Free-machining copper alloy casting and production method for free-machining copper alloy casting

A free-cutting copper alloy with a modified β phase, formed through high-temperature solid solution and rapid cooling, addresses the limitations of β phase alloys by enhancing corrosion and machinability, achieving superior performance in resistance and strength while reducing lead content.

WO2024228354A1PCT designated stage expired Publication Date: 2024-11-07MITSUBISHI MATERIALS CORP

Patent Information

Application Number
PCT/JP2024/016185
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-05
Filing Date
2024-04-25
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Current free-cutting copper alloys face challenges with dezincification corrosion resistance and machinability, particularly with the β phase, which has poor resistance and is brittle, and the alternatives proposed either compromise on machinability or introduce harmful Bi, a rare and environmentally problematic metal.

Method used

The development of a free-cutting copper alloy with a modified β phase (β1 phase) achieved by solid solution of Si and P at high temperatures, followed by rapid cooling, which enhances dezincification corrosion resistance and machinability without compromising ductility or introducing harmful elements.

Benefits of technology

The alloy exhibits improved dezincification corrosion resistance, stress corrosion cracking resistance, and high strength with excellent machinability, comparable to Pb-containing brass, while reducing lead content and maintaining impact properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This free-machining copper alloy contains prescribed amounts of Cu, Si, Pb, and P, and contains a prescribed amount of Bi as an optional element, with the remainder being Zn and unavoidable impurities. Among the unavoidable impurities, the total content of Fe, Mn, Co, and Cr is less than a prescribed amount, and the Al content is less than a prescribed amount. The compositional relationships f1 and f2, which are defined from the elemental composition, the structural relationships f3, f4, and f5, which are defined from the surface area ratios of the constituent phases of the metallographic structure, and structural / compositional relationship f6, which is defined from the composition and the metallographic structure, each fall within prescribed ranges. When etched using a liquid mixture of hydrogen peroxide and aqueous ammonia, grain boundaries can be observed in a β1 phase.
Need to check novelty before this filing date? Find Prior Art

Description

Free-machining copper alloy casting and method for manufacturing free-machining copper alloy casting

[0001] The present invention relates to a free-cutting copper alloy casting having good castability, good dezincification corrosion resistance, and excellent machinability, with a significantly reduced lead content, and a method for producing the free-cutting copper alloy casting.The present invention relates to a free-cutting copper alloy casting used in appliances and parts for drinking water consumed daily by humans and animals, appliances and parts for sanitary facilities such as kitchens, baths, and toilets, musical instruments, tableware, drainage appliances and parts, industrial piping parts, machine parts, sliding parts, medical parts, automobile parts, electrical and household appliance parts, pressure vessels, building hardware, instrument parts, daily necessities, stationery, toys, and parts related to drinking water, industrial water, wastewater, hydrogen, and other liquids and gases, and a method for producing the free-cutting copper alloy casting. Specific part names include faucet fittings, water supply taps, mixer taps, stop valves, valves, joints, stems, cocks, water meters, drain valves, pressure reducing valves, valve seats, gate valves, fire hydrants, gears, flanges, branch valves, faucet valves, ball valves, bends, bearings, sleeves, connectors, etc. The present invention relates to a free-cutting copper alloy casting used for these cutting-applied parts, and a method for manufacturing the free-cutting copper alloy casting. This application claims priority to Japanese Patent Application No. 2023-075579 filed in Japan on May 1, 2023, and Japanese Patent Application No. 2023-173342 filed in Japan on October 5, 2023, the contents of which are incorporated herein by reference.

[0002] Conventionally, Cu-Zn-Pb alloys (also known as free-cutting brass rods, forging brasses, and casting brasses) or Cu-Sn-Zn-Pb alloys (also known as leaded red brasses), which have excellent machinability, have generally been used for drinking water and sanitary equipment appliances and parts, automobile parts, electrical and home appliance parts, machine parts, stationery, metering parts, medical parts, and appliances and parts related to liquids and gases such as industrial water, wastewater, and hydrogen, specifically faucets, water taps, mixer taps, stopcocks, valves, cocks, joints, valves, water meters, connectors, etc. Here, the composition of the Cu-Zn-Pb alloy contains, for example, 56 to 70 mass% Cu, 1 to 4 mass% Pb, and the balance Zn. The composition of the Cu--Sn--Zn--Pb alloy contains, for example, 80 to 88 mass % Cu, 1 to 8 mass % Sn, 1 to 8 mass % Pb, and the balance being Zn.

[0003] However, in recent years, concerns have arisen about the effects of Pb on the human body and the environment, and countries around the world are actively moving toward regulating Pb. For example, in the state of California in the United States, a regulation came into effect in January 2010 limiting the Pb content in drinking water appliances to 0.25 mass% or less. Countries other than the United States are also rapidly moving toward such regulations, and there is a demand for the development of copper alloy materials that comply with the Pb content regulations.

[0004] Furthermore, in other industrial fields such as automobiles, electrical and electronic equipment, and machinery, for example, the European ELV Directive and RoHS Directive allow free-cutting copper alloys to have a Pb content of up to 4 mass% as an exception, but as in the field of drinking water, there is active discussion about strengthening regulations on Pb content, including the elimination of the exception.

[0005] In the midst of this trend toward stricter Pb restrictions on machinable copper alloys, the following alloys have been proposed: (1) Cu-Zn-Bi alloys and Cu-Zn-Bi-Se alloys, which contain Bi, which has machinability in place of Pb, and in some cases, Se together with Bi; (2) Cu-Zn alloys containing a high concentration of Zn to increase the amount of β phase and thereby improve machinability; (3) Cu-Zn-Si alloys and Cu-Zn-Sn alloys containing large amounts of γ-phase and κ-phase in place of Pb, which have excellent machinability; and (4) Cu-Zn-Sn-Bi alloys containing large amounts of γ-phase and Bi. For example, in Patent Document 1, 0.7 to 2.0 mass% of Sn and 0.5 to 2.0 mass% of Bi are added to a Cu-Zn alloy containing 59.5 to 66.0 mass% of Cu to precipitate a γ phase, thereby improving corrosion resistance and machinability.

[0006] However, alloys containing Bi instead of Pb have many problems, including that Bi is inferior to Pb in machinability, Bi may be harmful to the human body like Pb, Bi is a rare metal and therefore presents resource problems, and Bi makes copper alloy materials brittle, etc. Furthermore, as shown in Patent Document 1, even if a γ phase is precipitated in a Cu-Zn-Sn alloy, the γ phase containing Sn has poor machinability, and requires the co-addition of Bi, which has a machinability function.

[0007] In addition, in Patent Document 2, a large amount of Bi, 0.3 to 4 mass%, preferably 1.8 to 3.2 mass%, is added to a Cu-Zn alloy containing 59 to 62 mass% Cu. Furthermore, since the β phase has poor dezincification corrosion resistance, the machinability and dezincification corrosion resistance are improved by reducing the β phase and annealing at 350 to 550°C to separate the β phase with the α phase. Thus, the β phase of Cu-Zn alloys has traditionally been poor in dezincification corrosion resistance, and as an improvement measure, it has been essentially required to reduce the β phase and anneal to separate the β phase with the α phase.

[0008] On the other hand, Cu-Zn binary alloys containing a large amount of β phase contribute to improving machinability, but the β phase has inferior machinability function compared to Pb, and is inferior in dezincification corrosion resistance and stress corrosion cracking resistance, so they cannot possibly be a substitute for Pb-containing free-cutting copper alloys. Therefore, in recent years, Cu-Zn-Si alloys containing Si instead of Pb have been proposed as free-cutting copper alloys in Patent Documents 3 to 9.

[0009] In Patent Documents 3 to 8, the Cu content is roughly 58 to 65 mass% and the Si content is 0.2 to 1.5 mass%, and it is said that machinability is improved by the presence of Si contained in the β phase and fine P compounds formed from P, Zn, etc., and the area ratios of the β phase and γ phase are specified, and excellent machinability is achieved by the presence of P compounds combined with the inclusion of a small amount of Pb. However, as disclosed in Patent Document 2, it is a well-known fact that the β phase of Cu-Zn alloys has poor dezincification corrosion resistance and further poor stress corrosion cracking resistance. Therefore, Patent Documents 3 to 8 do not disclose specific data related to dezincification corrosion resistance and stress corrosion cracking resistance, and it is presumed that the dezincification corrosion resistance and stress corrosion cracking resistance, which are technical issues with the β phase of conventional Cu-Zn alloys, have not been improved.

[0010] Patent Document 9 specifies the Cu content to be 71.5 to 78.5 mass%, the Si content to be 2.0 to 4.5 mass%, and specifies the total area of ​​the γ and κ phases, which are formed from an alloy with high Cu and Si concentrations and have excellent machinability, thereby achieving excellent machinability with a small Pb content of 0.02 mass% or less. Furthermore, by including Sn and Al in amounts of 0.1 mass% or more, a large amount of γ phase is formed, further improving machinability and corrosion resistance.

[0011] In addition, in Patent Document 10, a Cu-Zn-Sn alloy is added with small amounts of Si, Pb, P, or Fe, and 0.5 mass% or less of Pb, and by devising a manufacturing method, Pb-enriched particles are dispersed in the matrix, and the number density of the Pb-enriched particles present in the α phase is increased, thereby obtaining excellent machinability. Patent Document 10 also discloses that a finish heat treatment at 400 to 600°C is essentially required to improve dezincification corrosion resistance.

[0012] Patent Document 11 relates to a technique for producing a near-net hollow hot forged product using a hollow material in a Cu-Zn-Si-Pb-P alloy, and proposes a copper alloy in which the area ratios of β, γ, and μ phases are limited. Patent Document 12 proposes a copper alloy casting in which Si, Pb, Sn, and Bi are selectively contained in a Cu-Zn-Zr-P alloy, and the crystal grains are refined by the action of Zr and P. Patent Document 13 proposes a copper alloy with excellent discoloration resistance in which Si and Pb are selectively contained in a Cu-Zn-Sn-Al alloy, and the area ratios of γ and β phases are limited. Patent Document 14 proposes a copper alloy casting in which Pb is not contained in a Cu-Zn-Si-Sn-Al-P alloy. Patent Document 15 proposes that the apparent Zn content is important for improving corrosion resistance in Cu-Zn-Si-Sn-Al alloys, and proposes copper alloys that substantially contain a large amount of Pb or Bi to improve machinability. Patent Document 16 describes a Cu-Zn-Si alloy containing 65 mass% or more of Cu, a Pb-free copper alloy casting with good castability and mechanical strength, and claims that the machinability is improved by the γ phase, and describes examples containing large amounts of Sn, Al, Mn, Ni, and Sb.

[0013] International Publication No. WO 2008 / 081947 JP 2002-003967 A JP 2021-042461 A JP 2021-042459 A JP 2021-042460 A International Publication No. WO 2020 / 261666 JP 2021-042462 A International Publication No. WO 2021 / 117528 International Publication No. 2007 / 034571 JP 2016-194123 A International Publication No. 2013 / 065830 International Publication No. 2006 / 016630 International Publication No. 2015 / 046421 JP 2010-133006 A Japanese Patent Application Laid-Open No. 2018-048398 A Special Publication No. 2019-508584

[0014] As shown in Patent Documents 1 to 16, no substantial improvement has been found to date in the dezincification corrosion resistance of the β phase present in Cu—Zn alloys, which has been a major technical problem for some time. Furthermore, there has been no disclosure of a Cu—Zn alloy that contains less than 0.2 mass% of Pb and Bi, and that exhibits low cutting resistance and excellent machinability in high-speed cutting at cutting speeds exceeding 100 m / min, even without requiring the inclusion of Bi.

[0015] The present invention has been made to solve the problems of the prior art, and it is an object of the present invention to provide a free-cutting copper alloy casting that is excellent in machinability and castability, and that has good dezincification corrosion resistance despite containing a large amount of β phase (β1 phase, described below), has high strength, good impact properties, and has a significantly reduced lead content, and a method for producing the free-cutting copper alloy casting.

[0016] In order to solve the above-mentioned problems and achieve the above-mentioned object, the inventors conducted extensive research and have discovered the following. In this specification, unless otherwise specified, the β phase includes the β' phase, the γ phase includes the γ' phase, and the α phase includes the α' phase. The β1 phase refers to a modified β phase, and the β phase and the β1 phase are distinguished from each other. The β1 phase is characterized in that, when observed under a metallurgical microscope using hydrogen peroxide and aqueous ammonia as an etching solution, a grain boundary pattern is observed within the β1 phase and is recognized as a grain boundary. When the β phase present in common Cu—Zn alloys, Cu—Zn—Bi alloys, Cu—Zn—Si alloys, etc. is etched with hydrogen peroxide and aqueous ammonia, no grain boundary pattern, i.e., no grain boundary, is observed within the β phase. Therefore, the β phase and the β1 phase can be clearly distinguished. For example, Figure 1A, which will be described later, shows the metallographic structure of an alloy of the present invention, which consists of two phases: a β1 phase modified from the β phase and an α phase. A grain boundary pattern can be observed within the β1 phase. In this application, the grain boundary pattern observed in Figure 1A is referred to as a crystal grain boundary, or simply referred to as a grain boundary. On the other hand, Figure 2A shows the metallographic structure of a comparative alloy consisting of a β phase and an α phase. No grain boundary pattern is observed within the β phase, i.e., no grain boundary exists. P compounds refer to compounds of P and primarily Zn and / or Si. Cold workability refers to performance in cold processing, such as drawing, wire drawing, crimping, and bending. Good or excellent machinability, unless otherwise specified, refers to low cutting resistance and good chip separation during peripheral cutting using a lathe. Conductivity refers to electrical conductivity, thermal conductivity, and electrical conductivity. Cooling rate refers to the average cooling rate within a certain temperature range. The cooling rate at a certain temperature, for example, 500°C, is the cooling rate when passing through 500°C from a temperature just above 500°C, and is the average cooling rate from a temperature several tens of degrees higher than 500°C to 500°C. Actual operation means manufacturing using actual mass production equipment.

[0017] The above-mentioned Patent Document 9 states that the β phase in a Cu-Zn-Si alloy does not contribute much to the machinability of the copper alloy, but rather impairs it. Patent Documents 11, 12, and 13 also significantly limit the amount of β phase. Patent Document 2 states that, as a method for improving the dezincification corrosion resistance of the β phase, a process of annealing at 350 to 550°C is required to reduce the β phase and divide the β phase with the α phase. Patent Document 10 states that, in order to improve the dezincification corrosion resistance of the β phase, a greater amount of Sn than Si is required, and that the alloy is heated to a temperature of 700 to 850°C, hot extruded, and then subjected to a finish heat treatment at 400 to 600°C for 30 minutes or more, with an average cooling rate of 0.2 to 10°C / second from 400 to 200°C.

[0018] On the other hand, Patent Documents 3 to 8 discovered that in Cu—Zn—Si alloys, the inclusion of a certain amount of Si in the β phase has a significant effect on the machinability of the β phase itself. It is then stated that the synergistic effects of the three elements—the presence of fine P compounds, a small amount of Pb, and possibly Bi—result in the alloy's excellent machinability. However, in order to ensure the presence of P compounds, it is preferable to cool the alloy after hot working or casting at an average cooling rate of about 0.1°C / min to about 70°C / min in the temperature range from about 530°C to about 450°C. Patent Documents 3 to 8 do not disclose data related to dezincification corrosion resistance or stress corrosion cracking resistance. Furthermore, there is no mention of modifying the β phase itself. In other words, it is presumed that there is no improvement in the dezincification corrosion resistance or stress corrosion cracking resistance of the β phase present in Cu—Zn—Si alloys, and no further improvement in machinability.

[0019] The present inventors further worked on modifying the β phase itself in Cu—Zn—Si alloys. As a result of extensive research, they found that even without the presence of P compounds, the modified β phase, i.e., the β1 phase, further improved machinability, particularly during high-speed cutting, and significantly improved the dezincification corrosion resistance of the β phase, a long-standing issue for Cu—Zn alloys. In addition, alloys containing the β1 phase instead of the β phase were able to further increase strength without impairing ductility. This β1 phase can be obtained by first solidifying Si and P into the β phase at a high temperature after solidification, and then maintaining the β phase at a high temperature above 500°C, i.e., above 500°C but below 700°C, and then increasing the cooling rate during cooling to room temperature to maintain the high-temperature metallographic structure at room temperature.

[0020] The β1 phase can be easily distinguished from the β phase of Cu-Zn alloys. The surface is mirror-polished and etched with a mixture of hydrogen peroxide and aqueous ammonia. For etching, an aqueous solution containing 3 mL of 3 vol% hydrogen peroxide and 22 mL of 14 vol% aqueous ammonia is used. When the polished metal surface is immersed in this solution for approximately 2 to 10 seconds at room temperature (approximately 15 to 25°C) and observed under a metallurgical microscope at 200 to 1000 magnifications, grain boundary patterns, i.e., crystal grain boundaries, are visible within the β1 phase, whereas no grain boundary patterns, i.e., crystal grain boundaries, are observed within the β phase of ordinary Cu-Zn alloys. The use of this etching solution is also disclosed in Patent Documents 3 to 8, 11, and 12, and metal structures are published in these documents.

