METHOD FOR PRODUCING β-Ga2O3 / β-Ga2O3 LAYERED PRODUCT, AND LAYERED PRODUCT OBTAINED USING SAID PRODUCTION METHOD

The liquid phase epitaxial growth method using specific solvent compositions and doping elements addresses the challenges of low crystal quality and slow growth in conventional β-Ga2O3 laminate production, achieving high crystallinity and fast growth rates for applications in power and optical devices.

WO2024225207A1PCT designated stage expired Publication Date: 2024-10-31MITSUBISHI GAS CHEM CO INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015664
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-22
Publication Date
2024-10-31

Smart Images

  • Figure JP2024015664_31102024_PF_FP_ABST
    Figure JP2024015664_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention is capable of providing a method for producing a β-Ga2O3 / β-Ga2O3 layered product, the method being characterized in that a β-Ga2O3 / β-Ga2O3 layered product is obtained by mixing and melting a combination of (1) Ga2O3 as a solute and (2) PbO or PbF2 as a solvent and any one selected from the group consisting of Bi2O3, B2O3 and V2O5 as a solvent (excluding a combination of PbO and Bi2O3), bringing the obtained molten liquid into direct contact with a β-Ga2O3 substrate, and growing a β-Ga2O3 single crystal on the β-Ga2O3 substrate using a liquid phase epitaxial growth method.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing β-Ga2O3 / β-Ga2O3 laminate and laminate obtained by said manufacturing method

[0001] The present invention is 2 O 3 / β-Ga 2 O 3 The present invention relates to a method for producing a laminate and a laminate obtained by the method.

[0002] Power devices are one of the key devices for improving power utilization efficiency to realize a low-carbon society. They are primarily used as elements in inverters that convert DC to AC power and adjust AC voltage and frequency. During this conversion, energy loss due to resistance when current flows through the device and the generation of wasted current associated with the recovery process of charge distribution within the device when the voltage applied to the device switches are unavoidable. The percentage of these losses varies depending on the power and frequency, but generally ranges from several percent to several tens of percent. While efforts have been made to improve the device structure of conventional Si-based power semiconductors, Si is approaching its physical properties, making further efficiency improvements difficult. Therefore, development of SiC and GaN as alternative power device materials is underway. SiC has a band gap of 3.3 eV, while GaN has a band gap of 3.4 eV, making them wider band gap materials than Si (1.1 eV). The wider the band gap of a material, the higher the breakdown voltage, which represents the electric field at the limit where charges are prevented from leaking into the semiconductor (avalanche breakdown), and the greater the device structure that can withstand higher voltages.

[0003] β-Ga 2 O 3 is a type of oxide semiconductor, and has been applied to transparent conductive substrates for GaN-based LEDs and solar blind ultraviolet detection elements, but in recent years it has also been attracting attention as a power device material, and it is expected to realize high-voltage and high-efficiency power semiconductors that exceed SiC and GaN. 2 O 3 The band gap of β-Ga is expected to be 4.5 to 4.9 eV, which is wider than that of SiC and GaN. 2 O 3The advantage of β-Ga is that it can be grown from a melt. However, it is difficult to grow SiC or GaN crystals from a melt, and the substrate is expensive. 2 O 3 has a melting point at atmospheric pressure, allowing for bulk crystal growth, and research and development is underway using the Edge-Defined Film-fed Growth (EFG) method and the vertical Bridgman method. For the former growth method, 2- to 4-inch substrates are commercially available, and for the latter growth method, 4-inch substrates are under development.

[0004] β-Ga 2 O 3 To apply this to power devices, two layers of β-Ga with different residual electron concentrations are required. 2 O 3 β-Ga composed of 2 O 3 (epitaxial layer) / β-Ga 2 O 3 A (substrate) laminate is required. The thickness of the epitaxial layer needs to be several μm to 20 μm, and conventionally, vapor phase growth methods such as metal organic chemical vapor deposition (MOCVD), molecular beam epitaxy (MBE), mist CVD, and halide vapor phase epitaxy (HVPE) have been used. However, vapor phase growth methods are non-thermodynamic growth methods and have the drawbacks of low crystal quality and slow growth rate.

