Structured product of white lignin and / or white lignin-polysaccharide copolymer
The extraction of white lignin or white lignin-polysaccharide copolymers in the reverse order of wood biosynthesis addresses the challenges of color contamination and structural alteration in traditional lignin isolation, enabling functional and versatile products with a β-O-4 type ether structure and specific bonding features.
Patent Information
- Application Number
- PCT/JP2024/016482
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
Current methods for isolating lignin often result in denatured, brown or black colored products, limiting their application due to color contamination issues, and existing purification techniques require complex steps that alter the chemical structure of lignin.
A new method involving the extraction of lignin in the reverse order of wood biosynthesis, resulting in white lignin or white lignin-polysaccharide copolymers with specific structural features, such as a β-O-4 type ether structure content of 50% or more, and specific bonds between lignin and polysaccharides, which are then complexed with organic acids or salts.
This approach allows for the production of white lignin or white lignin-polysaccharide copolymers with enhanced functionality and application potential, maintaining a structure closer to natural lignin while avoiding color contamination and chemical structure alteration.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Structured white lignin and / or white lignin-polysaccharide copolymer
[0001] The present invention relates to a structured product of lignin and / or lignin-polysaccharide copolymers.
[0002] Lignin, along with polysaccharides (cellulose and hemicellulose), is a major component of plant cell walls. Lignin is a naturally occurring aromatic polymer that has attracted attention. However, currently, most lignin is obtained as a by-product of the pulp and paper manufacturing process or the bioethanol production process. Because isolated lignin is denatured, it is difficult to enhance its functionality. Therefore, various methods for isolating lignin while minimizing denaturation have been proposed (Patent Document 1).
[0003] Lignin is generally colored brown or black. Therefore, lignin cannot be used in fields where coloration or contamination with brown or black colors is undesirable. To solve this problem, Patent Document 2 discloses a technique for decolorizing lignin after purifying it. However, this technique involves complicated steps and causes a change in the chemical structure of lignin.
[0004] JP 2013-241391 A JP 2021-017582 A
[0005] In the course of their research, the inventors came up with the idea of a new method for isolating lignin, which involves extracting lignin in the reverse order of wood biosynthesis, and discovered that this method allows the production of lignin in a state close to that of natural lignin. Based on this finding, the inventors conducted further research and discovered that it is possible to obtain white lignin or white lignin-polysaccharide copolymers with a structure closer to that of natural lignin.
[0006] In order to expand the possibilities for application of white lignin or white lignin-polysaccharide copolymers, it is important to develop new structures of white lignin or white lignin-polysaccharide copolymers.
[0007] Therefore, an object of the present invention is to provide a new structured product of white lignin or white lignin-polysaccharide copolymer.
[0008] The present inventors have conducted extensive research in light of the above-mentioned problems and have found that the above-mentioned problems can be solved by a structured product of white lignin and / or white lignin-polysaccharide copolymer, wherein the white lignin has a β-O-4 ether structure content of 50% or more, the white lignin-polysaccharide copolymer has at least one bond selected from the group consisting of an α-ether bond between the lignin and the polysaccharide, an α-ester bond between the lignin and the polysaccharide, and a γ-ester bond between the lignin and the polysaccharide, and the structured product is a complex of the white lignin and / or the white lignin-polysaccharide copolymer with an organic acid and / or a salt, and / or the structured product is a modified and / or substituted product of the hydroxyl groups of the white lignin and / or the white lignin-polysaccharide copolymer. Based on these findings, the present inventors have conducted extensive research and completed the present invention. Specifically, the present invention encompasses the following aspects:
[0009] Item 1. A structured product of white lignin and / or a white lignin-polysaccharide complex, wherein the white lignin has a β-O-4 ether structure content of 50% or more, the white lignin-polysaccharide complex has at least one bond selected from the group consisting of an α-ether bond between the lignin and the polysaccharide, an α-ester bond between the lignin and the polysaccharide, and a γ-ester bond between the lignin and the polysaccharide, and the structured product is a complex of the white lignin and / or the white lignin-polysaccharide complex with an organic acid and / or a salt, and / or the structured product is a modified or substituted product of hydroxyl groups of the white lignin and / or the white lignin-polysaccharide complex.
[0010] Item 2. The structured material is a complex of the white lignin and / or the white lignin-polysaccharide copolymer and / or a modified product and / or a substituted product thereof with an organic acid and / or a salt, and the structured material has a first derivative spectrum of infrared absorption spectroscopy that has a wavelength of 1080 to 950 cm -1 , 1480-1350 cm -1 , and 3000 to 2900 cm -1Item 2. The structured material according to Item 1, having a spectral structure unique to at least one wavenumber range selected from the group consisting of:
[0011] Item 3. The structured material has a first derivative spectrum of an infrared absorption spectrum of 1080 to 950 cm -1 , 1480-1350 cm -1 , and 3000 to 2900 cm -1 Item 3. The structured object according to Item 2, having three or more spectral structures specific to a wavenumber range consisting of:
[0012] Item 4. The structured product according to Item 2, which is in the form of a powder, a sol, or a gel.
[0013] Item 5. The structured material according to Item 2, wherein the structured material is a complex of the white lignin and / or the white lignin-polysaccharide copolymer with a compound having a carboxy structure and / or a carbonyl structure and / or an amine structure, and / or a salt containing a metal ion.
[0014] Item 6. The structured material according to Item 4, which is in a gel form.
[0015] Item 7. The structured product according to Item 1, wherein the structured product is a modified and / or substituted product of hydroxyl groups of the white lignin and / or the white lignin-polysaccharide copolymer, and contains at least one structure selected from the group consisting of a carbonylated structure, a halogenated structure, an aminated structure, a boron-modified structure, an acylated structure, and a crosslinked structure.
[0016] Item 8. The structured material according to Item 1, wherein the white lignin has a Hunter whiteness (W) of 60 or more, and / or the white lignin-polysaccharide complex has a Hunter whiteness (W) of 60 or more.
[0017] Item 9. A method for producing a structured product according to any one of Items 2 to 6 and 8, comprising the steps of: mixing the white lignin and / or the white lignin-polysaccharide copolymer with an organic acid and / or salt and a solvent to obtain a solution or dispersion; and reducing the solvent from the solution or dispersion.
[0018] Item 10. A method for producing a structured product according to Item 7 or 8, comprising a step of modifying or substituting hydroxyl groups of the white lignin and / or the white lignin-polysaccharide copolymer.
[0019] Item 11. An adsorbent, recovery agent, remover, or transporter for metal ions or salts containing the same, comprising white lignin and / or a white lignin-polysaccharide complex, wherein the white lignin has a β-O-4 ether structure content of 50% or more, and the white lignin-polysaccharide complex has at least one bond selected from the group consisting of an α-ether bond between the lignin and the polysaccharide, an α-ester bond between the lignin and the polysaccharide, and a γ-ester bond between the lignin and the polysaccharide.
[0020] Item 12. The adsorbent, recovery agent, removal agent, or transport agent according to claim 11, which is used to adsorb, recover, remove, or transport metal ions or salts containing such ions by forming a complex with the metal ions or salts containing such ions.
[0021] According to the present invention, a new structured product of white lignin or white lignin-polysaccharide copolymer can be provided.
[0022] This figure shows a flowchart of the M-APA method. This figure shows a flowchart of the A-APA method. This figure shows the microwave irradiation conditions, power, temperature, and pressure profiles for lignocellulosic component separation, and the specifications for the Biotage Initiator+ 60 microwave synthesizer, with an agitation speed of 600 rpm, cooling on, and absorption on high. This figure shows a 2D NMR spectrum of a low-denaturation, high-purity, high-ether-content lignin. This figure shows the analysis results of lignin isolated by the M-APA method using eucalyptus as the starting material (microwave treatment at 50°C for 10 minutes, acetic acid and peracetic acid 1% conditions). This figure shows the partial chemical structure of lignin interunit bonds and lignin-hemicellulose covalent bonds. This figure shows a 2D NMR spectrum (a-d) of a lignin-hemicellulose copolymer, with enlarged views of the interunit bonds and sugar regions (a'-d'). Lignin-hemicellulose copolymers isolated by the M-APA method from hardwood (a, b) and softwood (c, d) were analyzed. Circles in the figure represent LC bonds (ether and ester types). An example of a white lignin production scheme is shown. qNANO particle size distribution [A] and 3D fluorescence spectrum [B] of Eucalyptus-derived lignin microparticles in a diethyl sebacate / water solution (4:3). Measurements using qNANO revealed a mean particle size of 436 nm ±16 nm and a mode particle size of 304 nm [A]. Measurements using dynamic light scattering (DLS, Horiba, Ltd.) revealed a mean particle size of 462 nm ±27 nm and a mode particle size of 459 nm ±23 nm. Self-assembly resulted in clear long-wavelength fluorescence (Ex 380 nm, Em 440 nm) [B]. Lignin microparticles that disperse well in water were obtained using diethyl sebacate, a common, low-toxicity cosmetic base material. Pickering emulsions were also observed. 3D fluorescence spectra AD of white lignin nanoparticles. It has long wavelength fluorescence (400 nm - 550 nm) and characteristic anti-Stokes fluorescence (Ex 394 nm, Em 352 nm), (Ex 630 nm, Em 578 nm).The raw materials are A. white lignin derived from coniferous cedar, B. white lignin derived from coniferous cypress, C. white lignin derived from broad-leaved beech, D. white lignin derived from broad-leaved eucalyptus, E. white lignin derived from herbaceous rice straw, and F. white lignin derived from herbaceous sugarcane bagasse. This figure shows the absorption spectrum (normalized by the weight of lignin) obtained by diffuse reflectance spectroscopy for the white lignin-sodium acetate complex of Test Example 5-1. This figure shows a photograph of the appearance of the gel-like complex obtained using zinc chloride in Test Example 5. This figure shows the Raman spectrum of the white lignin-sodium acetate complex prepared in Test Example 5. This figure shows the first-derivative infrared absorption spectrum of the white lignin-citric acid complex prepared in Test Example 5. The arrows indicate typical absorptions characteristic of the complex. This figure shows the first-derivative infrared absorption spectrum of the white lignin-glycine complex prepared in Test Example 5. The arrows indicate typical absorptions characteristic of the complex. This shows the first-derivative infrared absorption spectrum of the white lignin / tartaric acid complex prepared in Test Example 5. The arrows indicate typical absorption characteristic of the complex. This shows the first-derivative infrared absorption spectrum of the white lignin / zinc chloride complex prepared in Test Example 5. The arrows indicate typical absorption characteristic of the complex. This shows the first-derivative infrared absorption spectrum of the white lignin / sodium acetate complex prepared in Test Example 5. The arrows indicate the spectral structure characteristic of the complex. 1 / 4 and 1 / 9 indicate the weight ratios of lignin to sodium acetate. This shows 2D HSQC NMR data for oxidized lignin A obtained in Test Example 6. This shows 13C-NMR data for oxidized lignin B obtained in Test Example 6. This shows 13C-NMR data for oxidized lignin C obtained in Test Example 6. This shows 119F-NMR data for halogenated lignin F1 obtained in Test Example 6. This shows differential spectra obtained in Test Examples 1-5. The raw materials are indicated in the upper right corner of each spectrum. The differential spectra obtained in Test Examples 1-5 are shown. The raw materials are indicated in the upper right corner of each spectrum. The differential spectra obtained in Test Examples 1-5 are shown. The raw materials are indicated in the upper right corner of each spectrum. The differential spectra obtained in Test Examples 1-5 are shown. The raw materials are indicated in the upper right corner of each spectrum. The differential spectra obtained in Test Examples 1-5 are shown. The raw materials are indicated in the upper right corner of each spectrum. The first-order differential infrared absorption spectrum of the bamboo white lignin / citric acid complex prepared in Test Example 6 is shown. The arrow indicates a representative absorption characteristic of the complex.Figure 1 shows the first-derivative infrared absorption spectrum of the bamboo white lignin / glycine complex prepared in Test Example 6. The arrows indicate representative absorptions specific to the complex. Figure 2 shows the first-derivative infrared absorption spectrum of the bamboo white lignin / tartaric acid complex prepared in Test Example 6. The arrows indicate representative absorptions specific to the complex. Figure 3 shows the first-derivative infrared absorption spectrum of the bamboo white lignin / zinc chloride complex in the wet state prepared in Test Example 6. The arrows indicate representative absorptions specific to the complex. The arrows indicate the spectral structure specific to the complex. Figure 4 shows the first-derivative infrared absorption spectrum of the dried bamboo white lignin / zinc chloride complex in the dry state (wet state) prepared in Test Example 6. The arrows indicate representative absorptions specific to the complex. Figure 5 shows the first-derivative infrared absorption spectrum of the swollen product obtained by adding water to the dry bamboo white lignin / zinc chloride complex prepared in Test Example 6. The arrows indicate representative absorptions specific to the complex.
[0043] Figure 1 shows the first-derivative infrared absorption spectrum of the bamboo white lignin / sodium acetate composite prepared in Test Example 6. The arrow indicates a representative absorption characteristic of the composite.
[0044] Figure 1 shows the first-derivative infrared absorption spectrum of the cypress white lignin / citric acid composite prepared in Test Example 6. The arrow indicates a representative absorption characteristic of the composite.
[0045] Figure 1 shows the first-derivative infrared absorption spectrum of the cypress white lignin / glycine composite prepared in Test Example 6. The arrow indicates a representative absorption characteristic of the composite.
[0046] Figure 1 shows the first-derivative infrared absorption spectrum of the cypress white lignin / tartaric acid composite prepared in Test Example 6. The arrow indicates a representative absorption characteristic of the composite.
[0047] Figure 1 shows the first-derivative infrared absorption spectrum of the cypress white lignin / zinc chloride composite prepared in Test Example 6. The arrow indicates a representative absorption characteristic of the composite.
[0048] Figure 1 shows the first-derivative infrared absorption spectrum of the cypress white lignin / sodium acetate composite prepared in Test Example 6. The arrow indicates a representative absorption characteristic of the composite.
[0023] In this specification, the expressions "contain" and "comprise" include the concepts of "contain," "comprise," "consist essentially of," and "consist only of."
[0024] 1. Method for Producing White Lignin or White Lignin-Polysaccharide Copolymer In one aspect, the present invention relates to a method for producing white lignin or white lignin-polysaccharide copolymer (sometimes referred to herein as the "production method of the present invention"), which comprises the steps of (a) contacting plant biomass with an alkaline solution to obtain an alkali-treated product, (b) washing the alkali-treated product with a liquid to obtain a washed product, and (c) contacting the washed product with a solution containing an organic acid. This method is described below.
[0025] The plant biomass is not particularly limited as long as it contains lignin and / or lignin-polysaccharide copolymer, and examples include the plant itself, mechanically processed plant products, etc. Plant biomass usually contains, in addition to lignin and / or lignin-polysaccharide copolymer, at least one selected from the group consisting of hemicellulose and cellulose, and preferably contains lignin, hemicellulose, lignin-polysaccharide copolymer, cellulose-hemicellulose complex, and cellulose.