[0021] The conditions for obtaining the β1 phase are that the molten metal is poured into a mold, and the casting after solidification is maintained in a β phase state at a high temperature above 500°C, i.e., above 500°C but below 700°C, and then brought down to room temperature. Specifically, to obtain the β1 phase, during the cooling process after solidification, the cooling treatment is preferably started at a temperature lower than 700°C but higher than 500°C, and when the temperature of the casting reaches 500°C, i.e., in the temperature range just above 500°C, the casting is cooled at a cooling rate of more than 300°C / min, and in the subsequent cooling treatment, the average cooling rate in the temperature range from 500°C to 300°C is at least more than 300°C / min. Unless otherwise specified, in this specification, cooling treatment refers to controlling the cooling rate by water cooling or a similar method, rather than natural cooling.

[0022] In Patent Documents 3 to 8, in order to obtain fine P-containing compounds, the casting or hot-worked material must be cooled at an average cooling rate of about 0.1°C / min to about 70°C / min in the temperature range from about 530°C to about 450°C after casting or hot working, which is slower than that of the present application. In other words, it is clear that the present application and Patent Documents 3 to 8 are directed in opposite directions in terms of cooling after solidification or hot working. However, for example, if the cooling rate around about 530°C during the cooling process is about 50°C / min and the average cooling rate in the temperature range from 530°C to 500°C, which is the cooling treatment start temperature, exceeds 300°C, an alloy containing both the β1 phase and P compounds may exist even in the present application.

[0023] The present invention significantly improves the machinability of Cu-Zn-Si alloys by modifying the β phase to the β1 phase, even without the presence of P compounds. Furthermore, the synergistic effect of the β1 phase and a small amount of fine Pb particles or particles containing Pb and Bi reduces cutting resistance and promotes chip fragmentation, maintaining good machinability even at high-speed cutting. More importantly, the dezincification corrosion resistance and stress corrosion cracking resistance, which were previously unresolved issues with the conventional β phase, are significantly improved and resolved by modifying the β phase to the β1 phase. Furthermore, the mechanical properties of the alloys retain the high strength of the conventional β phase, and by modifying the β phase to the β1 phase, they achieve higher strength without impairing ductility or impact properties. Furthermore, in the case of castings, cold working such as caulking is rarely performed, and in terms of application, they must be non-brittle, i.e., be able to withstand impact. Modifying the β phase to the β1 phase makes it possible to provide higher strength while preventing a decrease in impact properties. As a result of the above, the inventors have invented a copper alloy casting that has free-cutting performance comparable to that of conventional free-cutting brass containing a large amount of Pb, and that has better dezincification corrosion resistance and stress corrosion cracking resistance, as well as higher strength and better impact properties than conventional free-cutting brass.

[0024] A free-cutting copper alloy casting according to a first aspect of the present invention contains more than 60.5 mass% and less than 65.0 mass% Cu, more than 0.50 mass% and less than 1.20 mass% Si, 0.002 mass% or more and less than 0.20 mass% Pb, and more than 0.01 mass% and less than 0.18 mass% P, and contains, as an optional element, 0.0001 mass% or more and less than 0.20 mass% Bi, with the balance consisting of Zn and inevitable impurities, wherein the total content of Fe, Mn, Co, and Cr among the inevitable impurities is less than 0.50 mass%, and the content of Al is less than 0.30 mass%, the content of Cu is [Cu] mass%, the content of Si is [Si] mass%, and the content of P is [P] mass%. When the Cu content is [Pb] mass%, the P content is [P] mass%, and the Bi content is [Bi] mass%, the relationship of 57.3≦f1=[Cu]−4.8×[Si]+0.5×([Pb]+[Bi])−[P]≦60.8 is satisfied, and when Bi is contained, the relationship of 0.003≦f2=[Pb]+[Bi]<0.20 is satisfied. In addition, in the constituent phases of the metal structure excluding non-metallic inclusions, when the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, the following relationships are satisfied: 20≦f3=(α)<75, 25<f4=(β1)≦80, 0≦f5=(γ)<4, 28<f6=(β1)×(−0.5×[Si] 2 +1.5×[Si])-2×(γ)+([Pb]+[Bi]) 1/2 ×25+([P]) 1/2 ×12, and when etched with a mixed solution of hydrogen peroxide and aqueous ammonia, grain boundaries are observed within the β1 phase.

[0025] A free-cutting copper alloy casting according to a second aspect of the present invention contains 61.5 mass% to 64.8 mass% Cu, 0.65 mass% to 1.10 mass% Si, 0.003 mass% to less than 0.10 mass% Pb, and 0.03 mass% to 0.15 mass% P, and optionally contains 0.001 mass% to less than 0.10 mass% Bi, with the balance consisting of Zn and inevitable impurities, wherein the total content of Fe, Mn, Co, and Cr among the inevitable impurities is less than 0.35 mass%, and the content of Al is less than 0.15 mass%, the content of Cu is [Cu] mass%, the content of Si is [Si] mass%, and the content of P is [0.03 mass% to 0.15 mass%]. When the Cu content is [Pb] mass%, the P content is [P] mass%, and the Bi content is [Bi] mass%, the relationship of 58.0≦f1=[Cu]−4.8×[Si]+0.5×([Pb]+[Bi])−[P]≦60.5 is satisfied, and when Bi is contained, the relationship of 0.004≦f2=[Pb]+[Bi]<0.10 is satisfied. In addition, in the constituent phases of the metallographic structure excluding non-metallic inclusions, when the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, the following relationships are satisfied: 30≦f3=(α)≦70, 30≦f4=(β1)≦70, 0≦f5=(γ)<1, 35<f6=(β1)×(−0.5×[Si] 2 +1.5×[Si])-2×(γ)+([Pb]+[Bi]) 1/2 ×25+([P]) 1/2 ×12, and when etched with a mixed solution of hydrogen peroxide and aqueous ammonia, grain boundaries are observed within the β1 phase.

[0026] The free-cutting copper alloy casting of embodiment 3 of the present invention contains more than 60.5 mass% and less than 65.0 mass% Cu, more than 0.50 mass% and less than 1.20 mass% Si, 0.002 mass% or more and less than 0.20 mass% Pb, more than 0.01 mass% and less than 0.18 mass% P, and more than 0.05 mass% and less than 0.70 mass% Sn, and contains 0. The alloy contains 0.001 mass% or more and less than 0.20 mass% Bi, with the balance being Zn and inevitable impurities, and among the inevitable impurities, the total content of Fe, Mn, Co, and Cr is less than 0.50 mass%, and the Al content is less than 0.30 mass%, the Cu content is [Cu] mass%, the Si content is [Si] mass%, and the Pb content is [Pb] mass%. When the P content is [P] mass%, the Bi content is [Bi] mass%, and the Sn content is [Sn] mass%, the relationship of 57.3≦f1=[Cu]−4.8×[Si]+0.5×([Pb]+[Bi])−[P]−[Sn]≦60.8 is satisfied, and the relationship of f0=[Sn] / [Si]<0.8 is also satisfied. When Bi is contained, the relationship of 0.003≦ The relationship of f2 = [Pb] + [Bi] < 0.20 is satisfied, and in the constituent phases of the metal structure excluding non-metallic inclusions, when the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, the following relationships are satisfied: 20 ≦ f3 = (α) < 75, 25 < f4 = (β1) ≦ 80, 0 ≦ f5 = (γ) < 4, 28 < f6 = (β1) × (-0.5 × [Si] 2 +1.5×[Si])-2×(γ)+([Pb]+[Bi]) 1/2 ×25+([P]) 1/2 ×12, and when etched with a mixed solution of hydrogen peroxide and aqueous ammonia, grain boundaries are observed within the β1 phase.

[0027] A free-cutting copper alloy casting according to a fourth aspect of the present invention is characterized in that, in the free-cutting copper alloy casting according to any one of the first to third aspects of the present invention, it is used for appliances and parts relating to drinking water and sanitation facilities, water meters, valves, drainage appliances and parts, industrial piping parts, automobile parts, electric and home appliance parts, machine parts, stationery, toys, musical instruments, sliding parts, instrument parts, and medical parts.

[0028] A manufacturing method of a free-cutting copper alloy casting according to Aspect 5 of the present invention is a manufacturing method of a free-cutting copper alloy casting according to any one of Aspects 1 to 4 of the present invention, which includes a casting step, and is characterized in that in the cooling process of the final casting step in the casting step, the cooling rate at the time when the temperature of the casting reaches 500°C exceeds 300°C / min, and the average cooling rate in the temperature range from 500°C to 300°C exceeds 300°C / min.

[0029] A manufacturing method of a free-cutting copper alloy casting according to Aspect 6 of the present invention is a manufacturing method of a free-cutting copper alloy casting according to any one of Aspects 1 to 4 of the present invention, which includes a casting step, and is characterized in that in the cooling process of the final casting step of the casting step, the cooling treatment start temperature is higher than 500°C and lower than 700°C, the cooling rate when the temperature of the casting reaches 500°C exceeds 300°C / min, and the average cooling rate in the temperature range from 500°C to 300°C exceeds 300°C / min.

[0030] A method for producing a free-cutting copper alloy casting according to Aspect 7 of the present invention is a method for producing a free-cutting copper alloy casting according to any one of Aspects 1 to 4 of the present invention, comprising a casting step and a heat treatment step, characterized in that in the final heat treatment step, heating is performed under conditions of holding at a temperature above 520°C and lower than 650°C for 1 minute to 5 hours, and in the cooling treatment step after the heat treatment, cooling treatment is started at a temperature above 520°C, the cooling rate at the time the temperature of the casting reaches 500°C is above 300°C / min, and the average cooling rate in the temperature range from 500°C to 300°C is above 300°C / min.

[0031] According to one aspect of the present invention, it is possible to provide a free-cutting copper alloy casting that has excellent castability, good machinability, dezincification corrosion resistance, and stress corrosion cracking resistance, high strength, an excellent balance of strength, impact properties, and ductility, and has a significantly reduced Pb content, and a method for producing the free-cutting copper alloy casting.

[0032] 1 is a photograph of a microstructure of a copper alloy casting according to an embodiment. The copper alloy casting was obtained by subjecting Alloy No. S02 to Process No. A1. Specifically, Alloy No. S02 had a composition of Zn-62.9 mass% Cu-0.94 mass% Si-0.082 mass% P-0.067 mass% Pb-0.03 mass% Sn. In Process No. A1, the alloy was tapped at 1,080°C and cast into a sand mold, removed from the sand mold at 650°C, and cooled at 560°C. The average cooling rate in the temperature range from 550°C to 500°C was 900°C / min, and the average cooling rate in the temperature range from 500°C to 300°C was 900°C / min. 1A is a result of a dezincification corrosion test performed on the alloy casting of FIG. 1A according to the ISO 6509 test method, and is a cross-sectional metallographic photograph including a portion exhibiting maximum corrosion depth. This is a microstructure observation photograph of a copper alloy casting according to an embodiment, in which the copper alloy casting was obtained by performing Process No. A14H on Alloy No. S02. Specifically, Alloy No. S02 has a composition of Zn-62.9 mass% Cu-0.94 mass% Si-0.082 mass% P-0.067 mass% Pb-0.03 mass% Sn. In Process No. A14H, the alloy was tapped at 1,080°C and cast into a sand mold, removed from the sand mold at 650°C, and naturally cooled, with an average cooling rate of 20°C / min in the temperature range from 500°C to 300°C. 2A is a result of a dezincification corrosion test performed on the alloy casting of FIG. 2A in accordance with the ISO 6509 test method, and is a cross-sectional metallographic photograph including a portion exhibiting maximum corrosion depth. Also, a microstructure observation photograph of a copper alloy casting in an embodiment is shown. The copper alloy casting was obtained by performing Process No. B1 on Alloy No. S12. Specifically, Alloy No. S12 has a composition of Zn-63.6 mass% Cu-1.04 mass% Si-0.070 mass% P-0.062 mass% Pb alloy-0.003 mass% Bi. Process No. For B1, the molten metal was poured into a mold at 960°C, removed from the mold at 750°C, and the cooling treatment started at 560°C, with an average cooling rate of 1020°C / min in the temperature range from 550°C to 500°C and an average cooling rate of 1020°C / min in the temperature range from 500°C to 300°C.3A is a result of a dezincification corrosion test performed on the alloy casting of FIG. 3A according to the ISO 6509 test method, and is a cross-sectional metallographic photograph including a portion exhibiting maximum corrosion depth. This is a microstructure observation photograph of a copper alloy casting according to an embodiment, in which the copper alloy casting was obtained by performing Process No. B11H on Alloy No. S12. Specifically, Alloy No. S12 has a composition of Zn-63.6 mass% Cu-1.04 mass% Si-0.070 mass% P-0.062 mass% Pb-0.003 mass% Bi. In Process No. B11H, the molten metal was poured into a mold at 960°C and removed from the mold at 750°C, and the average cooling rate in the temperature range from 500°C to 300°C was 40°C / min. 4A is a cross-sectional metallographic photograph showing the results of a dezincification corrosion test performed on the alloy casting of FIG. 4A in accordance with the ISO 6509 test method, including the area showing the maximum corrosion depth. This is a microstructure observation photograph of a copper alloy casting according to an embodiment. The copper alloy casting was obtained by performing Process No. A14H and Process No. G1 on Alloy No. S02. Specifically, Alloy No. S02 has a composition of Zn-62.9 mass% Cu-0.94 mass% Si-0.082 mass% P-0.067 mass% Pb-0.03 mass% Sn. In Process No. A14H, the alloy was tapped at 1,080°C and cast into a sand mold, removed from the sand mold at 650°C, and naturally cooled. The average cooling rate in the temperature range from 500°C to 300°C was 20°C / min. The resulting casting was then subjected to Process No. In Process No. G1, the casting was heated at 580°C for 20 minutes, and cooling was initiated from 575°C, with an average cooling rate of 1200°C / min in the temperature range from 550°C to 500°C, and an average cooling rate of 1200°C / min in the temperature range from 500°C to 300°C. The alloy casting of Figure 5A was subjected to a dezincification corrosion test in accordance with the ISO 6509 test method, and the cross-sectional metallographic photograph includes the portion exhibiting the maximum corrosion depth.

[0033]

[0013] The free-cutting copper alloy castings and methods for producing the same according to embodiments of the present invention are described below. Applications of the free-cutting copper alloy castings according to embodiments of the present invention include drinking water and sanitary equipment, instruments, tableware, electrical, home appliance, and electronic equipment parts, automobile parts, machine parts, stationery, precision machine parts, medical parts, and equipment and parts related to industrial water, wastewater, hydrogen, and other liquids and gases. Specific part names include water taps, mixer taps, stop valves, valves, cocks, joints, water meters, gears, sensors, nuts, screws, connectors, etc.

[0034] In this specification, an element symbol in parentheses, such as [Zn], indicates the content (mass%) of that element. In this embodiment, this content representation method is used to define the compositional formulas f1, f2, and f0 as follows: The compositional formula f1 = [Cu] - 4.8 x [Si] + 0.5 x ([Pb] + [Bi]) - [P]. When Sn is contained in an amount exceeding 0.05 mass%, the compositional formula f1 = [Cu] - 4.8 x [Si] + 0.5 x ([Pb] + [Bi]) - [P] - [Sn]. When Bi is contained, the compositional formula f2 = [Pb] + [Bi]. When Sn is contained, the compositional formula f0 = [Sn] / [Si].