[0005] For example, Non-Patent Document 1 describes the growth of β-Ga on a sapphire substrate by HVPE. 2 O 3 According to this method, a sapphire substrate and β-Ga 2 O 3 Because the crystal structure of β-Ga is different, multiple rotation domains exist, and the epitaxial layer is not a single domain. Strictly speaking, the layer is not a single crystal and cannot be applied to power devices. In addition, the X-ray rocking curve half width of the epitaxial layer obtained by this method is as low as 0.5 deg (1800 arcsec), and the crystallinity is low. 2 O 3 β-Ga was grown on the substrate by HVPE method. 2 O 3The epitaxial growth of β-Ga 2 O 3 / β-Ga 2 O 3 Laminate (hereinafter simply referred to as "β-Ga 2 O 3 According to this method, a method for obtaining a β-Ga alloy is disclosed. 2 O 3 / β-Ga 2 O 3 Although a laminate can be obtained, the growth rate of the epitaxial layer is slow, at 2.7 to 6.0 μm / hr.

[0006] On the other hand, in the liquid phase growth method, crystal growth proceeds in principle at thermal equilibrium, and therefore has the advantage of being easier to produce high quality crystals than the vapor phase growth method. 2 O 3 has a high melting point of about 1970°C, and it is difficult to keep the melt surface stable near the melting point, making it difficult to grow by the Czochralski method, which is used for silicon single crystals, etc. Therefore, single crystals are grown by the EFG method or the vertical Bridgman method as mentioned above. However, the EFG method and the vertical Bridgman method do not produce β-Ga single crystals. 2 O 3 Methods for dissolving a target substance in an appropriate solvent, lowering the temperature of the resulting mixed solution to a supersaturated state, and growing the target substance from the melt include a static slow cooling method, a flux method, a floating zone method, a TSSG (Top Seeded Solution Growth) method, a solution pulling method, and a liquid phase epitaxy (LPE) method.

[0007] Patent Document 2 describes the method for growing β-Ga by LPE. 2 O 3 A method for obtaining an epitaxial layer is disclosed. According to this method, β-Ga is grown on a sapphire substrate by LPE. 2 O 3 Although single crystal layers are stacked, the substrate is sapphire, so β-Ga 2 O 3 Furthermore, the sapphire substrate has a corundum crystal structure, while the β-Ga 2O 3 has a monoclinic structure, and the crystal structure is different. Also, the lattice constants are not consistent, which causes the problem of low crystal quality.

[0008] β-Ga grown by liquid phase growth method such as LPE 2 O 3 When growing a single crystal layer, β-Ga 2 O 3 In Patent Document 2, a solvent capable of dissolving PbO or PbF is required. 2 are listed as examples of solvents, and either one is used. In order to establish a stable and reproducible single crystal growth method, it is common to maintain the melt at a temperature about 100 to 200°C higher than the melting point so that the solvent and solute are mixed uniformly. In Patent Document 2, the melt is maintained at 1100°C. The melting point of PbO is about 886°C, and that of PbF 2 The melting point of PbO or PbF is about 824°C. 2 When the temperature of the melt containing either PbO or PbF exceeds 1000°C, 2 A part of the β-Ga is evaporated, and the melt composition changes. 2 O 3 It is not suitable for growing single crystals. 2 Pb reacts with the furnace materials that make up the growth furnace, reducing the number of times the furnace materials are used, and since harmful Pb volatilizes, the growth furnace must be made airtight, which is a factor that increases costs.

[0009] As mentioned above, β-Ga is useful for power devices. 2 O 3 As a method for obtaining a laminate, β-Ga 2 O 3 β-Ga on the substrate 2 O 3 On the other hand, when using liquid phase epitaxy, which is theoretically close to thermal equilibrium growth and is expected to have high crystallinity and growth rate, the conventional melt growth method without using a solvent has the drawback of producing β-Ga. 2 O 3Furthermore, when a solvent is used, it is difficult to obtain a laminate. 2 It uses either one of the above as a solvent, has a high vapor pressure, and is stable and low-cost. 2 O 3 There was a problem in that it was difficult to grow a single crystal.