[0026] Examples of plant bodies include coniferous trees, hardwoods, and non-woody materials. Specific examples include cedar, pine, spruce, larch, black pine, Abies sachalinensis, Himekomatsu, yew, Japanese yew, spruce, Japanese spruce, Japanese spruce, Japanese yew, Japanese bead, fir, Japanese yew, Douglas fir, spruce, yellow cedar, Japanese cypress, Douglas fir, Sitka spruce, Radiata pine, eastern spruce, eastern white pine, western larch, western fir, and western Examples of suitable woods include conifers such as hemlock and tamarack; hardwoods such as asbestos, American black cherry, yellow poplar, walnut, birch, zelkova, sycamore, silver cherry, ash, teak, Chinese elm, Chinese maple, oak, beech, hard maple, hickory, pecan, white ash, white oak, white birch, red oak, acacia, and eucalyptus; and non-woody materials such as rice, sugarcane, wheat, corn, pineapple, oil palm, kenaf, cotton, alfalfa, timothy, bamboo, bamboo grass, and sugar beet.
[0027] Examples of mechanically processed products of plants include logs, timber, boards, solid wood, wood materials, laminated lumber, laminated veneer lumber, plywood, wood boards, particle boards, fiber boards, wood chips, particulate wood (chips, particles, wood flour, etc.), fibrous wood, compressed materials, crushed materials, etc.
[0028] In one embodiment of the present invention, the plant biomass can be wood flour. The volume-average particle size of the wood flour is, for example, 500 μm or less, 200 μm or less, or 100 μm or less. The lower limit of the average particle size is not particularly limited and can be, for example, 1 μm, 2 μm, or 5 μm. Wood flour can be obtained by pulverizing the plant biomass. The pulverization can be carried out according to or in accordance with known methods, for example, using various mills (e.g., ball mills, mixer mills, etc.).
[0029] The plant biomass may be one type alone or a combination of two or more types.
[0030] In step (a), plant biomass is contacted with an alkaline solution to obtain an alkali-treated product. Step (a) loosens the plant cell wall structure (reducing intermolecular interactions and cleaving hydrogen bonds) and cleaves intramolecular ester bonds, thereby improving yield. Furthermore, by combining step (a) with step (b), described below, colored components of lignin can be efficiently removed.
[0031] The alkaline solution is not particularly limited as long as it is an alkaline solution to the extent that the above-mentioned purpose can be achieved. For example, the alkaline solution can be a solution with a pH of 12 to 15. The pH of the solution is preferably 13 to 14. The alkaline solution can also be a solution containing, for example, 0.2 to 2 mass % (preferably 0.7 to 1.5 mass %) of an alkali metal hydroxide (e.g., sodium hydroxide, potassium hydroxide, etc.). The concentration of the alkali metal hydroxide is preferably 0.1 to 0.3 M.
[0032] The amount of alkaline solution used is not particularly limited as long as it is an alkaline solution of an amount sufficient to achieve the above-mentioned purpose. The amount of alkaline solution used can be, for example, 3 to 20 mL, preferably 5 to 12 mL, per 1 g of plant biomass.
[0033] The manner in which the plant biomass is brought into contact with the alkaline solution is not particularly limited, but from the viewpoint of treatment efficiency and the like, it is preferable to immerse the plant biomass in the alkaline solution.
[0034] The temperature of the alkaline solution is not particularly limited as long as it is a temperature that can achieve the above-mentioned object. The temperature of the alkaline solution is preferably relatively low, for example, 70°C or lower, preferably 60°C or lower, more preferably 50°C or lower, even more preferably 10 to 50°C, still more preferably 20 to 50°C, and particularly preferably 30 to 50°C.
[0035] From the viewpoint of further increasing the whiteness of the resulting lignin and / or lignin-polysaccharide copolymer, it is preferable to irradiate the plant biomass with ultrasound or microwaves in step (a). The microwave treatment conditions can be appropriately set, for example, using a commercially available microwave synthesizer, and the treatment can be carried out while stirring the solution. The ultrasonic treatment conditions can be appropriately set, for example, using a commercially available ultrasonic irradiation device. The microwave and ultrasound output conditions can be set so that the temperature of the alkaline solution can be maintained at the above-mentioned temperature.
[0036] The treatment time in step (a) is not particularly limited as long as it is long enough to achieve the above-mentioned object, and is, for example, 5 to 100 minutes, preferably 15 to 70 minutes, and more preferably 20 to 40 minutes.
[0037] In order to effectively promote the penetration of the alkaline solution into the plant cell structure and the dispersion and movement of the extracted components, ultrasonic irradiation, pressure changes (pressurization, depressurization and repeated application), microwave irradiation, and the generation of nanobubbles are used, which efficiently and quickly achieves alkaline swelling (loosening the packing between polymer chains within the plant cell wall, partially cleaving hydrogen bonds, and partially cleaving ester bonds, causing the cell wall to swell) and the extraction of coloring components.
[0038] It is also effective to reduce the solid-liquid interfacial tension of the alkaline solution and improve wettability. This can be achieved by adding a hydrophilic organic solvent (such as ethanol) or a surfactant.
[0039] After the contact treatment of the plant biomass with the alkaline solution, solid-liquid separation treatment (centrifugation, filtration, settling, etc.) is carried out as necessary to obtain an insoluble portion (alkali-treated product), which is then subjected to step (b).
[0040] In step (b), the alkali-treated product is washed with a liquid to obtain a washed product. The combination of steps (a) and (b) described above makes it possible to efficiently remove colored components of lignin.
[0041] The liquid used for washing is not particularly limited as long as it contains a solvent capable of removing coloring components of lignin. From the viewpoint of the efficiency of removing coloring components, it is preferable that the liquid contains water. The water content in the liquid is preferably 20% by mass or more, more preferably 40% by mass or more, even more preferably 60% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more, and the liquid is particularly preferably water.
[0042] The method of washing with a liquid is not particularly limited. For example, washing can be performed by mixing the alkali-treated product with a liquid, followed by solid-liquid separation and recovering the insoluble portion. The washing operation is preferably repeated multiple times. From the viewpoint of further increasing the whiteness of the resulting lignin and / or lignin-polysaccharide copolymer, washing is preferably performed until the washing waste liquid reaches a neutral range (e.g., pH 6.5 to 8.0, preferably pH 6.5 to 7.5).
[0043] The insoluble portion (washed matter) obtained after the completion of the washing operation is subjected to step (c).
[0044] In step (c), the washed material is contacted with a solution containing an organic acid.
[0045] The organic acid solution is not particularly limited as long as it contains an organic acid and is capable of extracting and solubilizing lignin and / or lignin-polysaccharide copolymer.
[0046] The organic acid is not particularly limited, and examples thereof include acetic acid, formic acid, glyoxylic acid, maleic acid, propionic acid, folic acid, isobutyric acid, valeric acid, isovaleric acid, pyruvic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, ketoglutaric acid, adipic acid, lactic acid, tartaric acid, fumaric acid, oxaloacetic acid, malic acid, isocitric acid, citric acid, benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, hemimellitic acid, trimellitic acid, trimesic acid, mellophanic acid, prenitic acid, pyromellitic acid, mellitic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, camphorsulfonic acid, p-toluenesulfinic acid, and benzenesulfinic acid. Of these, preferred are acetic acid, formic acid, glyoxylic acid, 3-oxopropanoic acid, 2-methyl-3-oxopropanoic acid, etc., more preferred are acetic acid, formic acid, glyoxylic acid, etc., and particularly preferred is acetic acid.
[0047] The organic acid may be one kind alone or a combination of two or more kinds.
[0048] From the viewpoint of the yield of white lignin and / or white lignin-polysaccharide copolymer, the organic acid solution preferably contains a peracid.
[0049] The peracid is not particularly limited as long as it is an acid having a hydroperoxide group (—O—OH), and examples thereof include organic peroxoacids such as percarboxylic acids, persulfuric acid, percarbonic acid, perphosphoric acid, and hypoperhalogen acids. Examples of percarboxylic acids include peracetic acid, performic acid, perbenzoic acid, and metachloroperbenzoic acid, and examples of hypoperhalogen acids include hypoperchloric acid, hypoperbromic acid, and hypoperiodic acid. In addition to the above, examples of peracids include hydrogen peroxide, lithium peroxide, sodium peroxide, potassium peroxide, sodium percarbonate, urea peroxide, sodium perborate, tert-butyl hydroperoxide, cumene hydroperoxide, di-tert-butyl peroxide, dimethyldioxirane, acetone peroxide, methyl ethyl ketone peroxide, and hexamethylene triperoxide diamine. Among these, preferred are organic peroxoacids, hydrogen peroxide, sodium percarbonate, urea peroxide, sodium perborate, etc., more preferred are percarboxylic acids (particularly peracetic acid), hydrogen peroxide, etc., and particularly preferred is hydroperoxy acid.
[0050] The peracid may be one kind alone or two or more kinds in combination.
[0051] The content of the organic acid in the organic acid solution is, for example, 5 to 30 mol / L, preferably 8 to 25 mol / L, and more preferably 10 to 20 mol / L. The content of the organic acid in the organic acid solution is preferably 3 to 10 g, more preferably 4 to 8 g, and even more preferably 5 to 7 g per 1 g of the material to be washed that is contacted with the organic acid solution. The content of the organic acid in the organic acid solution is preferably 50 to 100 mass%.
[0052] When the organic acid solution contains peracid, the content of peracid in the organic acid solution is, for example, 0.05 to 3 mol / L, preferably 0.08 to 2.5 mol / L, and more preferably 0.1 to 2 mol / L. The content of peracid in the organic acid solution is preferably 0.03 to 0.10 g, more preferably 0.04 to 0.08 g, and even more preferably 0.05 to 0.07 g per 1 g of the material to be washed that is contacted with the organic acid solution. When the organic acid solution contains peracid, the content of peracid in the organic acid solution is preferably 0.1 to 10%, more preferably 0.3 to 5%, and even more preferably 0.6 to 2%.
[0053] The manner of contacting the washed material with the organic acid solution is not particularly limited, but from the viewpoint of treatment efficiency, etc., it is preferable to immerse the washed material in the organic acid solution. From the viewpoint of the whiteness of the resulting lignin and / or lignin-polysaccharide copolymer, it is preferable to carry out step (c) under an inert gas or a gas other than oxygen (i.e., the gas in contact with the organic acid solution is an inert gas or a gas other than oxygen). Examples of such gases include nitrogen, rare gases, and hydrogen.
[0054] By keeping the temperature of the organic acid solution at 100°C or less, it is possible to obtain high-quality (low-condensation) lignin with a high content of β-O-4 ether structures among all bond types between monolignols. In this case, the temperature of the organic acid solution is preferably 90°C or less, more preferably 70°C or less, and even more preferably 60°C or less. The lower limit of the temperature is, for example, 15°C, preferably 30°C, and more preferably 40°C.
[0055] A high-quality lignin-polysaccharide copolymer can be obtained by setting the temperature of the organic acid solution to more than 100°C. In this case, the temperature of the organic acid solution is preferably 160°C or less, more preferably 150°C or less. The lower limit of the temperature is, for example, 105°C, preferably 110°C, more preferably 115°C.
[0056] In one embodiment of the present invention, step (c) is carried out using an organic acid solution at 100°C or less to obtain white lignin from the resulting soluble fraction, while step (c) is carried out using an organic acid solution at a temperature higher than 100°C to obtain white lignin-polysaccharide copolymer from the resulting soluble fraction.
[0057] The treatment time in step (c) is not particularly limited as long as it is long enough to achieve the above-mentioned objective. The treatment time is, for example, 1 to 60 minutes, preferably 1 to 30 minutes, and more preferably 5 to 20 minutes. Furthermore, when obtaining a lignin-polysaccharide copolymer, the whiteness of the target product can be further improved by setting the treatment time to a relatively short time, for example, 15 minutes or less, preferably 10 minutes or less, and more preferably 5 minutes or less.
[0058] In step (c), it is preferable to perform microwave treatment while the biomass is immersed in the solution. This improves the yield of lignin and / or lignin-polysaccharide copolymer. The microwave treatment conditions can be set appropriately, but for example, a commercially available microwave synthesis device can be used to perform the treatment while stirring the solution. The microwave treatment time can be, for example, 1 to 30 minutes, and is preferably about 10 minutes. When microwave treatment is performed in the isolation method of the present invention, irradiation for a relatively short period of time is sufficient, so it can easily be constructed as a batch system or a continuous system.
[0059] In step (c), it is preferable to irradiate the plant biomass with microwaves or ultrasound under the same irradiation conditions as above, in order to promote penetration of the solution into the pores inside the plant cell walls and thereby improve the yield.
[0060] In order to effectively promote the penetration of the organic acid solution into the plant cell structure and the dispersion and movement of the extracted components, ultrasonic irradiation, pressure changes (pressurization, depressurization and repeated changes), microwave irradiation, the generation of nanobubbles, and cavitation are used, thereby achieving efficient extraction of coloring components in a short period of time.
[0061] It is also effective to reduce the solid-liquid interfacial tension of the organic acid solution and improve wettability. This can be achieved by adding a hydrophilic organic solvent (such as ethanol) or a surfactant.
[0062] After step (c), a separation solvent is added as needed, followed by separation of the soluble and insoluble portions. The method for separating the soluble and insoluble portions is not particularly limited, and methods such as decantation, spin-down, and filtration can be used. When no separation solvent is added, or when a solvent with a relatively low water content or no water (e.g., a solvent with a water content of 0 to 50% by mass, preferably 0 to 30% by mass, more preferably 0 to 20% by mass, even more preferably 0 to 10% by mass, and particularly preferably 0 to 5% by mass) is added as the separation solvent, the soluble portion contains white lignin or white lignin-polysaccharide copolymer. On the other hand, when a solvent with a relatively high water content (e.g., a solvent with a water content of more than 50 to 100% by mass, preferably 70 to 100% by mass, more preferably 80 to 100% by mass, even more preferably 90 to 100% by mass, and particularly preferably 95 to 100% by mass) is added as the separation solvent, the insoluble portion contains white lignin or white lignin-polysaccharide copolymer.
[0063] Lignin and lignin-hemicellulose copolymers are isolated using separation solvents such as dioxane, ethanol, acetone, acetonitrile, DMSO, DMF, NMI, various alcohols (e.g., ethyl acetate, methanol, butanol), acetic acid, water, and mixtures of these. From the viewpoints of extraction efficiency, selectivity, and environmental impact, mixtures of water with organic solvents (e.g., ethanol, dioxane, acetone, acetonitrile) are preferred.
[0064] In one embodiment, the production method of the present invention preferably comprises the step of: (d) after the step (c), adding a first solvent to obtain a solution containing white lignin and / or a white lignin-polysaccharide copolymer.
[0065] The first solvent is not particularly limited, and examples thereof include the above-mentioned separation solvents. Among them, the first solvent is preferably at least one solvent selected from the group consisting of ethanol, methanol, acetone, acetonitrile, propanol, and water (particularly preferably ethanol), or a mixed solvent.
[0066] The first solvent is added and mixed as necessary, and then the soluble and insoluble portions are separated by any method, including decantation, spin-down, and filtration, to obtain a solution containing white lignin and / or a white lignin-polysaccharide copolymer.
[0067] When the production method of the present invention includes step (d), from the viewpoint of further increasing the whiteness of the resulting lignin and / or lignin-polysaccharide copolymer, it preferably also includes the step of: (e) adding a second solvent to the concentrate of the white lignin and / or white lignin-polysaccharide copolymer-containing solution to extract the white lignin and / or white lignin-polysaccharide copolymer.