[0035] Furthermore, in this embodiment, in the constituent phases of the metal structure excluding non-metallic inclusions, precipitates, and Pb or Bi particles, the area ratio of the α phase is represented by (α)%, the area ratio of the γ phase by (γ), the area ratio of the unmodified β phase by (β), and the area ratio of the modified β1 phase by (β1)%. The area ratio of each phase is also referred to as the amount of each phase, the proportion of each phase, or the proportion occupied by each phase. In this embodiment, a plurality of structure relational equations are defined as follows. Structure relational equation f3 = (α) Structure relational equation f4 = (β1) Structure relational equation f4A = (β) Structure relational equation f5 = (γ) Structure-composition relational equation f6 = (β1) × (-0.5 × [Si] 2 +1.5×[Si])-2×(γ)+([Pb]+[Bi]) 1/2 ×25+([P]) 1/2 × 12 Structure / composition relationship formula f6A = (β) × (-0.5 × [Si] 2+1.5×[Si])-2×(γ)+([Pb]+[Bi]) 1/2 ×25+([P]) 1/2 x12

[0036] A free-cutting copper alloy casting according to a first embodiment of the present invention contains more than 60.5 mass% and less than 65.0 mass% Cu, more than 0.50 mass% and less than 1.20 mass% Si, 0.002 mass% or more and less than 0.20 mass% Pb, more than 0.01 mass% and less than 0.18 mass% P, and contains 0.0001 mass% or more and less than 0.20 mass% Bi as an optional element, with the balance being Zn and inevitable impurities, wherein the total content of Fe, Mn, Co, and Cr among the inevitable impurities is less than 0.50 mass% and the content of Al is less than 0.30 mass%, the content of Cu is [Cu] mass%, the content of Si is [Si] mass%, %, the Pb content is [Pb] mass%, the P content is [P] mass%, and the Bi content is [Bi] mass%, then there is a relationship of 57.3≦f1=[Cu]−4.8×[Si]+0.5×([Pb]+[Bi])−[P]≦60.8, and when Bi is contained, there is also a relationship of 0.003≦f2=[Pb]+[Bi]<0.20. In addition, in the constituent phases of the metallographic structure excluding non-metallic inclusions, when the area fraction of the α phase is (α)%, the area fraction of the γ phase is (γ)%, and the area fraction of the β1 phase, which is a modified β phase, is (β1)%, then there are the following relationships: 20≦f3=(α)<75, 25<f4=(β1)≦80, 0≦f5=(γ)<4, 28<f6=(β1)×(−0.5×[Si] 2 +1.5×[Si])-2×(γ)+([Pb]+[Bi]) 1/2 ×25+([P]) 1/2 ×12, and when etched with a mixed solution of hydrogen peroxide and aqueous ammonia, grain boundaries are observed within the β1 phase.

[0037] A free-cutting copper alloy casting according to a second embodiment of the present invention contains 61.5 mass% or more and 64.8 mass% or less of Cu, 0.65 mass% or more and 1.10 mass% or less of Si, 0.003 mass% or more and less than 0.10 mass% of Pb, and 0.03 mass% or more and 0.15 mass% or less of P, and contains, as an optional element, 0.001 mass% or more and less than 0.10 mass% of Bi, with the balance being Zn and inevitable impurities, wherein the total content of Fe, Mn, Co, and Cr among the inevitable impurities is less than 0.35 mass%, and the content of Al is less than 0.15 mass%, the content of Cu is [Cu] mass%, the content of Si is [Si] mass%, %, the Pb content is [Pb] mass%, the P content is [P] mass%, and the Bi content is [Bi] mass%, then the relationship of 58.0≦f1=[Cu]−4.8×[Si]+0.5×([Pb]+[Bi])−[P]≦60.5 is satisfied, and when Bi is contained, the relationship of 0.004≦f2=[Pb]+[Bi]<0.10 is satisfied. In addition, in the constituent phases of the metallographic structure excluding non-metallic inclusions, when the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, then the following relationships are satisfied: 30≦f3=(α)≦70, 30≦f4=(β1)≦70, 0≦f5=(γ)<1, 35<f6=(β1)×(−0.5×[Si] 2 +1.5×[Si])-2×(γ)+([Pb]+[Bi]) 1/2 ×25+([P]) 1/2 ×12, and when etched with a mixed solution of hydrogen peroxide and aqueous ammonia, grain boundaries are observed within the β1 phase.

[0038] A free-cutting copper alloy casting according to a third embodiment of the present invention contains more than 60.5 mass% and less than 65.0 mass% Cu, more than 0.50 mass% and less than 1.20 mass% Si, 0.002 mass% or more and less than 0.20 mass% Pb, more than 0.01 mass% and less than 0.18 mass% P, and more than 0.05 mass% and less than 0.70 mass% Sn, and any optional elements. The alloy contains 0.0001 mass% or more and less than 0.20 mass% Bi, with the balance consisting of Zn and inevitable impurities, and among the inevitable impurities, the total content of Fe, Mn, Co, and Cr is less than 0.50 mass%, and the Al content is less than 0.30 mass%, the Cu content is [Cu] mass%, the Si content is [Si] mass%, and the Pb content is [Pb ] mass%, the P content is [P] mass%, the Bi content is [Bi] mass%, and the Sn content is [Sn] mass%, then the relationship of 57.3≦f1=[Cu]−4.8×[Si]+0.5×([Pb]+[Bi])−[P]−[Sn]≦60.8 is satisfied, and the relationship of f0=[Sn] / [Si]<0.8 is also satisfied, and when Bi is contained, 0.003 ≦f2=[Pb]+[Bi]<0.20, and in the constituent phases of the metal structure excluding non-metallic inclusions, when the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, the following relationships are satisfied: 20≦f3=(α)<75, 25<f4=(β1)≦80, 0≦f5=(γ)<4, 28<f6=(β1)×(−0.5×[Si] 2 +1.5×[Si])-2×(γ)+([Pb]+[Bi]) 1/2 ×25+([P]) 1/2 ×12, and when etched with a mixed solution of hydrogen peroxide and aqueous ammonia, grain boundaries are observed within the β1 phase.

[0039] The reasons for defining the chemical composition, compositional relational formulas f0, f1, and f2, structure relational formulas f3, f4 (f4A), and f5, structure-composition relational formula f6 (f6A), metal structure, and the like as described above will be explained below.

[0040] <Component Composition> (Cu) Cu is a major element of the free-cutting copper alloy of this embodiment. To overcome the problems of the present invention, it is necessary to contain at least 60.5 mass% Cu. If the Cu content is 60.5 mass% or less, depending on the contents of Si, Zn, P, Pb, Bi, and Sn and the manufacturing process, the proportion of the β1 phase exceeds 80%, resulting in low ductility and embrittlement. Furthermore, the β phase is not sufficiently modified, resulting in poor dezincification corrosion resistance, stress corrosion cracking resistance, and machinability, and poor ductility. Therefore, the lower limit of the Cu content is more than 60.5 mass%, preferably 61.0 mass% or more, more preferably 61.5 mass% or more, and even more preferably 62.0 mass% or more. On the other hand, if the Cu content is 65.0 mass% or more, the proportion of the β1 phase decreases, although this depends on the contents of Si, Zn, P, Pb, Bi, and Sn and the manufacturing process. As a result, excellent machinability cannot be obtained and strength also decreases. Therefore, the Cu content is less than 65.0 mass%, preferably 64.8 mass% or less, and more preferably 64.5 mass% or less.

[0041] (Si) Si is a major element in the free-cutting copper alloy of this embodiment, and Si contributes to the formation of metal phases such as the kappa, gamma, mu, beta, beta1, and zeta phases. By containing Cu, Zn, Si, and P in the above-mentioned ranges and performing the predetermined cooling treatment described below, the beta phase is modified to form the beta1 phase. The modified beta1 phase not only improves machinability but also significantly improves the dezincification corrosion resistance and stress corrosion cracking resistance that were previously drawbacks of the beta phase. A typical composition of the modified beta1 phase is approximately 61 mass% Cu, approximately 1.2 mass% Si, approximately 37.5 mass% Zn, and approximately 0.1 mass% P.

[0042] On the other hand, a typical composition of the α phase is approximately 66 mass% Cu, approximately 0.7 mass% Si, and approximately 33 mass% Zn. Within the composition range of this embodiment, the inclusion of Si slightly improves the machinability, dezincification corrosion resistance, and stress corrosion cracking resistance of the α phase, and also improves strength. The modified β1 phase and the improved α phase improve the machinability, dezincification corrosion resistance, stress corrosion cracking resistance, and strength of the alloy. Note that a certain amount of α phase is required to modify the β phase; for example, if there is no α phase, the β phase will not be modified. To improve the dezincification corrosion resistance, stress corrosion cracking resistance, machinability, impact properties, and ductility of the alloy, the α phase must have an area fraction of 20% or more, preferably 30% or more.

[0043] Si is an essential element for modifying the β phase. After solidification, Si dissolves in the β phase. The greater the Si content, the more the β phase is modified, resulting in a β1 phase with better properties. Furthermore, the inclusion of Si increases the strength of the alloy and improves the flowability during casting. To modify the β phase and further improve the β1 phase, Si must be present in an amount exceeding 0.50 mass%. Preferably, the Si content is 0.60 mass% or more, more preferably 0.65 mass% or more, and even more preferably 0.70 mass% or more. On the other hand, once the Si content reaches a predetermined amount, the modification of the β1 phase saturates. Furthermore, if the Si content is too high, the conductivity decreases, ductility decreases, and impact properties deteriorate. In some cases, a γ phase may appear. Patent Documents 3 to 9 state that the γ phase improves machinability. However, in the present invention, which is primarily composed of β1 phase and α phase, the presence of the γ phase actually worsens machinability, reduces the ductility and impact properties of the alloy, and worsens dezincification corrosion resistance and stress corrosion cracking resistance. Therefore, it is preferable to limit the amount of Si and the amount of γ phase. For these reasons, the amount of Si is less than 1.20 mass%, preferably 1.10 mass% or less. When prioritizing electrical conductivity and thermal conductivity, the amount of Si is 1.00 mass% or less.

[0044] (Zn) Zn, together with Cu and Si, is a major constituent element of the free-cutting copper alloy of this embodiment, and is an element necessary for improving machinability, strength, high-temperature properties, and castability. Although Zn is the balance, if forced to state, the Zn content is less than about 38.5 mass%, preferably less than 38.0 mass%, and more than about 32.0 mass%, preferably more than 33.0 mass%.

[0045] (P) Like Si, P is an essential element for reforming the β phase to the β1 phase. After solidification, P dissolves in the β phase together with Si. During the cooling process after solidification, the β1 phase is obtained by cooling the casting at a temperature of 500°C and in the temperature range from 500°C to 300°C at a cooling rate of more than 300°C / min. The reforming of the β phase to the β1 phase improves machinability and significantly improves the dezincification corrosion resistance and stress corrosion cracking resistance that were previously issues with the β phase. Meanwhile, compounds of P with Zn or Si reduce cutting resistance and improve chip breakability, but when the cooling process is initiated at a temperature above about 550°C or about 530°C and the cooling rate is above 300°C / min, P-containing compounds are absent or present in only small amounts. With regard to machinability, the effect of modifying the β phase to the β1 phase exceeds the effect of the presence of a compound of Si-containing β phase and P, and the effect of modifying to the β1 phase is significantly greater, especially during high-speed cutting. The inclusion of P improves the dezincification corrosion resistance of the α phase, leading to a significant improvement in the dezincification corrosion resistance of alloys consisting of the β1 and α phases.

[0046] To reform the β phase into the β1 phase, the P content must be at least 0.01 mass%. To further reform the β1 phase, the P content is preferably 0.03 mass% or more, more preferably 0.04 mass% or more, further improving dezincification corrosion resistance and machinability. P readily forms compounds with Zn, Si, Mn, Fe, Cr, Co, Al, and other elements. When P forms compounds with these elements, the amount of P dissolved in the β phase in the alloy decreases during the cooling process after solidification, preventing the transformation to the β1 phase. The formation of compounds between P and Zn and Si, the main elements of the present alloy, begins at approximately 550°C, and the amount of P compounds increases as the cooling rate slows. The formation of compounds between P and the inevitable impurities Mn, Fe, Cr, and Co begins at or above 550°C, and increasing the amounts of these elements further promotes the formation of P compounds. In other words, the presence of Mn, Fe, Cr, and Co hinders the transformation to the β1 phase, resulting in an increase in the cutting resistance of the alloy and a deterioration in dezincification corrosion resistance and stress corrosion cracking resistance. Therefore, the total content of at least Fe, Mn, Co, and Cr must be kept below 0.50 mass%, preferably below 0.35 mass%.

[0047] Although the formation of P-Zn and Si compounds has a positive effect on machinability, the transformation of the β phase to the β1 phase and the presence of P-Zn and Si compounds are fundamentally contradictory. As mentioned above, the formation of the β1 phase requires rapid cooling after solidification at 500°C and in the temperature range from 500°C to 300°C, whereas the sufficient formation of P-Zn and Si compounds requires slow cooling in the temperature range from about 530°C to about 450°C. Although the transformation of the β phase to the β1 phase and the formation of P compounds proceed in opposite directions, if the cooling rate increases rapidly during cooling, for example, at about 515°C, the β phase is simultaneously reformed while the P compounds are formed. However, in this case, the transformation of the β phase becomes somewhat insufficient.

[0048] On the other hand, even if P is contained in an amount of 0.18 mass% or more, the effect of forming the β1 phase is already saturated, and the P dissolved in the β1 phase reduces ductility and electrical conductivity. Therefore, the P content is less than 0.18 mass%, preferably 0.15 mass% or less, and more preferably 0.12 mass% or less.

[0049] (Pb) In this embodiment, the β1 phase containing Si and P provides good machinability for the alloy, but the inclusion of a small amount of Pb further improves machinability. In this composition, approximately 0.001 mass% of Pb is dissolved in the matrix, and any excess Pb exists as fine Pb particles with diameters of approximately 0.1 to approximately 2 μm. It is generally believed that a Pb content of approximately 0.1 mass% contributes little to improving machinability. For example, ASM Specialty Handbook, Copper and Copper Alloys, First Edition, August 2001, p. 267, Fig. 6, shows the relationship between the amount of Pb and machinability, assuming that the machinability of a Cu-Zn-Pb alloy containing 62 to 65 mass% Cu, approximately 3.2 mass% Pb, and the remainder Zn is 100%. As shown in Fig. 6 above, the addition of 0.1 mass% Pb only improves machinability by about 5%, reducing the machinability index from about 25% to about 30%. In contrast, in the present application, even trace amounts of Pb have a significant effect on machinability, and a Pb content of 0.002 mass% or more is effective. The Pb content is preferably 0.003 mass% or more, and more preferably 0.01 mass% or more. Furthermore, when cutting conditions become severe, such as when the cutting speed increases, the feed rate increases, the depth of cut increases, or the drill hole diameter increases, the Pb content is preferably 0.03 mass% or more. The machinability of the alloy is significantly improved by the β1 phase, which has significantly improved machinability, and the inclusion of a small amount of Pb. It is well known that Pb improves the machinability of copper alloys. For this reason, approximately 3 mass% of Pb is required in a Cu-Zn binary alloy, as exemplified by free-cutting brass rod C3604. In this embodiment, an alloy with excellent machinability is achieved by incorporating a β1 phase containing Si and P and a small amount of Pb particles, or Pb and Bi particles (described later), within the metal structure. However, because Pb is harmful to the human body, the upper limit of Pb is set to less than 0.20 mass%. Furthermore, the Pb content is preferably less than 0.10 mass%, and optimally 0.08 mass% or less, taking into account the impact on the human body and the environment.

[0050] (Bi) Like Pb, Bi dissolves in the matrix at approximately 0.0001 mass%, and any excess Bi exists as particles with diameters of approximately 0.1 to 2 μm. When both Pb and Bi are added, the Pb and Bi mixture generally exists as particles with diameters of approximately 0.1 to 2 μm. In this embodiment, it was found that by incorporating Bi together with Pb in the presence of the β1 phase, machinability equivalent to or superior to that achieved when Pb and Bi were each contained alone can be achieved. While the machinability-improving function of Bi was previously considered inferior to that of Pb, this embodiment has been found to exhibit the same effect as, and in some cases even greater than, Pb. Incidentally, Bi deteriorates the stress corrosion cracking resistance of brass, but when it exists as a mixture of Pb and Bi particles, or when the Bi content is small, its effect on stress corrosion cracking is almost eliminated.

[0051] When Bi is contained, at least 0.0001 mass% or more of Bi is required to have good machinability as an alloy even when a small amount of Pb is contained. The amount of Bi is preferably 0.001 mass% or more, more preferably 0.002 mass% or more. On the other hand, the amount of Bi is less than 0.20 mass%, preferably less than 0.10 mass%, and even more preferably 0.08 mass% or less. Furthermore, since Bi is more sensitive to cracking during casting than Pb, setting the amount as described above eliminates the risk of cracking during casting. Note that Bi can satisfactorily replace Pb, is a rare metal that has an environmental impact, and is also included in raw materials as an unavoidable impurity. Therefore, Bi is included as an optional element and may not be included. Furthermore, in consideration of the problems of environmental impact, stress corrosion cracking, and cracking during casting, the total content of Pb and Bi (compositional formula f2 described later) is set to less than 0.20 mass%, preferably less than 0.10 mass%.

[0052] (Sn) Sn dissolves in the β1 phase, further improving the dezincification corrosion resistance of the β1 phase and improving the dezincification corrosion resistance of the alloy. When Sn is contained, to obtain this effect, the Sn content must be more than 0.05 mass%, preferably 0.10 mass% or more. Incidentally, Sn is originally distributed more in the β phase and β1 phase than in the α phase, and a small amount of Sn improves dezincification corrosion resistance, but as the Sn concentration increases, the γ phase is more likely to form and the ductility decreases. The formation of the γ phase not only reduces the ductility of the alloy, but also reduces machinability and degrades dezincification corrosion resistance. In relation to the amount of Si, the Sn content must be kept at least less than 0.70 mass%, preferably less than 0.60 mass%, and more preferably 0.50 mass% or less.

