Retardation layer, projector, and head-up display system

The integration of a retardation layer with a liquid crystal compound in head-up display systems adjusts the polarization of projection light to prevent double images, addressing the issue of increased view angles and improving display quality.

WO2024232319A1PCT designated stage expired Publication Date: 2024-11-14FUJIFILM CORP

Patent Information

Application Number
PCT/JP2024/016764
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2024-05-01
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

In head-up display systems, increasing the angle of view leads to the occurrence of double images due to the mixing of P-polarized and S-polarized light on the windshield glass, which is undesirable.

Method used

A retardation layer with a liquid crystal compound is introduced between the light source and the windshield glass, where the molecular axis of the liquid crystal compound changes continuously or stepwise within the plane, adjusting the polarization direction of the projection light to prevent double images by ensuring either P-polarized or S-polarized light is reflected appropriately.

Benefits of technology

The retardation layer effectively suppresses the occurrence of double images by optimizing the polarization direction of the projection light, enhancing the display system's performance without compromising the angle of view.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016764_14112024_PF_FP_ABST
    Figure JP2024016764_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a retardation layer that, when built in a head-up display system, suppresses occurrence of a double image, a projector, and a head-up display system. A retardation layer according to the present invention is disposed between a light source that emits projection light in a head-up display system and a windshield glass that is irradiated with the projection light emitted from the light source. The retardation layer contains a liquid crystal compound, and the orientation of the molecular axis of the liquid crystal compound changes continuously or in stages along one in-plane direction of the retardation layer.
Need to check novelty before this filing date? Find Prior Art

Description

Retardation layer, projector, head-up display system

[0001] The present invention relates to a retardation layer, a projector, and a head-up display system.

[0002] Image projection systems that project various images, text information, etc. onto a screen are widely used. For example, Patent Document 1 discloses a so-called head-up display system that is developed as an in-vehicle display, in which various information is projected as an image onto the windshield or the like by a projector to convey the information to the driver.

[0003] Japanese Patent Application Publication No. 3-209210

[0004] Recently, there has been a demand for a head-up display system that can display an image with a larger angle of view, which is the angular range available for displaying an image. In other words, there has been a demand for a head-up display system that can project light onto a windshield glass with a larger area. The present inventors have found that, in the head-up display system described in Patent Document 1, the occurrence of double images becomes more pronounced when the angle of view is increased, and that an improvement in this regard is necessary.

[0005] In view of the above circumstances, an object of the present invention is to provide a retardation layer that suppresses the occurrence of double images when incorporated into a head-up display system. Another object of the present invention is to provide a projector and a head-up display system.

[0006] The present inventors have found that the above problems can be solved by the following configuration.

[0007] (1) A retardation layer disposed between a light source that emits projection light in a head-up display system and a windshield glass onto which the projection light emitted from the light source is irradiated, the retardation layer containing a liquid crystal compound, wherein the orientation of the molecular axis of the liquid crystal compound changes continuously or stepwise along one direction in the plane of the retardation layer. (2) The retardation layer according to (1), wherein the in-plane retardation at a wavelength of 550 nm is 100 to 500 nm, and the angle between the molecular axis of the liquid crystal compound located at one end in one direction and the molecular axis of the liquid crystal compound located at the other end in the same direction is 3 to 40°. (3) The retardation layer according to (1) or (2), wherein the in-plane retardation at a wavelength of 550 nm is 210 to 340 nm, and the angle between the molecular axis of the liquid crystal compound located at one end in one direction and the molecular axis of the liquid crystal compound located at the other end in the same direction is 7 to 15°. (4) A projector for a head-up display system, comprising a light source that emits projection light and the retardation layer described in any one of (1) to (3). (5) A head-up display system, comprising a projector including a light source that emits projection light, a windshield glass onto which the projection light emitted from the light source is irradiated, and the retardation layer described in any one of (1) to (3) disposed between the light source and the windshield glass. (6) The head-up display system described in (5), in which the windshield glass reflects P-polarized light and the projector irradiates P-polarized projection light. (7) The head-up display system described in (5), in which the windshield glass reflects S-polarized light and the projector irradiates S-polarized projection light.

[0008] According to the present invention, it is possible to provide a retardation layer that suppresses the occurrence of double images when incorporated into a head-up display system. Furthermore, according to the present invention, it is possible to provide a projector and a head-up display system.

[0009] FIG. 1 is a diagram illustrating an example of a head-up display system; FIG. 2 is a diagram illustrating the orientation (direction) of molecular axes of a liquid crystal compound in a retardation layer; FIG. 3 is a diagram illustrating an example of a conventional head-up display system in which a retardation layer is not arranged; FIG. 4 is a diagram illustrating an exposure method for a photo-alignment film; FIG. 5 is a diagram illustrating a polarizer used; FIG. 6 is a diagram illustrating an exposure method for a photo-alignment film; FIG. 7 is a diagram illustrating a polarizer used; FIG. 8 is a diagram illustrating an example of a windshield glass; FIG. 9 is a diagram illustrating the configuration of an evaluation system; FIG. 10 is a diagram illustrating the configuration of an evaluation system.

[0010] The retardation layer, projector, and head-up display system of the present invention will be described in detail below with reference to preferred embodiments shown in the accompanying drawings. The figures described below are merely illustrative for explaining the present invention, and the present invention is not limited to these figures. In the following, the use of "to" to indicate a numerical range includes the values ​​written on both sides. For example, when ε1 is between α1 and β1, the range of ε1 includes α1 and β1, and expressed mathematically as α1≦ε1≦β1. Angles such as "angles expressed by specific numerical values," "parallel," "horizontal," "vertical," and "orthogonal" include the error range generally accepted in the relevant technical field unless otherwise specified. Specifically, this means that the angle is within a range of ±10° from the exact angle, and the error from the exact angle is preferably 7° or less, and more preferably 5° or less. Furthermore, the term "same" includes the error range generally accepted in the relevant technical field, and terms such as "overall" also include the error range generally accepted in the relevant technical field.

[0011] Unless otherwise specified, the term "light" refers to visible light and natural light (unpolarized). Visible light is electromagnetic light with wavelengths visible to the human eye, and typically refers to light in the wavelength range of 380 to 780 nm. Invisible light is light in the wavelength range of less than 380 nm or greater than 780 nm. Furthermore, although not limited thereto, within visible light, light in the wavelength range of 420 to 490 nm is blue (B) light, light in the wavelength range of 495 to 570 nm is green (G) light, and light in the wavelength range of 620 to 750 nm is red (R) light.

[0012] The "visible light transmittance" is the A-light source visible light transmittance defined in JIS (Japanese Industrial Standards) R 3212:2015 (Test Methods for Automotive Safety Glass). That is, the transmittance is determined by measuring the transmittance at each wavelength in the wavelength range of 380 to 780 nm using a spectrophotometer with an A-light source, and multiplying the transmittance at each wavelength by a weighting coefficient obtained from the wavelength distribution and wavelength interval of the CIE (Commission Internationale de l'Eclairage) photopic standard relative luminosity factor, and calculating a weighted average. When simply referring to "reflected light" or "transmitted light," this term is used to include scattered light and diffracted light.

[0013] P-polarized light refers to polarized light that vibrates in a direction parallel to the plane of incidence of light, while S-polarized light refers to polarized light that vibrates in a direction perpendicular to the plane of incidence of light. The plane of incidence is perpendicular to the reflecting surface (such as the surface of a windshield glass) and refers to the plane that contains the incident and reflected light rays. In P-polarized light, the vibration plane of the electric field vector is parallel to the plane of incidence, while in S-polarized light, the vibration plane of the electric field vector is perpendicular to the plane of incidence.

[0014] The in-plane retardation (in-plane phase difference) is a value measured using an AxoScan manufactured by Axometrics. Unless otherwise specified, the measurement wavelength is 550 nm. The in-plane retardation is measured by irradiating light with a wavelength within the visible light wavelength range in the normal direction of the film (normal direction of the surface of the retardation layer).