[0068] The concentrate of the white lignin and / or white lignin-polysaccharide copolymer-containing solution is not particularly limited as long as it is obtained by distilling off part or all of the solvent from the white lignin and / or white lignin-polysaccharide copolymer-containing solution. The concentrate is preferably a dry product.
[0069] The second solvent is not particularly limited, and examples thereof include the separation solvents described above. Among these, a preferred second solvent is a mixed solvent of water and at least one organic solvent (particularly preferably dioxane) selected from the group consisting of dioxane, acetone, acetonitrile, allyl alcohol, propanol, 1-butanol, 2-methyl-1-propanol, 2-butanol, ethyl acetate, and pyridine. The content of the organic solvent in the mixed solvent is, for example, 60 to 95% by mass, preferably 70 to 90% by mass, and more preferably 75 to 85% by mass.
[0070] A second solvent is added and mixed as necessary to extract white lignin and / or white lignin-polysaccharide copolymer. The resulting extract (soluble portion) is then separated from the insoluble portion. The method for separating the soluble and insoluble portions is not particularly limited, and methods such as decantation, spin-down, and filtration can be used.
[0071] After step (c), the soluble portion obtained as described above can be concentrated and dried to obtain solid white lignin and / or white lignin-polysaccharide copolymer.
[0072] The production method of the present invention can obtain white lignin and / or white lignin-polysaccharide copolymers by suppressing reactions that cause color development during the extraction and separation process (oxidation reaction of lignin, over-decomposition, condensation, Maillard reaction, and coloration reaction) while suppressing the decomposition and degradation of lignin into smaller molecules.
[0073] Regarding the method for producing white lignin and / or white lignin-polysaccharide copolymer, the present invention includes the following aspects.
[0074] Item A1. A method for producing white lignin or a white lignin-polysaccharide copolymer, comprising: (a) a step of contacting plant biomass with an alkaline solution to obtain an alkali-treated product; (b) a step of washing the alkali-treated product with a liquid to obtain a washed product; and (c) a step of contacting the washed product with a solution containing an organic acid.
[0075] Item A2. The method according to Item A1, wherein the organic acid solution contains a peracid.
[0076] Item A3. The method according to Item A1 or 2, wherein the alkaline solution is at 70°C or lower.
[0077] Item A4. The method according to any one of Items A1 to A3, wherein the step (a) comprises irradiating the plant biomass with ultrasound or microwaves.
[0078] Item A5. The method according to any one of Items A1 to A4, wherein the liquid contains water.
[0079] Item A6. The method according to any one of Items A1 to A4, wherein the organic acid solution is at 60°C or lower.
[0080] Item A7. The method according to any one of Items A1 to A6, wherein the step (c) comprises irradiating the object to be washed with ultrasonic waves or microwaves.
[0081] Item A8. The method according to any one of Items A1 to A7, comprising: (d) after the step (c), adding a first solvent to obtain a solution containing white lignin or a white lignin-polysaccharide copolymer.
[0082] Item A9. The method according to Item A8, comprising: (e) adding a second solvent to the concentrate of the white lignin and / or white lignin-polysaccharide copolymer-containing solution to extract the white lignin.
[0083] Item A10. The method according to any one of Items A1 to A9, wherein the white lignin and / or the white lignin-polysaccharide copolymer has a Hunter whiteness (W) of 60 or more.
[0084] Item A11. The method according to any one of Items A1 to A10, wherein the organic acid solution is at 100°C or less and includes a step of obtaining a white lignin-containing solution.
[0085] Item A12. The method according to any one of Items A1 to A10, wherein the organic acid solution has a temperature of more than 100°C and includes a step of obtaining a white lignin-polysaccharide copolymer-containing solution.
[0086] 2. White Lignin In one embodiment, the production method of the present invention makes it possible to obtain white lignin characterized by at least a content of β-O-4 ether structures of 50% or more (preferably further characterized by a Hunter whiteness (W) of 60 or more).
[0087] According to the production method of the present invention, in one embodiment, it is possible to obtain white lignin characterized at least by a ratio of oxidized lignin structures of 0.3 or less (preferably further characterized by a Hunter whiteness (W) of 60 or more).
[0088] In one embodiment, the white lignin of the present invention may have a Hunter brightness (W) of 60 or more. The Hunter brightness is measured and calculated according to the method described in Test Examples 1-3 below. The Hunter brightness (W) of the white lignin of the present invention is preferably 70 or more, more preferably 75 or more, even more preferably 80 or more, and even more preferably 85 or more. The upper limit of the Hunter brightness (W) is not particularly limited, and may be, for example, 98, 95, or 92. Furthermore, since the white color of the present invention is derived from total reflection of light, the lignin is transparent when dissolved in solution. Furthermore, it has the characteristic of being able to make transparent mixtures with transparent resins and paints.
[0089] The white lignin of the present invention is lignin isolated from biomass (including natural lignin). Natural lignin has a wide variety of bonding modes. Representative bonding modes of natural lignin include the following:
[0090]
[0091] The above is called a β-O-4 bond.
[0092]
[0093] The above is called a resinol (β-β) bond.
[0094]
[0095] The above is called a phenylcoumaran (β-5) bond.
[0096]
[0097] The above is called a 5-5 bond.
[0098]
[0099] The above is called dibenzodioxin (DBDO 5-5 / 4-O-β) binding.
[0100]
[0101] The above is called a 4-O-5 bond.
[0102]
[0103] The above is called β-1 bond.
[0104]
[0105] The above is called spirodienone binding.
[0106] In natural lignin, the content of β-O-4 ether structures is the highest among all bond types between monolignols, although this varies depending on the plant species. For example, in coniferous trees, the content is said to be 40-60%. In broad-leaved trees, such as eucalyptus, the content is said to be around 45%.
[0107] The white lignin of the present invention has a β-O-4 ether structure content of 50% or more, preferably 60% or more, more preferably 65 to 85%, and even more preferably 70 to 80% of all bond types between monolignols.
[0108] The white lignin of the present invention preferably has a β-O-4 ether structure content (%) of all bond types between monolignols, where x% is the lignin content in the raw biomass. The upper limit is preferably 2x%.
[0109] The content of β-O-4 type ether structures among all the bond types between monolignols in lignin is specifically measured as follows. The sample is dissolved in deuterated dimethyl sulfoxide (DMSO-d6) to a concentration of 1-10 wt%, and an NMR spectrum is obtained using a Bruker Avance III 600 MHz NMR instrument equipped with a cryogenic probe. The content of β-O-4 type ether structures can be estimated from the signal volume in the HSQC (heteronuclear single-quantum correlation spectroscopy) spectrum. The content is calculated in terms of per 100 lignin aromatic rings. The aromatic nucleus is the syringyl nucleus, with the 2- and 6-positions S 2,6 (+S' 2,6The ether structure can be calculated from the C-H spin coupling signals at the α-position (benzyl position) and β-positions, based on the sum of the signal integrals of G2(+G'2) and G2 / 2 at the 2nd position of the guaiacyl nucleus (in herbs, the H nucleus is also summed). The quantitative values obtained using the 2D NMR method can be corrected according to the literature (Okamura, H. Nishimura, T. Nagata, T. Kigawa, T. Watanabe and M. Katahira, Accurate and molecular-size-tolerant NMR quantitation of diverse components in solution, Scientific Reports, 6, 21742. 2016) to calculate the accurate content.
[0110] The white lignin of the present invention exhibits high solubility in acetic acid and ethanol, and is characterized by an NMR-DMSO standard solubility index, as defined herein (described below), of 50 or more, preferably 70 or more, and more preferably 100 or more in acetic acid, and 30 or more, preferably 50 or more, and more preferably 60 or more in ethanol.
[0111] The NMR-DMSO reference solubility index was calculated as follows. 10 mg of lignin powder was weighed and dissolved in 0.5 mL of various NMR deuterated solvents for quantitative 1H-NMR measurements. Deuterated solvents used included DMSO-d6, deuterated acetic acid-d4, heavy water, and deuterated ethanol-d6. The integrals in the aromatic region of the resulting spectra (6-8 ppm) were then calculated. The integrals obtained from the 1H NMR spectra of lignin dissolved in DMSO-d6 were set to 100, and the ratios of the integrals for the lignin dissolved in each solvent were calculated. This allows for objective and quantitative calculation of the solubility in each solvent, which is defined as the DMSO reference solubility index. DSS (1 mM, chemical shift 0 ppm) can be used as an internal spectral reference for quantification. Additionally, 1-3% deuterated DMSO (chemical shift 39.6 ppm) can be added to each solvent as a reference reference.
[0112] The white lignin of the present invention preferably has a solubility of 2 w / v% or more in 60-80% ethanol at 25°C. Therefore, by using the white lignin of the present invention, the self-assembled bodies described below can be easily obtained, and highly stable self-assembled bodies can be obtained. The solubility is preferably 4 w / v% or more, more preferably 5 w / v% or more, even more preferably 6 w / v% or more, and even more preferably 7 w / v% or more.
[0113] The solubility is measured as follows: The sample is stirred and dissolved in 25°C ethanol, and then separated into an ethanol-soluble portion and an ethanol-insoluble portion by solid-liquid separation. A 25°C aqueous ethanol solution (1 / 1 ethanol / water) is added to the ethanol-insoluble portion, which is stirred and dissolved to obtain an aqueous ethanol-soluble portion. The aqueous ethanol-soluble portion is mixed with the ethanol-soluble portion to obtain a sample solution. The amount of aqueous ethanol added is adjusted so that the ethanol concentration of the sample solution is in the range of 60-80%. In the process of obtaining the soluble portion, the sample is dispersed and solubilized, if necessary, using an ultrasonic cleaner for 3 min at 28 kHz. The maximum sample concentration at which the sample solution becomes visually transparent is defined as the "solubility in 60-80% ethanol at 25°C."
[0114] The white lignin of the present invention preferably has a constituent ratio of biphenyl-type lignin, which has a condensed structure, of 5% or less.
[0115] The white lignin of the present invention preferably has a number average molecular weight (Mn) of 0.7 to 9 kDa, more preferably 1 to 5 kDa, and even more preferably 1.5 to 4 kDa.
[0116] The white lignin of the present invention preferably has a weight average molecular weight (Mw) of 1 to 10 kDa, more preferably 1.5 to 8 kDa, and even more preferably 2 to 6 kDa.
[0117] In this invention, the number-average molecular weight (Mn) and weight-average molecular weight (Mw) of lignin are specifically measured as follows. The molecular weight of lignin can be determined by size exclusion chromatography (SEC), also known as gel permeation chromatography (GPC). The sample is dissolved in a solution of acetic anhydride and a base (e.g., pyridine) and reacted for 3-6 hours to obtain an acetylated product. This is then dissolved in tetrahydrofuran (THF) at a concentration of 2.0 mg / mL and separated by high-performance liquid chromatography. A Tosoh HZ-M column (150 mm x 4.6 mm id, 4 μm, three columns connected in series) is used. Analysis is performed by injecting 10 μL of sample, using tetrahydrofuran (THF) as the mobile phase at a column temperature of 40°C and a flow rate of 0.35 mL / min. A mass calibration curve (calibration curve) is prepared using standard polystyrene, Tosoh PStQuickC (molecular weights (MW) of 2,110,000, 427,000, 37,900, and 5970), pinoresinol (MW 352), and vanillin (MW 152), to determine the Mw and Mn of the sample.
[0118] The white lignin of the present invention preferably has a polydispersity (Mw / Mn) of 2.5 or less, more preferably 2 or less.
[0119] The white lignin of the present invention has a ratio of oxidized lignin of preferably 0.5 or less, more preferably 0.3 or less, and even more preferably 0.1 or less.
[0120] Oxidized lignin is a compound in which the hydroxyl groups at the benzyl positions of the syringyl nucleus (S nucleus), guaiacyl nucleus (G nucleus), and p-hydroxyphenyl nucleus (H nucleus), which are the basic structural units of lignin, are oxidized to form ketone structures (α-carbonyl structures). Oxidation of the benzyl positions extends the conjugated system of the aromatic ring to the α-position, which is one cause of coloration. Traditionally, lignin oxidation could not be avoided through artificial manipulations involved in obtaining lignin. Lignin becomes colored when oxidized by fine grinding, high-temperature, high-pressure conditions, or strong acid conditions. We have found that the ratio of oxidized lignin is an indicator of white lignin.
[0121] The ratio of oxidized lignin can be calculated as follows:
[0122] <Calculation method for oxidized lignin ratio> Samples were dissolved in deuterated dimethyl sulfoxide (DMSO-d6) to a concentration of 1-10 wt%, and NMR spectra were acquired using a Bruker Avance III 600 MHz NMR instrument equipped with a cryogenic probe. The oxidized lignin ratio was calculated from the signal volume in the HSQC (heteronuclear single-quantum correlation spectroscopy) spectrum. Signal integration values were calculated using Bruker's Topspin 3.6 software. Since the integration region may vary slightly depending on the sample and measurement environment, the signal integration region was adjusted appropriately during analysis (this also applies to the other measurement methods described herein). Positions 2 and 6 of the syringyl nucleus (S, δH / δC = 6.7 ± 0.2 ppm / 103.6 ± 1.5 ppm region), position 2 of the guaiacyl nucleus (G, δH / δC = 6.96 ± 0.2 ppm / 111.1 ± 1.5 ppm region), positions 2 and 6 of the syringyl nucleoside derivative (S', δH / δC = 7.21 ± 0.2 ppm / 106.1 ± 1.2 ppm region), position 2 of the guaiacyl nucleoside derivative (G', δH / δC = 7.45 ± 0.2 ppm / 111.5 ± 1.2 ppm region). The oxidized lignin ratio (S) = [signal integral value of the S' region] / [signal integral value of the S region], and the oxidized lignin ratio (G) = [signal integral value of the G' region] / [signal integral value of the G region].
[0123]
[0124] The white lignin of the present invention can be used in healthcare, cosmetics, dyes, resins, composite materials, etc. The white lignin of the present invention is also suitable as a starting material for various biomass conversion research and reaction design. The white lignin of the present invention can also be colored in various colors (especially colors that cannot be expressed by mixing the original colors of lignin (brown, black)).
[0125] Regarding white lignin, the present invention includes the following aspects.
[0126] Item A13: White lignin having a β-O-4 ether structure content of 50% or more (preferably further characterized by a Hunter whiteness (W) of 60 or more).
[0127] Item A14. White lignin obtainable by the method according to Item A11.
[0128] Item A15. White lignin having a ratio of oxidized lignin structure of 0.3 or less (preferably further characterized by a Hunter whiteness (W) of 60 or more).
[0129] Item A16. In the first derivative spectrum of the infrared absorption spectrum, for hardwoods, the wavelength is 1007-1017 cm -1 , 1072-1082 cm -1 , 1108-1118 cm -1 , 1148-1154 cm -1 , 1179-1183 cm -1 , 1204-1210 cm -1 , 1257-1265 cm -1 , 1317-1321 cm -1 , 2893-2921 cm -1 Positive peak (convex upward), 1035-1041 cm -1 , 1130-1134 cm -1 , 1160-1167 cm -1 , 1331-1337 cm -1and the white lignin has a total of 6 or more, preferably 8 or more, more preferably 10 or more, and particularly preferably 12 or more of the above peaks.