[0053] As mentioned above, Sn is distributed in large amounts in the β phase and β1 phase, and it has been found that a high Sn content can cause problems in modifying the β phase containing Si and P. Specifically, it has been found that when the amount of Sn is greater than the amount of Si, the modification of the β phase becomes insufficient, and the effect of Sn content in improving dezincification corrosion resistance is canceled out. As will be described later, the amount of Si must exceed the amount of Sn.

[0054] (Inevitable Impurities, Particularly Fe, Mn, Co, and Cr / Al) In this embodiment, inevitable impurities include, for example, Mn, Fe, Al, Ni, Mg, Se, Te, Sn, Bi, Co, Ca, Zr, Cr, Ti, In, W, Mo, B, Ag, and rare earth elements. Conventionally, free-cutting copper alloys, particularly free-cutting brass containing approximately 30% or more of Zn, are primarily made from recycled copper alloys rather than high-quality raw materials such as electrolytic copper and electrolytic zinc. In downstream processes (downstream processing, machining processes) in this field, most components and parts are cut, resulting in a large amount of discarded copper alloy, at a ratio of 40 to 80 parts by mass per 100 parts by mass of raw material. Examples of such impurities include chips, scraps, burrs, runners, products with manufacturing defects, and discarded products. These discarded copper alloys are the primary raw materials. Inadequate separation of cutting swarf and scraps can result in the contamination of raw materials such as Pb, Fe, Mn, Si, Se, Te, Sn, P, Sb, As, Bi, Ca, Al, Zr, Ni, and rare earth elements from Pb-added free-cutting brass, Pb-free free-cutting copper alloys containing Bi, special brass alloys containing Si, Mn, Fe, and Al, and other copper alloys. Cutting swarf also contains Fe, W, Co, Mo, and other elements from tools. Recycled waste products, including plated products, can contain Ni, Cr, and Sn. Furthermore, pure copper scrap used in place of electrolytic copper can contain Mg, Sn, Fe, Cr, Ti, Co, In, Ni, Se, and Te. Brass-based scrap used in place of electrolytic copper or electrolytic zinc is often plated with Sn, resulting in Sn contamination.

[0055] From the viewpoint of resource reuse and cost considerations, scrap containing these elements is used as a raw material, at least to the extent that it does not adversely affect the properties. In the case of Pb-added free-cutting brass bar C3604 according to the JIS standard (JIS H 3250), the essential element Pb is contained in an amount of about 3 mass%, and impurities such as Fe of 0.5 mass% and Fe + Sn (the total amount of Fe and Sn) are permitted up to 1.0 mass%. Furthermore, in the case of Pb-added brass casting according to the JIS standard (JIS H 5120), the essential element Pb is contained in an amount of about 2 mass%, and the allowable limits for the remaining elements are Fe 0.8 mass%, Sn 1.0 mass%, Al 0.5 mass%, and Ni 1.0 mass%. In fact, free-cutting brass rods and brass castings may contain high concentrations of Fe, Sn, Al, and Ni, approaching the upper limit of the JIS standard.

[0056] Fe, Mn, Co, and Cr dissolve in the α and β phases of Cu-Zn alloys to a certain concentration. However, if Si or P is present, they tend to combine with the Si and P, potentially consuming the Si and P necessary for modifying the β phase. When combined with Si, Fe, Mn, Co, and Cr form Fe-Si compounds, Mn-Si compounds, Co-Si compounds, and Cr-Si compounds in the metal structure. Similarly, when combined with P, Fe, Mn, Co, and Cr form Fe-P compounds, Mn-P compounds, Co-P compounds, and Cr-P compounds in the metal structure. These intermetallic compounds are very hard, so they not only increase cutting resistance but also shorten tool life. Therefore, the amounts of Fe, Mn, Co, and Cr must be limited, and each content must be less than 0.35 mass%, preferably less than 0.25 mass%, and more preferably 0.15 mass% or less. In particular, the total content of Fe, Mn, Co, and Cr must be less than 0.50 mass%, preferably less than 0.35 mass%, more preferably less than 0.30 mass%, and even more preferably 0.25 mass% or less.

[0057] On the other hand, Al, which is mixed in from special brass rods, brass castings, etc., must be limited because a high content affects the modification and properties of the β phase. Furthermore, Al forms compounds with P or Si. In the alloy of this embodiment, the Al content must be less than 0.30 mass%, more preferably less than 0.15 mass%, and even more preferably 0.10 mass% or less.

[0058] As for other major unavoidable impurity elements, experience has shown that Ni is often mixed in from scrap, etc. Although Ni has a relatively small effect on mechanical properties such as machinability, it is necessary to limit its content in consideration of its effects on the human body. The Ni content is preferably less than 0.20 mass%, more preferably less than 0.10 mass%. As for Ag, Ag is generally considered to be Cu and has almost no effect on various properties, so there is no need to particularly limit its content, but the Ag content is preferably less than 0.05 mass%. Te and Se themselves have free machinability, and although rare, there is a risk of their being mixed in large amounts. In consideration of their effects on ductility and impact properties, the respective contents of Te and Se are preferably less than 0.10 mass%, more preferably less than 0.05 mass%, and even more preferably 0.02 mass% or less. In addition, corrosion-resistant brass contains As and Sb to improve the corrosion resistance of brass, but in consideration of ductility, the content of each of As and Sb is preferably less than 0.05 mass%, more preferably 0.02 mass% or less. The content of other elements such as Mg, Ca, Zr, Ti, In, W, Mo, B, and rare earth elements is preferably less than 0.05 mass%, more preferably less than 0.03 mass%, and even more preferably 0.02 mass% or less. The content of rare earth elements is the total amount of one or more of Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Tb, and Lu. As described above, the total amount of inevitable impurities other than Fe, Mn, Co, Cr, and Al is also preferably less than 0.70 mass%, more preferably less than 0.50 mass%.

[0059] (Compositional Relational Formula f1) Compositional Relational Formula f1 = [Cu] - 4.8 x [Si] + 0.5 x ([Pb] + [Bi]) - [P] - [Sn]. When the Sn content is 0.05 mass% or less, [Sn] in f1 is 0. When Bi is not contained, [Bi] in f1 is 0. When Sn is 0.05 mass% or less, the effect on compositional relational formula f1 is small, so compositional relational formula f1 does not specify it. Compositional relational formula f1 is an equation that expresses the relationship between composition and metal structure. Even if the amount of each element is within the range specified above, unless f1 satisfies the relational formula 57.3 ≦ f1 ≦ 60.8, the various properties targeted by this embodiment cannot be achieved. If the compositional formula f1 is less than 57.3, the proportion of β phase and β1 phase increases, resulting in insufficient modification of the β phase, and thus degraded dezincification corrosion resistance, stress corrosion cracking resistance, ductility, and impact properties. Therefore, the lower limit of the compositional formula f1 is 57.3 or more, preferably 58.0 or more, and more preferably 58.5 or more. As the compositional formula f1 falls within a more preferable range, the proportion of α phase increases, the modification of the β phase becomes sufficient, and excellent machinability is maintained while good dezincification corrosion resistance is achieved, resulting in good ductility and impact properties. On the other hand, the upper limit of the compositional formula f1 affects the proportion of β phase and β1 phase. If the compositional formula f1 is greater than 60.8, the proportion of β phase and β1 phase decreases. As a result, excellent machinability cannot be obtained and strength is reduced. The upper limit of f1 also affects castability. Castability and solidification temperature range are closely related, and exceeding the upper limit of f1 will result in a solidification temperature range exceeding 30°C, resulting in poor castability and an increase in defects in the final solidified portion. Therefore, the upper limit of the compositional relational formula f1 is 60.8 or less, preferably 60.5 or less, and more preferably 60.1 or less. Depending on the composition and process, as the value of the compositional relational formula f1 decreases, the amount of β1 phase increases, machinability improves, strength increases, the solidification temperature range narrows, and castability improves.

[0060] (Compositional Relational Formula f2) Bi is an optional element that substitutes for the function of Pb. However, when Bi is included, the following relational formula must be satisfied: 0.003≦f2=[Pb]+[Bi]<0.20. In other words, considering that Bi is a rare metal and has an environmental impact, the total amount of Pb and Bi must be limited. Furthermore, both Pb and Bi are low-melting-point metals and exist as metal particles in the metal structure, which may cause cracking during casting and therefore must be limited. Therefore, when Bi is included, the total amount of Pb and Bi must be less than 0.20 mass%, which is the upper limit for the amount of Pb, and preferably less than 0.10 mass%. On the other hand, when Bi is included to obtain good machinability, the total amount of Pb and Bi must be 0.003 mass% or more, and preferably 0.004 mass% or more.

[0061] (Compositional formula f0) Sn is contained to further improve dezincification corrosion resistance. Sn is contained in large amounts in the β phase, and the greater the amount of Sn, the more the dezincification corrosion of the β1 phase slows down. On the other hand, if the amount of Sn is greater than the amount of Si, it may hinder the modification of the β phase, resulting in a deterioration of dezincification corrosion resistance and machinability. In other words, when f0 = [Sn] / [Si], it has been found that in order to achieve an effect commensurate with the inclusion of Sn taking other properties into consideration, f0 must be less than 0.8. Note that f0 is preferably less than 0.65, and more preferably less than 0.50.

[0062] The free-cutting copper alloy casting of this embodiment, while containing a large amount of conventional β phase (in this application, β1 phase), exhibits excellent dezincification corrosion resistance and stress corrosion cracking resistance. It also possesses the contradictory properties of machinability, which requires low cutting resistance and a type of brittleness that allows chips to be broken into small pieces, and ductility and impact resistance. To achieve these excellent corrosion resistance, machinability, and mechanical properties, detailed consideration of not only the composition of each component but also the compositional relations f1, f2, and f0, as well as the structural relations f3 to f5 and the structural / compositional relation f6 described below, can provide an alloy more suited to the intended purpose and application. Note that Fe, Mn, Co, Cr, Al, and the separately defined inevitable impurities are not specified in the compositional relational expression f1 because their influence on the compositional relational expression f1 is minimal within the range of the inevitable impurities.

[0063] (Comparison with Patent Documents) Tables 1 to 4 show the results of comparing the compositions of the Cu-Zn-Si alloys and the like described in Patent Documents 1 to 16 with the alloy of this embodiment.

[0064]

[0065]

[0066]

[0067]

[0068] The present embodiment and Patent Document 9 differ in the contents of the major elements Si and Cu, the present embodiment and Patent Document 10 differ in the content of the major element Si, and the present embodiment and Patent Document 16 differ in the content of the major element Cu. Patent Documents 1 and 2 do not contain Si. Patent Documents 2, 14, and 16 state that Pb is not contained, and the Pb content is different. Patent Documents 9, 11, 12, and 13 significantly limit the β phase in the metal structure from the viewpoints of machinability, dezincification corrosion resistance, corrosion resistance, and the like. Although the β1 phase and the β phase are completely different, Patent Documents 9, 11, 12, and 13 specify the β phase to be 5% or less, 25% or less, 15% or less, and 0.9% or less, respectively.

[0069] Patent Document 11 relates to a near-net-shape tubular hot-forged product, and uses a tubular material. Patent Documents 2 and 10 state that heat treatment is performed at temperatures of 350 to 550°C or 400 to 600°C to reduce the β phase and to disrupt the β phase. Patent Document 10 describes a steel containing 0.2 mass% or more of Sn, containing Sn and Si to improve the dezincification corrosion resistance of the β phase, hot extrusion at temperatures of 700°C or higher to improve machinability, and heat treatment at 400 to 600°C to improve corrosion resistance. The proportion of the β phase is approximately 5 to 20%, and the Si content is 0.1 to 0.4 mass%, and may be controlled at 0.2 mass% or less.

[0070] In Patent Documents 13, 14, and 15, Al is essential for improving discoloration resistance, castability, and dezincification corrosion resistance. Patent Document 15 requires the inclusion of at least 0.1 mass% or more of Sn and Al each to improve dezincification corrosion resistance, and large amounts of Pb and Bi to obtain excellent machinability. Patent Document 16 requires the inclusion of a γ phase without Pb, and includes 65 mass% or more of Cu and Si, as well as trace amounts of Al, Sb, Sn, Mn, Ni, B, etc., to provide a corrosion-resistant copper alloy casting with good mechanical properties and castability.

[0071] Patent Documents 3 to 8 all require that the cooling process after casting and solidification or hot working be performed at an average cooling rate of about 0.1°C / min to about 70°C / min in the temperature range from about 530°C to about 450°C, resulting in the formation of P compounds present in the metal structure. Furthermore, they state that the γ phase is effective for machinability, but make no mention of modifying the β phase. They are silent on dezincification corrosion resistance and stress corrosion cracking resistance, and no data is disclosed. Furthermore, no data is disclosed regarding cutting resistance under high-speed cutting conditions. In the present application, the cooling process after casting and solidification is performed at a cooling rate exceeding 300°C / min when the casting temperature reaches 500°C, i.e., in the temperature range just above 500°C, and preferably begins at a temperature below 700°C and above 500°C, with an average cooling rate exceeding 300°C / min from 500°C to 300°C. This cooling is essentially contrary to Patent Documents 3 to 8. In the present application, compounds of P with Zn or Si may be present, but the amount of P compounds present is small, if any.

[0072] The most significant and clear difference between the present application and Patent Documents 3 to 8 is that none of Patent Documents 3 to 8 mentions the modification of the β phase or the modified β phase, i.e., the β1 phase. During cooling after solidification, the β phase containing solid solution Si and P is modified to the β1 phase by cooling at a cooling rate exceeding 300°C / min from 500°C and cooling at an average cooling rate exceeding at least 300°C / min in the temperature range from 500°C to 300°C. The β phase is not modified when cooling at an average cooling rate of about 0.1°C / min to about 70°C / min in the temperature range from about 530°C to about 450°C. Furthermore, when etched with a mixture of hydrogen peroxide and aqueous ammonia, grain boundaries can be observed within the β1 phase. However, even if the material contains a predetermined amount of Si and P, if the β phase remains unmodified, no grain boundaries can be observed within the β phase. Patent Documents 3 to 8 disclose metal structures etched with a mixture of hydrogen peroxide and aqueous ammonia, but in none of them are grain boundaries observed within the β phase.

[0073] Unlike conventional β phases, the β1 phase significantly improves dezincification corrosion resistance and stress corrosion cracking resistance. Furthermore, the machinability is further improved, and the presence of the β1 phase exceeds the machinability achieved when a P compound is present in addition to a Si-containing β phase. However, to achieve this, the β1 phase must be present in an area ratio of more than 25% in the metal structure. Furthermore, while the present application claims that the presence of a γ phase impairs machinability, Patent Documents 3 to 8 claim that the γ phase is effective in improving machinability.

[0074] <Metal structure> Cu-Zn-Si alloys contain more than 10 types of phases, and complex phase changes occur, so the desired properties cannot necessarily be obtained by simply determining the composition range and elemental relationships. Ultimately, the desired properties can be obtained by identifying and determining the types of phases present in the metal structure and the range of their area ratios. Therefore, the structure relationships are specified as follows: 20≦f3=(α)<75, 25<f4=(β1)≦80, where β1 phase is a modified β phase. 0≦f5=(γ)<4

[0075] (β1 Phase) The metal structure of this application is composed of α phase, β1 phase, and in some cases, a small amount or no γ phase. The metal structure only covers the above-mentioned constituent phases. In addition to the constituent phases, the metal structure may contain precipitates, crystallized particles, such as P-containing compounds and Si-containing compounds, Pb or Bi particles, oxides, sulfides, and inclusions. Castings often contain more oxides and crystallized particles than hot-extruded materials. The β phase and β1 phase are easily distinguishable. When the β1 phase is etched with a mixture of hydrogen peroxide and aqueous ammonia, grain boundary patterns, i.e., crystal boundaries, are observed within the β1 phase. However, in the case of the β phase, no crystal boundaries are observed within the β phase.

[0076] The β1 phase in this embodiment is obtained by maintaining the β phase, in which a certain amount of Si and P are dissolved, at a high temperature above 500°C after solidification, i.e., approximately 500-700°C, and then cooling it from that temperature range (cooling at a cooling rate of at least 300°C / min at 500°C and an average cooling rate from 500°C to 300°C, and continuing to cool to near room temperature) to maintain the metal structure state at 500-700°C to room temperature. Specifically, the cooling rate is increased in the temperature range from the cooling treatment start temperature of 500-700°C to 300°C, and the alloy is rapidly cooled to room temperature below 100°C. This maintains the metal structure state at 500-700°C. As a result, the β1 phase is obtained. A similar cooling process cannot be performed on the β phase of a Cu-Zn alloy that does not contain both the predetermined amounts of Si and P. Similarly, if an alloy containing a given amount of Si and P is cooled at a cooling rate of 300°C / min or less at 500°C, the β1 phase cannot be obtained. If the temperature range from 500°C to 300°C is cooled at an average cooling rate of 300°C / min or less, the β1 phase cannot be obtained. Cooling treatment from temperatures lower than 500°C, such as 450°C, also does not result in the β1 phase. Furthermore, a certain amount of α phase is required to modify the β phase; if the amount of α phase is small, the β phase will not be modified and the β1 phase will not be obtained. Furthermore, the degree of modification of the β phase is also affected by the amounts of Si and P, the amounts of unavoidable impurities such as Fe and Al, the cooling rate at 500°C, the average cooling rate from 500°C to 300°C, and the starting temperature of the cooling treatment. Improving the degree of modification of the β phase, i.e., the β1 phase being more modified, results in a material with better machinability, dezincification corrosion resistance, and stress corrosion cracking resistance. The degree of modification of the β phase begins to roughly saturate when the amount of Si is about 1 mass % and the amount of P is about 0.1 mass %, and if these amounts are too high, there is a risk of causing adverse effects such as deterioration in thermal conductivity, electrical conductivity, ductility, and the appearance of the γ phase.

