High-purity alumina active spherical carrier and preparation method therefor

By preparing high-purity alumina active sphere support and using it as a catalyst, the problems of high cost and low efficiency of catalysts in the preparation process of icimerin in the prior art are solved, and high yield and low cost production of compound B are achieved. Suitable for large-scale industrial applications.

WO2024229967A1PCT designated stage expired Publication Date: 2024-11-14YANGZHOU ZHONGTIANLI NEW MATERIAL
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/106295
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-05
Filing Date
2023-07-07
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

In the preparation process of icimerin in the prior art, the catalyst costs are high and the reaction efficiency is low, making it difficult to meet the needs of large-scale industrial production.

Method used

Using a high-purity alumina active sphere carrier, composed of ZSM-48 molecular sieve, lanthanide metal nitrate solution and high-purity alumina, it is prepared by impregnation, drying, calcining and pressurization treatment, and is used as a catalyst to promote the rearrangement of compound A. The reaction produces compound B.

Benefits of technology

It improves the yield of compound B, reduces production costs, is convenient to operate, is suitable for large-scale production, and has sufficient raw materials and is suitable for price.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023106295_14112024_PF_FP_ABST
    Figure CN2023106295_14112024_PF_FP_ABST
Patent Text Reader

Abstract

A high-purity alumina active spherical carrier and a preparation method therefor. The carrier is prepared from the following raw materials in parts by weight: 30-40 parts of a ZSM-48 molecular sieve, 45-60 parts of a nitrate solution of a lanthanide metal and 15-20 parts of high-purity alumina. When being used as a catalyst, the carrier prepared by combining the ZSM-48 molecular sieve modified with an ytterbium nitrate solution and the high-purity alumina active spheres effectively promotes a rearrangement reaction of a compound A to generate a compound B and improves the yield of the compound B, thereby expanding the source of icariin intermediates and reducing the production and preparation cost of icariin.
Need to check novelty before this filing date? Find Prior Art

Description

A high-purity alumina active spherical carrier and preparation method thereof Technical Field

[0001] The present invention relates to the technical field of alumina carriers, and in particular to a high-purity alumina active spherical carrier and a preparation method thereof. Background Art

[0002] Icariin, also known as icariin and icariin, is a new effective monomer obtained by enzymatic conversion of icariin, the main active ingredient extracted and isolated from the traditional Chinese medicine Epimedium. The preparation method of this compound is disclosed in CN101302548B. This method uses icariin as the raw material and hydrolyzes it with β-glucosidase. The hydrolyzate is centrifuged to obtain a precipitate, which is dissolved in acetone and centrifuged to obtain a supernatant. The supernatant is then recrystallized from water to obtain pure icariin.

[0003] In the March 2013 issue of Organic Chemistry, an article titled "Synthesis of Icariin" was published. The synthetic route described in this article is identical to that of 200610165354.7. However, in the rearrangement process from compound (12) to compound (13), tris(6,6,7,7,8,8,8-heptafluoro-2,2-dimethyl-3,5-octanedionato)europium was used as a catalyst. The reaction temperature during the catalytic process reached 80°C, the reaction time was 36 hours, and the yield was only 42%. To obtain a higher-purity compound 12 for the next reaction, the article separated compound (12) by column chromatography on a silica gel column. Although this separation method is feasible in the laboratory, it is too expensive to use in large-scale industrial production.

[0004] CN201710565818.1 discloses a method for synthesizing icariin, which involves the synthesis of an icariin intermediate, as shown in the figure below:

[0005] However, the yield of the target intermediate of this synthesis method is low, less than 50%, and the cost is high, which cannot meet the needs of large-scale production.

[0006] Based on the above situation, the present invention proposes a high-purity alumina active sphere carrier and a preparation method thereof, which can effectively solve the above problems as a catalyst in the above process.

[0007] Summary of the Invention

[0008] The purpose of the present invention is to provide a high-purity alumina active sphere carrier and a preparation method thereof.

[0009] To achieve the above objectives, the present invention provides a high-purity alumina active sphere carrier, which is prepared from the following raw materials in parts by weight: 30 to 40 parts of ZSM-48 molecular sieve, 45 to 60 parts of lanthanide metal nitrate solution, and 15 to 20 parts of high-purity alumina.

[0010] Preferably, the silicon to aluminum molar ratio of the ZSM-48 molecular sieve is 56-64.