[0130] Item A17. In the first derivative spectrum of the infrared absorption spectrum, for conifers, the wavelength range is 1010-1035 cm -1 , 1070-1088 cm -1 , 1112-1126 cm -1 , 1198-1212 cm -1 , 1250-1261 cm -1 , 1360-1365 cm -1 Positive peak (convex upward), 1033-1047 cm -1 , 1144-1148 cm -1 , 1161-1171 cm -1 , 1226-1244 cm -1 , 1270-1290 cm -1 The white lignin is characterized by having a negative peak (convex downward) at the peaks of 4 or more, preferably 6 or more, more preferably 8 or more, and particularly preferably 10 or more of the above peaks.
[0131] Item A18. In the first derivative spectrum of the infrared absorption spectrum, in herbs, the wavelength is 1005-1011 cm -1 , 1055-1072 cm -1 , 1072-1082 cm -1 , 1109-1126 cm -1 Positive peak (convex upward), 1030-1041 cm -1 , 1128-1136 cm -1 and the white lignin has a total of three or more, preferably four or more, and more preferably five or more of the above peaks.
[0132] 3. White Lignin-Polysaccharide Copolymer In one embodiment, the production method of the present invention makes it possible to obtain a white lignin-polysaccharide copolymer having at least one bond selected from the group consisting of an α-ether bond between lignin and polysaccharide, an α-ester bond between lignin and polysaccharide, and a γ-ester bond between lignin and polysaccharide (preferably further characterized by a Hunter whiteness (W) of 60 or more).
[0133] In one embodiment, the white lignin-polysaccharide copolymer of the present invention may have a Hunter brightness (W) of 60 or more. The Hunter brightness is measured and calculated according to the method described in Test Examples 1-3 below. The Hunter brightness (W) of the white lignin-polysaccharide copolymer of the present invention is preferably 70 or more, more preferably 75 or more, even more preferably 80 or more, and still more preferably 85 or more. The upper limit of the Hunter brightness (W) is not particularly limited, and may be, for example, 98, 95, or 92.
[0134] Polysaccharides include, for example, xylan and mannan, as well as glucomannan, galactoglucomannan, glucuronoxylan, and arabinoglucuronoxylan. Hemicellulose is primarily composed of glucomannan in conifers, glucuronoxylan in broad-leaved trees, and arabinoxylan in herbaceous plants. The monomers mentioned above include xylose, arabinose, glucose, mannose, galactose, and uronic acid. The side chains also contain acetyl and methoxy groups. In herbaceous plants, hemicellulose includes ferulic acid and diferulic acid bound to the arabinose side chain of arabinoxylan.
[0135] The white lignin-polysaccharide copolymer of the present invention is a lignin-polysaccharide copolymer that can be uniformly dispersed in a separation solvent and is characterized by a polymer structure in which lignin and polysaccharides are copolymerized through covalent bonds. The white lignin-polysaccharide copolymer of the present invention is isolated by hydrolyzing a small portion (less than 10% of the bonds) of the hemicellulose main chain bonds in the lignin-polysaccharide complex structure in plant cell walls. By carrying out the hydrolysis reaction under mild conditions, excessive decomposition, side reactions, and degradation to lower molecular weight compounds can be suppressed.
[0136] The white lignin-polysaccharide copolymer of the present invention is characterized by having at least one bond selected from the group consisting of an α-ether bond between lignin and polysaccharide (LC α-ether bond), an α-ester bond between lignin and polysaccharide (LC α-ester bond), and a γ-ester bond between lignin and polysaccharide (LC γ-ester bond).
[0137] In the white lignin-polysaccharide copolymer of the present invention, the α-ether bond (LC α-ether), which is the copolymerization point between the lignin and the polysaccharide, is preferably concentrated to a concentration of 1.2 times or more compared to the original bond unit composition ratio of the raw material biomass.
[0138] In biomass, lignin and polysaccharides are also bound together by non-covalent bonds. These non-covalent bonds are due to hydrophobic interactions, hydrogen bonds, electrostatic interactions, and entanglement of polymer chains. Therefore, previous studies have not provided clear evidence that lignin and polysaccharides, which are polymers with different properties, form copolymers through covalent bonds. Furthermore, conventional methods for preparing lignin polysaccharide copolymers involve multiple steps, resulting in low yields (less than 5%) or low purity (relative integral values of the signal at the α-position of the LC α-ether bond per 100 aromatic rings are each 1.5 or less).
[0139] Clear evidence of the copolymerization point (covalent bond) in the lignin-hemicellulose copolymer can be confirmed by signal assignment using HSQC, a two-dimensional NMR technique (Figures 3 and 4). Further clear evidence can be confirmed by continuous correlation analysis using HMBC and TOCSY-HSQC. For more details, please refer to the literature (Nishimura et al., Direct evidence for α ether linkage between lignin and carbohydrates in wood cell walls, Sci Rep 2018).
[0140] LC α ether: C–H correlation signals at the α-position of lignin (LC ether, δH / δC = 4.50 ±0.15 ppm / 80.1 ±1 ppm region) and (LC ether, δH / δC = 4.95 ±0.2 ppm / 81.5 ±1.5 ppm region), which are derived from the ether bond between the hydroxyl group of the 6-position of hexose or pentose and the α-position (benzylic position) of lignin.
[0141] LC α ester: A C–H correlation signal at the α-position of lignin (LC α ester, δH / δC = 5.88 ±0.15 ppm / 74.0 ±1.5 ppm region) derived from the ester bond between the carboxyl group at position 6 of glucuronic acid (uronic acid) and the α-position (benzylic position) of lignin.
[0142] LC γ ester: C–H correlation signal at the γ position of lignin (LC γ ester, δH / δC = 4.0 ±0.15 ppm, 4.4 ±0.15 ppm, / 64.8 ±1.5 ppm region) derived from the ester bond between the carboxy group at position 6 of glucuronic acid (uronic acid) and the γ position of lignin.
[0143] The white lignin-polysaccharide copolymer of the present invention is preferably characterized by a solubility of 2 w / v% or more in 60-80% ethanol at 25°C. Therefore, by using the white lignin-polysaccharide copolymer of the present invention, the self-assembled bodies described below can be easily obtained, and highly stable self-assembled bodies can be obtained. The solubility is preferably 4 w / v% or more, more preferably 5 w / v% or more, even more preferably 6 w / v% or more, and even more preferably 7 w / v% or more.
[0144] The white lignin-polysaccharide copolymer of the present invention exhibits high solubility in acetic acid and ethanol, and is characterized by an NMR-DMSO standard solubility index, as defined herein (described below), of 50 or more, preferably 70 or more, and more preferably 100 or more in acetic acid, and 30 or more, preferably 50 or more, and more preferably 60 or more in ethanol.
[0145] In the white lignin-polysaccharide copolymer of the present invention, the bond unit composition ratio of LC α ether and LC α ester, which are copolymerization points, is preferably 2% or more, more preferably 5% or more, in terms of the lignin aromatic ring ratio.
[0146] In the white lignin-polysaccharide copolymer of the present invention, the polysaccharide to lignin ratio is preferably 0.1-2, more preferably 0.3-1.
[0147] The white lignin-polysaccharide copolymer of the present invention preferably has a molecular weight (Mw) of 1 to 15 kDa, more preferably 2 to 7 kDa, and preferably has a polydispersity (Mw / Mn) of 3.5 or less, more preferably 2.5 or less.
[0148] The above-mentioned parameters can be measured according to the measurement method for white lignin of the present invention, the measurement method in the Examples described below, or known methods.
[0149] Regarding the white lignin-polysaccharide copolymer, the present invention includes the following aspects.
[0150] Item A16. A white lignin-polysaccharide copolymer having at least one bond selected from the group consisting of an α-ether bond between lignin and polysaccharide, an α-ester bond between lignin and polysaccharide, and a γ-ester bond between lignin and polysaccharide (preferably further characterized by a Hunter whiteness (W) of 60 or more).
[0151] Item A20. White lignin or white lignin polysaccharide copolymer that is soluble in deuterated acetic acid and has a NMR-DMSO standard solubility index of 50 or more, preferably 60 or more, more preferably 80 or more, and even more preferably 100 or more, or white lignin or white lignin polysaccharide copolymer that is soluble in deuterated ethanol and has a NMR-DMSO standard solubility index of 30 or more, preferably 40 or more, more preferably 50 or more, and even more preferably 60 or more.
[0152] Item A21: A white lignin-polysaccharide copolymer obtainable by the method according to Item A12.
[0153] 4. Structured Product In one aspect, the present invention relates to a structured product of white lignin and / or white lignin-polysaccharide copolymer, which will be described below.
[0154] The structured material may be a structured material made of white lignin alone, a structured material made of white lignin-polysaccharide copolymer alone, or a structured material made of a combination of white lignin and white lignin-polysaccharide copolymer.
[0155] In one embodiment, the structured product is a complex (structured product 1) of white lignin and / or white lignin-polysaccharide copolymer with an organic acid and / or salt. In the present invention, it has been found that white lignin and / or white lignin-polysaccharide copolymer has excellent solubility and dispersibility in solvents, and has a molecular structure characterized by having significantly fewer branched structures and colored structures than other lignins and / or lignin-polysaccharide copolymers, and that the above complex can be successfully obtained.
[0156] In one embodiment, the "complex" in Structure 1 refers to a crystal in the broad sense, and includes cocrystals, salts and hydrates, pseudopolymorphs, solvates, and crystalline polymorphs thereof.
[0157] The structured product 1 has a structure different from that of white lignin and / or white lignin, and organic acids and / or salts. Specifically, for example, the structured product 1 has a unique spectral structure in at least one wavenumber range selected from the group consisting of 1080 to 950 cm-1, 1480 to 1350 cm-1, and 3000 to 2900 cm-1 in the first derivative spectrum of the infrared absorption spectrum. The structured product 1 preferably has two, more preferably three, even more preferably at least four, and particularly preferably five or more unique spectral structures in any of the above groups.
[0158] The organic acid that forms the structured product 1 is not particularly limited, but examples thereof include maleic acid, formic acid, acetic acid, propionic acid, folic acid, isobutyric acid, valeric acid, isovaleric acid, pyruvic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, ketoglutaric acid, adipic acid, lactic acid, tartaric acid, fumaric acid, oxaloacetic acid, malic acid, isocitric acid, citric acid, benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, glucuronic acid, glyoxylic acid, hemimellitic acid, trimellitic acid, trimesic acid, mellophanic acid, prenitic acid, pyromellitic acid, mellitic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, camphorsulfonic acid, p-toluenesulfinic acid, and benzenesulfinic acid.
[0159] The organic acid may also include amino acids. Examples of the amino acids include amino acids having a basic side chain such as lysine, arginine, and histidine; amino acids having an acidic side chain such as aspartic acid and glutamic acid; amino acids having an uncharged polar side chain such as glycine, asparagine, glutamine, serine, threonine, tyrosine, and cysteine; amino acids having a nonpolar side chain such as alanine, valine, leucine, isoleucine, proline, phenylalanine, methionine, and tryptophan; amino acids having a β-branched side chain such as threonine, valine, and isoleucine; and amino acids having an aromatic side chain such as tyrosine, phenylalanine, tryptophan, and histidine. The organic acid may also include fatty acids.
[0160] It is preferable to use an organic acid that is solid at room temperature (20°C).
[0161] The organic acid may be one kind alone or a combination of two or more kinds.
[0162] The salt that forms the structured product 1 is not particularly limited, but is a compound containing an anion or halide ion of an organic acid (for example, the organic acid described above) or an inorganic acid and an inorganic cation or an organic cation, so long as it is not particularly limited.
[0163] Examples of inorganic acids include hydrochloric acid, sulfuric acid, nitric acid, carbonic acid, boric acid, boronic acid, hydrofluoric acid, hypochlorous acid, chlorous acid, chloric acid, perchloric acid, hypobromous acid, bromous acid, bromic acid, perbromic acid, hypoiodous acid, iodous acid, iodic acid, periodic acid, phosphorous acid, phosphoric acid, polyphosphoric acid, chromic acid, permanganic acid, etc. Examples of halide ions include fluoride ions, chloride ions, bromide ions, iodide ions, etc.
[0164] Examples of inorganic cations include metal ions. Examples of metals include typical metals (alkali metals: Li, Na, K, Rb, Cs; alkaline earth metals: Ca, Sr, Ba, Ra); magnesium group elements: Be, Mg, Zn, Cd, Hg; aluminum group elements: Al, Ga, In; rare earth elements: Y, La, Ce, Pr, Nd, Sm, Eu; tin group elements: Ti, Zr, Sn, Hf, Pb, Th; iron group elements: Fe, Co, Ni; earth elements: V, Nb, Ta; chromium group elements: Cr, Mo, W, U; manganese group elements: Mn, Re; precious metals: Cu, Ag, etc.
[0165] The organic cation may be, for example, an ammonium ion (i.e., NH4 + ) and substituted ammonium ions (e.g., NHR X+ , NH2R X 2 + , NHR X 3 + , N.R. X 4 + ) are included, but are not limited to these.
[0166] Specific examples of salts include sodium acetate, zinc chloride, and ammonium acetate.
[0167] The salt may be one type alone or a combination of two or more types.
[0168] The structured product 1 may contain, as the organic acid and / or salt, a divalent or higher organic acid and / or a salt containing a divalent or higher metal ion. In this case, the white lignin and / or the white lignin-polysaccharide copolymer is more likely to form a network structure, making it easier to obtain a gel.
[0169] The structure 1 can be, for example, in the form of a solid (eg, powder), a sol, or a gel.
[0170] Structure 1 is useful, for example, as a UV protection material. Formulation using structure 1 is a powerful form for stable application development, offering advantages in terms of stabilization, transportation, delivery, storage, and addition at room temperature.
[0171] The structured product 1 can be produced by a method including the steps of mixing white lignin and / or white lignin-polysaccharide copolymer, an organic acid and / or a salt, and a solvent to obtain a solution or dispersion, and reducing the solvent from the solution or dispersion.
[0172] The solvent is not particularly limited as long as it can dissolve or uniformly disperse the white lignin and / or white lignin-polysaccharide copolymer and the organic acid and / or salt. Examples of the solvent include water, alcohol, acetic acid, dimethyl sulfoxide, dioxane, pyridine, ionic liquid, and deep eutectic solvent. The solvent can also be a mixed solvent of two or more solvents.
[0173] The order of mixing is not particularly limited. For example, the order may be such that white lignin and / or white lignin-polysaccharide copolymer is added to a solvent and then an organic acid and / or salt is added, or the order may be such that white lignin and / or white lignin-polysaccharide copolymer is added to solvent 1, and an organic acid and / or salt is added to solvent 2, and then the two liquids are mixed.
[0174] The temperature during mixing is not particularly limited, but can be, for example, 4 to 50°C, preferably 15 to 30°C.
[0175] The concentration of the organic acid and / or salt in the solution or dispersion is preferably 0.01 mg / mL or more, more preferably 0.02 mg / mL or more, even more preferably 0.05 mg / mL or more, even more preferably 0.07 mg / mL or more, and still more preferably 0.08 mg / mL or more, from the viewpoint of the formation efficiency of the structured product 1. The upper limit of the concentration is not particularly limited, and may be, for example, 1000 mg / mL, 700 mg / mL, 500 mg / mL, 300 mg / mL, 200 mg / mL, 100 mg / mL, or 50 mg / mL.