[0010] Patent No. 6744523 Patent No. 5794955

[0011] Journal of the Japanese Society for Crystal Growth Vol. 42, No. 2, (2015) P. 141-147

[0012] The present invention aims to solve at least one of the above-mentioned problems in the prior art. 2 O 3 β-Ga with high crystallinity and fast growth rate is grown on the substrate. 2 O 3 Single crystals are layered by liquid phase epitaxial growth to form β-Ga 2 O 3 / β-Ga 2 O 3 It is an object of the present invention to provide a method for manufacturing a laminate. 2 O 3 / β-Ga 2 O 3 The laminate is a β-Ga 2 O 3 On a substrate containing β-Ga 2 O 3 It means a stack of epitaxial layers including single crystals.

[0013] As a result of extensive research into solving the above problems, the present inventors have found that the above problems can be solved by the following invention. That is, the present invention is as follows: <1> (1) A solute, Ga 2 O 3 and (2) solvents PbO and PbF 2 and a solvent, Bi 2 O 3 , B 2 O 3 , and V 2 O 5and any one selected from the group consisting of PbO and Bi 2 O 3 (excluding the combination of and) are mixed and melted, and then the resulting melt is added with β-Ga 2 O 3 The substrate is directly contacted with the β-Ga by liquid phase epitaxial growth. 2 O 3 The single crystal was 2 O 3 β-Ga is grown on the substrate. 2 O 3 / β-Ga 2 O 3 β-Ga characterized by obtaining a laminate 2 O 3 / β-Ga 2 O 3 <2> The method for producing a laminate, wherein the combination of (2) is a combination of PbO as a solvent and B as a solvent. 2 O 3 and V 2 O 5 or a solvent, PbF 2 and solvent B 2 O 3 <3> The β-Ga GaN grown by liquid phase epitaxial growth is a method for producing a β-Ga GaN layer. 2 O 3 The method for producing a β-GaAs / GaAs alloy according to any one of the above items <1> to <4>, wherein the layer containing the single crystal contains 0.01 mol % to 20 mol % of a different element. <4> The method for producing a β-GaAs / GaAs alloy according to the above item <3>, wherein the different element is at least one element selected from the group consisting of Be, Mg, Ca, Sr, Ba, Ti, Zr, Hf, Fe, Co, Ni, Cu, Zn, Cd, Al, In, Si, Ge, Sn, Pb, and Bi. <5> The method for producing a β-GaAs / GaAs alloy according to any one of the above items <1> to <4>, wherein the layer containing the single crystal contains at least one element selected from the group consisting of Be, Mg, Ca, Sr, Ba, Ti, Zr, Hf, Fe, Co, Ni, Cu, Zn, Cd, Al, In, Si, Ge, Sn, Pb, and Bi. 2 O 3 / β-Ga 2 O 3 A laminate comprising β-Ga 2 O 3 β-Ga on the substrate 2 O 3β-Ga having a layer containing a single crystal 2 O 3 / β-Ga 2 O 3 <6> The β-Ga 2 O 3 The β-Ga according to <5> above, wherein the rocking curve half width in the layer containing the single crystal is 5 to 100 arcsec. 2 O 3 / β-Ga 2 O 3 <7> The β-Ga alloy according to <5> or <6> above, 2 O 3 / β-Ga 2 O 3 <8> An optical material including the β-Ga as described in <5> or <6> above. 2 O 3 / β-Ga 2 O 3 An electronic device including the laminate.

[0014] According to a preferred embodiment of the present invention, evaporation of the solvent is suppressed, and stable crystal growth with little compositional variation is possible. In addition, consumption of furnace materials is suppressed, and the growth furnace does not need to be a closed system, which enables low-cost production. Furthermore, since the crystal growth method is a liquid phase growth method, β-Ga can be grown with high crystallinity and a high growth rate. 2 O 3 The β-GaAs produced in this embodiment can be grown as a single crystal layer. 2 O 3 The laminate is made of β-Ga, which is expected to develop in the future. 2 O 3 The laminate can be used in electronic devices, particularly power devices, and is also expected to be used as an optical material.