[0015] "Projection image" means an image based on the projection of light from the projector used, rather than the surrounding scenery such as the front. A projection image is perceived by an observer as a virtual image that appears to appear beyond the windshield glass. "Screen image" means an image displayed on the projector's drawing device, or an image drawn by the drawing device on an intermediate image screen or the like. A projection image is a virtual image, while a screen image is a real image. Both the image and the projection image may be a monochromatic image, a multi-color image with two or more colors, or a full-color image.

[0016] As will be described later, a feature of the present invention is the use of a retardation layer in which the molecular axes of liquid crystal compounds are oriented in a predetermined direction.

[0017] An example of a head-up display system of the present invention is shown in Fig. 1. The head-up display system 10 of the present invention shown in Fig. 1 is an in-vehicle head-up display system, and includes a projector 12 for the head-up display system, a windshield glass 14, and a retardation layer 16 disposed between the projector 12 and the windshield glass 14.

[0018] 1 includes an image forming unit 20, an intermediate image screen 22, a reflecting member 24, and a concave mirror 26. In the following description, the projector 12 for the head-up display system will also be simply referred to as a "projector."

[0019] 1, the projection light projected by the projector 12 passes through a transmission window 32 provided in a dashboard 30 and a retardation layer 16 provided in the transmission window 32, is projected onto the windshield glass 14, and is observed by the observer OB. Note that, as with a normal head-up display system, in the example illustrated in FIG. 1, the observer OB observes the image projected onto the windshield glass 14 as a virtual image through the windshield glass 14.

[0020] In Fig. 1, a projector 12 emits P-polarized projection light, and a windshield glass 14 reflects the P-polarized light. The present invention is not limited to the embodiment shown in Fig. 1, and may be an embodiment in which the projector emits S-polarized projection light, and the windshield glass reflects the S-polarized light.

[0021] Hereinafter, each component of the head-up display system 10 will be described in detail. First, the retardation layer 16, which is a characteristic feature of the head-up display system 10, will be described in detail.

[0022] <Retardation Layer> As described above, the retardation layer 16 is disposed between the light source 34 that emits projection light in the projector 10 and the windshield glass 14 onto which the projection light emitted from the light source 34 is irradiated. That is, the retardation layer 16 is disposed on the optical path of the projection light between the light source 34 that emits projection light in the projector 10 and the windshield glass 14 onto which the projection light emitted from the light source 34 is irradiated. Note that in FIG. 1 , the retardation layer 16 is disposed on the transmission window 32, but this is not a limitation as long as the retardation layer 16 is disposed between the light source that emits projection light in the projector and the windshield glass onto which the projection light emitted from the light source is irradiated. That is, it is sufficient if the retardation layer is disposed on the optical path of the projection light between the light source and the windshield glass. The retardation layer may also be disposed inside the projector.

[0023] FIG. 2 shows a plan view of the retardation layer 16 as viewed from the direction of the white arrow in FIG. 1 . The bottom side of FIG. 2 corresponds to the viewer OB side in FIG. 1 . That is, the bottom side of FIG. 2 is located inside the vehicle. As shown in FIG. 2 , the retardation layer 16 contains a liquid crystal compound LC, and the orientation of the molecular axis 18 of the liquid crystal compound LC changes while continuously rotating clockwise in one direction indicated by arrow X. Note that in FIG. 2 , the orientation of the molecular axis 18 of the liquid crystal compound LC rotates clockwise, but the present invention is not limited to this embodiment and may rotate counterclockwise. Note that the molecular axis 18 of the liquid crystal compound LC is the axis along which the refractive index of the liquid crystal compound LC is highest. For example, when the liquid crystal compound LC is a rod-shaped liquid crystal compound that is horizontally aligned, the molecular axis is aligned along the long axis direction of the rod shape. When the liquid crystal compound LC is a discotic liquid crystal compound that is vertically aligned, the molecular axis is aligned along a direction perpendicular to the thickness direction of the disc.

[0024] The liquid crystal compounds LC contained in the retardation layer 16 are aligned in the Y direction perpendicular to the direction of the arrow X, i.e., in the Y direction perpendicular to one direction in which the molecular axes 18 continuously rotate. In other words, among the liquid crystal compounds LC contained in the retardation layer 16, the angles formed by the directions of the molecular axes 18 and the direction of the arrow X are equal among the liquid crystal compounds LC aligned in the Y direction.

[0025] FIG. 2 shows an embodiment in which the molecular axis of the liquid crystal compound LC rotates (changes) continuously in the direction of the arrow X, but the present invention is not limited to this embodiment, and the molecular axis may rotate (change) stepwise.

[0026] The angle formed by the molecular axis of the liquid crystal compound located at one end in the arrow X direction of the retardation layer 16 and the molecular axis of the liquid crystal compound located at the other end in the arrow X direction of the retardation layer 16 is not particularly limited, but is preferably 3 to 40°, more preferably 7 to 15°, in terms of further suppressing the occurrence of double images in a head-up display system including the retardation layer of the present invention (hereinafter simply referred to as "the advantage of the present invention being better"). In other words, the rotation angle of the molecular axis of the liquid crystal compound from one end to the other end in the arrow X direction of the retardation layer 16 (one direction in which the molecular axis 18 continuously rotates) is preferably 3 to 40°, more preferably 7 to 15°.

[0027] The in-plane retardation of the retardation layer 16 at a wavelength of 550 nm is not particularly limited, but is preferably 100 to 500 nm, more preferably 210 to 340 nm, in terms of achieving better effects of the present invention.

[0028] The reason why the use of the above-described retardation layer 16 achieves the desired effect is as follows. FIG. 3 is a diagram showing the configuration of a conventional head-up display system in which the retardation layer 16 is not provided. In the head-up display system, as shown by the solid arrow in FIG. 3 , light is irradiated from near the edge of the transmission window 32 of the projector onto the irradiation region R of the windshield glass 14, and is reflected toward the observer OB, as shown by the dashed arrow. When the angle of view in the head-up display system is large, it becomes necessary to tilt the irradiation angle from near the edge of the transmission window 32 to the irradiation region R of the windshield glass 14 more. In such a configuration with a large angle of view, for example, when P-polarized projection light is irradiated from near the center of the transmission window 32 toward the windshield glass 14, the irradiated projection light is irradiated onto the windshield glass 14 as P-polarized light. On the other hand, when the projection light is irradiated onto the windshield glass 14 from near the edge of the transmission window 32, the irradiation angle becomes more oblique as shown in FIG. 3 , and when the projection light is irradiated onto the windshield glass 14, a mixture of P-polarized and S-polarized light is irradiated onto the windshield glass 14. This leads to the occurrence of double images. In contrast, in the head-up display system 10 including the retardation layer 16 of the present invention shown in FIG. 1 , the molecular axis of the liquid crystal compound LC in the retardation layer 16 is changed as shown in FIG. 2 , thereby adjusting the polarization direction of the projection light that passes through the retardation layer 16 from near the edge of the transmission window 32 and is irradiated onto the windshield glass 14. For example, in the embodiment shown in FIG. 1 , the polarization direction of the P-polarized projection light is adjusted when it passes through the retardation layer 16, so that it is irradiated onto the windshield glass 14 as P-polarized light. This prevents the occurrence of double images.