[0176] The concentration of the white lignin and / or white lignin-polysaccharide copolymer in the solution or dispersion is preferably 0.01 mg / mL or more, more preferably 0.02 mg / mL or more, even more preferably 0.05 mg / mL or more, even more preferably 0.1 mg / mL or more, still more preferably 0.2 mg / mL or more, and particularly preferably 0.3 mg / mL or more, from the viewpoint of the efficiency of forming the structured product 1. The upper limit of the concentration is not particularly limited, but may be, for example, 100 mg / mL, 70 mg / mL, 50 mg / mL, 30 mg / mL, 20 mg / mL, or 15 mg / mL.
[0177] The method for reducing the solvent from the solution or dispersion is not particularly limited as long as it allows the formation of a complex, but particularly preferred is a method that involves a cooling step and a decompression step, such as freeze-drying.
[0178] Structured Product 1 has excellent applicability as a pharmaceutical preparation.
[0179] In the present invention, we have found that structured material 1 forms a network structure and undergoes sol / gel transformation. Examples of sol / gels include hydrosol / gels and organosol / gels. Sol / gels can be formed by mixing white lignin and / or white lignin-polysaccharide copolymers with a crosslinker or a solution containing a crosslinker (e.g., an aqueous solution) and dissolving or uniformly dispersing them. Sol / gel formation can be optimized by known methods (adjusting the concentration of the constituent components, concentration, temperature control, and pH control). The crosslinker can be either organic or inorganic, but molecules capable of hydrogen bonding or coordination with lignin can also be used. Organic substances containing multiple carboxylic acids, aldehydes, ketones, amines, or ether structures within the molecule, or divalent or higher metal ions, can also be used.
[0180] In one aspect, the present invention utilizes the formation of structured material 1. The present invention relates to an adsorbent, recovery agent, remover, or transporter for metal ions or salts containing the same, which contains white lignin and / or a white lignin-polysaccharide complex. The white lignin and / or the white lignin-polysaccharide complex can be used to adsorb, recover, remove, or transport the metal ions or salts containing the same by forming a complex with the metal ions or salts containing the same.
[0181] Specifically, white lignin and / or white lignin-polysaccharide complexes, these agents, and structured product 1 can be used for, for example, the removal of metal ions in the manufacturing process of pharmaceuticals and foods, bioremediation (removal of heavy metals, water purification, soil purification), protection of metal catalysts, carriers, storage, energy carriers, additives to electrolytes, recovery of precious metals and rare metals, etc.
[0182] In one embodiment, the structurant is a modified or substituted hydroxyl group of white lignin and / or white lignin-polysaccharide copolymer (structurant 2).
[0183] In the present invention, attention is focused on the fact that white lignin and / or white lignin-polysaccharide copolymers are characterized by being linear aromatic polymers with few branched structures and a high content of aryl ether bond units in the molecule, and attention is focused on modifying or substituting the hydroxyl groups of white lignin and / or white lignin-polysaccharide copolymers.
[0184] The modified or substituted hydroxyl groups are those obtained by, for example, oxidizing (carbonylating), halogenating, amminating, boron-modifying, acylating, or crosslinking with other structures the hydroxyl groups (e.g., α-position (secondary hydroxyl groups), γ-position (primary hydroxyl groups), phenolic hydroxyl groups, etc.) of white lignin and / or white lignin-polysaccharide copolymers, and are not particularly limited thereto. In one embodiment of the present invention, structure 2 comprises at least one structure selected from the group consisting of a carbonylated structure, a halogenated structure, an aminated structure, a boron-modified structure, an acylated structure, and a crosslinked structure.
[0185] The structured product 2 (oxidized lignin / lignin-polysaccharide copolymer) containing a carbonyl-modified structure is an important intermediate for complexation, derivatization, functionalization, and crosslinking. Due to the extent of the conjugated system, it exhibits a red color and has the ability to absorb ultraviolet and visible light. By reacting with visible light and a photocatalyst, the ether bond of lignin can be cleaved to produce lignin monomers and lignin dimers.
[0186] The references for the following reactions are as follows: ACS Catalysis 2019 9 (3), 2252-2260 DOI: 10.1021 / acscatal.8b04172, Nature 515, 249-252 (2014).
[0187]
[0188] The structured material 2 (halogenated lignin / lignin-polysaccharide copolymer) containing a halogenated modified structure has improved stability, hydrophobicity, etc. by fluorinating the hydroxyl groups that are the starting points for reactions, ionic bonds, and hydrogen bonds.
[0189] Representative structural units contained in white lignin and white lignin-polysaccharide copolymers are shown below.
[0190]
[0191] Representative structural units contained in the oxidized forms of white lignin and white lignin-polysaccharide copolymer are shown below.
[0192]
[0193] The structural units contained in the oxidized white lignin and white lignin-polysaccharide copolymer are shown below.
[0194]
[0195] Representative structural units contained in fluorides of white lignin and white lignin-polysaccharide copolymers are shown below.
[0196]
[0197] The modification or substitution of hydroxyl groups can be carried out according to known methods for modifying or substituting hydroxyl groups of lignin. In particular, the above-mentioned oxidation (carbonylation), halogenation, amination, boron modification, acylation, and cross-linking with other structures are widely known, and therefore methods according to or similar to these methods can be employed.
[0198] <Value in industrial applications> (Prior art) Gel of a mixture of polysaccharides such as lignin and chitosan https: / / doi.org / 10.1016 / j.msec.2019.04.038 Reaction product with formaldehyde crosslinking agent US4244728A Reaction product with crosslinking agent such as chlorohydrin US4131573A The reaction product with the crosslinking agent is irreversible because the lignin skeleton itself becomes a crosslinked structure.
[0199] (The Present Invention) We have discovered that a structured material can be obtained by non-covalent bonding through an extremely simple process: adding salt or organic acid to lignin alone or lignin polysaccharide copolymers. Because the structured material is not crosslinked by covalent bonds, it can be reversibly restored to its original state, making it a recyclable material. The newly observed infrared absorption spectrum characteristics of the lignin structured material indicate the formation of a partially ordered structure, a self-organization via non-covalent bonding. These characteristics can also be confirmed by Raman and UV spectroscopy. Structured materials with acetate salts exhibit approximately four times the UV-A and UV-B protection of unstructured lignin. This represents the enhanced functionality of lignin as a UV absorber and scatterer. In addition to the cosmetics field, gels have a wide range of applications, including medical applications such as medical gels, electronic materials such as conductors and capacitors, surface processing and treatment applications such as paints and adhesives, and 3D printing materials. Functional gels that respond to stimuli and temperature also have a significant impact on a wide range of industrial fields. What is particularly noteworthy is that the structured material is derived from wood, a natural product, and is not derived from fossil fuels, making it a material that is kind to both people and the earth.
[0200] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples.
[0201] Reference Test Example 1. Isolation of lignin, lignin-polysaccharide copolymer, hemicellulose, cellulose-hemicellulose complex, and cellulose Lignin, lignin-polysaccharide copolymer, hemicellulose, cellulose-hemicellulose complex, and cellulose were isolated from biomass using the M-APA method, the A-APA method, or a method for examining their conditions, and the yield and physical properties of the isolated products were measured. The isolation method of the present invention is a production method that enables highly efficient isolation of soluble lignin, lignin-polysaccharide copolymer, hemicellulose, cellulose-hemicellulose complex, and cellulose from natural polymers in biomass, and includes a step (A) of contacting plant biomass with a solution containing an organic acid and a peracid. Specifically, the method was carried out as follows.
[0202] <Reference Test Example 1-1. Preparation of finely pulverized wood flour> Fine powder (finely pulverized wood flour) with a volume average particle size of 10 μm (1-100 μm) was prepared from wood flour of broad-leaved trees (eucalyptus or beech), conifers (red pine, cedar, or cypress), or herbs (bagasse (sugarcane) or bamboo) using a ball mill or bead mill method. Powder of Moso bamboo (3-year-old, produced in Fukuoka Prefecture, Kyushu) was used as the bamboo.
[0203] An example of a preparation method using a ball mill is shown below. A planetary ball mill (P-6, Fritsch) was used. 2 g of wood flour and 100 g of 3 mm diameter zirconia beads were placed in an 80 cc agate container and sealed in a twin overpot. After evacuating the overpot for 20 minutes, inert nitrogen gas was injected. One cycle consisted of 1 minute of milling followed by a 1 minute 20 second pause, and the milling was carried out for 180 cycles at 550 rpm (a total of 3 hours). These conditions allowed for the production of finely powdered wood flour while suppressing oxidation and heat-induced degradation during milling.
[0204] Reference Test Example 1-2. Preparation of wood flour In two pots, left and right, of a mixer mill (MM301, manufactured by Retsch), 1 g each of wood flour or wood chips (10 mm x 10 mm x 1 mm) from a broadleaf tree (eucalyptus or beech), a conifer (red pine, cedar, or cypress), or a herbaceous plant (bagasse (sugar cane) or bamboo) was placed and ground for a grinding time of 5 minutes at a frequency of 1 / 15 seconds, yielding a powder (wood flour) with a volume average particle size of 0.1 mm.
[0205] Reference Test Example 1-3. M-APA (Milling-Acid-PerAcid) Method The starting material was the finely ground wood flour (average particle size 10 μm) obtained in Reference Test Example 1-1. 2 g of finely ground wood flour and 10 mL of an acetic acid-peracetic acid solution (composition: 17.4 M acetic acid (99%), 0.14 M peracetic acid (slightly less than 1%), 0.01 M hydrogen peroxide, and trace amounts of water) were placed in an initiator vial and microwaved for 10 min using a Biotage Initiator+ 60 microwave synthesizer at 50°C, initial power 400 W, and stirring speed 600 rpm. After microwave treatment, the soluble fraction was separated by adding 10 mL of separation solvent (acetone) and spinning down (RCF 8000 xg, 5 min). The insoluble fraction was extracted with 10 mL of separation solvent (acetone) and washed three times, and then combined with the soluble fraction. This soluble lignin is called acid peroxyacid lignin (APA lignin).
[0206] The insoluble fraction was subjected to the same extraction procedure as the second step, but the microwave heating conditions were changed to 140°C. The soluble fraction was identified as a lignin-hemicellulose copolymer. The insoluble fraction was obtained as a cellulose-based copolymer.
[0207] <Reference Test Example 1-4. A-APA Method (Alkali-Acid-PerAcid Method)> The wood flour (average particle size 0.1 mm) obtained in Reference Test Example 1-2 was used as the starting material. A 0.25 M sodium hydroxide solution was prepared (1N diluted 4 times). 2.4 mL of 0.25 M sodium hydroxide solution was added to 0.3 g of wood flour, and microwave extraction was performed (100°C, 30 min). The required amount of alkali is approximately 1 mmol of NaOH per 1 g of wood flour.
[0208] After microwave treatment, the soluble and insoluble fractions can be easily separated by decantation, spin-down, or filtration. An additional three rounds of acetone (separation solvent) extraction were performed and combined with the soluble fraction. The insoluble fraction was extracted using the same extraction method as the M-APA method in Reference Test Example 1-3 to obtain soluble lignin: acid peroxide lignin (APA lignin) and lignin-hemicellulose copolymer. The insoluble fraction was composed primarily of cellulose.
[0209] <Reference Test Example 1-5. Conditions> Studies were conducted using other organic acids (formic acid, glyoxylic acid) instead of acetic acid. Furthermore, studies were conducted using other peracids (hydrogen peroxide) instead of peracetic acid. When other peracids (hydrogen peroxide) were used, the composition was 12M acetic acid, and the hydrogen peroxide concentration was the concentration shown in the table below.
[0210] The contact temperature between plant biomass or insoluble matter and organic acid + peracid was varied from room temperature to 180°C. In addition, the heating method used was an external heating method using an oil bath, instead of an internal heating method using microwaves.
[0211] <Reference Test Example 1-6. Analysis and Measurement Methods> Lignin, lignin-polysaccharide copolymer, and cellulose were analyzed and measured by the following methods.
[0212] <Reference Test Example 1-6-1. Molecular Weight (Mn, Mw, and Polydispersity) Measurement Method> Molecular weight was determined by size exclusion chromatography (SEC), also known as gel permeation chromatography (GPC). The sample was dissolved in a solution of acetic anhydride and a base (e.g., pyridine) and reacted for 3-6 hours to obtain the acetylated product. This was dissolved in tetrahydrofuran (THF) at a concentration of 2.0 mg / mL and separated by high-performance liquid chromatography (Shimadzu Corporation, high-pressure gradient SEC analysis system). A Tosoh HZ-M column (150 mm x 4.6 mm id, 4 μm, three columns connected in series) was used. Analysis was performed by injecting 10 μL of sample, at a column temperature of 40°C, using tetrahydrofuran (THF) as the mobile phase at a flow rate of 0.35 mL / min. Mass calibration curves were constructed using standard polystyrene, Tosoh PStQuickC (molecular weights (MW) of 2,110,000, 427,000, 37,900, and 5970), pinoresinol (MW 352), and vanillin (MW 152), to determine the weight-average molecular weight (Mw) and number-average molecular weight (Mn) of the samples. Polydispersity was calculated as Mw / Mn.
[0213] <Reference Test Example 1-6-2. Calculation Method for the Composition Ratio of Molecular Bonding Units> Samples were dissolved in deuterated dimethyl sulfoxide (DMSO-d6) to a concentration of 1-10 wt%, and NMR spectra were acquired using a Bruker Avance III 600 MHz NMR instrument equipped with a cryogenic probe. The composition ratio of lignin interunit bonding units was calculated from the signal volume in the HSQC (heteronuclear single-quantum correlation spectroscopy) spectrum. The composition ratio was calculated as the ratio per 100 lignin aromatic rings. The content of ether-type bonding units was estimated from the sum of the integrals of the C-H correlation signals at the β-position (δH / δC = 4.0 ± 0.2 ppm / 85.6 ± 1.2 ppm region, δH / δC = 4.3 ± 0.2 ppm / 83.0 ± 0.7 ppm region). Quantitation in the two-dimensional NMR method was performed by correcting using the TAF method described in the literature (H. Okamura, H. Nishimura, T. Nagata, T. Kigawa, T. Watanabe and M. Katahira, Accurate and molecular-size-tolerant NMR quantitation of diverse components in solution, Scientific Reports, 6, 21742. 2016), and accurate content was calculated.
[0214] <Reference Test Example 1-6-3. Method for calculating the composition ratio of lignin and polysaccharide> The sum of the integral values of the C-H correlation signals at the anomeric position (1st position) of the polysaccharide was calculated by the NMR method described above, and after correction by the TAF method, the ratio was calculated as a ratio per 100 lignin aromatic rings.
[0215] <Reference Test Example 1-6-4. Method for calculating the composition ratio of lignin-polysaccharide copolymerization points> As described above, the sum of the integral values of the C-H correlation signals (LC ether, δH / δC = 4.50 ± 0.15 ppm / 80.1 ± 1 ppm region) and (LC ester, δH / δC = 5.88 ± 0.15 ppm / 74.0 ± 1.5 ppm region) derived from LC α ether and LC α ester bond units was calculated using 2D HSQC NMR. After correction using the TAF method, the ratio was calculated as a ratio per 100 lignin aromatic rings. Note that although the A-APA method hydrolyzes some of the ester bonds upon alkali treatment, it is also possible to obtain LC α ester-type lignin-hemicellulose copolymers.
