm, an outer diameter of 2.5 cm, and a total length of 6.5 cm, including the length MT of hollow magnet 7 of 2.0 cm. Here, Z [cm] in the figure indicates the distance from the center on optical axis 6, and the sample length L [cm] is calculated as 2×Z.

[0088] Comparing the above results between Example 1 and Comparative Example 1, it was confirmed that Example 1 could achieve a size reduction of 90% or more in terms of the volume ratio calculated from the outer diameter and length of the magnets of both examples compared to the TGG optical isolator of Comparative Example 1.

[0089] Furthermore, since the Verdet constant is wavelength dependent and it is generally known that the constant decreases as the wavelength becomes longer, the Verdet constant was also evaluated at 820 nm, the upper limit wavelength in the 780-820 nm band. As a result, the Verdet constant was 0.26 min / (Oe cm) for the TGG of Comparative Example 1, while it was 0.80 min / (Oe cm) for Example 1, confirming that even at the long wavelength of 800 nm, the performance was more than three times higher.

[0090] Therefore, it was confirmed that the optical isolator of this example can be put into practical use as a sufficiently compact optical isolator having low loss and high isolation characteristics in the 780-820 nm band.

[0091] The present invention includes the following aspects: [1]: An optical isolator for the 780-820 nm wavelength band, which is composed of a composite oxide containing an oxide represented by the following formula (A) as a main component, and which is composed of a Faraday rotator having a Verdet constant of 0.80 min / (Oe cm) or more at a wavelength of 800 nm, and a hollow magnet arranged on the outer periphery of the Faraday rotator, wherein the sample length L (cm) of the Faraday rotator is within the range of the following formula (1), and the magnetic flux density B (Oe) applied to the Faraday rotator is within the range of the following formula (2). (Tb x R 1-x ) 2 O 3 (A) In the above formula (A), x is 0.8≦x≦1.0, and R includes at least one element selected from the group consisting of lanthanoid elements other than scandium, yttrium, and Tb (terbium). 0.8≦L≦1.1 (1) B≦0.4×10 4 (2) [2]: The optical isolator according to [1] above, characterized in that the oxide is a ceramic. [3]: The optical isolator according to [1] or [2] above, characterized in that the Faraday rotator has an insertion loss of 1 dB or less and an extinction ratio of 30 dB or more over the sample length L (cm). [4]: ​​The optical isolator according to any one of [1] to [3] above, characterized in that the hollow magnet is made of a neodymium-iron-boron (NdFeB) magnet.

[0092] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.

Claims

1. An optical isolator for the 780-820 nm wavelength band, comprising a composite oxide containing an oxide represented by the following formula (A) as a main component, a Faraday rotator having a Verdet constant of 0.80 min / (Oe·cm) or more at a wavelength of 800 nm, and a hollow magnet arranged on the outer periphery of the Faraday rotator, characterized in that the sample length L (cm) of the Faraday rotator is within the range of the following formula (1), and the magnetic flux density B (Oe) applied to the Faraday rotator is within the range of the following formula (2). (Tb x R 1-x ) 2 O 3 (A) In the above formula (A), x is 0.8≦x≦1.0, and R includes at least one element selected from the group consisting of lanthanoid elements other than scandium, yttrium, and Tb (terbium). 0.8≦L≦1.1 (1) B≦0.4×10 4 (2) 2. An optical isolator according to claim 1, wherein said oxide is a ceramic.

3. An optical isolator according to claim 1, wherein said Faraday rotator has an insertion loss of 1 dB or less and an extinction ratio of 30 dB or more in said sample length L (cm).

4. An optical isolator according to any one of claims 1 to 3, characterized in that the hollow magnet is made of a neodymium-iron-boron (NdFeB) magnet.

Citation Information

Patent Citations

  • Optoisolator with bandwidth of 1 mu m

    CN103364972A

  • Optical isolator

    JP2015018145A

  • One micrometer band optical isolator

    JP2016109743A

  • Optical isolator

    JP2022170038A