[0029] 1 and 2, in which P-polarized light is used as the projection light, the direction corresponding to the vertical downward direction on the surface of the windshield glass when projected onto the surface of the retardation layer (the direction of the white arrow in FIG. 2) (hereinafter also referred to simply as the "reference direction") is defined as an azimuth angle of 90°, and when the retardation layer is observed from the windshield glass side and the azimuth angle increases in the direction of rotation counterclockwise with respect to the reference direction, the average direction of molecular axes 18 of the liquid crystal compound in the retardation layer 16 is positioned at an azimuth angle of 90°, but is not limited to this embodiment, and is preferably positioned at an azimuth angle within a range of 80 to 100°. In FIG. 2, the angle formed between the molecular axes of the liquid crystal compound 18 at the center position of the arrow X direction of the retardation layer 16 (one direction in which the molecular axes 18 continuously rotate) and the reference direction (corresponding to the direction that forms 90° with the arrow X direction) is 0°, but the angle formed is preferably 0 to 5°. The vertically downward direction on the surface of the windshield glass 14 is the Z direction indicated by the arrow in FIG. 1 , which is the direction along the surface of the windshield glass 14. The direction of the Z direction shown in FIG. 1 projected onto the surface of the retardation layer 16 is set to an azimuth angle of 90°, and the direction of the molecular axes of the liquid crystal compounds is defined. The average direction of the molecular axes of the liquid crystal compounds in the retardation layer is the average direction of the changing molecular axis directions of the liquid crystal compounds. Furthermore, when the projected light is S-polarized light, the average direction of the molecular axes 18 of the liquid crystal compounds in the retardation layer 16 is preferably located at an azimuth angle range of 35 to 55°, when the reference direction is set to an azimuth angle of 90° and the azimuth angle increases in the direction of counterclockwise rotation relative to the reference direction when the retardation layer is observed from the windshield glass side.

[0030] The angle formed by the direction in which the orientation of the molecular axis 18 of the liquid crystal compound LC in the retardation layer 16 changes continuously or stepwise and the reference direction is preferably 80 to 100°.

[0031] The thickness of the retardation layer 16 is not particularly limited, and is preferably adjusted so as to fall within the above-mentioned range of in-plane retardation, with a range of 0.6 to 3.0 μm being preferred, and a range of 1.2 to 2.0 μm being more preferred.

[0032] The retardation layer 16 contains a liquid crystal compound LC. As the liquid crystal compound, either a polymer liquid crystal compound or a low molecular weight liquid crystal compound can be used. Here, the term "polymer liquid crystal compound" refers to a liquid crystal compound having a repeating unit in its chemical structure. The term "low molecular weight liquid crystal compound" refers to a liquid crystal compound having no repeating unit in its chemical structure. The liquid crystal compound may be either a rod-shaped liquid crystal compound or a discotic liquid crystal compound, but a rod-shaped liquid crystal compound is preferred.

[0033] The liquid crystal compound in the retardation layer 16 may be fixed. In addition, the liquid crystal compound in the retardation layer 16 may no longer exhibit liquid crystallinity. For example, when the retardation layer 16 is formed using a polymerizable liquid crystal compound, the liquid crystal compound may be polymerized by a curing reaction and may no longer have liquid crystallinity.

[0034] The retardation layer 16 is preferably a layer formed using a composition containing a polymerizable liquid crystal compound. The polymerizable liquid crystal compound is a liquid crystal compound having a polymerizable group. Examples of the polymerizable group include an unsaturated polymerizable group, an epoxy group, and an aziridinyl group. An unsaturated polymerizable group is preferred, and an ethylenically unsaturated polymerizable group is more preferred.

[0035] The method for manufacturing the retardation layer 16 is not particularly limited, and a known method can be used. For example, a method including, in this order, a step of applying a retardation layer-forming composition containing a liquid crystal compound onto an alignment film to form a coating film (hereinafter also referred to as a "coating film forming step") and a step of orienting the liquid crystal compound contained in the coating film (hereinafter also referred to as an "orientation step"). Each step will be described below.

[0036] The coating film forming step is a step of forming a coating film by applying a retardation layer forming composition onto an alignment film. The retardation layer forming composition contains a liquid crystal compound. As described above, the liquid crystal compound may be a polymerizable liquid crystal compound. The retardation layer forming composition may contain components other than the liquid crystal compound (e.g., a solvent, a polymerization initiator, etc.).

[0037] Examples of the method for applying the composition for forming the retardation layer include known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spraying, and inkjet.

[0038] The alignment film may be any film that aligns the liquid crystal compound that can be contained in the retardation layer-forming composition. It can be formed by means such as rubbing an organic compound (preferably a polymer) onto the film surface, oblique deposition of an inorganic compound, formation of a layer with microgrooves, or accumulation of an organic compound (e.g., ω-tricosanoic acid, dioctadecylmethylammonium chloride, methyl stearate) by the Langmuir-Blodgett method (LB film). Furthermore, alignment films that exhibit alignment function upon application of an electric field, application of a magnetic field, or light irradiation are also known. Among these, photo-alignment films formed by light irradiation are also preferred from the viewpoint of uniformity of alignment.

[0039] As the photo-alignment film, a photo-alignment film containing an azobenzene dye or polyvinyl cinnamate or the like is used.

[0040] Methods for imparting an orientation pattern to a photo-alignment film to align liquid crystal compounds include known exposure processes. Among these, a method of exposing a photo-alignment film using a combination of a mask having regions with different transmittances and a polarizer (e.g., a wire grid) (hereinafter, also referred to simply as a "specification method") is exemplified. An example of the specific method is described in detail below. To manufacture an alignment film having an orientation pattern capable of forming a liquid crystal layer with the molecular axes of liquid crystal compounds as shown in FIG. 2 using the specific method, two exposures are performed on the photo-alignment film. First, as shown in FIG. 4, a polarizer 42A and a mask 44A are placed on the photo-alignment film 40, and exposure is performed from the direction indicated by the white arrow. The transmission axis of the polarizer 42A is rotated counterclockwise by a predetermined angle relative to the front-to-back direction of the paper in FIG. 4. More specifically, FIG. 5 is a view of the polarizer 42A observed from the direction of the white arrow in FIG. 4, where the dashed arrow corresponds to the front-to-back direction of the paper in FIG. 4, and the solid arrow corresponds to the transmission axis of the polarizer 42A. The mask 44A has a transmittance that increases in the direction indicated by the arrow in FIG. 4 . During the first exposure, the photo-alignment film 40 is irradiated with light along the transmission axis direction of the polarizer 42A. However, depending on the transmittance distribution of the mask 44A, stronger exposure is performed in the left region of the photo-alignment film 40 in FIG. 4 . Next, as shown in FIG. 6 , the second exposure is performed by placing a polarizer 42B and a mask 44B on the photo-alignment film 40 that has been subjected to the first exposure, and exposure is performed from the direction indicated by the white arrow. The transmission axis of the polarizer 42B is rotated clockwise by a predetermined angle relative to the front-to-back direction in FIG. 6 . More specifically, FIG. 7 is a view of the polarizer 42B observed from the direction indicated by the white arrow in FIG. 6 . The dashed arrow corresponds to the front-to-back direction in FIG. 6 , and the solid arrow corresponds to the transmission axis of the polarizer 42B. The mask 44B has a transmittance that increases in the direction indicated by the arrow in FIG. 6 . When the second exposure is performed, the photo-alignment film 40 is irradiated with light along the transmission axis direction of the polarizer 42B. However, depending on the transmittance distribution of the mask 44B, stronger exposure is performed in the right region of the photo-alignment film 40 in the plane of the paper in Figure 6. When the above-mentioned two exposures are performed, the photo-alignment film 40 is endowed with the function of aligning the liquid crystal compound in different directions near the end portions thereof.Furthermore, the effects of the two exposures cancel each other out near the center of the photo-alignment film 40, providing a function of aligning the liquid crystal compound in a direction intermediate between the alignment directions at both ends of the photo-alignment film 40. As a result, when a retardation layer is formed on such an alignment film, a retardation layer as shown in Fig. 2 is obtained. Note that the direction in which the polarizer is arranged in the above-mentioned specific method is appropriately selected to be optimal depending on the material of the photo-alignment film used.

[0041] The alignment step is a step of aligning the liquid crystal compound contained in the coating film. The alignment step may include a drying treatment. The drying treatment can remove components such as a solvent from the coating film. The drying treatment may be performed by leaving the coating film at room temperature for a predetermined time (for example, natural drying), or by heating and / or blowing air.