[0216] <Reference Test Example 1-6-5. Calculation method for yield from raw biomass> After checking the pH of each obtained component using a pH meter or pH test paper or peracid test paper (potassium iodide starch paper), neutralization and peracid quenching were performed as necessary. Neutralization was performed by adding 1N HCl or 1N NaOH in small amounts. Peracid quenching was performed by adding 1M aqueous sodium sulfite solution dropwise. The organic solvent was removed using an evaporator. A dry powder was then obtained by freeze-drying. If salts were generated by neutralization, the concentrated solution after organic solvent removal was re-extracted with a separation solvent (acetone) for desalting. The solvent was then removed again using an evaporator, and a dry powder was obtained by freeze-drying. Each obtained component was weighed, and the yield per raw biomass was calculated.
[0217] <Results> The molecular structure, molecular weight, and yield of the obtained polymer are desirable under the following conditions. The results are shown in Tables 1 to 7.
[0218] Table 1 shows the peracid conditions in the two-stage microwave extraction reaction of the M-APA method and the yields of each polymeric lignocellulose component (weight %, raw material biomass ratio, raw material is eucalyptus).
[0219]
[0220] Table 2 shows the yields (wt %, ratio to raw material biomass) of each polymeric lignocellulose component of various biomass in the A-APA method two-stage microwave extraction reaction.
[0221]
[0222] Table 3 shows the peracid conditions in the two-stage microwave extraction reaction of the M-APA method and the molecular weights of each component of high molecular weight lignocellulose (acetylated GPC analysis values).
[0223]
[0224] Table 4 shows the yields (wt %, ratio to raw material biomass) of each polymeric lignocellulose component of various biomass in the two-stage microwave extraction reaction of the M-APA method.
[0225]
[0226] Solvent: Acetic acid (containing 1% peracetic acid, 0.14 mol / L) Microwave extraction conditions: 50°C, 10 min (first stage) to obtain APA lignin soluble fraction, 140°C, 10 min (second stage) to obtain lignin hemicellulose copolymer Table 5 shows the yields (wt%, ratio of raw biomass) of each polymeric lignocellulose component of various biomass in the A-APA method one-stage microwave extraction reaction.
[0227]
[0228] Table 6 shows the molecular weights (acetylated GPC analysis values) of each component of high molecular weight lignocellulose obtained from various biomass materials by the A-APA method.
[0229]
[0230] As a result of examining the conditions, it was found that when the starting material is woody biomass, a contact temperature of 40 to 90°C with organic acid and peracid is suitable for obtaining soluble lignin, and a contact temperature of 100 to 160°C is suitable for obtaining lignin-hemicellulose copolymer.Furthermore, as a result of examining the conditions, it was found that when the starting material is herbaceous biomass, a contact temperature of room temperature to 60°C is suitable for obtaining soluble lignin, and a contact temperature of 70 to 150°C is suitable for obtaining lignin-hemicellulose copolymer.
[0231] As a result of examining the conditions, it was found that the heating time by microwave irradiation is 5-30 min, preferably 10 min. The net irradiation time is short. See Figure 2 for the microwave profile, temperature, and pressure data.
[0232] As a result of examining the conditions, it was found that microwave heating had higher yield and selectivity than external heating under conditions of low temperature, short time, and low energy input. In other words, the microwave effects of local heating, internal heating, electron transfer, and drug penetration promotion were confirmed.
[0233] As a result of examining the conditions, lignin could be isolated using all of the organic acids, acetic acid, formic acid, and glyoxylic acid, but acetic acid was the most suitable from the standpoints of yield, purity, and industrial application.
[0234] The NMR results for Reference Test Examples 1-6-2 and 1-6-3 are shown in Figure 3. Figure 3 shows the analysis results for lignin isolated by the M-APA method (microwave treatment at 50°C for 10 minutes, acetic acid and peracetic acid 1% conditions) using eucalyptus as the starting material. The proportion of lignocellulose interunit bonds was quantified using TAF-NMR, revealing that 99% of the signals were derived from lignin and 1% from polysaccharides (hemicellulose). The breakdown of lignin interunit bonds was 81% ether-type β-O-4, 5% β-5, 11% β-β, 1% dibenzodioxocine, and 1% other. See Figure 4 for partial chemical structures of lignin interunit bonds and lignin-hemicellulose covalent bonds.
[0235] The NMR results for Reference Test Example 1-6-4 are shown in Figure 5. Figure 5 shows the analysis results for lignin-hemicellulose copolymers isolated by the M-APA method (microwave treatment at 50°C for 10 minutes, acetic acid peracetic acid 1% condition) using each plant as the starting material. LC bonds (ether and ester types), shown by circles in the figure, are the main branched structures present in proportions equal to or greater than the β-5 and β-β bonds, which are the main interunit bonds of lignin. The isolated lignin-hemicellulose copolymers are characterized by the presence of LCα-ester type bonds in particular.
[0236] Reference Test Example 2: Solubility Measurement The solubility of lignin and lignin-hemicellulose copolymers obtained by the method of Reference Test Example 1 or a method similar thereto was measured in 60-80% ethanol at 25°C. Details of the measured samples are shown in Table 7. The abbreviations in Table 7 are explained as follows: PA: Peracetic acid (peracetic acid), HP: Hydrogen Peroxide, 50: MW50 ACTN, microwave-treated at 50°C, high-quality polymeric lignin, 140: MW50-MW140 ACTN, residue after microwave-treated at 50°C, second-stage treatment at 140°C, lignin-hemicellulose copolymer, A50: Acetic acid-peracetic acid system, HP, PA 1% AA, Mw50 ACN, microwave-treated at 50°C, high-quality polymeric lignin, H50: Acetic acid-hydrogen peroxide system, HP, 1M hydrogen peroxide, Mw50 ACN, microwave-treated at 50°C, high-quality polymeric lignin.
[0237]
[0238] The solubility was measured as follows. The sample was dissolved in 25°C ethanol by stirring, and then separated into ethanol-soluble and ethanol-insoluble portions by solid-liquid separation. A 25°C aqueous ethanol solution (1 / 1 ethanol / water) was added to the ethanol-insoluble portion and stirred to dissolve, obtaining an aqueous ethanol-soluble portion. The aqueous ethanol-soluble portion was mixed with the ethanol-soluble portion to obtain a sample solution. The amount of aqueous ethanol added was adjusted so that the ethanol concentration of the sample solution was in the range of 60-80%. In the process of obtaining the soluble portion, dispersion and solubilization were performed using an ultrasonic cleaner at 28 kHz for 3 min, as needed. The maximum sample concentration at which the sample solution became visually transparent was defined as the "solubility in 60-80% ethanol at 25°C."
[0239] The results are shown in Table 8. It was found that the lignin and lignin-hemicellulose copolymer obtained by the method of the present invention exhibited good ethanol solubility.
[0240]
[0241] Test Example 1. Production of White Lignin 1 White lignin was produced by treating biomass with alkali, washing the resulting alkali-treated product with a liquid, and treating the washed product by the APA method. Specifically, the procedure was as follows.
[0242] The following were used for the measurements: Analysis software included with each device was used for analysis.
[0243] UV-Visible absorption spectra: Shimadzu UV-2700 spectrophotometer. A black quartz cell (light path length: 10 mm) or a High Precision Cell, Art. No Light Path, 10 x 10 mm, was used. Lignin microparticle samples were diluted with 30% EtOH aq to a final lignin concentration of 0.005 w / v%. Wavelength scans (200-900 nm, 250-600 nm) were performed.
[0244] Fluorescence spectrum: Spectrofluorometer RF-6000 (Shimadzu Corporation). Fluorescence measurement: A fully transparent synthetic quartz cell (optical path length: 10 mm) and a Starna triangular quartz cell SF3 were used. The lignin microparticle sample was diluted with 30 v / v% EtOH aq to a final lignin concentration of 0.005 w / v%.
[0245] The 3D fluorescence spectrum was measured at an excitation wavelength of 240-650 nm with a data interval of 2 nm, an emission wavelength of 240-650 nm with a data interval of 2 nm, a scan speed of 6000 nm / min, and a UV cut filter U310 attached to the excitation side to reduce the effects of scattered light and multi-order light. The bandwidth was 10 nm on the excitation side and 20 nm on the emission side, and the sensitivity was set to Low.
[0246] Fluorescence microscope measurement: An all-in-one fluorescence microscope BZ-X810 (Keyence) was used.
[0247] Particle size distribution (DLS) and zeta potential measurements were performed using a DLS dynamic light scattering nanoparticle measurement device SZ-100 (Horiba, Ltd.). Samples were placed in a particle size measurement cell and a zeta potential measurement cell (Horiba, Ltd.), and measurements were performed. Measurements were repeated 3-5 times, and the average value was calculated.
[0248] Particle size distribution measurements were performed using the qNano Gold TRPS Measurement System (Meiwafosis, Izon Science). Measurements were performed using a nanopore NP200 or NP400, with 35 μL of sample added. Measurements were performed for 30 seconds or more, up to 500-1000 particle counts.
[0249] The pore stretch was set to 37.00 mm, and the voltage was measured at a constant voltage of 2.0 V.
[0250] Test Example 1-1. Preparation of wood flour 1 g each of wood flour or wood chips (10 mm x 10 mm x 2 mm) from a broadleaf tree (eucalyptus), a conifer (Japanese red pine, cedar, or cypress), or a herbaceous plant (bagasse (sugar cane) or bamboo) was placed in two pots, one on each side, of a mixer mill (MM301, manufactured by Retsch), and milling was carried out under the conditions of a milling time of 5 minutes and a frequency of 1 / 15 seconds, to obtain a powder (wood flour) with a volume average particle size of 0.1 mm.
[0251] Test Example 1-2. Alkali Treatment, Washing, and APA Method Treatment Example 1: 14.4 mL of 0.25 M aqueous sodium hydroxide was added to 1.8 g of eucalyptus wood flour obtained in Test Example 1-1 in a container. The container was immersed in a 60°C water bath and treated for 1 hour. After the water bath treatment, the mixture was spun down to separate the soluble and insoluble portions, and the insoluble portion was washed with water. The water washing was continued until the washing waste liquid became neutral. The resulting washed material (containing 6.5 mL of water) and an acetic acid-hydrogen peroxide-containing solution (14.1 mL of 99% acetic acid (17.1 M) and 0.294 mL of 30% v / v hydrogen peroxide solution) were placed in an initiator vial and microwave-treated for 10 minutes using a Biotage Initiator+ 60 microwave synthesizer at 50°C, initial power 400 W, and stirring speed 600 rpm. After irradiation, 14.4 mL of separation solvent 1 (70% aqueous ethanol) was added, mixed, and then spun down (RCF 10,000 × g, 5 min) to recover the soluble portion (supernatant). The solvent from the soluble portion was evaporated, and 6 mL of separation solvent 2 (80% aqueous dioxane) was added to the resulting dried product, mixed, and then spun down (RCF 10,000 × g, 5 min) to recover the soluble portion (supernatant). This soluble portion was dried to obtain 58 mg of white lignin powder.
[0252] Example 2: The same procedure as in Example 1 was repeated, except that ultrasonic treatment was used instead of hot water bath treatment in the alkali treatment, to obtain 113 mg of white lignin powder. For the ultrasonic treatment, 1.8 g of the eucalyptus wood flour obtained in Test Example 1-1 was placed in a container with 14.4 mL of 0.25 M sodium hydroxide solution, and the mixture was irradiated intermittently with 28 kHz ultrasonic waves for 30 minutes using an ultrasonic irradiation device (manufactured by AS ONE, product name: ULTRASONIC CLEANER MODEL VS-100III). During this time, the liquid temperature was maintained at 30-50°C.
[0253] Example 3: 47 mg of white lignin powder was obtained in the same manner as in Example 1, except that 0.1 M sodium hydroxide solution was used instead of 0.25 M sodium hydroxide solution in the alkali treatment and microwave treatment was performed instead of water bath treatment in the alkali treatment. For the microwave treatment, 14.4 mL of 0.25 M sodium hydroxide solution was placed in an initiator vial for 1.8 g of the eucalyptus wood flour obtained in Test Example 1-1, and microwave irradiation was performed for 30 minutes using a Biotage Initiator+ 60 microwave synthesizer under conditions of 40°C, initial power 400 W, and stirring speed 600 rpm.
[0254] Example 4 The same procedure as in Example 2 was carried out except that cypress wood flour (Test Example 1-1) was used instead of eucalyptus wood flour, and 29 mg of white lignin powder was obtained.
[0255] (Example 5) The same procedure as in Example 1 was repeated, except that in the alkali treatment, 0.1 M aqueous sodium hydroxide solution was used instead of 0.25 M aqueous sodium hydroxide solution, and in the alkali treatment, water bath treatment at 30°C for 30 minutes was performed instead of water bath treatment at 60°C for 1 hour, to obtain 56 mg of white lignin powder.
[0256] Example 6 The same procedure as in Example 1 was carried out, except that in the alkali treatment, the water bath treatment at 30°C for 30 minutes was performed instead of the water bath treatment at 60°C for 1 hour, and 63 mg of white lignin powder was obtained.
[0257] Example 7 The same procedure as in Example 2 was carried out except that a 0.1 M aqueous sodium hydroxide solution was used in place of the 0.25 M aqueous sodium hydroxide solution in the alkali treatment, and 47 mg of white lignin powder was obtained.
[0258] Example 8 The same procedure as in Example 3 was carried out except that in the alkali treatment, a 0.25 M aqueous solution of sodium hydroxide was used instead of a 0.1 M aqueous solution of sodium hydroxide, to obtain 80 mg of white lignin powder.
[0259] Example 9 The same procedure as in Example 2 was carried out except that in the APA treatment, an acetic acid stock solution (17.5 M) was used instead of the acetic acid-hydrogen peroxide-containing solution, and 46 mg of white lignin powder was obtained.
[0260] Example 10: The procedure of Example 2 was repeated except that the washed material obtained after the alkali treatment in the APA method (containing 6.5 mL of water) and an acetic acid-hydrogen peroxide solution (14.1 mL of 99% (17.1 M) acetic acid and 0.029 mL of 30% v / v hydrogen peroxide) were used to obtain 53 mg of white lignin powder (final concentrations: acetic acid / hydrogen peroxide / water = 68% / 0.048% / 31.6%).
[0261] Example 11 The same procedure as in Example 1 was carried out, except that in the alkali treatment, the water bath treatment at 30°C for 10 minutes was performed instead of the water bath treatment at 60°C for 1 hour, and 37 mg of white lignin powder was obtained.
[0262] Example 12: When separating the soluble and insoluble fractions in the alkali and APA treatments, suction filtration was used instead of spinning down. The procedure was the same as in Example 2, except that the washed material obtained after the alkali treatment (containing 1.9 mL of water) was replaced with an acetic acid-hydrogen peroxide solution (14.1 mL of 99% (17.1 M) acetic acid and 0.29 mL of 30% v / v hydrogen peroxide solution). This yielded 24 mg of white lignin powder. (Final concentrations were acetic acid / hydrogen peroxide / water = 86.5% / 0.613% / 12.8%). For the ultrasonic treatment in the alkali treatment, an AS ONE ultrasonic cleaner MCD-10P was used instead of an AS ONE Ultrasonic Cleaner Model VS-100III. 28 kHz ultrasonic waves were applied intermittently for 30 minutes. The liquid temperature remained at 30-50°C.