[0077] The modified β1 phase can overcome the drawbacks of the β phase in Cu—Zn-based alloys, which have been major issues with the alloy's dezincification corrosion resistance and stress corrosion cracking resistance. That is, as an example, expressed in specific figures, the progression of dezincification corrosion can be delayed by approximately half or even less. As described in Patent Document 2, dezincification corrosion of Cu—Zn-based alloys containing a β phase is a major problem. Since dezincification corrosion occurs first along the β phase, the amount of β phase is limited to 25% or less or 20% or less, and heat treatment at 350 to 550°C is performed to further reduce the amount of β phase and to disrupt the β phase. While strength largely depends on the area ratio of the constituent phases, the modified β phase, i.e., the β1 phase, has higher strength than the β phase and better ductility and impact properties than the β phase, resulting in an alloy with a good strength-ductility balance.

[0078] (β1 phase, structural formula f4) In the Cu—Zn—Si—P—Pb alloy, which is the free-cutting copper alloy of this embodiment, in order to achieve good machinability while minimizing the Pb content, the β1 phase must have an area ratio of at least more than 25%. Furthermore, in order to improve machinability and strength, the β1 phase is preferably 30% or more, more preferably 33% or more. On the other hand, if the β1 phase is too high, for example, 95%, the β phase is not modified. Because the β phase is modified in the presence of the α phase, a certain amount of α phase is necessary. Furthermore, with regard to dezincification corrosion and stress corrosion cracking, although the β1 phase significantly slows the progression of dezincification corrosion and stress corrosion cracking compared to the β phase, it is still inferior to the α phase in dezincification corrosion resistance and stress corrosion cracking resistance. Specifically, with regard to dezincification corrosion, when a dezincification corrosion test according to ISO 6509 is performed on a Cu-Zn alloy whose metal structure is composed of α and β phases, the β phase is selectively dezincified first, and dezincification corrosion progresses, ultimately reaching a dezincification corrosion depth of approximately 500 to 550 μm. On the other hand, in the present alloy whose metal structure is composed of α and β1 phases, although the β1 phase is selectively dezincified, the dezincification corrosion depth is approximately 20 to 240 μm, and the progression of dezincification corrosion is significantly suppressed compared to when the metal structure is composed of α and β phases. In this way, the β phase is reformed to the β1 phase, and although the dezincification corrosion resistance is significantly improved, the dezincification corrosion resistance and impact properties are inferior to those of the α phase. Therefore, if the area ratio of the β1 phase is high, the dezincification corrosion resistance and impact properties of the alloy will be deteriorated. Based on the above, and as a result of extensive research, it has been determined that the area ratio of the β1 phase needs to be set to 80% or less, preferably 70% or less, and more preferably 65% ​​or less. The unmodified β phase is distinguished as structure formula f4A.

[0079] (α phase, structural relational expression f3) The metal structure of the present application is basically composed of α phase and β1 phase. A cooling treatment is performed to transform the β phase into β1 phase, but the α phase is hardly affected by the cooling treatment. Furthermore, a certain amount of α phase is required to transform the β phase. If there is too much β1 phase, the alloy's ductility and impact properties will be affected, so an appropriate amount of ductile α phase is required. Conversely, if there is too much α phase, the strength will be reduced. Furthermore, α phases containing Si only slightly improve machinability compared to α phases without Si, and the amount of α phase is therefore limited, especially from the viewpoint of machinability. However, even if an alloy is composed of a β1 phase with excellent machinability and an α phase with somewhat poor machinability, the soft α phase acts as a cushioning material during cutting or as a stress concentration source at the boundary with the hard β1 phase. Therefore, even if the alloy contains up to approximately 75% α phase, the cutting resistance of the alloy is maintained low and chips are broken. Because the α phase acts as a cushioning material during cutting and as a stress concentration source at the boundary with the β1 phase, a fine, granular α phase is preferred. Based on extensive research into the modification of the β phase and the alloy's dezincification corrosion resistance, stress corrosion cracking resistance, machinability, and mechanical properties, the amount of α phase must be at least 20%, preferably at least 30%, and more preferably at least 35%. On the other hand, the upper limit of the α phase is less than 75%, preferably 70% or less, and more preferably 67% or less.

[0080] (γ Phase, Structure Relationship Formula f5) As described in Patent Documents 9 and 11, the γ phase contributes to machinability in Cu—Zn—Si alloys having a Cu concentration of approximately 69 to 80 mass% and a Si concentration of approximately 2 to 4 mass%. Patent Document 16 states that the γ phase is essential in Pb-free Cu—Zn—Si alloys. Furthermore, Patent Documents 3 to 7 also state that the Si-containing β phase has good machinability, while the Si-containing γ phase also contributes to machinability. In this embodiment, the γ phase is considered to hinder the machinability of the alloy, and is assigned a negative coefficient greater than the coefficient for the amount of β phase in the structure-composition relationship formula f6 described below. Furthermore, the γ phase impairs impact properties and reduces dezincification corrosion resistance. This is because, in this embodiment, the β phase is modified but the γ phase is not. In Cu—Zn—Si alloys, the appearance of the γ phase may be unavoidable, but must at least be limited. That is, the proportion (area ratio) of the γ phase needs to be less than 4%, preferably less than 2%, more preferably less than 1%, and optimally, no γ phase is present, i.e., f5=0.

[0081] (Structure-composition relationship formula f6) f6 = (β1) × (-0.5 × [Si] 2 +1.5×[Si])-2×(γ)+([Pb]+[Bi]) 1/2 ×25+([P]) 1/2 ×12 The structure-composition relational expression f6 is a simple conditional expression for obtaining good machinability as an alloy. f6 is organized as a positive effect of the amount of β1 phase, the amount of Si contained in the alloy within the composition range of the present application, the amount of Pb and Bi, and the amount of P, and is organized as a negative effect of the amount of γ phase. That is, it is a β1 phase containing Si and P, and the amount of β1 phase is multiplied by (-0.5 × [Si] 2 +1.5×[Si]), the sum of the amounts of Pb and Bi multiplied by a coefficient of 25, the amount of P multiplied by a coefficient of 12, and the amount of γ phase multiplied by a coefficient of 2 from the sum of these.

[0082] The performance of the β1 phase is directly affected by the Si concentration, which in turn is affected by the P concentration. Furthermore, the inclusion of very small amounts of Pb or Bi improves machinability. On the other hand, in the present application, the γ phase inhibits machinability. It has been discovered that the degree of improvement in machinability due to Pb or Bi is closely related to the ½ power of the amount of Pb and Bi. Even very small amounts of Pb and Bi exert a significant effect, and as the content increases, the effect of improving machinability increases, but the effect gradually becomes more gradual. In alloys composed of a β1 phase with a modified β phase, a small amount of Pb or Bi exerts a significant effect on machinability, an effect that cannot be achieved by the relationship between the Pb content and machinability of conventional Cu-Zn-Pb alloys.

[0083] As a result of extensive research, it has been found that in order to obtain good machinability, the value of the structure-composition relationship f6 should be greater than 28, preferably greater than 35, and even more preferably greater than 40, approaching the machinability of free-cutting brass rods containing 3 mass% Pb. Meanwhile, machinability peaks when the value of the structure-composition relationship f6 is approximately 55-80, and as the value of f6 increases, machinability actually decreases. This is because the effect of the amount of β1 phase on machinability saturates at approximately 60%, and the effect of Si on machinability saturates at roughly 1 mass%. Even for alloys composed of unmodified β phase, the amount of β phase f4A (β phase) is substituted for the amount of β1 phase f4 (β1 phase), and this is applied to the formula for f6 to calculate a reference value, f6A.

[0084] 1A to 5B show metallographic photographs of various alloy castings and photographs of the results of ISO 6509 dezincification corrosion tests. FIG. 1A is a photograph of the microstructure of a copper alloy casting according to an embodiment. The copper alloy casting was obtained by subjecting Alloy No. S02 to Process No. A1. Specifically, Alloy No. S02 has a composition of Zn-62.9 mass% Cu-0.94 mass% Si-0.082 mass% P-0.067 mass% Pb-0.03 mass% Sn. Process No. In the case of alloy No. A1, the alloy was tapped at 1,080°C and cast into a sand mold, removed from the sand mold at 650°C, and cooling treatment was initiated at 560°C, with an average cooling rate of 900°C / min in the temperature range from 550°C to 500°C and an average cooling rate of 900°C / min in the temperature range from 500°C to 300°C. Figure 1B shows the results of a dezincification corrosion test performed on the alloy casting of Figure 1A in accordance with the ISO 6509 test method, and is a cross-sectional metallographic photograph including the portion exhibiting the maximum corrosion depth. Figure 2A is a photograph of the structure of a copper alloy casting according to an embodiment, which was obtained by performing Process No. A14H on Alloy No. S02. Specifically, Alloy No. S02 has a composition of Zn-62.9 mass% Cu-0.94 mass% Si-0.082 mass% P-0.067 mass% Pb-0.03 mass% Sn. In Process No. A14H, the alloy was tapped at 1,080°C and cast into a sand mold, removed from the sand mold at 650°C, and naturally cooled in that state, with an average cooling rate of 20°C / min in the temperature range from 500°C to 300°C. Figure 2B shows the results of a dezincification corrosion test performed on the alloy casting of Figure 2A in accordance with the ISO 6509 test method, and is a cross-sectional metallographic photograph including the area exhibiting the maximum corrosion depth.

[0085] 3A is a photograph of the structure of a copper alloy casting according to an embodiment. The copper alloy casting was obtained by subjecting Alloy No. S12 to Process No. B1. Specifically, Alloy No. S12 has a composition of Zn-63.6 mass% Cu-1.04 mass% Si-0.070 mass% P-0.062 mass% Pb-0.003 mass% Bi. In Process No. B1, the molten metal was poured into a mold at 960°C, removed from the mold at 750°C, and cooled at 560°C. The average cooling rate in the temperature range from 550°C to 500°C was 1020°C / min, and the average cooling rate in the temperature range from 500°C to 300°C was 1020°C / min. Figure 3B shows the results of a dezincification corrosion test performed on the alloy casting of Figure 3A according to the ISO 6509 test method, and is a cross-sectional metallographic photograph including the portion exhibiting the maximum corrosion depth. Figure 4A shows a microstructure observation photograph of a copper alloy casting according to an embodiment, obtained by performing Process No. B11H on Alloy No. S12. Specifically, Alloy No. S12 has a composition of Zn-63.6 mass% Cu-1.04 mass% Si-0.070 mass% P-0.062 mass% Pb-0.003 mass% Bi. In Process No. B11H, the molten metal was poured into a mold at 960°C and removed from the mold at 750°C, with an average cooling rate of 40°C / min in the temperature range from 500°C to 300°C. FIG. 4B shows the results of a dezincification corrosion test performed on the alloy casting of FIG. 4A in accordance with the ISO 6509 test method, and is a cross-sectional metallographic photograph including the portion exhibiting the maximum corrosion depth.

[0086] 5A is a photograph of the structure of a copper alloy casting according to an embodiment. The copper alloy casting was obtained by subjecting Alloy No. S02 to Process No. A14H and Process No. G1. Specifically, Alloy No. S02 had a composition of Zn-62.9 mass% Cu-0.94 mass% Si-0.082 mass% P-0.067 mass% Pb-0.03 mass% Sn. In Process No. A14H, the alloy was tapped at 1,080°C and cast into a sand mold, removed from the sand mold at 650°C, and naturally cooled. The average cooling rate in the temperature range from 500°C to 300°C was 20°C / min. The resulting casting was then subjected to Process No. G1. For G1, the casting was heated at 580°C for 20 minutes, and cooling treatment was started from 575°C, with an average cooling rate of 1200°C / min in the temperature range from 550°C to 500°C, and an average cooling rate of 1200°C / min in the temperature range from 500°C to 300°C. Figure 5B shows the results of a dezincification corrosion test performed on the alloy casting of Figure 5A in accordance with the ISO 6509 test method, and is a cross-sectional metallographic photograph including the portion exhibiting the maximum corrosion depth.

[0087] As shown in Figures 1A, 3A, and 5A, the grain boundary patterns are clearly visible within the β1 phase in the sand casting, the permanent metal casting, and the heat-treated sand casting. Here, "grain boundary" refers to the linear pattern that penetrates the β1 phase grains, as seen in Figure 1A. On the other hand, in Figures 2A and 4A, no grain boundary-like pattern is observed within the β phase, and the difference between the two is clear. Instead, in Figures 2A and 4A, numerous fine black granular precipitates are observed, primarily within the β phase and at the phase boundary between the β and α phases. Conversely, in Figures 1A, 3A, and 5A, only a few black granular precipitates are observed.

[0088] As seen in Figures 2A and 4A, numerous black granular precipitates, approximately 0.5 to 3 μm in size, are present primarily within the β phase and at the phase boundary between the β and α phases. The granular precipitates are primarily compounds of P with either Zn and / or Si, known as P compounds. Furthermore, some inclusions, such as Pb particles, mixed particles of Pb and Bi, compounds of Fe, Mn, etc. with P or Si, compounds of Al with P or Si, and oxides, are also present. While these compounds and inclusions can be identified by microscopic observation, they are somewhat difficult to distinguish from printed photographs. In Figures 2A and 4A, approximately 300 P compounds are present within the field of view of the printed photographs. In Figures 1A, 3A, and 5A, fine granular P compounds are absent or present only in small amounts, at least one-tenth the number of compounds in Figures 2A and 4A. Whether or not grain boundaries exist within the β1 phase or the β phase based on the cooling history of each sample, and whether or not there are many P compounds, depend on the cooling rate at the time when the temperature of the casting reaches 500°C, i.e., in the temperature range just above 500°C, and whether the average cooling rate from 500°C to 300°C is faster or slower than 300°C / min. In this application, the cooling rate at the time when the temperature of the casting reaches 500°C, i.e., in the temperature range just above 500°C, is defined as the average cooling rate from 550°C to 500°C. If the cooling treatment start temperature is lower than 550°C, the average cooling rate from the cooling treatment start temperature to 500°C is defined.

[0089] The results of ISO 6509 dezincification corrosion tests on these alloys are shown in Figures 1B, 2B, 3B, 4B, and 5B. The magnifications in Figures 1B, 3B, and 5B are twice those in Figures 2B and 4B. The maximum corrosion depths of the samples in which grain boundaries were observed within the β1 phase (Figures 1A, 3A, and 5A) were all 110 μm or less (Figures 1B, 3B, and 5B). However, the maximum corrosion depths of the samples in which grain boundaries were not observed within the β phase (Figures 2A and 4A) were 480 μm and 420 μm, respectively (Figures 2B and 4B), a difference of more than three times. However, the dezincification corrosion morphology in all cases was selective corrosion of the β1 and β phases. Even in the case of a modified β1 phase, the β1 phase is preferentially corroded by dezincification, just like the β phase, but the progress of dezincification corrosion of the β1 phase can be delayed to at least about 1 / 2, or even to about 1 / 3 or less, compared to the β phase.

[0090] <Characteristics> (Strength, toughness, ductility) Generally, compared to materials that have undergone hot processing, such as hot extruded rods, castings have elemental segregation, large crystal grains, and contain some inclusions such as oxides and microscopic defects. For this reason, castings are said to be "brittle" compared to hot-processed materials, and a high impact value is desirable in evaluating toughness and ductility. On the other hand, materials that excel in chip breakability during cutting require a certain degree of brittleness. Impact properties and machinability are, in some respects, contradictory properties.

[0091] There is a strong demand for thinner and lighter materials and components, such as drinking water appliances, that are the target of use in this embodiment. For example, in drinking water appliances, thinner materials and lighter weight can be achieved by providing materials with good corrosion resistance and high strength. As mentioned above, castings can have component segregation and microscopic defects, and are not often used for components that undergo cold working such as crimping or components that require ductility during use. In this embodiment, hardness (Vickers hardness, Rockwell hardness) is used to evaluate strength, in accordance with the properties of the castings, and impact test values ​​(U-notch) are used to evaluate toughness and ductility.