[0042] The orientation step preferably includes a heat treatment. From the viewpoint of manufacturability, the heat treatment is preferably performed at a temperature of 10 to 250° C., more preferably 25 to 190° C. The heating time is preferably 1 to 300 seconds, more preferably 1 to 60 seconds.

[0043] The orientation step may include a cooling treatment carried out after the heating treatment. The cooling treatment is a treatment in which the coated film after heating is cooled to about room temperature (20 to 25°C). This further fixes the orientation of the liquid crystal compound contained in the coated film, thereby increasing the degree of orientation of the liquid crystal compound. The cooling method is not particularly limited and can be carried out by a known method.

[0044] After the alignment step, a step of curing the retardation layer (hereinafter also referred to as a "curing step") may be included. The curing step is performed, for example, by heating and / or light irradiation (exposure). Among these, the curing step is preferably performed by light irradiation. As the light source used for curing, various light sources such as infrared light, visible light, and ultraviolet light can be used, but ultraviolet light is preferred. Furthermore, ultraviolet light may be irradiated while heating during curing, or ultraviolet light may be irradiated through a filter that transmits only specific wavelengths. Furthermore, exposure may be performed under a nitrogen atmosphere.

[0045] <Projector> In the projector 12, the image forming section 20 has a light source 34, a polarizing plate 36, and an optical deflector 38. The image forming section 20 is a so-called light beam scanner that forms an image by scanning a light beam.

[0046] The image forming unit 20 emits a light beam modulated according to the projection image from the light source 34, converts the modulated light beam into P-polarized light by the polarizing plate 36, and performs secondarily scanning by the optical deflector 38. The projector 12 secondarily scans the light beam modulated according to the projection image by the optical deflector 38, forms a real image on the intermediate image screen 22, and reflects this real image along a predetermined optical path by the reflecting member 24 and the concave mirror 26. As described above, this reflected light passes through the transmission window 32 and the retardation layer 16 provided in the dashboard 30, is projected onto the windshield glass 14, and is observed as a virtual image through the windshield glass 14 by the observer OB.

[0047] There are no particular limitations on the type of light source 34, and various light sources used for image formation can be used. Examples of the light source 34 include an LED (Light Emitting Diode), a discharge tube, and a laser light source. Note that the LED includes a light emitting diode and an organic light emitting diode (OLED).

[0048] The polarizing plate 36 converts the incident light beam into P-polarized light (p-linearly polarized light). The type of polarizing plate 36 is not particularly limited, and various types of ordinary linear polarizing plates (linear polarizers) can be used. An example of the polarizing plate 36 is a polarizing plate formed by laminating thin films with different refractive index anisotropies. Examples of polarizing plates formed by laminating thin films with different refractive index anisotropies include those described in JP-A-9-506837. Specifically, polarizing plates can be formed using a wide variety of materials by processing them under conditions selected to obtain the refractive index relationship. Commercially available polarizing plates formed by laminating thin films with different refractive index anisotropies may be used. Examples of commercially available polarizing plates include DBEF (manufactured by 3M) and APF (Advanced Polarizing Film). Furthermore, general linear polarizing plates such as an absorptive polarizing plate containing an iodine compound and a reflective polarizing plate such as a wire grid can also be used as the polarizing plate 36. In the embodiment shown in Fig. 1, the polarizing plate 36 converts the incident light beam into P-polarized light (p-linearly polarized light), but the present invention is not limited to this embodiment, and the polarizing plate may convert the incident light beam into S-polarized light (s-linearly polarized light). In this case, the retardation layer may convert S-polarized light into P-polarized light. When the light is converted into S-polarized light by the polarizing plate, it may be possible to reduce the loss of light intensity at each subsequent reflecting member.

[0049] Various types of ordinary optical deflectors capable of secondarily scanning a light beam can be used as the optical deflector 38. Examples of the optical deflector 38 include a galvanometer mirror, a combination of a galvanometer mirror and a polygon mirror, and a microelectromechanical system (MEMS). Of these, MEMS is preferably used.

[0050] In the projector 12, the image forming unit 20 forms a projection image and an image by scanning a light beam, but the present invention is not limited to this. That is, in the projector of the present invention, various image forming devices commonly used in projectors (imagers) of head-up display systems can be used as the image forming device. Examples of image forming devices include LCDs (Liquid Crystal Displays) and LCOS (Liquid Crystal on Silicon) that use fluorescent tubes or liquid crystals. Another example of an image forming device is an organic electroluminescence (organic EL) display. Another example of an image forming device is DLPs (Digital Light Processing) that use DMDs (Digital Micromirror Devices).

[0051] The projection light emitted from the image forming unit 20 is then formed into a real image (visible image) by the intermediate image screen 22. There are no particular restrictions on the type of intermediate image screen 22, and any known intermediate image screen can be used as appropriate.

[0052] As described above, the projection light that has formed a real image on the intermediate image screen 22 is reflected along a predetermined optical path by the reflecting member 24 and the concave mirror 26. The types of the reflecting member 24 and the concave mirror 26 are not particularly limited, and known components can be used as appropriate. While the projector 12 illustrated in FIG. 1 uses the reflecting member 24 and the concave mirror 26 as components that change the optical path of the projection light, the present invention is not limited to this. That is, the projector of the present invention may not include a concave mirror and may only include a reflecting member as a component that changes the optical path of the projection light, or may include one or more other optical reflecting elements in addition to the reflecting member and the concave mirror. As the optical reflecting element, in addition to a concave mirror and a normal mirror, a free-form mirror or the like can also be used. That is, the projector of the present invention can be configured using various optical reflecting elements as long as it includes the reflecting member of the present invention. In addition to the concave mirror described above, a diffractive reflecting element may also be used as a component that changes the optical path of the projection light. Examples of diffractive reflecting elements include a holographic diffraction grating and a surface relief diffraction grating.

[0053] <Windshield Glass> The windshield glass 14 refers to the window glass and windshield glass of vehicles such as cars and trains, airplanes, ships, motorcycles, and playground equipment. The windshield glass is preferably used as the windshield or windshield glass located in front of the vehicle in the traveling direction.

[0054] An example of a windshield glass is shown in Fig. 8. The windshield glass 14 shown in Fig. 8 has, in this order, a first glass plate 50, an intermediate film 52, a reflective film 54, a heat seal layer 56, and a second glass plate 58. In Fig. 8, the reflective film 54 has, in this order from the first glass plate 50 side, a polarization conversion layer 60, a selective reflection layer 62, a retardation layer 64, and a transparent substrate 66.

[0055] When a windshield glass is used in a vehicle, curved glass is often used as the first glass plate 50 and the second glass plate 58. In this case, if the first glass plate 50 is located on the inside of the vehicle and the second glass plate 58 is located on the outside of the vehicle, the first glass plate 50 is arranged with its convex side facing the second glass plate 58, and the second glass plate 58 is arranged with its concave side facing the first glass plate 50.

[0056] Although there are no restrictions on the visible light transmittance of the windshield glass 14, a higher value is preferable. The visible light transmittance of the windshield glass 14 is preferably 70% or more, more preferably greater than 70%, even more preferably 75% or more, and particularly preferably 80% or more. The above-mentioned visible light transmittance is preferably satisfied at all positions on the windshield glass 14, and particularly preferably at the position where the reflective film 54 is present.

[0057] (First Glass Sheet and Second Glass Sheet) Glass sheets commonly used for windshield glass can be used for the glass sheets such as the first glass sheet 50 and the second glass sheet 58. For example, glass sheets having a visible light transmittance of 80% or less, such as 73% or 76%, such as green glass with high heat insulation properties may be used.

[0058] The thickness of the first glass plate 50 and the second glass plate 58 is not particularly limited, but may be about 0.5 to 5.0 mm, preferably 1.0 to 3.0 mm, and more preferably 2.0 to 2.3 mm. The materials or thicknesses of the first glass plate 50 and the second glass plate 58 may be the same or different.