[0263] Example 13 The same procedures as in Example 12 were carried out except that in the alkali treatment and APA treatment, acetone was used instead of the 70% aqueous ethanol solution as the separation solvent 1, to obtain 51 mg of a white lignin powder.
[0264] (Example 14) The same procedure as in Example 12 was carried out, except that eucalyptus wood flour in the form of Willey mill (sawdust) was prepared on a scale of 1.8 g instead of the eucalyptus wood flour obtained in Test Example 1-1, and 52 mg of white lignin powder was obtained.
[0265] (Example 15) The same procedure as in Example 14 was carried out, except that 2.0 g of Willey mill-like (sawdust-like) cedar wood flour was used instead of the eucalyptus wood flour obtained in Test Example 1-1, and 76 mg of white lignin powder was obtained.
[0266] (Example 16) In the APA treatment, after microwave irradiation, only the acetic acid-hydrogen peroxide-containing solution was collected, neutralized by dialysis, desalted, and then freeze-dried, and the same procedure as in Example 12 was carried out to obtain 22 mg of white lignin powder.
[0267] Example 17: The APA treatment was carried out in the same manner as in Example 12, except that the extraction vessel was replaced with nitrogen, to obtain 51 mg of white lignin powder. Compared to Example 12, the whiteness (increased from 77.6 to 81.9) and yield were improved for the same sample under the same conditions.
[0268] (Example 18) The same procedure as in Example 12 was carried out, except that instead of the eucalyptus wood flour obtained in Test Example 1-1, Willey mill-like (sawdust-like) beech wood flour was prepared on a 2.0 g scale, and 65.5 mg of white lignin powder was obtained.
[0269] (Example 19) The same procedure as in Example 12 was carried out, except that instead of the eucalyptus wood flour obtained in Test Example 1-1, Willey mill-like (sawdust-like) cypress wood flour was prepared on a scale of 2.0 g, and 87.7 mg of white lignin powder was obtained.
[0270] (Example 20) The same procedure as in Example 12 was carried out, except that instead of the eucalyptus wood flour obtained in Test Example 1-1, Willey mill-like (sawdust-like) red pine wood flour was prepared on a 2.0 g scale, and 56.3 mg of white lignin powder was obtained.
[0271] (Example 21) The same procedure as in Example 12 was repeated, except that instead of the eucalyptus wood flour obtained in Test Example 1-1, moso bamboo powder (3 years old, produced in Fukuoka Prefecture, Kyushu) was prepared on a 2.0 g scale, and 67.9 mg of white lignin powder was obtained.
[0272] (Example 22) The same procedure as in Example 12 was carried out, except that instead of the eucalyptus wood flour obtained in Test Example 1-1, Willey mill-like (sawdust-like) rice straw flour was prepared on a 2.0 g scale, and 51.4 mg of white lignin powder was obtained.
[0273] (Example 23) The same procedure as in Example 12 was carried out, except that Willey mill-like (sawdust-like) bagasse flour was prepared on a scale of 2.0 g instead of the eucalyptus wood flour obtained in Test Example 1-1, and 45.8 mg of white lignin powder was obtained.
[0274] Example 24 The same procedure as in Example 20 was carried out, except that in the APA method treatment, water bath treatment was used instead of microwave treatment and heat treatment was performed for 15 minutes instead of 10 minutes, to obtain 51.1 mg of white lignin powder.
[0275] Example 25 The same procedure as in Example 24 was carried out except that Willey milled eucalyptus wood flour was used instead of Willey milled (sawdust-like) red pine wood flour, and 64.9 mg of white lignin powder was obtained.
[0276] (Example 26) The eucalyptus wood flour obtained in Test Example 1-1 was prepared on a scale of 1.8 g, and the APA method treatment was carried out in the same manner as in Example 25, except that after the sample was sealed in an initiator vial, air was introduced through the septum at the top of the vial using a syringe, and the pressure inside the container after sealing was set to 2.25 bar, and 42.18 mg of white lignin powder was obtained.
[0277] Additionally, the APA-treated wood flour was placed in an initiator vial together with the acetic acid-hydrogen peroxide solution shown in Example 1, and heated for 10 minutes using a hot stirrer equipped with a heat block preheated to 140°C. The extraction procedure was carried out in the same manner as in Example 1, yielding 220.7 mg of white LCC powder.
[0278] Example 27 The same procedures as in Example 24 were carried out except that in the alkali treatment, instead of 30 minutes of ultrasonic treatment at 30 to 50°C, 10 minutes of water bath treatment at 23.3 to 26.3°C was carried out, and instead of Willey milled (sawdust-like) red pine wood flour, Willey milled (cypress) wood flour was prepared in a glass container on a 50 g scale, 0.01 M sodium hydroxide aqueous solution was used instead of 0.25 M sodium hydroxide aqueous solution in the alkali treatment, and 17.5 M acetic acid stock solution was used instead of the acetic acid-hydrogen peroxide-containing solution in the APA method treatment, and 1224.9 mg of white lignin powder was obtained.
[0279] (Example 28) The same procedure as in Example 12 was carried out, except that instead of the eucalyptus wood flour obtained in Test Example 1-1, beech wood flour in a 2.0 g scale that had been defatted and depectinated in a Willey mill (sawdust-like) state and had had the extractive components of the raw material removed was used, and 72.5 mg of white lignin powder was obtained.
[0280] (Example 29) Instead of Willey milled (sawdust-like) red pine wood flour, Willey milled eucalyptus wood flour was prepared in a glass container on a 100 g scale, and the APA method treatment was carried out in the same manner as in Example 24, except that water bath treatment was used instead of microwave treatment, water bath treatment was performed for 60 minutes instead of 15 minutes, and pressing was used to separate the treatment solution from the wood flour. 2183.3 mg of white lignin powder was obtained.
[0281] (Example 30) Instead of Willey milled (sawdust-like) red pine wood flour, 100 g of Moso bamboo powder (3-year-old, produced in Fukuoka Prefecture, Kyushu) was prepared in a glass container, and the procedure was repeated as in Example 27, except that a spin-down was used to separate the treatment solution from the wood flour, and 2092.6 mg of white lignin powder was obtained.
[0282] <Test Example 1-3. Measurement of Whiteness> For the white lignin powders obtained in Examples 1 to 17, L*, a*, and b* were measured using a spectrophotometer (CM-R5, manufactured by Konica Minolta). In addition, for the white lignin powders obtained in Examples 6 to 17, L*, a*, and b* were measured using a spectrophotometer (SPECTRO 1, manufactured by Variabl). Based on the measured values, Hunter whiteness (W) was calculated using the following formula: W = 100 - sqr [(100 - L*)^2 + ((a*)^2 + (b*)^2)]. The results are shown in Table 9.
[0283]
[0284] Furthermore, the white lignin obtained in each example was obtained by a method that applied the above-mentioned Reference Test Examples 1 and 2, and therefore, apart from color, has similar physical properties to the lignin obtained in the above-mentioned Reference Test Examples 1 and 2, although there are some differences in solubility.
[0285] Test Example 1-4: Measurement of oxidized lignin ratio and content of β-O-4 ether structure For the white lignin powders of the examples, the content of β-O-4 ether structure was measured according to the method described in the Reference Test Example. Furthermore, the oxidized lignin ratio (ratio of oxidized lignin structures) was measured according to the method described in "Calculation method for oxidized lignin ratio" in the section "2. White lignin." The results are shown in Table 10, along with the measurement results of whiteness W (Test Example 1-3).
[0286]
[0287] *Reference example (M-APA lignin): Eucalyptus wood flour was finely ground in a ball mill, then microwaved in an acetic acid solution containing 3% peracetic acid at 100°C for 10 minutes to extract the lignin. The lignin was brown (whiteness was about 60 based on color comparison).
[0288] The oxidized lignin ratio and ether bond content (converted to per 100 lignin aromatic rings, calculated from the ratio of the corresponding part of the same spectrum in the 2D HSQC NMR spectrum) of white lignin.
[0289] <Test Example 1-5. Measurement of infrared absorption spectrum> For the FT-IR measurement of the white lignin powder in the examples, a PerkinElmer FT-IR device, Spectrum Two Diamond ATR, was used. The measurement range was 400-4000 cm -1 The number of scans was 10. 1800 cm -1 The absorbance at 619 cm -1 The absorbance of the sample was normalized to 1, and then differentiation was performed. The obtained derivative spectra are shown in Figures 21 to 25.
[0290] Test Example 2. Production of white lignin and white lignin-polysaccharide copolymer White lignin and white lignin-polysaccharide copolymer were produced by treating biomass with alkali, washing the resulting alkali-treated product with a liquid, and treating the washed product by the APA method. Specifically, the process was carried out as follows.
[0291] <Test Example 2-1. Preparation of finely ground wood powder> Wood chips of hardwood (eucalyptus) and softwood (cypress) were powdered using a Willey mill (Yoshida Seisakusho, Model 1029-D). The Willey mill powder for eucalyptus was further pulverized using a mixer mill. Powder of Moso bamboo (3-year-old bamboo from Fukuoka Prefecture, Kyushu) was used for the bamboo.
[0292] Test Example 2-2. Preparation of wood flour 1 g of hardwood (eucalyptus) wood flour was placed in each of the two pots on the left and right sides of a mixer mill (MM301, manufactured by Retsch), and milling was carried out under the conditions of a milling time of 5 minutes and a frequency of 1 / 15 seconds, to obtain a powder (wood flour) with a volume average particle size of 0.1 mm.
[0293] Test Example 2-3. Extraction of White Lignin: Wood flour obtained in Test Example 2-1 or 2-2 was used as the starting material. A 0.25 M sodium hydroxide solution was prepared (1 M diluted 4 times). 14.4 mL of 0.25 M sodium hydroxide solution was added to 1.8 g of wood flour, and ultrasonic irradiation was performed using an ultrasonic cleaner (MCD-10P, manufactured by AS ONE). The frequency was 28 kHz, and the irradiation time was 30 minutes. During irradiation, the water in the washing tank was cooled using an immersion chiller (ECS-0, manufactured by Tokyo Rika) to prevent the water temperature from rising.
[0294] After sonication, the solution and wood flour were separated by filtration, and the wood flour was washed with purified water. The washed wood flour and 14.4 mL of acetic acid (Fujifilm Wako Pure Chemical Industries, special grade) or acetic acid-hydrogen peroxide solution (Santoku Chemical Industry, 31% hydrogen peroxide solution (specific gravity 1.11) 0.294 mL = 0.612% = 0.2 M, acetic acid 14.106 mL) were placed in an initiator vial and microwaved for 10 minutes using a Biotage Initiator EXP microwave synthesizer at 50 °C, initial power 400 W, and stirring speed 600-900 rpm. After microwave treatment, the wood flour and solution were separated by filtration, and the wood flour was washed three times with 14.4 mL of 70% (v / v) ethanol solution. The filtered solution and washings were combined and the solvent removed using a rotary evaporator. If the resulting dried product gave off an acetic acid odor, 70% (v / v) ethanol solution was added, washed, and the solvent was evaporated in an evaporator until the product was dry. The resulting dried product was designated "white lignin." If necessary, the dried product was dissolved in 80% (v / v) dioxane solution (dioxane: Fujifilm Wako Pure Chemical Industries, Ltd.), frozen, and then freeze-dried.
[0295] In these test examples, the atmosphere was normal pressure unless otherwise specified, and when pressurized, the sample was sealed in an initiator vial, and then air was introduced through the septum at the top of the vial with a syringe. After sealing, the pressure inside the container was 2.25 bar.
[0296] Instead of the microwave treatment described above, when heating and stirring were performed, heating was performed using a hot stirrer. The initiator vial containing the sample was placed in a heat block, and the heat block was heated with a hot stirrer to obtain the required extraction temperature.
[0297] Test Example 2-4. Extraction of White Lignin-Polysaccharide Copolymer (LCC) The wood flour from Test Example 2-3 after acetic acid treatment was collected and 14.4 mL of acetic acid (Fujifilm Wako Pure Chemical Industries, special grade) or acetic acid-hydrogen peroxide mixed solution (Santoku Chemical Industry, 0.1294 mL of 31% hydrogen peroxide, 14.106 mL of acetic acid) was placed in an initiator vial. The mixture was microwaved for 1 or 10 minutes using a Biotage Initiator EXP microwave synthesizer at 120-140°C, initial power of 400 W, and stirring speed of 600-900 rpm. After microwave treatment, the soluble fraction was separated from the wood flour and solution by filtration. The wood flour was washed three times with 14.4 mL of 70% (v / v) ethanol solution. The filtered solution and washings were combined and the solvent was removed using a rotary evaporator. If the resulting dried product gave off an acetic acid odor, 70% (v / v) aqueous ethanol was added, washed, and the solvent was evaporated to dryness using an evaporator. The resulting dried product was designated "white LCC." If necessary, the dried product was dissolved in 80% (v / v) aqueous dioxane, frozen, and then lyophilized.
[0298] In this test example, the atmosphere was air unless otherwise specified, and when an argon atmosphere was specified, the initiator vial containing the sample was purged with argon gas before being sealed prior to microwave treatment.
[0299] Instead of the microwave treatment described above, when heating and stirring were performed, heating was performed using a hot stirrer. The initiator vial containing the sample was placed in a heat block, and the heat block was heated with a hot stirrer to obtain the required extraction temperature.
[0300] The whiteness of the white lignin (Test Example 2-3) and the whiteness of the white lignin-polysaccharide copolymer (white LCC: Test Example 2-4) are shown in Table 9. The measurement method was the same as in Test Example 1. The oxidized lignin ratio and ether bond content (converted to per 100 lignin aromatic rings, calculated from the ratio of the corresponding part of the same spectrum in the 2D HSQC NMR spectrum) of the white lignin were measured.
[0301] Example 31 The procedure of Example 9 was repeated except that filtration was used to separate the treatment solution from the wood flour, yielding 39.3 mg of white lignin powder.
[0302] In addition, the same procedure as in Example 26 was carried out on the AAPA-treated wood flour, except that acetic acid stock solution (17.5 M) was used instead of the acetic acid-hydrogen peroxide-containing solution in the treatment at 140°C, thereby obtaining 279.2 mg of white LCC powder.
[0303] (Example 32) In the APA treatment, the same procedure as in Example 31 was carried out except that an acetic acid-hydrogen peroxide-containing solution was used instead of the acetic acid stock solution (17.5 M), and microwave treatment at 140°C for 1 minute was performed instead of microwave treatment at 140°C for 10 minutes, thereby obtaining 51.3 mg of white lignin powder and 259.79 mg of white LCC powder.
[0304] (Example 33) Instead of the Willey mill-like (sawdust-like) eucalyptus wood flour, moso bamboo powder (3 years old, produced in Fukuoka Prefecture, Kyushu) was used, and the APA treatment was carried out in the same manner as in Example 31, except that the atmosphere was replaced with argon gas and the microwave treatment was carried out at 120°C for 1 minute instead of at 140°C for 10 minutes. As a result, 59.1 mg of white lignin powder and 49.9 mg of white LCC powder were obtained.