[0011] Preferably, the lanthanide metal nitrate solution includes one of ytterbium nitrate solution, europium nitrate solution, cerium nitrate solution, and praseodymium nitrate solution.

[0012] Preferably, the lanthanide metal nitrate solution is ytterbium nitrate solution.

[0013] Preferably, the concentration of the ytterbium nitrate solution is 0.1 to 0.3 g of ytterbium nitrate per milliliter of aqueous solution.

[0014] Preferably, the purity of the high-purity alumina is 99.9%, and the specific surface area is 100-130m 2 / g, and the average particle size is 200-250nm.

[0015] The present invention also provides a method for preparing a high-purity alumina active sphere carrier, the method comprising the following steps:

[0016] (1) adding ZSM-48 molecular sieve to ytterbium nitrate solution, impregnating at room temperature for 12 to 13 hours, filtering, collecting solid particles, and drying at 150° C. for 2 to 3 hours to obtain a precursor;

[0017] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring and mixing at 100-150 rpm for 30-45 minutes to uniformly mix, and then calcining at 300-350° C. for 8-10 hours to obtain an unactivated carrier;

[0018] (3) The carrier obtained in step (3) is added to a pressurized environment filled with inert gas and treated for 10 to 12 hours, wherein the pressurized environment is 1.5 to 2 MPa, thereby obtaining the high-purity alumina active sphere carrier.

[0019] Preferably, the inert gas is one of nitrogen, carbon dioxide, argon and helium.

[0020] The present invention also provides a use of a high-purity alumina active sphere carrier, which is used as a catalyst in the process of synthesizing compound B from compound A:

[0021] The method for synthesizing compound B from compound A is as follows: under nitrogen protection, compound A, solvent toluene, and high-purity alumina activated sphere carrier are sequentially added to a reaction vessel; the reaction solution is heated to 80-90° C. and stirred for 18 hours; the reaction solution is cooled to room temperature and filtered, and the filter cake is washed with dichloromethane and acetonitrile in sequence; and then filtered and dried to obtain compound B.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention uses a ZSM-48 molecular sieve modified with an ytterbium nitrate solution and a carrier prepared by combining it with high-purity alumina activated balls. When used as a catalyst, it effectively promotes the rearrangement reaction of compound A to produce compound B, thereby increasing the yield of compound B, thereby expanding the source of icariin intermediates and reducing the production and preparation cost of icariin.

[0024] 2. The preparation method of the present invention is easy to operate, easy to mass produce, and has stable quality.

[0025] 3. The raw materials of the present invention are abundant in the country and are reasonably priced, so that there is no high cost restriction for large-scale production. DETAILED DESCRIPTION

[0026] Example 1

[0027] The amount of each raw material is shown in Table 1.

[0028] (1) adding ZSM-48 molecular sieve to ytterbium nitrate solution, impregnating at room temperature for 12 h, filtering, collecting solid particles, and drying at 150 ° C for 2 h to obtain a precursor;

[0029] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring at 100 rpm for 45 minutes to uniformly mix, and then calcining at 300° C. for 10 hours to obtain an unactivated support;

[0030] (3) The carrier obtained in step (3) is added to a pressurized environment filled with inert gas and treated for 12 hours, wherein the pressurized environment is 1.5 MPa, thereby obtaining a high-purity alumina active sphere carrier.

[0031] Example 2

[0032] The amount of each raw material is shown in Table 1.

[0033] (1) adding ZSM-48 molecular sieve to ytterbium nitrate solution, impregnating at room temperature for 13 h, filtering, collecting solid particles, and drying at 150 ° C for 3 h to obtain a precursor;

[0034] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring at 150 rpm for 30 min to uniformly mix, and then calcining at 350° C. for 8 h to obtain an unactivated support;

[0035] (3) The carrier obtained in step (3) is placed in a pressurized environment filled with inert gas and treated for 10 hours, wherein the pressurized environment is 2 MPa, to obtain a high-purity alumina active sphere carrier.

[0036] Example 3

[0037] The amount of each raw material is shown in Table 1.