[0059] (Interlayer Film) The interlayer film 52 prevents glass from penetrating into the vehicle interior and scattering in the event of an accident. In the example shown in FIG. 8 , the interlayer film 52 bonds the reflective film 54 and the first glass plate 50 together.

[0060] Any known interlayer film can be used as the interlayer film 52 (interlayer film sheet). For example, a resin film containing a resin selected from the group consisting of polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer, and chlorine-containing resin can be used. The above-mentioned resin is preferably the main component of the interlayer film. Note that "main component" refers to a component that accounts for 50% or more by mass of the interlayer film.

[0061] Of the above resins, polyvinyl butyral or ethylene-vinyl acetate copolymer is preferred, and polyvinyl butyral is more preferred. The resin is preferably a synthetic resin. Polyvinyl butyral can be obtained by acetalizing polyvinyl alcohol with butyraldehyde. The degree of acetalization of the above polyvinyl butyral is preferably 40 to 85%, more preferably 60 to 75%.

[0062] The thickness of the intermediate film 52 is not particularly limited, and may be set in accordance with the forming material, etc., in the same manner as the intermediate film of a known windshield glass.

[0063] (Heat Seal Layer) The heat seal layer (adhesive layer) 56 is not particularly limited and may be, for example, a layer made of a coating type adhesive. In the example shown in Fig. 8, the reflective film 54 is attached to the second glass plate 58 by the heat seal layer 56. Note that although the embodiment in Fig. 8 shows a heat seal layer, the reflective film may be attached directly to the second glass plate.

[0064] The type of heat seal layer 56 is not particularly limited, and any known adhesive made of various types of coating type adhesive can be used as long as it can ensure the transparency required for the windshield glass 14 and can bond the reflective film 54 and the second glass plate 58 with the required adhesive strength. The heat seal layer 56 may be made of the same material as the interlayer 52, such as PVB.

[0065] The heat seal layer 56 may be formed from an adhesive. From the viewpoint of the curing method, adhesives include hot melt type, heat curing type, light curing type, reaction curing type, and pressure sensitive adhesive type that does not require curing.

[0066] The heat seal layer 56 may be formed using a highly transparent adhesive transfer tape (OCA tape). As the highly transparent adhesive transfer tape, a commercially available product for image display devices, particularly a commercially available product for the surface of the image display unit of an image display device, may be used. Examples of commercially available products include adhesive sheets (PD-S1, etc.) manufactured by Panac Corporation and adhesive sheets from the MHM series manufactured by Nichiei Kako Co., Ltd.

[0067] (Polarization Conversion Layer) The polarization conversion layer 60 exhibits optical rotation and birefringence for visible light and converts the polarization state of incident light. The polarization conversion layer 60 converts projected P-polarized light (linearly polarized light) into circularly polarized light reflected by the cholesteric liquid crystal layer of the selective reflection layer 62. The polarization conversion layer 60 is preferably a layer in which a helical orientation structure of a liquid crystal compound is fixed. In particular, the polarization conversion layer 60 is preferably a layer in which a helical orientation structure of a liquid crystal compound is fixed, and the pitch number x of the helical orientation structure and the film thickness y (unit: μm) of the polarization conversion layer preferably satisfy all of the following relational expressions (a) to (c): 0.1≦x≦1.0 (equation (a)); 0.5≦y≦3.0 (equation (b)); and 3000≦(1560×y) / x≦50000 (equation (c)). Note that one pitch of the helical structure of the liquid crystal compound is one turn of the helix of the liquid crystal compound. That is, the pitch number is defined as 1 when the director of the helically aligned liquid crystal compound (the long axis direction in the case of a rod-like liquid crystal) rotates 360°.

[0068] When the polarization conversion layer 60 has a helical structure of a liquid crystal compound, it exhibits optical rotation and birefringence for visible light, which has a wavelength shorter than the reflection peak wavelength in the infrared range. Therefore, it is possible to control polarization in the visible range. By setting the pitch number x of the helical orientation structure of the polarization conversion layer 60 and the film thickness y of the polarization conversion layer 60 within the above ranges, it is possible to provide the polarization conversion layer 60 with the function of optically compensating for visible light or the function of converting linearly polarized light (P-polarized light) incident on the reflective film 54 into circularly polarized light.

[0069] The liquid crystal compound has a helical structure that satisfies the relational expressions (a) to (c), so that the polarization conversion layer 60 exhibits optical rotation and birefringence for visible light. In particular, by setting the pitch P of the helical structure of the polarization conversion layer 60 to a length that corresponds to the pitch P of the cholesteric liquid crystal layer whose selective reflection center wavelength is in the long-wavelength infrared region, the polarization conversion layer 60 exhibits high optical rotation and birefringence for short-wavelength visible light.

[0070] The pitch number x of the helical structure of the polarization conversion layer 60 is more preferably 0.1 to 0.8, and the film thickness y is more preferably 0.6 to 2.6 μm. Furthermore, "(1560×y) / x" is more preferably 5000 to 13000.

[0071] Such a polarization conversion layer 60 can basically be formed in the same manner as a known cholesteric liquid crystal layer.

[0072] A layer in which the helical orientation structure (helical structure) of a liquid crystal compound is fixed is called a cholesteric liquid crystal layer, meaning a layer in which a cholesteric liquid crystal phase is fixed. A cholesteric liquid crystal layer may be any layer in which the orientation of a liquid crystal compound in a cholesteric liquid crystal phase is maintained. A cholesteric liquid crystal layer is typically a layer in which a polymerizable liquid crystal compound is oriented in a cholesteric liquid crystal phase, then polymerized and cured by ultraviolet irradiation, heating, or the like to form a non-fluid layer, and at the same time, changed to a state in which the orientation form does not change due to an external field or external force. It is sufficient for a cholesteric liquid crystal layer to retain the optical properties of the cholesteric liquid crystal phase within the layer; the liquid crystal compound in the layer may no longer exhibit liquid crystallinity. For example, a polymerizable liquid crystal compound may be polymerized by a curing reaction and no longer have liquid crystallinity.

[0073] (Selective Reflection Layer) The selective reflection layer 62 has three cholesteric liquid crystal layers (68R, 68G, 68B). The three cholesteric liquid crystal layers have different selective reflection center wavelengths. In the illustrated example, the selective reflection layer 62 has, in this order, a cholesteric liquid crystal layer 68R having a selective reflection center wavelength in the red wavelength region, a cholesteric liquid crystal layer 68G having a selective reflection center wavelength in the green wavelength region, and a cholesteric liquid crystal layer 68B having a selective reflection center wavelength in the blue wavelength region. In the illustrated example, each cholesteric liquid crystal layer is in direct contact with any of the other cholesteric liquid crystal layers.

[0074] The cholesteric liquid crystal layer is a layer in which liquid crystal compounds are fixed in a helical oriented state of a cholesteric liquid crystal phase, and reflects light with a selective reflection center wavelength corresponding to the pitch of the helical structure and transmits light in other wavelength ranges. The cholesteric liquid crystal layer also exhibits selective reflection for either left- or right-handed circularly polarized light at a specific wavelength.

[0075] In the illustrated example, the selective reflection layer 62 has three cholesteric liquid crystal layers with different selective reflection center wavelengths, but this is not limited to this, and the selective reflection layer 62 may have one cholesteric liquid crystal layer, or two or four or more cholesteric liquid crystal layers.

[0076] The total thickness of the selective reflection layer 62 is preferably 0.4 to 2.0 μm, more preferably 0.6 to 1.8 μm, and even more preferably 0.8 to 1.4 μm.

[0077] (Retardation Layer) The retardation layer 64 imparts a phase difference (optical path difference) between two orthogonal polarization components to change the state of incident polarized light. When the retardation layer 64 is disposed on the exterior side of the vehicle and provides optical compensation, the front retardation of the retardation layer 64 may be a retardation that allows optical compensation. In this case, the front retardation of the retardation layer 64 at a wavelength of 550 nm is preferably 50 to 160 nm. Furthermore, when the direction corresponding to the vertically upward direction of the surface of the first glass plate 50 when the windshield glass 14 having the reflective film 54 is mounted on a vehicle is defined as 0°, the angle of the slow axis of the retardation layer 64 is preferably 10 to 50° or -50 to -10°.