[0305] (Example 34) The same procedure as in Example 31 was carried out except that cypress wood flour was used instead of Willey mill-like (sawdust-like) eucalyptus wood flour, the atmosphere in the APA treatment was replaced with argon gas, and microwave treatment was performed at 130°C for 1 minute instead of at 140°C for 10 minutes, thereby obtaining 67.7 mg of white lignin powder and 29.6 mg of white LCC powder.
[0306] Test Example 3. Production of Self-Assembled Bodies (Hollow Spherical Particles) A white lignin sample was dissolved in DMSO to prepare a 10 w / v % DMSO solution, and water, a poor solvent, was gradually added to produce microparticles. During dissolution, a dispersion treatment was performed using ultrasonic irradiation. For NMR measurement samples, a 1:1:8 DMSO-d6:Ethanol-d6:D2O solvent was used. In experiments involving the inclusion of drugs, pigments, etc., the compound to be incorpo-rated was pre-dissolved in DMSO or ethanol, and this was mixed with white lignin or white LCC to produce microparticles using the same method as described above. Measurement results, such as particle size, are shown in Table 11.
[0307]
[0308] Test Example 4. Solubility Measurements. The NMR-DMSO standard solubility index was calculated. Lignin samples were dissolved in DMSO-d6 at a concentration of 2 w / v%, and quantitative 1H NMR measurements were performed. The integral value of the aromatic region of the NMR spectrum (6-8 ppm) was normalized to 100. Dissolution and measurement were performed under the same conditions. The integral values of the spectra of samples dissolved in deuterated acetic acid and deuterated ethanol were normalized to the deuterated DMSO condition to calculate the index. The measurement temperature was 313 K for deuterated DMSO solvent and 298 K for the others. White lignin (derived from bamboo) had an index of 115 in deuterated acetic acid and an index of 68 in deuterated ethanol. White lignin (derived from eucalyptus) had an index of 104 in deuterated acetic acid and an index of over 60 in deuterated ethanol. On the other hand, eucalyptus MWL (ground lignin) had an index of 27 in deuterated acetic acid and an index of less than 20 in deuterated ethanol. The cedar MWL (ground lignin) had an index of 41 in deuterated acetic acid and an index of less than 25 in deuterated ethanol.
[0309] Test Example 5. Preparation of structured product 1 <5-1. Preparation of white lignin-sodium acetate complex> 5 mg of eucalyptus-derived white lignin was dissolved in 500 μL to 1000 μL of acetic acid (special grade, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). 5 to 45 mg of sodium acetate (anhydrate, special grade, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was then added and completely dissolved. The resulting solution was freeze-dried to obtain a complex.
[0310] 5-2. Preparation of White Lignin-Salt Complex Eucalyptus-derived white lignin was dissolved in dimethyl sulfoxide (DMSO) at a concentration of 10 mg / mL. Separately, aqueous solutions containing glycine (Nacalai Tesque, biotechnology grade), citric acid monohydrate (hereafter referred to as Fujifilm Wako Pure Chemical Industries, special grade), L(+)-tartaric acid, sodium chloride, zinc chloride, sodium acetate (anhydrous), sodium acetate trihydrate, or ammonium acetate were prepared at a concentration of 5 mg / mL. 400 μL of the lignin-dimethyl sulfoxide solution was mixed with 8 mL of the aqueous solution, and the mixture was freeze-dried to obtain the complex.
[0311] <5-3. Complex Purification Method> The formed complex can be purified by washing with chilled acetone or ethanol (which do not dissolve the complex itself). 1 mL of chilled acetone was added to 10 mg of complex, and the supernatant was collected after spinning down. This process was repeated three times. This yielded a complex from which impurities attached to the surface and lignin that did not form a complex had been removed.
[0312] 5-4. Obtaining infrared absorption spectra A PerkinElmer FT-IR Spectrum Two Diamond ATR was used for FT-IR measurements of the samples. The measurement range was 400-4000 cm-1, and the number of scans was 10. The spectra were subjected to ATR correction, normalized to the absorbance at the wavenumber where the absorbance was maximum between 4000 and 400 cm-1 as 1, and then differentiated.
[0313] 5-5. Results When glycine, sodium chloride, sodium acetate (anhydrous), and sodium acetate trihydrate were used, solid (powder) products were obtained after freeze-drying. On the other hand, when citric acid monohydrate, L(+)-tartaric acid, and zinc chloride were used, gel-like products were obtained after freeze-drying (Figure 10).
[0314] The gelation inducers (citric acid monohydrate, L(+)-tartaric acid, and zinc chloride) are highly soluble in DMSO (zinc chloride is slightly soluble and forms a suspension). The non-gelation inducers are poorly soluble in DMSO (they settle as a precipitate).
[0315] In the differential form (first derivative spectrum) of the infrared absorption spectrum of the white lignin-sodium acetate complex, new peaks were observed that were not seen in white lignin alone or sodium acetate alone, confirming the formation of a complex structure (see Figures 12 to 16 for examples). Regardless of the tree species and the organic acids and salts that form the complex, the following wavenumber range was observed: 1080-950 cm -1 1480-1350 cm -1 3000-2900 cm -1 A new peak was observed.
[0316] In the middle panel of Figure 15, the spectrum attributed to zinc chloride disappears in the complex. In this example, the complex was formed at a weight ratio of lignin to zinc chloride of 2:1. This demonstrates the ability of the present invention to efficiently coordinate and adsorb with lignin and metal ions.
[0317] 5-6. Absorbance Measurement The absorbance of the white lignin-sodium acetate complex of Test Example 5-1 was measured by the diffuse reflectance method using a spectrophotometer (Shimadzu Corporation, UV-2700) and an integrating sphere unit (Shimadzu Corporation, ISR-2600). The powdered sample was filled into a dedicated holder and measured. A baseline was obtained using barium sulfate (Nacalai Tesque), and the scan speed was medium. The resulting reflectance spectrum is shown in Figure 9. The spectrum was normalized by the weight of lignin. Compared to lignin alone, the complex exhibited significantly increased absorption. Absorption in the UV-B region (280-320 nm) increased by 4.3 times, and in the UV-A region (320-400 nm) by 3.7 times.
[0318] <5-7. Raman Spectroscopic Measurement> Raman spectra were measured using a Nanophoton laser Raman microscope RAMANtouch under the conditions of an excitation wavelength of 785 nm, an objective lens of 10x, and 0.30 NA. 1 mg of sample was applied as a thin film on a glass slide, and Raman spectroscopy was performed. The results are shown in Figure 11. The wavenumber range (1200 - 1400 cm) indicated by the dashed circle in the figure was -1 ) and detected characteristic peaks resulting from the complexation.
[0319] Test Example 6. Production of structured product 2 <6-1. Synthesis of oxidized lignin A>
[0320]
[0321] A white lignin sample (20 mg) was dissolved and dispersed in 3 mL of CH3CN, and 10 mg of Bobbitt's Salt (4-(Acetylamino)-2,2,6,6-tetramethyl-1-oxo-piperidinium tetrafluoroborate, 745537 Sigma-Aldrich) was added and the mixture was vigorously stirred at room temperature. After 10 hours (overnight), the mixture was purified by solid-phase extraction (Waters Oasis HLB, 6 cc) to obtain oxidized lignin A. 2D HSQC NMR confirmed that the desired product had been obtained (Figure 17).
[0322] 6-2. Synthesis of Oxidized Lignin B: A white lignin sample (383 mg) was added with 30 mg of catalyst MoO2Cl2(DMSO)2 and then dissolved in 8 mL of DMSO. The solution was microwave-heated (160 °C, 10 min), then ethyl acetate was added. The DMSO was removed by washing with brine and then water. The solution was dried over sodium sulfate and concentrated to obtain oxidized lignin B (391 mg). 2D HSQC NMR and C-NMR confirmed that the desired product was obtained (Figure 18).
[0323] <6-3. Reductive Amination of Oxidized Lignin B> Oxidized lignin B (235 mg) was dissolved in 2.5 mL of methanol, containing 495 mg of ammonium formate as an aminating agent, 199 μL of acetic acid as a reactant, and 5 mg of chloro[4-(dimethylamino)-N-(dimethylamino)pheny-2-pyridinecarboxamidato](pentamethylcyclopentadienyl)iridium(III) (Ir-PA2) as a catalyst. The mixture was then refluxed at 70 °C for 3 hours under argon gas. The reaction solution was returned to room temperature, and 1 M sodium hydroxide solution (2 mL) was added to terminate the reaction. Ethyl acetate was then added to precipitate the insoluble material. The ethyl acetate-soluble portion, which was the unreacted material, and the precipitated insoluble material, which was the aminated product, were both washed twice with water to remove the water-soluble components. The insoluble material was recovered, ethyl acetate was added, and the mixture was precipitated by simple centrifugation to obtain aminated lignin (85 mg). 2D HSQC NMR confirmed that the target product had been obtained.
[0324] 6-4. Synthesis of Oxidized Lignin C: A white lignin sample (20 mg) was dissolved and dispersed in 0.7 mL of DMSO, and 1 mg of Palladium(II) Acetate (Fujifilm Wako SG) was added and vigorously stirred at 60°C. After 18 hours (overnight), the mixture was concentrated by nitrogen gas spraying and purified by solid-phase extraction (Waters Oasis HLB, 6 cc) to obtain oxidized lignin C. 13C NMR and 2D HSQC NMR confirmed that the target product had been obtained (Figure 19).
[0325] 6-5. Synthesis of Halogenated Lignin F1: A white lignin sample (20 mg) was dissolved in 1 mL of 1,4-dioxane (Wako, dehydrated type 040-31651). 10 mg of PyFluor (Pyridine-2-sulfonyl Fluoride, B0440 Sigma-Aldrich) and 0.1 mL of N,N-Diisopropylethylamine (DIPEA) (TCI, D1599) were added, and the mixture was stirred at 80°C for 10 hours. The mixture was concentrated by nitrogen gas injection and purified by solid-phase extraction (Waters Oasis HLB, 6 cc) to obtain halogenated lignin F1. 2D HSQC NMR and 19F NMR confirmed the desired product (Figure 20).
[0326] 6-6. Synthesis of Halogenated Lignin F2: A white lignin sample (20 mg) was dissolved in 1 mL of 1,4-dioxane (Fujifilm Wako, dehydrated type 040-31651), and 10 mg of XtraFluor-M (Product No. 719447, Sigma-Aldrich) and 0.1 mL of N,N-Diisopropylethylamine (DIPEA) (TCI, D1599) were added. The mixture was stirred at 80°C for 10 hours. The mixture was concentrated by nitrogen gas injection and purified by solid-phase extraction (Waters Oasis HLB, 6 cc) to obtain halogenated lignin F2. The desired product was confirmed by 2D HSQC NMR and 19F NMR.
[0327] Test Example 7. Production of Structured Product 3 Using white lignin derived from bamboo or cypress, a composite was produced and purified in the same manner as in Test Example 5, and an infrared absorption spectrum was obtained. The first derivative infrared absorption spectra of the composite are shown in Figures 26 to 37. In the first derivative spectrum of the infrared absorption spectrum, -1 , 1480-1350 cm -1 , and 3000-2900 cm -1It was found that the bamboo white lignin-zinc chloride complex has a unique spectral structure in at least one wavenumber range selected from the group consisting of 3500-2500 cm. Furthermore, the first derivative spectra of the infrared absorption spectrum of the dried bamboo white lignin-zinc chloride complex and the swollen gel obtained by adding water to the dried bamboo white lignin-zinc chloride complex were similar (Figures 29-31). This indicates that the regular higher-order structure unique to the complex is maintained in both the dried and swollen samples. Furthermore, the swollen sample exhibited a spectral structure in the range of 3500-2500 cm. -1 A broad and large absorption characteristic of water is observed, indicating that the sample is a hydrogel containing a large amount of water.
Claims
1. A structured product of white lignin and / or white lignin-polysaccharide complex, wherein the white lignin has a β-O-4 ether structure content of 50% or more, the white lignin-polysaccharide complex has at least one bond selected from the group consisting of an α-ether bond between lignin and polysaccharide, an α-ester bond between lignin and polysaccharide, and a γ-ester bond between lignin and polysaccharide, and the structured product is a complex of the white lignin and / or the white lignin-polysaccharide complex with an organic acid and / or a salt, and / or the structured product is a modification or substitution of hydroxyl groups of the white lignin and / or the white lignin-polysaccharide complex.
2. The structured material is a complex of the white lignin and / or the white lignin-polysaccharide copolymer and / or their modified and / or substituted products with an organic acid and / or a salt, and the structured material has a first derivative spectrum of infrared absorption spectrum of 1080 to 950 cm -1 , 1480-1350 cm -1 , and 3000 to 2900 cm -1 The structured material according to claim 1, having a spectral structure specific to at least one wavenumber range selected from the group consisting of:
3. The structured material has a wavelength of 1080 to 950 cm in the first differential spectrum of the infrared absorption spectrum. -1 , 1480-1350 cm -1 , and 3000 to 2900 cm -1 The structured object according to claim 2, having three or more spectral structures specific to a wavenumber range consisting of:
4. The structured material according to claim 2, which is in the form of a powder, a sol, or a gel.
5. The structure according to claim 2, wherein the structure is a complex of the white lignin and / or the white lignin-polysaccharide copolymer with a compound having a carboxy structure, a carbonyl structure, and / or an amine structure, and / or a salt containing a metal ion.
6. The structured material of claim 4, which is in the form of a gel.
7. The structure according to claim 1, wherein the structure is a modification and / or substitution product of hydroxyl groups of the white lignin and / or the white lignin-polysaccharide copolymer, and contains at least one structure selected from the group consisting of a carbonylation structure, a halogenation structure, an aminated structure, a boron-modified structure, an acylation structure, and a cross-linked structure.
8. The structure of claim 1, wherein the white lignin has a Hunter Whiteness (W) of 60 or greater and / or the white lignin-polysaccharide complex has a Hunter Whiteness (W) of 60 or greater.
9. A method for producing a structured material according to any one of claims 2 to 6 and 8, comprising the steps of: mixing the white lignin and / or the white lignin-polysaccharide copolymer with an organic acid and / or salt, and a solvent to obtain a solution or dispersion; and reducing the solvent from the solution or dispersion.
10. A method for producing a structured product according to claim 7 or 8, comprising a step of modifying or substituting the hydroxyl groups of the white lignin and / or the white lignin-polysaccharide copolymer.
11. An adsorbent, recovery agent, remover, or transporter for metal ions or a salt containing the same, comprising white lignin and / or a white lignin-polysaccharide complex, wherein the white lignin has a content of β-O-4 type ether structures of 50% or more, and the white lignin-polysaccharide complex has at least one bond selected from the group consisting of an α-ether bond between the lignin and the polysaccharide, an α-ester bond between the lignin and the polysaccharide, and a γ-ester bond between the lignin and the polysaccharide.
12. The adsorbent, recovery agent, removal agent, or transport agent according to claim 11, which is used to adsorb, recover, remove, or transport metal ions or salts containing the same by forming a complex with the metal ions or salts containing the same.
Citation Information
Patent Citations
Method for producing lignin decomposed product
JP2013241391A
Decoloration method of lignin, preparation method of decolored lignin, production method of transparent film of lignin, and white lignin
JP2021017582A
Process for making lignin gels in bead form
US4131573A
Preparation method and application of magnetic carboxylated lignin
CN115722207A
Lignin grafted N-[(dimethylamino) methylene] thiourea type heavy metal adsorbent as well as preparation method and application thereof
CN115845818A