[0038] (1) adding ZSM-48 molecular sieve to ytterbium nitrate solution, impregnating at room temperature for 13 h, filtering, collecting solid particles, and drying at 150 ° C for 3 h to obtain a precursor;

[0039] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring at 150 rpm for 45 minutes to uniformly mix, and then calcining at 350° C. for 10 hours to obtain an unactivated support;

[0040] (3) The carrier obtained in step (3) is added to a pressurized environment filled with inert gas and treated for 12 hours, wherein the pressurized environment is 2 MPa, to obtain a high-purity alumina active sphere carrier.

[0041] Comparative Example 1

[0042] The amount of each raw material is shown in Table 1.

[0043] (1) adding ZSM-5 molecular sieve to ytterbium nitrate solution, impregnating at room temperature for 13 h, filtering, collecting solid particles, and drying at 150 ° C for 3 h to obtain a precursor;

[0044] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring at 150 rpm for 45 minutes to uniformly mix, and then calcining at 350° C. for 10 hours to obtain an unactivated support;

[0045] (3) The carrier obtained in step (3) is added to a pressurized environment filled with inert gas and treated for 12 hours, wherein the pressurized environment is 2 MPa, to obtain a high-purity alumina active sphere carrier.

[0046] Comparative Example 2

[0047] The amount of each raw material is shown in Table 1.

[0048] (1) adding ZSM-22 molecular sieve to ytterbium nitrate solution, impregnating at room temperature for 13 h, filtering, collecting solid particles, and drying at 150 ° C for 3 h to obtain a precursor;

[0049] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring at 150 rpm for 45 minutes to uniformly mix, and then calcining at 350° C. for 10 hours to obtain an unactivated support;

[0050] (3) The carrier obtained in step (3) is added to a pressurized environment filled with inert gas and treated for 12 hours, wherein the pressurized environment is 2 MPa, to obtain a high-purity alumina active sphere carrier.

[0051] Comparative Example 3

[0052] The amount of each raw material is shown in Table 1.

[0053] (1) adding ZSM-48 molecular sieve to ytterbium trifluoromethanesulfonate solution, impregnating at room temperature for 13 h, filtering, collecting solid particles, and drying at 150 ° C for 3 h to obtain a precursor;

[0054] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring at 150 rpm for 45 minutes to uniformly mix, and then calcining at 350° C. for 10 hours to obtain an unactivated support;

[0055] (3) The carrier obtained in step (3) is added to a pressurized environment filled with inert gas and treated for 12 hours, wherein the pressurized environment is 2 MPa, to obtain a high-purity alumina active sphere carrier.

[0056] Comparative Example 4

[0057] The amount of each raw material is shown in Table 1.

[0058] (1) adding ZSM-48 molecular sieve to ytterbium nitrate solution, impregnating at room temperature for 13 h, filtering, collecting solid particles, and drying at 150 ° C for 3 h to obtain a precursor;

[0059] (2) The precursor obtained in step (3) is added to a pressurized environment filled with inert gas and treated for 12 hours, wherein the pressurized environment is 2 MPa, to obtain a carrier.

[0060] Comparative Example 5

[0061] The amount of each raw material is shown in Table 1.

[0062] (1) adding ZSM-48 molecular sieve to ytterbium nitrate solution, impregnating at room temperature for 13 h, filtering, collecting solid particles, and drying at 150 ° C for 3 h to obtain a precursor;

[0063] (2) The precursor obtained in step (1) was mixed with high-purity alumina, stirred at 150 rpm for 45 minutes to make it uniform, and then calcined at 350° C. for 10 hours to obtain a high-purity alumina active sphere carrier.

[0064] Table 1

[0065] Catalyst performance evaluation test

[0066] The high-purity alumina active sphere carriers prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were crushed and sieved to a particle size of 20 to 30 mesh. Under nitrogen protection, compound A (50 g, 0.11 mol), toluene (500 mL, 10 mL / g) (solvent), and the above-mentioned catalyst (25 g) were added to the reaction flask. The reaction solution was heated to 80 to 90°C and stirred for 18 hours; the reaction solution was cooled to room temperature, filtered, and the filter cake was washed with dichloromethane (200 mL, 4 mL / g). The filtrates were combined and concentrated to 100 mL. Acetonitrile (250 mL, 5 mL / g) was added to the concentrated solution and concentrated to 100 mL. Acetonitrile (250 mL, 5 mL / g) was further added and concentrated to 250 mL. After stirring at 50-60°C for 1 hour, the temperature was lowered to 0°C over 2 hours and stirred for 1 hour. The mixture was filtered, and the filter cake was washed with acetonitrile (50 mL, 1 mL / g) and dried to obtain Compound B. The yield of Compound B was calculated. The results are shown in Table 2.