[0092] In order for a copper alloy casting to have high strength, it is preferable that the Vickers hardness is at least 100 Hv or more and the Rockwell B scale hardness is at least 52. More preferably, the Vickers hardness is at least 110 Hv and the Rockwell B scale hardness is at least 60. There is a correlation between hardness, tensile strength and yield strength, and in this embodiment, the Vickers hardness of 100 Hv is approximately 400 N / mm 2 Tensile strength of approximately 120 N / mm 2 Incidentally, brass casting CAC203 containing 1 to 2 mass% of Pb has a Vickers hardness of approximately 75 Hv, a Rockwell B scale hardness of approximately 30, and a tensile strength of approximately 350 N / mm 2 , yield strength is about 80N / mm 2 is.

[0093] As mentioned above, the casting must not only have high strength but also be at least not brittle, i.e., be a tough material that can withstand impact. To this end, when a Charpy impact test is carried out using a U-notch test piece, the Charpy impact test value is preferably 25 J / cm 2 More preferably, 30 J / cm 2 On the other hand, for example, the Charpy impact test value is about 70 J / cm 2 If the temperature exceeds this value, the viscosity of the material increases, which increases the cutting resistance and makes it easier for chips to form continuous pieces, resulting in poor machinability.

[0094] (Conductivity) Applications of this embodiment include electrical and home appliance parts, automotive parts, etc., and it is also a replacement material for brass casting CAC203 and bronze casting CAC406, which contain Pb. Currently, for the above applications, phosphor bronze (JIS standards, C5191 and C5210) containing 6 mass% or 8 mass% Sn is widely used in wrought copper products. The electrical conductivities of these copper alloys are approximately 14% IACS and approximately 12% IACS, respectively, while the electrical conductivities of CAC203 and CAC406 are approximately 24% IACS and approximately 15% IACS, respectively. Therefore, as long as the electrical conductivity of the copper alloy of this embodiment is 15% IACS or higher, no problems with electrical conductivity will arise. Note that the upper limit of electrical conductivity is not particularly specified, since improved conductivity poses almost no practical problems.

[0095] (Castability) The primary premise of the free-cutting copper alloy casting of this embodiment is that it produces a sound casting. First, the inclusion of Si suppresses Zn vapor during melting, allowing for good melting and casting. Furthermore, the inclusion of Si and the limited amounts of Cu, Zn, and f1 provide good fluidity, allowing the molten metal to penetrate thin-walled sections, enabling complex shapes to be cast, and reducing the occurrence of casting defects such as porous shrinkage cavities. Furthermore, the casting must be free of cracks. Regarding casting cracks, the primary consideration is whether or not a low-melting-point metal is present as a molten metal at high temperatures after solidification. If a low-melting-point metal is present, this is determined by its amount and whether or not the matrix is ​​ductile at high temperatures. In this embodiment, the total amount of low-melting-point metals Pb and Bi present as a molten metal in the matrix during the solidification and cooling process of the casting is significantly limited to less than 0.20 mass%, making casting cracks unlikely. Furthermore, if the composition and various relational expressions of this embodiment are satisfied, the alloy contains a large amount of β1 phase, which has excellent ductility at high temperatures, and this can cover the adverse effects of the low-melting-point metal contained in small amounts, eliminating the problem of cracking of the casting.

[0096] <Manufacturing Process> Next, a method for manufacturing a free-cutting copper alloy casting according to an embodiment of the present invention will be described. The metal structure of the free-cutting copper alloy casting according to this embodiment varies not only depending on the composition but also on the manufacturing process. Various casting methods, such as metal mold casting, sand casting, continuous casting, die casting, and lost-wax casting, are available for manufacturing castings. The cooling rate of the casting after solidification is largely determined by the thickness and shape of the casting, and the material and thickness of the metal mold or sand mold. The cooling rate can be changed by various cooling methods, such as heat retention, water cooling, oil cooling, and forced air cooling. Meanwhile, various changes in the metal structure occur during the cooling process after solidification, and the metal structure changes significantly depending on the cooling rate. Changes in the metal structure refer to significant changes in the types of constituent phases and the amounts (area fractions) of those constituent phases. As a result of extensive research into the cooling process after solidification, it was found that the cooling rate at 500°C and the average cooling rate in the temperature range from 500°C to 300°C are the most important factors during the cooling process, significantly affecting dezincification corrosion resistance and machinability.

[0097] (Melting and Casting) Depending on the casting method, melting is performed at a temperature of about 950 to 1200°C, which is about 100 to 300°C higher than the melting point (liquidus temperature) of the alloy of this embodiment. Molten metal at a temperature of about 900 to 1150°C, which is about 50 to 250°C higher than the melting point, is poured into a predetermined mold such as a metal mold, sand mold, or die, and cooled. After solidification, the constituent phases change in various ways.

[0098] (Pouring (Casting) and Solidification) The cooling rates after casting and solidification vary depending on the weight, thickness, and thermal conductivity of the cast copper alloy, as well as the material of the mold, such as a sand mold or a metal mold. When a conventional copper alloy casting is cast into a mold made of copper alloy or iron, i.e., in the case of permanent mold casting, the casting is removed from the mold at a temperature of about 750°C or lower after casting and is air-cooled or slowly cooled at an average cooling rate of about 10 to 200°C / min in the temperature range from 500°C to 300°C. Since most copper alloy castings contain 1 mass% or more of Pb or Bi, they are rarely cooled at a cooling rate of 300°C / min or higher in the temperature range above about 300°C or about 250°C, at which Pb or Bi solidifies. This is because when the temperature of the casting is 300° C. or higher, the Pb particles or Bi particles are in a molten state, and if the cooling rate is too fast, there is a risk that the casting will crack due to thermal contraction.

[0099] In continuous casting, cooling is performed in roughly the same manner as in permanent mold casting. The cast rod emerging from the iron mold is generally air-cooled, with the cooling rate primarily determined by the cross-sectional area of ​​the continuously cast rod and the casting speed. For a 20 mm diameter continuously cast rod, cooling occurs at an average cooling rate of approximately 40 to 100°C / min in the temperature range from 500°C to 300°C. In sand casting, the copper alloy cast into the sand mold is often cooled at an average cooling rate of approximately 0.6 to 60°C / min in the temperature range from 500°C to 300°C, depending on the size of the casting and the material and size of the sand mold. When the temperature drops below approximately 300°C or approximately 250°C, the casting is either removed from the sand mold and air-cooled, or left to cool to near room temperature while still in the sand mold. The cooling rate at 500°C for these castings is roughly the same as or slightly faster than the average cooling rate in the temperature range from 500°C to 300°C.

[0100] In the free-cutting copper alloy casting of this embodiment, after being cast and solidified, at a high temperature of, for example, 800°C, the metal structure is a single β phase. Subsequent cooling results in the formation of various phases, such as α phase and γ phase. In the free-cutting copper alloy casting of this embodiment, during the cooling process after solidification, the cooling rate exceeds 300°C / min when the casting temperature reaches 500°C, and the average cooling rate from 500°C to 300°C is adjusted to exceed 300°C / min, thereby reforming the β phase to the β1 phase. The cooling treatment continues even at temperatures below 300°C. Here, when the cooling treatment start temperature is lower than 550°C, the cooling rate at 500°C is taken as the average cooling rate from the cooling treatment start temperature to 500°C.

[0101] A preferred cooling method is to start the cooling process after solidification in a temperature range of 700°C to 500°C. The average cooling rate from the cooling start temperature to 500°C is roughly the same as the average cooling rate from 500°C to 300°C. After the casting temperature reaches 300°C, the cooling process continues even at temperatures below 300°C. The average cooling rate is slightly slower than the average cooling rate from 500°C to 300°C, but is roughly the same. In some cases, the cooling start temperature cannot be specified. If the cooling rate exceeds 300°C / min when the casting temperature reaches 500°C, and the average cooling rate from 500°C to 300°C is then increased to exceed 300°C / min. If the metallographic structure requirements are met, the β phase will be reformed to the β1 phase.

[0102] These cooling processes transform the β phase into the β1 phase, and when etched with a mixture of hydrogen peroxide and ammonia, grain boundaries appear within the β1 phase, which is transformed into the β1 phase, which has different properties from the conventional β phase, replacing it. As a result, machinability is improved and dezincification corrosion resistance, which was a problem with the conventional β phase, is significantly improved.

[0103] The degree of β-phase modification is affected by the amounts of Si and P, Al, Fe, and Sn, the value of the compositional relation f1, and the amount of α-phase. It is also affected by the average cooling rate from 500°C to 300°C during the cooling process after solidification, the cooling rate at 500°C, and the starting temperature of the cooling treatment. If the starting temperature of the cooling treatment is 700°C or higher, the proportion of β-phase increases, which may result in insufficient modification of the β-phase. The starting temperature of the cooling treatment is preferably lower than 700°C, more preferably 650°C or lower. On the other hand, if the cooling rate is 300°C / min or lower when the casting temperature is 500°C, or if the starting temperature of the cooling treatment is 500°C or lower, the β-phase will not be modified. Starting the cooling treatment at a temperature of preferably 530°C or higher, more preferably 550°C or higher, further modifies the β-phase, improving the dezincification corrosion resistance and machinability of the alloy.

[0104] Furthermore, if the average cooling rate from 500°C to 300°C after the start of the cooling treatment is 300°C / min or less, the β phase will not be reformed. The average cooling rate in the temperature range from 500°C to 300°C should be at least 300°C / min or more, preferably more than 600°C / min, and more preferably 900°C / min or more. Cooling at a preferred cooling rate converts the β phase to a more reformed β1 phase, resulting in better dezincification corrosion resistance and machinability. The upper limits of the cooling rate at 500°C and the average cooling rate in the temperature range from 500°C to 300°C are sufficient if they are achieved using conventional production equipment, and although no particular restrictions are imposed, a cooling rate of approximately 9000°C / min or less is preferred. While ingots made from castings are sometimes used as raw materials for castings, the reformation of the β phase is not affected by the thermal history of the raw materials used; whether or not the β phase is reformed is determined during the cooling process after solidification of the final casting.

[0105] (Heat Treatment) In the production of castings, it can be difficult to cool the casting after casting at a cooling rate of more than 300°C / min at 500°C, and to cool the casting from 500°C to 300°C at an average cooling rate of more than 300°C / min. The β phase can be reformed to the β1 phase by subjecting such castings to heat treatment. Specifically, the casting is heated at a temperature higher than 520°C and lower than 650°C for 1 minute to 5 hours, and the cooling treatment is initiated at a temperature lower than 650°C and higher than 520°C. When the casting temperature reaches 500°C, the cooling rate exceeds 300°C / min, and the casting is cooled at an average cooling rate of more than 300°C / min in the temperature range from 500°C to 300°C.

[0106] When the heat-treated casting of this embodiment is mirror-polished and etched with a mixture of hydrogen peroxide and ammonia, grain boundaries within the β1 phase become visible, revealing that the β1 phase has been replaced with a β1 phase with different properties from conventional β phases. The heating temperature during heat treatment and the starting temperature for the cooling treatment are preferably 540°C or higher, more preferably 550°C or higher. On the other hand, if the starting temperature for the cooling treatment is higher than 650°C, the proportion of the β1 phase increases, resulting in poor dezincification corrosion resistance and impact properties. Therefore, a temperature of 620°C or lower is preferred. Furthermore, the faster the cooling rate at 500°C and the average cooling rate from 500°C to 300°C, the more the β phase is modified. Cooling at a rate of more than 600°C / min, preferably 900°C / min or higher, is more preferred. The upper limits of the cooling rate at 500°C and the average cooling rate in the temperature range from 500°C to 300°C are sufficient, and are not specifically specified. However, a preferred cooling rate is approximately 9000°C / min or less. Even if the β1 phase is formed by the heat treatment described above, if an additional heat treatment not satisfying the above conditions is performed or the casting is reheated to 300°C or higher, the β1 phase reforming is lost and the β1 phase reverts to the normal β phase. When a casting that has undergone the final specified cooling treatment, or a casting that has undergone the final specified heat treatment, is heated to 300°C or higher, the β1 phase reforming is lost and the β1 phase present in the specified casting reverts to the normal β phase. As a result, when the metal structure is observed, the grain boundaries present within the β1 phase are no longer observed.

[0107] By this manufacturing method, the free-cutting copper alloy castings according to the first to third embodiments of the present invention are manufactured.

[0108] According to the free-cutting copper alloy castings of the first to third embodiments of the present invention having the above-described configurations, the alloy composition, compositional formula, metal structure, structure-structure formula, and structure-compositional formula are defined as described above, and therefore, even with a small Pb content, excellent machinability can be obtained, and the castings can be provided with good dezincification corrosion resistance, high strength, and good impact properties.

[0109] Although the embodiment of the present invention has been described above, the present invention is not limited to this and can be modified as appropriate within the scope of the technical requirements of the invention.

[0110] The following shows the results of confirmation experiments conducted to confirm the effects of this embodiment. Note that the following examples are intended to explain the effects of this embodiment, and the components, processes, and conditions described in the examples do not limit the technical scope of this embodiment.

[0111] Copper alloy sand castings were prototyped and tested using a low-frequency melting furnace in actual operation. Furthermore, copper alloy castings were prototyped using laboratory equipment, and continuous cast rods were produced using an actual mold continuous casting machine. Furthermore, some samples were heat-treated in the laboratory. The alloy compositions are shown in Tables 5 to 7. The manufacturing processes are shown in Tables 8 to 11. In the compositions, "Mm" stands for misch metal, which indicates the total amount of rare earth elements. Each manufacturing process is described below.

[0112]

[0113]

[0114]

[0115]

[0116]

[0117]

[0118]

[0119] Process A: Production by actual equipment, sand casting (Process Nos. A1 to A6, A11H to A14H) Approximately 400 kg of raw materials were charged into a 1-ton low-frequency melting furnace in actual operation, melted at 1,080°C, transferred to a ladle, and cast at approximately 970°C into a sand mold (made of silica sand with added resin) to obtain Type A specimens as described in JIS H 5120, Section 7.2. The cast product was cooled at a cooling rate of approximately 30°C / min, and when the temperature of the casting reached 650°C or 750°C, the Type A specimen casting was removed from the sand mold and allowed to cool naturally. The castings removed from the sand molds were cooled at an average cooling rate of 35°C / min, and then cooling treatment was initiated from 460°C to 720°C, with the average cooling rate from 500°C to 300°C being adjusted to 20°C / min, 210°C / min, 420°C / min, 660°C / min, 780°C / min, or 900°C / min. The average cooling rate from the cooling treatment start temperature to 500°C was adjusted to be the same as the average cooling rate from 500°C to 300°C. When the cooling treatment start temperature was 550°C or higher, the average cooling rate from 550°C to 500°C was measured. When the cooling treatment start temperature of the castings was lower than 550°C, the average cooling rate from the cooling treatment start temperature to 500°C was measured.

[0120] However, in Process No. A12H, the average cooling rate from the time of removal of the casting to 460°C was 35°C / min, and the average cooling rate from 460°C to 300°C was 660°C / min. In Process No. A14H, the average cooling rate from the time of removal of the casting to 500°C was 35°C / min, and the average cooling rate from 500°C to 300°C was 20°C / min. Cooling methods employed included natural air cooling, forced air cooling, shower water cooling, water cooling, and simple heat retention. Temperature measurements were primarily performed using a radiation thermometer, with a contact thermometer also used in some cases. The temperature of the Type A specimen casting was measured from the time it was removed from the sand mold until it reached 300°C. The radiation thermometer used for temperature measurements was a Model IGA8Pro / MB20 manufactured by LumaSense Technologies Inc. The obtained test material A was subjected to metallurgical microscope observation, cutting test, dezincification corrosion test, hardness test, and impact test.

[0121] Process B: Laboratory Production, Mold Casting (Process Nos. B1-B5, B11H-B14H) In a laboratory, raw materials were melted at a predetermined composition ratio. In consideration of actual production, unavoidable impurities such as Fe were intentionally added to some samples. The molten metal at approximately 950°C was then cast into an iron mold with an inner diameter of 40 mm and a depth of 200 mm. Considering actual casting, when the casting reached approximately 750°C, the sample was removed from the mold and cooled at a rate of approximately 60°C / min. Then, a cooling treatment was initiated in the temperature range of 730°C to 470°C. The average cooling rate in the temperature range from 500°C to 300°C was varied to 1200°C / min, 1020°C / min, 900°C / min, 480°C / min, 240°C / min, or 40°C / min, and the sample was cooled to room temperature. The cooling rate at 500°C, i.e., the average cooling rate from 550°C or the cooling treatment start temperature to 500°C, was adjusted to be approximately the same as the average cooling rate from 500°C to 300°C.

[0122] However, in Process No. B13H, the average cooling rate from the time after the casting was removed to 470°C was 60°C / min, and the average cooling rate from 470°C to 300°C was 900°C / min. In Process No. B11H, the average cooling rate from the time after the casting was removed to 500°C was 45°C / min, and the average cooling rate from 500°C to 300°C was adjusted to 40°C / min. Regarding temperature measurement, the temperature of the casting was measured using a radiation thermometer and a contact thermometer in combination, and the average cooling rate in each temperature range was adjusted to a predetermined value. The obtained metal mold casting was then subjected to metallurgical microscope observation and cutting tests, dezincification corrosion tests, hardness tests, and impact tests.