[0015] FIG. 1 shows PbO—B 2 O 3 Fig. 2 is a schematic diagram showing an example of a general LPE growth furnace. Fig. 3 is a diagram showing an X-ray rocking curve of the (002) plane of the epitaxial layer of the laminate obtained in Example 1.

[0016] One embodiment of the present invention is a method for producing a crystalline silicon alloy comprising: (1) a solute, Ga; 2 O3 and (2) solvents PbO and PbF 2 and a solvent, Bi 2 O 3 , B 2 O 3 , and V 2 O 5 and any one selected from the group consisting of PbO and Bi 2 O 3 (Excluding the combination of and) are mixed and melted, and then β-Ga is added to the resulting melt. 2 O 3 The substrate is directly contacted with the β-Ga by liquid phase epitaxial growth. 2 O 3 The single crystal was 2 O 3 β-Ga is grown on the substrate. 2 O 3 / β-Ga 2 O 3 β-Ga characterized in that a laminate is obtained 2 O 3 / β-Ga 2 O 3 In one embodiment of the present invention, the combination of (2) above is a combination of PbO as a solvent and B 2 O 3 and V 2 O 5 and a combination of any one selected from the group consisting of PbF 2 and solvent B 2 O 3 The principle of one embodiment of the present invention will be described below. 2 O 3 (Reference: The System PbO-B2O3, J. Res. Natl. Bur. Stand., 18, 585-593, 1937, RF Geller, et al.) 2 and a solvent, Bi 2 O 3 , B 2 O 3 , and V2 O 5 A combination of PbO and any one selected from the group consisting of PbO and B forms a eutectic system, and mixing the two can lower the melting point. 2 O 3 When these are mixed, the PbO concentration is in the range of 2 to 96 mol%, and PbO + B 2 O 3 The melting point of the mixture can be made lower than the melting point of PbO alone. This means that the evaporation amount of PbO in the above PbO concentration range can be suppressed compared to PbO alone. 2 O 3 Although it has a low melting point of 450°C, it has a very high viscosity and is difficult to use as a solvent by itself. 2 O 3 It can be used as a solvent with a suitable viscosity when the concentration is in the range of 2 to 65 mol %.

[0017] PbO and B 2 O 3 When using PbO:B, the solvent composition ratio is 2 O 3 PbO:B = 35 to 98 mol %: 65 to 2 mol % is preferable, and PbO:B = 35 to 98 mol %: 65 to 2 mol % is more preferable. 2 O 3 = 50 to 90 mol %: 50 to 10 mol %. PbO and V 2 O 5 When using PbO:V, the solvent composition ratio is 2 O 5 PbO:V = 40 to 95 mol %: 60 to 5 mol %, more preferably PbO:V 2 O 5 = 45 to 80 mol %: 55 to 20 mol %. 2 and B 2 O 3 When using PbF, the solvent composition ratio is 2 : B 2 O 3 = 35 to 90 mol %: 65 to 10 mol %, more preferably PbF 2 : B 2 O 3= 60 to 80 mol %: 40 to 20 mol %. Since a single solvent increases the LPE growth temperature (temperature during epitaxial growth), the above-mentioned mixed solvent is preferable.

[0018] (1) Ga as a solute 2 O 3 and (2) solvents PbO and PbF 2 and a solvent, Bi 2 O 3 , B 2 O 3 , and V 2 O 5 and any one selected from the group consisting of PbO and Bi 2 O 3 The mixing ratio of the solute to the solvent (excluding the combination of the solute and the solvent) is preferably 5-30 mol %:95-70 mol %. More preferably, the solute concentration is 7 mol % or more and 26 mol % or less. If the solute concentration is less than 5 mol %, the crystal growth rate is slow, and if it exceeds 30 mol %, the LPE growth temperature becomes high and solvent evaporation may increase. In addition, the crystal growth rate may become too fast, which may result in a deterioration in crystal quality. In one embodiment of the present invention, β-Ga GaN formed by liquid phase epitaxial growth is 2 O 3 The growth rate of the layer containing the single crystal (epitaxial layer) is preferably 10 to 50 μm / hr, and more preferably 20 to 30 μm / hr. If the growth rate is less than 10 μm / hr, the growth rate may be slow, resulting in increased costs. If the growth rate exceeds 50 μm / hr, the crystal quality may deteriorate. Here, the growth rate can be determined from the difference in film thickness before and after LPE growth and the growth time.