[0078] Furthermore, when the retardation layer 64 converts linearly polarized light into circularly polarized light, the retardation layer 64 is preferably configured to provide an in-plane retardation of λ / 4, or may be configured to provide an in-plane retardation of 3λ / 4. The retardation layer 64 may be disposed such that the angle of the slow axis thereof is oriented in a direction that converts incident linearly polarized light into circularly polarized light.

[0079] In this case, the retardation layer 64 preferably has an in-plane retardation at a wavelength of 550 nm in the range of 100 to 450 nm, more preferably in the range of 120 to 200 nm or 300 to 400 nm.

[0080] The type of the retardation layer 64 is not particularly limited and can be appropriately selected depending on the purpose. Examples of the retardation layer 64 include a stretched polycarbonate film, a stretched norbornene-based polymer film, a transparent film containing and oriented inorganic particles having birefringence such as strontium carbonate, a thin film obtained by obliquely depositing an inorganic dielectric on a support, a film in which a polymerizable liquid crystal compound is uniaxially oriented and fixed in orientation, and a film in which a liquid crystal compound is uniaxially oriented and fixed in orientation.

[0081] The thickness of the retardation layer 64 is not particularly limited, but is preferably 0.2 to 300 μm, more preferably 0.5 to 150 μm, and even more preferably 1.0 to 80 μm.

[0082] (Transparent Substrate) The transparent substrate 66 can also be used as a substrate when forming the selective reflection layer 62. The transparent substrate 66 used for forming the selective reflection layer 62 may be a temporary support that is peeled off after the selective reflection layer 62 is formed.

[0083] The material of the transparent substrate 66 is not particularly limited, and examples thereof include polyesters such as polyethylene terephthalate (PET), polycarbonate, acrylic resins, epoxy resins, polyurethanes, polyamides, polyolefins, cellulose derivatives, and plastic films such as silicone.

[0084] The thickness of the transparent substrate 66 may be about 5.0 to 1000 μm, preferably 10 to 250 μm, and more preferably 15 to 90 μm.

[0085] When the projection light is S-polarized, the windshield glass may include a first glass plate and a second glass plate, and further include a λ / 2 plate disposed between the first and second glass plates. When using the above-described windshield glass including a λ / 2 plate, if projection light is incident from the first glass plate side, the projection light that passes through the first glass plate and enters the λ / 2 plate is converted from S-polarized to P-polarized and then passes through the second glass plate as is, thereby reducing double images.

[0086] <Uses> The head-up display system of the present invention can be used in a variety of applications, including, for example, an in-vehicle head-up display system.

[0087] The features of the present invention will be explained in more detail below with reference to examples. The materials, reagents, amounts and proportions of substances, and procedures shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the following examples.

[0088] <Preparation of Retardation Layer> A glass substrate (Corning EAGLE) was prepared as a support. The following coating liquid for forming an alignment film was applied to the support by spin coating. The support on which the coating film of the coating liquid for forming an alignment film was formed was dried on a hot plate at 60°C for 60 seconds to form an alignment film P-1.

[0089] --Coating liquid for forming alignment film---------------------------------- 1.00 parts by mass of the following photoalignment material; 16.00 parts by mass of water; 42.00 parts by mass of butoxyethanol; 42.00 parts by mass of propylene glycol monomethyl ether.

[0090] Material for photo alignment

[0091]

[0092] The obtained alignment film P-1 was subjected to light irradiation in a specific method of performing two exposures as described in FIGS. 4 to 7. The transmission axis of the polarizer and the transmittance of the mask used were adjusted so as to obtain a retardation layer 1 exhibiting the characteristics described below. Specifically, the transmission axis of the polarizer (wire grid) in the first exposure was positioned at a position rotated 30° counterclockwise with respect to the direction of the arrow indicating the transmittance distribution of the mask 44A, and the first exposure was performed by irradiating ultraviolet light at an exposure dose of 100 mJ / cm. 2 In addition, the transmission axis of the polarizer (wire grid) in the second exposure was positioned at a position rotated 30° clockwise with respect to the direction of the arrow indicating the transmittance distribution of the mask 44B, and the second exposure was performed by irradiating ultraviolet light with an exposure dose of 100 mJ / cm. 2 It was.

[0093] Next, the following components were mixed to prepare a coating liquid for forming a retardation layer having the following composition: Mixture 1: 100 parts by mass Fluorine-based horizontal alignment agent 1 (alignment control agent 1): 0.05 parts by mass Fluorine-based horizontal alignment agent 2 (alignment control agent 2): 0.01 parts by mass Polymerization initiator IRGACURE OXE01 (manufactured by BASF Corporation): 1.0 part by mass Solvent (methyl ethyl ketone): amount to give a solute concentration of 20% by mass

[0094]

[0095]

[0096]

[0097] The retardation layer-forming coating solution was dropped onto the alignment film P-1 that had been subjected to the exposure treatment obtained above, and spin-coated to a film thickness of about 1.5 μm, followed by drying to obtain a coating film of the retardation layer-forming coating solution. Next, the obtained support with the coating film was placed on a hot plate at 50° C., and heated with an electrodeless lamp "D bulb" (60 mW / cm) manufactured by Fusion UV Systems in an environment with an oxygen concentration of 1000 ppm or less. 2) was used to irradiate the coating with ultraviolet light for 6 seconds to fix the liquid crystal phase. As a result, a retardation layer 1 was obtained whose thickness was adjusted to achieve the desired in-plane retardation. The in-plane retardation of the central part of the prepared retardation layer 1 and the orientation of the molecular axis of the liquid crystal compound were measured using an AxoScan, and were found to be 276 nm and 90°. Furthermore, the in-plane retardation of the left end of the prepared retardation layer 1 and the orientation of the molecular axis of the liquid crystal compound were 276 nm and 95°, and the in-plane retardation of the right end of the prepared retardation layer 1 and the orientation of the molecular axis of the liquid crystal compound were 276 nm and 85°. In the retardation layer 1, the orientation of the molecular axis of the liquid crystal compound continuously changed (rotated) in the direction from one end (left end) of the retardation layer 1 to the other end (right end) (see FIG. 2). The rotation angle of the molecular axis of the liquid crystal compound was 10°. The orientation (azimuth angle) of the molecular axis of the liquid crystal compound is a value expressed under the condition that the above-mentioned reference direction is set to 90° and the angle of the azimuth angle increases in the direction of counterclockwise rotation with respect to the reference direction when the retardation layer is observed from the windshield glass side.

[0098] Retardation layers 2 to 7 were produced according to the same procedure as that for producing the retardation layer 1, except that the mask density, the transmission axis of the wire grid, and the thickness of the retardation layer were appropriately adjusted. The characteristics of each retardation layer are shown in the table below. In retardation layers 2 to 7, the orientation of the molecular axis of the liquid crystal compound continuously changed (rotated) in the direction from one end (left end) of each layer to the other end (right end). Retardation layers C1 to C3 were produced by a known method. In retardation layers C1 to C3, the orientation of the molecular axis of the liquid crystal compound was constant.

[0099] <Preparation of Windshield Glass> A 40 μm thick cellulose acylate film was prepared by the same preparation method as in Example 20 of WO 2014 / 112575. UV-531 manufactured by Teisei Kako Co., Ltd. was added to this cellulose acylate film as an ultraviolet absorber. The amount added was 3 phr (per hundred resin). The prepared cellulose acylate film was passed through a dielectric heating roll at a temperature of 60° C., and the film surface temperature was raised to 40° C. Thereafter, an alkaline solution having the composition shown below was applied to one side of the film using a bar coater in an amount of 14 mL / m 2 The coating was then allowed to stand for 10 seconds under a steam-type far-infrared heater (manufactured by Noritake Co., Ltd.) heated to 110°C. Next, pure water was applied at a rate of 3 mL / m using the same bar coater. 2 The film was then washed with water using a fountain coater and then dried with an air knife three times, and then allowed to stay in a drying zone at 70°C for 5 seconds to dry, thereby preparing a saponified cellulose acylate film. The in-plane retardation of the saponified cellulose acylate film was measured with an AxoScan and found to be 1 nm.