[0067] Table 2 Reaction results

[0068] The foregoing descriptions of specific exemplary embodiments of the present invention are for purposes of illustration and description. These descriptions are not intended to limit the invention to the precise forms disclosed, and it is apparent that many variations and modifications are possible in light of the foregoing teachings. The exemplary embodiments have been selected and described for the purpose of explaining the specific principles of the invention and their practical application, thereby enabling those skilled in the art to realize and utilize a variety of exemplary embodiments of the invention and various options and modifications. The scope of the invention is intended to be defined by the claims and their equivalents.

Claims

1. A high-purity alumina active spherical carrier, characterized in that: The high-purity alumina active sphere carrier is prepared from the following raw materials in parts by weight: 30 to 40 parts of ZSM-48 molecular sieve, 45 to 60 parts of nitrate solution of lanthanide metals, and 15 to 20 parts of high-purity alumina.

2. The high-purity alumina active sphere carrier according to claim 1, characterized in that: The silicon-aluminum molar ratio of the ZSM-48 molecular sieve is 56-64.

3. The high-purity alumina active sphere carrier according to claim 1, characterized in that: The lanthanide metal nitrate solution includes one of ytterbium nitrate solution, europium nitrate solution, cerium nitrate solution and praseodymium nitrate solution.

4. The high-purity alumina active sphere carrier according to claim 3, characterized in that: The lanthanide metal nitrate solution is ytterbium nitrate solution.

5. The high-purity alumina active sphere carrier according to claim 4, characterized in that: The concentration of the ytterbium nitrate solution is 0.1-0.3 g of ytterbium nitrate per milliliter of aqueous solution.

6. The high-purity alumina active sphere carrier according to claim 1, characterized in that: The purity of the high-purity alumina is 99.9%, and the specific surface area is 100-130m 2 / g, and the average particle size is 200-250nm.

7. A method for preparing the high-purity alumina active spherical carrier according to claim 1, characterized in that: The method comprises the following steps: (1) adding ZSM-48 molecular sieve to ytterbium nitrate solution, impregnating at room temperature for 12 to 13 hours, filtering, collecting solid particles, and drying at 150° C. for 2 to 3 hours to obtain a precursor; (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring the mixture at 100 to 150 rpm for 30 to 45 minutes to make it uniform, and then calcining the mixture at 300 to 350° C. for 8 to 10 hours to obtain a carrier; (3) The carrier obtained in step (3) is placed in a pressurized environment filled with inert gas and treated for 10 to 12 hours, wherein the pressurized environment is 1.5 to 2 MPa, to obtain a supported catalyst.

8. The method according to claim 1, characterized in that The inert gas is one of nitrogen, carbon dioxide, argon and helium.

9. Use of the high-purity alumina active sphere carrier according to claim 1, characterized in that: The use is to use compound A as a catalyst in the process of synthesizing compound B:

10. The use according to claim 9, characterized in that The method for synthesizing compound B from compound A is as follows: under nitrogen protection, compound A, solvent toluene, and high-purity alumina active ball carrier catalyst are sequentially added into a reaction container; the reaction liquid is heated to 80-90° C. and stirred for 18 hours; the reaction liquid is cooled to room temperature, filtered, and the filter cake is sequentially washed with dichloromethane and acetonitrile; filtered, and dried to obtain compound B.

Citation Information

Patent Citations

  • Fischer-Tropsch synthesis catalyst comprising zeolite molecular sieve, and preparation method and application thereof

    CN103007982A

  • Shape-selective catalyst high in toluene methylation efficiency and preparation method and application thereof

    CN106807442A

  • Hydrated alumina composition containing composite molecular sieve, catalyst, preparation methods of hydrated alumina composition containing composite molecular sieve, and catalyst, and hydroisomerization method

    CN107999044A

  • Hydrated alumina composition containing ZSM-48 type molecular sieve, catalyst, preparation methods of hydrated alumina composition containing ZSM-48 type molecular sieve, and catalyst, and hydroisomerization method

    CN107999141A

  • Method of hydrorefining catalyst manufacture

    US4419275A