[0019] In one embodiment of the present invention, Ga 2 O 3 One or more third components can be added to the solvent for the purposes of controlling the LPE growth temperature, adjusting the solvent viscosity, and doping with different elements, as long as the solubility of the solvent and the evaporation amount of the solvent combination in (2) above do not change significantly. 2 O 5 , MoO 3 , W.O. 3, Ba 2 O 3 , La 2 O 3 , Ge 2 O 3 The β-Ga in the present invention 2 O 3 The growth method of the laminate is as follows: 2 O 3 Liquid phase epitaxial growth using a substrate is most preferred.

[0020] β-Ga useful for power devices 2 O 3 In the stack, it is necessary to control the residual electron concentration in the epitaxial layer. 2 O 3 In one embodiment of the present invention, β-Ga is a trivalent oxide and generally exhibits n-type conductivity. 2 O 3 By doping a different element, it is possible to give residual electron concentration, band gap, insulating property, etc. 2 O 3 However, if MgO or ZnO is doped as a divalent impurity, the residual electrons can be reduced. 2 and SnO 2 Doping with FeO can increase the residual electron concentration. Also, doping with FeO can impart insulating properties. 2 O 3 Wider band gaps such as MgO and Al 2 O 3 The band gap can be increased by doping with ZnO or CdO to form a mixed crystal.

[0021] β-Ga grown by liquid phase epitaxial growth 2 O 3 The layer containing the single crystal preferably contains, as a hetero element, one or more elements selected from the group consisting of Be, Mg, Ca, Sr, Ba, Ti, Zr, Hf, Fe, Co, Ni, Cu, Zn, Cd, Al, In, Si, Ge, Sn, Pb, and Bi.

[0022] β-Ga grown by liquid phase epitaxial growth 2 O 3 The layer containing the single crystal preferably contains 0.01 mol% or more and 20 mol% or less of a different element. The content of the different element is more preferably 0.1 mol% or more, even more preferably 0.5 mol% or more, and even more preferably 10 mol% or less. If the doping amount of the different element is less than 0.01 mol%, the characteristics may be poorly expressed, and if it exceeds 20 mol%, crystal growth may become difficult.

[0023] β-Ga grown by liquid phase epitaxial growth 2 O 3 The layer containing the single crystal preferably contains one or more different elements selected from the group consisting of Be, Mg, Ca, Sr, Ba, Ti, Zr, Hf, Fe, Co, Ni, Cu, Zn, Cd, Al, In, Si, Ge, Sn, Pb, and Bi in an amount of 0.01 to 20 mol%, more preferably 0.1 to 20 mol%, and particularly preferably 0.5 to 10 mol%. If the doping amount of the different element is less than 0.01 mol%, the characteristics may not be fully expressed, and if it exceeds 20 mol%, crystal growth may become difficult.

[0024] FIG. 2 is a schematic diagram showing an example of a typical LPE growth furnace. Inside the LPE growth furnace, a platinum crucible 7 containing melted raw materials (melt 8) is placed on a crucible stand 9 made of mullite (a compound of aluminum oxide and silicon dioxide). Three side heaters (upper heater 1, central heater 2, and lower heater 3) are installed outside and to the sides of the platinum crucible 7 to heat and melt the raw materials in the platinum crucible 7. The heaters have independently controlled outputs, allowing for independent adjustment of the heat amount applied to the melt 8. A mullite furnace tube 11 is located between the heater and the inner wall of the furnace, and a mullite furnace cover 12 is installed above the furnace tube 11. A pulling mechanism is installed above the platinum crucible 7. An alumina pulling shaft 5 is fixed to the pulling mechanism, and a substrate holder 6 and a substrate 4 fixed by the holder are installed at the tip of the shaft. A mechanism for rotating the shaft is installed above the pulling shaft 5. A thermocouple 10 is also installed at the bottom of the crucible.