[0123] Process C: Continuous Casting (Process Nos. C1-C3, C11H) Approximately 900 kg of raw materials were charged into a 2-ton low-frequency melting furnace and melted at 1,080°C. The molten metal in the 1,010°C holding furnace was passed through the mold of the continuous casting equipment at a casting speed of 200 mm / min to produce a continuously cast rod with a diameter of 21 mm. Cooling was performed by water cooling the mold itself, air cooling, or by directly water-cooling the continuously cast rod with a shower installed at an appropriate position from the mold. The shower position and water volume were adjusted. The temperature of the continuously cast rod was measured using a combination of a radiation thermometer and a contact thermometer. The cooling rate at 500°C was adjusted to be the same as the average cooling rate from 500°C to 300°C, and was set to 900°C / min, 660°C / min, 480°C / min, or 60°C / min. Note that the cooling start temperature was not specified in this method. The obtained continuously cast rods were subjected to metallurgical microscope observation, cutting test, dezincification corrosion test, hardness test and impact test.

[0124] Process G: Heat Treatment (Processes Nos. G1-G3, G11H-G14H) In Process G, some of the sand and metal mold castings produced in Processes A, B, and C were further heat-treated. The sand and metal mold castings and continuously cast rods produced in Processes A14H, B11H, and C11H were used, and all were heated at 580°C for 20 minutes. In Processes G1, G2, and G3, cooling was initiated at 575°C after heating, and the average cooling rates from 550°C to 500°C and from 500°C to 300°C were the same, at 1200°C / min. In Processes G11H and G12H, the cooling start temperature was 470°C, and the average cooling rate from 580°C to 470°C was 50°C / min, and the average cooling rate from 470°C to 300°C was 900°C / min. In Process Nos. G13H and G14H, after heat treatment at 580°C, no special cooling treatment was performed, and the average cooling rate from 500°C to 300°C was 25°C / min. These heat-treated materials were subjected to metallurgical microscope observation and cutting tests, dezincification corrosion tests, hardness tests, and impact tests.

[0125] (Comparative Materials) A 40 mm diameter rod of free-cutting brass C3604 containing 3 mass% Pb was prepared as a comparative material and designated Alloy X. An ingot of casting brass CAC203 containing 2 mass% Pb was also prepared and designated Alloy Y. The alloys were melted and cast in the same manner as in Steps B1 and B11H, yielding metal mold castings measuring 40 mm diameter and 200 mm in length. Alloys X and Y are commercially available. These alloys were subjected to metallurgical microscope observation, cutting tests, dezincification corrosion tests, hardness tests, and impact tests.

[0126] The above test materials were evaluated for the following items. The evaluation results are shown in Tables 10 to 21.

[0127] (Observation of Metal Structure) The metal structure was observed using the following method, and the area ratio (%) of each phase, such as the α phase, β phase, and γ phase, was measured by image analysis. Note that β phases in which grain boundaries were observed were classified as β1 phases to distinguish them from the β phase, while α' phase, β' phase, and γ' phases were included in the α phase, β phase, and γ phase, respectively. Note that in Tables 12 to 20, β phases, i.e., unmodified β phases, are listed as f4A to distinguish them from the β1 phase (f4). Regarding f6, when f4 = (β1) = 0, the value calculated using the value of f4A = (β) instead of (β1) is listed as the reference value f6A in the (β1) section.

[0128] Each test material casting was cut parallel to the longitudinal direction. The surface was then mirror-polished and etched with a mixture of hydrogen peroxide and aqueous ammonia. For the etching, an aqueous solution was used, which was a mixture of 3 mL of 3 vol% hydrogen peroxide and 22 mL of 14 vol% aqueous ammonia. The polished metal surface was immersed in this aqueous solution for approximately 2 to 10 seconds at room temperature of approximately 15 to 25°C. Note that when the β1 phase is present, corrosion resistance is improved compared to when the β phase is present, so the immersion time for etching had to be longer, at 5 to 10 seconds.

[0129] The metallographic structure was observed at 500x magnification using a metallurgical microscope to determine the proportion of each phase. Depending on the condition of the metallographic structure, observations were also performed at 1000x magnification to confirm the phases and compounds. In the five-field micrographs, each phase (α phase, β phase, β1 phase, γ phase) was manually filled in using the image processing software "Photoshop CC." To distinguish between β phase and β1 phase, if one or more β phase grain boundaries were observed within a field of view, all β phase within that field of view was filled in as β1 phase. The images were then binarized using the image analysis software "WinROOF2013" to determine the area ratio of each phase. Specifically, the average area ratio of each phase across the five fields of view was calculated, and this average value was used as the phase ratio of each phase. Compounds containing P and Si, precipitates, oxides, Pb or Bi particles, sulfides, and precipitated particles were excluded, and the total area ratio of all constituent phases was set to 100%. Compared to hot extrusion bars made in mass production facilities, non-metallic oxides and sulfides were frequently observed in the cast specimens.

[0130] When the β phase is modified, grain boundary patterns, i.e., crystal grain boundaries, are observed within the β phase when observed under a metallurgical microscope using the etching solution. In this application, when crystal grain boundaries are observed within the β phase, the β phase is designated as the β1 phase and is distinguished from ordinary β phase. Here, the crystal grain boundary refers to the linear pattern that penetrates the β1 phase grains observed within the β1 phase, as shown in Figure 1A. In addition to the β phase, P, Si compounds, and precipitates may also be present in the metal structure. Compounds of P with Zn or Si exist as dark gray particles of approximately 0.5 to 2 μm under a 500x microscope, primarily within the β phase, the β1 phase, and at the phase boundary between the β phase and the α phase. Compounds of Fe, Mn, Cr, and P or Si can be seen as light blue particles of approximately 1 to 5 μm. Pb or Bi particles, and particles formed by combining Pb and Bi, exist as fine black particles of 2 μm or less. These compounds can be roughly distinguished under a microscope. In Tables 10 to 15, when grain boundaries were observed in the β1 phase (β phase) in the metal structure, they were marked as "B," and when they were not, they were marked as "D."

[0131] Regarding P compounds, when the P content was 0.06 mass% and the sample was cooled from 500°C to 300°C at an average cooling rate of 15 to 60°C / min, approximately 250 to 500 P compounds were observed in a 500x magnification field (80 mm x 120 mm when printed). However, in the printed metallographic structure, it is difficult to distinguish between P compounds and compounds of Fe, Mn, Cr, Al, P, or Si, Pb particles, oxide particles, etc. Therefore, when determining the presence or absence of P compounds from a printed metallographic photograph, if there are fewer than 25 P compounds within the field of view of the photograph, including P compounds and compounds that may be P compounds, the photograph is rated as "D" for the absence of P compounds; if there are 25 to 125 P compounds within the field of view of the photograph, the photograph is rated as "C" for the presence but few P compounds; and if there are 125 or more P compounds, the photograph is rated as "B" for the presence of P compounds. The presence or absence of P compounds, or the amount of P compounds, is one indicator of whether the processing was appropriate.

[0132] When it was difficult to identify the phases, compounds, and precipitates, the phases and precipitates were identified by the FE-SEM-EBSP (Electron Backscattering Diffracton Pattern) method using a field emission scanning electron microscope (FE-SEM) (JSM-7000F manufactured by JEOL Ltd.) and an attached EDS under conditions of an acceleration voltage of 15 kV and a current value (set value 15) at a magnification of 500x or 2000x.

[0133] (Conductivity) Conductivity was measured using a conductivity measuring device (SIGMATEST D2.068) manufactured by Nippon Foerster Co., Ltd. In this specification, the terms "electrical conduction" and "conductivity" are used to mean the same thing. In addition, since thermal conductivity and electrical conductivity are strongly correlated, the higher the conductivity, the better the thermal conductivity.

[0134] (Machinability Test Using a Lathe) Machinability was evaluated by a cutting test using a lathe as follows. The No. A test material obtained by sand casting in process A, the metal mold casting obtained in process B, the continuously cast rod obtained in process C, and the heat-treated material obtained in process G were first machined to produce test materials with a diameter of 18 mm. A K10 carbide tool (tip) without a chip breaker was attached to a lathe. Using this lathe, the circumference of the 18 mm diameter test material was cut in a dry state under two conditions: rake angle: 0°, nose radius: 0.4 mm, clearance angle: 6°, cutting speed: 40 m / min or 110 m / min, depth of cut: 1.0 mm, and feed rate: 0.11 mm / rev. In the present embodiment, the effect of cutting speed was also investigated.

[0135] The signals emitted from a three-part dynamometer (AST-type tool dynamometer AST-TL1003, manufactured by Miho Electric Manufacturing Co., Ltd.) attached to the tool were converted into electrical voltage signals and recorded on a recorder. These signals were then converted into cutting resistance (principal force, feed force, thrust force, N). In order to reduce the influence of tip wear, the cutting test was carried out by repeating the test sequence A → B → C → ..., ... → C → B → A twice, with each sample being measured four times. Cutting resistance can be calculated using the following formula: Cutting resistance (resultant of principal force, feed force, thrust force) = ((principal force) 2 + (feed force) 2 + (back force) 2 ) 1/2 Here, the cutting resistance is determined largely by the magnitude of the principal force, so the principal force was used as the cutting resistance, and the average value of four measured values ​​was calculated to determine the cutting resistance.

[0136] The cutting resistance (principal force) of a commercially available free-cutting brass bar C3604 (Alloy X, φ40 mm) made of a Zn-59 mass% Cu-3 mass% Pb-0.2 mass% Fe-0.3 mass% Sn alloy was set to 100, and the relative value of the cutting resistance (machinability index) of the sample was calculated and evaluated relative to that. In other words, the higher the machinability index, the lower the cutting resistance and the better the machinability. The machinability index was calculated as follows: Index of cutting test results of sample (machinability index) = (Cutting resistance (principal force) of C3604 / Cutting resistance (principal force) of sample) × 100

[0137] Cutting resistance (principal force) depends on the shear strength or tensile strength of the material, and the stronger the material, the higher the cutting resistance tends to be. For example, a copper alloy with machinability equivalent to that of C3604 but approximately 1.2 times stronger than C3604 has a cutting resistance approximately 20% higher than that of C3604. Therefore, for copper alloys with high strength, a cutting resistance approximately 40% higher than that of C3604 is considered practically satisfactory. In this embodiment, the Vickers hardness is approximately 1.2 and 1.4 times that of extruded C3604 rods and cast CAC203 containing 2% Pb. Therefore, the machinability evaluation criteria in this embodiment were evaluated using a machinability index of 70 as the boundary (boundary value). Specifically, a machinability index of 78 or higher was evaluated as having excellent machinability (rating: A, excellent) and approximately the same machinability as C3604. If the machinability index was 70 or more and less than 78, the machinability was evaluated as good (evaluation: B, good). If the machinability index was 63 or more and less than 70, the machinability was evaluated as fair (evaluation: C, fair). If the machinability index was less than 63, the machinability was evaluated as unacceptable (evaluation: D, poor). In this application, the aim was to achieve good machinability, so a machinability index of 70 or more was considered acceptable.

[0138] (Dezincification corrosion test: ISO 6509 dezincification corrosion test) The dezincification corrosion test method was evaluated using the ISO 6509 dezincification corrosion test. This test method is adopted in many countries and is also specified in the JIS standard, JIS H 3250. The dezincification corrosion test procedure was as follows: first, the test material was embedded in a phenolic resin material. The sample surface was polished with emery paper up to 1200 grit, then ultrasonically cleaned in pure water and dried. Each sample was then immersed in a solution of 1.0% cupric chloride dihydrate (CuCl 2 ・2H 2 The specimen was immersed in an aqueous solution (12.7 g / L) of HCl (O) and held at 75°C for 24 hours. The specimen was then removed from the aqueous solution and re-embedded in phenolic resin. The specimen was then cut so that the cross section of the corroded area was the longest cut. The specimen was then polished. Using a metallurgical microscope, the dezincification corrosion depth was observed at 100 to 500 times magnification in 10 different fields of the microscope. The deepest corrosion point was recorded as the maximum dezincification corrosion depth.

[0139] When a typical Pb-containing free-cutting brass bar C3604 or free-cutting brass casting CAC203 was tested according to ISO 6509, the maximum corrosion depth was approximately 500 μm or more. In this application, if the maximum corrosion depth was less than 250 μm, which is 50% less than the maximum corrosion depth of C3604 or CAC203, the material was evaluated as having good dezincification corrosion resistance in practical use (rating: B, good). In particular, if the maximum corrosion depth was 100 μm or less, the material was evaluated as having excellent dezincification corrosion resistance in practical use (rating: A, excellent). On the other hand, if the maximum corrosion depth exceeded 400 μm, the dezincification corrosion resistance was equivalent to, or in some cases worse than, that of C3604 or CAC203, and the material was evaluated as not having dezincification corrosion resistance, being evaluated as "D" (poor). When the maximum corrosion depth was 250 μm or more and 400 μm or less, the dezincification corrosion resistance was evaluated as fair (evaluation: C, fair). In this application, the aim was to provide good dezincification corrosion resistance, so good (evaluation: B, good) and excellent (evaluation: A, excellent) were evaluated as passing.

[0140] (Mechanical Properties) (Hardness) The hardness of each test material was measured using a Vickers hardness tester under a load of 49 kN for the samples whose metal structure had been observed. Furthermore, the hardness of the test pieces after the cutting test was measured on the Rockwell B scale. A Vickers hardness of preferably 100 Hv or more, more preferably 110 Hv or more, can be said to be at a high level in terms of strength among free-cutting copper alloy castings. Similarly, a Rockwell B scale hardness of 52 or more, more preferably 60 or more, can be said to be at a high level in terms of strength among free-cutting copper alloy castings. The aforementioned good dezincification corrosion resistance and high strength can lead to a reduction in the amount of material used.

[0141] (Impact Properties) The impact test was carried out in the following manner. U-notch test pieces (notch depth 2 mm, notch bottom radius 1 mm) according to JIS Z 2242 were taken. A Charpy impact test was carried out using an impact blade with a radius of 2 mm to measure the impact value. In order to maintain good toughness and impact properties, the Charpy impact test value is preferably 25 J / cm. 2 More preferably, 30 J / cm 2 That's all.

[0142]

[0143]

[0144]

[0145]

[0146]

[0147]

[0148]

[0149]

[0150]

[0151]

[0152]

[0153]

[0154]

[0155]

[0156]

[0157]

[0158]

[0159]

[0160]

[0161]

[0162]

[0163]

[0164]

[0165]

[0166]

[0167]

[0168]

[0169] From the above measurement results, the following findings were obtained: 1) It was confirmed that by satisfying the composition of this embodiment and satisfying the compositional relations f1, f2, and f0, the structure relations f3 to f5, and the structure-compositional relation f6, it is possible to obtain castings with a small amount of Pb that have good machinability, good dezincification corrosion resistance, good conductivity of 15% IACS or more, high strength, and good impact properties (Alloy Nos. S01, S02, S11 to S14, and S21 to S42).

[0170] 2) By adding more than 0.50 mass% Si, the β phase was modified, and grain boundaries were observed within the β1 phase. As a result, dezincification corrosion resistance and machinability were good. When the Si content was 0.65 mass% or more, dezincification corrosion resistance and machinability were further improved. On the other hand, when the Si content was more than 1.20 mass%, electrical conductivity was reduced. (Alloy Nos. S01, S30, S32, S42, S51, S52, etc.) 3) By adding more than 0.01 mass% P, the β phase was modified, and grain boundaries were observed within the β1 phase. As a result, dezincification corrosion resistance and machinability were good. When the P content was 0.03 mass% or more, dezincification corrosion resistance and machinability were further improved. When the P content exceeded 0.18 mass%, the impact properties deteriorated (Alloy Nos. S01, S26-S28, S54, S58, etc.). 4) When the Cu content exceeded 60.5 mass%, the β phase was modified, and grain boundaries were observed within the β1 phase. As a result, dezincification corrosion resistance and machinability improved. When the Cu content was 61.5 mass% or more, dezincification corrosion resistance and machinability were further improved. When the Cu content was higher than 65.0 mass%, the β1 phase decreased, and in some cases, the γ phase began to appear, resulting in poor machinability (Alloy Nos. S01, S32, S24, S14, S42, S55, S65, etc.).