[0100] - Composition of alkaline solution - Potassium hydroxide 4.7 parts by mass Water 15.7 parts by mass Isopropanol 64.8 parts by mass Surfactant (C 16 H 33 O (CH 2 CH 2 O) 10 H) 1.0 part by mass Propylene glycol 14.9 parts by mass

[0101] A coating solution for forming an alignment layer having the composition shown below was applied to the saponified surface of a saponified cellulose acylate film (transparent support) at a rate of 24 mL / m using a wire bar coater. 2 The coating was then dried with hot air at 100°C for 120 seconds.

[0102] Composition of coating liquid for forming alignment film: Modified polyvinyl alcohol shown below: 28 parts by mass Citrate ester (AS3, manufactured by Sankyo Chemical Co., Ltd.) 1.2 parts by mass Photoinitiator (Irgacure 2959, manufactured by BASF) 0.84 parts by mass Glutaraldehyde 2.8 parts by mass Water 699 parts by mass Methanol 226 parts by mass

[0103] (Modified polyvinyl alcohol)

[0104]

[0105] The cellulose acylate film having the alignment layer formed thereon was used as a support (transparent substrate). One side of the support facing the alignment layer was subjected to rubbing treatment (rayon cloth, pressure: 0.1 kgf (0.98 N), rotation speed: 1000 rpm (revolutions per minute), conveyance speed: 10 m / min, number of strokes: 1 round trip) in a direction rotated 45° clockwise from the long side direction of the support.

[0106] The above-mentioned coating solution for forming a retardation layer was applied to the rubbed surface of the alignment film on the support using a wire bar, and then dried to obtain a coating film of the coating solution for forming a retardation layer. Next, the obtained support with the coating film was placed on a hot plate at 50°C, and heated with an electrodeless lamp "D bulb" (60 mW / cm) manufactured by Fusion UV Systems in an environment with an oxygen concentration of 1000 ppm or less. 2 The coating film was irradiated with ultraviolet light for 6 seconds using a UV ray irradiator to fix the liquid crystal phase. This resulted in a retardation layer having a thickness adjusted to a desired in-plane retardation. The in-plane retardation of the prepared retardation layer was measured with an AxoScan and found to be 126 nm.

[0107] The following cholesteric liquid crystal layer-forming coating solution (B1) was applied to the surface of the obtained retardation layer using a wire bar at room temperature so that the dry film thickness after drying would be 0.3 μm, thereby obtaining a coating film. The coating film was dried at room temperature for 30 seconds and then heated in an atmosphere at 85°C for 2 minutes. Thereafter, in an environment with an oxygen concentration of 1000 ppm or less, the coating film was irradiated with ultraviolet light at 60% output for 6 to 12 seconds using a Fusion D bulb (90 mW / cm lamp) at 60°C, thereby fixing the cholesteric liquid crystal phase, and obtaining a cholesteric liquid crystal layer B1 with a thickness of 0.3 μm.

[0108] -Coating Solution (B1) for Forming Cholesteric Liquid Crystal Layer- The following components were mixed to prepare a coating solution (B1) for forming a cholesteric liquid crystal layer having the following composition. The amount of right-handed chiral agent LC756 used was adjusted so that the resulting cholesteric liquid crystal layer had a selective reflection center wavelength of 450 nm. - Mixture 1: 100 parts by mass - Fluorine-based horizontal alignment agent 1 (alignment control agent 1): 0.05 parts by mass - Fluorine-based horizontal alignment agent 2 (alignment control agent 2): 0.02 parts by mass - Right-handed chiral agent LC756 (manufactured by BASF) - Polymerization initiator IRGACURE OXE01 (manufactured by BASF) 1.0 part by mass - Solvent (methyl ethyl ketone): Amount to give a solute concentration of 20% by mass

[0109] Next, the same process was repeated using the cholesteric liquid crystal layer forming coating liquid (G1) to laminate a cholesteric liquid crystal layer G1 having a thickness of 0.54 μm on the surface of the obtained cholesteric liquid crystal layer B1.

[0110] —Coating Solution (G1) for Forming Cholesteric Liquid Crystal Layer— A coating solution (G1) for forming a cholesteric liquid crystal layer was prepared by mixing the same components as in the coating solution (B1) for forming a cholesteric liquid crystal layer, except that the amount of the right-handed chiral dopant LC756 used in the coating solution (B1) for forming a cholesteric liquid crystal layer was adjusted so that the selective reflection center wavelength of the resulting cholesteric liquid crystal layer was 680 nm.

[0111] Next, the same process was repeated using the following cholesteric liquid crystal layer forming coating liquid (R1) to laminate a cholesteric liquid crystal layer R1 having a thickness of 0.36 μm on the surface of the obtained cholesteric liquid crystal layer G1.

[0112] —Coating Solution (R1) for Forming Cholesteric Liquid Crystal Layer— A coating solution (R1) for forming a cholesteric liquid crystal layer was prepared by mixing the same components as in the coating solution (B1) for forming a cholesteric liquid crystal layer, except that the amount of the right-handed chiral dopant LC756 used in the coating solution (B1) for forming a cholesteric liquid crystal layer was adjusted so that the selective reflection center wavelength of the resulting cholesteric liquid crystal layer was 820 nm.

[0113] In this way, a selective reflection layer having three cholesteric liquid crystal layers on the retardation layer was obtained. The reflection spectrum of the selective reflection layer was measured with a spectrophotometer (V-670, manufactured by JASCO Corporation), and it was found that the reflection spectrum satisfied the requirements (i) to (iii).

[0114] Next, a polarization conversion layer was formed on the surface of the obtained cholesteric liquid crystal layer by applying a coating solution for forming a polarization conversion layer to a target thickness, thereby producing a reflective film. The polarization conversion layer was formed in the same manner as the formation of the cholesteric liquid crystal layer described above. The pitch number, film thickness, and selective reflection center wavelength of the polarization conversion layer were 0.265, 1.7 μm, and 10,000 nm, respectively.

[0115] - Coating liquid for forming polarization conversion layer - The following components were mixed to prepare a coating liquid for forming a polarization conversion layer having the following composition. The amount of right-handed chiral agent LC756 used was adjusted so as to obtain a polarization conversion layer with the above-mentioned characteristics. - Mixture 1: 100 parts by mass - Fluorine-based horizontal alignment agent 1 (alignment control agent 1): 0.05 parts by mass - Fluorine-based horizontal alignment agent 2 (alignment control agent 2): 0.02 parts by mass - Right-handed chiral agent LC756 (manufactured by BASF) - Polymerization initiator IRGACURE OXE01 (manufactured by BASF) 1.0 part by mass - Solvent (methyl ethyl ketone): Amount to give a solute concentration of 20% by mass

[0116] A first glass plate (FL2, manufactured by Central Glass Co., Ltd., visible light transmittance 90%) measuring 300 mm long x 300 mm wide and 2 mm thick was prepared as the first glass plate and the second glass plate. A 0.76 mm thick PVB film manufactured by Sekisui Chemical Co., Ltd. was prepared as the interlayer film.