[0025] Another embodiment of the present invention is a β-Ga alloy obtained by the above-described production method. 2 O 3 / β-Ga 2 O 3 A laminate comprising β-Ga 2 O 3 β-Ga on the substrate 2 O 3 β-Ga having a layer containing a single crystal 2 O 3 / β-Ga 2 O 3 In one embodiment of the present invention, the β-Ga 2 O 3 The rocking curve half width in the layer containing the single crystal is preferably 5 to 100 arcsec, more preferably 5 to 95 arcsec, and even more preferably 5 to 90 arcsec. If it exceeds 100 arcsec, the crystallinity is low and the power device performance may be reduced. 2 O 3 / β-Ga 2 O 3The laminate is characterized by high crystallinity. In the present invention, the rocking curve half width can be measured by the method described in the Examples below.

[0026] Hereinafter, β-Ga according to one embodiment of the present invention will be described. 2 O 3 / β-Ga 2 O 3 As a method for growing a laminate, β-Ga 2 O 3 β-Ga on the substrate 2 O 3 A method for forming an epitaxial layer will be described below. The present invention is not limited to the following examples.

[0027] An example of the manufacturing method of the present invention will be described below with reference to Figure 2. A platinum crucible 7, which melts raw materials and stores them as a melt 8, is placed on a crucible stand 9. Outside and to the sides of the platinum crucible 7, three-stage side heaters (upper heater 1, central heater 2, and lower heater 3) are provided to heat and melt the raw materials in the platinum crucible 7. The heaters have their outputs independently controlled, and the amount of heat applied to the melt 8 is independently adjusted. A furnace core tube 11 is provided between the heater and the inner wall of the manufacturing furnace, and a furnace lid 12 is provided above the furnace core tube 11. A pulling mechanism is provided above the platinum crucible 7. An alumina pulling shaft 5 is fixed to the pulling mechanism, and at its tip, a substrate holder 6 and a substrate 4 (β-Ga 2 O 3 A mechanism for rotating the shaft is provided above the pulling shaft 5. Additionally, a thermocouple 10 is provided at the bottom of the crucible.

[0028] To melt the raw materials in the platinum crucible 7, the temperature of the manufacturing furnace is raised until the raw materials are melted. Preferably, the temperature is raised to 600 to 1000°C, more preferably 700 to 900°C, and the raw material melt is allowed to stand for 2 to 3 hours to homogenize. Alternatively, instead of leaving it to stand, a platinum plate may be fixed to the tip of an alumina shaft, which may be immersed in the melt, and the shaft may be rotated to stir the melt and homogenize it. β-Ga 2 O 3It is desirable that the growth of the single crystal layer proceeds only directly below the substrate. 2 O 3 As the single crystal growth progresses, the grown single crystal adheres to the substrate due to convection in the melt, resulting in a different phase with a different growth orientation, which is undesirable. Therefore, the three-stage heater is offset to adjust the temperature so that the bottom of the crucible is several degrees higher than the melt surface. After the melt temperature has stabilized, the seed crystal substrate is brought into contact with the melt surface. After the seed crystal substrate has been immersed in the melt, the temperature is kept constant or begins to decrease at a rate of 0.025 to 5°C / hr, and the desired β-Ga is deposited on the surface of the seed crystal substrate. 2 O 3 A single crystal layer is grown. During growth, the seed crystal substrate is rotated at 5 to 300 rpm by the rotation of the growth shaft, and is rotated in the opposite direction at regular intervals. After crystal growth for 30 minutes to 24 hours, the growth shaft is pulled up to separate the grown crystal from the melt, and the growth shaft is rotated at 50 to 300 rpm to separate the melt components adhering to the surface of the grown crystal. The crystal is then cooled to room temperature over 1 to 24 hours, and the desired β-Ga 2 O 3 / β-Ga 2 O 3 A laminate can be obtained.