[0171] 5) When the Pb content was less than 0.002 mass%, the machinability was poor (Alloy No. S59). When the Pb content was 0.003 mass% or more, or even 0.01 mass% or more, the machinability was improved (Alloy Nos. S29 and S21). It was confirmed that the inclusion of Bi provided machinability equivalent to that of Pb (Alloy Nos. S01, S24, etc.). 6) When the Sn content exceeded 0.05 mass%, the dezincification corrosion resistance was further improved. When the Sn content exceeded 0.10 mass%, the dezincification corrosion resistance was further improved. On the other hand, when the Sn content was 0.70 mass% or more, the γ phase appeared, which actually worsened the dezincification corrosion resistance, reduced the impact properties, and lowered the machinability index. Furthermore, when the Sn / Si ratio was 0.8 or more, the β phase was not modified, and the dezincification corrosion resistance and machinability index were deteriorated (Alloy Nos. S33 to S35, S60, S61, etc.).

[0172] 7) It was confirmed that the inclusion of unavoidable impurities at levels common in actual production did not significantly affect various properties (Alloy Nos. S01, S02, S21, S22, S37, S39, etc.). 8) When the total content of the unavoidable impurities, Fe, Mn, Cr, and Co, was 0.50 mass% or more, the β phase was modified, but machinability was poor and dezincification corrosion resistance was also slightly poor. As the total content of Fe, Mn, Cr, and Co decreased to less than 0.50 mass%, and further to less than 0.35 mass%, the machinability and dezincification corrosion resistance improved. The decrease in machinability and dezincification corrosion resistance is thought to be due to the combination of Fe, Mn, etc. with a portion of Si and P to form intermetallic compounds of Fe, Mn, etc. with Si and P. As a result, compounds of Fe, etc. with Si and P were present, and the concentrations of Si and P, which effectively functioned, were reduced, presumably resulting in poor machinability and corrosion resistance (Alloy Nos. S02, S38, S39, S63, etc.). 9) When the amount of Al, an unavoidable impurity, was 0.30 mass% or more, the β phase was not modified, and dezincification corrosion resistance, machinability, and impact properties were poor. When the amount of Al was less than 0.30 mass%, dezincification corrosion resistance and machinability were improved, and when the amount of Al was less than 0.15 mass%, the effect of Al was further reduced, and machinability and dezincification corrosion resistance were good (Alloy Nos. S01, S62, S36, S37, etc.).

[0173] 10) When the value of the compositional relational expression f1 was less than 57.3, the β phase was not modified or was modified insufficiently, resulting in poor dezincification corrosion resistance and poor machinability in high-speed cutting. When the value of the compositional relational expression f1 was greater than 60.8, the area fraction of the β1 phase was small, resulting in poor machinability (Alloy Nos. S57 and S53). When the value of the compositional relational expression f1 was 57.3 or more, the β phase was modified, improving dezincification corrosion resistance and machinability, and at 58.0 or more, these were further improved. On the other hand, when the value of the compositional relational expression f1 was 60.8 or less, the area fraction of the β1 phase increased, and at 60.5 or less, it was even greater, resulting in a high machinability index, including high-speed cutting (e.g., Alloy Nos. S14, S32, and S25).

[0174] 11) When the β1 phase area ratio, f4, was less than 25%, good machinability was not obtained. The hardness index was also low. When the β1 phase area ratio exceeded 25%, and even 30% or more, machinability improved, including high-speed cutting. On the other hand, when the β1 phase area ratio exceeded 80%, the β phase was often not modified, resulting in a low machinability index, especially at high-speed cutting (110 m / min), and poor dezincification corrosion resistance. The impact value also decreased. When the β1 phase area ratio was 80% or less, or even 70% or less, the β phase was further modified, improving dezincification corrosion resistance and machinability. As a result of the modification of the β phase, the progression of dezincification corrosion was significantly delayed, but the β1 phase was preferentially dezincified. Therefore, if the area ratio of the β1 phase is high, the progress of dezincification corrosion will be slightly accelerated (Alloy Nos. S57, S55, S53, S14, S11, Process No. A6, No. B5, Process No. A11H, No. B12H, etc.).

[0175] 12) When the area fraction of the γ phase was 4% or more, γ had a negative effect on machinability, resulting in a low machinability index even when f4 and f6 were satisfied. The impact value was also low (Alloy No. S61). 13) Even when f1 and f4 were satisfied, when the value of f6 in the structure-composition relationship was less than 28, machinability was poor. When the value of f6 was 28 or greater, or even greater than 35, machinability improved (Alloy Nos. S64 and S41). On the other hand, machinability peaked when the value of f6 was 55 to 80. It is believed that machinability is roughly saturated when the amount of β1 phase (f4) was 45 to 60% and the amount of Si was 1 mass% (e.g., Alloy Nos. S02, S12, Process Nos. A1 and A2, etc.). 14) When the amount of β phase (f4A) that was not modified to β1 phase was 45 or more and f6A exceeded 40, the dezincification corrosion depth was large and the machinability, particularly at high speeds, was poor (Test Nos. S22, S106, S223, etc.).

[0176] 15) During cooling after casting, when the cooling treatment start temperature was lower than 700°C but exceeded 500°C, and the average cooling rate from 500°C to 300°C exceeded 300°C / min, the β phase was modified and grain boundaries were observed within the β1 phase. When the β phase was modified, cutting resistance was reduced, dezincification corrosion resistance was significantly improved, and strength was high. Regarding machinability, when the β phase was modified, even at higher cutting speeds, there was only a slight decrease in machinability, which was significantly different from samples without β phase modification (Process Nos. A1 to A6, A11H to A14H, B1 to B5, B11H to B14H, etc.). 16) When the cooling treatment start temperature was higher than 500°C but lower than approximately 550°C, grain boundaries were observed within the β1 phase and a small amount of P compounds was present. When a small amount of P compounds was present, the cutting resistance was slightly higher and the dezincification corrosion resistance was slightly worse than when no P compounds were present (Steps Nos. A1, A5, B1, B4, etc.). 17) When the cooling treatment starting temperature was 550°C to 650°C, the machinability and dezincification corrosion resistance were further improved. Furthermore, when the cooling rate at 500°C and the average cooling rate from 500°C to 300°C exceeded 600°C / min, or even exceeded 900°C / min, the faster the cooling rate, the higher the machinability index, particularly at 110 m / min, and the better the dezincification corrosion resistance. Thus, it was found that the cooling treatment starting temperature, the cooling rate at 500°C, and the cooling rate from 500°C to 300°C all affected the modification of the β phase. In other words, it is believed that the β phase was further modified (Steps Nos. A1 to A6, B1 to B5, C1 to C6, etc.).

[0177] 18) A cooling rate of approximately 300°C / min at 500°C and an average cooling rate of approximately 300°C / min from 500°C to 300°C are the boundary values ​​for whether grain boundaries are observed within the β phase, i.e., whether the β phase is reformed. Machinability and dezincification corrosion resistance, especially at high speeds, changed dramatically (Process Nos. A4, A13, B3, B14H, etc.). 19) When the cooling treatment starting temperature was higher than 700°C, the proportion of β1 phase increased, the machinability index was slightly lower, and machinability, especially at high speeds, and dezincification corrosion resistance also deteriorated. When the proportion of β1 phase exceeded 80%, the β phase was sometimes not reformed. Furthermore, the dezincification corrosion occurred selectively in the β1 phase, and a higher proportion of β1 phase appeared to slightly accelerate the rate of dezincification corrosion (Process Nos. A1-A6, A11H, B1-B5, B12H, etc.). 20) When the average cooling rate from 500°C to 300°C was about 200-250°C / min, no grain boundaries were observed within the β phase, and in many cases, small amounts of P compounds were present. As a result of no grain boundaries being observed within the β phase, i.e., the β phase not being modified, machinability, particularly at 110 m / min, was poor, and dezincification corrosion resistance was also poor (Process Nos. A13H, B14H, etc.).

[0178] 21) Even when the cooling start temperature after casting is not specified, it was confirmed that the β phase is reformed and dezincification corrosion resistance and machinability are significantly improved by cooling at a rate of more than 300°C / min from 550°C to 500°C and an average cooling rate of more than 300°C / min in the temperature range from 500°C to 300°C (Process Nos. C1 to C3, C11H). 22) Even when a cooling process with a rapid cooling rate was performed from a high temperature exceeding 500°C after casting, no cracks were observed in the casting (Process Nos. A1 to A6, B1 to B5, C1 to C3). 23) It was confirmed that when a casting in which the β phase was not modified was annealed at 580°C for 20 minutes, and the cooling rate at 500°C and the average cooling rate from 500°C to 300°C exceeded 300°C / min, the β phase was modified and dezincification corrosion resistance and machinability were significantly improved (Process Nos. G1 to G3, C11H).

[0179] From the above, the alloy of this embodiment, in which the contents of each additive element, the compositional relationship, and the structural relationship are within appropriate ranges, has good machinability, dezincification corrosion resistance, and mechanical properties. Furthermore, in order to obtain excellent properties from the alloy of this embodiment, the cooling conditions after casting and the heat treatment conditions must be set within appropriate ranges.

[0180] The free-cutting copper alloy casting of this embodiment has a small Pb content, excellent machinability, dezincification corrosion resistance, and castability, and exhibits high strength and good impact properties. Therefore, the free-cutting copper alloy of this embodiment is suitable for drinking water and sanitation equipment and parts, food preparation equipment, electrical and home appliance parts, automobile parts, machine parts, stationery, toys, musical instruments, sliding parts, instrument parts, precision machine parts, medical parts, water meters, and parts related to industrial water, wastewater, hydrogen, and other liquids and gases. Specifically, the free-cutting copper alloy casting is suitable for use in the above-mentioned fields as a component material for products such as water taps, hot and cold water mixer taps, stop valves, water meters, shower heads, valves, joints, cocks, gears, shafts, bearings, shafts, sleeves, spindles, sensors, bolts, nuts, and connectors.

Claims

1. Cu is more than 60.5 mass% and less than 65.0 mass%, Si is more than 0.50 mass% and less than 1.20 mass%, Pb is 0.002 mass% or more and less than 0.20 mass%, P is more than 0.01 mass% and less than 0.18 mass%, Bi is 0.0001 mass% or more and less than 0.20 mass% as an optional element, and the balance is Zn and inevitable impurities, wherein the total content of Fe, Mn, Co and Cr among the inevitable impurities is less than 0.50 mass%, and the content of Al is less than 0.30 mass%, When the Cu content is [Cu] mass%, the Si content is [Si] mass%, the Pb content is [Pb] mass%, the P content is [P] mass%, and the Bi content is [Bi] mass%, the relationship of 57.3≦f1=[Cu]-4.8×[Si]+0.5×([Pb]+[Bi])-[P]≦60.8 is satisfied, and when Bi is contained, the relationship of 0.003≦f2=[Pb]+[Bi]<0.20 is satisfied. In addition, when the area ratio of the α phase, the area ratio of the γ phase, and the area ratio of the β1 phase, which is a modified β phase, are (α)%, (γ)%, and (β1)%, respectively, in the constituent phases of the metal structure excluding nonmetallic inclusions, the area ratio of the α phase, the area ratio of the γ phase, and the area ratio of the β1 phase, which is a modified β phase, are (β1), the following relationships are satisfied: 20≦f3=(α)<75, 25<f4=(β1)≦80, 0≦f5=(γ)<4, 28<f6=(β1)×(-0.5×[Si] 2 +1.5×[Si])-2×(γ)+([Pb]+[Bi]) 1/2 ×25+([P]) 1/2 x 12, and when etched with a mixed solution of hydrogen peroxide and aqueous ammonia, grain boundaries are observed within the β1 phase.

2. Contains 61.5 mass% or more and 64.8 mass% or less of Cu, 0.65 mass% or more and 1.10 mass% or less of Si, 0.003 mass% or more and less than 0.10 mass% of Pb, and 0.03 mass% or more and 0.15 mass% or less of P, and contains 0.001 mass% or more and less than 0.10 mass% of Bi as an optional element, with the balance being Zn and inevitable impurities, wherein the total content of Fe, Mn, Co and Cr among the inevitable impurities is less than 0.35 mass%, and the content of Al is less than 0.15 mass%, When the Cu content is [Cu] mass%, the Si content is [Si] mass%, the Pb content is [Pb] mass%, the P content is [P] mass%, and the Bi content is [Bi] mass%, the relationship of 58.0≦f1=[Cu]-4.8×[Si]+0.5×([Pb]+[Bi])-[P]≦60.5 is satisfied, and when Bi is contained, the relationship of 0.004≦f2=[Pb]+[Bi]<0.10 is satisfied. In addition, when the area ratio of the α phase, the area ratio of the γ phase, and the area ratio of the β1 phase, which is a modified β phase, are (α)%, (γ)%, and (β1)%, respectively, in the constituent phases of the metal structure excluding non-metallic inclusions, the area ratio of the α phase, the area ratio of the γ phase, and the area ratio of the β1 phase, which is a modified β phase, are (β1), the following relationships are satisfied: 30≦f3=(α)≦70, 30≦f4=(β1)≦70, 0≦f5=(γ)<1, 35<f6=(β1)×(-0.5×[Si] 2 +1.5×[Si])-2×(γ)+([Pb]+[Bi]) 1/2 ×25+([P]) 1/2 x 12, and when etched with a mixed solution of hydrogen peroxide and aqueous ammonia, grain boundaries are observed within the β1 phase.

3. Cu is more than 60.5 mass% and less than 65.0 mass%, Si is more than 0.50 mass% and less than 1.20 mass%, Pb is 0.002 mass% or more and less than 0.20 mass%, P is more than 0.01 mass% and less than 0.18 mass%, Sn is more than 0.05 mass% and less than 0.70 mass%, Bi is contained as an optional element in an amount of 0.0001 mass% or more and less than 0.20 mass%, and the balance is Zn and inevitable impurities, wherein the total content of Fe, Mn, Co and Cr among the inevitable impurities is less than 0.50 mass%, and the content of Al is less than 0.30 mass%, When the Cu content is [Cu] mass%, the Si content is [Si] mass%, the Pb content is [Pb] mass%, the P content is [P] mass%, the Bi content is [Bi] mass%, and the Sn content is [Sn] mass%, there is a relationship of 57.3≦f1=[Cu]-4.8×[Si]+0.5×([Pb]+[Bi])-[P]-[Sn]≦60.8, and there is also a relationship of f0=[Sn] / [Si]<0.8, and when Bi is contained, there is a relationship of 0.003≦f2=[Pb]+[Bi]<0.20, and In the constituent phases of the metal structure excluding nonmetallic inclusions, if the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, then 20≦f3=(α)<75, 25<f4=(β1)≦80, 0≦f5=(γ)<4, 28<f6=(β1)×(−0.5×[Si] 2 +1.5×[Si])-2×(γ)+([Pb]+[Bi]) 1/2 ×25+([P]) 1/2 x 12, and when etched with a mixed solution of hydrogen peroxide and aqueous ammonia, grain boundaries are observed within the β1 phase.

4. The free-cutting copper alloy casting according to any one of claims 1 to 3, characterized in that it is used for appliances and parts relating to drinking water and sanitation facilities, water meters, valves, drainage appliances and parts, industrial piping parts, automobile parts, electric and home appliance parts, machine parts, stationery, toys, musical instruments, sliding parts, instrument parts, and medical parts.

5. A method for producing a free-cutting copper alloy casting according to any one of claims 1 to 3, comprising a casting step, characterized in that in the cooling process of the final casting step, the cooling rate at the time when the temperature of the casting is 500°C exceeds 300°C / min, and the average cooling rate in the temperature range from 500°C to 300°C exceeds 300°C / min.

6. A method for producing a free-cutting copper alloy casting as defined in any one of claims 1 to 3, comprising a casting step, characterized in that in the cooling process of the final casting step, the cooling treatment start temperature is higher than 500°C and lower than 700°C, the cooling rate at the time when the temperature of the casting reaches 500°C exceeds 300°C / min, and the average cooling rate in the temperature range from 500°C to 300°C exceeds 300°C / min.

7. A method for producing a free-cutting copper alloy casting according to any one of claims 1 to 3, comprising a casting step and a heat treatment step, characterized in that in the final heat treatment step, the casting is heated at a temperature above 520°C and below 650°C for a holding time of 1 minute to 5 hours, and in the cooling treatment step after the heat treatment, the cooling treatment is started at a temperature above 520°C, the cooling rate at the time when the casting temperature reaches 500°C exceeds 300°C / min, and the average cooling rate in the temperature range from 500°C to 300°C exceeds 300°C / min.

Citation Information

Patent Citations

  • Copying device with zoom variable power function

    JP1995005579A

  • Lead-free free cutting brass excellent in dezincification corrosion resistance and its production method

    JP2002003967A

  • Lead-free free-cutting silicon brass alloy

    JP2010133006A

  • Brass excellent in corrosion resistance

    JP2018048398A

  • Lead-free, free-cutting brass alloy with excellent castability, its manufacturing method, and its uses

    JP2019508584A

Cited By

  • Free-machining copper alloy, and method for manufacturing a free-machining copper alloy

    JP7913655B2

  • Free-machining copper alloy and production method for free-machining copper alloy

    JPWO2024228355A1

  • Cu-zn-si-pb-p-based alloy continuous cast wire rod material

    WO2025100166A1