[0117] The following components were mixed to prepare a coating solution for forming a heat seal layer: PVB sheet piece (S-LEC film, manufactured by Sekisui Chemical Co., Ltd.) 5.0 parts by weight, methanol 90.25 parts by weight, butanol 4.75 parts by weight. The coating solution for forming a heat seal layer was applied to the support (transparent substrate) side of the reflective film using a wire bar, then dried and heat-treated at 50 ° C for 1 minute to obtain a heat seal layer with a thickness of 1 μm. Next, each component was laminated to form a structure of second glass plate / heat seal layer / transparent substrate / retardation layer / selective reflection layer / polarization conversion layer / interlayer / first glass plate. This laminate was then held at 90 ° C and 10 kPa (0.1 atmosphere) for 1 hour, and then heated in an autoclave (manufactured by Kurihara Seisakusho) at 115 ° C and 1.3 MPa (13 atmospheres) for 20 minutes to remove air bubbles, obtaining windshield glass 1. Windshield glass 1 is capable of reflecting P-polarized light.

[0118] A λ / 2 plate was prepared according to the same procedure as above, except that the thickness was adjusted so that the in-plane retardation was 126 nm to 276 nm. Next, each component was laminated to form a structure of second glass plate / heat seal layer / transparent substrate / retardation layer / interlayer / first glass plate. This laminate was then held at 90°C and 10 kPa (0.1 atm) for one hour, and then heated in an autoclave (manufactured by Kurihara Seisakusho) at 115°C and 1.3 MPa (13 atm) for 20 minutes to remove air bubbles, thereby obtaining a windshield glass 2. The windshield glass 2 is capable of reflecting S-polarized light.

[0119] <Preparation of Evaluation System> Assuming a head-up display system with a field angle of 20°, the retardation layer 1 prepared on an iPad (registered trademark) was placed, and a windshield glass 1 exhibiting P-polarized reflection characteristics was placed at a predetermined position relative to the center of the iPad (registered trademark) and the viewer. Specifically, as shown in Fig. 9, the evaluation system 1 was prepared such that the angle θ1 between the direction of light emitted from the center of the iPad (registered trademark) 72 through the retardation layer 74 and the normal direction of the windshield glass 70, and the angle θ2 between the direction of light reflected by the windshield glass 70 and the normal direction of the windshield glass 70 were both 65°, and the angle θ3 between the direction of light emitted from the vicinity of the end of the retardation layer 74 to the windshield glass 70 and reflected by the windshield glass 70 toward the viewer OB and the normal direction of the windshield glass 70 were 10° or 15°. The retardation layer 1 was arranged so that the orientation (direction) of the molecular axis of the liquid crystal compound at the end of the retardation layer 74 on the left side of the paper shown in FIG. 10 was 95° as described above, and the orientation (direction) of the molecular axis of the liquid crystal compound at the end of the retardation layer 74 on the left side of the paper shown in FIG. 10 was 85°. Instead of the retardation layer 1, retardation layers 2 to 7 and C1 to C3 were used, respectively, and the type of windshield glass was changed, and evaluation systems 2 to 7 and C1 to C3 were prepared in the same manner as evaluation system 1. The orientation of the retardation layers 2 to 7 and C1 to C3 was in accordance with Table 1 described below. The polarized light emitted from the iPad (registered trademark) was circularly polarized, and a λ / 4 film was sandwiched between the iPad (registered trademark) and the retardation layer, so that the polarized light incident on the retardation layer was appropriately S-polarized, P-polarized, or circularly polarized.

[0120] In the evaluation system obtained above, a grid pattern was displayed on an iPad (registered trademark) and double images were evaluated. Evaluation was carried out for two cases where θ3 was 10° and 15°. A: No double image (secondary image) was visible. B: The double image (secondary image) was faintly visible (not bothersome level). C: The double image (secondary image) was clearly visible.

[0121] In Table 1, the "In-plane retardation [nm]" column indicates the in-plane retardation (nm) of each retardation layer at a wavelength of 550 nm. In Table 1, the "Average direction angle [°]" column indicates the angle (°) of the average direction of the molecular axis orientation of the liquid crystal compound in the retardation layer. In Table 1, the "Angle at left end [°]" column indicates the angle (°) of the molecular axis orientation of the liquid crystal compound located at the left end of the retardation layer (the end on the left side of the retardation layer 74 in FIG. 10). In Table 1, the "Angle at right end [°]" column indicates the angle (°) of the molecular axis orientation of the liquid crystal compound located at the right end of the retardation layer (the end on the right side of the retardation layer 74 in FIG. 10). Note that the above angles are values ​​expressed under the condition that the reference direction is 90° and the retardation layer is observed from the windshield glass side, and the azimuth angle increases in the direction of rotation counterclockwise relative to the reference direction. In Table 1, the "Angle difference [°]" column indicates the difference between the value in the "Angle at left end [°]" column and the angle in the "Angle at right end [°]" column. In Table 1, the "Light source" column indicates the type of light emitted to the retardation layer.

[0122]

[0123] As shown in Table 1, the head-up display system incorporating the retardation layer of the present invention exhibited the desired effects. In particular, a comparison between Examples 2 and 5 showed that a more excellent effect was obtained when the in-plane retardation of the retardation layer at a wavelength of 550 nm was 210 to 340 nm. Furthermore, a comparison between Examples 2 to 4 showed that a more excellent effect was obtained when the angle difference was 7 to 15°. Furthermore, a comparison between Example 6 and the other Examples showed that a more excellent effect was obtained when the light emitted to the retardation layer was P-polarized or S-polarized.

[0124] 10 Head-up display system 12 Projector 14, 70 Windshield glass 16, 74 Retardation layer 18 Molecular axis 20 Image forming section 22 Intermediate image screen 24 Reflection member 26 Concave mirror 30 Dashboard 32 Transmitting window 34 Light source 36 Polarizing plate 38 Optical deflector 40 Photo-alignment film 42A, 42B Polarizer 44A, 44B Mask 50 First glass plate 52 Intermediate film 54 Reflection film 56 Heat seal layer 58 Second glass plate 60 Polarization conversion layer 62 Selective reflection layer 64 Retardation layer 66 Transparent substrate 68R, 68G, 68B Cholesteric liquid crystal layer 72 iPad (registered trademark)

Claims

1. A retardation layer disposed between a light source that emits projection light in a head-up display system and a windshield glass onto which the projection light emitted from the light source is irradiated, the retardation layer containing a liquid crystal compound, the orientation of the molecular axis of the liquid crystal compound changing continuously or stepwise along one direction within the plane of the retardation layer.

2. The retardation layer according to claim 1, wherein the in-plane retardation at a wavelength of 550 nm is 100 to 500 nm, and the angle between the molecular axis of the liquid crystal compound located at one end in said one direction and the molecular axis of the liquid crystal compound located at the other end in said one direction is 3 to 40 degrees.

3. The retardation layer according to claim 1, wherein the in-plane retardation at a wavelength of 550 nm is 210 to 340 nm, and the angle between the molecular axis of the liquid crystal compound located at one end in said one direction and the molecular axis of the liquid crystal compound located at the other end in said one direction is 7 to 15°.

4. A projector for a head-up display system, comprising a light source that emits projection light and the retardation layer according to any one of claims 1 to 3.

5. A head-up display system comprising: a projector including a light source that emits projection light; a windshield glass onto which the projection light emitted from the light source is irradiated; and a retardation layer according to any one of claims 1 to 3 that is disposed between the light source and the windshield glass.

6. The head-up display system according to claim 5, wherein the windshield glass reflects P-polarized light, and the projector emits P-polarized projection light.

7. The head-up display system according to claim 5, wherein the windshield glass reflects S-polarized light, and the projector emits S-polarized projection light.

Citation Information

Patent Citations

  • Head-up display device and head-up display system

    JP2021162703A

  • Optically functional film for head-up display, optical laminate, functional glass, and head-up display system

    JP2022089820A

  • Method for improving image quality in a HUD system, polarizing element, and HUD system with such a polarizing element

    JP2023502408A

  • Projected-image display member and projected-image display system

    WO2016052367A1

  • Projection image display member, windshield glass, and head-up display system

    WO2020080355A1

Cited By

  • Reflective film and head-up display system

    WO2025159009A1

  • Head-up display system for transportation means

    WO2026186490A1