[0029] (Example 1) In a platinum crucible 7 having an inner diameter of 75 mm, a height of 75 mm, and a thickness of 1 mm, 1100 g of PbO (purity 99.999%) and 100 g of B 2 O 3 (purity 99.99%) and 230 g of Ga 2 O 3 250 g of Ga (purity 99.999%) was added. 2 O 3 and the solvent PbO and B 2 O 3 The mixing ratio of solute:solvent is 14 mol%:86 mol%, and the solvent PbO and B 2 O 3 The mixing ratio of PbO:B 2 O 3The platinum crucible 7 containing the raw materials was placed in the LPE furnace shown in FIG. 2, and the raw materials were melted at a temperature of about 980°C. After stirring the melt for 6 hours using a platinum plate, the temperature was lowered until the temperature of the crucible bottom reached 850°C (the LPE growth temperature). β-Ga GaN crystals with a C-plane orientation and a size of 11 mm x 11 mm x 650 μm in thickness were grown by the EFG method. 2 O 3 The substrate was brought into contact with the liquid. Growth was carried out at the same temperature for 3 hours while rotating the alumina pulling shaft 5 at 60 rpm. At this time, the shaft rotation was reversed every 5 minutes. Thereafter, the pulling shaft 5 was pulled up to separate it from the melt, and the melt components were separated by rotating the pulling shaft 5 at 200 rpm. Thereafter, the substrate was cooled to room temperature to separate β-Ga. 2 O 3 / β-Ga 2 O 3 A laminate was obtained. The remaining melt components were removed with hydrochloric acid. The average thickness of the epitaxial layer was about 72 μm.

[0030] Comparative Examples 1 and 2 β-Ga was grown in the same manner as in Example 1, except that the raw material composition was changed to the composition shown in Table 1 below, and the raw material melting temperature and LPE growth temperature were changed as shown in Table 1. 2 O 3 / β-Ga 2 O 3 An attempt was made to fabricate a laminate.

[0031] Here, the β-Ga obtained in Example 1 2 O 3 / β-Ga 2 O 3 The crystallinity of the epitaxial layer of the laminate was evaluated by the half-width of the rocking curve of the (002) plane. The results are shown in Figure 3. The half-width of the rocking curve of the (002) plane was 0.016 deg (=56 arcsec). The half-width of the rocking curve was measured using an X-ray diffractometer (Spectris X'pertMRD). Using this diffractometer, 2θ, ω, χ, and φ were adjusted to obtain the β-Ga 2 O 3After adjusting the axis so that the peak of the (002) plane could be detected, measurements were made at a tube voltage of 45 kV and a tube current of 40 mA. The incident light was monochromated using four crystals of the Ge (220) plane. Other measurement conditions were as follows: Light source: Cu-Kα Wavelength: 0.15418 nm Measurement mode: ω scan (incident angle scan) ω range: β-Ga 2 O 3 The angle at which the (002) plane appears is set for each sample. ω range: 0.1 deg ω step: 0.0005 deg 2θ position: β-Ga 2 O 3 The angle at which the (002) plane appears is set for each sample. Collimator diameter: 0.5 mm. Anti-scattering slit: 1.5 mm.

[0032] Examples 2 to 11 β-Ga were prepared in the same manner as in Example 1, except that the raw material composition was changed to the composition shown in Table 1 below, and the raw material melting temperature and LPE growth temperature were changed as shown in Table 1. 2 O 3 / β-Ga 2 O 3 The epitaxial layer obtained in Example 4 was a β-Ga alloy containing 5.4 mol% Mg. 2 O 3 and MgO mixed crystal layer.

[0033]

[0034] As described above, the solute Ga 2 O 3 and solvents PbO and PbF 2 and a solvent, Bi 2 O 3 , B 2 O 3 , and V 2 O 5 and any one selected from the group consisting of PbO and Bi 2 O 3 The resulting melt was mixed with β-Ga and dissolved in water. 2 O 3By directly contacting the substrate, β-Ga 2 O 3 / β-Ga 2 O 3 As can be seen from a comparison between Examples 1 to 11 and Comparative Examples 1 and 2, PbO and PbF 2 One of the following and Bi 2 O 3 , B 2 O 3 , and V 2 O 5 Any one selected from the group consisting of (provided that PbO and Bi 2 O 3 By mixing with PbO or PbF 2 Therefore, the raw material melting temperature and β-Ga 2 O 3 The growth temperature is lower than when a single solvent is used. This means that the amount of evaporation of the solvent component can be reduced. According to this method, the amount of evaporation of the solvent is suppressed, so that stable crystal growth can be performed with less composition fluctuation, and the consumption of furnace materials can be suppressed, and the growth furnace does not need to be a closed system, making it possible to manufacture at low cost. Furthermore, as mentioned above, the present invention is a liquid phase growth method that is close to thermal equilibrium growth. Therefore, the growth rate is fast at 12 to 28 μm / hr, and as shown in Table 1 above, β-Ga by the LPE method can be grown at a rate of 12 to 28 μm / hr. 2 O 3 The rocking curve half-width of the (002) plane of the epitaxial layer was narrow at 56 to 95 arcsec, indicating high crystallinity. On the other hand, Comparative Examples 1 and 2 did not melt unless heated to over 1000°C, and the solvent volatilized at temperatures above 1000°C, making it impossible to produce a laminate.

[0035] REFERENCE SIGNS LIST 1 Upper heater 2 Central heater 3 Lower heater 4 Substrate 5 Pulling shaft (made of alumina) 6 Substrate holder 7 Platinum crucible 8 Melt in crucible 9 Crucible stand (made of mullite) 10 Crucible bottom thermocouple 11 Furnace tube (made of mullite) 12 Furnace lid (made of mullite)

Claims

1. (1) Ga, the solute 2 O 3 and (2) the solvents PbO and PbF 2 and a solvent, Bi 2 O 3 , B 2 O 3 , and V 2 O 5 A combination of any one selected from the group consisting of PbO and Bi 2 O 3 (Except for the combination of 2 O 3 The substrate is directly contacted with the β-Ga by liquid phase epitaxial growth. 2 O 3 The single crystal was 2 O 3 By growing β-Ga on the substrate, 2 O 3 / β-Ga 2 O 3 A method for obtaining a laminate of β-Ga 2 O 3 / β-Ga 2 O 3 A method for manufacturing a laminate.

2. The combination of (2) above is a mixture of PbO and B 2 O 3 and V 2 O 5 or a combination of PbF as a solvent. 2 and solvent B 2 O 3 The method of claim 1 , which is a combination of 3. The β-Ga formed by liquid phase epitaxial growth method 2 O 3 The method according to claim 1 or 2, wherein the layer containing the single crystal contains 0.01 mol % or more and 20 mol % or less of a different element.

4. The manufacturing method according to claim 3, wherein the different elements are one or more selected from the group consisting of Be, Mg, Ca, Sr, Ba, Ti, Zr, Hf, Fe, Co, Ni, Cu, Zn, Cd, Al, In, Si, Ge, Sn, Pb, and Bi.

5. β-Ga obtained by the method according to any one of claims 1 to 4. 2 O 3 / β-Ga 2 O 3 A laminate comprising β-Ga 2 O 3 β-Ga on the substrate 2 O 3 A layer including a single crystal, 2 O 3 / β-Ga 2 O 3 Laminate.

6. The β-Ga 2 O 3 The β-GaAs according to claim 5, wherein the half-width of the rocking curve in the layer containing the single crystal is 5 to 100 arcsec. 2 O 3 / β-Ga 2 O 3 Laminate.

7. The β-Ga according to claim 5 or 6. 2 O 3 / β-Ga 2 O 3 An optical material comprising a laminate.

8. The β-Ga according to claim 5 or 6. 2 O 3 / β-Ga 2 O 3 An electronic device comprising the laminate.

Citation Information

Patent Citations

  • Method for manufacturing a substrate with a β-Ga2O3 single crystal film.

    JP5794955B2

  • Semiconductor substrate, epitaxial wafer and manufacturing method thereof

    JP6744523B2

  • Paramagnetic garnet single crystal, and method for manufacturing the same

    JP2012254901A

  • SUBSTRATE WITH ??-Ga2O3 SINGLE CRYSTAL FILM AND ITS MANUFACTURING METHOD

    JP2014015366A

  • Method for producing metal oxide crystal, method for producing metal oxide epitaxial crystal laminated substrate, method for producing semiconductor device, metal oxide crystal, metal oxide epitaxial crystal laminated substrate, semiconductor device, and device for producing metal oxide crystal

    JP2023044693A